Tire rubber composition, tread rubber, and tire
The rubber composition for tires, featuring isoprene skeleton and styrene-butadiene rubber with silica and nitrogen-silicon modifiers, addresses the balance issue between fuel efficiency, wet braking, and wear resistance, surpassing previous silica-based compositions by optimizing the interaction between rubber and fillers.
Patent Information
- Application Number
- PCT/JP2023/043332
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2023-12-04
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional rubber compositions for tires containing silica fail to achieve an optimal balance between low fuel consumption, wet braking performance, and wear resistance, particularly when compared to those using carbon black, leading to insufficient wear resistance in some cases.
A rubber composition for tires comprising a rubber component with isoprene skeleton rubber and styrene-butadiene rubber, along with silica as a filler, where the composition is formulated to satisfy specific mass ratios to enhance breaking strength, fuel efficiency, and wear resistance, and may include modifiers like nitrogen and silicon-containing compounds to improve interaction with fillers.
The proposed rubber composition achieves an excellent balance between fuel efficiency, wet braking performance, and wear resistance, outperforming previous silica-based compositions by improving the interaction between rubber components and fillers, thereby enhancing the tire's overall performance.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Rubber composition for tires, tread rubber and tires
[0001] The present invention relates to a rubber composition for a tire, a tread rubber, and a tire.
[0002] Conventionally, rubber compositions for tires containing silica have been proposed to achieve both low fuel consumption and wet braking performance. For example, Patent Document 1 discloses that by applying a rubber composition containing a rubber component containing 70 mass % or more of natural rubber, a thermoplastic resin, and a filler containing silica to the tread rubber of a tire, the braking performance of the tire on both dry and wet road surfaces is improved. Furthermore, from the perspective of tire economics, when developing rubber compositions for tires, it is necessary to improve wear resistance in addition to low fuel consumption and wet braking performance.
[0003] International Publication No. 2015 / 079703
[0004] However, although the rubber composition of Patent Document 1 imparts the reinforcing properties of silica by using a silane coupling agent in combination, there are cases where, for example, the abrasion resistance is insufficient compared to conventional rubber compositions for tires containing carbon black.
[0005] Therefore, an object of the present invention is to provide a rubber composition for a tire that solves the above-mentioned problems of the conventional technology and can provide a product to which the composition is applied with an excellent balance of fuel economy, wet braking performance, and wear resistance, and a tread rubber that uses the rubber composition for a tire.A further object of the present invention is to provide a tire that includes the tread rubber and that has an excellent balance of fuel economy, wet braking performance, and wear resistance.
[0006] The rubber composition for a tire, tread rubber, and tire of the present invention that solve the above problems are summarized as follows.
[0007] [1] A rubber composition for a tire, comprising a rubber component and a filler, wherein the rubber component comprises at least an isoprene-skeleton rubber and a styrene-butadiene rubber, the filler comprises at least silica, and the following formula (X) is satisfied: 10≦A 0.5 +B 1.5 ≦100 (X) (wherein A is the amount (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the amount of bound styrene (% by mass) of the styrene-butadiene rubber), and the following formula (Y): 0.55≦C / D≦0.75 (Y) (wherein C is the amount (parts by mass) of the silica relative to 100 parts by mass of the rubber component, and D is the amount (parts by mass) of the filler relative to 100 parts by mass of the rubber component). A rubber composition for a tire that satisfies the following formula (Y): 0.55≦C / D≦0.75 (Y) (wherein C is the amount (parts by mass) of the silica relative to 100 parts by mass of the rubber component, and D is the amount (parts by mass) of the filler relative to 100 parts by mass of the rubber component).
[0008] [2] The rubber composition for a tire according to [1], further comprising a resin component.
[0009] [3] The rubber composition for a tire according to [1] or [2], wherein the styrene-butadiene rubber is modified with a modifier containing nitrogen and silicon.
[0010] [4] The rubber composition for a tire according to any one of [1] to [3], wherein the styrene-butadiene rubber is modified with a modifier having a nitrogen-containing functional group and an alkoxy group.
[0011] [5] The rubber composition for a tire according to any one of [1] to [4], wherein the content of the isoprene skeleton rubber is more than 0 parts by mass and less than 70 parts by mass per 100 parts by mass of the rubber component.
[0012] [6] The following formula (Z): 10≦A 0.5 +B 1.5 ≦85 (Z) (wherein A is the amount (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the amount (% by mass) of bound styrene in the styrene-butadiene rubber).
[0013] [7] The rubber composition for a tire according to any one of [1] to [6], wherein the rubber component does not contain butadiene rubber.
[0014] [8] The rubber composition for a tire according to any one of [1] to [7], wherein the amount of sulfur in the rubber composition is 2.5 parts by mass or less per 100 parts by mass of the rubber component.
[0015] [9] The rubber composition for a tire according to any one of [1] to [8], wherein the styrene-butadiene rubber has a bound styrene content of less than 15% by mass.
[0016]
[10] A tread rubber using the rubber composition according to any one of [1] to [9].
[0017]
[11] A tire comprising the tread rubber according to
[10] .
[0018] According to the present invention, it is possible to provide a rubber composition for a tire that can provide a product to which the composition is applied with an excellent balance of fuel economy, wet braking performance, and wear resistance, and a tread rubber that uses the rubber composition for a tire. Also, according to the present invention, it is possible to provide a tire that includes the tread rubber and that has an excellent balance of fuel economy, wet braking performance, and wear resistance.
[0019] The rubber composition for a tire, the tread rubber, and the tire of the present invention will be described in detail below based on embodiments thereof.
[0020] The compounds described herein may be derived in part or in whole from fossil sources, biological sources such as plant sources, recycled sources such as used tires, or a mixture of two or more of fossil, biological, and recycled sources.
[0021] <Rubber Composition for Tire> The rubber composition for tire of the present invention is a rubber composition containing a rubber component and a filler. The rubber component contains at least an isoprene-skeleton rubber and a styrene-butadiene rubber, and the filler contains at least silica. Furthermore, the rubber composition for tire of the present invention satisfies the following formula (X): 10≦A 0.5 +B1.5 ≦100 (X) (wherein A is the content (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the amount of bound styrene (% by mass) of the styrene-butadiene rubber), and the following formula (Y): 0.55≦C / D≦0.75 (Y) (wherein C is the content (parts by mass) of the silica per 100 parts by mass of the rubber component, and D is the content (parts by mass) of the filler per 100 parts by mass of the rubber component). In the rubber composition for tires of the present invention, the rubber component contains an isoprene skeleton rubber, which makes it possible to increase the breaking strength of the rubber composition, and as a result, to improve the fuel economy of products to which the rubber composition is applied. In addition, in the rubber composition for tires of the present invention, the rubber component contains a styrene-butadiene rubber, which makes it possible to improve the wear resistance of products to which the rubber composition for tires is applied. Furthermore, by satisfying the above formula (X), the rubber composition for a tire of the present invention can achieve both fuel economy and wet braking performance in a product to which the rubber composition for a tire is applied.Furthermore, by satisfying the above formula (Y), the rubber composition for a tire of the present invention can ensure wear resistance.Thus, by satisfying both the above formulas (X) and (Y), the rubber composition for a tire of the present invention can achieve an excellent balance between fuel economy, wet braking performance, and wear resistance in a product to which the rubber composition for a tire is applied.
[0022] (Rubber Component) The rubber composition for a tire of the present invention contains a rubber component. The rubber component contains at least an isoprene-based rubber and a styrene-butadiene rubber. The rubber composition for a tire of the present invention may further contain other rubber components.
[0023] -Isoprene Skeleton Rubber- The isoprene skeleton rubber is a rubber having an isoprene unit as the main skeleton. Examples of isoprene skeleton rubber include natural rubber (NR) and synthetic isoprene rubber (IR). When the rubber component contains an isoprene skeleton rubber, the breaking strength of the rubber composition for tires can be increased. As a result, the rolling resistance of a product to which the rubber composition for tires is applied can be reduced, improving fuel economy and the wear resistance of the product.
[0024] The content of the isoprene skeleton rubber is preferably more than 0 part by mass and less than 70 parts by mass, and more preferably 1 to 40 parts by mass, per 100 parts by mass of the rubber component. When the content of the isoprene skeleton rubber is within the above range, it is possible to improve the wet braking performance and fuel economy of a product to which the rubber composition for a tire is applied.
[0025] -Styrene-butadiene rubber (SBR)- The rubber component includes styrene-butadiene rubber (SBR).
[0026] The content of the styrene-butadiene rubber (SBR) is preferably 20 to 99 parts by mass, more preferably 30 to 99 parts by mass, more preferably 40 to 99 parts by mass, even more preferably 50 to 99 parts by mass, and still more preferably 60 to 99 parts by mass, per 100 parts by mass of the rubber component. When the content of the styrene-butadiene rubber is within the above range, the fuel economy and wet braking performance of a product to which the rubber composition for a tire is applied can be improved.
[0027] The styrene-butadiene rubber contained in the rubber composition for a tire of the present invention may be one type alone, or may be two or more different types of styrene-butadiene rubber. As the two or more different types of styrene-butadiene rubber, for example, two or more types of styrene-butadiene rubber having different amounts of bound styrene can be used.
[0028] The styrene-butadiene rubber preferably has a bound styrene content of less than 15% by mass, more preferably 14% by mass or less, more preferably 13% by mass or less, and even more preferably 12% by mass or less. When the bound styrene content of the styrene-butadiene rubber is less than 15% by mass, the glass transition temperature tends to be low. Furthermore, the bound styrene content of the styrene-butadiene rubber is preferably 5% by mass or more, more preferably 7% by mass or more, and even more preferably 8% by mass or more. When the bound styrene content of the styrene-butadiene rubber is 5% by mass or more, the abrasion resistance of products to which the rubber composition for tires is applied can be improved. The bound styrene content of the styrene-butadiene rubber refers to the proportion of styrene units contained in the styrene-butadiene rubber. The bound styrene content of the styrene-butadiene rubber can be adjusted by the amount of monomers used in the polymerization of the styrene-butadiene rubber, the degree of polymerization, and the like. The amount of bound styrene is measured using a spectrophotometer "UV-2450" manufactured by Shimadzu Corporation, based on the amount of absorption of ultraviolet light at a wavelength (near 254 nm) by the phenyl group of styrene, as the amount of bound styrene (% by mass) relative to 100% by mass of the sample.
[0029] The styrene-butadiene rubber may be modified with a modifier. When two or more types of styrene-butadiene rubbers are used, only one of the styrene-butadiene rubbers may be modified, or all of the styrene-butadiene rubbers may be modified. When two or more types of styrene-butadiene rubbers are modified, each styrene-butadiene rubber may be modified with a different modifier.
[0030] --Modified Styrene-Butadiene Rubber-- The styrene-butadiene rubber is preferably modified with a modifier containing nitrogen and silicon. When the styrene-butadiene rubber is modified with a modifier containing nitrogen and silicon, the balance between fuel economy, wet braking performance, and wear resistance of a product to which the rubber composition for tires is applied can be further improved, and in particular, fuel economy and wear resistance can be further improved. Here, the modifier containing nitrogen and silicon is a general term for modifiers containing at least one nitrogen and at least one silicon.
[0031] The styrene-butadiene rubber is more preferably modified with a hydrocarbyloxysilane compound containing nitrogen and silicon. When modified with a hydrocarbyloxysilane compound containing nitrogen and silicon, a so-called dual-end modified styrene-butadiene rubber is obtained, which can further enhance the dispersibility and reinforcing properties of fillers such as carbon black and silica.
[0032] Specific examples of the hydrocarbyloxysilane compound containing nitrogen and silicon that can be used as the modifying agent include N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldimethoxysilane, N,N-bis(trimethylsilyl)aminoethylmethyldiethoxysilane, and 1-trimethylsilyl-2,2-diethoxymethyl-1-aza-2-silacyclopentane, N-(1,3-dimethylbutylidene)-3-(triethoxysilyl)-1-propanamine, N-{3-(triethoxysilyl)propyl}-4,5-dihydroimidazole, N,N-bis(trimethylsilyl)aminopropyltriethoxysilane, and dimethylaminopropyltriethoxysilane, with N,N-bis(trimethylsilyl)aminopropylmethyldimethoxysilane being particularly preferred. These modifiers may be used alone or in combination of two or more.
[0033] Furthermore, the styrene-butadiene rubber is preferably modified with a modifier having a nitrogen-containing functional group and an alkoxy group. When the styrene-butadiene rubber is modified with a modifier having a nitrogen-containing functional group and an alkoxy group, the balance between fuel economy, wet braking performance, and wear resistance of a product to which the tire rubber composition is applied can be further improved, and in particular, fuel economy and wear resistance can be further improved. Here, the modifier having a nitrogen-containing functional group and an alkoxy group is a general term for modifiers having at least one nitrogen-containing functional group and at least one alkoxy group.
