Conductive resin composition

A conductive resin composition using tin powder, specific epoxy resin, and dicarboxylic acid compounds addresses the challenges of storage stability and conductivity, offering a cost-effective solution with excellent adhesion and conductivity for electronic applications.

WO2024224871A1PCT designated stage expired Publication Date: 2024-10-31SAKATA INX

Patent Information

Application Number
PCT/JP2024/010273
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-08
Filing Date
2024-03-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conductive resin compositions with tin powder face challenges in achieving both excellent storage stability and conductivity while maintaining low volume resistivity, and existing solutions are costly or have poor adhesion to substrates.

Method used

A conductive resin composition comprising tin powder, a specific epoxy resin with an epoxy equivalent of 400 g/eq or more, and a dicarboxylic acid compound, which can include a thiol-based compound, to form a conductive film with low volume resistivity and excellent conductivity without using thiol-based or amine-based epoxy resin curing agents.

Benefits of technology

The composition provides a cost-effective solution with excellent storage stability at room and refrigerated temperatures, low volume resistivity, and high conductivity, suitable for various electronic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing a conductive resin composition containing a tin powder, in which the conductive resin composition is excellent in storage stability at room temperature (25°C) and storage stability when refrigerated (4°C), capable of forming an electroconductive film having low volume resistivity and excellent electroconductivity, and advantageous in terms of cost. As a means for solving said problem, provided is a conductive resin composition comprising a tin powder (a), an epoxy resin (b), and a dicarboxylic acid compound (c). The epoxy resin (b) includes an epoxy resin that has an epoxy equivalent of 400 g / eq or more and is a solid or a semi-solid at 25°C. The dicarboxylic acid compound (c) includes a dicarboxylic acid compound having 4-9 carbons.
Need to check novelty before this filing date? Find Prior Art

Description

Conductive resin composition

[0001] The present invention relates to a conductive resin composition. The present invention also relates to a conductive film, a conductive material used when forming a circuit or the like by printing on a substrate by a method such as screen printing, a conductive adhesive, and a circuit connecting material used when conductively connecting electronic components to a circuit board or the like.

[0002] A wide variety of conductive resin compositions are known, and they are used in a variety of applications, such as forming electronic circuits and bonding electronic components, as conductive pastes, conductive films, conductive materials, conductive paints, circuit connecting materials, and conductive adhesives. For example, there is a demand for conductive resin compositions that can form conductive films with low volume resistivity and excellent conductivity in order to form conductive structures such as conductive circuits and electrodes. There is a demand for conductive materials that can be applied to various printing methods and are useful for manufacturing flexible plastic substrates and the like that have conductive structures such as interconnections, traces, and electrodes. For example, there is a demand for circuit connecting materials that enable high-density packaging and high integration of various electronic components, such as LED elements, semiconductor elements, and capacitors, on the same circuit board in electronic devices such as computers and mobile phones.

[0003] Known conductive resin compositions include conductive resin compositions (conductive pastes) containing various resins and various conductive particles. However, conventional conductive resin compositions do not have a sufficiently low volume resistivity. Therefore, when used in applications requiring excellent conductivity (low volume resistivity), silver particles must be used as the conductive particles, which poses a cost problem. Furthermore, when a large amount of conductive particles is added to reduce the volume resistivity of a conductive film formed from the conductive resin composition, the adhesion (bonding strength) of the film to various substrates decreases, which is unsatisfactory.

[0004] Patent Document 1 discloses a conductive paste composition in which the conductive powder is a silver-based powder containing at least silver, the resin component is at least one of a thermosetting resin and a thermoplastic resin, and further contains an ester-based compound or its salt, or an ether / amine-based compound, having a specific molecular weight and structure. Patent Document 2 discloses a conductive resin composition containing tin powder, a resin, and an organic acid compound. This conductive resin composition has a low volume resistivity when a conductive film is formed, exhibits good conductivity, and is usable as a substitute for silver paste. It is said to be a conductive resin composition useful as a conductive material, conductive adhesive, circuit connection material, etc. Patent Document 3 discloses a conductive adhesive containing 85% to 92% by weight of a conductive metal powder and the remainder being a binder, the binder including an epoxy resin, an acid anhydride-based curing agent, an organic acid, and rubber particles having a particle size of 100 nm to 300 nm, the proportion of the rubber particles being 8% to 25% by weight relative to 100% by weight of the binder. This conductive adhesive is said to be capable of bonding metals together at temperatures lower than the melting point of the conductive metal powder and to have reduced bleeding. Patent Document 4 discloses a conductive adhesive comprising an organic resin and a conductive filler, the conductive main filler being 20 to less than 100 wt % of tin and / or a tin alloy, another conductive filler being a powder of silver and / or a silver alloy, or gold and / or a gold alloy, or a powder filler plated with these metals, a binder, and an organic acid such as adipic acid or a derivative thereof. This conductive adhesive is said to be an inexpensive solder substitute with excellent conductivity and repairability. Patent Document 5 discloses a conductive adhesive containing a Sn-containing conductive metal powder, a thermosetting resin, an acid anhydride curing agent, and an organic acid, and uses an organic acid metal salt produced by the reaction of the conductive metal powder and the organic acid during heating as a curing accelerator. This conductive adhesive is said to be able to cure the thermosetting resin in a short time.

[0005] Japanese Patent Application Publication No. 2020-205245 Japanese Patent Application Publication No. 2022-172874 Japanese Patent No. 6428716 Japanese Patent Application Publication No. 2000-309773 International Publication No. 2015 / 019666

[0006] Although conductive resin compositions containing silver particles can form conductive films with excellent conductivity, they are disadvantageous in terms of cost because silver particles are very expensive. On the other hand, conductive resin compositions containing conductive particles other than silver particles can result in conductive films with high volume resistivity and insufficient conductivity. Furthermore, when a large amount of conductive particles is added to reduce volume resistivity, adhesion to various substrates can be insufficient. Conductive resin compositions containing tin powder are known from Patent Documents 2 to 5, etc., but are unsatisfactory in terms of storage stability at room temperature and under refrigeration, or volume resistivity when a conductive film is formed. Therefore, no conductive resin composition has been known that satisfies the high demand for both excellent storage stability and excellent conductivity.

[0007] One problem to be solved by the present invention is to provide a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated storage stability (4°C), is capable of forming a conductive film with low volume resistivity and excellent conductivity, and is cost-effective. Another problem to be solved by the present invention is to provide a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated storage stability (4°C), is capable of forming a conductive film with low volume resistivity and excellent conductivity, has excellent curability without using a thiol-based epoxy resin curing agent, an amine-based epoxy resin curing agent, an acid anhydride-based epoxy resin curing agent, or a phenol-based epoxy resin curing agent, and is cost-effective. Another problem to be solved by the present invention is to provide a conductive film with low volume resistivity formed from the conductive resin composition, a conductive material containing the conductive resin composition, a conductive adhesive containing the conductive resin composition, and a circuit connecting material containing the conductive resin composition, all at low cost.

[0008] The present inventors conducted extensive research to solve the above-mentioned problems, and discovered that the above-mentioned problems can be solved by using a conductive resin composition with a specific composition, leading to the completion of the present invention. Specifically, the present invention is as follows: [Item 1] A conductive resin composition comprising: (a) tin powder; (b) an epoxy resin; and (c) a dicarboxylic acid compound, wherein the (b) epoxy resin comprises an epoxy resin having an epoxy equivalent of 400 g / eq or more and being solid or semi-solid at 25°C, and the (c) dicarboxylic acid compound comprises a dicarboxylic acid compound having 4 to 9 carbon atoms. [Item 2] The conductive resin composition according to Item 1, wherein the content of the (a) tin powder is 92.01% by mass to 99.50% by mass, based on 100% by mass of the total amount of components in the conductive resin composition other than the solvent. [Item 3] The conductive resin composition according to Item 1 or 2, wherein the (c) dicarboxylic acid compound further comprises a dicarboxylic acid compound having 10 or more carbon atoms. [Item 4] The conductive resin composition according to any one of items 1 to 3, further comprising (d) a thiol-based compound. [Item 5] A conductive resin composition according to any one of items 1 to 4, having a volume resistivity of 4.0 × 10 -4 A conductive film having a resistivity of less than Ω cm. [Item 6] A conductive material comprising the conductive resin composition according to any one of items 1 to 4. [Item 7] A conductive adhesive comprising the conductive resin composition according to any one of items 1 to 4. [Item 8] A circuit connecting material comprising the conductive resin composition according to any one of items 1 to 4.

[0009] The present invention provides a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated storage stability (4°C), is capable of forming a conductive film with low volume resistivity and excellent conductivity, and is cost-effective.The present invention provides a conductive resin composition containing tin powder, which has excellent storage stability at room temperature (25°C) and refrigerated storage stability (4°C), is capable of forming a conductive film with low volume resistivity and excellent conductivity, and has excellent curability without the use of a thiol-based epoxy resin curing agent, an amine-based epoxy resin curing agent, an acid anhydride-based epoxy resin curing agent, or a phenol-based epoxy resin curing agent, and is cost-effective.The present invention makes it possible to provide, at low cost, a conductive film with low volume resistivity formed from the conductive resin composition, a conductive material containing the conductive resin composition, a conductive adhesive containing the conductive resin composition, and a circuit connecting material containing the conductive resin composition. The conductive resin composition of the present invention is useful as a printed electronics material, and is extremely useful in mass production of various electronic devices such as display devices, vehicle-related parts, IoT, and mobile communication systems.

[0010] The present invention relates to a conductive resin composition, a conductive film, a conductive material, a conductive adhesive, and a circuit connecting material, which will be described in detail below.

[0011] [Conductive Resin Composition] <(a) Tin Powder> The (a) tin powder contained in the conductive resin composition of the present invention is composed of 99.5% by mass or more of tin and may contain components other than tin (e.g., inevitable impurities). Examples include tin powder containing only inevitable impurities and tin powder containing 0.5% by mass or less of components other than tin. The tin content in the (a) tin powder can be easily measured using an X-ray fluorescence (XRF) analyzer or the like. Examples of components other than tin that may be contained in the (a) tin powder include one or more other atoms selected from the group consisting of Mn, Sb, Si, K, Na, Li, Ba, Sr, Ca, Mg, Be, Zn, Pb, Cd, Tl, V, Al, Zr, W, Mo, Ti, Co, Ag, Cu, Ni, Au, B, C, N, O, Ge, Sb, In, As, Al, and Fe. The content of other atoms in the (a) tin powder is preferably less than 0.3% by mass, more preferably 0.1% by mass or less.

