Film-like adhesive for semiconductor, method for producing film-like adhesive for semiconductor, adhesive tape, method for producing semiconductor device, and semiconductor device
The film adhesive with distinct adhesive regions addresses the issue of oxidation and impurities in semiconductor connections by using specific epoxy resins and imidazole curing agents, enhancing sealing and reliability while reducing fillet formation and voids.
Patent Information
- Application Number
- PCT/JP2024/007416
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-24
- Filing Date
- 2024-02-28
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional methods for connecting semiconductor chips and substrates, such as wire bonding and flip chips, face challenges with oxidation and impurities leading to reduced connection reliability, and existing solutions like OSP treatment compromise solder wettability.
A film adhesive with distinct regions, one without a flux compound and the other with a flux compound, utilizing specific epoxy resins, imidazole curing agents, and (meth)acrylic compounds, is used to ensure adequate sealing and reduce fillet formation while maintaining connection reliability.
The film adhesive effectively suppresses fillet formation and ensures sufficient sealing performance, improving connection reliability and preventing voids and excessive adhesive flow during the connection process.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Film-like adhesive for semiconductors, method for producing film-like adhesive for semiconductors, adhesive tape, method for producing semiconductor device, and semiconductor device
[0001] The present disclosure relates to a film-like adhesive for semiconductors, a method for manufacturing a film-like adhesive for semiconductors, an adhesive tape, a method for manufacturing a semiconductor device, and a semiconductor device.
[0002] Conventionally, wire bonding, which uses thin metal wires such as gold wires, has been widely used to connect semiconductor chips to substrates. However, in order to meet demands for higher performance, higher integration, and faster speeds in semiconductor devices, flip-chip connection (FC) technology, in which conductive protrusions called bumps are formed on the semiconductor chip or substrate to directly connect the semiconductor chip to the substrate, is becoming more widespread.
[0003] For example, the COB (Chip On Board) type connection method, which is widely used for connecting semiconductor chips and substrates in BGA (Ball Grid Array), CSP (Chip Size Package), etc., also falls under the category of FC connection. The FC connection method is also widely used in COC (Chip On Chip) type connection methods, which form connection parts (e.g., bumps and wiring) on semiconductor chips to connect semiconductor chips.
[0004] Furthermore, in packages where further miniaturization, thinning, and high functionality are strongly required, chip-stacked packages, POP (Package On Package), TSV (Through-Silicon Via), and the like, which use the above-mentioned connection methods to stack chips and create multiple layers, are beginning to become widely used. These stacking and multi-layering technologies arrange connecting members such as semiconductor chips three-dimensionally, allowing for smaller packages compared to methods that arrange the connecting members two-dimensionally. Furthermore, because they are effective in improving semiconductor performance, reducing noise, reducing mounting area, and saving power, they are attracting attention as a next-generation semiconductor wiring technology.
[0005] Generally, metal bonding is used to connect connecting parts to each other in order to ensure sufficient connection reliability (e.g., insulation reliability). Main metals used for the above-mentioned connecting parts (e.g., bumps and wiring) include solder, tin, gold, silver, copper, nickel, etc., and conductive materials containing a combination of these metals are also used. The metals used for the connecting parts may oxidize on their surfaces to form oxide films, or impurities such as oxides may adhere to the surfaces, resulting in impurities on the connecting surfaces of the connecting parts. If such impurities remain, there is a concern that the connection reliability (e.g., insulation reliability) between a semiconductor chip and a substrate or between two semiconductor chips may be reduced, thereby undermining the benefits of adopting the above-mentioned connection method.
[0006] In addition, one method for suppressing the generation of these impurities is to coat the connection parts with an anti-oxidation film, which is known as an OSP (Organic Solderability Preservatives) treatment, but this anti-oxidation film can sometimes cause a decrease in solder wettability and connectivity during the connection process.
[0007] Therefore, as methods for removing the above-mentioned oxide film and impurities, a method using a single-layer film containing a fluxing agent in a semiconductor material (see, for example, Patent Document 1), a method using a two-layer film consisting of a thermosetting resin layer and a thermoplastic resin layer containing an acid component, and the like have been proposed (see, for example, Patent Document 2).
[0008] International Publication No. 2013 / 125086 International Publication No. 2016 / 117350
[0009] An object of one aspect of the present disclosure is to provide a film-like adhesive for semiconductors that can reduce the amount of fillet formation while ensuring sufficient sealing properties.
[0010] The present disclosure provides the following [1] to
[15] .
[0011] [1] A film-like adhesive for semiconductors, having, along the thickness direction, a first adhesive region that does not contain a flux compound and a second adhesive region that contains a flux compound, wherein the first adhesive region contains a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound, and the second adhesive region contains a second epoxy resin, a second imidazole-based curing agent, and the flux compound.
[0012] [2] The film-like adhesive for semiconductors according to [1], wherein the first adhesive region does not contain a radical polymerization initiator.
[0013] [3] The film-like adhesive for semiconductors according to [1] or [2], wherein at least one of the first epoxy resin and the second epoxy resin contains an epoxy resin that is liquid at 25°C.
[0014] [4] The film-like adhesive for semiconductors according to any one of [1] to [3], wherein at least one of the first epoxy resin and the second epoxy resin contains a triphenolmethane type epoxy resin.
[0015] [5] The film-like adhesive for semiconductors according to any one of [1] to [4], wherein at least one of the first imidazole-based curing agent and the second imidazole-based curing agent has a triazine ring.
[0016] [6] A film-like adhesive for semiconductors according to any one of [1] to [5], wherein the ratio of the content of the first epoxy resin to the content of the (meth)acrylic compound in the first adhesive region is 3 to 11 in mass ratio.
[0017] [7] The film-like adhesive for semiconductors according to any one of [1] to [6], wherein the (meth)acrylic compound comprises a polyfunctional (meth)acrylic compound having 2 to 8 (meth)acryloyl groups.
[0018] [8] The film-like adhesive for semiconductors according to any one of [1] to [7], wherein the flux compound contains a polycarboxylic acid.
[0019] [9] A film-like adhesive for semiconductors according to any one of [1] to [8], wherein the thickness of the first adhesive region is 1 to 50 μm, and the thickness of the second adhesive region is 0.5 to 2 times the thickness of the first adhesive region.
[0020]
[10] The film-like adhesive for semiconductors according to any one of [1] to [9], which is non-conductive.
[0021]
[11] A film-like adhesive for semiconductors according to any one of [1] to
[10] , which is used to bond a semiconductor chip and a base and to seal the gap between the semiconductor chip and the base.
[0022]
[12] A method for producing a film-like adhesive for semiconductors according to any one of [1] to
[11] , comprising a step of providing one of a first adhesive layer and a second adhesive layer on top of the other, wherein the first adhesive layer does not contain a flux compound and is a layer containing the first epoxy resin, the first imidazole curing agent, and the (meth)acrylic compound, and the second adhesive layer is a layer containing the second epoxy resin, the second imidazole curing agent, and the flux compound.
[0023]
[13] An adhesive tape comprising: a film-like adhesive for a semiconductor according to any one of [1] to
[11] ; and a backgrind tape provided on the film-like adhesive for a semiconductor, on the opposite side of the first adhesive region from the second adhesive region.
[0024]
[14] A method for manufacturing a semiconductor device, comprising: a step of preparing a semiconductor chip with a film adhesive, the semiconductor chip comprising: a semiconductor chip; and a film adhesive for semiconductors according to any one of [1] to
[11] , which is provided on the semiconductor chip so that the surface of the first adhesive region opposite the second adhesive region faces the semiconductor chip; and a step of placing the semiconductor chip with the film adhesive on a base from the film adhesive side and heating the semiconductor chip with the film adhesive, thereby electrically connecting the connection portions of the semiconductor chip and the connection portions of the base and sealing the gap between the semiconductor chip and the base.
[0025]
[15] A semiconductor device comprising: a semiconductor chip having a first connection portion; a base having a second connection portion electrically connected to the first connection portion; and a sealing portion that joins the semiconductor chip and the base and fills a gap between the semiconductor chip and the base, wherein the sealing portion is a cured product of the film-like adhesive for semiconductors described in any one of [1] to
[11] .
[0026] According to the present disclosure, it is possible to provide a film-like adhesive for semiconductors that can reduce the amount of fillet formation while ensuring sufficient sealing properties.
[0027] FIG. 1 is a schematic cross-sectional view showing one embodiment of a film-like adhesive for semiconductors according to the present disclosure. FIG. 2(a) is a schematic cross-sectional view showing one embodiment of a semiconductor device according to the present disclosure, and FIG. 2(b) is a schematic cross-sectional view showing another embodiment of a semiconductor device according to the present disclosure. FIG. 3 is a schematic cross-sectional view showing another embodiment of a semiconductor device according to the present disclosure. FIG. 4 is a process cross-sectional view schematically showing one embodiment of a method for manufacturing a semiconductor device according to the present disclosure. FIG. 5 is a process cross-sectional view schematically showing a process following FIG. 4. FIG. 6 is a process cross-sectional view schematically showing a process following FIG. 5. FIG. 7 is a process cross-sectional view schematically showing a process following FIG. 6. FIG. 8 is a process cross-sectional view schematically showing a process following FIG. 7.
[0028] In this specification, "(meth)acrylic" refers to at least one of acrylic and its corresponding methacrylic. The same applies to other similar expressions such as "(meth)acryloyl" and "(meth)acrylate." Furthermore, a numerical range indicated using "to" indicates a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. Furthermore, unless specifically stated otherwise, the units of the numerical values before and after "to" are the same. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range may be replaced with the value shown in the examples. Furthermore, the individually described upper and lower limits can be arbitrarily combined. Furthermore, unless otherwise specified, the materials exemplified below may be used alone or in combination of two or more. When multiple substances corresponding to each component are present in the composition, the content of each component in the composition refers to the total amount of the multiple substances present in the composition, unless otherwise specified.