[0034] The nitrogen atom-containing functional group is preferably selected from the following: a monovalent hydrocarbon group having a straight-chain, branched, alicyclic, or aromatic ring and having 1 to 30 carbon atoms, and having a functional group selected from the group consisting of a primary amino group, a primary amino group protected with a hydrolyzable protecting group, an onium salt residue of a primary amine, an isocyanate group, a thioisocyanate group, an imine group, an imine residue, an amide group, a secondary amino group protected with a hydrolyzable protecting group, a cyclic secondary amino group, an onium salt residue of a cyclic secondary amine, an acyclic secondary amino group, an onium salt residue of an acyclic secondary amine, an isocyanuric acid triester residue, a cyclic tertiary amino group, an acyclic tertiary amino group, a nitrile group, a pyridine residue, an onium salt residue of a cyclic tertiary amine, and an onium salt residue of an acyclic tertiary amine, or a monovalent hydrocarbon group having a straight-chain, branched, alicyclic, or aromatic ring and having 1 to 30 carbon atoms, which may contain at least one heteroatom selected from an oxygen atom, a sulfur atom, and a phosphorus atom.
[0035] ---Modified Styrene-Butadiene Rubber of First Preferred Embodiment--- The styrene-butadiene rubber (SBR) is preferably modified with an aminoalkoxysilane compound, and from the viewpoint of having a high affinity for fillers, it is more preferable that the terminals of the styrene-butadiene rubber be modified with an aminoalkoxysilane compound. When the terminals of the styrene-butadiene rubber are modified with an aminoalkoxysilane compound, the interaction between the modified styrene-butadiene rubber and the filler (particularly silica) becomes particularly strong.
[0036] The modified site of the styrene-butadiene rubber may be the molecular terminal as described above, or may be the main chain. Styrene-butadiene rubber having a molecular terminal modified can be produced by reacting various modifiers with the terminal of a styrene-butadiene copolymer having an active terminal, for example, according to the methods described in WO 2003 / 046020 and JP 2007-217562 A.
[0037] In a preferred embodiment, the styrene-butadiene rubber having modified molecular terminals can be produced by reacting an aminoalkoxysilane compound with the terminals of a styrene-butadiene copolymer having active terminals with a cis-1,4 bond content of 75% or more, and then reacting the resulting mixture with a carboxylic acid partial ester of a polyhydric alcohol for stabilization, according to the methods described in WO 2003 / 046020 and JP 2007-217562 A.
[0038] The carboxylic acid partial ester of a polyhydric alcohol refers to an ester of a polyhydric alcohol and a carboxylic acid, which has one or more hydroxyl groups. Specifically, esters of fatty acids with sugars or modified sugars having 4 or more carbon atoms are preferably used. More preferred examples of this ester include (1) fatty acid partial esters of polyhydric alcohols, particularly partial esters (monoesters, diesters, or triesters) of saturated or unsaturated higher fatty acids having 10 to 20 carbon atoms with polyhydric alcohols, and (2) ester compounds in which 1 to 3 partial esters of polycarboxylic acids and higher alcohols are bonded to a polyhydric alcohol. Polyhydric alcohols used as raw materials for the partial esters include preferably sugars (hydrogenated or unhydrogenated) having 5 or 6 carbon atoms and at least three hydroxyl groups, glycols, polyhydroxy compounds, and the like. Furthermore, the raw fatty acids are preferably saturated or unsaturated fatty acids having 10 to 20 carbon atoms, such as stearic acid, lauric acid, and palmitic acid. Among the fatty acid partial esters of polyhydric alcohols, sorbitan fatty acid esters are preferred, and specific examples include sorbitan monolaurate, sorbitan monopalmitate, sorbitan monostearate, sorbitan tristearate, sorbitan monooleate, and sorbitan trioleate.
[0039] The aminoalkoxysilane compound is not particularly limited, but is preferably an aminoalkoxysilane compound represented by the following general formula (i): 11 a -Si-(OR 12 ) 4-a ... (i) In general formula (i), R 11 and R 12 each independently represents a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms; R 11 and R 12 At least one of the groups is substituted with an amino group, a is an integer of 0 to 2, and OR 12 If there are multiple, each OR 12may be the same or different, and the molecule does not contain any active protons.
[0040] The aminoalkoxysilane compound is also preferably an aminoalkoxysilane compound represented by the following general formula (ii): In the general formula (ii), n1+n2+n3+n4=4 (wherein n2 is an integer of 1 to 4, and n1, n3, and n4 are integers of 0 to 3). 1 is at least one functional group selected from a saturated cyclic tertiary amine compound residue, an unsaturated cyclic tertiary amine compound residue, a ketimine residue, a nitrile group, a (thio)isocyanate group, an isocyanuric acid trihydrocarbyl ester group, a nitrile group, a pyridine group, a (thio)ketone group, an amide group, and a primary or secondary amino group having a hydrolyzable group. 1 may be the same or different, and A 1 may be a divalent group that bonds with Si to form a cyclic structure. 21 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when n1 is 2 or more, they may be the same or different. 22 is a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, both of which may contain a nitrogen atom and / or a silicon atom. 22 may be the same or different, or may be joined together to form a ring. 23 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or a halogen atom, and when n3 is 2 or greater, may be the same or different. 24represents a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and may be the same or different when n4 is 2 or greater. As the hydrolyzable group in the primary or secondary amino group having a hydrolyzable group, a trimethylsilyl group or a tert-butyldimethylsilyl group is preferred, and a trimethylsilyl group is particularly preferred.
[0041] The aminoalkoxysilane compound represented by the above general formula (ii) is preferably an aminoalkoxysilane compound represented by the following general formula (iii). In the general formula (iii), p1+p2+p3=2 (wherein p2 is an integer of 1 to 2, and p1 and p3 are integers of 0 to 1). 2 is NRa (Ra is a monovalent hydrocarbon group, a hydrolyzable group, or a nitrogen-containing organic group). 25 is a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 26 is a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or a nitrogen-containing organic group, any of which may contain a nitrogen atom and / or a silicon atom. 26 may be the same or different, or may be joined together to form a ring. 27 R is a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or a halogen atom. 28 is a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. As the hydrolyzable group, a trimethylsilyl group or a tert-butyldimethylsilyl group is preferred, and a trimethylsilyl group is particularly preferred.
[0042] The aminoalkoxysilane compound represented by the above general formula (ii) is also preferably an aminoalkoxysilane compound represented by the following general formula (iv) or (v). In the general formula (iv), q1+q2=3 (wherein q1 is an integer of 0 to 2, and q2 is an integer of 1 to 3). 31 is a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 32 and R 33 are each independently a hydrolyzable group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 34 are monovalent aliphatic or alicyclic hydrocarbon groups having 1 to 20 carbon atoms or monovalent aromatic hydrocarbon groups having 6 to 18 carbon atoms, and when q1 is 2, they may be the same or different. 35 represents a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when q2 is 2 or more, may be the same or different.
[0043] In the general formula (v), r1+r2=3 (where r1 is an integer of 1 to 3, and r2 is an integer of 0 to 2). 36 is a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 37 represents a dimethylaminomethyl group, a dimethylaminoethyl group, a diethylaminomethyl group, a diethylaminoethyl group, a methylsilyl(methyl)aminomethyl group, a methylsilyl(methyl)aminoethyl group, a methylsilyl(ethyl)aminomethyl group, a methylsilyl(ethyl)aminoethyl group, a dimethylsilylaminomethyl group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and when r1 is 2 or more, they may be the same or different. R 38represents a hydrocarbyloxy group having 1 to 20 carbon atoms, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and may be the same or different when r2 is 2. A specific example of the aminoalkoxysilane compound represented by general formula (v) is N-(1,3-dimethylbutylidene)-3-triethoxysilyl-1-propanamine.
[0044] The aminoalkoxysilane compound represented by the above general formula (ii) is also preferably an aminoalkoxysilane compound represented by the following general formula (vi) or (vii): In general formula (vi), R 40 is a trimethylsilyl group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 41 R is a hydrocarbyloxy group having 1 to 20 carbon atoms, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 42 is a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms, where TMS represents a trimethylsilyl group (the same applies hereinafter).
[0045] In general formula (vii), R 43 and R 44 are each independently a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 45 is a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, and each R 45 may be the same or different.
[0046] The aminoalkoxysilane compound represented by the above general formula (ii) is also preferably an aminoalkoxysilane compound represented by the following general formula (viii) or the following general formula (ix). In general formula (viii), s1+s2 is 3 (wherein s1 is an integer of 0 to 2, and s2 is an integer of 1 to 3).46 is a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 47 and R 48 are each independently a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 47 or R 48 may be the same or different.
[0047] In general formula (ix), X is a halogen atom. 49 is a divalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms or a divalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 50 and R 51 are each independently a hydrolyzable group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms, or R 50 and R 51 are bonded to form a divalent organic group. 52 and R 53 are each independently a halogen atom, a hydrocarbyloxy group, a monovalent aliphatic or alicyclic hydrocarbon group having 1 to 20 carbon atoms, or a monovalent aromatic hydrocarbon group having 6 to 18 carbon atoms. 50 and R 51 As the hydrolyzable group, a hydrolyzable group is preferred, and as the hydrolyzable group, a trimethylsilyl group or a tert-butyldimethylsilyl group is preferred, and a trimethylsilyl group is particularly preferred.
[0048] The aminoalkoxysilane compound represented by the above general formula (ii) is also preferably an aminoalkoxysilane compound represented by the following general formula (x), the following general formula (xi), the following general formula (xii), or the following general formula (xiii). In the general formulas (x) to (xii), the symbols U and V are each an integer of 0 to 2 and satisfy U+V=2. 54 ~ 92may be the same or different and are monovalent or divalent aliphatic or alicyclic hydrocarbon groups having 1 to 20 carbon atoms, or monovalent or divalent aromatic hydrocarbon groups having 6 to 18 carbon atoms. α and β in general formula (xiii) are integers of 0 to 5.
[0049] Among the compounds satisfying general formula (x), general formula (xi), and general formula (xii), N1,N1,N7,N7-tetramethyl-4-((trimethoxysilyl)methyl)heptane-1,7-diamine, 2-((hexyl-dimethoxysilyl)methyl)-N1,N1,N3,N3-2-pentamethylpropane-1,3-diamine, N1-(3-(dimethylamino)propyl)-N3,N3-dimethyl-N1-(3-(trimethoxysilyl)propyl)propane-1,3-diamine, and 4-(3-(dimethylamino)propyl)-N1,N1,N7,N7-tetramethyl-4-((trimethoxysilyl)methyl)heptane-1,7-diamine are particularly preferred. Among the compounds satisfying general formula (xiii), N,N-dimethyl-2-(3-(dimethoxymethylsilyl)propoxy)ethanamine, N,N-bis(trimethylsilyl)-2-(3-(trimethoxysilyl)propoxy)ethanamine, N,N-dimethyl-2-(3-(trimethoxysilyl)propoxy)ethanamine, and N,N-dimethyl-3-(3-(trimethoxysilyl)propoxy)propan-1-amine are particularly preferred.
[0050] ---Modified Styrene-Butadiene Rubber of Second Preferred Embodiment--- It is also preferable that the styrene-butadiene rubber (SBR) is modified with a coupling agent represented by the following general formula (I). In this case, the fuel economy and wear resistance of a product to which the rubber composition for tires is applied can be further improved. In the above general formula (I), R 1 , R 2 and R 3 R each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms. 4 , R 5 , R 6 , R 7 and R 9R each independently represents an alkyl group having 1 to 20 carbon atoms. 8 and R 11 R each independently represents an alkylene group having 1 to 20 carbon atoms. 10 represents an alkyl group or a trialkylsilyl group having 1 to 20 carbon atoms, m represents an integer of 1 to 3, and p represents 1 or 2. R 1 ~R 11 When a plurality of i, j, and p are present, they are each independent. i, j, and k each independently represent an integer of 0 to 6, provided that (i + j + k) is an integer of 3 to 10. A represents a hydrocarbon group having 1 to 20 carbon atoms, or an organic group having at least one atom selected from the group consisting of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a phosphorus atom, and having no active hydrogen. Here, in general formula (I), the hydrocarbon group represented by A includes saturated, unsaturated, aliphatic, and aromatic hydrocarbon groups. Examples of organic groups having no active hydrogen include a hydroxyl group (-OH), a secondary amino group (>NH), a primary amino group (-NH 2 ), a functional group having an active hydrogen such as a sulfhydryl group (-SH), or an organic group not having such a functional group.
[0051] The styrene-butadiene rubber modified with the coupling agent represented by the general formula (I) has a weight average molecular weight (Mw) of 20×10 4 ~300 x 10 4 and the molecular weight is 200 × 10 relative to the total amount of the modified styrene-butadiene rubber. 4 ~500 x 10 4 It is preferable that the modified styrene-butadiene rubber contains 0.25 to 30 mass % of the modified styrene-butadiene rubber represented by the formula (I) and has a shrinkage factor (g') of less than 0.64.
