Fluoroolefin production method
The method enhances fluoroolefin production by using an alumina-containing catalyst with controlled metal and silicon content and α-alumina structure, achieving higher conversion rates and selectivity in producing fluoroolefins like trifluoroethylene.
Patent Information
- Application Number
- PCT/JP2024/014304
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional methods for producing fluoroolefins often result in low conversion rates due to the use of various aluminas as catalysts, with the content of alkali metal elements, alkaline earth metal elements, and silicon in alumina-containing catalysts influencing the reaction efficiency.
A method involving the use of an alumina-containing catalyst with a total content of alkali metal elements and alkaline earth metal elements of 100 mass ppm or less and a Si content of 1000 mass ppm or less, specifically containing α-alumina, to contact fluorocarbons like 1,1,1,2-tetrafluoroethane at temperatures between 300°C to 800°C, in the presence of an inert gas, to produce fluoroolefins such as trifluoroethylene with enhanced conversion rates.
The method achieves a higher conversion rate of fluoroolefins compared to conventional methods, with the specific composition of the alumina-containing catalysts and reaction conditions optimizing the selectivity and durability of the catalyst, thereby improving industrial productivity.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Fluoroolefin production method
[0001] The present disclosure relates to a process for producing fluoroolefins.
[0002] In recent years, fluoroolefins have attracted attention as compounds with low global warming potential, and methods for producing them have been investigated. For example, Non-Patent Document 1 describes a method for obtaining trifluoroethylene by using α-alumina, γ-alumina, θ-alumina, or the like in the dehydrofluorination reaction of 1,1,1,2-tetrafluoroethane.
[0003] Catalysis Letters 2015, Vol. 145, p654-661
[0004] However, as shown in Figure 1 of Non-Patent Document 1, when various aluminas were used as catalysts, the conversion rate of the reaction was sometimes low.
[0005] An object of one embodiment of the present disclosure is to provide a method for producing a fluoroolefin with a higher conversion rate than conventional methods.
[0006] The present disclosure includes the following aspects: <1> A method for producing a fluoroolefin, comprising the step of bringing a fluorocarbon represented by the following formula (1) into contact with an alumina-containing catalyst to produce a fluoroolefin represented by the following formula (2), wherein the alumina-containing catalyst satisfies at least one of the following (I) and (II): CX 1 X 2 F-CX 3 X 4 H...(1) CX 1 X 2 =CX 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4at least one of which is a fluorine atom. (I) The total content of alkali metal elements and alkaline earth metal elements is 100 ppm by mass or less. (II) The content of Si is 1000 ppm by mass or less. <2> The method for producing a fluoroolefin according to <1>, wherein the alumina contained in the alumina-containing catalyst includes α-alumina. <3> The method for producing a fluoroolefin according to <1> or <2>, wherein the fluorocarbon is at least one selected from the group consisting of 1,1,1-trifluoroethane, 1,1,2-trifluoroethane, 1,1,2,2-tetrafluoroethane, and 1,1,1,2-tetrafluoroethane. <4> The method for producing a fluoroolefin according to any one of <1> to <3>, wherein the fluoroolefin is at least one selected from the group consisting of 1,2-difluoroethylene, 1,1-difluoroethylene, and trifluoroethylene. <5> The method for producing a fluoroolefin according to any one of <1> to <4>, wherein the fluorocarbon is 1,1,1,2-tetrafluoroethane and the fluoroolefin is trifluoroethylene. <6> The method for producing a fluoroolefin according to any one of <1> to <5>, wherein the fluorocarbon is contacted with the alumina-containing catalyst at a temperature of 300 to 800°C. <7> The method for producing a fluoroolefin according to any one of <1> to <6>, wherein the fluorocarbon is contacted with the alumina-containing catalyst in the presence of an inert gas, the inert gas being at least one selected from the group consisting of nitrogen, helium, argon, octafluorocyclobutane, and carbon dioxide. <8> The method for producing a fluoroolefin according to any one of <1> to <7>, further comprising a step of drying the alumina-containing catalyst before contacting the fluorocarbon with the alumina-containing catalyst. <9> The method for producing a fluoroolefin according to any one of <1> to <8>, wherein the fluorocarbon and the alumina-containing catalyst are contacted in a gas phase in the presence of water, and the concentration of the water is less than 500 ppm by mass based on the total amount of the raw material gas containing the fluorocarbon.
[0007] According to the present disclosure, a method for producing a fluoroolefin with a higher conversion rate than conventional methods is provided.
[0008] In the present disclosure, a numerical range indicated using "to" means a range that includes the numerical values before and after "to" as the minimum and maximum values, respectively. In the numerical ranges described in stages in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with the upper or lower limit value of another numerical range described in stages. Furthermore, in the numerical ranges described in the present disclosure, the upper or lower limit value described in a certain numerical range may be replaced with a value shown in the examples. In the present disclosure, a combination of two or more preferred embodiments is a more preferred embodiment. In the present disclosure, when there are multiple substances corresponding to each component, the amount of each component means the total amount of multiple substances, unless otherwise specified.
[0009] [Fluoroolefin Production Method] The fluoroolefin production method of the present disclosure includes a step of bringing a fluorocarbon represented by the following formula (1) into contact with an alumina-containing catalyst to produce a fluoroolefin represented by the following formula (2), wherein the alumina-containing catalyst satisfies at least one of the following (I) and (II): CX 1 X 2 F-CX 3 X 4 H...(1) CX 1 X 2 =CX 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the above is a fluorine atom. (I) The total content of alkali metal elements and alkaline earth metal elements is 100 ppm by mass or less. (II) The content of Si is 1000 ppm by mass or less.