[0029] Hereinafter, embodiments of the present disclosure will be described in detail, with reference to the drawings where appropriate. In the drawings, identical or corresponding parts are designated by the same reference numerals, and duplicate explanations will be omitted. Furthermore, unless otherwise specified, positional relationships such as up, down, left, and right are based on the positional relationships shown in the drawings. Furthermore, the dimensional ratios of the drawings are not limited to those shown in the drawings.
[0030] <Film-like adhesive for semiconductors> One embodiment of the film-like adhesive for semiconductors (hereinafter simply referred to as "film-like adhesive") is an adhesive used for connecting (joining) and sealing connecting members such as semiconductor chips, and can be used to join a semiconductor chip to a base and to seal gaps between the semiconductor chip and the base.
[0031] FIG. 1 is a schematic cross-sectional view showing a film-like adhesive according to one embodiment. The film-like adhesive 1 shown in the figure has, along the thickness direction (the vertical direction in FIG. 1 ), a first adhesive region 2 that does not contain a flux compound and a second adhesive region 3 that contains a flux compound. The first adhesive region 2 contains an epoxy resin, an imidazole-based curing agent, and a (meth)acrylic compound, while the second adhesive region contains an epoxy resin, an imidazole-based curing agent, and the flux compound. Hereinafter, the adhesive constituting the first adhesive region 2 will be referred to as the "first adhesive," and the adhesive constituting the second adhesive region 3 will be referred to as the "second adhesive." The epoxy resin and imidazole-based curing agent contained in the first adhesive will be referred to as the "first epoxy resin" and the "first imidazole-based curing agent," respectively, and the epoxy resin and imidazole-based curing agent contained in the second adhesive will be referred to as the "second epoxy resin" and the "second imidazole-based curing agent," respectively.
[0032] The first adhesive region 2 and the second adhesive region 3 have a predetermined thickness and extend, for example, along the main surface direction of the film-like adhesive 1 (the left-right direction in FIG. 1 ) as shown in FIG. 1 . The first adhesive region 2 and the second adhesive region 3 may be layered. That is, the first adhesive region 2 and the second adhesive region 3 may be a first adhesive layer and a second adhesive layer, respectively. The boundary between the first adhesive region 2 and the second adhesive region 3 is not necessarily clear and may not be visible. Note that in FIG. 1 , the first adhesive region 2 and the second adhesive region 3 are adjacent to each other, but a region different from the first adhesive region 2 and the second adhesive region 3 (for example, a region containing a mixture of the first adhesive and the second adhesive) may exist between the first adhesive region 2 and the second adhesive region 3.
[0033] Recently, with the increasing sophistication and integration of packages, the gaps between layers and the pitch between wiring lines have become narrower. This has led to the tendency for adhesives that flow during connection to overflow from the edges of connecting members (e.g., semiconductor chips), resulting in the formation of overflowing portions known as fillets. Because such fillets can cause damage to connecting members, there is a need to develop a method for reducing the amount of fillets while ensuring sufficient sealing. Simply using a low-fluidity adhesive to suppress fillets can result in insufficient filling of the gaps between connecting members, leading to defects such as voids. Therefore, simply reducing the fluidity of the adhesive is not enough to solve the above problem.
[0034]
[0013] Meanwhile, as a result of investigations by the inventors of the present disclosure, it has become clear that the above-mentioned film-like adhesive can ensure sufficient sealing properties while suppressing the occurrence of voids and fillets due to excessive flow of the adhesive when connecting connecting members. While the reason for this effect is unclear, it is presumed that the first adhesive region 2 and the second adhesive region 3 have the above-mentioned specific compositions, so that the first adhesive region 2 has an appropriate fluidity that makes it difficult to create unfilled areas that cause voids when attached, and hardens faster than the second adhesive region 3 when connected, making it difficult to create excessive flow that causes fillets; and the second adhesive region 3 is more fluid than the first adhesive region 2 and is therefore difficult to create unsealed areas.
[0035] The thickness of the first adhesive region 2 (the length in the thickness direction of the film-like adhesive 1) may be set appropriately in relation to the height of the connection portion in the connecting member to which the film-like adhesive 1 is attached. If the height of the connection portion is y1 and the thickness of the first adhesive region 2 is x1, then x1<y1 or 1.0x1<y1≦1.5x1 may be satisfied, from the viewpoint of making it difficult for the cured product of the first adhesive to intervene between the connection portions and further improving connection reliability. Specifically, the thickness of the first adhesive region 2 may be 1 to 50 μm, 3 to 50 μm, 4 to 30 μm, or 5 to 20 μm.
[0036] The thickness of the second adhesive region 3 may be 0.5 to 2 times, 0.5 to 2.5 times, or 0.5 to 3 times the thickness of the first adhesive region 2. Specifically, the thickness of the second adhesive region 3 (the length in the thickness direction of the film-like adhesive 1) may be 1 to 50 μm, 3 to 50 μm, 4 to 30 μm, or 5 to 20 μm.
[0037] The thickness of the film-like adhesive 1 (e.g., the sum of the thickness of the first adhesive region 2 and the thickness of the second adhesive region 3) may be appropriately set in relation to the connection portions of the connecting member. If the sum of the heights of the connection portions is x and the total thickness of the film-like adhesive is y, then from the viewpoints of connectivity during pressure bonding and adhesive filling, 0.70x≦y≦1.3x or 0.80x≦y≦1.2x may be satisfied. From the viewpoint of making it difficult for the cured product of the first adhesive to intervene between the connection portions and further improving connection reliability, y>x may be satisfied. Specifically, the thickness of the film-like adhesive 1 may be 2 to 100 μm, 6 to 100 μm, 8 to 60 μm, or 10 to 40 μm.
[0038] The first adhesive constituting the first adhesive region 2 and the second adhesive constituting the second adhesive region 3 will be described below.
[0039] (First adhesive) The first adhesive contains a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound, but does not contain a flux compound. Here, "the first adhesive does not contain a flux compound" means that the content of the flux compound in the first adhesive is below the current detection limit (for example, 0.01 mass % or less based on the total amount of the first adhesive).
[0040] [First Epoxy Resin] The first epoxy resin is a compound having two or more epoxy groups in the molecule. Examples of the first epoxy resin include bisphenol A epoxy resins, bisphenol F epoxy resins, naphthalene epoxy resins, phenol novolac epoxy resins, cresol novolac epoxy resins, phenol aralkyl epoxy resins, biphenyl epoxy resins, triphenylmethane epoxy resins, triphenolmethane epoxy resins, dicyclopentadiene epoxy resins, and various polyfunctional epoxy resins. These can be used alone or as a mixture of two or more. Among these, triphenolmethane epoxy resins (epoxy resins containing a triphenolmethane skeleton) tend to further reduce the amount of fillet formation.
[0041] The first epoxy resin may be an epoxy resin having a thermal weight loss rate of 5% or less at the temperature at which the epoxy resin is connected, in order to prevent decomposition and generation of volatile components during connection at high temperatures. For example, if the temperature at which the epoxy resin is connected is 250°C, an epoxy resin having a thermal weight loss rate of 5% or less at 250°C may be used. Furthermore, if the temperature at which the epoxy resin is connected is 300°C, an epoxy resin having a thermal weight loss rate of 5% or less at 300°C may be used.
[0042] As the first epoxy resin, an epoxy resin that is liquid at 25°C (hereinafter simply referred to as "liquid epoxy resin") may be used from the viewpoint of easily suppressing the occurrence of cracks and fissures on the film surface. Here, "liquid at 25°C" means that the viscosity at 25°C measured with an E-type viscometer is 400 Pa s or less. Examples of liquid epoxy resins include glycidyl ethers of bisphenol A, glycidyl ethers of bisphenol AD, glycidyl ethers of bisphenol S, glycidyl ethers of bisphenol F, glycidyl ethers of hydrated bisphenol A, glycidyl ethers of ethylene oxide adducts of bisphenol A, glycidyl ethers of propylene oxide adducts of bisphenol A, glycidyl ethers of naphthalene resins, and trifunctional or tetrafunctional glycidyl amines.
[0043] The content of the liquid epoxy resin in the first adhesive may be 5% by mass or more, 10% by mass or more, or 20% by mass or more, based on the total amount of the first epoxy resin contained in the first adhesive, from the viewpoint of easily suppressing the occurrence of cracks and fissures on the film surface. The content of the liquid epoxy resin may be 30% by mass or less, 20% by mass or less, or 10% by mass or less, based on the total amount of the first epoxy resin, from the viewpoint of easily suppressing an excessive increase in tackiness of the film and easily suppressing edge fusion.
[0044] The epoxy equivalent of the first epoxy resin may be 100 to 3000 g / eq, 100 to 2000 g / eq, or 100 to 1500 g / eq. When the epoxy equivalent of the first epoxy resin is within the above range, a good balance between reactivity and fluidity during heating tends to be achieved.
[0045] The content of the first epoxy resin in the first adhesive may be 25% by mass or more, 30% by mass or more, or 35% by mass or more, based on the total amount of the first adhesive, from the viewpoint of easily suppressing the occurrence of fillets. The content of the first epoxy resin may be 50% by mass or less, 45% by mass or less, or 40% by mass or less, based on the total amount of the first adhesive, from the viewpoint of easily obtaining good sealing properties and easily suppressing the occurrence of voids.