[0052] In general, polymers having branches tend to have smaller molecular size compared to linear polymers having the same absolute molecular weight, and the shrinkage factor (g') is an index of the ratio of the molecular size to that of a linear polymer having the same assumed absolute molecular weight. In other words, the shrinkage factor (g') tends to decrease as the degree of branching of a polymer increases. In this embodiment, intrinsic viscosity is used as an index of molecular size, and linear polymers have an intrinsic viscosity [η] = -3.883 M 0.771 The shrinkage factor (g') for each absolute molecular weight of the modified styrene-butadiene rubber is calculated, and the shrinkage factor (g') is used as the value that follows the relational expression below when the absolute molecular weight is 100 x 10 4 ~200 x 10 4The average value of the contraction factor (g') when the above formula is used is the contraction factor (g') of the modified styrene-butadiene rubber. Here, "branching" refers to a branch formed by direct or indirect bonding of one polymer to another polymer. Furthermore, the "degree of branching" refers to the number of polymers that are directly or indirectly bonded to one branch. For example, when five styrene-butadiene copolymer chains (described below) are indirectly bonded to each other via coupling residues (described below), the degree of branching is 5. Note that the coupling residue is a structural unit of the modified styrene-butadiene rubber that is bonded to the styrene-butadiene copolymer chain, and is, for example, a structural unit derived from a coupling agent that is generated by reacting a styrene-butadiene copolymer (described below) with a coupling agent. Furthermore, the styrene-butadiene copolymer chain is a structural unit of the modified styrene-butadiene rubber, and is, for example, a structural unit derived from a styrene-butadiene copolymer that is generated by reacting a styrene-butadiene copolymer (described below) with a coupling agent. The shrinkage factor (g') is preferably less than 0.64, more preferably 0.63 or less, more preferably 0.60 or less, even more preferably 0.59 or less, and particularly preferably 0.57 or less. The lower limit of the shrinkage factor (g') is not particularly limited and may be below the detection limit, but is preferably 0.30 or more, more preferably 0.33 or more, even more preferably 0.35 or more, and particularly preferably 0.45 or more. By using a modified styrene-butadiene rubber having a shrinkage factor (g') within this range, the processability of the rubber composition is improved. Since the shrinkage factor (g') tends to depend on the degree of branching, the shrinkage factor (g') can be controlled, for example, using the degree of branching as an index. Specifically, when a modified styrene-butadiene rubber has a branching degree of 6, its shrinkage factor (g') tends to be 0.59 or more and 0.63 or less, and when a modified styrene-butadiene rubber has a branching degree of 8, its shrinkage factor (g') tends to be 0.45 or more and 0.59 or less.
[0053] The styrene-butadiene rubber modified with the coupling agent represented by the general formula (I) preferably has branches and a degree of branching of 5 or more. Furthermore, the modified styrene-butadiene rubber has one or more coupling residues and a styrene-butadiene copolymer chain bonded to the coupling residue, and more preferably, the branches include branches in which five or more styrene-butadiene copolymer chains are bonded to one coupling residue. By specifying the structure of the modified styrene-butadiene rubber so that the degree of branching is 5 or more and the branches include branches in which five or more styrene-butadiene copolymer chains are bonded to one coupling residue, the contraction factor (g') can be more reliably reduced to less than 0.64. The number of styrene-butadiene copolymer chains bonded to one coupling residue can be confirmed from the value of the contraction factor (g'). Furthermore, the modified styrene-butadiene rubber more preferably has branches and a degree of branching of 6 or more. Furthermore, it is more preferable that the modified styrene-butadiene rubber has one or more coupling residues and a styrene-butadiene copolymer chain bonded to the coupling residue, and further, that the branching includes branches in which six or more styrene-butadiene copolymer chains are bonded to one coupling residue. By specifying the structure of the modified styrene-butadiene rubber so that the branching degree is 6 or more and the branching includes branches in which six or more styrene-butadiene copolymer chains are bonded to one coupling residue, the shrinkage factor (g') can be made 0.63 or less. Furthermore, it is more preferable that the modified styrene-butadiene rubber has branches, and the branching degree is 7 or more, and even more preferably 8 or more. The upper limit of the branching degree is not particularly limited, but it is preferably 18 or less.Furthermore, the modified styrene-butadiene rubber has one or more coupling residues and styrene-butadiene copolymer chains bonded to the coupling residues, and further, it is more preferable that the branches include branches in which seven or more styrene-butadiene copolymer chains are bonded to one coupling residue, and it is particularly preferable that the branches include branches in which eight or more styrene-butadiene copolymer chains are bonded to one coupling residue. By specifying the structure of the modified styrene-butadiene rubber so that the branching degree is 8 or more and the branches include branches in which eight or more styrene-butadiene copolymer chains are bonded to one coupling residue, the shrinkage factor (g') can be made 0.59 or less.
[0054] It is preferable that at least one end of the styrene-butadiene copolymer chain is bonded to a silicon atom of each coupling residue. In this case, the ends of a plurality of styrene-butadiene copolymer chains may be bonded to one silicon atom. Alternatively, an end of the styrene-butadiene copolymer chain and an alkoxy group or hydroxyl group having 1 to 20 carbon atoms may be bonded to one silicon atom, and as a result, that one silicon atom may constitute an alkoxysilyl group or silanol group having 1 to 20 carbon atoms.
[0055] The modified styrene-butadiene rubber may be an oil-extended rubber obtained by adding an extender oil. The modified styrene-butadiene rubber may be either non-oil-extended or oil-extended, but from the viewpoint of abrasion resistance, the Mooney viscosity measured at 100°C is preferably 20 or more and 100 or less, and more preferably 30 or more and 80 or less.
[0056] The weight average molecular weight (Mw) of the modified styrene-butadiene rubber is preferably 20×10 4 300 x 10 or more 4 or less, more preferably 50×10 4 or more, and more preferably 64×10 4 More preferably, it is 80×10 4 The weight average molecular weight is preferably 250×10 4or less, and more preferably 180×10 4 or less, and even more preferably 150×10 4 The weight average molecular weight is 20×10 or less. 4 When the weight average molecular weight is 300×10 or more, it is possible to sufficiently improve the low loss property and the wear resistance of the product to which the rubber composition for tires is applied. 4 When it is equal to or less than this, the processability of the rubber composition is improved.
[0057] The modified styrene-butadiene rubber has a molecular weight of 200×10 relative to the total amount (100% by mass) of the modified styrene-butadiene rubber. 4 Above 500 x 10 4 It is preferable that the modified styrene-butadiene rubber (hereinafter also referred to as "specific high molecular weight component") contains 0.25% by mass or more and 30% by mass or less of the specific high molecular weight component. When the content of the specific high molecular weight component is 0.25% by mass or more and 30% by mass or less, the low loss and wear resistance of a product to which the rubber composition for tires is applied can be sufficiently improved. The modified styrene-butadiene rubber contains the specific high molecular weight component preferably at least 1.0% by mass, more preferably at least 1.4% by mass, more preferably at least 1.75% by mass, even more preferably at least 2.0% by mass, particularly preferably at least 2.15% by mass, and extremely preferably at least 2.5% by mass. Furthermore, the modified styrene-butadiene rubber contains the specific high molecular weight component preferably at most 28% by mass, more preferably at most 25% by mass, even more preferably at most 20% by mass, and particularly preferably at most 18% by mass. In this specification, the "molecular weight" of the rubber component refers to the standard polystyrene equivalent molecular weight obtained by GPC (gel permeation chromatography). In order to obtain a modified styrene-butadiene rubber having a content of a specific high molecular weight component within this range, it is preferable to control the reaction conditions in the polymerization step and reaction step described below. For example, in the polymerization step, the amount of an organic monolithium compound used as a polymerization initiator, described below, may be adjusted. Furthermore, in the polymerization step, whether the polymerization method is continuous or batchwise, it is preferable to use a method having a residence time distribution, that is, to widen the time distribution of the propagation reaction.
[0058] In the modified styrene-butadiene rubber, the molecular weight distribution (Mw / Mn), which is the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn), is preferably 1.6 to 3.0. When the molecular weight distribution of the modified styrene-butadiene rubber is in this range, the processability of the rubber composition is good.
[0059] The method for producing the modified styrene-butadiene rubber is not particularly limited, but preferably includes a polymerization step of copolymerizing butadiene and styrene using an organic monolithium compound as a polymerization initiator to obtain a styrene-butadiene copolymer, and a reaction step of reacting an active terminal of the styrene-butadiene copolymer with a pentafunctional or higher reactive compound (hereinafter also referred to as a "coupling agent").
[0060] The polymerization step is preferably a propagation polymerization by a living anionic polymerization reaction, which can produce a styrene-butadiene copolymer having active terminals and a modified styrene-butadiene rubber with a high modification rate. The styrene-butadiene copolymer is obtained by copolymerizing 1,3-butadiene and styrene.
[0061] The amount of the organic monolithium compound used as a polymerization initiator is preferably determined based on the target molecular weight of the styrene-butadiene copolymer or modified styrene-butadiene rubber. The amount of monomers, such as 1,3-butadiene and styrene, used relative to the amount of polymerization initiator is related to the degree of polymerization, i.e., the number average molecular weight and / or weight average molecular weight. Therefore, to increase the molecular weight, it is advisable to adjust the amount of polymerization initiator to a smaller amount, and to decrease the molecular weight, it is advisable to adjust the amount of polymerization initiator to a larger amount. The organic monolithium compound is preferably an alkyllithium compound from the viewpoints of industrial availability and ease of control of the polymerization reaction. In this case, a styrene-butadiene copolymer having an alkyl group at the polymerization initiation terminal is obtained. Examples of alkyllithium compounds include n-butyllithium, sec-butyllithium, tert-butyllithium, n-hexyllithium, benzyllithium, phenyllithium, and stilbenelithium. As the alkyllithium compound, n-butyllithium and sec-butyllithium are preferred from the viewpoints of industrial availability and ease of control of the polymerization reaction. These organic monolithium compounds may be used alone or in combination of two or more.
[0062] In the polymerization step, examples of the polymerization reaction mode include batch and continuous polymerization modes. In a continuous mode, one or two or more connected reactors can be used. Continuous reactors, for example, tank-type or tubular reactors equipped with a stirrer, are used. In a continuous mode, preferably, monomers, an inert solvent, and a polymerization initiator are continuously fed into the reactor, a polymer solution containing a polymer is obtained in the reactor, and the polymer solution is continuously discharged. Batch reactors, for example, tank-type reactors equipped with a stirrer, are used. In a batch mode, preferably, monomers, an inert solvent, and a polymerization initiator are fed, and if necessary, monomers are added continuously or intermittently during polymerization, a polymer solution containing a polymer is obtained in the reactor, and the polymer solution is discharged after the polymerization is completed. In this embodiment, in order to obtain a styrene-butadiene copolymer having a high proportion of active ends, a continuous mode is preferred, which allows the polymer to be continuously discharged and subjected to the next reaction in a short period of time.
[0063] The polymerization step is preferably carried out in an inert solvent. Examples of the solvent include hydrocarbon solvents such as saturated hydrocarbons and aromatic hydrocarbons. Specific hydrocarbon solvents include, but are not limited to, aliphatic hydrocarbons such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, and methylcyclohexane; aromatic hydrocarbons such as benzene, toluene, and xylene, and hydrocarbons consisting of mixtures thereof. Treating impurities such as allenes and acetylenes with an organometallic compound before subjecting the mixture to the polymerization reaction tends to produce a styrene-butadiene copolymer having a high concentration of active terminals, and thus tends to produce a modified styrene-butadiene rubber with a high modification rate, which is preferable.
[0064] A polar compound may be added in the polymerization step. Adding a polar compound allows styrene to be randomly copolymerized with 1,3-butadiene, and the polar compound also tends to be useful as a vinylating agent for controlling the microstructure of the 1,3-butadiene moiety. Examples of the polar compound include ethers such as tetrahydrofuran, diethyl ether, dioxane, ethylene glycol dimethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, diethylene glycol dibutyl ether, dimethoxybenzene, and 2,2-bis(2-oxolanyl)propane; tertiary amine compounds such as tetramethylethylenediamine, dipiperidinoethane, trimethylamine, triethylamine, pyridine, and quinuclidine; alkali metal alkoxide compounds such as potassium tert-amylate, potassium tert-butylate, sodium tert-butylate, and sodium tert-amylate; and phosphine compounds such as triphenylphosphine. These polar compounds may be used alone or in combination of two or more.
[0065] In the polymerization step, from the viewpoint of productivity, the polymerization temperature is preferably 0° C. or higher, more preferably 120° C. or lower, and particularly preferably 50° C. or higher and 100° C. or lower. When the temperature is within such a range, it tends to be possible to ensure a sufficient amount of the coupling agent to react with the active terminals after the completion of polymerization.