[0010] According to the method for producing fluoroolefins of the present disclosure, the conversion rate is higher than that of conventional methods. The reason for this is not clear, but is presumed to be as follows.
[0011] In the reaction of obtaining the fluoroolefin represented by formula (2) from the fluorocarbon represented by formula (1), hydrogen fluoride is generated. The generated hydrogen fluoride reacts with the fluoroolefin represented by formula (2) to return to the fluorofluorocarbon represented by formula (1), and therefore, the conversion rate of the fluorocarbon represented by formula (1) has conventionally been very low.
[0012] As shown in the above-mentioned Non-Patent Document 1, when alumina was used as a catalyst, the conversion rate was sometimes low. This is thought to be due to differences in the crystal structure of α-alumina, γ-alumina, etc., but it is also thought to be due to other reasons. Therefore, the present inventors performed compositional analysis of various alumina-containing catalysts and found that the alkali metal and alkaline earth metal contents, as well as the Si content, in the alumina-containing catalyst affect the conversion rate. Further investigations have led to experimentally finding that the use of an alumina-containing catalyst that satisfies at least one of the above (I) and (II) results in a high conversion rate.
[0013] (Fluorocarbon Represented by Formula (1)) In the method for producing a fluoroolefin according to the present disclosure, a fluorocarbon represented by the following formula (1) is used as a raw material: CX 1 X 2 F-CX 3 X 4 H...(1) In formula (1), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.
[0014] Examples of the fluorocarbon represented by formula (1) include the following compounds: CHF 2 CH 3: 1,1-difluoroethane (HFC-152a) CH 2 FCH 2 F: 1,2-difluoroethane (HFC-152) CF 3 CH 3 : 1,1,1-trifluoroethane (HFC-143a) CHF 2 CH 2 F: 1,1,2-trifluoroethane (HFC-143) CF 3 CH 2 F: 1,1,1,2-tetrafluoroethane (HFC-134a) CHF 2 CHF 2 : 1,1,2,2-tetrafluoroethane (HFC-134) CF 3 CHF 2 : 1,1,1,2,2-pentafluoroethane (HFC-125)
[0015] Among these, the fluorocarbon represented by formula (1) is preferably at least one selected from the group consisting of HFC-143a, HFC-143, HFC-134a, and HFC-134, from the viewpoint of minimizing side reactions and suppressing the production of by-products. Furthermore, the fluorocarbon represented by formula (1) is preferably HFC-134a, since one type of fluoroolefin can be obtained with high selectivity.
[0016] (Fluoroolefin represented by formula (2)) In the method for producing a fluoroolefin according to the present disclosure, a fluoroolefin represented by the following formula (2) is obtained as a reaction product: CX 1 X 2 =CX 3 X 4 ...(2) In formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the groups is a fluorine atom.
[0017] Examples of the fluoroolefin represented by formula (2) include the following compounds: CHF=CH 2 : Fluoroethylene CF 2 =CH 2 : 1,1-difluoroethylene (HFO-1132a) CHF=CHF: 1,2-difluoroethylene (HFO-1132(E), HFO-1132(Z)) CHF=CF 2 : Trifluoroethylene (HFO-1123) CF 2 =CF 2 : Tetrafluoroethylene
[0018] Among these, the fluoroolefin represented by formula (2) is preferably at least one selected from the group consisting of HFO-1132, HFO-1132a, and HFO-1123, from the viewpoint of usefulness as a refrigerant composition.
[0019] In particular, in the fluoroolefin production method of the present disclosure, from the viewpoint of allowing the reaction to proceed more selectively, it is preferable that the fluorocarbon is HFC-134a and the fluoroolefin is HFO-1123.
[0020] It should be noted that olefins other than the fluoroolefin of formula (2) may be produced together with the fluoroolefin of formula (2), and the olefins other than the fluoroolefin of formula (2) may include ethylene.
[0021] (Alumina-Containing Catalyst) In the method for producing a fluoroolefin of the present disclosure, a fluorocarbon represented by formula (1) is contacted with an alumina-containing catalyst. The alumina-containing catalyst contacted with the fluorocarbon satisfies at least one of the following (I) and (II): (I) The total content of alkali metal elements and alkaline earth metal elements is 100 ppm by mass or less. (II) The Si content is 1,000 ppm by mass or less.
[0022] In the above (I), "100 ppm by mass or less" includes both the case where the target element is contained at 100 ppm by mass or less and the case where the target element is not contained (i.e., 0 ppm by mass). The same applies when only the upper limit value is specified for the content of other elements.
[0023] In the present disclosure, an alumina-containing catalyst refers to a catalyst that contains aluminum (Al) and oxygen (O) when subjected to elemental analysis by X-ray fluorescence analysis (XRF). The alumina-containing catalyst preferably contains 1.0 mass% or more of Al, may contain 5.0 mass% or more, or may contain 10 mass% or more of Al.
[0024] Hereinafter, the content of each element in the catalyst is the value obtained by elemental analysis using XRF. XRF is performed using an X-ray fluorescence analyzer (e.g., a scanning X-ray fluorescence analyzer, ZSX Primus II, manufactured by Rigaku Corporation) to perform qualitative and quantitative analysis measurements. All elements present in the measurement area are measured, and the atomic weights of these elements and the atomic weight of a specific metal element are calculated. Then, the atomic weights of all elements present in the measurement area and the atomic weight of the target element are each converted to mass. From these results, the percentage of the mass of each element relative to the mass of all elements present in the measurement area is calculated.