[0046] The content of the first epoxy resin in the first adhesive may be set in relation to the content of the (meth)acrylic compound. When the ratio of the content of the first epoxy resin to the content of the (meth)acrylic compound in the first adhesive is 3 to 11 by mass, high connection reliability tends to be obtained and the amount of fillet generation tends to be further reduced. The ratio may be 5 or more, 7 or more, or 9 or more from the viewpoint of further reducing the amount of fillet generation, and may be 10 or less from the viewpoint of easily obtaining good sealing properties and easily suppressing the generation of voids in addition to the above effect.
[0047] [First Imidazole-Based Curing Agent] Examples of the imidazole-based curing agent include 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyano-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6 Examples of the curing agent include 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct, 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and adducts of epoxy resin and imidazoles. Microencapsulated latent curing agents containing these compounds can also be used. These compounds can be used alone or in combination of two or more. Among these, compounds having a triazine ring may be used from the viewpoint of obtaining better sealing properties and suppressing the occurrence of voids.
[0048] The content of the first imidazole curing agent in the first adhesive may be 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more relative to 100 parts by mass of the first epoxy resin contained in the first adhesive, from the viewpoint of improving curing properties when heated. The content of the first imidazole curing agent may be 10 parts by mass or less, 7 parts by mass or less, or 5 parts by mass or less relative to 100 parts by mass of the first epoxy resin, from the viewpoint of making it more unlikely that the first adhesive will intervene between connected portions.
[0049] [(Meth)acrylic Compound] A (meth)acrylic compound is a compound having one or more (meth)acryloyl groups in the molecule. Examples of (meth)acrylic compounds include (meth)acrylic compounds containing a bisphenol A, bisphenol F, naphthalene, phenol novolac, cresol novolac, phenol aralkyl, biphenyl, triphenylmethane, dicyclopentadiene, fluorene, adamantane, or isocyanuric acid skeleton; and various polyfunctional (meth)acrylic compounds (excluding (meth)acrylic compounds containing the above skeleton). Examples of polyfunctional (meth)acrylic compounds include pentaerythritol tri(meth)acrylate, dipentaerythritol poly(meth)acrylate (dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, etc.), and trimethylolpropane di(meth)acrylate. Among these, when a polyfunctional (meth)acrylic compound is used, the effects of the present invention tend to be more improved, and when dipentaerythritol poly(meth)acrylate is used, the effects of the present invention tend to be even more improved. The number of functional groups (the number of (meth)acryloyl groups) of the polyfunctional (meth)acrylic compound may be 2 to 8, or may be 3 to 7, or may be 4 to 6.
[0050] The molecular weight of the (meth)acrylic compound is, for example, 400 to 2000. The molecular weight of the (meth)acrylic compound may be less than 2000, or may be 1000 or less. The smaller the molecular weight of the (meth)acrylic compound, the more easily the reaction proceeds, and the higher the curing reaction rate.
[0051] The (meth)acrylic compounds can be used alone or in combination of two or more.
[0052] The content of the (meth)acrylic compound in the first adhesive may be 1% by mass or more, 3% by mass or more, or 5% by mass or more, based on the total amount of the first adhesive, from the viewpoint of further reducing the occurrence of fillets. The content of the (meth)acrylic compound may be 10% by mass or less, 7% by mass or less, or 5% by mass or less, based on the total amount of the first adhesive, from the viewpoint of improving sealing performance and suppressing the occurrence of voids. From these viewpoints, the content of the (meth)acrylic compound may be 1 to 10% by mass, 3 to 7% by mass, or 3 to 5% by mass, based on the total amount of the first adhesive.
[0053] [Other Components] The first adhesive may further contain components (other components) other than those described above.
[0054] For example, the first adhesive may contain a thermosetting resin other than an epoxy resin (a compound that hardens by reacting with a thermosetting agent due to heat). Examples of thermosetting resins other than an epoxy resin include phenolic resin and acrylic resin. When the first adhesive contains a thermosetting resin other than an epoxy resin, the content of the first epoxy resin in the first adhesive may be 80% by mass or more, 90% by mass or more, or even 100% by mass, based on the total amount of the thermosetting resin contained in the first adhesive.
[0055] Furthermore, for example, the first adhesive may contain a heat curing agent other than an imidazole-based curing agent. Examples of heat curing agents other than an imidazole-based curing agent include a phenolic resin-based curing agent, an acid anhydride-based curing agent, an amine-based curing agent, and a phosphine-based curing agent. When the first adhesive contains a heat curing agent other than an imidazole-based curing agent, the content of the first imidazole-based curing agent in the first adhesive may be 80 mass% or more, 90 mass% or more, or even 100 mass% based on the total amount of the heat curing agent contained in the first adhesive, from the viewpoints of allowing rapid curing when heated at low temperatures and improving connection reliability through flux activity that suppresses the formation of an oxide film at the connection portion.
[0056] Furthermore, for example, the first adhesive may contain a radically polymerizable compound other than a (meth)acrylic compound (a compound capable of undergoing a radical polymerization reaction in association with the generation of radicals due to heat, light, radiation, electrochemical action, etc.). Examples of radically polymerizable compounds other than a (meth)acrylic compound include vinyl compounds. When the first adhesive contains a radically polymerizable compound other than a (meth)acrylic compound, the content of the (meth)acrylic compound in the first adhesive may be 80% by mass or more, 90% by mass or more, or even 100% by mass, based on the total amount of radically polymerizable compounds contained in the first adhesive.
[0057] Furthermore, for example, the first adhesive may contain a thermoplastic resin. The thermoplastic resin contributes to improving heat resistance and film formability. Examples of thermoplastic resins include phenoxy resin, polyimide resin, polyamide resin, polycarbodiimide resin, cyanate ester resin, acrylic resin, polyester resin, polyethylene resin, polyethersulfone resin, polyetherimide resin, polyvinyl acetal resin, urethane resin, and acrylic rubber. Among these, from the viewpoint of easily obtaining excellent heat resistance and film formability, any of phenoxy resin, polyimide resin, acrylic rubber, cyanate ester resin, and polycarbodiimide resin may be used. From the viewpoint of more easily obtaining excellent heat resistance and film formability, any of phenoxy resin, polyimide resin, and acrylic rubber may be used. These thermoplastic resins can be used alone or as a mixture or copolymer of two or more types.
[0058] The weight average molecular weight of the thermoplastic resin is, for example, 10,000 or more, and may be 20,000 or more, or 30,000 or more. Such a thermoplastic resin can further improve the heat resistance and film formability of the first adhesive. The weight average molecular weight of the thermoplastic resin may be 1,000,000 or less, or may be 500,000 or less, from the viewpoint of making it easier to obtain the effect of improving heat resistance. In this specification, the weight average molecular weight means the weight average molecular weight measured in polystyrene equivalent terms using high performance liquid chromatography (manufactured by Shimadzu Corporation, product name: C-R4A). For measurement, the following conditions can be used, for example. Detector: LV4000 UV Detector (Hitachi, Ltd., product name) Pump: L6000 Pump (Hitachi, Ltd., product name) Column: Gelpack GL-S300MDT-5 (total of 2 columns) (Hitachi Chemical Co., Ltd., product name) Eluent: THF / DMF = 1 / 1 (volume ratio) + LiBr (0.03 mol / L) + H3PO4 (0.06 mol / L) Flow rate: 1 mL / min
[0059] The glass transition temperature (Tg) of the thermoplastic resin may be 120° C. or lower, 100° C. or lower, or 85° C. or lower, from the viewpoint of excellent adhesion of the film-like adhesive 1 to a connecting member (e.g., a semiconductor chip). The Tg is the Tg measured using a DSC (manufactured by PerkinElmer, trade name: DSC-7 model) under the following conditions: a sample amount of 10 mg, a heating rate of 10° C. / min, and a measurement atmosphere of air.
[0060] The content of the thermoplastic resin in the first adhesive may be 5% by mass or more, 7% by mass or more, or 10% by mass or more, based on the total amount of the first adhesive, from the viewpoint of easily improving the heat resistance and film formability of the first adhesive. The content of the thermoplastic resin may be 30% by mass or less, 25% by mass or less, or 20% by mass or less, based on the total amount of the first adhesive, from the viewpoint of easily suppressing the occurrence of fillets.
[0061] Furthermore, for example, the first adhesive may contain a filler (filling agent). The filler is effective in controlling the viscosity of the first adhesive and the physical properties of the cured product of the first adhesive. Specifically, the use of a filler can suppress the generation of voids during connection and reduce the moisture absorption rate of the cured product of the first adhesive. The filler may be an inorganic filler (inorganic particles) or an organic filler (organic particles). Examples of inorganic fillers include insulating inorganic fillers such as glass, silica, alumina, titanium oxide, mica, and boron nitride. Among these, the above-mentioned effect is more easily achieved when at least one selected from the group consisting of silica, alumina, titanium oxide, and boron nitride is used, and the above-mentioned effect is even more easily achieved when at least one selected from the group consisting of silica, alumina, and boron nitride is used. Examples of organic fillers include resin fillers (resin particles). Examples of resin fillers include polyurethane and polyimide. Resin fillers can impart flexibility at high temperatures such as 260°C. It should be noted that organic fillers made of thermoplastic resins are not considered to be included in the above-mentioned thermoplastic resins.
[0062] From the viewpoint of achieving even better insulation reliability, the filler may be insulating. The first adhesive does not need to contain a filler containing a conductive material such as silver, solder, or carbon black (conductive filler).