[0066] The amount of bound butadiene in the styrene-butadiene copolymer or modified styrene-butadiene rubber is not particularly limited, but is preferably 40% by mass or more and 100% by mass or less, and more preferably 55% by mass or more and 80% by mass or less. The amount of bound butadiene can be determined from the amount of bound styrene measured by ultraviolet absorption of phenyl groups.
[0067] In the styrene-butadiene copolymer or modified styrene-butadiene rubber, the amount of vinyl bonds in the butadiene bond units is not particularly limited, but is preferably 10 mol % or more and 75 mol % or less, and more preferably 20 mol % or more and 65 mol % or less. When the amount of vinyl bonds is within the above range, the low loss properties and wear resistance of products to which the rubber composition for tires is applied can be further improved. Note that for modified styrene-butadiene rubber, the amount of vinyl bonds (1,2-bond amount) in the butadiene bond units can be determined by Hampton's method [R. R. Hampton, Analytical Chemistry, 21, 923 (1949)].
[0068] The alkoxysilyl group possessed by the coupling agent represented by the general formula (I) above tends to react with, for example, the active terminal possessed by the styrene-butadiene copolymer, dissociating the alkoxylithium and forming a bond between the terminal of the styrene-butadiene copolymer chain and the silicon of the coupling residue. The number of alkoxysilyl groups possessed by the coupling residue is the value obtained by subtracting the number of SiOR groups subtracted by the reaction from the total number of SiOR groups possessed by one molecule of the coupling agent. Furthermore, the azasilacycle group possessed by the coupling agent forms an >N-Li bond and a bond between the terminal of the styrene-butadiene copolymer and the silicon of the coupling residue. Note that the >N-Li bond tends to easily become >NH and LiOH upon exposure to water, etc. during finishing. Furthermore, any alkoxysilyl groups remaining unreacted in the coupling agent tend to easily become silanols (Si-OH groups) upon exposure to water, etc. during finishing.
[0069] The reaction temperature in the reaction step is preferably the same as the polymerization temperature of the styrene-butadiene copolymer, preferably 0°C or higher and 120°C or lower, more preferably 50°C or higher and 100°C or lower. The temperature change from the end of the polymerization step to the addition of the coupling agent is preferably 10°C or lower, more preferably 5°C or lower. The reaction time in the reaction step is preferably 10 seconds or longer, more preferably 30 seconds or longer. From the viewpoint of the coupling rate, the shorter the time from the end of the polymerization step to the start of the reaction step, the more preferably it is within 5 minutes. Mixing in the reaction step may be performed by mechanical stirring, stirring with a static mixer, or the like. When the polymerization step is continuous, the reaction step is also preferably continuous. For example, a tank-type or tubular reactor equipped with a stirrer is used in the reaction step. The coupling agent may be diluted with an inert solvent and continuously supplied to the reactor. When the polymerization step is batchwise, the reaction step may be performed by either adding the coupling agent to the polymerization reactor or transferring it to a separate reactor.
[0070] In the general formula (I), A is preferably represented by any one of the following general formulas (II) to (V): When A is represented by any one of the general formulas (II) to (V), a modified styrene-butadiene rubber having better performance can be obtained.
[0071] In the general formula (II), B 1 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 1 are each independent of each other.
[0072] In the general formula (III), B 2 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, B 3 represents an alkyl group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 2 and B 3 are each independent of each other.
[0073] In the general formula (IV), B 4 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 4 are each independent of each other.
[0074] In the general formula (V), B 5 represents a single bond or a hydrocarbon group having 1 to 20 carbon atoms, and a represents an integer of 1 to 10. 5 are each independent of each other.
[0075] B in the general formulas (II) to (V) 1 , B 2 , B 4 , B 5 Regarding the above, examples of the hydrocarbon group having 1 to 20 carbon atoms include an alkylene group having 1 to 20 carbon atoms.
[0076] Preferably, in the general formula (I), A is represented by the general formula (II) or (III), and k is 0. More preferably, in the general formula (I), A is represented by the general formula (II) or (III), and k is 0, and in the general formula (II) or (III), a is an integer of 2 to 10. Even more preferably, in the general formula (I), A is represented by the general formula (II), and k is 0, and in the general formula (II), a is an integer of 2 to 10. Examples of such coupling agents include bis(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]amine, tris(3-trimethoxysilylpropyl)amine, tris(3-triethoxysilylpropyl)amine, tris(3-trimethoxysilylpropyl)-[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, tetrakis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-1,3-propanediamine, and tetrakis(3-trimethoxysilylpropyl). bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trismethoxysilylpropyl)methyl-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-propanediamine, tetrakis(3-trimethoxysilylpropyl)-1,3-bisaminomethylcyclohexane, tris(3-trimethoxysilylpropyl)-methyl-1,3-propanediamine, bis[3-(2,2-dimethoxy-1-aza-2-silacyclopentane)propyl]-(3-trismethoxysilylpropyl)-methyl-1,3-propanediamine, and the like are particularly preferred among these.
[0077] The amount of the compound represented by general formula (I) added as the coupling agent can be adjusted so that the moles of styrene-butadiene copolymer to the moles of coupling agent react in a desired stoichiometric ratio, which tends to achieve a desired degree of branching. Specifically, the moles of the polymerization initiator are preferably 5.0 times or more, more preferably 6.0 times or more, relative to the moles of the coupling agent. In this case, in general formula (I), the number of functional groups of the coupling agent ((m-1) x i + p x j + k) is preferably an integer of 5 to 10, and more preferably an integer of 6 to 10.
[0078] In order to obtain a modified styrene-butadiene rubber having the specific polymer component, the molecular weight distribution (Mw / Mn) of the styrene-butadiene copolymer is preferably 1.5 or more and 2.5 or less, more preferably 1.8 or more and 2.2 or less. The obtained modified styrene-butadiene rubber is preferably one in which a single peak is detected in the molecular weight curve by GPC. The peak molecular weight of the modified styrene-butadiene rubber by GPC is Mp 1 , the peak molecular weight of the styrene-butadiene copolymer is Mp 2 In this case, it is preferable that the following formula is satisfied: 1 / Mp 2 )<1.8×10-12×(Mp 2 -120 x 10 4 ) 2 +2 MP 2 is 20 x 10 4 Above 80 x 10 4 Below, Mp 1 is 30 x 10 4 Above 150 x 10 4 The following is more preferable. 1 and Mp 2 is calculated by gel permeation chromatography (GPC).
[0079] The modification rate of the modified styrene-butadiene rubber is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. When the modification rate is 30% by mass or more, the low loss property and the wear resistance of a product to which the rubber composition for a tire is applied can be further improved.
[0080] After the reaction step, a deactivator, neutralizer, or the like may be added to the copolymer solution as needed. Examples of deactivators include, but are not limited to, water; alcohols such as methanol, ethanol, and isopropanol; and neutralizers include, but are not limited to, carboxylic acids such as stearic acid, oleic acid, and versatic acid (a highly branched carboxylic acid mixture having 9 to 11 carbon atoms, with the majority having 10 carbon atoms); aqueous solutions of inorganic acids; and carbon dioxide gas. Furthermore, from the viewpoint of preventing gel formation after polymerization and improving stability during processing, it is preferable to add an antioxidant such as 2,6-di-tert-butyl-4-hydroxytoluene (BHT), n-octadecyl-3-(4'-hydroxy-3',5'-di-tert-butylphenol)propionate, or 2-methyl-4,6-bis[(octylthio)methyl]phenol to the modified styrene-butadiene rubber.
[0081] The modified styrene-butadiene rubber can be obtained from the polymer solution by any known method, including, for example, a method in which the solvent is separated by steam stripping or the like, the polymer is filtered, and then the polymer is dehydrated and dried to obtain the polymer, a method in which the polymer is concentrated in a flashing tank and then devolatilized using a vent extruder or the like, and a method in which the polymer is directly devolatilized using a drum dryer or the like.
[0082] The modified styrene-butadiene rubber obtained by reacting the coupling agent represented by the above general formula (I) with a styrene-butadiene copolymer is represented, for example, by the following general formula (VI).
[0083] In the general formula (VI), D represents a styrene-butadiene copolymer chain, and the weight average molecular weight of the styrene-butadiene copolymer chain is 10 × 10 4~100 x 10 4 The styrene-butadiene copolymer chain is a structural unit of a modified styrene-butadiene rubber, and is, for example, a structural unit derived from a styrene-butadiene copolymer, which is generated by reacting a styrene-butadiene copolymer with a coupling agent. 12 , R 13 and R 14 R each independently represents a single bond or an alkylene group having 1 to 20 carbon atoms. 15 and R 18 R each independently represents an alkyl group having 1 to 20 carbon atoms. 16 , R 19 , and R 20 R each independently represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. 17 and R 21 R each independently represents an alkylene group having 1 to 20 carbon atoms. 22 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms. m and x represent integers of 1 to 3, with x≦m, p represents 1 or 2, y represents an integer of 1 to 3, with y≦(p+1), and z represents an integer of 1 or 2. When there are multiple D and R, 12 ~R 22 , m, p, x, y, and z are each independent and may be the same or different. Furthermore, i represents an integer of 0 to 6, j represents an integer of 0 to 6, k represents an integer of 0 to 6, (i + j + k) is an integer of 3 to 10, and ((x × i) + (y × j) + (z × k)) is an integer of 5 to 30. A represents a hydrocarbon group having 1 to 20 carbon atoms, or an organic group having at least one atom selected from the group consisting of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a phosphorus atom, and having no active hydrogen. The hydrocarbon group represented by A includes saturated, unsaturated, aliphatic, and aromatic hydrocarbon groups. Examples of the organic group having no active hydrogen include a hydroxyl group (—OH), a secondary amino group (>NH), a primary amino group (—NH 2 ), a functional group having an active hydrogen such as a sulfhydryl group (-SH), or an organic group not having such a functional group.
[0084] In the general formula (VI), A is preferably represented by any one of the general formulas (II) to (V). When A is represented by any one of the general formulas (II) to (V), the low loss property and wear resistance of a product to which the rubber composition for a tire is applied can be further improved.
[0085] ---Third Preferred Embodiment of Modified Styrene-Butadiene Rubber--- It is also preferable that at least one end of the styrene-butadiene rubber (SBR) is modified with a modifier containing a compound (alkoxysilane) represented by the following general formula (1):
[0086] By using, as the rubber component, a styrene-butadiene rubber modified with a modifier containing a compound represented by the general formula (1) containing an oligosiloxane, which is a filler affinity functional group, and a tertiary amino group, the dispersibility of fillers such as silica can be improved. As a result, the rubber composition for tires of the present invention has improved filler dispersibility, and therefore, the low loss properties are significantly improved, and the rolling resistance of tires using the rubber composition for tires can be reduced, thereby improving fuel economy.
[0087] In the above general formula (1), R 1 ~R 8 are each independently an alkyl group having 1 to 20 carbon atoms; L 1 and L 2 are each independently an alkylene group having 1 to 20 carbon atoms; and n is an integer of 2 to 4.
[0088] Specifically, in formula (1), R 1 ~R 4 may each independently represent a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, 1 ~R 4When substituted, each independently may be substituted with one or more substituents selected from the group consisting of an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 3 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, a cycloalkoxy group having 4 to 10 carbon atoms, an aryl group having 6 to 12 carbon atoms, an aryloxy group having 6 to 12 carbon atoms, an alkanoyloxy group having 2 to 12 carbon atoms (Ra-COO-, where Ra is an alkyl group having 1 to 9 carbon atoms), an aralkyloxy group having 7 to 13 carbon atoms, an arylalkyl group having 7 to 13 carbon atoms, and an alkylaryl group having 7 to 13 carbon atoms. More specifically, 1 ~R 4 may be a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, and more specifically, 1 ~R 4 may each independently be a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms.
[0089] In addition, in formula (1), R 5 ~R 8 are each independently a substituted or unsubstituted alkyl group having 1 to 20 carbon atoms, specifically a substituted or unsubstituted alkyl group having 1 to 10 carbon atoms, more specifically a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, and when substituted, 1 ~R 4 It should be noted that the R 5 ~R 8 is not an alkyl group but a hydrolyzable substituent, N-R 5 R 6 and N-R 7 R 8 The bond can be hydrolyzed to N--H in the presence of moisture, adversely affecting the processability of the polymer.
[0090] More specifically, in the compound represented by the formula (1), R 1 ~R 4 is a methyl group or an ethyl group, and R 5 ~R 8 can be an alkyl group having 1 to 10 carbon atoms.
[0091] The amino group in the compound represented by the formula (1), i.e., N—R5 R 6 and N-R 7 R 8 is preferably a tertiary amino group. The tertiary amino group makes the compound represented by formula (1) have better processability when used as a modifying agent. 5 ~R 8 If a protecting group for protecting the amino group is bonded to the terminal of the polymer or if hydrogen is bonded to the terminal of the polymer, it may be difficult to realize the effect of the compound represented by formula (1). If hydrogen is bonded, the anion reacts with hydrogen during the modification process, losing its reactivity and making the modification reaction impossible. If a protecting group is bonded, the modification reaction occurs, but the terminal of the polymer is deprotected by hydrolysis during post-processing to become a primary or secondary amino group. The deprotected primary or secondary amino group may cause the viscosity of the compound to increase during subsequent blending, potentially resulting in reduced processability.