[0025] When the alumina-containing catalyst is used after undergoing various treatments such as drying treatment and activation treatment, the elemental analysis of the alumina-containing catalyst may be carried out either before or after the treatments.
[0026] The alumina contained in the alumina-containing catalyst may be used alone or in combination of two or more types. Alumina is a dehydrated product of aluminum hydroxide, and its properties vary depending on the degree of dehydration and the degree of crystallinity. Examples of alumina contained in the alumina-containing catalyst include β-alumina, γ-alumina, θ-alumina, η-alumina, boehmite, and gibbsite, and it is more preferable to contain α-alumina. Compared with other alumina structures, α-alumina is a high-temperature stable phase with a high degree of crystallinity, and although it has a small specific surface area, it is thermally stable and has a high thermal conductivity. Furthermore, compared with other alumina structures, α-alumina has a higher barrier for the conversion of Al—O to Al—F in the presence of hydrogen fluoride. Therefore, by using a catalyst containing α-alumina, it is possible to reduce the AlF 3This can suppress the generation of α-alumina, thereby more effectively suppressing catalyst deactivation and a decrease in selectivity. The reason why selectivity is improved with α-alumina compared to γ-alumina is not clear, but it is thought that this is due to the fact that the crystal structure of γ-alumina changes significantly in a high-temperature environment, which changes the bond distance between alkali metal elements, alkaline earth metal elements, and Si and Al in the alumina-containing catalyst. Furthermore, since α-alumina has higher catalyst durability than γ-alumina, a decrease in conversion rate during long-term production is effectively suppressed when a large amount of raw material is supplied to the catalyst. Therefore, by using a catalyst containing α-alumina, it is possible to increase the amount of raw material supplied to the catalyst, which is advantageous for industrial production.
[0027] The presence of α-alumina in an alumina-containing catalyst can be confirmed by a diffraction pattern obtained by X-ray diffraction, in other words, XRD (X-ray diffractometer). A commercially available XRD device can be used, for example, the "SmartLab" manufactured by Rigaku Corporation. If peaks at d = 26.62, 35.21, 37.85, 43.43, 52.65, and 57.61 Å are present in the diffraction pattern, it can be determined that α-alumina is present. Note that this analysis is performed on the alumina-containing catalyst immediately before contact with a fluorocarbon or on an alumina-containing catalyst in the same state as the alumina-containing catalyst immediately before contact with a fluorocarbon.
[0028] The alumina-containing catalyst may also contain aluminum oxide fluoride, aluminum fluoride, or the like, which is a fluorinated alumina.
[0029] The alumina-containing catalyst may contain a compound other than alumina, such as an oxide other than alumina, including chromium oxide, copper oxide, iron oxide, nickel oxide, magnesium oxide, zinc oxide, and zirconium oxide.
[0030] In particular, from the viewpoint of maintaining the durability of the alumina-containing catalyst, it is preferred that the alumina-containing catalyst has, in a diffraction pattern obtained by X-ray diffraction, a peak at d=43.43 Å among peaks attributable to α-alumina that has a higher diffraction intensity than the diffraction intensity of peaks attributable to compounds other than α-alumina, or that the alumina-containing catalyst has only peaks attributable to α-alumina. In other words, it is preferred that the alumina-containing catalyst be mainly composed of α-alumina.
[0031] As described above, the peaks derived from α-alumina are the peaks at d=26.62, 35.21, 37.85, 43.43, 52.65, and 57.61 Å.
[0032] When the alumina-containing catalyst contains α-alumina, the content of the α-alumina crystal structure may be 65% by mass or more, 70% by mass or more, 75% by mass or more, 80% by mass or more, 85% by mass or more, or even 100% by mass. The content of the α-alumina crystal structure in the alumina-containing catalyst can be confirmed by performing Rietveld analysis on the crystal structure of XRD. Specifically, the peaks obtained by XRD measurement of the catalyst are compared with known peak models derived from each alumina structure, and Rietveld analysis is performed to calculate the mass proportion of each crystal structure.
[0033] The total content of alkali metal elements and alkaline earth metal elements in the alumina-containing catalyst is 100 ppm by mass or less, preferably 80 ppm by mass or less, more preferably 50 ppm by mass or less, and may be 0 ppm by mass (i.e., not contained). When the Si content in the alumina-containing catalyst is 1000 ppm by mass or less, the total content of alkali metal elements and alkaline earth metal elements in the alumina-containing catalyst may exceed 100 ppm by mass, but is preferably 100 ppm by mass or less.
[0034] The alkali metal element content in the alumina-containing catalyst is 100 ppm by mass or less, preferably 40 ppm by mass or less, more preferably 25 ppm by mass or less, and may be 0 ppm by mass (i.e., not contained). When the Si content in the alumina-containing catalyst is 1000 ppm by mass or less, the alkali metal element content in the alumina-containing catalyst may exceed 100 ppm by mass, but is preferably 100 ppm by mass or less.
[0035] Among alkali metal elements, elements that are likely to be contained in an alumina-containing catalyst include Na and K. The total content of Na and K in the alumina-containing catalyst is 100 ppm by mass or less, preferably 40 ppm by mass or less, more preferably 25 ppm by mass or less, and may be 0 ppm by mass (i.e., not contained).
[0036] The content of alkaline earth metal elements in the alumina-containing catalyst is 100 ppm by mass or less, preferably 40 ppm by mass or less, more preferably 25 ppm by mass or less, and may be 0 ppm by mass (i.e., not contained). When the Si content in the alumina-containing catalyst is 1000 ppm by mass or less, the content of alkaline earth metal elements in the alumina-containing catalyst may exceed 100 ppm by mass, but is preferably 100 ppm by mass or less.
