Polishing agent, polishing method, method for producing semiconductor component, and additive liquid for polishing agent
The polishing agent with anionic polymers and acidic compounds addresses the challenge of achieving high selectivity and stability in CMP processes, ensuring effective polishing and storage stability for semiconductor manufacturing.
Patent Information
- Application Number
- PCT/JP2024/014312
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-08
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional chemical mechanical polishing (CMP) methods face challenges in achieving high selectivity between silicon oxide films and stopper films while maintaining the polishing rate of silicon oxide films, especially in semiconductor manufacturing, where high flatness and miniaturization are critical, and existing solutions lack storage stability and pH/viscosity control.
A polishing agent comprising abrasive grains, an anionic polymer with specific acid value and hydrophobic monomer distribution, and an acidic compound, which maintains a pH difference within 1.5 units of the acidic compound's pKa, ensuring high selectivity and stability, is used in conjunction with a polishing method involving relative movement between the polishing pad and semiconductor substrate.
The solution achieves high selectivity between silicon oxide and stopper films, maintains the polishing rate of silicon oxide films, and exhibits excellent storage stability and pH/viscosity control, enabling high-speed polishing and improved flatness in semiconductor component manufacturing.
Smart Images

Figure JP2024014312_31102024_PF_FP_ABST
Abstract
Description
Abrasive, polishing method, semiconductor component manufacturing method, and additive for abrasive
[0001] The present disclosure relates to an abrasive, a polishing method, a method for manufacturing semiconductor components, and an additive liquid for an abrasive.
[0002] As semiconductor integrated circuits become more highly integrated and functional, microfabrication techniques are being developed to miniaturize and increase the density of semiconductor elements. Conventionally, in the manufacture of semiconductor integrated circuit devices (hereinafter also referred to as semiconductor devices), chemical mechanical polishing (hereinafter referred to as CMP) has been used to planarize interlayer insulating films, buried wiring, etc., in order to prevent problems such as unevenness (steps) on layer surfaces exceeding the depth of focus of lithography, making it impossible to obtain sufficient resolution. As the demand for higher definition and miniaturization of elements becomes more stringent, the importance of high planarization by CMP is increasing.
[0003] Furthermore, in the manufacture of semiconductor devices, shallow trench isolation (hereinafter referred to as STI), which uses a narrow element isolation width, has been introduced to promote further miniaturization of semiconductor elements. STI is a technique for forming an electrically isolated element region by forming a trench (groove) in a silicon substrate and filling the trench with an insulating film. An example of STI will be described with reference to FIGS. 1A and 1B . In this example, as shown in FIG. 1A , an element region of a silicon substrate 1 is first masked with a stopper film 2, and then a trench 3 is formed in the silicon substrate 1, and an insulating film such as a silicon oxide film 4 is deposited to fill the trench 3. Next, the silicon oxide film 4 on the stopper film 2, which is the protruding portion, is polished and removed by CMP while leaving the silicon oxide film 4 in the trench 3, which is the recessed portion. As shown in FIG. 1B , an element isolation structure in which the silicon oxide film 4 is filled in the trench 3 is obtained.
[0004] In CMP for STI, by increasing the selectivity (polishing rate ratio) between the silicon oxide film and the stopper film, the polishing can be stopped when the stopper film is exposed. Examples of such stopper films include nitride films and polysilicon. Polishing methods using stopper films can obtain smoother surfaces than conventional polishing methods. Furthermore, a high selectivity is required in recent CMP technology.
[0005] For example, Patent Document 1 discloses a polishing agent containing a specific water-soluble polymer, cerium oxide particles, and water, and having a pH of 4 to 9, as a method for increasing the selectivity between a silicon dioxide film and a silicon nitride film.
[0006] JP 2019-87660 A
[0007] In view of the above problems, the present disclosure aims to provide a polishing agent that can obtain a high selectivity between a silicon oxide film and a stopper film while maintaining the polishing rate of the silicon oxide film and that also has excellent storage stability, an additive liquid for the polishing agent for use in preparing the polishing agent, a polishing method that allows high-speed polishing, and a method for manufacturing semiconductor components using the polishing method.