[0063] The physical properties of the filler may be appropriately adjusted by surface treatment. The filler may be a filler that has been subjected to a surface treatment from the viewpoint of improving dispersibility or adhesive strength. Examples of the surface treatment agent include glycidyl-based (epoxy-based), amine-based, phenyl-based, phenylamino-based, (meth)acrylic-based, and vinyl-based compounds.
[0064] The average particle size of the filler is, for example, 0.5 to 1.5 μm. The average particle size of the filler may be 1.5 μm or less from the viewpoint of preventing jamming during flip-chip connection, and may be 1.0 μm or less from the viewpoint of excellent visibility (transparency). The average particle size of the filler is the particle size at the point corresponding to 50% volume when a cumulative frequency distribution curve of particle sizes is calculated assuming the total volume of the particles to be 100%, and can be measured using a particle size distribution measuring device using a laser diffraction scattering method, for example.
[0065] The content of the filler in the first adhesive may be 25% by mass or more, 30% by mass or more, or 35% by mass or more, based on the total amount of the first adhesive, from the viewpoint of suppressing a decrease in heat dissipation and of easily suppressing the occurrence of voids, an increase in moisture absorption rate, etc. The content of the filler may be 60% by mass or less, 55% by mass or less, or 50% by mass or less, based on the total amount of the first adhesive, from the viewpoint of suppressing the filler from getting caught (trapping) in the connection portion.
[0066] When the filler includes an inorganic filler and an organic filler, the content of the inorganic filler in the first adhesive may be 60% by mass or more, 70% by mass or more, or 80% by mass or more, and may be 98% by mass or less, 95% by mass or less, or 90% by mass or less, or may be 60 to 98% by mass, 70 to 95% by mass, or 80 to 90% by mass, based on the total amount of fillers included in the first adhesive.
[0067] Furthermore, for example, the first adhesive may contain a radical polymerization initiator. The radical polymerization initiator may be a photoradical polymerization initiator or a thermal radical polymerization initiator.
[0068] The photoradical polymerization initiator is, for example, a compound that decomposes upon irradiation with light having a wavelength in the range of 150 to 750 nm (for example, ultraviolet light) to generate free radicals, and examples thereof include known photopolymerization initiators having a structure such as an oxime ester structure, a bisimidazole structure, an acridine structure, an α-aminoalkylphenone structure, an aminobenzophenone structure, an N-phenylglycine structure, an acylphosphine oxide structure, a benzyl dimethyl ketal structure, an α-hydroxyalkylphenone structure, or an α-hydroxyacetophenone structure.
[0069] Examples of thermal radical polymerization initiators include 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl) peroxydicarbonate, di(2-ethylhexyl) peroxydicarbonate, cumyl peroxyneodecanoate, dilauroyl peroxide, 1-cyclohexyl-1-methylethyl peroxyneodecanoate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, and t-butyl peroxyneodecanoate. Pivalate, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy-2-ethylhexanoate, t-butylperoxy-2-ethylhexanoate, t-butylperoxyneoheptanoate, t-amylperoxy-2-ethylhexanoate, di-t-butylperoxyhexahydroterephthalate, t-amylperoxy-3,5, 5-trimethylhexanoate, 3-hydroxy-1,1-dimethylbutylperoxyneodecanoate, t-amylperoxyneodecanoate, di(3-methylbenzoyl) peroxide, dibenzoyl peroxide, di(4-methylbenzoyl) peroxide, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, 2, organic peroxides such as 5-dimethyl-2,5-di(3-methylbenzoylperoxy)hexane, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexyl peroxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butyl peroxybenzoate, dibutyl peroxytrimethyl adipate, t-amyl peroxy normal octoate, t-amyl peroxy isononanoate, and t-amyl peroxybenzoate;Examples of azo compounds include 2,2'-azobis-2,4-dimethylvaleronitrile, 1,1'-azobis(1-acetoxy-1-phenylethane), 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 4,4'-azobis(4-cyanovaleric acid), and 1,1'-azobis(1-cyclohexanecarbonitrile);
[0070] From the viewpoint of further enhancing the effects of suppressing fillets, reducing voids, and improving sealing properties, the content of the radical polymerization initiator in the first adhesive may be less than 0.1 parts by mass, or may be 0.01 parts by mass or less, relative to 100 parts by mass of the (meth)acrylic compound contained in the first adhesive. From the same viewpoint, the first adhesive may be free of a radical polymerization initiator. Here, "the first adhesive is free of a radical polymerization initiator" means that the content of the radical polymerization initiator in the first adhesive is below the current detection limit (for example, 0.01% by mass or less based on the total amount of the first adhesive).
[0071] The first adhesive may further contain additives such as an antioxidant, a silane coupling agent, a titanium coupling agent, a leveling agent, an ion trapping agent, etc. These may be used alone or in combination of two or more. The content of these additives may be appropriately adjusted so that the effects of each additive are exerted.
[0072] (Second Adhesive) The second adhesive contains a second epoxy resin, a second imidazole-based curing agent, and a flux compound.
[0073] [Second Epoxy Resin and Second Imidazole Curing Agent] The second epoxy resin and second imidazole curing agent can be the same as those exemplified as the first epoxy resin and first imidazole curing agent, and their preferred embodiments are also the same. The first epoxy resin and the second epoxy resin may be the same or different. The first imidazole curing agent and the second imidazole curing agent may be the same or different.
[0074] The content of the second epoxy resin in the second adhesive may be 25% by mass or more, 30% by mass or more, or 35% by mass or more, based on the total amount of the second adhesive, from the viewpoint of easily suppressing the occurrence of fillets. The content of the second epoxy resin may be 50% by mass or less, 45% by mass or less, or 40% by mass or less, based on the total amount of the second adhesive, from the viewpoint of easily obtaining good sealing properties and adhesive properties.
[0075] The content of the second imidazole curing agent in the second adhesive may be 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more relative to 100 parts by mass of the second epoxy resin contained in the second adhesive, from the viewpoint of improving curing properties when heated. The content of the second imidazole curing agent may be 10 parts by mass or less, 7 parts by mass or less, or 5 parts by mass or less relative to 100 parts by mass of the second epoxy resin contained in the second adhesive, from the viewpoint of making it more unlikely that the second adhesive will intervene between connected parts.
[0076] [Flux Compound] The flux compound is a compound having flux activity. As the flux compound, any known compound can be used without particular limitation as long as it reduces and removes an oxide film on the surface of solder or the like, facilitating metal bonding. The flux compound may be used alone or in combination of two or more.
[0077] The flux compound may be a compound having a carboxy group (carboxylic acid) or a polycarboxylic acid having two or more carboxy groups, from the viewpoint of obtaining sufficient flux activity and achieving better connection reliability. Polycarboxylic acids are less likely to volatilize at high temperatures during connection than compounds having one carboxy group (monocarboxylic acid), so the use of polycarboxylic acids can further suppress the occurrence of voids. Furthermore, among polycarboxylic acids, polycarboxylic acids having two carboxy groups are superior in suppressing the increase in viscosity of the film-like adhesive 1 during storage, connection work, etc., compared to polycarboxylic acids having three or more carboxy groups.
[0078] The flux compound having a carboxy group may be a compound having a group represented by the following formula (1):
[0079]
[0080] In formula (1), R 1 represents a hydrogen atom or an electron-donating group.
[0081] From the viewpoint of excellent reflow resistance and even more excellent connection reliability, R 1 In this embodiment, the second adhesive contains an epoxy resin and, in addition, a compound having a group represented by formula (1), R 1 is an electron donating group. In this case, it becomes easy to fabricate a semiconductor device that is more excellent in reflow resistance and connection reliability even in a flip-chip connection system.
[0082] Examples of the electron-donating group include an alkyl group, a hydroxyl group, an amino group, an alkoxy group, an alkylamino group, etc. The electron-donating group may be a group that is difficult to react with other components (e.g., epoxy resins), and specifically may be an alkyl group, a hydroxyl group, or an alkoxy group.
[0083] The alkyl group may be linear or branched. The alkyl group may be an alkyl group having 1 to 10 carbon atoms, or may be an alkyl group having 1 to 5 carbon atoms. The larger the number of carbon atoms in the alkyl group, the greater the electron donating property and steric hindrance tend to be. An alkyl group having a carbon number within the above range has an excellent balance between electron donating property and steric hindrance.
[0084] The flux compound having two carboxy groups may be a compound represented by the following formula (2): The compound represented by the following formula (2) can further improve the reflow resistance and connection reliability of the semiconductor device.
[0085]
[0086] In formula (2), R 1 has the same meaning as formula (1). 2 represents a hydrogen atom or an electron-donating group, and n represents 0 or an integer of 1 or more.
[0087] R 2 The electron donating property represented by R 1 The examples of the electron-donating group are the same as those described above. 2 is R 1 A plurality of R may be the same as or different from each other. 2 may be the same or different from each other.
[0088] In formula (2), n may be 1 or more. When n is 1 or more, the flux compound is less likely to volatilize even at high temperatures during connection, and the generation of voids can be further suppressed, compared to when n is 0. Furthermore, n in formula (2) may be 15 or less, or may be 11 or less, 6 or less, or 4 or less. When n is 15 or less, even better connection reliability can be obtained.
[0089] Specific examples of such flux compounds include dicarboxylic acids such as succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, undecanedioic acid, and dodecanedioic acid, as well as compounds in which an electron-donating group is substituted at the 2-position of these dicarboxylic acids (e.g., 2-methylglutaric acid). Among these, when 2-methylglutaric acid is used in combination with an epoxy resin and an imidazole-based curing agent, there is a tendency for effects such as suppression of fillets, reduction of voids, and improvement of sealing properties to be improved.