[0037] Among alkaline earth metal elements, Mg and Ca are examples of elements that are likely to be contained in an alumina-containing catalyst. The total content of Mg and Ca in the alumina-containing catalyst is 100 ppm by mass or less, preferably 40 ppm by mass or less, more preferably 25 ppm by mass or less, and may be 0 ppm by mass (i.e., not contained).
[0038] The Si content in the alumina-containing catalyst is 1000 ppm by mass or less, preferably 800 ppm by mass or less, more preferably 600 ppm by mass or less, and may be 0 ppm by mass (i.e., not contained). When the alkaline earth metal element content in the alumina-containing catalyst is 100 ppm by mass or less, the Si content in the alumina-containing catalyst may exceed 1000 ppm by mass, but is preferably 1000 ppm by mass or less.
[0039] The alumina-containing catalyst may contain other elements such as C, Fe, Zn, and Ga in addition to Al and O. The content of other elements in the alumina-containing catalyst may be within a range that does not impair the effects of the present disclosure. For example, the content of Fe may be 0.02 mass% or less, or the alumina-containing catalyst may be free of Fe. Furthermore, the content of Fe in the alumina-containing catalyst may be more than 0.02 mass%.
[0040] The alumina-containing catalyst may also contain other elements in addition to those described above. Examples of other elements include Sc, Y, Ti, Zr, Hf, V, Nb, Ta, Cr, Mo, W, Mn, Re, Fe, Ru, Co, Rh, Ir, Ni, Pd, Pt, Cu, Ag, Au, Zn, La, and Ce. The origin of these elements is not limited, and they may be derived from raw materials or manufacturing equipment. The content of other elements in the alumina-containing catalyst may be within a range that does not impair the effects of the present disclosure.
[0041] Alumina may function not only as a catalyst but also as a support while functioning as a catalyst, or alumina may be supported on a support other than alumina.
[0042] Supports other than alumina include, for example, carbon, zirconia, silica, and titania.
[0043] The form of the alumina-containing catalyst is not particularly limited, and it may be in the form of a powder, pellets, or spheres.
[0044] In order to provide excellent packing properties when packed into a reactor and excellent flowability of the reaction gas, α-alumina is preferably in the form of a molded body such as a sphere or pellet from the viewpoint of handling when used for about 10 hours. A molded body differs from a powder and is obtained, for example, by placing the powder in a mold and compressing it.
[0045] The form of the alumina-containing catalyst is not particularly limited, and may be a powder, pellet, or sphere. From the viewpoints of packing properties when filling a reactor, flowability of reaction gas, and ease of handling when used for about 10 hours, α-alumina is preferably in the form of a molded body such as a sphere or pellet. A molded body differs from a powder and is obtained, for example, by placing the powder in a mold and compressing it.
[0046] (Reaction Conditions) In the fluoroolefin production method of the present disclosure, the feedstock gas only needs to contain the fluorocarbon represented by formula (1), and may contain components other than the fluorocarbon represented by formula (1). The feedstock gas may consist solely of the fluorocarbon represented by formula (1), or may contain isomers, disproportionation products, impurities, and the like obtained during the production of the fluorocarbon represented by formula (1). From the viewpoint of suppressing side reactions and catalyst deactivation, the feedstock gas preferably contains an inert gas such as nitrogen, argon, helium, carbon dioxide, or octafluorocyclobutane in addition to the fluorocarbon represented by formula (1). The inert gas can dilute the target product and the by-product hydrogen fluoride. The content of the fluorocarbon represented by formula (1) is preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 75 mol% or more, and particularly preferably 80 mol% or more, based on the total amount of the feedstock gas.
[0047] The method for producing a fluoroolefin of the present disclosure may be carried out in a gas phase or a liquid phase. Since the fluorocarbon represented by formula (1) is a gas at room temperature, it is preferable to contact the fluorocarbon with the alumina-containing catalyst in a gas phase.
[0048] The reactor in which the fluorocarbon is brought into contact with the alumina-containing catalyst may be any reactor capable of withstanding the temperatures and pressures described below, and its shape and structure are not particularly limited. Examples of reactors include cylindrical vertical reactors. Examples of reactor materials include glass, stainless steel, iron, nickel, and alloys containing iron or nickel as the main component. The reactor may be equipped with a heating means, such as an electric heater, for heating the interior of the reactor.
[0049] The alumina-containing catalyst may be accommodated in any of the fixed bed, fluidized bed, and moving bed types. When it is a fixed bed type, it may be either a horizontal fixed bed type or a vertical fixed bed type.
[0050] The reaction may be carried out in a flow manner or a batch manner.
[0051] Fixed-bed reactors are filled with various types of catalyst-supported carriers to reduce pressure loss in the reaction fluid. Similar to fixed-bed reactors, a moving bed reactor is used in which an alumina-containing catalyst is loaded, moved by gravity, and then removed from the bottom of the reactor for regeneration. In fluidized-bed reactors, the catalyst bed is operated in a manner that makes it appear as if it were a fluid, and the catalyst particles are suspended in the reaction fluid and move within the reactor. Fixed-bed reactors are preferred because of the wide range of alumina-containing catalyst shape options and the ability to suppress alumina-containing catalyst wear. Fixed-bed reactors include tubular and tank-type reactors, with tubular reactors being preferred due to the ease of reaction temperature control. Furthermore, multi-tube heat exchange reactors, in which multiple small-diameter reaction tubes are arranged in parallel and a heat transfer medium is circulated outside, can be used. When multiple reactors are arranged in series, multiple catalyst layers are installed. At least one catalyst layer is sufficient, but two or more are also acceptable.