[0012] (a) The shape of the tin powder is not particularly limited. For example, flaky, flat, spherical, approximately spherical (for example, with a length-to-width aspect ratio of 1.5 or less), block, plate, polygonal pyramid, polyhedron, rod, fiber, needle, irregular shape, etc. can be used depending on the application. In the present invention, flaky, spherical, approximately spherical, and flat shapes are preferred from the viewpoints of volume resistivity, dispersibility, handleability, etc.

[0013] When the (a) tin powder is spherical, its volume average particle diameter (50% particle diameter D50 of the cumulative frequency % diameter in the volume-based particle size distribution) is not particularly limited. D50 is, for example, 0.5 μm or more, preferably 1.0 μm or more, more preferably 3.0 μm or more, and for example, 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less. When D50 is 0.5 μm or more, the dispersibility and handleability of the (a) tin powder are improved. When D50 is 300 μm or less, the volume resistivity can be reduced, and the dispersibility and handleability are improved. The method for measuring D50 is not particularly limited, but examples include laser diffraction / scattering particle size distribution measurement methods.

[0014] (a) When the tin powder is flat or flaky, its average diameter, average thickness, and aspect ratio (average diameter / average thickness) are not particularly limited. The average diameter is, for example, 0.5 μm or more, preferably 1.0 μm or more, more preferably 5.0 μm or more, and for example, 500.0 μm or less, preferably 300.0 μm or less, more preferably 150.0 μm or less. The average thickness is, for example, 0.1 μm or more, preferably 0.5 μm or more, more preferably 1.0 μm or more, and for example, 50.0 μm or less, preferably 20.0 μm or less, more preferably 10.0 μm or less. The aspect ratio is, for example, 2 or more, preferably 10 or more, more preferably 50 or more. The method for measuring the average diameter and average thickness is not particularly limited, and examples thereof include measurement using a scanning electron microscope.

[0015] The content of (a) tin powder in the conductive resin composition is not particularly limited. It is, for example, 88.00% by mass or more, preferably 90.10% by mass or more, more preferably 92.01% by mass or more, and for example, 99.50% by mass or less, preferably 99.00% by mass or less, more preferably 98.00% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition. If the content of (a) tin powder is less than 88.00% by mass, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition, the conductivity may decrease and the volume resistivity may increase. If it exceeds 99.50% by mass, there may be problems such as inability to form a film, low substrate adhesion, long curing times, decreased dispersibility of the (a) tin powder, inability to form a uniform composition, and decreased storage stability.

[0016] <(b) Epoxy Resin> The (b) epoxy resin contained in the conductive resin composition of the present invention is not particularly limited as long as it contains an epoxy resin having two or more epoxy groups in the molecule, an epoxy equivalent of 400 g / eq or more, and being solid or semi-solid at 25°C. In the present invention, an epoxy resin having an epoxy equivalent of 400 g / eq or more and being solid at 25°C is an epoxy resin that does not exhibit fluidity at 25°C and has a melting point or softening point of 25°C or higher. There are no particular limitations on the upper limit of the melting point or softening point, but it is preferably 150°C or lower, for example. In the present invention, the softening point is a value measured by a softening point test (ring and ball method) (measurement conditions: in accordance with JIS-K7234:1986). In the present invention, an epoxy resin having an epoxy equivalent of 400 g / eq or more and being semi-solid at 25°C is an epoxy resin having a Gardner viscosity standard solution designation of Z-Z2 at 25°C (measurement conditions: concentration 60%, butyl carbitol solvent, JIS K 5600).

[0017] Examples of epoxy resins that have an epoxy equivalent of 400 g / eq or more and are solid or semi-solid at 25°C include biphenyl-type epoxy resins; bisphenol-type epoxy resins such as bisphenol A-type epoxy resins, bisphenol F-type epoxy resins, and tetramethylbisphenol F-type epoxy resins; naphthalene-type epoxy resins; alkylene oxide-modified bisphenol-type resins; chelate-modified epoxy resins; stilbene-type epoxy resins; glycol-type epoxy resins; pentaerythritol-type epoxy resins; novolac-type epoxy resins such as phenol novolac-type epoxy resins, cresol novolac-type epoxy resins, and bisphenol A novolac-type epoxy resins; polyfunctional epoxy resins such as trisphenolmethane-type epoxy resins and alkyl-modified trisphenolmethane-type epoxy resins; phenol aralkyl-type epoxy resins having a phenylene skeleton; naphthol-type epoxy resins such as dihydroxynaphthalene-type epoxy resins and epoxy resins obtained by glycidyl etherifying a dihydroxynaphthalene dimer; triazine nucleus-containing epoxy resins such as triglycidyl isocyanurate and monoallyl diglycidyl isocyanurate; urethane-modified epoxy resins such as resins obtained by reacting a urethane bond-containing compound having an isocyanate group with a hydroxy group-containing epoxy compound; bridged cyclic hydrocarbon compound-modified phenol-type epoxy resins such as dicyclopentadiene-modified phenol-type epoxy resins; chelate-modified epoxy resins; dimer acid-modified epoxy resins; rubber-modified epoxy resins; polysulfide-modified epoxy resins; glycidylamine-type epoxy resins; and glycidyl ester-type epoxy resins.Examples of epoxy resins include compounds containing two or more glycidyl groups per molecule, such as bisphenol compounds such as bisphenol A, bisphenol F, and biphenol, or derivatives thereof; alicyclic epoxy resins such as polydiols having an alicyclic structure, such as cyclohexanediol, cyclohexanedimethanol, and cyclohexanediethanol, or epoxidized derivatives thereof; aliphatic epoxy resins such as aliphatic polydiols, such as butanediol, hexanediol, octanediol, nonanediol, decanediol, and polybutadiene polyol, or epoxidized derivatives thereof; epoxy resins having a trihydroxyphenylmethane skeleton (trisphenolmethane skeleton); aminophenol-type epoxy resins; polyether-modified epoxy resins; polyfunctional aromatic epoxy resins; and hydrogenated bisphenol-type epoxy resins. One type of epoxy resin may be used alone, or two or more types may be used in combination.

[0018] The epoxy resin having an epoxy equivalent of 400 g / eq or more and being in a solid or semi-solid state at 25° C. may be a synthesized product or a commercially available product. Commercially available epoxy resins having an epoxy equivalent of 400 g / eq or more and in a solid or semi-solid state at 25°C include, for example, YD-011, YD-012, YD-013, YD-014, YD-017, YD-019, YD-901, YD-902, YD-903N, YD-904, YD-907, YD-7910, YDF-2001, and YDF-2004 manufactured by Nippon Steel Chemical & Material Co., Ltd.; jER-4005P, jER-4007P, jER-4010P, and jER-1010 manufactured by Mitsubishi Chemical Corporation; and EPICLON 5500, EPICLON 5800, EPICLON 1050, and EPICLON 1010 manufactured by DIC Corporation. 1055, EPICLON 3050, EPICLON 4050, EPICLON 7050, EPICLON AM-030-P, EPICLON AM-040-P, EPICLON HM-091, EPICLON TSR-601; LCE-2615 manufactured by Nippon Kayaku Co., Ltd.; and the like.

[0019] In the present invention, the epoxy resin (b) may contain (i) an epoxy resin that is liquid at 25° C. and / or (ii) an epoxy resin that has an epoxy equivalent of less than 400 g / eq and is solid or semi-solid at 25° C. Examples of such epoxy resins include bisphenol-type epoxy resins, naphthalene-type epoxy resins, alicyclic epoxy resins such as glycidyl ester-type epoxy resins, glycidyl amine-type epoxy resins, phenol novolac-type epoxy resins, and alicyclic epoxy resins having an ester skeleton, cyclohexane-type epoxy resins, cyclohexane dimethanol-type epoxy resins, glycidyl amine-type epoxy resins, and epoxy resins having a structure that is an epoxidized product of polybutadiene polyol, rubber-modified epoxy resins, chelate-modified epoxy resins, urethane-modified epoxy resins, and polysulfide-modified epoxy resins. Preferably, one or more selected from the group consisting of bisphenol-type epoxy resins, rubber-modified epoxy resins, alicyclic epoxy resins, glycidylamine-type epoxy resins, urethane-modified epoxy resins, polysulfide-modified epoxy resins, chelate-modified epoxy resins, trisphenolmethane-type epoxy resins, and dicyclopentadiene-modified epoxy resins are used.

[0020] The content of the (b) epoxy resin in the conductive resin composition is not particularly limited. It is, for example, 0.1% by mass or more, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and for example, 10.0% by mass or less, preferably 9.0% by mass or less, more preferably 8.0% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition. If the content of the (b) epoxy resin is less than 0.1% by mass, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition, there are concerns that film formation is impossible, curing takes a long time, the dispersibility of the tin powder is reduced, and a uniform composition cannot be formed, etc. If the content exceeds 10.0% by mass, there are concerns that the conductivity is reduced and the volume resistivity is increased, etc.

[0021] The content of epoxy resins in the (b) epoxy resins, which have an epoxy equivalent of 400 g / eq or more and are solid or semi-solid at 25°C, is, relative to the total amount of the (b) epoxy resins as 100 mass%, for example, 10 mass% or more, preferably 25 mass% or more, and more preferably 50 mass% or more, and can be 100 mass% or less (only epoxy resins which have an epoxy equivalent of 400 g / eq or more and are solid or semi-solid at 25°C are used).

[0022] <(c) Dicarboxylic Acid Compound> The (c) dicarboxylic acid compound is, for example, R—(COOH) 2 (wherein R is hydrogen or an organic group having 1 to 50 carbon atoms. R may also contain an oxygen atom, a nitrogen atom, or a sulfur atom.) In the present invention, the (c) dicarboxylic acid compound includes a dicarboxylic acid compound having from 4 to 9 carbon atoms. Examples of the dicarboxylic acid compound having from 4 to 9 carbon atoms include one or more selected from the group consisting of succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, maleic acid, fumaric acid, citraconic acid, glutaconic acid, itaconic acid, mesaconic acid, 2-pentenedioic acid, methylenesuccinic acid, allylmalonic acid, hexadienedioic acid, terephthalic acid, isophthalic acid, o-phthalic acid, 1,4-cyclohexyldicarboxylic acid, malic acid, tartaric acid, 2,4-diethylglutaric acid, diglycolic acid, glutamic acid, aspartic acid, and thiodiglycolic acid. Among these, aliphatic dicarboxylic acid compounds having from 4 to 9 carbon atoms are preferred, aliphatic dicarboxylic acid compounds having from 5 to 9 carbon atoms are more preferred, and aliphatic dicarboxylic acid compounds having from 6 to 8 carbon atoms are even more preferred. In the aliphatic dicarboxylic acid having from 4 to 9 carbon atoms, the aliphatic group may be linear or branched.

