Method for managing electrodeposition liquid, and electrodeposition device

By controlling organic acid concentration in the electrodeposition solution through anion exchange and using polyimide and fluororesin, the method addresses blistering issues in anionic electrodeposition, achieving stable and high-quality insulating films.

WO2024224969A1PCT designated stage expired Publication Date: 2024-10-31MITSUBISHI MATERIALS CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/013841
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-02-07
Filing Date
2024-04-03
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

The anionic electrodeposition method for forming insulating films on conductive substrates often results in blistering during the baking process due to increased organic acid concentration in the electrodeposition solution, leading to instability in the electrodeposited film.

Method used

The method involves controlling the concentration of organic acids in the electrodeposition solution through anion exchange treatment, maintaining it within a range of 5 mg/L to 500 mg/L to prevent excessive pH drops and blistering, and using a combination of polyimide resin and fluororesin for enhanced insulation properties.

Benefits of technology

This approach effectively suppresses blistering during baking and stabilizes the formation of insulating films with excellent insulation properties, ensuring consistent film quality even during continuous electrodeposition.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024013841_31102024_PF_FP_ABST
    Figure JP2024013841_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Disclosed is a method for managing an electrodeposition liquid that is used for the formation of an electrodeposition film on a conductive base material by means of anionic electrodeposition, wherein the concentration of an organic acid contained in the electrodeposition liquid is adjusted by performing an anion exchange treatment on the electrodeposition liquid. Also disclosed is an electrodeposition device (10) which is used when an electrodeposition film is formed on a conductive base material by means of anionic electrodeposition, and which comprises: an electrodeposition tank (20) in which an electrodeposition liquid is retained, and the base material and a counter electrode are immersed therein; an anion exchange means (30) for performing an anion exchange treatment on the electrodeposition liquid; and an electrodeposition liquid circulation means (40) for circulating the electrodeposition liquid between the electrodeposition tank (20) and the anion exchange means (30).
Need to check novelty before this filing date? Find Prior Art

Description

Electrodeposition liquid management method and electrodeposition apparatus

[0001] The present invention relates to a method for managing an electrodeposition solution used when electrodepositing an electrodeposition film on a conductive substrate by anionic electrodeposition, and an electrodeposition apparatus. This application claims priority based on Japanese Patent Application No. 2023-070848 filed on April 24, 2023, and Japanese Patent Application No. 2024-017168 filed on February 7, 2024, the contents of which are incorporated herein by reference.

[0002] Insulated conductors, which are made by covering a conductive substrate with an insulating coating made of an insulating resin, are widely used as conductive materials and heat sink materials for various electrical devices that require insulation. Various resins are used as constituent materials for the insulating coating. For example, Patent Document 1 discloses a material using a polyimide-based resin such as a polyamide-imide resin, and Patent Document 2 proposes a material using a mixed resin of a polyimide-based resin and a fluorine-based resin.

[0003] Electrodeposition is a known method for forming an insulating film made of such an insulating resin on the surface of a conductive substrate. The electrodeposition method involves immersing the substrate on which the insulating film is to be formed and a counter electrode in an electrodeposition solution in which the insulating film material is dispersed, and applying a voltage between the substrate and the counter electrode to deposit the insulating film material on the surface of the substrate. The formed electrodeposited film is then heated to bake the electrodeposited film onto the substrate, thereby forming the insulating film.

[0004] Electrodeposition methods include anionic electrodeposition, in which a voltage is applied to the substrate as an anode to form an insulating coating on the surface of the substrate, and cationic electrodeposition, in which a voltage is applied to the substrate as a cathode to form an insulating coating on the surface of the substrate.

[0005] Japanese Patent Application Publication No. 2017-115120 (A) Japanese Patent Application Publication No. 2018-070663 (A)

[0006] The anionic electrodeposition solution used in the anionic electrodeposition method contains solid components including the resin described above, water, an organic solvent, and a neutralizer. When a voltage is applied, the pH decreases near the surface of the anode (substrate), and the solid components precipitate on the surface of the anode (substrate), forming an electrodeposited film. However, if electrodeposition is continued using the anionic electrodeposition method, there is a risk of blistering when the electrodeposited film formed on the surface of the anode is baked to form an insulating coating.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a method for managing an electrodeposition liquid and an electrodeposition apparatus that can suppress the occurrence of blisters when baking an electrodeposition film and enable stable formation of an insulating coating.