[0052] From the viewpoint of improving the conversion rate, the fluoroolefin production method of the present disclosure is preferably carried out in a flow system using a fixed-bed reactor (particularly a vertical fixed-bed reactor).
[0053] From the viewpoint of improving industrial productivity, the feed rate of fluorocarbon to the alumina-containing catalyst (raw material feed rate) is preferably 0.1 g / hr / g or more, more preferably 0.2 g / hr / g or more, and even more preferably 0.3 g / hr / g or more. Furthermore, from the viewpoint of maintaining a constant or higher conversion rate, the feed rate of raw material is preferably 5.0 g / hr / g or less, more preferably 4.5 g / hr / g or less, and even more preferably 4.0 g / hr / g or less. The feed rate of raw material refers to the amount of fluorocarbon (raw material) per unit time (g / hr) fed per 1 g of alumina-containing catalyst, and the amount of fluorocarbon that comes into contact with the catalyst by being fed is preferably within the above range.
[0054] In the fluoroolefin production method of the present disclosure, the fluorocarbon is contacted with the alumina-containing catalyst at a temperature of preferably 300 to 800° C., more preferably 400 to 700° C., and even more preferably 400 to 600° C. When the contact temperature is 300° C. or higher, the conversion rate of the fluoroolefin is improved. On the other hand, when the contact temperature is 800° C. or lower, decomposition of the fluoroolefin can be suppressed.
[0055] When the contact temperature is 300° C. or higher, the reaction proceeds appropriately. On the other hand, when the contact temperature is 800° C. or lower, the selectivity decreases due to cleavage of the carbon-carbon bonds of the raw material, and the disproportionation reaction of the product (unsaturated compound) is suppressed.
[0056] Since the dehydrofluorination reaction is generally an endothermic reaction, a decrease in the conversion rate can be suppressed by appropriately maintaining the reaction temperature. As the reaction temperature in the catalyst layer increases, the conversion rate of the raw material increases. Therefore, it is preferable to maintain the reaction temperature in the catalyst layer at a desired temperature so as to maintain a high conversion rate. One way to maintain the reaction temperature in the catalyst layer at a desired temperature is, for example, to heat the catalyst layer externally with a heat medium or the like. Catalysts typically deteriorate over time as the reaction progresses. Even when a decrease in the conversion rate of the raw material occurs due to catalyst deterioration, the decrease in the conversion rate can be suppressed by heating the catalyst layer with a heat medium or the like and appropriately maintaining or increasing the reaction temperature. When maintaining or increasing the temperature of the catalyst layer, it is preferable to limit the temperature increase to 50° C. or less in order to suppress rapid catalyst deterioration.
[0057] At the start of the reaction, the reaction zone begins at the inlet of the raw material gas. As the catalyst at the inlet of the raw material gas deteriorates over time as the reaction progresses, the reaction zone moves downstream in the gas flow direction. Because the low-temperature product gas generated in the reaction zone flows into the vicinity of the downstream side of the reaction zone, the vicinity of the downstream side is usually the coldest in the catalyst layer. In the present disclosure, the temperature of this lowest temperature region of the catalyst layer is referred to as the "lowest temperature of the catalyst layer." The temperature further downstream from the vicinity of the downstream side usually increases from the lowest temperature of the catalyst layer as it moves away from the reaction zone.
[0058] In the fluoroolefin production method of the present disclosure, the fluorocarbon-containing raw material gas may be supplied to the reactor at room temperature. However, it is preferable to appropriately heat (preheat) the raw material gas before supplying it to the reactor. When preheating is performed, it is preferable to heat the raw material gas to a temperature of 80 to 600°C before supplying it to the reactor. Preheating to 80°C or higher makes it difficult for the internal temperature of the reactor to decrease, making it easier to achieve the set conversion rate. Furthermore, preheating to 600°C or lower makes it difficult for the internal temperature of the reactor to increase, suppressing undesirable reactions and improving selectivity.
[0059] The dehydrofluorination reaction in the present disclosure is a reaction in which the number of molecules increases, and therefore increasing the pressure makes the forward reaction unfavorable. The pressure when contacting the fluorocarbon with the alumina-containing catalyst is not particularly limited, but from the viewpoint of improving the conversion rate, it is preferably −0.05 to 2 MPa, more preferably −0.01 to 1 MPa, and even more preferably atmospheric pressure to 0.5 MPa. In the present disclosure, pressure means gauge pressure.
[0060] The contact time (seconds) between the fluorocarbon and the alumina-containing catalyst is preferably 0.5 to 100.0 seconds, more preferably 1.0 to 50.0 seconds, and even more preferably 2.0 to 20.0 seconds.
[0061] The contact time (seconds) is calculated using the following formula: Contact time (seconds) = [length (cm) of the reactor packed with the alumina-containing catalyst] / [linear velocity (cm / second)] The linear velocity refers to the speed at which the fluorocarbon passes through the alumina-containing catalyst per unit time.
[0062] Furthermore, the contact time (g sec / mL) between the fluorocarbon and the alumina-containing catalyst is preferably 1 to 200 g sec / mL, more preferably 5 to 175 g sec / mL, even more preferably 7 to 150 g sec / mL, and particularly preferably 10 to 125 g sec / mL. When the contact time (g sec / mL) is 1 g sec / mL or more, the conversion rate is improved. When the contact time (g sec / mL) is 200 g sec / mL or less, equipment costs can be reduced.