[0023] In the present invention, the dicarboxylic acid compound (c) may contain a dicarboxylic acid other than a dicarboxylic acid compound having from 4 to 9 carbon atoms (such as a dicarboxylic acid compound having from 2 to 3 carbon atoms or a dicarboxylic acid compound having 10 or more carbon atoms). Examples of the dicarboxylic acid compound having from 2 to 3 carbon atoms include one or more selected from the group consisting of oxalic acid, malonic acid, etc. Examples of the dicarboxylic acid compound having 10 or more carbon atoms include sebacic acid, undecanedioic acid, dodecanedioic acid, tridecanedioic acid, tetradecanedioic acid, pentadecanedioic acid, hexadecanedioic acid, heptadecanedioic acid, octadecanedioic acid, eicosane diacid, nonadecanedioic acid, docosane diacid, eicosadienedioic acid, isoeicosane diacid, isodocosane diacid, isodocosadienedioic acid, butyloctanedioic acid, 2-methylazelaic acid, dimethylmethylcellulose, methylcellulose, methylcellulose diol ... and at least one selected from the group consisting of methyltrimethyldimethoxycarbonyltridecane dicarboxylic acid, ...

[0024] (c) By using a dicarboxylic acid compound containing a dicarboxylic acid compound having 4 to 9 carbon atoms as the dicarboxylic acid compound, it is possible to improve the dispersibility of the tin powder, increase the content of the tin powder, and increase the conductivity.

[0025] The content of the (c) dicarboxylic acid compound in the conductive resin composition is not particularly limited. It is, for example, 0.1% by mass or more, preferably 0.3% by mass or more, more preferably 0.5% by mass or more, and for example, 4.0% by mass or less, preferably 3.5% by mass or less, more preferably 3.0% by mass or less, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition. If the content of the (c) dicarboxylic acid compound is less than 0.1% by mass, based on 100% by mass of the total amount of components other than the solvent in the conductive resin composition, there are concerns that film formation is impossible, curing takes a long time, the dispersibility of the tin powder is reduced, and a uniform composition cannot be formed, etc. If the content exceeds 4.0% by mass, there are concerns that the conductivity is reduced, the volume resistivity is increased, and storage stability is reduced, etc.

[0026] The content of the dicarboxylic acid compounds having 4 to 9 carbon atoms in the (c) dicarboxylic acid compounds is, for example, 10% by mass or more, preferably 25% by mass or more, and more preferably 50% by mass or more, relative to the total amount of the (c) dicarboxylic acid compounds being 100% by mass, and can be 100% by mass or less (only dicarboxylic acid compounds having 4 to 9 carbon atoms are used).

[0027] <(d) Thiol-Based Compound> The conductive resin composition of the present invention may further contain (d) a thiol-based compound. The (d) thiol-based compound can act as a curing agent for the (b) epoxy resin in the conductive resin composition, and can cause the curing of the conductive resin composition to proceed more quickly and reliably.

[0028] The (d) thiol compound may be one or more compounds having one or more thiol groups in the molecule that can react with an epoxy group. Preferably, one or more compounds having two or more thiol groups. The (d) thiol compound is more preferably one having 2 to 6 (difunctional to hexafunctional) thiol groups in one molecule, and even more preferably one having 3 to 6 (trifunctional to hexafunctional) thiol groups in one molecule.

[0029] (d) Examples of thiol compounds include trimethylolpropane tris(3-mercaptopropionate) (abbreviation: TMTP), pentaerythritol tetrakis(3-mercaptopropionate) (abbreviation: PEMP), dipentaerythritol hexakis(3-mercaptopropionate) (abbreviation: DPMP), tris-[(3-mercaptopropionyloxy)-ethyl]-isocyanurate (abbreviation: TEMPIC), tris(3-mercaptopropyl)isocyanurate (abbreviation: TMPIC), ethylene glycol bisthioglycolate (abbreviation: EGTG), trimethylolpropane tristhioglycolate (abbreviation: TMTG), pentaerythritol tetrakisthioglycolate (abbreviation: PETG), and pentaerythritol tetrakis(3-mercaptobutylate). 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptobutyrate) (abbreviation: TPMB), trimethylolethane tris(3-mercaptobutyrate) (abbreviation: TEMB), 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril, 1,3,4,6-tetrakis(2-mercaptopropyl)glycoluril, 4,4'-isopropylidenebis[(3-mercaptopropoxy)benzene], thiocyanuric acid (1,3,5-triazine-2,4,6-trithiol), polysulfide polymers having a thiol group, and the like can be mentioned as one or more selected from the group consisting of 1,4-bis(3-mercaptobutyryloxy)butane, 1,3,5-tris(3-mercaptobutyryloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, trimethylolpropane tris(3-mercaptobutyrate) (abbreviation: TPMB), trimethylolethane tris(3-mercaptobutyrate) (abbreviation: TEMB), 1,3,4,6-tetrakis(2-mercaptoethyl)glycoluril, 1,3,4,6-tetrakis(2-mercaptopropyl)glycoluril, 4,4'-isopropylidenebis[(3-mercaptopropoxy)benzene], thiocyanuric acid (1,3,5-triazine-2,4,6-trithiol), polysulfide polymers having a thiol group, and the like.

[0030] Specific examples include thiol compounds manufactured by SC Organic Chemical Industry Co., Ltd. (TMMP-LV, PEMP-LV, DPMP, TEMPIC, PEMP, etc.), thiol compounds manufactured by Toray Fine Chemical Co., Ltd. (QE-340M, LP-3, LP-55, LP-31, etc.), thiol compounds manufactured by Shikoku Chemical Industry Co., Ltd. (TS-G, C3TS-G, etc.), thiol compounds manufactured by Resonac Corporation (PE-1, BD-1, NR-1, TPMB, TEMB, etc.), thiol compounds manufactured by Yodo Chemical Industry Co., Ltd. (OTG, EGTG, TMTG, PETG, 3-MPA, TMTP, PETP, etc.), and thiol compounds manufactured by Sakai Chemical Industry Co., Ltd. (TEMP, PEMP, TEMPIC, DPMP, etc.).

[0031] The content of the (d) thiol compound in the conductive resin composition is not particularly limited. In the present invention, the conductive resin composition can be cured without using a (d) thiol compound. When a (d) thiol compound is contained, the amount of thiol groups (—SH groups) in the (d) thiol compound is preferably, for example, 0.05 equivalents or more, preferably 0.10 equivalents or more, more preferably 0.15 equivalents or more, and for example, 4.00 equivalents or less, preferably 3.50 equivalents or less, more preferably 1.50 equivalents or less, relative to 1 equivalent of epoxy groups in the epoxy resin. If the content of the (d) thiol compound exceeds 4.00 equivalents, the coating film may be poorly cured due to the influence of excess unreacted curing agent, resulting in a decrease in coating film hardness. Furthermore, when the thiol compound (d) is contained, the amount thereof is, for example, 1.0 part by mass or more, preferably 1.5 parts by mass or more, and more preferably 2.0 parts by mass or more, relative to 100 parts by mass of the epoxy resin, and can be, for example, 250 parts by mass or less, preferably 200 parts by mass or less, and more preferably 180 parts by mass or less. If the amount of the thiol compound (d) relative to 100 parts by mass of the epoxy resin exceeds 250 parts by mass, the conductive resin composition may not become solid.

[0032] <(e) Solvent> The conductive resin composition of the present invention may further contain (e) a solvent. This can improve the fluidity of the conductive resin composition and contribute to improving workability. Furthermore, by mixing the conductive resin composition with a solvent, a conductive resin paste, a conductive material, a conductive adhesive, or a circuit connecting material can be produced.

[0033] The solvent may be any one or more selected from the group consisting of water and various organic solvents. Examples of the organic solvent include alcohol-based solvents and alcohol ether-based solvents such as ethyl alcohol, propyl alcohol, butyl alcohol, pentyl alcohol, hexyl alcohol, heptyl alcohol, octyl alcohol, nonyl alcohol, decyl alcohol, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monobutyl ether, diethylene glycol monobutyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, propylene glycol monobutyl ether, methyl methoxybutanol, α-terpineol, β-terpineol, hexylene glycol, benzyl alcohol, 2-phenylethyl alcohol, isopalmityl alcohol, isostearyl alcohol, lauryl alcohol, ethylene glycol, propylene glycol, and glycerin; acetone, methyl ethyl ketone, methyl ... ketone solvents such as ethyl isobutyl ketone, cyclohexanone, diacetone alcohol (4-hydroxy-4-methyl-2-pentanone), 2-octanone, isophorone (3,5,5-trimethyl-2-cyclohexen-1-one) or diisobutyl ketone (2,6-dimethyl-4-heptanone); ethyl acetate, butyl acetate, diethyl phthalate, dibutyl phthalate, acetoxyethane, methyl butyrate, methyl hexanoate, methyl octanoate, methyl decanoate, methyl cellosolve acetate, ethylene glycol monobutyl ester-based solvents such as ethylene glycol ether acetate, propylene glycol monomethyl ether acetate, and 1,2-diacetoxyethane; ether-based solvents such as tetrahydrofuran, dimethyl ether, diethyl ether, dipropyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, propylene glycol dimethyl ether, ethoxyethyl ether, 1,2-bis(2-diethoxy)ethane, and 1,2-bis(2-methoxyethoxy)ethane;Examples of the solvent include one or more solvents selected from the group consisting of ester ethers such as 2-(2-butoxyethoxy)ethane acetate, ether alcohol solvents such as 2-(2-methoxyethoxy)ethanol, hydrocarbon solvents such as benzene, toluene, xylene, n-paraffin, isoparaffin, dodecylbenzene, turpentine oil, kerosene, and light oil, nitrile solvents such as acetonitrile and propionitrile, nitrogen-containing polar solvents such as dimethylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone, and silicone oil solvents. Among these, preferred is one or more solvents selected from the group consisting of alcohol solvents, alcohol ether solvents, ether solvents, ester solvents, and ketone solvents, more preferred is one or more solvents selected from the group consisting of alcohol ether solvents, ether solvents, ester solvents, and ketone solvents, and even more preferred is one or more solvents selected from the group consisting of alcohol ether solvents, ether solvents, and ester solvents. When an organic solvent is used, the amount used is not particularly limited, and may be appropriately adjusted so that the viscosity of the conductive resin composition is such that it can be appropriately applied or printed on a substrate and / or can be appropriately impregnated into a porous body.