[0090] The melting point of the flux compound may be 150°C or lower, or may be 140°C or lower, or 130°C or lower. Such a flux compound is likely to fully exhibit flux activity before the curing reaction between the epoxy resin and the imidazole-based curing agent occurs. Therefore, by using such a flux compound, a semiconductor device with even more excellent connection reliability can be obtained. The flux compound may be solid at room temperature (25°C). The melting point of the flux compound may be 25°C or higher, or may be 50°C or higher. In this specification, a melting point of 150°C or lower means that the upper limit of the melting point is 150°C or lower, and a melting point of 25°C or higher means that the lower limit of the melting point is 25°C or higher.
[0091] The content of the flux compound in the second adhesive may be 0.1 mass % or more, 0.3 mass % or more, or 0.5 mass % or more, based on the total amount of the second adhesive, from the viewpoint of obtaining a better flux effect. The content of the flux compound may be 5 mass % or less, 3 mass % or less, or 2 mass % or less, based on the total amount of the second adhesive, from the viewpoint of reducing the amount of warpage of a wafer during fabrication of a semiconductor device.
[0092] [Other Components] The second adhesive may contain the components exemplified as other components that may be contained in the first adhesive. The thermoplastic resin in the first adhesive and the thermoplastic resin in the second adhesive may be the same or different. The same applies to other components such as fillers.
[0093] The content of the thermoplastic resin in the second adhesive may be 5% by mass or more, 7% by mass or more, or 10% by mass or more, based on the total amount of the second adhesive, from the viewpoint of easily improving the heat resistance and film formability of the second adhesive. The content of the thermoplastic resin may be 30% by mass or less, 25% by mass or less, or 20% by mass or less, based on the total amount of the second adhesive, from the viewpoint of easily suppressing the occurrence of fillets.
[0094] The content of the filler in the second adhesive may be 25% by mass or more, 30% by mass or more, or 35% by mass or more, based on the total amount of the second adhesive, from the viewpoint of suppressing a decrease in heat dissipation and of easily suppressing the occurrence of voids, an increase in moisture absorption rate, etc. The content of the filler may be 60% by mass or less, 55% by mass or less, or 50% by mass or less, based on the total amount of the second adhesive, from the viewpoint of suppressing the filler from getting caught (trapping) in the connection portion.
[0095] The content of the radical polymerization initiator in the second adhesive may be 0.01 parts by mass or less based on the total amount of the second adhesive. The second adhesive may not contain a radical polymerization initiator.
[0096] Because some flux compounds react with radicals and because the presence of a radically polymerizable compound causes a curing reaction to proceed rapidly upon heating, making it easier for a cured product to intervene between the joints, the second adhesive does not need to contain a radically polymerizable compound. The content of the radically polymerizable compound may be 0.5% by mass or less, 0.05% by mass or less, or 0% by mass, based on the total amount of the second adhesive.
[0097] The film adhesive 1 may be non-conductive, that is, the film adhesive 1 may be a so-called NCF (Non Conductive Film).
[0098] The film adhesive 1 described above may be provided with a substrate such as a support film or a protective film provided on the surface of the first adhesive region 2 (the side opposite to the second adhesive region 3) and / or the surface of the second adhesive region 3 (the side opposite to the first adhesive region 2). In the present disclosure, a laminate comprising a substrate and a film adhesive provided on the substrate is referred to as an adhesive tape.
[0099] The substrate can be any of the substrates exemplified as substrates used in the manufacturing method for a film-like adhesive described below, but the substrate provided on the second adhesive region 3 side of the film-like adhesive 1 may be a backgrind tape. That is, another embodiment of the present disclosure is an adhesive tape (adhesive tape with backgrind tape) comprising the above-mentioned film-like adhesive 1 and a backgrind tape provided on the film-like adhesive 1 on the side opposite the first adhesive region 2 side as viewed from the second adhesive region 3.
[0100] The backgrind tape is usually configured so that one main surface is an adhesive layer, but in this case, the backgrind tape is provided on the film adhesive 1 so that the surface on the adhesive layer side faces the film adhesive 1 (for example, so that the adhesive layer and the film adhesive are in contact). The thickness of the substrate (for example, the thickness of the backgrind tape) may be 20 to 300 μm.
[0101] The adhesive tape may be a laminate of a substrate and a film-like adhesive obtained by the manufacturing method of a film-like adhesive described below, i.e., a method of applying a coating liquid to a substrate, forming a coating film, and drying it, or may be a laminate obtained by attaching a substrate to the film-like adhesive 1 (for example, laminating the film-like adhesive 1 and the substrate). When the substrate is a backgrind tape, applying and drying the coating liquid on the adhesive layer of the backgrind tape may cause problems such as destruction of the adhesive layer and component migration between the adhesive and the adhesive, so the adhesive tape may be obtained by attaching the backgrind tape to the film-like adhesive 1.
[0102] <Method of Manufacturing a Film-Like Adhesive for Semiconductors> One embodiment of a method of manufacturing a film-like adhesive 1 includes a step of providing one of a first adhesive layer and a second adhesive layer on the other. Here, the first adhesive layer is a layer composed of the first adhesive (i.e., a layer that does not contain a flux compound and contains a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound), and forms a first adhesive region 2 in the film-like adhesive 1. The second adhesive layer is a layer composed of the second adhesive (i.e., a layer that contains a second epoxy resin, a second imidazole-based curing agent, and a flux compound), and forms a second adhesive region 3 in the film-like adhesive 1.
[0103] In one embodiment, the step may be, for example, a step of bonding a first adhesive film having the first adhesive layer to a second adhesive film having the second adhesive layer. In this embodiment, the method for producing the film adhesive 1 may further include a step of preparing the first adhesive film and the second adhesive film.
[0104] The step of preparing the first adhesive film may include forming a first adhesive layer on a substrate (e.g., a film-like substrate). When forming a first adhesive layer on a substrate, for example, first, a first epoxy resin, a first imidazole-based curing agent, a (meth)acrylic compound, and other components (fillers, thermoplastic resins, additives, etc.) added as needed are added to an organic solvent, and dissolved or dispersed by stirring, mixing, kneading, etc. to prepare a coating liquid containing the first adhesive. The coating liquid is then applied to a release-treated substrate using a knife coater, roll coater, applicator, etc. to form a coating film, and the organic solvent is then reduced from the coating film by heating. This allows the first adhesive layer to be formed on the substrate.
[0105] The organic solvent used in preparing the coating liquid may be one that has the property of being able to uniformly dissolve or disperse each component. Examples of such organic solvents include dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. These organic solvents can be used alone or in combination of two or more. The stirring, mixing, and kneading in preparing the coating liquid can be performed using, for example, a stirrer, a kneading machine, a three-roll mill, a ball mill, a bead mill, or a homodisper.
[0106] The substrate is not particularly limited as long as it has heat resistance sufficient to withstand the heating conditions when volatilizing the organic solvent, and examples thereof include polyolefin films such as polypropylene film and polymethylpentene film, polyester films such as polyethylene terephthalate film and polyethylene naphthalate film, polyimide film, and polyetherimide film. The substrate is not limited to a single layer made of these films, but may also be a multilayer film made of two or more materials. The substrate may also be a film whose surface has been subjected to a release treatment.
[0107] The drying conditions for volatilizing the organic solvent from the coating film on the substrate may be conditions that allow the organic solvent to volatilize sufficiently. Specifically, heating may be performed, for example, at 50 to 200°C for 0.1 to 90 minutes. As long as there is no effect on voids or viscosity adjustment after mounting, the organic solvent may be removed to 1.5 mass% or less of the total amount of the first adhesive.
[0108] The step of preparing the second adhesive film may include forming a second adhesive layer on the substrate by a method similar to that for forming the first adhesive layer, except that the second epoxy resin, the second imidazole curing agent, the flux compound, and other components (fillers, thermoplastic resins, additives, etc.) that are added as needed are used.
[0109] Examples of methods for bonding the first adhesive film and the second adhesive film include hot pressing, roll lamination, vacuum lamination, etc. Lamination may be performed under heating conditions of, for example, 30 to 120°C.
[0110] The film adhesive 1 may be obtained, for example, by forming one of a first adhesive layer and a second adhesive layer on a substrate, and then forming the other of the first adhesive layer and the second adhesive layer on the obtained first adhesive layer or second adhesive layer. The first adhesive layer and the second adhesive layer can be formed by the method described above.
[0111] For example, the film adhesive 1 may be obtained by forming the first adhesive and the second adhesive substantially simultaneously on a substrate. Examples of methods for simultaneously coating and preparing the first adhesive and the second adhesive include coating methods such as a sequential coating method and a multi-layer coating method.
[0112] <Semiconductor Device> Next, a semiconductor device manufactured using the film-like adhesive for semiconductors of the above embodiment will be described.
[0113] FIG. 2 is a schematic cross-sectional view showing one embodiment of a semiconductor device. The semiconductor device 100 shown in FIG. 2( a) includes a semiconductor chip 20 and a base 25 facing each other, wiring (first and second connection portions) 15 disposed on the opposing surfaces of the semiconductor chip 20 and the base 25, connection bumps 30 connecting the wiring 15 of the semiconductor chip 20 and the base 25 to each other, and a sealing portion 40 made of a cured product of adhesive (first and second adhesives) that fills the gap between the semiconductor chip 20 and the base 25. The semiconductor chip 20 and the base 25 are flip-chip connected by the wiring 15 and the connection bumps 30. The wiring 15 and the connection bumps 30 are sealed with the cured product of the adhesive and are isolated from the external environment. The sealing portion 40 includes an upper portion 40 a containing the cured product of the first adhesive and a lower portion 40 b containing the cured product of the second adhesive.