[0063] The contact time (g·sec / mL) is calculated using the following formula: Contact time (g·sec / mL)=[alumina-containing catalyst loading (g)] / [fluorocarbon flow rate (mL / sec)]
[0064] From the viewpoint of further suppressing the decrease in conversion, it is preferable to contact the fluorocarbon with the alumina-containing catalyst in the presence of an inert gas. The inert gas is preferably at least one selected from the group consisting of nitrogen, helium, argon, octafluorocyclobutane, and carbon dioxide. Among these, the inert gas is preferably nitrogen.
[0065] The molar ratio of the fluorocarbon to the inert gas in the gas phase is preferably 0.1 to 30, more preferably 0.5 to 25.
[0066] From the viewpoint of further suppressing a decrease in conversion rate, it is preferable that the fluorocarbon and the alumina-containing catalyst are contacted in the gas phase in the presence of water, and the water concentration is less than 500 ppm by mass relative to the total amount of the raw material gas containing the fluorocarbon. When the dehydrofluorination reaction is carried out in the gas phase in the presence of water, water is adsorbed to the Lewis acid sites on the surface of the alumina-containing catalyst. It is presumed that by making the water concentration less than 500 ppm by mass relative to the total amount of the raw material gas containing the fluorocarbon, the Lewis acid sites on the surface of the alumina-containing catalyst are suppressed from being crushed and forming a structure similar to a Bronsted acid site, thereby suppressing a decrease in catalytic activity. It is presumed that this increases the conversion rate and enables the target product to be obtained with high selectivity. The water concentration is preferably 300 ppm by mass or less, more preferably 100 ppm by mass or less, even more preferably 50 ppm by mass or less, and particularly preferably 10 ppm by mass or less, in order to further improve the conversion rate and obtain the target compound with even higher selectivity. Although a lower water concentration is preferred, from the viewpoints of the cost of dehydration treatment of fluorocarbons and inert gases and the difficulty of process control, a water concentration of 0.5 mass ppm or more is preferred, and 1 mass ppm or more is more preferred. When water reacts with an alkali metal or alkaline earth metal in the alumina-containing catalyst, the alumina-containing catalyst becomes alkaline. This changes the structure of the acid sites that exhibit the activity of dehydrofluorination, and it is preferable to suppress a decrease in catalytic activity.
[0067] A common method for measuring the water concentration is to use a commercially available Karl Fischer moisture meter.
[0068] The water concentration is the water content in the raw material gas when the fluorocarbon is brought into contact with the alumina-containing catalyst. Note that the water concentration may be replaced with the water content in the raw material gas before it is introduced into the reactor.
[0069] The method for producing a fluoroolefin of the present disclosure preferably further comprises a step of drying the alumina-containing catalyst before contacting the fluorocarbon with the alumina-containing catalyst. By drying the alumina-containing catalyst, water contained in the alumina-containing catalyst is removed, increasing the reactivity of the alumina-containing catalyst with the fluorocarbon and improving the conversion rate.
[0070] The method for drying the alumina-containing catalyst is not particularly limited, and the alumina-containing catalyst may be dried before being packed into the reactor, or may be dried after being packed into the reactor. When the alumina-containing catalyst is packed into the reactor and then dried, it is preferable because the reactor can be preheated while drying the alumina-containing catalyst. Specifically, it is preferable to dry the alumina-containing catalyst by packing the alumina-containing catalyst into the reactor and heating the reactor while circulating an inert gas.
[0071] In the fluoroolefin production method of the present disclosure, hydrogen fluoride is produced as a by-product. Hydrogen fluoride fluorides fluorinate the oxides contained in the alumina-containing catalyst, thereby strengthening its acidity. Therefore, it is preferable to reduce the concentration of hydrogen fluoride. Reducing the hydrogen fluoride concentration maintains the selectivity, suppresses deactivation of the alumina-containing catalyst, and suppresses a decrease in reaction activity due to a decrease in the specific surface area of the alumina-containing catalyst. One method for reducing the hydrogen fluoride concentration is to dilute it with an inert gas. Since the use of an inert gas increases the energy load in the purification process after the reaction, it is preferable to appropriately control the use of the inert gas. The hydrogen fluoride concentration during the reaction is preferably 15 mol% or less. From the viewpoint of extending the catalyst life, the hydrogen fluoride concentration is more preferably 13 mol% or less, even more preferably 10 mol% or less, particularly preferably 8 mol% or less, and most preferably 7 mol% or less. Furthermore, from the viewpoints of productivity and energy load in the purification step, the concentration of hydrogen fluoride is preferably 0.5 mol % or more, more preferably 0.8 mol % or more, even more preferably 1.0 mol % or more, particularly preferably 1.3 mol % or more, and most preferably 1.5 mol % or more.
[0072] The fluoroolefin production method of the present disclosure is preferably carried out in the presence of an oxidizing agent. The oxidizing agent is preferably oxygen, chlorine, bromine, or iodine, from the viewpoints of high conversion and high selectivity for obtaining the target compound. Of these, oxygen is more preferred as the oxidizing agent. In the present disclosure, the concentration of the oxidizing agent is preferably 0.01 to 21 mol% relative to the raw material gas. The concentration of the oxidizing agent is more preferably 1 to 20 mol%, even more preferably 5 to 18 mol%, and particularly preferably 7.5 to 16 mol%, relative to the raw material compound, from the viewpoints of further improving the conversion and obtaining the target compound with higher selectivity.