[0034] <(f) Other Components> In addition to the components (a) to (e), the conductive resin composition of the present invention may contain, as necessary, one or more additives as "(f) other components" selected from the group consisting of organic acid compounds, epoxy resin curing agents, epoxy resin curing accelerators, conductive powders other than tin powder, adhesion promoters, viscoelasticity modifiers, wetting and dispersing agents, reactive diluents, resins other than epoxy resins, pigments, fillers, antioxidants, corrosion inhibitors, antifoaming agents, coupling agents, anti-settling agents, leveling agents, heavy metal deactivators, gap adjusters, and the like.

[0035] (Organic Acid Compound) The organic acid compound is an organic acid compound other than a dicarboxylic acid compound, for example, R—X n(wherein R is hydrogen or an organic group having 1 to 50 carbon atoms, X is an acid group and a plurality of Xs may be different from each other, and n is an integer of 1 or more). Examples of the acid group represented by X include a carboxyl group (-COOH), a sulfonic acid group (-SO 3 H), phosphate group (-PO 4 H 2 Examples of the organic acid compound include one or more compounds selected from the group consisting of organic carboxylic acid compounds other than dicarboxylic acid compounds, organic sulfonic acid compounds, organic phosphonic acid compounds, etc. Preferably, the organic carboxylic acid compound is an organic carboxylic acid compound other than dicarboxylic acid compounds.

[0036] {Organic Carboxylic Acid Compound} The organic carboxylic acid compound is not particularly limited as long as it is a compound having one or three or more carboxyl groups (—COOH) in its molecular structure and having 1 to 50 carbon atoms. Examples of organic carboxylic acid compounds include formic acid, acetic acid, propionic acid, butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, octylic acid, caproic acid, enanthic acid, caprylic acid, pelargonic acid, capric acid, lauric acid, myristic acid, pentadecylic acid, palmitic acid, margaric acid, stearic acid, 12-hydroxystearic acid, ricinoleic acid, oleic acid, vaccenic acid, linoleic acid, linolenic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, montanic acid, melissic acid, behenic acid, arachidonic acid, eicosapentaenoic acid, docosahexaenoic acid, lactic acid, gluconic acid, citric acid, ascorbic acid, abietic acid, dimethylolpropionic acid, dimethylolbutanoic acid, dimethylolbutyric acid, dimethylolvaleric acid, trimethylolpropanoic acid, trimethylolpropanoic acid, methylolpropionic acid, methylolbutanoic acid, dimethylolbutyric acid, dimethylolvaleric acid, trimethylolpropanoic acid, methylolpropionic acid, methylolpropionic acid, methylolpropionic acid, methylolpropionic acid, methylolpropionic acid, methylolbutanoic acid, methylolbutyric acid, dimethylolvaleric acid, trimethylolpropanoic acid, methylolpropionic ... Examples of the carboxylic acid include one or more selected from the group consisting of methylol butanoic acid, benzoic acid, salicylic acid, pyruvic acid, paramethylbenzoic acid, toluic acid, 4-ethylbenzoic acid, 4-propylbenzoic acid, 2-methylpropanoic acid, isopentanoic acid, 2-ethylhexanoic acid, acrylic acid, methacrylic acid, propiolic acid, crotonic acid, 2-ethyl-2-butenoic acid, hexanetricarboxylic acid, cyclohexylcarboxylic acid, ethylenediaminetetraacetic acid, trimellitic acid, pyromellitic acid, monomethyl glutarate, glycolic acid, isoleucine, leucine, lysine, methionine, phenylalanine, threonine, tryptophan, valine, histidine, tyrosine, cysteine, asparagine, serine, glutamine, proline, glycine, alanine, arginine, and the like.

[0037] {Organic sulfonic acid compound} An organic sulfonic acid compound has a sulfonic acid group (-SO ) in its molecular structure. 3H), there is no particular limitation. For example, benzenesulfonic acid, n-butylbenzenesulfonic acid, n-octylbenzenesulfonic acid, n-dodecylbenzenesulfonic acid, pentadecylbenzenesulfonic acid, 2,5-dimethylbenzenesulfonic acid, p-chlorobenzenesulfonic acid, 2,5-dichlorobenzenesulfonic acid, p-phenolsulfonic acid, cumenesulfonic acid, xylenesulfonic acid, o-cresolsulfonic acid, m-cresolsulfonic acid, p-cresolsulfonic acid, p-toluenesulfonic acid, 2-naphthalenesulfonic acid, 1-naphthalenesulfonic acid, styrenesulfonic acid, 4,4-biphenyldisulfonic acid, anthraquinone-2-sulfonic acid, m-benzenedisulfonic acid, Examples of the sulfonic acid include aromatic sulfonic acid compounds such as aniline-2,4-disulfonic acid, anthraquinone-1,5-disulfonic acid, and polystyrene sulfonic acid; aliphatic sulfonic acid compounds such as methanesulfonic acid, ethanesulfonic acid, 1-propanesulfonic acid, n-octylsulfonic acid, pentadecylsulfonic acid, trifluoromethanesulfonic acid, trichloromethanesulfonic acid, 1,2-ethanedisulfonic acid, 1,3-propanedisulfonic acid, aminomethanesulfonic acid, and 2-aminoethanesulfonic acid; and alicyclic sulfonic acid compounds such as cyclopentanesulfonic acid, cyclohexanesulfonic acid, and 3-cyclohexylaminopropanesulfonic acid. Preferably, examples of the sulfonic acid include benzenesulfonic acid, dodecylbenzenesulfonic acid, methanesulfonic acid, p-phenolsulfonic acid, p-toluenesulfonic acid, and (poly)styrenesulfonic acid.

[0038] {Organic Phosphonic Acid Compound} An organic phosphonic acid compound has a phosphonic acid group (-PO) in the molecular structure. 3 H 2) is not particularly limited as long as it is a compound having one or more of the following. For example, 1-hydroxyethylidene-1,1-diphosphonic acid, 1-hydroxypropylidene-1,1-diphosphonic acid, 1-hydroxybutylidene-1,1-diphosphonic acid, aminotrimethylenephosphonic acid, methyldiphosphonic acid, nitrotrimethylenephosphonic acid, ethylenediaminetetramethylenephosphonic acid, ethylenediaminebismethylenephosphonic acid, hexamethylenediaminetetramethylenephosphonic acid, diethylenetriaminepentamethylenephosphonic acid, cyclohexanediaminetetramethylenephosphonic acid, and at least one selected from the group consisting of phosphonic acid, carboxyethylphosphonic acid, phosphonoacetic acid, 2-phosphonobutane-1,2,4-tricarboxylic acid, 2,3-dicarboxypropane-1,1-diphosphonic acid, phosphonobutyric acid, phosphonopropionic acid, sulfonylmethylphosphonic acid, N-carboxymethyl-N,N-dimethylenephosphonic acid, N,N-dicarboxymethyl-N-methylenephosphonic acid, 2-ethylhexyl acid phosphate, stearyl acid phosphate, benzenephosphonic acid, and the like.

[0039] Organic phosphonic acid compounds have a phosphate group (-PO 4 H 2) may also be used. As surfactants having a phosphate group, those having a polyoxyethylene group or a phenyl group in the molecular structure are preferred. For example, one or more surfactants selected from the group consisting of polyoxyethylene alkyl phenyl ether phosphate, polyoxyethylene alkyl ether phosphate, dipolyoxypropylene lauryl ether phosphate, dipolyoxyethylene oleyl ether phosphate, dipolyoxyethylene oxypropylene lauryl ether phosphate, dipolyoxypropylene oleyl ether phosphate, ammonium lauryl phosphate, ammonium octyl ether phosphate, ammonium cetyl ether phosphate, polyoxyethylene lauryl ether phosphate, polyoxyethylene oxypropylene lauryl ether phosphate, polyoxypropylene lauryl ether phosphate, polyoxyethylene tristyryl phenyl ether phosphate, polyoxyethylene oxypropylene tristyryl phenyl ether phosphate, polyoxypropylene tristyryl phenyl ether phosphate, polyoxypropylene tristyryl phenyl ether phosphate, and the like may be used. As surfactants having a phosphate group, one or more surfactants selected from the group consisting of commercially available products such as Phosphanol (trade name) manufactured by Toho Chemical Industry Co., Ltd. and DISPERBYK (trade name) manufactured by BYK Japan KK may be used.

[0040] (Epoxy Resin Curing Agent) The conductive resin composition of the present invention may contain (d) an epoxy resin curing agent other than a thiol-based compound. This improves the curability of the conductive resin composition, contributing to improvements in bonding strength, etc. Examples of epoxy resin curing agents include amine-based curing agents, acid anhydride-based curing agents, and phenol-based curing agents. These may be used alone or in combination of two or more. From the viewpoint of more effectively improving workability, handleability, etc., the conductive resin composition of the present invention preferably contains a curing agent that is liquid at 20°C.

[0041] {Amine-Based Curing Agent} Examples of the amine-based curing agent include diethylenetriamine, triethylenetetramine, diethylaminopropylamine, menthanediamine, isophoronediamine, bis[4-amino-3-methyldicyclohexyl]methane, diaminodicyclohexylmethane, bis(aminomethyl)cyclohexane, m-xylylenediamine, metaphenylenediamine, diaminodiphenylmethane, diaminodiethyldiphenylmethane, and modified polyamines and polyamidoamines obtained by modifying these by epoxy adduct, Michael addition, Mannich reaction, etc. These may be used alone or in combination of two or more.

[0042] {Acid Anhydride Curing Agent} The acid anhydride curing agent is not particularly limited as long as it is a compound having one or more carboxylic acid anhydride groups (—C(═O)—O—C(═O)—) in its molecular structure. The acid anhydride curing agent is obtained by intermolecular dehydration of two organic carboxylic acid molecules and / or intramolecular dehydration of one organic carboxylic acid molecule. In the present invention, for example, among the organic carboxylic acids, one or more selected from the group consisting of those obtained by intermolecular dehydration of an organic monocarboxylic acid and those obtained by intramolecular dehydration and / or intermolecular dehydration of an organic polycarboxylic acid may be used. For example, one or more selected from the group consisting of aliphatic monocarboxylic acid anhydrides, aliphatic polycarboxylic acid anhydrides, alicyclic polycarboxylic acid anhydrides, aromatic polycarboxylic acid anhydrides, etc. may be used. Preferably, one or more selected from the group consisting of acetic anhydride, glutaric anhydride, propionic anhydride, oxalic anhydride, maleic anhydride, phthalic anhydride, benzoic anhydride, succinic anhydride, 2-methylsuccinic anhydride, trimellitic anhydride, pyromellitic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, (poly)adipic anhydride, (poly)azelaic anhydride, (poly)sebacic anhydride, norbornene-2,3-dicarboxylic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride, and the like.