[0092] In addition, L in the compound represented by the formula (1) 1 and L 2 are each independently a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms. 1 and L 2 may each independently be an alkylene group having 1 to 10 carbon atoms, more specifically an alkylene group having 1 to 6 carbon atoms, such as a methylene group, an ethylene group, or a propylene group.
[0093] L in the compound represented by formula (1) 1 and L 2 Regarding the above, the shorter the distance between the Si atom and the N atom in the molecule, the better the effect. However, when Si is directly bonded to N, there is a risk that the bond between Si and N may break during the subsequent treatment process, and the secondary amino group generated in this case is likely to be washed away by water during the post-treatment. In the modified styrene-butadiene rubber produced, it is difficult for the amino group, which promotes bonding with fillers such as silica, to bond with the filler, and as a result, the effect of improving the dispersibility of the filler may be reduced. In this way, when the improvement effect depending on the length of the bond between Si and N is taken into consideration, the above L 1 and L 2is more preferably each independently an alkylene group having 1 to 3 carbon atoms such as a methylene group, an ethylene group, or a propylene group, and more specifically, can be a propylene group. 1 and L 2 First, R 1 ~R 4 It may be substituted with substituents as described above.
[0094] The compound represented by formula (1) is preferably, for example, any one of the compounds represented by the following structural formulas (1-1) to (1-5), because this allows for the realization of even better low loss properties.
[0095] The compound represented by formula (1) has an alkoxysilane structure that bonds to the active terminal of the styrene-butadiene copolymer, while the Si—O—Si structure and three or more amino groups bonded to the terminal exhibit affinity for fillers such as silica, thereby promoting bonding between the filler and the modified styrene-butadiene rubber compared to conventional modifiers containing a single amino group per molecule. Furthermore, the degree of bonding at the active terminal of the styrene-butadiene copolymer is uniform, and when observing the change in molecular weight distribution before and after coupling, the molecular weight distribution remains constant without increasing after coupling compared to before coupling. Therefore, there is no deterioration in the physical properties of the modified styrene-butadiene rubber itself, and the aggregation of the filler in the rubber composition can be prevented, increasing the dispersibility of the filler, thereby improving the processability of the rubber composition. These effects, particularly when the rubber composition is applied to tires, enable a balanced improvement in fuel economy and wet braking performance.
[0096] The compound represented by formula (1) can be produced through a condensation reaction represented by the following reaction scheme.
[0097] In the above reaction scheme, R 1 ~R 8 , L 1 and L 2and n are the same as those defined in the above formula (1), and R′ and R″ are any substituents that do not affect the condensation reaction. For example, R′ and R″ are each independently R 1 ~R 4 It can be identical to any one of the following:
[0098] The reaction in the above reaction scheme proceeds in the presence of an acid, and any acid generally used in condensation reactions can be used without limitation. Those skilled in the art can select an optimal acid depending on various process variables such as the type of reactor in which the reaction is carried out, starting materials, and reaction temperature.
[0099] The styrene-butadiene rubber modified with a modifier containing the compound represented by formula (1) can have a narrow molecular weight distribution (Mw / Mn, also referred to as "polydispersity index (PDI)") of 1.1 to 3.0. If the molecular weight distribution of the modified styrene-butadiene rubber exceeds 3.0 or is less than 1.1, there is a risk of reduced tensile properties and viscoelasticity when applied to a rubber composition. Considering the significant effect of improving tensile properties and viscoelasticity by controlling the molecular weight distribution of the modified styrene-butadiene rubber, the molecular weight distribution of the modified styrene-butadiene rubber is preferably in the range of 1.3 to 2.0. By using the modifier, the modified styrene-butadiene rubber has a molecular weight distribution similar to that of the styrene-butadiene copolymer before modification.
[0100] The molecular weight distribution of the modified styrene-butadiene rubber can be calculated from the ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn). The number average molecular weight (Mn) is the common average of the molecular weights of individual polymers calculated by measuring the molecular weights of n polymer molecules, summing the molecular weights, and dividing by n. The weight average molecular weight (Mw) represents the molecular weight distribution of the polymer composition. The average of the total molecular weight can be expressed in grams per mole (g / mol). The weight average molecular weight and number average molecular weight are each polystyrene-equivalent molecular weights analyzed by gel permeation chromatography (GPC).
[0101] Furthermore, the modified styrene-butadiene rubber satisfies the above-mentioned molecular weight distribution conditions, and at the same time, the weight average molecular weight (Mw) can be 100,000 g / mol to 4,000,000 g / mol, more specifically, 300,000 g / mol to 1,500,000 g / mol. The modified styrene-butadiene rubber can have a number average molecular weight (Mn) of 50,000 g / mol to 2,000,000 g / mol, more specifically, 200,000 g / mol to 800,000 g / mol. When the weight average molecular weight (Mw) of the modified styrene-butadiene rubber is 100,000 g / mol or more and the number average molecular weight (Mn) is 50,000 g / mol or more, a decrease in tensile properties can be suppressed when the modified styrene-butadiene rubber is applied to a rubber composition. Furthermore, when the weight average molecular weight (Mw) is 4,000,000 g / mol or less and the number average molecular weight (Mn) is 2,000,000 g / mol or less, the deterioration of the processability of the modified styrene-butadiene rubber can be suppressed, the workability of the rubber composition does not deteriorate, and the physical properties of the rubber composition can be sufficiently improved. More specifically, when the modified styrene-butadiene rubber simultaneously satisfies the conditions of the weight average molecular weight (Mw) and the number average molecular weight (Mn) as well as the molecular weight distribution, when applied to a rubber composition, it can improve the viscoelasticity and processability of the rubber composition in a balanced manner.
[0102] The modified styrene-butadiene rubber preferably has a vinyl bond content in the butadiene moiety of 5% or more, more preferably 10% or more, and preferably 60% or less. By adjusting the vinyl bond content in the butadiene moiety to fall within the above range, the glass transition temperature can be adjusted to an appropriate range.
[0103] The modified styrene-butadiene rubber may have a Mooney viscosity (MV) at 100°C of 40 to 140, specifically 60 to 100. A Mooney viscosity within this range can exhibit better processability. The Mooney viscosity can be measured using a Mooney viscometer, for example, a Monsanto MV2000E, at 100°C, a rotor speed of 2±0.02 rpm, and a large rotor. The sample used here is left at room temperature (23±3°C) for 30 minutes or more, and then 27±3 g of the sample is taken and filled into the die cavity. The platen is then operated to measure the viscosity.
[0104] As described above, the modified styrene-butadiene rubber is preferably modified at one end with a modifier containing a compound represented by the above general formula (1), and is preferably further modified at the other end with a modifier containing a compound represented by the following general formula (2). By modifying both ends of the modified styrene-butadiene rubber, the dispersibility of the filler in the rubber composition is further improved, and a tire using the rubber composition for tires can achieve both low fuel consumption and wet braking performance at a higher level. In the above general formula (2), R 9 ~R 11 are each independently hydrogen, an alkyl group having 1 to 30 carbon atoms, an alkenyl group having 2 to 30 carbon atoms, an alkynyl group having 2 to 30 carbon atoms, a heteroalkyl group having 1 to 30 carbon atoms, a heteroalkenyl group having 2 to 30 carbon atoms, a heteroalkynyl group having 2 to 30 carbon atoms, a cycloalkyl group having 5 to 30 carbon atoms, an aryl group having 6 to 30 carbon atoms, or a heterocyclic group having 3 to 30 carbon atoms. 12 is a single bond; a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene group having 5 to 20 carbon atoms; or a substituted or unsubstituted arylene group having 5 to 20 carbon atoms, wherein the substituent is an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms. 13is an alkyl group having 1 to 30 carbon atoms; an alkenyl group having 2 to 30 carbon atoms; an alkynyl group having 2 to 30 carbon atoms; a heteroalkyl group having 1 to 30 carbon atoms; a heteroalkenyl group having 2 to 30 carbon atoms; a heteroalkynyl group having 2 to 30 carbon atoms; a cycloalkyl group having 5 to 30 carbon atoms; an aryl group having 6 to 30 carbon atoms; a heterocyclic group having 3 to 30 carbon atoms; or a functional group represented by the following general formula (2a) or general formula (2b), wherein m is an integer of 1 to 5, and R 13 At least one of the functional groups is represented by the following general formula (2a) or (2b), and when m is an integer of 2 to 5, a plurality of R 13 may be the same as or different from each other.
[0105] In the above general formula (2a), R 14 is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene group having 5 to 20 carbon atoms; or a substituted or unsubstituted arylene group having 6 to 20 carbon atoms, wherein the substituent is an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms. 15 and R 16 are each independently an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an alkylene group having 1 to 20 carbon atoms which is substituted or unsubstituted with an aryl group having 6 to 20 carbon atoms. 17 is hydrogen; an alkyl group having 1 to 30 carbon atoms; an alkenyl group having 2 to 30 carbon atoms; an alkynyl group having 2 to 30 carbon atoms; a heteroalkyl group having 1 to 30 carbon atoms; a heteroalkenyl group having 2 to 30 carbon atoms; a heteroalkynyl group having 2 to 30 carbon atoms; a cycloalkyl group having 5 to 30 carbon atoms; an aryl group having 6 to 30 carbon atoms; or a heterocyclic group having 3 to 30 carbon atoms; and X is an N, O, or S atom, provided that when X is O or S, R 17 does not exist.
[0106] In the above general formula (2b), R 18is a substituted or unsubstituted alkylene group having 1 to 20 carbon atoms; a substituted or unsubstituted cycloalkylene group having 5 to 20 carbon atoms; or a substituted or unsubstituted arylene group having 6 to 20 carbon atoms, wherein the substituent is an alkyl group having 1 to 10 carbon atoms, a cycloalkyl group having 5 to 10 carbon atoms, or an aryl group having 6 to 20 carbon atoms. 19 and R 20 are each independently an alkyl group having 1 to 30 carbon atoms; an alkenyl group having 2 to 30 carbon atoms; an alkynyl group having 2 to 30 carbon atoms; a heteroalkyl group having 1 to 30 carbon atoms; a heteroalkenyl group having 2 to 30 carbon atoms; a heteroalkynyl group having 2 to 30 carbon atoms; a cycloalkyl group having 5 to 30 carbon atoms; an aryl group having 6 to 30 carbon atoms; or a heterocyclic group having 3 to 30 carbon atoms.
[0107] In addition, in the compound represented by the general formula (2), R 9 ~R 11 are each independently hydrogen; an alkyl group having 1 to 10 carbon atoms; an alkenyl group having 2 to 10 carbon atoms; or an alkynyl group having 2 to 10 carbon atoms; R 12 is a single bond; or an unsubstituted alkylene group having 1 to 10 carbon atoms, R 13 is an alkyl group having 1 to 10 carbon atoms; an alkenyl group having 2 to 10 carbon atoms; an alkynyl group having 2 to 10 carbon atoms; or a functional group represented by the above general formula (2a) or (2b), and in the above general formula (2a), R 14 is an unsubstituted alkylene group having 1 to 10 carbon atoms, and R 15 and R 16 are each independently an unsubstituted alkylene group having 1 to 10 carbon atoms, and R 17 is an alkyl group having 1 to 10 carbon atoms; a cycloalkyl group having 5 to 20 carbon atoms; an aryl group having 6 to 20 carbon atoms; or a heterocyclic group having 3 to 20 carbon atoms, and in the above general formula (2b), R 18 is an unsubstituted alkylene group having 1 to 10 carbon atoms, and R 19 and R 20 may each independently be an alkyl group having 1 to 10 carbon atoms; a cycloalkyl group having 5 to 20 carbon atoms; an aryl group having 6 to 20 carbon atoms; or a heterocyclic group having 3 to 20 carbon atoms.
[0108] More specifically, the compound represented by the general formula (2) can be a compound represented by the following structural formulas (2-1) to (2-3).
[0109] When the styrene-butadiene copolymer is modified with a modifying agent containing a compound represented by the general formula (2), the modifying agent containing the compound represented by formula (2) is used as a modification initiator. Specifically, for example, a butadiene monomer and a styrene monomer are polymerized in a hydrocarbon solvent in the presence of a modifying agent containing a compound represented by formula (2), thereby imparting a modifying group derived from the compound represented by formula (2) to the styrene-butadiene copolymer.