[0008] In order to solve the above problems, the present inventors conducted extensive research and found that when electrodeposition is continued using an anionic electrodeposition method, the concentration of organic acid contained in the electrodeposition solution increases, causing blistering when the electrodeposited film is baked. Therefore, they discovered that by appropriately controlling the concentration of organic acid contained in the electrodeposition solution, it is possible to suppress the occurrence of blistering during baking.

[0009] The present invention has been made based on the above-mentioned findings, and a method for managing an electrodeposition solution according to Aspect 1 of the present invention is a method for managing an electrodeposition solution used when forming an electrodeposition film on a conductive substrate by anionic electrodeposition, and is characterized in that the concentration of an organic acid contained in the electrodeposition solution is adjusted by subjecting the electrodeposition solution to an anion exchange treatment.

[0010] According to the method for managing an electrodeposition solution of aspect 1 of the present invention, the concentration of the organic acid contained in the electrodeposition solution is controlled. Therefore, even when electrodeposition is continuously performed, the concentration of the organic acid does not become excessively high, and the occurrence of blistering during baking can be suppressed, making it possible to stably form an insulating coating.

[0011] A method for managing an electrodeposition solution according to a second aspect of the present invention is the method for managing an electrodeposition solution according to the first aspect of the present invention, characterized in that the electrodeposition solution contains water, an organic solvent, a solid component, and a neutralizing agent, and the solid component contains at least a polyimide resin. According to the method for managing an electrodeposition solution according to the second aspect of the present invention, since the solid component contains at least a polyimide resin, it is possible to stably form an insulating film having excellent insulating properties.

[0012] A method for managing an electrodeposition solution according to Aspect 3 of the present invention is characterized in that, in the method for managing an electrodeposition solution according to Aspect 1 or Aspect 2 of the present invention, the electrodeposition solution contains at least a carboxylic acid as the organic acid. According to the method for managing an electrodeposition solution according to Aspect 3 of the present invention, since the electrodeposition solution contains at least a carboxylic acid as the organic acid, a rapid decrease in pH on the surface of the anode (substrate) can be suppressed by the pH buffering effect of the carboxylic acid, which is an organic acid, and an electrodeposition film can be stably formed.

[0013] A method for managing an electrodeposition solution according to Aspect 4 of the present invention is characterized in that, in the method for managing an electrodeposition solution according to Aspect 1 or Aspect 2 of the present invention, the electrodeposition solution contains at least a hydroxy acid as the organic acid. According to the method for managing an electrodeposition solution according to Aspect 4 of the present invention, since the electrodeposition solution contains at least a hydroxy acid as the organic acid, a rapid decrease in pH on the surface of the anode (substrate) can be suppressed by the pH buffering effect of the hydroxy acid, which is an organic acid, and an electrodeposition film can be stably formed.

[0014] A method for managing an electrodeposition solution according to Aspect 5 of the present invention is the method for managing an electrodeposition solution according to any one of Aspects 1 to 4 of the present invention, characterized in that the concentration of the organic acid in the electrodeposition solution is adjusted to a range of 5 mg / L to 500 mg / L. According to the electrodeposition solution of Aspect 5 of the present invention, the concentration of the organic acid is adjusted to a range of 5 mg / L to 500 mg / L, so that an appropriate pH buffering effect can be exerted, an electrodeposition film can be stably formed, and the occurrence of blistering during baking can be appropriately suppressed.

[0015] A method for managing an electrodeposition solution according to a sixth aspect of the present invention is characterized in that, in the electrodeposition solution according to any one of the first to fifth aspects of the present invention, the solid components contain a fluororesin as well as a polyimide resin. According to the method for managing an electrodeposition solution according to the sixth aspect of the present invention, since the solid components contain a fluororesin as well as a polyimide resin, it is possible to form an insulating film that is particularly excellent in insulating properties and dielectric properties.

[0016] The electrodeposition apparatus of aspect 7 of the present invention is an electrodeposition apparatus used to form an electrodeposited film on a conductive substrate by anionic electrodeposition, and is characterized by comprising: an electrodeposition tank in which an electrodeposition solution is stored and in which the substrate and a counter electrode are immersed; an anion exchange means for performing an anion exchange treatment on the electrodeposition solution; and an electrodeposition solution circulation means for circulating the electrodeposition solution between the electrodeposition tank and the anion exchange means.