[0043] In the present invention, the following structural formula (1) (In structural formula (1), R 1 is a linear or branched hydrocarbon group having 10 or more carbon atoms. One or more polyacid polyanhydrides represented by the following formula may be used as the acid anhydride curing agent. Such polyacid polyanhydrides are obtained by an intermolecular dehydration condensation reaction of long-chain aliphatic dicarboxylic acids. Examples include SL-12AH, SL-20AH, SB-20AH, IPU-22AH, and ST-2PAH manufactured by Okamura Oil Mills. In particular, SB-20AH, IPU-22AH, and ST-2PAH, which are liquid at 25°C, are preferably used.

[0044] {Phenol-Based Curing Agent} Examples of phenol-based curing agents include compounds having one or more, preferably two or more, phenolic hydroxyl groups in the molecule that can react with epoxy groups. Examples include bisphenols such as bisphenol A, bisphenol B, bisphenol F, bisphenol AD, and bisphenol S; biphenols such as biphenol and tetramethylbiphenol; phenols such as hydroxyphenol and bis(4-hydroxyphenyl)ether; alkylphenols; phenol novolacs such as 2,6-bis[(2-hydroxyphenyl)methyl]-phenol and phenol biphenylene novolac (biphenyl aralkylphenol); cresol novolacs such as o-cresol novolac, m-cresol novolac, and p-cresol novolac; and phenol resins. These may be used alone or in combination of two or more.

[0045] {Epoxy Resin Curing Agent Content} The content of the epoxy resin curing agent in the conductive resin composition of the present invention is not particularly limited. In the present invention, the conductive resin composition can be cured without using a curing agent. When a curing agent is contained, the amount of groups reactive with the epoxy groups in the curing agent (e.g., hydroxyl groups, amino groups, and carboxyl groups (formed from acid anhydride groups)) is, for example, 0.7 equivalents or more, preferably 0.8 equivalents or more, and more preferably 0.9 equivalents or more, and can be, for example, 1.3 equivalents or less, preferably 1.2 equivalents or less, and more preferably 1.1 equivalents or less, relative to 1 equivalent of the epoxy groups in the epoxy resin. If the amount exceeds 1.3 equivalents, the coating film may be poorly cured due to the influence of excess unreacted curing agent, resulting in a decrease in coating hardness. A curing agent content of 1.0 equivalent is most preferred.

[0046] (Epoxy Resin Curing Accelerator) The conductive resin composition of the present invention may contain a curing accelerator (curing catalyst) for accelerating the curing of the epoxy resin. The curing accelerator is not particularly limited, but examples thereof include amine-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, and phosphonium-based curing accelerators. These may be used alone or in combination of two or more. For example, ethyleneamines such as ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, and pentaethylenehexamine; aliphatic tertiary amines such as triethylamine, tripropylamine, tributylamine, dimethylbutylamine, dimethylpentylamine, and dimethylcyclohexylamine; dimethylbenzylamine, dimethylaminomethylphenol, dimethylamino-p-cresol, piperidine, α-picoline, pyridine, 2,4,6-tris(dimethylaminomethyl)phenol, 3,4,5-tris(dimethylaminomethyl)phenol, 2-methylimidazole, 2-ethyl-4-methylimidazole, 2-undecylimidazole, 2-phenylimidazole, 1-benzyl-2-methylimidazole, 1-cyanoethyl-2-methylimidazole; Examples of the compound include 1-cyanoethyl-2-ethyl-4-methylimidazole, N-aminoethylpiperazine, 1,3,6-trisaminomethylhexane, m-xylenediamine, p-xylenediamine, N-(2-aminoethyl)piperazine, m-phenylenediamine, p-phenylenediamine, diaminophenylmethane, methylenedianiline, 2,4-toluenediamine, 2,4-diaminoanisole, 2,4-toluenediamine, 2,4-diaminodiphenylamine, 4,4'-methylenedianiline, 1,3-diaminocyclohexane, 3,9-bis(3-aminopropyl)-2,4,8,10-tetrapyro[5.5]undecane, 1,8-diazabicyclo[5.4.0]undecene-7, polyamines, polyamidoamines, polyamides, modified polyamines, modified polyamidoamines, modified polyamides, etc. These compounds may be used alone or in combination of two or more.

[0047] (Conductive Powder Other than Tin Powder) The conductive resin composition of the present invention may contain a conductive powder other than tin powder. Examples of such conductive powders include lead-free solder powder, gold powder, silver powder, copper powder, silver-coated copper powder, silver-coated silica powder, silver-coated nickel powder, resin-core metal-coated fine particles, nickel powder, and conductive carbon powder. For example, the lead-free solder powder is not particularly limited as long as it does not contain more than the amount of lead that is unavoidably contained due to the impact on workers, users, the environment, etc. The melting point of the lead-free solder powder is preferably 300°C or less, more preferably 240°C or less, and even more preferably 50 to 240°C. If the melting point of the lead-free solder powder exceeds 300°C, there is a risk of thermal destruction or thermal degradation of connected components such as circuit boards and electronic components. If the melting point is less than 50°C, there is a risk of reduced mechanical strength and reduced reliability of the conductive connection.

[0048] (Adhesion Imparting Agent) The conductive resin composition of the present invention may contain an adhesion imparting agent. This can improve the adhesion to the substrate when the conductive resin composition is applied to the substrate. Examples of adhesion imparting agents include triazole compounds, thiazole compounds, triazine compounds, porphyrin compounds, polymers having functional groups (carboxylic acid groups, amino groups, hydroxyl groups, etc.) and salts thereof. These may be used alone or in combination of two or more. Examples of adhesion imparting agents include the BYK series (4509, 4510, 4512, etc.) manufactured by BYK Japan.

[0049] (Viscoelasticity modifier) ​​The conductive resin composition of the present invention may contain a viscoelasticity modifier (rheology control agent). This can adjust the viscoelasticity (rheology) of the conductive resin composition, contributing to improved workability, etc. Examples of the viscoelasticity modifier (rheology control agent) include polyamide-based, aminoplast-based, polycarboxylic acid-based, urethane-based, cellulose-based, and inorganic layered compound-based viscoelasticity modifiers (rheology control agents). For example, RHEOBYK series manufactured by BYK Japan (H370, H400, H600, H600VF, 100, 405, 410, 411, 415, 430, 431, 440, 7410ET, etc.); DISPARLON series manufactured by Kusumoto Chemicals Co., Ltd. (AQ-600, AQH-800, 3600N, 3900EF, etc.); SN Thickener series manufactured by San Nopco Ltd. (613, 617, 618, 630, 634, 636, 621N, 623N, etc.); ADEKA Adekanol series manufactured by ADEKA Corporation (UH-814N, UH-752, UH-750, UH-462, etc.); HEC Daicel series manufactured by Daicel Corporation (SP600N, etc.); BENTONE manufactured by Elementis Japan Co., Ltd. These may be used alone or in combination of two or more.

[0050] (Wetting and Dispersing Agent) The conductive resin composition of the present invention may contain a dispersing agent, if necessary, to prevent aggregation of the tin powder. Specific examples of wetting and dispersing agents include the Solsperse series (9000, 12000, 17000, 20000, 21000, 24000, 26000, 27000, 28000, 32000, 35100, 54000, etc.) manufactured by Lubrizol Japan Corporation, and the EFKA series (4008, 4009, 4010, 4015, 4046, 4047, 4060, 4080, 7462, 4020, 4050, 4055, 4400, 4401, 4402, 4403, 4300, 4330, 4340, 6220, 6225, 6700, 6780, 6782, 8503, etc.) manufactured by EFKA Additives Co., Ltd. ), Ajinomoto Fine-Techno Co., Ltd. Ajisper series (PA111, PB711, PB821, PB822, PN411, etc.), BYK Japan DISPERBYK series (101, 106, 108, 116, 130, 140, 145, 161, 163, 166, 168, 171, 180, 192, 2000, 2001, 2020, 2025, 2070, 2152, 2155, 2164, 220S, 300, 320, 340, 378, 380N, 410, 425, 430, etc. These may be used alone or in combination of two or more.

[0051] (Reactive Diluent) The curable resin composition of the present invention may contain a reactive diluent for adjusting the viscosity or curability of the conductive resin composition. The reactive diluent is not particularly limited, and examples thereof include one or more compounds having one epoxy group in the molecular structure, compounds having one or more oxetane groups in the molecular structure, etc. Examples of the reactive diluent include glycidyl phenyl ether, glycidyl lauryl ether, 2-phenylphenol glycidyl ether, allyl glycidyl ether, 4-tert-butylphenyl glycidyl ether, N-glycidyl phthalimide, 2-ethylhexyl glycidyl ether, 2-ethylhexyl glycidyl ether, YED111N, YED111AN, and YED188 manufactured by Mitsubishi Chemical Corporation, ADEKA GLYCIROL ED-502 and ADEKA GLYCIROL ED-502S manufactured by ADEKA Corporation, Examples of such an agent include ADEKA GLYCILOR ED-509E, ADEKA GLYCILOR ED-509S, ADEKA GLYCILOR ED-529, DENACOL EX-145, DENACOL EX-171, and DENACOL EX-192 manufactured by Nagase ChemteX Corporation, EPOLYTE M-1230 and EPOLYTE 100MF manufactured by Kyoeisha Chemical Co., Ltd., ARON OXETANE OXT-101, ARON OXETANE OXT-212, ARON OXT-121, and ARON OXT-221 manufactured by Toagosei Co., Ltd., and ETERNACOLL EHO, ETERNACOLL HBOX, ETERNACOLL OXMA, and ETERNACOLL OXBP manufactured by UBE Co., Ltd. One of these may be used alone, or two or more may be used in combination.