[0110] -Other Rubbers- The rubber component may further contain other rubbers in addition to the isoprene skeleton rubber and the styrene-butadiene rubber. Specific examples of the other rubbers include butadiene rubber (BR), chloroprene rubber (CR), butyl rubber (IIR), halogenated butyl rubber, ethylene-propylene rubber (EPR, EPDM), fluororubber, silicone rubber, and urethane rubber. As described above, butadiene rubber (BR) may also be contained as the other rubber, but from the viewpoint of preventing a decrease in wet braking performance, it is preferable that butadiene rubber (BR) is not contained. By not including butadiene rubber in the rubber component, a decrease in wet braking performance can be suppressed.
[0111] (Filler) The rubber composition for tires of the present invention contains a filler. The inclusion of a filler improves the reinforcement properties of the rubber composition. Examples of such fillers include silica and carbon black. The content of the filler in the rubber composition for tires is preferably in the range of 40 to 125 parts by mass per 100 parts by mass of the rubber component. When the content of the filler is 40 parts by mass or more per 100 parts by mass of the rubber component, the tire to which the rubber composition for tires is applied is sufficiently reinforced, and the wear resistance can be further improved. Furthermore, when the content of the filler is 125 parts by mass or less per 100 parts by mass of the rubber component, the wet braking performance can be further improved. From the viewpoint of further reducing the rolling resistance of the tire (from the viewpoint of improving fuel economy), the content of the filler in the rubber composition for tires is preferably 45 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 55 parts by mass or more per 100 parts by mass of the rubber component. Furthermore, from the viewpoint of improving the wet braking performance of the tire, the content of the filler in the rubber composition for a tire is more preferably 120 parts by mass or less, more preferably 115 parts by mass or less, and even more preferably less than 100 parts by mass, per 100 parts by mass of the rubber component.
[0112] -Silica- The filler contains silica. Examples of the silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, and aluminum silicate. Among these, wet silica is preferred. These silicas may be used alone or in combination of two or more.
[0113] From the viewpoint of reducing environmental impact, silica derived from siliceous plants is also preferred as the silica. Examples of siliceous plants include mosses, ferns, horsetails, Cucurbitaceae, Urticaceae, and Gramineae plants. Among these plants, grasses are preferred. Examples of grasses include rice, bamboo, and sugarcane, with rice being preferred. Rice is widely cultivated for food and therefore can be procured locally over a wide area. Furthermore, rice husks are generated in large quantities as industrial waste, making it easy to secure a sufficient supply. Therefore, from the viewpoint of availability, silica derived from rice husks (hereinafter also referred to as "rice husk silica") is particularly preferred as silica. The use of rice husk silica allows for the effective use of rice husks, which are industrial waste, and also allows for the local procurement of raw materials near tire manufacturing plants, thereby reducing the energy and costs involved in transportation and storage, which is environmentally preferable from various viewpoints. The rice husk silica may be a powder of rice husk charcoal obtained by carbonizing rice husks by heating, or may be precipitated silica produced by a wet process using an alkali silicate aqueous solution, which is prepared by extracting rice husk ash generated when rice husks are burned as fuel in a biomass boiler with an alkali. The method for producing the rice husk charcoal is not particularly limited, and various known methods can be used. For example, rice husk charcoal can be obtained by pyrolyzing rice husks by steaming them in a kiln. The rice husk charcoal obtained in this manner can be pulverized using a known pulverizer (e.g., a ball mill), and then sorted and classified into a predetermined particle size range to obtain rice husk charcoal powder. The rice husk-derived precipitated silica can be produced by the method described in JP 2019-38728 A, for example.
[0114] The silica has a nitrogen adsorption specific surface area (BET method) of 80 m 2 / g or more 330m 2 The nitrogen adsorption specific surface area (BET method) of silica is preferably less than 80 m 2 When the silica has a nitrogen adsorption specific surface area (BET method) of 330 m / g or more, the product to which the rubber composition for tires is applied can be sufficiently reinforced, and the rolling resistance of the product can be further reduced. 2When the modulus of elasticity of the rubber composition for a tire is less than 1 / g, the modulus of elasticity of the rubber composition for a tire is not too high, and the wet braking performance of the product to which the rubber composition for a tire is applied is further improved. From the viewpoint of further reducing the rolling resistance and further improving the wear resistance of the product, the nitrogen adsorption specific surface area (BET method) of the silica is 110 m 2 / g or more, and 2 / g or more is more preferable, and 150m 2 / g or more, and more preferably 180m 2 From the viewpoint of further improving the wet braking performance of the tire, it is particularly preferable that the nitrogen adsorption specific surface area (BET method) of the silica is 300 m 2 / g or less, and 2 / g or less is more preferable, and 270m 2 It is even more preferable that the SiO2 content is 1 / g or less.
[0115] From the viewpoints of improving the mechanical strength and further improving the abrasion resistance of a product to which the rubber composition for a tire is applied, the content of silica in the rubber composition for a tire is preferably 25 parts by mass or more, more preferably 28 parts by mass or more, and even more preferably 31 parts by mass or more, per 100 parts by mass of the rubber component. Also, from the viewpoint of further improving the wet braking performance of the tire, the content of silica in the rubber composition for a tire is preferably 93 parts by mass or less, more preferably 86 parts by mass or less, and even more preferably less than 75 parts by mass, per 100 parts by mass of the rubber component.
[0116] -Carbon Black- The filler may contain carbon black. The carbon black reinforces the rubber composition for tires and can improve the abrasion resistance of products to which the rubber composition for tires is applied. The carbon black is not particularly limited, and examples thereof include GPF, FEF, HAF, ISAF, and SAF grade carbon black. These carbon blacks may be used alone or in combination of two or more.
[0117] As the carbon black, plant-derived carbon black and recycled carbon black are particularly preferred. Examples of plant-derived carbon black include those derived from castor oil and pine oil. Examples of recycled carbon black include carbon black obtained by pyrolysis of used tires and carbon black obtained from waste oil.
[0118] From the viewpoint of improving the abrasion resistance of a product to which the rubber composition for a tire is applied, the content of carbon black in the rubber composition for a tire is preferably 12 parts by mass or more, more preferably 14 parts by mass or more, and even more preferably 16 parts by mass or more, per 100 parts by mass of the rubber component. Also, from the viewpoint of the wet braking performance of the rubber composition for a tire, the content of carbon black in the rubber composition for a tire is preferably 56 parts by mass or less, more preferably 45 parts by mass or less, and even more preferably 35 parts by mass or less, per 100 parts by mass of the rubber component.
[0119] Other Fillers The filler may include inorganic fillers such as clay, talc, calcium carbonate, and aluminum hydroxide, in addition to silica and carbon black.
[0120] (Regarding Formula (X)) The rubber composition for a tire of the present invention satisfies the formula (X): 10≦A 0.5 +B 1.5 ≦100 (X) (wherein A is the content (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the bound styrene amount (% by mass) of the styrene-butadiene rubber), and satisfies formula (Z): 10≦A 0.5 +B 1.5It is preferable that the following is satisfied: ≦85 (Z) (wherein A is the content (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the amount of bound styrene (% by mass) of the styrene-butadiene rubber). When the rubber composition for a tire of the present invention satisfies formula (X), it is possible to achieve both low fuel consumption performance and wet braking performance, and further, when formula (Z) is satisfied, it is possible to improve the low fuel consumption performance. In addition, when the rubber composition for a tire of the present invention satisfies both formula (X) and formula (Y) described below, it is possible to achieve an excellent balance between low fuel consumption performance, wet braking performance, and wear resistance of a product to which the rubber composition for a tire is applied.
[0121] When two or more types of styrene-butadiene rubber are used, the amount of bound styrene in the styrene-butadiene rubber is an average value taking into account their mass ratios. For example, when two types of styrene-butadiene rubber are used, B in formula (X): the amount of bound styrene in the styrene-butadiene rubber (mass %) is calculated as follows. If the two types of styrene-butadiene rubber are styrene-butadiene rubber 1 and styrene-butadiene rubber 2, respectively, then B = x x a / (a + b) + y x b / (a + b) (x: amount of bound styrene in styrene-butadiene rubber 1 (mass %) y: amount of bound styrene in styrene-butadiene rubber 2 (mass %) a: content (parts by mass) of styrene-butadiene rubber 1 b: content (parts by mass) of styrene-butadiene rubber 2) Similarly, when n types of styrene-butadiene rubber are used, the nth type of styrene-butadiene rubber is referred to as "SBR" n " Then, the following equation is used: B = Σ(SBR n Amount of bound styrene × SBR n Content of SBR) / Σ(SBR n It can be calculated from the content of
[0122] [A 0.5 +B 1.5From the viewpoint of achieving both low fuel consumption and wet braking performance, the value is preferably 15 or more, more preferably 25 or more, even more preferably 30 or more, and particularly preferably 35 or more. From the same viewpoint, the value is preferably 85 or less, more preferably 80 or less, even more preferably 75 or less, and particularly preferably 70 or less.
[0123] [A 0.5 +B 1.5 ] can be adjusted by changing the amount of various rubbers contained in the rubber component. 0.5 +B 1.5 ] can be achieved by increasing the content of natural rubber in the rubber component, using a styrene-butadiene rubber with a higher bound styrene content, and when using two or more types of styrene-butadiene rubber, increasing the amount of the styrene-butadiene rubber with a higher bound styrene content. 0.5 +B 1.5 In addition, the value of [A 0.5 +B 1.5 ] can be improved by, for example, reducing the content of natural rubber in the rubber component, using a styrene-butadiene rubber with a lower bound styrene content, compounding a rubber other than styrene-butadiene rubber, such as butadiene rubber, and, when using two or more types of styrene-butadiene rubber, increasing the amount of the styrene-butadiene rubber with a lower bound styrene content. 0.5 +B 1.5 ] can be reduced.
[0124] (Regarding Formula (Y)) The rubber composition for tires of the present invention satisfies formula (Y): 0.55≦C / D≦0.75 (Y) (wherein C is the content (parts by mass) of the silica per 100 parts by mass of the rubber component, and D is the content (parts by mass) of the filler per 100 parts by mass of the rubber component). When the rubber composition for tires satisfies formula (Y), abrasion resistance can be ensured. Furthermore, when the rubber composition for tires satisfies both formulas (X) and (Y) described above, a product to which the rubber composition for tires is applied can have an excellent balance of fuel economy, wet braking performance, and abrasion resistance.
[0125] From the viewpoint of ensuring wear resistance, [C / D] in the formula (Y) is 0.55 or more, preferably 0.57 or more, and from the same viewpoint, is 0.75 or less, preferably 0.73 or less.
[0126] The value of [C / D] in the formula (Y) can be adjusted by adjusting the content of silica contained in the filler, the total amount of the filler, or the like.
[0127] (Resin Component) The rubber composition for a tire of the present invention may contain a resin component. The resin component is not particularly limited, and various resin components can be used. When the rubber composition for a tire of the present invention contains a resin component, the wet braking performance of a product to which the rubber composition for a tire is applied can be improved.
[0128] Although not limited thereto, the resin component is at least partially hydrogenated, and the difference in SP value (solubility parameter) between the resin component and the isoprene skeleton rubber is 1.40 (cal / cm 3 ) 1/2 In this case, compatibility with the isoprene skeleton rubber is increased, the mobility of the rubber component is controlled, and the hysteresis loss (tan δ) in the low temperature range can be improved, thereby improving the wet braking performance of a product to which the rubber composition for tires is applied. From the viewpoint of further improving compatibility, the difference in SP value between the resin component and the isoprene skeleton rubber is preferably 1.35 (cal / cm 3 ) 1/2It is preferable that the value is 0.50 (cal / cm 3 ) 1/2 More preferably, it is 0.45 (cal / cm 3 ) 1/2 More preferably, it is 0.3 (cal / cm 3 ) 1/2 It is even more preferable that the calorie content is 0.25 (cal / cm 3 ) 1/2 It is particularly preferable that the difference in SP value between the resin component and the isoprene skeleton rubber is 0.50 (cal / cm 3 ) 1/2 When the solubility parameter (SP) of the isoprene skeleton rubber and the resin component is not more than 100%, the compatibility between the resin component and the isoprene skeleton rubber is further improved, and the wet braking performance of the product to which the rubber composition is applied is further improved. The SP values (solubility parameters) of the isoprene skeleton rubber and the resin component are calculated according to the Fedors method.
[0129] Furthermore, the mass ratio of the resin component to the isoprene skeleton rubber [mass ratio of resin component / isoprene skeleton rubber] is preferably 0.5 or more. In this case, the wet braking performance of a product to which the rubber composition for a tire is applied can be further improved. The mass ratio of the resin component to the isoprene skeleton rubber [mass ratio of resin component / isoprene skeleton rubber] is preferably 0.65 or more, more preferably 0.7 or more, and still more preferably 0.8 or more, and is preferably 2.0 or less, more preferably 1.9 or less, and even more preferably 1.8 or less.