[0017] According to the electrodeposition apparatus of aspect 7 of the present invention, the apparatus is equipped with an electrodeposition tank, an anion exchange means for performing an anion exchange treatment on the electrodeposition solution, and an electrodeposition solution circulation means for circulating the electrodeposition solution between the electrodeposition tank and the anion exchange means. This makes it possible to appropriately control the concentration of the organic acid contained in the electrodeposition solution, and even when electrodeposition is performed continuously, the concentration of the organic acid does not become excessively high, making it possible to suppress the occurrence of blistering during baking and enabling the stable formation of an insulating coating.

[0018] According to the present invention, it is possible to provide a method for managing an electrodeposition solution and an electrodeposition apparatus that can suppress the occurrence of blisters when baking an electrodeposition film and can stably form an insulating film.

[0019] It is to be understood that both the foregoing general description and the following detailed description are exemplary and explanatory and are not restrictive of the invention, as claimed.

[0020] An electrodeposition liquid control method and an electrodeposition apparatus according to one embodiment of the present invention will be described below. The electrodeposition liquid control method according to this embodiment is for controlling an electrodeposition liquid used in forming an electrodeposition film, which serves as a precursor of an insulating film, on the surface of a conductive substrate. Note that this embodiment controls an electrodeposition liquid used in an anionic electrodeposition method in which a voltage is applied using the substrate as the anode to form an insulating film on the surface of the anode substrate.

[0021] In this embodiment, the electrodeposition solution to be managed contains water, an organic solvent, a solid component, and a neutralizing agent. As described above, the electrodeposition solution of this embodiment is used in an anionic electrodeposition method, and therefore contains an amine as a neutralizing agent. The electrodeposition solution of this embodiment may also contain an appropriate amount of organic acid in advance. By including an appropriate amount of organic acid in the electrodeposition film, it is possible to prevent the occurrence of fine cracks in the baking step S03 described below.

[0022] The organic acid may contain at least a carboxylic acid. Examples of carboxylic acids include formic acid, acetic acid, propionic acid, butyric acid, valeric acid, oxalic acid, malonic acid, benzoic acid, phthalic acid, trimellitic acid, and hydroxy acids. In particular, it is preferable that the organic acid contains at least a carboxylic acid. Examples of hydroxy acids include glycolic acid, hydroxypropionic acid, hydroxybutyric acid, tartronic acid, and glyceric acid. Note that hydroxypropionic acid and hydroxybutyric acid exert their effects regardless of the position of the functional group, so that even positional isomers can produce the effect.

[0023] In this embodiment, the solid component contains at least a polyimide resin, and preferably contains two types of resin: a polyimide resin and a fluororesin. Examples of polyimide resins include polyamideimide, polyetherimide, and polyimide. Examples of fluororesins include polytetrafluoroethylene and perfluoroalkoxyalkane.

[0024] The average particle size of the solid component may be from 50 to 300 nm, more preferably from 50 to 250 nm, and even more preferably from 50 to 200 nm. The standard deviation of the particle size of the solid component may be 250 nm or less, more preferably 150 nm or less, and even more preferably 100 nm or less.

[0025] The water and organic solvent are used to disperse the solid components of the polyimide resin and fluorine resin. Examples of the organic solvent include N,N-dimethylacetamide, propylene carbonate, dimethyl sulfoxide, N,N-dimethylformamide, 4-butyrolactone, N-methyl-2-pyrrolidone, and N-methyl-2-pyrrolidone.

[0026] The water content in the electrodeposition solution is preferably 15% by mass or more, and more preferably 50% by mass or more. On the other hand, the water content in the electrodeposition solution is preferably 85% by mass or less, and more preferably 75% by mass or less. Furthermore, the organic solvent content in the electrodeposition solution is preferably 15% by mass or more, and more preferably 50% by mass or more. On the other hand, the organic solvent content in the electrodeposition solution is preferably 85% by mass or less, and more preferably 75% by mass or less.

[0027] Next, a method for producing an insulating film using an electrodeposition liquid will be described with reference to Fig. 1. As shown in Fig. 1, the method for producing an insulating film in this embodiment includes a surface pretreatment step S01, an electrodeposition film formation step S02, and a baking step S03.

[0028] (Surface pretreatment step S01) First, a substrate on which an electrodeposited film (insulating film) is to be formed is prepared. This substrate is conductive and is made of a metal material such as copper or a copper alloy, aluminum or an aluminum alloy, etc. Then, oils and greases adhering to the surface of the substrate are removed using a surface treatment liquid such as an organic solvent or a surfactant.