[0114] The semiconductor device 200 shown in FIG. 2( b) includes a semiconductor chip 20 and a base 25 facing each other, bumps (first and second connection portions) 32 disposed on the facing surfaces of the semiconductor chip 20 and the base 25, respectively, and a sealing portion 40 made of a cured product of adhesive (first and second adhesives) that fills the gap between the semiconductor chip 20 and the base 25. The semiconductor chip 20 and the base 25 are flip-chip connected by connecting the facing bumps 32 to each other. The bumps 32 are sealed with the cured product of the adhesive and are isolated from the external environment. The sealing portion 40 includes an upper portion 40 a containing the cured product of the first adhesive and a lower portion 40 b containing the cured product of the second adhesive.
[0115] The semiconductor chip 20 is not particularly limited, and may be a semiconductor chip made of an elemental semiconductor made of the same type of element such as silicon or germanium, or a semiconductor chip made of a compound semiconductor such as gallium arsenide or indium phosphide.
[0116] The substrate 25 is not particularly limited as long as it can be used to mount the semiconductor chip 20, and examples thereof include a semiconductor chip, a semiconductor wafer, and a wiring circuit board.
[0117] Examples of semiconductor chips that can be used as the base 25 are the same as the examples of the semiconductor chip 20 described above, and the same semiconductor chip as the semiconductor chip 20 may be used as the base 25 .
[0118] The semiconductor wafer that can be used as the base 25 is not particularly limited, and may have a configuration in which a plurality of semiconductor chips such as the semiconductor chip 20 are connected together.
[0119] The wired circuit board that can be used as the base 25 is not particularly limited, and examples that can be used include a circuit board having wiring (wiring pattern) 15 formed by etching away unnecessary portions of a metal film on the surface of an insulating substrate whose main component is glass epoxy, polyimide, polyester, ceramic, epoxy, bismaleimide triazine, or the like; a circuit board in which wiring 15 is formed on the surface of the insulating substrate by metal plating, or the like; and a circuit board in which wiring 15 is formed by printing a conductive material on the surface of the insulating substrate.
[0120] The connecting portions of the wiring 15, bumps 32, etc. contain, as main components, gold, silver, copper, solder (main components include, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper, etc.), nickel, tin, lead, etc., and may contain multiple metals.
[0121] Among the above metals, gold, silver, and copper may be used from the viewpoint of providing a package with excellent electrical and thermal conductivity at the connection portion. Silver, copper, and solder, which are inexpensive materials, may be used from the viewpoint of providing a package with reduced costs. Since the formation of an oxide film on the surface of a metal at room temperature can reduce productivity and increase costs, gold, silver, copper, and solder may be used from the viewpoint of suppressing the formation of an oxide film.
[0122] A metal layer containing gold, silver, copper, solder (main components of which may be, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, etc.), tin, nickel, etc. as a main component may be formed on the surfaces of the wiring 15 and bumps 32 by, for example, plating. This metal layer may be composed of only a single component, or may be composed of multiple components. Furthermore, the metal layer may have a structure in which a single layer or multiple metal layers are laminated.
[0123] The semiconductor device may be a stack of multiple structures (packages) such as those shown in the semiconductor devices 100 and 200. In this case, the semiconductor devices 100 and 200 may be electrically connected to each other by bumps, wiring, or the like containing gold, silver, copper, solder (the main component of which is, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper, etc.), tin, nickel, or the like.
[0124] As shown in FIG. 3 , a technique for stacking multiple semiconductor devices includes, for example, TSV (Through-Silicon Via) technology. In the semiconductor device 500 shown in FIG. 3 , wiring 15 formed on an interposer 50 is connected to wiring 15 of a semiconductor chip 20 via connection bumps 30, thereby flip-chip connecting the semiconductor chip 20 and the interposer 50. The gap between the semiconductor chip 20 and the interposer 50 is filled with a cured adhesive (first adhesive and second adhesive), forming a sealing portion 40. On the surface of the semiconductor chip 20 opposite the interposer 50, semiconductor chips 20 are repeatedly stacked via wiring 15, connection bumps 30, and sealing portion 40. The wiring 15 on the pattern surfaces on the front and back of the semiconductor chip 20 are connected to each other by through electrodes 34 filled in holes penetrating the interior of the semiconductor chip 20. Copper, aluminum, or the like can be used as the material for the through electrodes 34.
[0125] Such TSV technology makes it possible to acquire signals from the back surface of the semiconductor chip, which is not normally used. Furthermore, because the through electrodes 34 are passed vertically through the semiconductor chip 20, the distance between opposing semiconductor chips 20 and between the semiconductor chip 20 and the interposer 50 can be shortened, allowing for flexible connections. The semiconductor film-like adhesive of this embodiment can be used as a semiconductor film-like adhesive between opposing semiconductor chips 20 and between the semiconductor chip 20 and the interposer 50 in such TSV technology.
[0126] Furthermore, with highly flexible bump formation methods such as area bump chip technology, semiconductor chips can be directly mounted on motherboards without an interposer. The film-like adhesive for semiconductors of this embodiment can also be applied to cases where such semiconductor chips are directly mounted on motherboards. The film-like adhesive for semiconductors of this embodiment can also be applied to sealing the gap (air gap) between two wiring circuit boards when they are stacked.
[0127] <Method for Manufacturing a Semiconductor Device> Next, a method for manufacturing a semiconductor device using the film-like adhesive for semiconductors of the above embodiment will be described.
[0128] A method for manufacturing a semiconductor device according to one embodiment includes, for example, the steps of: preparing a semiconductor chip with a film adhesive; and the film adhesive for semiconductors according to the above embodiment, the film adhesive being provided on the semiconductor chip so that the surface of the first adhesive region opposite the second adhesive region faces the semiconductor chip; and placing the semiconductor chip with the film adhesive on a base from the film adhesive side and heating the semiconductor chip to electrically connect the connection portions of the semiconductor chip and the connection portions of the base and seal any gaps between the semiconductor chip and the base. The method for manufacturing a semiconductor device may further include the step of attaching the film adhesive for semiconductors according to the above embodiment to the connection surface of the semiconductor chip or its precursor from the first adhesive region side. Here, the semiconductor chip precursor refers to a component that will be processed into a semiconductor chip. A specific example of a semiconductor chip precursor is a semiconductor wafer. When a semiconductor wafer is used as the semiconductor chip precursor, the method for manufacturing a semiconductor device may further include the step of dicing the semiconductor wafer or the semiconductor wafer with the film adhesive.
[0129] The method for manufacturing a semiconductor device may use the adhesive tape with back-grinding tape described above. In this case, the method for manufacturing a semiconductor device may further include a laminating step of attaching the adhesive tape with back-grinding tape from the film-like adhesive side for semiconductors to the connection surface of a semiconductor wafer, which is a precursor of a semiconductor chip, and a back-grinding step of grinding the semiconductor wafer with the adhesive tape attached from the side opposite to the adhesive tape.
[0130] Hereinafter, the method for manufacturing a semiconductor device will be described in more detail, taking as an example an embodiment in which a precursor of a semiconductor chip (semiconductor wafer) is used.
[0131] 4 to 8 are cross-sectional views illustrating steps in one embodiment of a method for manufacturing a semiconductor device. The manufacturing method of this embodiment includes the following steps (a) to (e): Step (a): preparing a laminate 6 including a semiconductor wafer A having connection portions (first connection portions) 5 on one main surface (connection surface) and a film-like adhesive 1 provided on the main surface of the semiconductor wafer A so that the surface on which the first adhesive region 2 is located faces the semiconductor wafer A (see FIG. 4); Step (b): back-grinding a side of the laminate 6 opposite the side on which the film-like adhesive 1 is provided (the side opposite the side on which the connection portions 5 of the semiconductor wafer A are provided) (see FIG. 5); Step (c): singulating the laminate 6 to obtain semiconductor chips 8 with a film-like adhesive having connection portions 5 (see FIG. 6); and Step (d): picking up the semiconductor chips 8 with a film-like adhesive from the singulated film-like adhesive 1a side (see FIG. 7). Step (e): A step of placing a semiconductor chip 8 with a film-like adhesive on one of the main surfaces (connection surfaces) of a base 9 having a connection portion (second connection portion) 10 on the main surface from the film-like adhesive 1a side, and heating the semiconductor chip 8 with a film-like adhesive to electrically connect the connection portion 5 of the semiconductor chip 8 with the connection portion 10 of the base 9, and sealing the gap between the semiconductor chip 8 and the base 9 (see Figure 8). Note that if a semiconductor wafer whose thickness has been adjusted in advance is used, step (b) does not need to be performed.
[0132] (Step (a)) Step (a) may be a step of preparing a laminate 6 that has been produced in advance, or may be a step of producing the laminate 6. The laminate 6 may be produced, for example, by the following method.
[0133] First, an adhesive tape is prepared in which a substrate 4 is provided on the second adhesive region 3 side of the film-like adhesive 1, and this is placed in a predetermined device (see FIG. 4( a)). The substrate 4 is, for example, a backgrind tape. Next, a semiconductor wafer A having connection portions 5 (wiring, bumps, etc.) on one main surface is prepared, and the film-like adhesive 1 is attached to this main surface (the surface on which the connection portions 5 are provided, the connection surface) of the semiconductor wafer A. This results in a laminate 6 in which the semiconductor wafer A, first adhesive region 2, and second adhesive region 3 are laminated in this order (see FIG. 4( b)).