[0130] The content of the resin component is preferably 1 part by mass or more and less than 50 parts by mass per 100 parts by mass of the rubber component. When the content of the resin component in the rubber composition is 1 part by mass or more per 100 parts by mass of the rubber component, the effect of the resin component is fully exhibited, and when it is less than 50 parts by mass, the resin component is less likely to precipitate from the tire, allowing the effect of the resin component to be fully exhibited. From the viewpoint of further enhancing the effect of the resin component, the content of the resin component in the rubber composition is preferably 5 parts by mass or more, more preferably 7 parts by mass or more, more preferably 9 parts by mass or more, still more preferably 15 parts by mass or more, and still more preferably 17 parts by mass or more per 100 parts by mass of the rubber component. Furthermore, from the viewpoint of suppressing precipitation of the resin component from the tire and suppressing deterioration of the tire appearance, the content of the resin component in the rubber composition is more preferably 45 parts by mass or less, and still more preferably 40 parts by mass or less per 100 parts by mass of the rubber component.
[0131] The resin component preferably has a softening point higher than 110°C and a weight-average molecular weight in polystyrene equivalent of 200 to 1600 g / mol. By applying a rubber composition for tires containing such a resin component to a product, the wear resistance of the product can be further improved. Here, the softening point of the resin component is measured in accordance with JIS-K2207-1996 (ring and ball method). The weight-average molecular weight of the resin component is measured by gel permeation chromatography (GPC) and calculated as a polystyrene equivalent value.
[0132] When the softening point of the resin component is higher than 110°C, a product to which the rubber composition for a tire is applied can be sufficiently reinforced, and abrasion resistance can be further improved. From the viewpoint of abrasion resistance of a tire, the softening point of the resin component is preferably 116°C or higher, more preferably 120°C or higher, more preferably 123°C or higher, and even more preferably 127°C or higher. Furthermore, from the viewpoint of processability, the softening point of the resin component is preferably 160°C or lower, more preferably 150°C or lower, more preferably 145°C or lower, more preferably 141°C or lower, and even more preferably 136°C or lower.
[0133] When the polystyrene-equivalent weight-average molecular weight of the resin component is 200 g / mol or more, the resin component is less likely to precipitate from the tire and the effects of the resin component can be fully exhibited, and when it is 1600 g / mol or less, the resin component is more likely to be compatible with the rubber component. From the viewpoint of suppressing the resin component from precipitating from the tire and suppressing deterioration of the tire appearance, the polystyrene-equivalent weight-average molecular weight of the resin component is preferably 500 g / mol or more, more preferably 550 g / mol or more, even more preferably 600 g / mol or more, even more preferably 650 g / mol or more, and still more preferably 700 g / mol or more. Furthermore, from the viewpoint of improving the compatibility of the resin component with the rubber component and further enhancing the effects of the resin component, the polystyrene-equivalent weight average molecular weight of the resin component is more preferably 1570 g / mol or less, more preferably 1530 g / mol or less, more preferably 1500 g / mol or less, more preferably 1470 g / mol or less, more preferably 1430 g / mol or less, more preferably 1400 g / mol or less, more preferably 1370 g / mol or less, more preferably 1330 g / mol or less, more preferably 1300 g / mol or less, more preferably 1200 g / mol or less, more preferably 1100 g / mol or less, more preferably 1000 g / mol or less, and even more preferably 950 g / mol or less.
[0134] The weight average molecular weight (Mw HR ) (unit: g / mol) to the softening point (Ts HR ) (unit: °C) ratio (Ts HR / Mw HR ) is preferably 0.07 or more, more preferably 0.083 or more, more preferably 0.095 or more, more preferably 0.104 or more, more preferably 0.125 or more, more preferably 0.135 or more, more preferably 0.14 or more, and even more preferably 0.141 or more.HR / Mw HR ) is preferably 0.25 or less, preferably 0.24 or less, preferably 0.23 or less, preferably 0.19 or less, more preferably 0.18 or less, and even more preferably 0.17 or less. The weight average molecular weight in terms of polystyrene is calculated by measuring the average molecular weight of the resin by gel permeation chromatography (GPC) under the following conditions: Column temperature: 40°C Injection volume: 50 μL Carrier and flow rate: tetrahydrofuran 0.6 mL / min Sample preparation: About 2.5 mg of resin component is dissolved in 10 mL of tetrahydrofuran.
[0135] The hydrogenated resin component mentioned above means a resin obtained by reducing and hydrogenating a resin. The resins that can be used as raw materials for the hydrogenated resin component include C 5 based resin, C 5 -C 9 based resin, C 9 These resins may be used singly or in combination of two or more.
[0136] Said C 5 As a resin based on C, there is C obtained by thermal decomposition of naphtha in the petrochemical industry. 5 and aliphatic petroleum resins obtained by (co)polymerizing the distillate. 5 The fraction usually contains olefinic hydrocarbons such as 1-pentene, 2-pentene, 2-methyl-1-butene, 2-methyl-2-butene, and 3-methyl-1-butene, and diolefinic hydrocarbons such as 2-methyl-1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, and 3-methyl-1,2-butadiene. 5 Commercially available resins can be used.
[0137] Said C 5 -C 9 The C-based resin is 5 -C 9 It refers to synthetic petroleum resin, 5 -C9 Examples of the resin include petroleum-derived C 5 -C 11 The fraction was treated with AlCl 3 , B.F. 3 More specifically, copolymers containing styrene, vinyl toluene, α-methyl styrene, indene, etc. as the main component may be mentioned. 5 -C 9 As the resin, 9 Resins containing less of the above components are preferred from the viewpoint of compatibility with the rubber component. 9 "Low amount of the above components" means that the C 9 This means that the above components are contained in an amount of less than 50% by mass, preferably 40% by mass or less. 5 -C 9 Commercially available resins can be used.
[0138] Said C 9 The C-based resin is 9 This refers to synthetic petroleum resins, such as AlCl 3 or BF 3 Using a Friedel-Crafts type catalyst such as C 9 It refers to a solid polymer obtained by polymerizing the fraction. 9 Examples of the resin include copolymers containing indene, α-methylstyrene, vinyltoluene, etc. as main components.
[0139] The terpene resin is a solid resin obtained by blending turpentine, which is obtained simultaneously when rosin is extracted from pine trees, or a polymerization component separated from the blend, and polymerizing the blend using a Friedel-Crafts catalyst. Examples of such resins include β-pinene resin and α-pinene resin. Furthermore, a representative example of a terpene-aromatic compound resin is terpene-phenol resin. This terpene-phenol resin can be obtained by reacting terpenes with various phenols using a Friedel-Crafts catalyst, or by further condensing the terpene with formalin. There are no particular limitations on the terpenes used as raw materials; monoterpene hydrocarbons such as α-pinene and limonene are preferred, with those containing α-pinene being more preferred, and α-pinene being particularly preferred. Styrene or the like may also be included in the skeleton.
[0140] The dicyclopentadiene resin is, for example, AlCl 3 or BF 3 This refers to a resin obtained by polymerizing dicyclopentadiene using a Friedel-Crafts catalyst such as
[0141] The resin that is the raw material for the hydrogenated resin component is, for example, C 5 A resin (C) copolymerized with the fraction and dicyclopentadiene (DCPD) 5 -DCPD-based resin). When the dicyclopentadiene-derived component is 50% by mass or more in the total amount of the resin, C 5 -DCPD-based resins are included in dicyclopentadiene-based resins. When the dicyclopentadiene-derived component is less than 50% by mass in the total amount of resin, C 5 -DCPD resin is C 5 The same applies to cases where a small amount of a third component is contained.
[0142] From the viewpoints of increasing the compatibility between the rubber component and the resin component, further improving the wet braking performance of a product to which the rubber composition for a tire is applied, and further reducing the rolling resistance, the resin component is 5 based resin, hydrogenated C 5 -C 9The resin is preferably at least one selected from the group consisting of hydrogenated dicyclopentadiene resins (hydrogenated DCPD resins), hydrogenated terpene resins, and hydrogenated C 5 Resin and hydrogenated C 5 -C 9 It is more preferable that the resin is at least one selected from the group consisting of hydrogenated C 5 Furthermore, it is preferable that the resin has at least a hydrogenated DCPD structure or a hydrogenated cyclic structure in the monomer.
[0143] (Styrene-based thermoplastic elastomer) The rubber composition for tires of the present invention may further contain a styrene-based thermoplastic elastomer (TPS). The styrene-based thermoplastic elastomer (TPS) has a styrene-based polymer block (hard segment) and a conjugated diene-based polymer block (soft segment), where the styrene-based polymer portion forms physical crosslinks and serves as a crosslinking point, while the conjugated diene-based polymer block imparts rubber elasticity. The double bonds of the conjugated diene-based polymer block (soft segment) may be partially or completely hydrogenated. Note that the styrene-based thermoplastic elastomer (TPS) is thermoplastic, while the rubber component (preferably, a diene-based rubber) is not thermoplastic. Therefore, in this specification, the styrene-based thermoplastic elastomer (TPS) is not included in the rubber component.
[0144] The content of the styrene-based thermoplastic elastomer (TPS) is preferably in the range of 1 to 30 parts by mass per 100 parts by mass of the rubber component.
[0145] Examples of the styrene-based thermoplastic elastomer (TPS) include at least one of styrene / butadiene / styrene (SBS) copolymer, styrene / isoprene / styrene (SIS) block copolymer, styrene / butadiene / isoprene / styrene (SBIS) block copolymer, styrene / isoprene (SI) block copolymer, styrene / butadiene / isoprene (SBI) block copolymer, styrene / ethylene / butylene / styrene (SEBS) block copolymer, styrene / ethylene / propylene / styrene (SEPS) block copolymer, styrene / ethylene / ethylene / propylene / styrene (SEEPS) block copolymer, styrene / ethylene / butylene (SEB) block copolymer, and styrene / ethylene / ethylene / propylene (SEEP) block copolymer.
[0146] (Others) In addition to the rubber component, filler, resin component, and styrene-based thermoplastic elastomer described above, the rubber composition for a tire of the present invention may contain, as necessary, various components commonly used in the rubber industry, such as silane coupling agents, antioxidants, waxes, softeners, processing aids, stearic acid, zinc oxide (zinc white), vulcanization accelerators, vulcanizing agents, etc., which are appropriately selected within ranges that do not impair the object of the present invention. Commercially available products can be suitably used as these compounding ingredients.
[0147] Silane Coupling Agent—The rubber composition for a tire of the present invention contains silica, and therefore preferably contains a silane coupling agent to enhance the effect of the silica. Examples of the silane coupling agent include bis(3-triethoxysilylpropyl)tetrasulfide, bis(3-triethoxysilylpropyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, 2-mercaptoethyltrimethoxysilane, 2-mercaptoethyltriethoxysilane, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide, and 3-triethoxysilylpropyl-N,N-dimethylthiocarbamoyltetrasulfide. Examples of such tetrasulfides include N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, 3-trimethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl benzothiazolyl tetrasulfide, 3-triethoxysilylpropyl methacrylate monosulfide, 3-trimethoxysilylpropyl methacrylate monosulfide, bis(3-diethoxymethylsilylpropyl)tetrasulfide, 3-mercaptopropyldimethoxymethylsilane, dimethoxymethylsilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, and dimethoxymethylsilylpropyl benzothiazolyl tetrasulfide.
[0148] The content of the silane coupling agent is preferably in the range of 2 to 20 parts by mass, more preferably in the range of 5 to 15 parts by mass, per 100 parts by mass of the silica.
[0149] - Antiaging Agent - Examples of the antioxidant include N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6C), 2,2,4-trimethyl-1,2-dihydroquinoline polymer (TMDQ), 6-ethoxy-2,2,4-trimethyl-1,2-dihydroquinoline (AW), N,N'-diphenyl-p-phenylenediamine (DPPD), etc. The content of the antioxidant is not particularly limited, and is preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 1 part by mass or more and 4 parts by mass or less, per 100 parts by mass of the rubber component.
[0150] —Wax— Examples of the wax include paraffin wax, microcrystalline wax, etc. The amount of the wax is not particularly limited, and is preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 1 part by mass or more and 4 parts by mass or less, per 100 parts by mass of the rubber component.
[0151] - Zinc Oxide (Zinc Oxide) - The content of the zinc oxide (zinc oxide) is not particularly limited and is preferably 0.1 parts by mass or more and 10 parts by mass or less, and more preferably 1 part by mass or more and 8 parts by mass or less, per 100 parts by mass of the rubber component.
[0152] -Vulcanization accelerator- Examples of the vulcanization accelerator include sulfenamide-based vulcanization accelerators, guanidine-based vulcanization accelerators, thiazole-based vulcanization accelerators, thiuram-based vulcanization accelerators, and dithiocarbamate-based vulcanization accelerators. These vulcanization accelerators may be used alone or in combination of two or more. The content of the vulcanization accelerator is not particularly limited, and is preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 0.2 parts by mass or more and 4 parts by mass or less, per 100 parts by mass of the rubber component.