[0029] (Electrodeposited Film Formation Step S02) Next, the substrate and counter electrode are immersed in the electrodeposition solution of this embodiment, and a voltage is applied between the anode (substrate) and the cathode (counter electrode) with the substrate as the anode and the counter electrode as the cathode. This reduces the pH of the electrodeposition solution around the substrate, causing a solid component (in this embodiment, a mixture of polyimide resin and fluororesin) to precipitate on the surface of the substrate. This forms an electrodeposited film on the surface of the substrate. At this time, since an organic acid is added to the electrodeposition solution in this embodiment, the organic solvent is appropriately contained in the electrodeposited film due to the pH buffering effect of the organic acid.

[0030] The temperature of the electrodeposition solution in the electrodeposition film forming step S02 (liquid temperature) is preferably adjusted to a range of 5° C. or higher and 35° C. or lower. By setting the liquid temperature to 5° C. or higher, it is possible to prevent water from being mixed into the electrodeposition solution due to condensation. On the other hand, by setting the liquid temperature to 35° C. or lower, the storage stability of the electrodeposition solution is improved, and the electrodeposition film can be stably formed.

[0031] The voltage applied between the substrate (anode) and the counter electrode (cathode) in the electrodeposition film forming step S02 is preferably in the range of 10 V or more and 600 V or less. By setting the applied voltage to 10 V or more, the electrodeposition rate can be ensured and productivity can be improved. On the other hand, by setting the applied voltage to 600 V or less, the generation of many bubbles on the surface of the substrate can be suppressed, and the bursting of the bubbles in the subsequent baking step S03 can be suppressed, thereby suppressing the generation of numerous irregularities in the insulating coating.

[0032] (Baking step S03) In the baking step S03, the substrate on which the electrodeposition film containing the solid components obtained in the electrodeposition film formation step S02 has been formed is dried, for example, within a temperature range of 200°C or higher and lower than the melting point of the solid components to remove the residual electrodeposition liquid, and then the electrodeposition film is baked onto the substrate to form an insulating coating.

[0033] The baking temperature in the baking step S03 may be within a temperature range in which the electrodeposited film of the solid components is formed and an insulating coating is formed on the substrate, for example, within a range of 200° C. to 400° C. The baking time may be within a range of 0.5 minutes to 60 minutes, for example.

[0034] Through the above steps, an insulating coating containing solid components is formed on the conductive substrate. If electrodeposition is continued, organic acids such as carboxylic acids are generated, and the concentration of the organic acids in the electrodeposition solution increases. This can cause swelling when the electrodeposition film is baked. Therefore, in this embodiment, the electrodeposition solution is managed to control the concentration of the organic acids in the electrodeposition solution.

[0035] An electrodeposition apparatus 10 according to this embodiment and a method for managing an electrodeposition solution using this electrodeposition apparatus 30 will now be described with reference to Fig. 2. The electrodeposition apparatus 10 shown in Fig. 2 includes an electrodeposition tank 20 in which an electrodeposition solution is stored and in which a substrate and a counter electrode are immersed, an anion exchange means 30 that performs an anion exchange treatment on the electrodeposition solution, and an electrodeposition solution circulation means 40 (an outlet pipe 41 and a return pipe 42) that circulates the electrodeposition solution between the electrodeposition tank 20 and the anion exchange means 30.

[0036] An electrodeposition solution is stored in the electrodeposition tank 20, and the substrate, which serves as the anode, and the counter electrode, which serves as the cathode, are immersed in this electrodeposition solution. A voltage is applied between the substrate and the counter electrode, thereby forming an electrodeposited film on the surface of the substrate.

[0037] As shown in Fig. 2, the anion exchange means 30 includes an anion exchange tank 31 in which an anion exchange resin 32 is disposed. The electrodeposition solution is supplied from the electrodeposition tank 20 to the anion exchange tank 31 via an outlet pipe 41. The electrodeposition solution is stored in the anion exchange tank 31, and organic acids contained in the electrodeposition solution are removed by the anion exchange resin 32. This makes it possible to control the concentration of organic acids contained in the electrodeposition solution. Examples of organic acids contained in the electrodeposition solution include carboxylic acids.

[0038] The electrodeposition solution in which the organic acid concentration has been controlled in this anion exchange tank 31 is then supplied to the electrodeposition tank 20 via the return pipe 42. Here, it is preferable that the organic acid concentration in the electrodeposition solution stored in the electrodeposition tank 20 be controlled within the range of 5 mg / L or more and 500 mg / L or less.