[0052] (Resins Other Than Epoxy Resins) The conductive resin composition of the present invention may contain a resin other than an epoxy resin. Such a resin may be either a thermoplastic resin or a thermosetting resin, and one or more types may be used alone or in combination. Examples of the thermoplastic resin include one or more types selected from the group consisting of polyvinyl acetal resins, acrylic resins, polyester resins, phenoxy resins, polyimide resins, polyolefin resins, thermoplastic polyurethane resins, polyamide resins, polycarbonate resins, polyphenylene ether resins, polyvinyl ether resins, polyvinyl alcohol resins, polyvinyl acetate resins, ionomer resins, and block urethane resins. Examples of the thermosetting resin include one or more types selected from the group consisting of resol-type phenolic resins, polyimide resins, xylene resins, polyurethane resins, melamine resins, urea resins, and furan resins. In the present invention, the resin preferably contains one or more selected from the group consisting of polyvinyl acetal resins, resol-type phenolic resins, acrylic resins, polyester resins, phenoxy resins, polyimide resins, and xylene resins. Among these, polyvinyl acetal resins are preferably used from the viewpoints of film formation state, connection reliability, adhesion to substrates, etc.

[0053] (Coupling Agent) The epoxy resin composition of the present invention may contain a coupling agent. This can improve the short-term heating bonding strength of the epoxy resin composition. Examples of coupling agents include silane coupling agents, titanium coupling agents, aluminum coupling agents, and zirconium coupling agents. Examples of silane coupling agents include amino group-containing silane compounds such as aminoethylaminopropyltrimethoxysilane, aminoethylaminopropylmethyldimethoxysilane, and aminoethylaminopropylmethylmethoxysilane; vinyl group-containing silane compounds such as vinyltrimethoxysilane; epoxy group-containing silane compounds such as γ-glycidoxypropyltrimethoxysilane; (meth)acryloyl group-containing silane compounds such as γ-methacryloxypropyltrimethoxysilane; mercaptosilanes such as γ-mercaptopropyltrimethoxysilane; and isocyanate group-containing silane compounds such as γ-isocyanatopropyltrimethoxysilane. Examples of titanium coupling agents include tetraisopropyl titanate, tetra-normal butyl titanate, butyl titanate, tetraoctyl titanate, titanium acetylacetonate, titanium tetraacetylacetonate, titanium ethylacetoacetate, dodecylbenzenesulfonic acid titanium compound, titanium octylene glycolate, titanium ethylacetoacetate, titanium lactate ammonium salt, titanium lactate, titanium triethanolamine, tetraisopropyl titanate, tetratertiary butyl titanate, tetrastearyl titanate, titanium acetylacetonate, titanium octylene glycolate, titanium isostearate, titanium diethanolamine, titanium aminoethylaminoethanolate, titanium oligomer, etc. Examples of aluminum coupling agents include aluminate compounds having an alkoxide group such as alkylacetoacetate aluminum diisopropylate, and aluminate compounds having an acetylacetonate group such as aluminum trisacetylacetonate.Examples of zirconium coupling agents include tetra-n-propoxyzirconium, tetra-butoxyzirconium, zirconium tetraacetylacetonate, zirconium dibutoxybis(acetylacetonate), zirconium tributoxyethylacetoacetate, zirconium butoxyacetylacetonate bis(ethylacetoacetate), tetrakis(2,4-pentanedionate)zirconium, etc. One type of coupling agent may be used alone, or two or more types may be used.

[0054] <Properties of Conductive Resin Composition> The conductive resin composition of the present invention may be in any form, such as powder, solid, paste, liquid (varnish), etc. When used as a conductive material, conductive adhesive, or circuit connecting material, it is suitable for the composition to be in a paste or liquid (varnish) form at room temperature (25°C).

[0055] <Characteristics of Conductive Resin Composition> The conductive resin composition of the present invention has excellent conductivity. For example, the conductive resin composition is cast or applied onto a release substrate, dried, and then peeled off to obtain a conductive film having a volume resistivity of 3.0 × 10 -4 The volume resistivity of the conductive film is preferably less than 2.0×10 -4 The volume resistivity is less than Ω·cm. Here, the volume resistivity is obtained by the method described in the Examples. The conductive resin composition of the present invention has excellent adhesion to various substrates. For example, it has excellent adhesion to glass, metal, or plastic (e.g., polyester, etc.). The conductive resin composition of the present invention does not solidify, skin on the surface, or separate from the liquid, whether it is stored at room temperature (25°C) for 24 hours (storage at room temperature (25°C) for 24 hours) or stored in a refrigerator (4°C) for 1 week (storage refrigerated (4°C) for 1 week), and there is little increase in viscosity before and after storage at room temperature for 24 hours and storage in the refrigerator for 1 week, thereby exhibiting excellent storage stability.

[0056] <Method for Preparing Conductive Resin Composition> When preparing the conductive resin composition of the present invention, tin powder, a specific epoxy resin, and a specific dicarboxylic acid compound are used as essential components, and a thiol compound, a solvent, and other components are added to a mixing vessel in any order and mixed. For mixing, a mixing method using, for example, a centrifugal mixer, a ball mill, a roll mill, a bead mill, a planetary mixer, a tumbler, a stirrer, a mixer, a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, a V-type blender, a Nauta mixer, a Banbury mixer, a kneading roll, or a single-screw or twin-screw extruder is appropriately used.

[0057] The temperature at which the conductive resin composition is prepared (the temperature at which each component is mixed) is not particularly limited. Heating or the like can be performed as necessary, and the conductive resin composition can be prepared at, for example, 10 to 100°C. The atmosphere at which the conductive resin composition is prepared is not particularly limited. Preparation can be performed in air or in an inert atmosphere.

[0058] <Uses of Conductive Resin Composition> The conductive resin composition of the present invention is used in the manufacture of a conductive object. The conductive object may contain other components in addition to the conductive resin composition. Examples of the conductive object include one or more selected from the group consisting of conductive materials, circuit connection materials, conductive pastes, conductive films, conductive fibers, conductive paints, conductive materials for semiconductor packages, conductive materials for microelectronic devices, antistatic materials, electromagnetic wave shielding materials, conductive adhesives (such as die attach adhesives), die attach pastes, actuators, sensors, and conductive resin molded articles.

[0059] For example, by using a solvent as a component of the conductive resin composition, conductive materials, circuit connection materials, conductive pastes, conductive paints, conductive adhesives, etc. can be produced. The viscosity is not particularly limited, and can be anything from a low-viscosity varnish to a high-viscosity paste, etc., depending on the application. For example, a conductive resin composition containing a solvent, etc., as needed, can be applied to various substrates by casting, dipping, bar coating, dispenser coating, roll coating, gravure coating, screen printing, flexographic printing, spray coating, spin coating, inkjet printing, etc., and then heated and dried at a temperature of 300°C or less to form a conductive film. The atmosphere during drying can be one or more selected from the group consisting of air, inert gas, vacuum, reduced pressure, etc. In particular, from the viewpoint of suppressing deterioration of the conductive film (preventing oxidation of tin powder, etc.), an inert gas atmosphere such as nitrogen or argon is preferred.

[0060] The conductive resin composition of the present invention can be molded by a molding method such as extrusion molding, injection molding, compression molding, etc. and used as a molded article. Examples of the molded article include electronic device parts, automobile parts, mechanical parts, food containers, films, sheets, fibers, etc.

[0061] [Conductive Film] The conductive film of the present invention can be formed from the conductive resin composition. -4 The volume resistivity of the conductive film is preferably less than 2.0×10 -4 less than Ω cm, more preferably less than 1.0 × 10 -4 The conductive film of the present invention has a resistivity of less than 1.0×10 -4 Less than Ω cm (10 -5 It is also possible to obtain a volume resistivity of the order of Ω·cm, which is comparable to that of a conductive film formed from a silver paste. Here, the volume resistivity is obtained by the method described in the examples.

[0062] The method for forming a conductive film from the conductive resin composition is not particularly limited. For example, the conductive resin composition may be made to contain a solvent, and the conductive film may be coated or printed on any substrate and dried to form a conductive film. Alternatively, the conductive film may be obtained by casting or coating the conductive resin composition on a peelable substrate, drying, or the like, and then peeling it off. The conditions for forming the conductive film are not particularly limited and can be appropriately set depending on the substrate, etc. The temperature during drying after coating the conductive resin composition is, for example, 50°C or higher, preferably 90°C or higher, and, for example, 250°C or lower, preferably 220°C or lower. The drying time is, for example, 5 minutes or higher, preferably 7 minutes or higher, and, for example, 300 minutes or lower, preferably 200 minutes or lower. In the present invention, when forming a conductive film, either the wet film thickness and / or the dry film thickness can be adjusted depending on the application, coating / printing method, etc. The wet film thickness of the conductive film (wet film thickness of the conductive resin composition) is not particularly limited and can be appropriately adjusted depending on the application, etc. For example, it is 5 μm or more, preferably 10 μm or more, and for example, 1000 μm or less, preferably 500 μm or less. The dry film thickness of the conductive film is not particularly limited and can be appropriately adjusted depending on the application, etc. For example, it is 1 μm or more, preferably 5 μm or more, and for example, 1000 μm or less, preferably 500 μm or less.

[0063] [Conductive Material] The conductive material of the present invention contains the conductive resin composition. For example, the conductive material can be obtained by dissolving and / or dispersing the conductive resin composition in the solvent as needed. In addition to the tin powder, the specific epoxy resin, and the specific dicarboxylic acid compound, the conductive material may further contain various additives for forming the conductive material (e.g., conductive powders other than tin powder, various curing agents, surfactants, pH adjusters (e.g., amine-based compounds), adhesion promoters, viscoelasticity adjusters, wetting and dispersing agents, leveling agents, pigments, UV absorbers, antioxidants, flame retardants, etc.). The conductive material can be obtained by placing the components in a mixing container and mixing them using one or more mixers selected from the group consisting of a rotation-revolution mixer, a ball mill, a roll mill, a bead mill, a planetary mixer, a tumbler, a stirrer, a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, etc., to form a varnish or paste.

[0064] The conductive material can be used, for example, as a printing conductive ink for forming wiring, a circuit-forming material, or a material for forming internal and external electrodes of passive components. When the conductive material is used as a printing conductive ink, examples of the printing method include one or more methods selected from the group consisting of screen printing, metal mask printing, inkjet printing, flexographic printing, gravure printing, and dispenser methods. In the present invention, it is preferable to use one or more printing methods selected from the group consisting of screen printing, inkjet printing, and the like, because they have excellent printability and shape retention. Here, the mesh used in the screen printing method can be selected as appropriate, and it is preferable to use a mesh that does not excessively remove the conductive powder or lead-free solder powder in the conductive material.