[0134] The film-like adhesive 1 can be applied by hot pressing, roll lamination, vacuum lamination, etc. The supply area and thickness of the film-like adhesive 1 are set appropriately depending on the sizes of the semiconductor wafer and substrate, the height of the connection portion, etc. In Figure 4, the thickness of the film-like adhesive 1 is greater than the height of the connection portion 5 of the semiconductor wafer A, and the connection portion 5 is covered by the film-like adhesive 1, but the thickness of the film-like adhesive 1 may also be smaller than the height of the connection portion 5.
[0135] (Step (b)) In step (b), the semiconductor wafers A of the stack 6 are ground using, for example, a grinder G (see FIGS. 5(a) and 5(b)). This thins the semiconductor wafers A. The thickness of the semiconductor wafers after grinding may be, for example, 10 μm to 300 μm. From the viewpoint of miniaturizing and thinning the semiconductor device, the thickness of the semiconductor wafers may be 20 μm to 100 μm.
[0136] (Step (c)) In step (c), for example, first, a dicing tape 7 is attached to the semiconductor wafer A side of the laminate 6, and the laminate is placed in a predetermined device (see FIG. 6(a)). The substrate 4 may be peeled off before or after the laminate 6 is attached to the dicing tape 7. Next, the laminate 6 is diced with a dicing saw D. In this way, the laminate 6 is divided into individual pieces, and semiconductor chips 8 with a film adhesive 1a on the semiconductor chip A' are obtained (see FIG. 6(b)). A connection portion 5 is provided on the surface of the semiconductor chip A' facing the film adhesive 1a. The film adhesive 1a has a first adhesive region (region made of the first adhesive) 2a and a second adhesive region (region made of the second adhesive) 3a.
[0137] (Step (d)) In step (d), for example, the dicing tape 7 is expanded to separate the semiconductor chips 8 with the film-like adhesive obtained by the dicing, and the semiconductor chips 8 with the film-like adhesive pushed up by the needles N from the dicing tape 7 side are picked up from the film-like adhesive 1a side by a pickup tool P (see FIG. 7). The picked-up semiconductor chips 8 with the film-like adhesive are transferred to a bonding tool and used for bonding in step (e).
[0138] (Step (e)) In step (e), for example, first, a base 9 for mounting a semiconductor chip is prepared, the base 9 having connection portions 10 (second connection portions) on one surface thereof, and the semiconductor chip 8 with a film-like adhesive is aligned with the base 9. Next, using a bonding tool, the semiconductor chip 8 with a film-like adhesive is placed on the main surface of the base 9 on which the connection portions 10 (wiring, bumps, etc.) are provided, with the film-like adhesive 1a side facing the base 9, and heated to bond the semiconductor chip 8 with a film-like adhesive to the base 9 (see FIGS. 8(a) and 8(b)). As a result, the connection portions 5 of the semiconductor chip 8 with a film-like adhesive and the connection portions 10 of the base 9 are electrically connected, and a sealing portion 1a' made of a cured product of the film-like adhesive 1a is formed between the semiconductor chip A' and the base 9, sealing the gap between the semiconductor chip 8 and the base 9, thereby obtaining a semiconductor device 11 that is a bonded assembly of the semiconductor chip 8 with a film-like adhesive and the base 9. The sealing portion 1a' has an upper portion 2a' containing the cured product of the first adhesive and a lower portion 3a' containing the cured product of the second adhesive.
[0139] When a solder bump is used for one of the connection portions 5 and 10 (for example, when the connection portion 5 or the connection portion 10 is a wiring provided with a solder bump), the connection portion 5 and the connection portion 10 are electrically and mechanically connected by being soldered together.
[0140] The heating in step (e) may be performed while the semiconductor chip is being placed, or may be performed after the semiconductor chip is placed. The heating and placement in step (e) may be thermocompression bonding. Step (e) may include a step of temporarily fixing the semiconductor chip A' after alignment (temporary fixing step), and a step of melting bumps (e.g., solder bumps) provided on the connection portion by heat treatment to bond the semiconductor chip A' to the base 9 and seal the connection portion (sealing step). Since it is not necessary to form a metal bond during the temporary fixing step, the temporary fixing step can be performed under low load, in a short time, and at a low temperature. Therefore, when the temporary fixing step and the sealing step are performed in step (e), productivity is improved and deterioration of the connection portion can be suppressed.
[0141] The load applied for temporary fixation is appropriately set taking into consideration the number of connection portions (bumps), absorbing variations in the height of the connection portions (bumps), and controlling the amount of deformation of the connection portions (bumps). The greater the load, the easier it is to eliminate voids and bring the connection portions into contact. The load may be, for example, 0.009 N to 0.2 N per connection portion (e.g., bump).
[0142] Heating in the sealing step may be performed using an apparatus capable of heating to a temperature equal to or higher than the melting point of the metal of the connection portion. The heating temperature may be a temperature at which the film-like adhesive begins to harden or may be a temperature at which the film-like adhesive is completely hardened. The heating temperature and heating time are set appropriately.
[0143] The heating time in the sealing step varies depending on the type of metal constituting the connection, but productivity tends to improve as the heating time shortens. When solder bumps are used for the connection, the heating time may be 20 seconds or less, or may be 10 seconds or less, or may be 5 seconds or less. In the case of copper-copper or copper-gold metal connections, the connection time may be 60 seconds or less.
[0144] In the sealing process, heating and pressure may be applied using an apparatus capable of heating and pressure. That is, the heating in the sealing process may be heating by thermocompression bonding. In this case, the load (connection load) is set taking into consideration the size of the connection member, the number of connection parts, height variation, the amount of deformation of the connection parts due to pressure, etc. The connection load may be, for example, 1 MPa or less above atmospheric pressure. The higher the connection load, the easier it is to suppress voids and improve connectivity. On the other hand, the smaller the connection load, the easier it is to suppress fillets. From these perspectives, the load may be 0.05 to 0.5 MPa. The compression time (connection time) varies depending on the type of metal constituting the connection parts, but a shorter compression time tends to improve productivity. When the connection parts are solder bumps, the compression time may be 20 seconds or less, 10 seconds or less, or 5 seconds or less. Note that, since direct pressure using a crimping machine makes it difficult for the heat of the crimping machine to be transferred to the fillets, pressure may be applied by air pressure from the viewpoint of making it easier to fully apply the heat to the fillets. From the viewpoint of en bloc sealing and suppressing fillet formation, the pressure applied during heating may be atmospheric pressure (pressure applied using a pressure reflow furnace, a pressure oven, or the like).
[0145] After the semiconductor chip A' and the base 9 are connected, a heat treatment may be carried out in an oven or the like to further improve the connection reliability.
[0146] The present disclosure will be described in more detail below using examples, but the present disclosure is not limited to these examples.
[0147] Details of the materials used in the examples and comparative examples are as follows. (Liquid epoxy resins) YX7110B80: Flexible epoxy, manufactured by Mitsubishi Chemical Corporation, trade name "jERYX7110B80", "jER" is a registered trademark (same below) YL983U: Bisphenol F type liquid epoxy, manufactured by Mitsubishi Chemical Corporation, trade name "jERYL983U" (Solid epoxy resins) EP1032: Triphenolmethane skeleton-containing multifunctional solid epoxy, manufactured by Mitsubishi Chemical Corporation, trade name "jER1032H60" (Imidazole-based curing agents) 2PHZ-PW: 2-phenyl-4,5-dihydroxymethylimidazole, manufactured by Shikoku Chemical Industries, Ltd., trade name 2MAOK-PW: 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, manufactured by Shikoku Chemical Industries, Ltd., trade name (Phenoxy resins) ZX-1356-2: Phenoxy resin, trade name, manufactured by Tohto Kasei Co., Ltd., Tg = approx. 71°C, weight average molecular weight Mw = approx. 63,000 (Acrylic compounds) A-DPH: Dipentaerythritol polyacrylate, trade name, manufactured by Shin-Nakamura Chemical Co., Ltd. (Organic fillers) EXL-2655: Core-shell type organic fine particles, trade name, manufactured by Rohm and Haas Japan Co., Ltd. (Silica fillers) KE180G-HLA: Silica filler, trade name, manufactured by Admatechs Co., Ltd. (Flux compounds) 2-methylglutaric acid: manufactured by Aldrich Chemicals, melting point = approx. 78°C
[0148] Examples 1 to 7 and Comparative Example 1 (Preparation of First Adhesive Film) The components shown in Table 1 were added to an organic solvent (methyl ethyl ketone) so that the NV value ([mass of coating component after drying] / [mass of coating component before drying]×100) was 60%, to obtain a mixed solution. At this time, the amount of each component added was the amount (unit: parts by mass) shown in Table 1. Then, beads with a diameter of 1.0 mm and beads with a diameter of 2.0 mm were added to the mixed solution, and the mixture was stirred for 30 minutes with a bead mill (Fritsch Japan Co., Ltd., planetary fine grinder P-7). The amount of beads added was the same mass as the non-volatile content of the mixed solution (total amount of components other than the organic solvent). After stirring, the beads were removed by filtration. In this way, coating solutions 1A to 8A for forming a first adhesive layer were obtained.
[0149] Using the resulting coating solutions 1A to 8A, first adhesive films (first adhesive films 1A to 8A) comprising first adhesive layers 1A to 8A, respectively, were obtained. Specifically, the coating solution was first applied to a substrate film (manufactured by Teijin DuPont Films Co., Ltd., product name "Purex A54") using a small precision coating device (Kazui Seiki) so that the film thickness after drying would be 4.5 μm. The coating film was then dried (80°C / 10 min) in a clean oven (manufactured by ESPEC), thereby obtaining a first adhesive film comprising a first adhesive layer.