[0039] According to the method for managing an electrodeposition solution of this embodiment configured as described above, the concentration of the organic acid contained in the electrodeposition solution is controlled. Therefore, even when electrodeposition is continuously performed, the concentration of the organic acid does not become excessively high, and the occurrence of blistering during baking can be suppressed, making it possible to stably form an insulating coating.

[0040] In this embodiment, when the electrodeposition solution contains water, an organic solvent, a solid component, and a neutralizing agent, and the solid component contains at least a polyimide-based resin, an electrodeposition film containing at least a polyimide-based resin can be formed, and an insulating film with excellent insulating properties can be stably formed.

[0041] In this embodiment, when the electrodeposition solution contains at least a carboxylic acid as an organic acid, the pH buffering effect of the organic acid can suppress a rapid decrease in pH on the surface of the anode (substrate), allowing for stable formation of an electrodeposition film.

[0042] In this embodiment, when the electrodeposition solution contains at least a hydroxy acid as an organic acid, the pH buffering effect of the organic acid can suppress a rapid decrease in pH on the surface of the anode (substrate), allowing for stable formation of an electrodeposition film.

[0043] In this embodiment, when the concentration of the organic acid in the electrodeposition solution is adjusted to a range of 5 mg / L or more and 500 mg / L or less, an appropriate pH buffering effect can be exerted, allowing for stable deposition of an electrodeposition film and accurately suppressing the occurrence of blistering during baking.

[0044] In this embodiment, when the electrodeposition solution contains a fluororesin as well as a polyimide resin as solid components, an electrodeposition film containing a mixed resin of a polyimide resin and a fluororesin can be formed, and an insulating film with particularly excellent insulating properties can be stably formed.

[0045] The electrodeposition apparatus 10 of this embodiment is equipped with an electrodeposition tank in which the electrodeposition liquid is stored and in which the substrate and the counter electrode are immersed, an anion exchange means for performing an anion exchange treatment on the electrodeposition liquid, and an electrodeposition liquid circulation means for circulating the electrodeposition liquid between the electrodeposition tank and the anion exchange means. Therefore, the concentration of the organic acid contained in the electrodeposition liquid can be appropriately adjusted, and even when electrodeposition is performed continuously, the concentration of the organic acid does not become excessively high, which prevents the occurrence of blistering during baking and enables the stable formation of an insulating coating.

[0046] While the present invention has been described above as an embodiment, it is not limited thereto and can be modified as appropriate without departing from the technical spirit of the invention. In this embodiment, the electrodeposition apparatus shown in Figure 2 has been described as an example, but the present invention is not limited thereto and electrodeposition apparatuses of other configurations may also be used.

[0047] For example, the electrodeposition apparatus 110 shown in Fig. 3 may be used. In the electrodeposition apparatus 110 shown in Fig. 3, the anion exchange means 130 for performing anion exchange treatment on the electrodeposition solution may include an ultrafiltration device 131 and an exchange membrane tank 132 in which anion exchange membranes 133 and cation exchange membranes 134 are alternately arranged. As another method for controlling organic acids, a method using electrodialysis may also be applied.

[0048] The results of confirmation experiments conducted to confirm the effectiveness of the present invention will be described below.

[0049] As shown in Tables 1 and 2, water, an organic solvent, a solid component, a neutralizing agent, and an organic acid were prepared and mixed in the mass ratios shown in Tables 1 and 2 to obtain electrodeposition solutions. In Inventive Examples 1 to 24, the electrodeposition solutions were subjected to anion exchange treatment using the electrodeposition apparatus shown in Figure 2. The resulting changes in the concentration of the organic acid are shown in Tables 1 and 2.

[0050] The concentration of organic acids in the electrodeposited film was evaluated as follows. The electrodeposition solution was diluted with ultrapure water, impurities were removed, and the filtrate was passed through a membrane filter to prepare the solution for ion chromatography. Measurements were then performed using a Thermo Fisher Scientific ICS-5000+ ion chromatograph. The stationary phase of the ion chromatograph was an anion exchange column, Dionex IonPac AG15 or Dionex IonPac AS15, the eluent was potassium hydroxide aqueous solution, the suppressor was Dionex ADRS 600, and the detector was electrical conductivity.

[0051] The electrodeposition solutions of Examples 1 to 24 of the present invention, which had undergone anion exchange treatment, and Comparative Examples 1 to 3, which had not undergone anion exchange treatment, were evaluated for stability. When the electrodeposition solutions were kept at 40°C for 5 days, those that showed precipitation or separation were rated "B," and those that did not show precipitation or separation were rated "A." The evaluation results are shown in Tables 1 and 2.