[0065] The coating method for coating an article or the like with a conductive material is not particularly limited. Any coating method can be adopted depending on the shape and usage form of the article or the like. Examples of the coating method include one or more coating methods selected from the group consisting of spin coating, dip coating, immersion, die coating, air spraying, airless spraying, electrostatic coating, brush coating, roller coating, roll coating, curtain flow coater, roller curtain coater, die coater, inkjet coating, and coating with a dispenser.

[0066] The thickness of the coating film formed by applying the conductive material is not particularly limited and can be an appropriate thickness depending on various applications. For example, it is 1 μm or more, preferably 2 μm or more, more preferably 5 μm or more, and 400 μm or less, preferably 200 μm or less, more preferably 100 μm or less. The conductive material has excellent storage stability under refrigeration and at room temperature, electrical conductivity, and one or more properties selected from the group consisting of adhesion to various substrates, leveling (surface smoothness), printability, etc.

[0067] [Conductive Adhesive] The conductive adhesive of the present invention contains the conductive resin composition. For example, the conductive adhesive can be obtained by dissolving and / or dispersing the conductive resin composition in the solvent as needed. The conductive adhesive is used to bond parts to be bonded so as to have electrical conductivity. For example, it is used when performing adhesion that requires electrical conductivity in the manufacture of batteries and electrical / electronic devices. The conductive adhesive may further contain one or more selected from the group consisting of a solvent, a curing agent for curing epoxy resins, an adhesion promoter, a viscoelasticity modifier, a wetting and dispersing agent, a curing accelerator (curing catalyst), a reactive diluent, a conductive powder other than tin powder, a resin other than epoxy resin, an antioxidant, a pigment, a filler, a corrosion inhibitor, an antifoaming agent, a coupling agent, an anti-settling agent, a leveling agent, a heavy metal deactivator, a surfactant, a pH adjuster, an ultraviolet absorber, a flame retardant, an adhesion promoter, etc. The conductive adhesive can be obtained by placing the above components in a mixing container, mixing them using one or more mixers selected from the group consisting of a rotation / revolution mixer, a ball mill, a roll mill, a bead mill, a planetary mixer, a tumbler, a stirrer, an agitator, a mechanical homogenizer, an ultrasonic homogenizer, a high-pressure homogenizer, a paint shaker, a V-type blender, a Nauta mixer, a Banbury mixer, a kneading roll, a single-screw extruder, a twin-screw extruder, and the like, to form a varnish or paste.

[0068] The conductive adhesive of the present invention can be used as an anisotropic conductive adhesive. This allows for highly reliable conductive connections to be formed in electronic components such as miniaturized IC chips and light-emitting diodes, and in electrode connections between circuit boards. Examples of adhesive structures in which bonded members are bonded together via the conductive adhesive of the present invention include RFID-related products such as IC cards and IC tags in which an IC chip is bonded to a substrate having electrodes, and light-emitting electronic components in which a light-emitting diode is bonded to a substrate having electrodes. For example, a bonded structure using the conductive adhesive can be formed by forming multiple electrodes on at least one surface of a substrate, applying the conductive adhesive of the present invention so that each electrode is at least covered, forming an adhesive film, and then pressing the electrodes of electronic components against each electrode and allowing the adhesive layer to harden.

[0069] The means for applying the conductive adhesive of the present invention to a substrate is not particularly limited. Examples include a method of applying the conductive resin composition to a substrate. In the present invention, the application can be performed by printing, dispensing, or the like. The printing method is preferably one or more selected from the group consisting of screen printing, metal mask printing, inkjet printing, flexographic printing, gravure printing, dispenser printing, and the like. Because of their excellent printability and shape retention, it is preferable to use one or more printing methods selected from the group consisting of screen printing, inkjet printing, and the like. Here, the mesh used in screen printing can be selected appropriately, and it is preferable to use a mesh that does not excessively remove the conductive powder in the conductive adhesive. The thickness of the adhesive film formed by applying the conductive adhesive can be adjusted to an appropriate thickness depending on the application. For example, it is 1 μm or more, preferably 2 μm or more, more preferably 5 μm or more, and 200 μm or less.

[0070] The conductive adhesive of the present invention may be formed into a film before use. A film-like conductive adhesive can be obtained, for example, by adding a solvent or the like to a conductive adhesive composition as needed, coating the resulting conductive adhesive solution on a releasable support, and then removing the solvent or the like. A film-like conductive adhesive is more convenient in terms of handling, etc. It can also be used as a multilayer structure, comprising one or more layers of the film-like conductive adhesive, and, if necessary, one or more insulating adhesive layers, one or more releasable material layers, etc. The conductive adhesive of the present invention can typically be used to bond adherends together using heat and pressure. The heating temperature is not particularly limited as long as it does not damage the adherends, and is, for example, 70°C or higher and 250°C or lower. The pressure is not particularly limited as long as it does not damage the adherends, and is, for example, 0.1 MPa or higher and 10 MPa or lower. The heating and pressure are preferably performed for, for example, 0.5 seconds or higher and 120 seconds or lower.

[0071] The conductive adhesive of the present invention is used to electrically bond adherends to each other. For example, it can be used as an adhesive for heterogeneous adherends, bonding and electrically connecting adherends made of different materials with different thermal expansion coefficients. Furthermore, the conductive adhesive of the present invention can be used as a circuit connection material such as an anisotropic conductive adhesive, a conductive paste, or a conductive adhesive film, or as an adhesive material for semiconductor elements such as an underfill material or LOC tape.

[0072] [Circuit Connecting Material] The circuit connecting material of the present invention contains the conductive resin composition. It is used for conductive connections between various electronic components and circuit boards and for connecting (adhering) electrical and electronic circuits to each other. The shape of the circuit connecting material is not particularly limited, but it is preferably in liquid or film form. A liquid circuit connecting material can be obtained, for example, by mixing the conductive resin composition of the present invention with a solvent such as an organic solvent to liquefy it. A film circuit connecting material can be obtained, for example, by directly casting and applying the liquefied conductive resin composition of the present invention onto a release substrate to form a film, drying to remove the solvent, forming a film, and then peeling it off from the release substrate. Alternatively, a film circuit connecting material can be obtained, for example, by impregnating a nonwoven fabric or the like with the liquefied conductive resin composition of the present invention, forming the film on a release substrate, drying to remove the solvent, and then peeling it off from the release substrate.

[0073] The method of electrical connection using the circuit connection material is not particularly limited. For example, a method can be used in which the circuit connection material is provided between an electrode of an electronic component, a circuit, or the like and an opposing electrode on a substrate, and then heated to electrically connect and bond the two electrodes. Pressure can be applied during heating, as necessary. The method of providing the circuit connection material between opposing electrodes is not particularly limited. For example, a method can be used in which a liquid circuit connection material is applied, or a method can be used in which a film-like circuit connection material is sandwiched between the electrodes. Another example can be used in which, when electrically connecting a pin of an electronic component or the like to a circuit, the circuit connection material is provided at the base of the pin, and then the pin is butt-joined to form an electrically conductive connection.

[0074] The circuit connection material can be used essentially as an anisotropic conductive material, and can also be used in an electrode connection method in which a highly adhesive circuit connection material is formed between opposing electrodes on a substrate, and then heated and pressurized to bring the electrodes into contact and bond the substrates together. Substrates on which electrodes are formed include inorganic materials such as semiconductors, glass, and ceramics, organic materials such as polyimide resins and polycarbonate resins, and composite combinations of these materials such as glass / epoxy. When the circuit connection material contains a solder powder that melts at a low temperature, conductive connection can be achieved at temperatures as low as 250°C or below, for example, 200°C or below.

[0075] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by mass."

[0076] [Components Used] The components used in the examples are as follows. Tin powder 1: spherical tin powder (D50=5.5 μm, Sn≧99.5% by mass) Epoxy resin 1: solid bisphenol A type epoxy resin ("YD-014" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent 900 to 1000 g / eq; softening point 100°C) Epoxy resin 2: solid bisphenol A type epoxy resin ("YD-011" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent 440 to 510 g / eq; softening point 66°C) Epoxy resin 3: solid bisphenol A type epoxy resin ("YD-019" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent 2200 to 2900 g / eq; softening point 138°C) Epoxy resin 4: solid epoxy resin ("LCE-2615" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 494 g / eq; softening point 93°C) Epoxy resin 5: solid bisphenol F type epoxy resin ("YDF-2004" manufactured by Nippon Steel Chemical & Material Co., Ltd.; epoxy equivalent weight 850 to 1050 g / eq; softening point 85°C) Epoxy resin 6: solid bisphenol F type epoxy resin ("jER-4005P" manufactured by Mitsubishi Chemical Corporation; epoxy equivalent weight 950 to 1200 g / eq; softening point 87°C) Epoxy resin 7: semi-solid rubber-modified epoxy resin ("TSR-601" manufactured by DIC Corporation; epoxy equivalent weight 450 to 500 g / eq) Epoxy resin 8: solid dicyclopentadiene type epoxy resin ("HP-7200" manufactured by DIC Corporation; epoxy equivalent weight 254 to 264 g / eq; softening point 57 to 68°C) Epoxy resin 9: solid phenol novolac type epoxy resin ("N-770" manufactured by DIC Corporation; epoxy equivalent 183 to 193 g / eq; softening point 65 to 75°C) Epoxy resin 10: solid biphenyl aralkyl type epoxy resin ("NC-3000" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 276 g / eq; softening point 57°C) Epoxy resin 11: solid naphthol-cresol novolac type epoxy resin ("NC-7000L" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 232 g / eq; softening point 90°C) Epoxy resin 12: liquid bisphenol A type epoxy resin ("EP-4100G" manufactured by ADEKA Corporation; epoxy equivalent 190 g / eq; softening point less than 25°C) Epoxy resin 13: liquid propylene oxide-added bisphenol A epoxy resin ("EP-4000S" manufactured by ADEKA Corporation);Epoxy resin 14: liquid phenol novolac epoxy resin ("RE-305S" manufactured by Nippon Kayaku Co., Ltd.; epoxy equivalent 173 g / eq; softening point less than 25°C) Linear dicarboxylic acid compound 1: adipic acid (HOOC-(CH; 2 ) 4 -COOH) Linear dicarboxylic acid compound 2: pimelic acid (HOOC-(CH 2 ) 5 -COOH) Linear dicarboxylic acid compound 3: sebacic acid (HOOC-(CH 2 ) 8 -COOH) Linear dicarboxylic acid compound 4: succinic acid (HOOC-(CH 2 ) 2 -COOH) Linear dicarboxylic acid compound 5: glutaric acid (HOOC-(CH 2 ) 3 -COOH) Linear dicarboxylic acid compound 6: diglycolic acid (HOOC-CH 2 -O-CH 2 -COOH) Branched dicarboxylic acid compound 1: long-chain branched dibasic acid ("MMA-10R" manufactured by Okamura Oil Mills) Branched dicarboxylic acid compound 2: long-chain branched dibasic acid ("SB-12" manufactured by Okamura Oil Mills) Thiol compound 1: thiocyanuric acid (1,3,5-triazine-2,4,6-trithiol) Solvent 1: diethylene glycol monobutyl ether (butyl carbitol) Solvent 2: diethylene glycol dibutyl ether (dibutyl carbitol)

[0077] <Evaluation of Conductivity> The volume resistivity of the conductive film (dried coating film) formed from the conductive resin composition was determined by the following method, and the conductivity was evaluated by the following method.