[0153] - Vulcanizing Agent - Examples of the vulcanizing agent include sulfur. The content of the vulcanizing agent is preferably 2.5 parts by mass or less, and more preferably 1.4 parts by mass or more and 2.5 parts by mass or less, in terms of sulfur content, per 100 parts by mass of the rubber component. When the content of the vulcanizing agent is within the above range, deterioration of wet braking performance can be suppressed. Furthermore, the content of the vulcanizing agent is more preferably 1.6 parts by mass or more and 2.3 parts by mass or less, and even more preferably 1.7 parts by mass or more and 2.2 parts by mass or less, per 100 parts by mass of the rubber component.
[0154] (Method for producing rubber composition for tire) The method for producing the rubber composition for tire is not particularly limited, but the rubber composition for tire can be produced, for example, by blending various components appropriately selected as necessary with the above-mentioned rubber component and filler, and kneading, heating, extruding, etc. Furthermore, the obtained rubber composition can be vulcanized to produce a vulcanized rubber.
[0155] As described above, a rubber composition for a tire that satisfies formula (X) can be produced by adjusting the amounts of various rubbers contained in the rubber component, etc. Also, a rubber composition for a tire that satisfies formula (Y) can be produced by adjusting the amount of silica contained in the filler or the total amount of the filler.
[0156] The conditions for the kneading are not particularly limited, and various conditions such as the input volume of the kneading device, the rotation speed of the rotor, the ram pressure, the kneading temperature, the kneading time, the type of kneading device, etc. can be appropriately selected depending on the purpose. Examples of the kneading device include a Banbury mixer, an intermix, a kneader, a roll, etc. that are usually used for kneading rubber compositions.
[0157] The conditions for the heat-in are not particularly limited, and various conditions such as the heat-in temperature, heat-in time, and heat-in device can be appropriately selected depending on the purpose. Examples of the heat-in device include a heat-in roll mill typically used for heat-in of rubber compositions.
[0158] The extrusion conditions are not particularly limited, and various conditions such as extrusion time, extrusion speed, extrusion device, and extrusion temperature can be appropriately selected depending on the purpose. Examples of the extrusion device include an extruder typically used for extruding rubber compositions. The extrusion temperature can be appropriately determined.
[0159] The vulcanization apparatus, method, conditions, etc. are not particularly limited and can be appropriately selected depending on the purpose. Examples of apparatuses for vulcanization include molding vulcanizers using molds used for vulcanizing rubber compositions. The vulcanization temperature is, for example, about 100 to 190°C.
[0160] <Tread Rubber> The tread rubber of the present invention is characterized by using the above-mentioned rubber composition for tires. Because the tread rubber of the present invention uses the above-mentioned rubber composition for tires, by applying it to a tire, the tire can have an excellent balance of fuel economy performance, wet braking performance, and wear resistance. The tread rubber of the present invention may be applied to a new tire or a retread tire.
[0161] <Tire> The tire of the present invention is characterized by including the tread rubber described above. Because the tire of the present invention includes the tread rubber described above, it has an excellent balance of fuel economy performance, wet braking performance, and wear resistance.
[0162] <Method for manufacturing tread rubber and tire> Depending on the type of tire to be applied, the tire of the present invention may be obtained by molding an unvulcanized rubber composition and then vulcanizing it, or by molding a semi-vulcanized rubber that has been subjected to a pre-vulcanization step or the like and then further vulcanizing it. The tire of the present invention is preferably a pneumatic tire, and the gas to be filled into the pneumatic tire may be normal air or air with an adjusted oxygen partial pressure, or an inert gas such as nitrogen, argon, or helium.
[0163] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0164] <Analysis Method of Rubber Component> The rubber component was analyzed by the following method.
[0165] (1) Bound Styrene Amount The synthesized styrene-butadiene rubber was used as a sample, and 100 mg of the sample was diluted with chloroform to 100 mL and dissolved to prepare a measurement sample. The amount of bound styrene (mass%) relative to 100 mass% of the sample was measured based on the amount of absorption at the ultraviolet absorption wavelength (near 254 nm) by the phenyl group of styrene. A spectrophotometer "UV-2450" manufactured by Shimadzu Corporation was used as the measurement device.
[0166] (2) Glass Transition Temperature (Tg) Using the synthesized styrene-butadiene rubber as a sample, a DSC curve was recorded using a DSC250 manufactured by TA Instruments, while increasing the temperature from −100° C. at a rate of 20° C. / min under a helium flow of 50 mL / min, and the peak top (inflection point) of the DSC differential curve was determined as the glass transition temperature.
[0167] (3) SP Value (Solubility Parameter) The SP values (solubility parameters) of natural rubber (isoprene skeleton rubber) and styrene-butadiene rubber were calculated according to the Fedors method.
[0168] <Method of Analyzing Resin Components> The resin components were analyzed by the following method.
[0169] (4) Softening Point The softening point of the resin component was measured in accordance with JIS-K2207-1996 (ring and ball method).
[0170] (5) Weight-average molecular weight The average molecular weight of the resin component was measured by gel permeation chromatography (GPC) under the following conditions, and the weight-average molecular weight in terms of polystyrene was calculated: Column temperature: 40°C Injection volume: 50 μL Carrier and flow rate: tetrahydrofuran 0.6 mL / min Sample preparation: Approximately 2.5 mg of the resin component was dissolved in 10 mL of tetrahydrofuran.
[0171] (6) SP Value (Solubility Parameter) The SP value (solubility parameter) of the resin component was calculated according to the Fedors method.
[0172] <Preparation of Rubber Composition> Rubber compositions of Examples and Comparative Examples were prepared by blending and kneading each component according to the formulations shown in Tables 1 and 2. In Tables 1 and 2, the amount of each component is the amount (parts by mass) relative to 100 parts by mass of the rubber component.
[0173]
[0174] *1 Natural rubber: TSR #20, SP value = 8.20 (cal / cm 3 ) 1/2 *2 SBR1: Hydrocarbyloxysilane compound modified styrene-butadiene rubber synthesized by the following method, Tg = -65°C, SP value = 8.65 (cal / cm 3 ) 1/2 *3 SBR2: Modified styrene-butadiene rubber obtained by modifying the terminals of styrene-butadiene rubber obtained using butyllithium as an initiator with N-(1,3-dimethylbutylidene)-3-triethoxysilyl-1-propanamine, Tg = -38°C, SP value = 8.95 (cal / cm 3 ) 1/2 , bound styrene content = 35% by mass * 4 BR: Manufactured by UBE Elastomers Co., Ltd., trade name "BR150" * 5 Carbon black: Manufactured by Asahi Carbon Co., Ltd., trade name "Asahi #70" * 6 Silica: Manufactured by Tosoh Silica Corporation, trade name "Nipsil AQ" * 7 Silane coupling agent: Manufactured by Evonik, trade name "Si75" * 8 Resin component: Hydrogenated C 5 Resin, manufactured by Eastman Co., Ltd., trade name "Impera P1780", softening point = 130°C, weight average molecular weight (Mw) = 909 g / mol, SP value = 8.35 (cal / cm 3 ) 1/2 * 9 Anti-aging agent: Manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Nocrac 6C" * 10 Wax: Manufactured by Nippon Seiro Co., Ltd., trade name "Ozoace 0701" * 11 Vulcanization accelerator A: Manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Nocceler DM-P" * 12 Vulcanization accelerator B: Manufactured by Sanshin Chemical Industry Co., Ltd., trade name "Suncerer NS-G"
[0175] (Method for synthesizing SBR1 (*2)) A cyclohexane solution of 1,3-butadiene and a cyclohexane solution of styrene were added to a dried, nitrogen-purged 800 mL pressure-resistant glass vessel so that the total amount of 1,3-butadiene and styrene were 67.5 g and 7.5 g, respectively, and 0.6 mmol of 2,2-ditetrahydrofurylpropane and 0.8 mmol of n-butyllithium were added, followed by polymerization at 50°C for 1.5 hours. To the polymerization reaction system, which had reached a polymerization conversion rate of nearly 100%, 0.72 mmol of N,N-bis(trimethylsilyl)-3-[diethoxy(methyl)silyl]propylamine was added as a modifier, and a modification reaction was carried out at 50°C for 30 minutes. Thereafter, 2 mL of a 5 mass % solution of 2,6-di-t-butyl-p-cresol (BHT) in isopropanol was added to terminate the reaction, and the mixture was dried in a conventional manner to obtain a modified SBR. Measurement of the microstructure of the resulting modified SBR revealed that the bound styrene content was 10% by mass and the glass transition temperature (Tg) was -65°C.
[0176] <Preparation and Evaluation of Vulcanized Rubber> The rubber compositions of the examples and comparative examples were vulcanized to obtain vulcanized rubber test pieces. The vulcanized rubber test pieces were evaluated for fuel economy, wet braking performance, and abrasion resistance by the following methods.
[0177] (1) Fuel Economy Performance The loss tangent (tan δ) of the test specimen was measured using a viscoelasticity measuring device (manufactured by Rheometrics) under conditions of a temperature of 50°C, a strain of 1%, and a frequency of 52 Hz. The test results were expressed as an index, with the reciprocal of tan δ of Comparative Example 1 set to 100. A larger index value indicates a smaller tan δ and better fuel economy.
[0178] (2) Wet braking performance The coefficient of friction of the test specimen against a wet asphalt road surface was measured using a portable friction tester. The test results were expressed as an index, with the coefficient of friction of Comparative Example 1 being 100. A larger index value indicates a larger coefficient of friction and better wet braking performance.
[0179] (3) Abrasion Resistance Performance According to JIS K 6264-2:2005, sandpaper was attached to the grinding wheel using a Lambourn abrasion tester manufactured by Ueshima Seisakusho Co., Ltd., and the amount of abrasion was measured at room temperature with a slip rate of 15%. The test results were expressed as an index, with the reciprocal of the amount of abrasion of Comparative Example 1 set to 100. A larger index value indicates a smaller amount of abrasion and better abrasion resistance.
[0180]
[0181] From Table 1, it can be seen that the rubber compositions for tires of Examples 1 to 4, which satisfy both formula (X) (and formula (Z)) and formula (Y), have an excellent balance of fuel economy performance, wet braking performance, and wear resistance. On the other hand, the rubber compositions for tires of Comparative Examples 1 and 2 satisfy formula (X) (and formula (Z)), but do not satisfy formula (Y), and therefore are inferior in fuel economy performance or wet braking performance. Furthermore, it can be seen that the rubber compositions for tires of Comparative Examples 3 to 6 satisfy formula (Y), but do not satisfy formula (X) (and formula (Z)), and therefore are inferior in either fuel economy performance, wet braking performance, or wear resistance.
[0182] The rubber composition for tires of the present invention can be used mainly in the tire manufacturing industry.
Claims
1. A rubber composition for tires, comprising a rubber component and a filler, wherein the rubber component comprises at least an isoprene skeleton rubber and a styrene-butadiene rubber, the filler comprises at least silica, and the filler satisfies the following formula (X): 10≦A 0.5 +B 1.5 A rubber composition for tires which satisfies: ≦100 (X), (wherein A is the amount (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the bound styrene amount (% by mass) of the styrene-butadiene rubber), and the following formula (Y): 0.55≦C / D≦0.75 (Y), (wherein C is the amount (parts by mass) of the silica relative to 100 parts by mass of the rubber component, and D is the amount (parts by mass) of the filler relative to 100 parts by mass of the rubber component).
2. The rubber composition for tires according to claim 1, further comprising a resin component.
3. The rubber composition for tires according to claim 1, wherein the styrene-butadiene rubber is modified with a modifier containing nitrogen and silicon.
4. The rubber composition for tires according to claim 1, wherein the styrene-butadiene rubber is modified with a modifier having a nitrogen-containing functional group and an alkoxy group.
5. The rubber composition for tires according to claim 1, wherein the content of the isoprene skeleton rubber is more than 0 part by mass and less than 70 parts by mass per 100 parts by mass of the rubber component.
6. The following formula (Z): 10≦A 0.5 +B 1.5 2. The rubber composition for tires according to claim 1, which satisfies the following formula: ≦85 (Z), wherein A is the content (parts by mass) of the isoprene skeleton rubber in 100 parts by mass of the rubber component, and B is the bound styrene amount (% by mass) of the styrene-butadiene rubber.
7. The rubber composition for tires according to claim 1, wherein the rubber component does not contain butadiene rubber.
8. The rubber composition for tires according to claim 1, wherein the amount of sulfur in the rubber composition is 2.5 parts by mass or less per 100 parts by mass of the rubber component.
9. The rubber composition for tires according to claim 1, wherein the styrene-butadiene rubber has a bound styrene content of less than 15 mass %.
10. A tread rubber using the rubber composition according to claim 1.
11. A tire comprising a tread rubber according to claim 10.
Citation Information
Patent Citations
Rubber composition and tire using the same
JP2007217562A
Method for producing precipitated silica
JP2019038728A
Conjugated diene polymer, process for its production and rubber compositions containing the same
WO2003046020A1
Rubber composition and tire
WO2015079703A1
Pneumatic tire
JP1991252433A