[0073] In the present disclosure, the conversion rate refers to the ratio (mol %) of the total molar amount of compounds other than the raw material compounds contained in the gas effluent from the reactor outlet to the molar amount of the raw material compounds supplied to the reactor. Generally, a higher conversion rate is preferable from the viewpoint of productivity. However, in the dehydrofluorination reaction of the present disclosure, it is preferable to appropriately control the conversion rate. When the conversion rate is controlled, the concentration of hydrogen fluoride produced in the gas phase is reduced, and it is thought that deactivation of the alumina-containing catalyst by hydrogen fluoride is suppressed. Although a method of diluting the gas phase with an inert gas is conceivable, the use of an inert gas increases the energy load in the purification process after the reaction, so the use of an excessive inert gas is not preferable. From the viewpoint of extending the catalyst life, it is preferable to suppress the hydrogen fluoride concentration during the reaction to 15 mol % or less.
[0074] In particular, in the fluoroolefin production process of the present disclosure, by using HFC-134a as the fluorocarbon, the conversion rate does not become too high and deactivation of the alumina-containing catalyst is suppressed.
[0075] From the above viewpoints, the conversion rate 10 hours after contacting the fluorocarbon with the catalyst is preferably 5.0 to 15.0%, more preferably 7.0 to 13.0%, and even more preferably 5.0 to 12.5%.
[0076] In the present disclosure, selectivity refers to the ratio (mol %) of the molar amount of the target product contained in the reactor outlet gas to the total molar amount of compounds other than the raw material compounds contained in the reactor outlet gas. A selectivity of 100% is preferable because a post-reaction purification step is unnecessary, but side reactions may occur in the reaction temperature range required to obtain a desired conversion rate. A higher selectivity is preferable because it reduces the amount of waste, the energy load in the post-reaction purification step, and the catalyst life can be extended. The selectivity 10 hours after contacting the fluorocarbon with the alumina-containing catalyst is preferably 90% or more, more preferably 93% or more, and even more preferably 95% or more. In particular, in the fluoroolefin production method of the present disclosure, HFO-1123 can be obtained with high selectivity by using HFC-134a as the fluorocarbon.
[0077] Examples of compounds other than the raw material compounds and the target product contained in the reactor outlet gas include hydrogen fluoride, carbon monoxide, carbon dioxide, water, etc. For example, when HFC-134a is used as the fluorocarbon raw material compound, examples of other compounds include HFC-134, 1,1-difluoroethylene (VdF), E / Z-1,2-difluoroethylene (HFO-1132(E) / (Z)), etc.
[0078] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to the following examples as long as it does not depart from the gist of the disclosure. Examples 1 to 9 are examples, and Examples 10 to 13 are comparative examples.
[0079] Example 1 1 mL of γ-alumina (product name "N612N", manufactured by JGC Catalysts and Chemicals) was weighed out and used as a catalyst. A stainless steel (SUS304) reaction tube with an inner diameter of 10 mm and a length of 30 cm was packed with the catalyst and placed in a tubular electric furnace. The catalyst-packed section was heated to 475°C in the tubular furnace while flowing nitrogen, thereby dehydrating the catalyst. Thereafter, a 0.1 / 1 (mol / mol) mixed gas of nitrogen / HFC-134a was passed through the tube for a contact time of 4.7 seconds, thereby carrying out a dehydrogenation reaction to produce HFO-1123. The water concentration in the 0.1 / 1 (mol / mol) mixed gas of nitrogen / HFC-134a was measured using a Karl Fischer moisture content analyzer and was found to be 5 ppm.
[0080] [Examples 2 to 13] In Examples 2 to 13, the HF deprotection reaction was carried out in the same manner as in Example 1, except that the catalyst was changed and the various conditions were changed to the values shown in Table 2. The catalysts used in Examples 2 to 13 are described below.
[0081] (Example 2) γ-alumina (product name "N612N", manufactured by JGC Catalysts and Chemicals Co., Ltd.) was pulverized in a mortar to obtain a powder. The obtained powder was calcined in an air atmosphere at 1300°C for 6 hours, and then analyzed by X-ray diffraction, which revealed that α-alumina was the main component. This powder was used as a catalyst.
[0082] Example 3 α-alumina (product name "SA52124", manufactured by Saint-Gobain) was used as a catalyst.
[0083] Example 4 α-alumina (product name "SA52238", manufactured by Saint-Gobain) was used as a catalyst.
[0084] Example 5 α-alumina (product name "FGL-30", manufactured by Iwatani Chemical Industries, Ltd.) was used as a catalyst.
[0085] Example 6 α-alumina (product name "FGL-40", manufactured by Iwatani Chemical Industries, Ltd.) was used as a catalyst.
[0086] Example 7 α-alumina (product name "C500", manufactured by Nippon Light Metal Co., Ltd.) was used as a catalyst.
[0087] Example 8 α-alumina (product name "LT303D", manufactured by Nippon Light Metal Co., Ltd.) was used as a catalyst.
[0088] Example 9 α-alumina (product name "AKQ-10", manufactured by Sumitomo Chemical Co., Ltd.) was used as a catalyst.
[0089] Example 10 α-alumina (product name "SA51161", manufactured by Saint-Gobain) was used as a catalyst.
[0090] Example 11 α-alumina (product name "SA5561", manufactured by Saint-Gobain) was used as a catalyst.
[0091] Example 12 α-alumina (product name "SA5218", manufactured by Saint-Gobain) was used as a catalyst.
[0092] Example 13 α-alumina (product name "SA5252", manufactured by Saint-Gobain) was used as a catalyst.
[0093] Elemental analysis of each catalyst was carried out using a ZSX Primus II (scanning X-ray fluorescence analyzer) manufactured by Rigaku Corporation under conditions of an X-ray output of 50 kV, 72 mA, a measurement area of 20 mmφ, and a measurement time of 30 minutes. The results of the elemental analysis of the catalysts used in Examples 1 to 13 are shown in Table 1. The values in the table are in mass%, and blank spaces indicate that the corresponding element was below the detection limit.