[0150]
[0151] (Preparation of Second Adhesive Film) The components shown in Table 2 were added to an organic solvent (methyl ethyl ketone) so that the NV value was 60%, to obtain a mixed solution. At this time, the amount of each component added was the amount shown in Table 2 (unit: parts by mass). Then, Φ1.0 mm beads and Φ2.0 mm beads were added to the mixed solution, and the mixture was stirred for 30 minutes with a bead mill (Fritsch Japan Co., Ltd., planetary fine grinder P-7). The amount of beads added was the same mass as the non-volatile content of the mixed solution (total amount of components other than the organic solvent). After stirring, the beads were removed by filtration, and Coating Liquid 1B and Coating Liquid 2B for forming the second adhesive layer were obtained.
[0152] The obtained coating liquid 1B was applied to a substrate film (manufactured by Teijin DuPont Films Co., Ltd., product name "Purex A54") using a small precision coating device (Kanei Seiki) so that the film thickness after drying would be 4.5 μm. The coating film was then dried (80°C / 10 min) in a clean oven (manufactured by ESPEC) to obtain a second adhesive film 1B comprising a second adhesive layer 1B. A second adhesive film 2B comprising a second adhesive layer 2B was also obtained in the same manner, except that coating liquid 2B was used instead of coating liquid 1B.
[0153]
[0154] (Preparation of film-like adhesive) Any one of the first adhesive films 1A to 8A prepared above was laminated with the second adhesive film 1B or 2B in the combinations shown in Table 3 to laminate the first adhesive layer and the second adhesive layer, thereby preparing the film-like adhesives (total thickness 9.0 μm) of Examples 1 to 7 and Comparative Example 1. The lamination temperature was 50° C.
[0155] <Comparative Example 2> A second adhesive film 1B having a second adhesive layer 1B was obtained in the same manner as in the above "Preparation of a second adhesive film", and then two layers of the obtained second adhesive layer 1B were laminated to obtain a film-like adhesive of Comparative Example 2 (total thickness 9.0 μm).
[0156] <Evaluation> Connection structures (semiconductor devices) were produced using the film-like adhesives obtained in Examples 1 to 7 and Comparative Examples 1 and 2 according to the following procedure. Furthermore, the resulting connection structures were used to evaluate fillet length, voids, and sealing performance according to the methods described below. The results are shown in Table 3.
[0157] (Preparation of Connection Structure) The film-like adhesives obtained in Examples 1 to 7 and Comparative Examples 1 and 2 were cut to a predetermined size (8 mm long x 8 mm wide x 9.0 μm thick) to prepare evaluation samples. The evaluation samples were then attached to the solder bump-bearing surfaces (connection surfaces) of a semiconductor chip with solder bumps (chip size: 7.3 mm long x 7.3 mm wide x 0.15 mm thick, bump height: copper pillar + solder total approximately 40 μm, number of bumps: 328) to obtain a laminate of the evaluation sample and the semiconductor chip with solder bumps. In Examples 1 to 7 and Comparative Example 1, the first adhesive layer (opposite the second adhesive layer) was attached to the semiconductor chip with solder bumps. Next, using a flip mounter "FCB3" (manufactured by Panasonic, product name), the laminate was mounted on a glass epoxy substrate (glass epoxy substrate: 420 μm thick, copper wiring: 9 μm thick) from the evaluation sample side. The mounting was performed under the conditions of a pressure head temperature of 350° C., a pressure bonding time of 3 seconds, and a pressure bonding pressure of 0.5 MPa, thereby obtaining a connection structure (semiconductor device) in which the glass epoxy substrate and the semiconductor chip with solder bumps were daisy-chain connected.
[0158] (Fillet Amount) The connection structure obtained above was observed from the semiconductor chip side using a digital microscope VHX-6000 (manufactured by Keyence Corporation), and the length of the adhesive (fillet) protruding from the four peripheral sides of the semiconductor chip was measured. The length of the fillet on each side was taken as the maximum value of the shortest distance from the end of the protruding adhesive to the semiconductor chip. The fillet amount was evaluated by the average value of the fillet lengths measured on each of the four sides. If the average value was less than 100 μm, it was determined that the amount of fillet generation had been sufficiently reduced, and if the average value was 100 μm or more, it was determined that the fillet suppression effect was insufficient.
[0159] (Voids) For the connection structure obtained above, an external image was taken using an ultrasound imaging diagnostic device (trade name "Insight-300", manufactured by Insight), and an image of the adhesive layer on the chip (a layer consisting of a cured product of a film-like adhesive for semiconductors) was captured using a scanner GT-9300UF (trade name, manufactured by Epson Corporation). Using image processing software Adobe Photoshop (registered trademark), voids were identified by color correction and two-tone gradation, and the proportion occupied by the voids was calculated using a histogram. The area of the adhesive portion on the chip was taken as 100%, and evaluation was carried out with a void occurrence rate of 5% or less as "A", a rate of more than 5% and 10% or less as "B", and a rate of more than 10% as "C".
[0160] (Sealability) The connection structure obtained above was observed from the semiconductor chip side using a semiconductor / FPD inspection microscope MX63 (manufactured by Olympus), and the length of the unfilled part of the chip square was measured. The length of the unfilled part was taken as the maximum value of the shortest distance from the chip square to the filled part. The sealability was evaluated as "A" if the length of the unfilled part was less than 500 μm, and "B" if it was 500 μm or more.
[0161]
[0162] 1, 1a...film-like adhesive for semiconductor, 2, 2a...first adhesive region, 3, 3a...second adhesive region, 4...substrate, 5...connection portion (first connection portion), 9...base body, 10...connection portion (first connection portion), 11...semiconductor device, 15...wiring (first connection portion and second connection portion), 20...semiconductor chip, 25...base body, 30...connection bump, 32...bump (first connection portion and second connection portion), 40...sealing portion, 100, 200, 500...semiconductor device, A...semiconductor wafer, A'...semiconductor chip.
Claims
1. A film-like adhesive for semiconductors having, along a thickness direction, a first adhesive region not containing a flux compound and a second adhesive region containing a flux compound, the first adhesive region containing a first epoxy resin, a first imidazole-based curing agent, and a (meth)acrylic compound, and the second adhesive region containing a second epoxy resin, a second imidazole-based curing agent, and the flux compound.
2. The film-like adhesive for semiconductors according to claim 1, wherein the first adhesive region does not contain a radical polymerization initiator.
3. The film-like adhesive for semiconductors according to claim 1, wherein at least one of the first epoxy resin and the second epoxy resin comprises an epoxy resin that is liquid at 25°C.
4. A film-like adhesive for semiconductors according to claim 1, wherein at least one of the first epoxy resin and the second epoxy resin contains a triphenolmethane type epoxy resin.
5. A film-like adhesive for semiconductors according to claim 1, wherein at least one of the first imidazole-based curing agent and the second imidazole-based curing agent has a triazine ring.
6. A film-like adhesive for semiconductors as described in claim 1, wherein the ratio of the content of the first epoxy resin to the content of the (meth)acrylic compound in the first adhesive region is 3 to 11 in mass ratio.
7. The film-like adhesive for semiconductors according to claim 1, wherein the (meth)acrylic compound comprises a polyfunctional (meth)acrylic compound having 2 to 8 (meth)acryloyl groups.
8. The film-like adhesive for semiconductors according to claim 1, wherein the flux compound comprises a polycarboxylic acid.
9. A film-like adhesive for semiconductors as described in claim 1, wherein the thickness of the first adhesive region is 1 to 50 μm, and the thickness of the second adhesive region is 0.5 to 2 times the thickness of the first adhesive region.
10. The film adhesive for semiconductors according to claim 1, which is non-conductive.
11. The film-like adhesive for semiconductors according to claim 1, which is used to bond a semiconductor chip to a substrate and to seal the gap between the semiconductor chip and the substrate.
12. A method for producing a film-like adhesive for semiconductors as described in any one of claims 1 to 11, comprising a step of providing one of a first adhesive layer and a second adhesive layer on the other, wherein the first adhesive layer does not contain a flux compound and is a layer containing the first epoxy resin, the first imidazole-based curing agent, and the (meth)acrylic compound, and the second adhesive layer is a layer containing the second epoxy resin, the second imidazole-based curing agent, and the flux compound.
13. An adhesive tape comprising: a film-like adhesive for semiconductors according to any one of claims 1 to 11; and a backgrind tape provided on the film-like adhesive for semiconductors, on the side opposite the first adhesive region when viewed from the second adhesive region.
14. A method for manufacturing a semiconductor device, comprising: a step of preparing a semiconductor chip with a film-like adhesive, the semiconductor chip comprising: a semiconductor chip; and a film-like adhesive for semiconductors according to any one of claims 1 to 11, the film-like adhesive being provided on the semiconductor chip such that the surface of the first adhesive region opposite the second adhesive region faces the semiconductor chip; and a step of placing the semiconductor chip with the film-like adhesive on a base from the film-like adhesive side, and heating the semiconductor chip with the film-like adhesive, thereby electrically connecting the connection parts of the semiconductor chip and the connection parts of the base, and sealing any gaps between the semiconductor chip and the base.
15. A semiconductor device comprising: a semiconductor chip having a first connection portion; a base having a second connection portion electrically connected to the first connection portion; and a sealing portion that bonds the semiconductor chip to the base and fills a gap between the semiconductor chip and the base, wherein the sealing portion is a cured product of a film-like adhesive for semiconductors described in any one of claims 1 to 11.
Citation Information
Patent Citations
Film for semiconductor, method for manufacturing semiconductor device, and semiconductor device
JP2009239138A
Semiconductor device, and method for manufacturing the same
JP2010123911A
Film-like adhesive for semiconductors, semiconductor device manufacturing method and semiconductor device
JP2022186809A