[0078] (Preparation of Conductive Film (Dried Coating Film) for Measurement) Using a metal mask with a pattern of 2 cm × 2 cm and a thickness of 100 microns, the conductive resin composition was hand-printed to prepare a coating film of 2 cm × 2 cm on a glass substrate of 5 cm × 5 cm. The coating film was then heat-cured at 160°C for 60 minutes to prepare a conductive film (dry coating film) for measuring volume resistivity.

[0079] (Volume Resistivity) The volume resistivity of the obtained conductive film (dried coating film) was measured in two directions (a direction passing through the center of the coating film and parallel to the upper edge of the coating film, and a direction perpendicular to the direction) by the four-terminal method using a resistivity meter "Loresta GP-MCP T610" (manufactured by Nitto Seiko Analytech Co., Ltd.), and the average volume resistivity was calculated. Furthermore, two conductive films (dried coating films) were prepared for each conductive resin composition, and the average volume resistivity of the two conductive films (dried coating films) was calculated and used as the volume resistivity. The calculated volume resistivities are also shown in Tables 1 to 6. Note that when the volume resistivity was too high to measure (volume resistivity measurement impossible), it was indicated as "UM" in Tables 1 to 6, and when the coating performance of the conductive resin composition was poor and it was impossible to apply it uniformly (poor coating), it was indicated as "UC" in Tables 1 to 6.

[0080] (Evaluation of Electrical Conductivity) The volume resistivity and conductivity were evaluated according to the following criteria. In this evaluation, A is a pass, and D is a fail. A: The volume resistivity was 3.0×10 -4 (Ω cm) or less D: Volume resistivity is 3.0 × 10 -4 (Ω·cm) or more, volume resistivity measurement impossible (UM) or coating failure (UC)

[0081] The viscosity of the conductive resin composition was measured and its storage stability was evaluated by the following methods. <Viscosity Measurement> The viscosity of the conductive resin composition was measured using a rheometer (Rheometer DHR-2 manufactured by TA Instruments) with a 20 mm cone plate, 25°C, and a shear rate of 10 s -1 The measurement was started at 180 seconds, and the viscosity was recorded 180 seconds after the start of the measurement.

[0082] <Storage Stability> The prepared conductive resin compositions were placed in a container and left to stand at room temperature (25°C) for 24 hours (room temperature (25°C) 24 hour storage) and left to stand in a refrigerator (4°C) for 1 week (refrigerated (4°C) 1 week storage), and then the storage stability of each conductive resin composition was evaluated using the following evaluation items and criteria. Furthermore, based on each evaluation, an overall evaluation of the 24 hour storage at room temperature (25°C) and 1 week storage in a refrigerator (4°C) was performed using the following criteria. In this evaluation, A is pass and D is fail. The evaluation results are also shown in Tables 1 to 6. A: All four evaluations of solidification, skinning, liquid separation, and viscosity increase rate were passed. D: One or more of the four evaluations of solidification, skinning, liquid separation, and viscosity increase rate were failed.

[0083] (Solidification) After storage under specified conditions, each conductive resin composition was touched with a spatula. If the conductive resin composition could be scooped up with the spatula, it was not solidified and was rated A. If the conductive resin composition had no fluidity and could not be scooped up with the spatula, it was solidified and was rated D. In this evaluation, A is a pass, and D is a fail. In addition, if the volume resistivity was "UC (poor application)", solidification was not checked and is indicated by a diagonal line in the table.

[0084] (Skinning) After storage under specified conditions, the appearance of each conductive resin composition was checked, and if there was no skinning on the surface of the conductive resin composition, it was rated as A, and if there was skinning, it was rated as D. Here, "skinning" refers to a state in which a film is formed on the surface of the conductive resin composition that comes into contact with air. In this evaluation, A is a pass, and D is a fail. Note that if the volume resistivity was "UC (poor coating)" or if solidification was confirmed, skinning was not checked, and this is indicated by a diagonal line in the table.

[0085] (Liquid Separation) After storage under specified conditions, the appearance of each conductive resin composition was checked, and if the liquid did not separate and float on the surface of the conductive resin composition, it was rated as A, and if the liquid separated and floated, it was rated as D. In this evaluation, A is a pass, and D is a fail. Note that if the volume resistivity was "UC (poor coating)" or if solidification or skinning was confirmed, separation of the liquid was not checked, and this is indicated by a diagonal line in the table.

[0086] (Viscosity) After storage under predetermined conditions, the viscosity of each conductive resin composition was measured using a rheometer (Rheometer DHR-2 manufactured by TA Instruments) with a 20 mm cone plate, at 25°C, and at a shear rate of 10 s -1 The measurement was started at 0°C, and the viscosity value was the viscosity 180 seconds after the start of the measurement. In addition, when the viscosity could not be measured (viscosity measurement impossible) due to the occurrence of solidification, skinning, or liquid separation after storage, this was recorded as "UM" in Tables 1 to 6. In addition, when the volume resistivity was "UC (uncoated)," the viscosity was not measured, and this is indicated by a diagonal line in the tables.

[0087] (Viscosity Increase Rate) The viscosity of each conductive resin composition was measured after storage under specified conditions, and the viscosity was measured immediately after preparation of the conductive resin composition to compare the measured value to calculate the viscosity increase rate, which was then evaluated according to the following criteria. In this evaluation, A and B indicate pass, and D indicates fail. Viscosity increase rate [%] = {(Viscosity after storage under specified conditions / Viscosity immediately after preparation) - 1} x 100 A: Viscosity increase rate is less than 50% B: Viscosity increase rate is 50% or more but less than 100% D: Viscosity increase rate is 100% or more or viscosity measurement is impossible

[0088] Example 1 15.00 parts of tin powder 1, 0.84 parts of epoxy resin 1, 0.40 parts of linear dicarboxylic acid compound 1, and 1.00 parts of solvent 1 were mixed and stirred using a planetary centrifugal mixer (Thinky Corporation, "Awatori Rentaro AR-100") to obtain a conductive resin composition. In the obtained conductive resin composition, the amount of tin powder (amount of tin powder relative to the total amount of non-solvent components) in the amount of all components other than the solvent (in Example 1, the total amount of tin powder 1, epoxy resin 1, and linear dicarboxylic acid compound 1) was 92.36 mass%. The viscosity of the obtained conductive resin composition was measured. A conductive film (dried coating film) was prepared from the obtained conductive resin composition, and its volume resistivity was measured and evaluated. The storage stability of the obtained conductive resin composition was evaluated (storage at room temperature (25°C) for 24 hours and storage in a refrigerator (4°C) for 1 week). The results are also shown in Table 1.

[0089] [Examples 2 to 32, Comparative Examples 1 to 13] Conductive resin compositions were prepared in the same manner as in Example 1, except that the constituent components of the conductive resin compositions and their contents (parts) were as shown in Tables 1 to 6, respectively. The viscosity of the obtained conductive resin compositions was measured. Conductive films (dried coating films) were prepared from the obtained conductive resin compositions, and the volume resistivity was measured and evaluated. The storage stability of the obtained conductive resin compositions was evaluated (storage at room temperature (25°C) for 24 hours and storage in a refrigerator (4°C) for 1 week). These results are also shown in Tables 1 to 6.

[0090]

[0091]

[0092]

[0093]

[0094]

[0095]

[0096] The conductive films formed from the conductive resin compositions according to Examples 1 to 32 all had a volume resistivity of 3.0×10 -4 Less than Ω cm, in some cases 1.0 × 10 -4 The conductive resin compositions according to Examples 1 to 32 exhibited conductivity of less than Ω cm, which was equal to or greater than that of silver paste, and thus had excellent conductivity. This shows that a conductive resin composition was formed that was less expensive than silver paste and exhibited high conductivity equivalent to that of silver paste. Furthermore, the conductive resin compositions according to Examples 1 to 32 did not solidify, skin on the surface, or separate from the liquid when stored at room temperature (25°C) for 24 hours or in a refrigerator (4°C) for one week, and showed only a small increase in viscosity before and after storage at room temperature for 24 hours and in a refrigerator for one week, demonstrating excellent storage stability.

Claims

1. A conductive resin composition comprising: (a) tin powder; (b) an epoxy resin; and (c) a dicarboxylic acid compound, wherein the epoxy resin (b) comprises an epoxy resin having an epoxy equivalent of 400 g / eq or more and being solid or semi-solid at 25°C; and the dicarboxylic acid compound (c) comprises a dicarboxylic acid compound having 4 to 9 carbon atoms.

2. The conductive resin composition according to claim 1, wherein the content of the (a) tin powder is 92.01% by mass or more and 99.50% by mass or less, with the total amount of components other than the solvent in the conductive resin composition being 100% by mass.

3. The conductive resin composition according to claim 1 or 2, wherein the (c) dicarboxylic acid compound further comprises a dicarboxylic acid compound having 10 or more carbon atoms.

4. The conductive resin composition according to claim 1 or 2, further comprising (d) a thiol compound.

5. A conductive resin composition having a volume resistivity of 4.0×10 -4 A conductive film having a resistivity of less than Ω·cm.

6. A conductive material comprising the conductive resin composition according to claim 1 or 2.

7. A conductive adhesive comprising the conductive resin composition according to claim 1 or 2.

8. A circuit connecting material comprising the conductive resin composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Conductive adhesive and bonding method using same

    JP2000309773A

  • Conductive paste composition

    JP2020205245A

  • Electroconductive resin composition

    JP2022172874A

  • Conductive adhesives, joints and joints

    JP6428716B2

  • Electrically conductive adhesive agent, joined body, and joint

    WO2015019666A1

Cited By

  • Conductive resin composition

    WO2026186335A1