[0094]
[0095] The contact time (seconds) was calculated using the following formula: Contact time (seconds) = [length of catalyst packed in reactor (cm)] / [linear velocity (cm / second)] The linear velocity refers to the speed at which the fluorocarbon passes through the catalyst per unit time.
[0096] The contact time (g min / mL) was calculated using the following formula: Contact time (g min / mL) = [catalyst loading (g)] / [fluorocarbon flow rate (mL / min)]
[0097] In the reactions of Examples 1 to 13, the product gas (hereinafter also referred to as "reactor outlet gas") taken out from the outlet of the reactor 10 hours after the start of the reaction was analyzed by gas chromatography. Specifically, a column (product name "DB-1301", manufactured by Agilent, length 60 m, inner diameter 0.25 mm, film thickness 1 μm) was attached to a gas chromatograph (product name "GC6850", manufactured by Agilent) and the analysis was performed. The conversion of HFC-134a and the selectivity of HFO-1123 were calculated using the molar amount calculated from the area ratio (GCArea%) of the reactor outlet gas.
[0098] (Conversion rate of HFC-134a) The molar amount M of HFC-134a fed to the reactor 134a The conversion rate of HFC-134a (%) is calculated by the following formula: M1 / M 134a ) x 100
[0099] (Selectivity of HFO-1123) The molar amount M of HFO-1123 contained in the reactor outlet gas relative to the total molar amount M1 of compounds other than HFC-134a contained in the reactor outlet gas is 1123 The selectivity of HFO-1123 (%) = (M 1123 / M1) x 100
[0100]
[0101] As shown in Table 2, Examples 1 to 9 included a step of contacting a fluorocarbon represented by formula (1) with a catalyst to produce a fluoroolefin represented by formula (2), and the alumina-containing catalyst satisfied at least one of the following conditions: (I) a total content of alkali metal elements and alkaline earth metal elements of 100 ppm by mass or less, and (II) a Si content of 1,000 ppm by mass or less. Therefore, it was found that the conversion rate was higher than that of conventional methods. On the other hand, Examples 10 to 13, which did not satisfy either (I) or (II), had significantly lower conversion rates than Examples 1 to 9. Furthermore, Examples 10 to 13 also had significantly lower selectivities than Examples 1 to 9.
[0102] The disclosure of Japanese Patent Application No. 2023-072721 is incorporated herein by reference in its entirety. All documents, patent applications, and technical standards mentioned herein are incorporated herein by reference to the same extent as if each individual document, patent application, and technical standard was specifically and individually indicated to be incorporated by reference.
Claims
1. A method for producing a fluoroolefin, comprising the step of contacting a fluorocarbon represented by the following formula (1) with an alumina-containing catalyst to produce a fluoroolefin represented by the following formula (2), wherein the alumina-containing catalyst satisfies at least one of the following (I) and (II): 1 X 2 F-CX 3 X 4 H ... (1) CX 1 X 2 = C.X. 3 X 4 ... (2) In formula (1) and formula (2), X 1 , X 2 , X 3 , and X 4 each independently represents a hydrogen atom or a fluorine atom, provided that X 1 , X 2 , X 3 , and X 4 At least one of the above is a fluorine atom. (I) The total content of alkali metal elements and alkaline earth metal elements is 100 ppm by mass or less. (II) The content of Si is 1000 ppm by mass or less.
2. The method for producing a fluoroolefin according to claim 1, wherein the alumina contained in the alumina-containing catalyst comprises α-alumina.
3. The method for producing a fluoroolefin according to claim 1 or 2, wherein the fluorocarbon is at least one selected from the group consisting of 1,1,1-trifluoroethane, 1,1,2-trifluoroethane, 1,1,2,2-tetrafluoroethane, and 1,1,1,2-tetrafluoroethane.
4. The method for producing a fluoroolefin according to claim 1 or 2, wherein the fluoroolefin is at least one selected from the group consisting of 1,2-difluoroethylene, 1,1-difluoroethylene, and trifluoroethylene.
5. A method for producing a fluoroolefin according to claim 1 or 2, wherein the fluorocarbon is 1,1,1,2-tetrafluoroethane and the fluoroolefin is trifluoroethylene.
6. The method for producing a fluoroolefin according to claim 1 or 2, wherein the fluorocarbon is contacted with the alumina-containing catalyst at a temperature of 300 to 800°C.
7. The method for producing a fluoroolefin according to claim 1 or 2, wherein the fluorocarbon is contacted with the alumina-containing catalyst in the presence of an inert gas, and the inert gas is at least one selected from the group consisting of nitrogen, helium, argon, octafluorocyclobutane, and carbon dioxide.
8. The method for producing a fluoroolefin according to claim 1 or 2, further comprising the step of drying the alumina-containing catalyst prior to contacting the fluorocarbon with the alumina-containing catalyst.
9. The method for producing a fluoroolefin according to claim 1 or 2, wherein the fluorocarbon and the alumina-containing catalyst are contacted in a gas phase in the presence of water, and the concentration of the water is less than 500 ppm by mass based on the total amount of the raw material gas containing the fluorocarbon.
Citation Information
Patent Citations
Method for co-production of trifluoroethylene and hydrogen fluoride
CN103288589A
Catalytic process for producing 1,3,3,3 - tetrafluoropropene
JP2016520097A
Method for producing trifluoroethylene
WO2015147063A1
Process for producing hydrofluoroolefin
WO2016163522A1
Method for producing hydrofluoroolefin
WO2017104829A1