[0052] An oxygen-free copper rectangular bar (1.47 mm x 2.94 mm x 25 cm long) was prepared as the conductive substrate, and a cylindrical copper plate was prepared as the counter electrode. The substrate and counter electrode were immersed in the above-mentioned electrodeposition solution, and an electrodeposition film was formed at a temperature of 20°C, an applied voltage of 300 V, and a holding time of 0.5 minutes. The electrodeposition film was then baked using a three-stage heating profile: a work temperature of 140-170°C for 10 minutes, a temperature of 240-260°C for 5 minutes, and a temperature of 340-350°C for 90 seconds, followed by rapid cooling, to form an insulating coating.

[0053] The appearance of the formed insulating film was then observed and evaluated for blistering. Visual observation rated the insulating film as "present" if blistering was observed, and "absent" if no blistering was observed. Furthermore, the dielectric constant of the insulating film was measured as follows. The evaluation results are shown in Tables 1 and 2. Silver paste was applied to the surface of the insulating film at two 10 mm edges and at a 100 mm center to prepare a measurement sample. The capacitance between the conductor and the silver paste in the center was measured using a Hioki E.E. LCR meter IM3536, and the dielectric constant was calculated from the measured capacitance and the thickness of the film.

[0054]

[0055]

[0056] In Comparative Examples 1 to 3, the organic acid concentration in the electrodeposition solution was not adjusted, and therefore the stability of the electrodeposition solution was evaluated as "B." In addition, blisters occurred in the insulating coating after baking.

[0057] In contrast, in Inventive Examples 1 to 24, the organic acid concentration in the electrodeposition solution was adjusted, and the stability of the electrodeposition solution was evaluated as "A." Furthermore, no blisters occurred in the insulating coating after baking. Furthermore, Inventive Examples 18 and 19 contained polyimide resin and fluororesin as solid components, which resulted in a sufficiently low relative dielectric constant and particularly excellent insulating properties.

[0058] From the results of the above confirmation experiments, it was confirmed that the present invention can provide a method for managing an electrodeposition liquid and an electrodeposition apparatus that can suppress the occurrence of blistering when baking an electrodeposition film and can stably form an insulating coating.

[0059] It is possible to provide a method for managing an electrodeposition solution and an electrodeposition device that can prevent the occurrence of blisters when baking an electrodeposition film and can stably form an insulating film.​

Claims

1. A method for managing an electrodeposition solution used in forming an electrodeposition film on a conductive substrate by anion electrodeposition, comprising the steps of: subjecting the electrodeposition solution to an anion exchange treatment to adjust the concentration of an organic acid contained in the electrodeposition solution.

2. The method for managing an electrodeposition solution according to claim 1, characterized in that the electrodeposition solution contains water, an organic solvent, a solid component, and a neutralizing agent, and the solid component contains at least a polyimide-based resin.

3. The method for managing an electrodeposition solution according to claim 1, characterized in that the electrodeposition solution contains at least a carboxylic acid as the organic acid.

4. The method for managing an electrodeposition solution according to claim 1, characterized in that the electrodeposition solution contains at least a hydroxy acid as the organic acid.

5. The method for managing an electrodeposition solution according to claim 1, characterized in that the concentration of said organic acid in said electrodeposition solution is adjusted to within the range of 5 mg / L or more and 500 mg / L or less.

6. The method for managing an electrodeposition liquid according to claim 1, characterized in that the electrodeposition liquid contains, as solid components, a fluororesin in addition to a polyimide resin.

7. An electrodeposition apparatus used in forming an electrodeposition film on a conductive substrate by anion electrodeposition, comprising: an electrodeposition tank for storing an electrodeposition liquid and in which the substrate and a counter electrode are immersed; an anion exchange means for performing an anion exchange treatment on the electrodeposition liquid; and an electrodeposition liquid circulation means for circulating the electrodeposition liquid between the electrodeposition tank and the anion exchange means.

Citation Information

Patent Citations

  • Method of anionic electrodeposition

    JP1978010639A

  • Pretreating agent and pretreatment for painting of steel material

    JP1984229496A

  • Method for managing electrodeposition bath

    JP1993327183A

  • Electrodeposition coating method and electrodeposition coating equipment

    JP2022096090A

  • Electrodeposition solution and method for producing conductor with insulating film using same