[0008] The present disclosure provides a polishing compound, a polishing compound additive, a polishing method, and a method for manufacturing semiconductor components, each having the following configuration: [1] A polishing compound comprising abrasive grains, an anionic polymer, an acidic compound selected from a phosphoric acid compound and an organic acid compound, and water, wherein the anionic polymer is a copolymer containing a hydrophobic monomer and an anionic monomer, the anionic polymer has an acid value of 20 mg KOH / g to 400 mg KOH / g, the hydrophobic monomer has a partition coefficient (log D) of 0 to 4, and the anionic monomer comprises at least one selected from unsaturated monocarboxylic acids and salts thereof, and wherein, when the acidic compound with the highest molar concentration among the acidic compounds is designated as a first acidic compound, the pKa of the first acidic compound and the pH of the polishing compound satisfy the relationship shown in formula (1): |pKa - pH| ≦ 1.5 (1) where, when the first acidic compound has two or more acid dissociation constants, the pKa represents the acid dissociation constant closest to the pH. [2] The abrasive of [1], wherein the abrasive grains comprise at least one selected from the group consisting of silica particles, alumina particles, zirconia particles, cerium compound particles, titania particles, germania particles, composite particles thereof, and core-shell particles. [3] The abrasive of [1] or [2], wherein the abrasive grains comprise cerium compound particles. [4] The abrasive of any one of [1] to [3], wherein the abrasive grains comprise ceria particles. [5] The abrasive of any one of [1] to [4], wherein the abrasive grains are contained in an amount of 0.01% by mass to 10.0% by mass relative to the total mass of the abrasive. [6] The abrasive of any one of [1] to [5], wherein the anionic polymer has an acid value of 20 mg KOH / g to 300 mg KOH / g. [7] The abrasive of any one of [1] to [6], wherein the hydrophobic monomer has a partition coefficient (log D) of 0 to 3. [8] The polishing agent of any one of [1] to [7], wherein the hydrophobic monomer comprises alkyl(meth)acrylate. [9] The polishing agent of any one of [1] to [8], wherein the weight-average molecular weight of the anionic polymer is 1,000 to 100,000.
[10] The polishing agent of any one of [1] to [9], wherein the ratio of the hydrophobic monomer in the anionic polymer is 10 to 95 mol % based on the total monomers constituting the anionic polymer.
[11] The polishing agent of any one of [1] to
[10] , wherein the content of the anionic polymer is 0.02% by mass to 0.5% by mass relative to the total mass of the polishing agent.
[12] The polishing agent of any one of [1] to
[11] , wherein the pKa is 4 to 9.
[13] The polishing agent of any one of [1] to
[12] , further comprising a nonionic polymer.
[14] The polishing agent of any one of [1] to
[13] , wherein the pH is 4 to 9.
[15] A polishing method in which a polished surface of a semiconductor substrate is brought into contact with a polishing pad while supplying an abrasive, and polishing is performed by the relative movement of the two, wherein the abrasive is the abrasive of any one of [1] to
[14] .
[16] A method for producing semiconductor components, wherein semiconductor components are obtained by singulating a semiconductor substrate having a polished surface polished by the polishing method of
[15] .
[17] An additive liquid for an abrasive comprising an anionic polymer, an acidic compound selected from a phosphoric acid compound and an organic acid compound, and water, wherein the anionic polymer is a copolymer containing a hydrophobic monomer and an anionic monomer, the anionic polymer has an acid value of 20 mg KOH / g to 400 mg KOH / g, the hydrophobic monomer has a partition coefficient (log D) of 0 to 4, and the anionic monomer comprises at least one selected from unsaturated monocarboxylic acids and salts thereof, and wherein, when the acidic compound having the highest molar concentration is designated as a first acidic compound, the pKa of the first acidic compound and the pH of the additive liquid for an abrasive satisfy the relationship shown in formula (1): |pKa - pH| ≦ 1.5 (1), where, when the first acidic compound has two or more acid dissociation constants, the pKa represents the acid dissociation constant closest to the pH.
[0009] According to the present disclosure, it is possible to provide an abrasive that can obtain a high selectivity between a silicon oxide film and a stopper film while maintaining the polishing rate of the silicon oxide film and that also has excellent storage stability, an abrasive additive liquid for preparing the abrasive, a polishing method that allows high-speed polishing, and a method for manufacturing semiconductor components using the polishing method.
[0010] 1 is a cross-sectional view showing an example of a polishing method, the cross-sectional view showing a state of an object to be polished before polishing, a cross-sectional view showing an example of a polishing method, the cross-sectional view showing a state of an object to be polished after polishing, and a schematic view showing an example of a polishing apparatus.
[0011] Hereinafter, embodiments of the present invention will be described. The present invention is not limited to the following embodiments, and other embodiments may also fall within the scope of the present invention as long as they are consistent with the spirit of the present invention. For clarity of explanation, the following description and drawings have been simplified as appropriate. Also, for the purpose of explanation, the scale of each component in the drawings may differ significantly.
[0012] In this disclosure, the term "surface to be polished" refers to the surface to be polished of the object to be polished, for example, the surface. In this specification, the term "surface to be polished" also includes intermediate surfaces that appear on semiconductor substrates in the process of manufacturing semiconductor devices. "Silicon oxide" is primarily silicon dioxide, but is not limited to this and may include silicon oxides other than silicon dioxide. "Selectivity" refers to the polishing rate (R A ) the polishing rate (R B ) to the ratio (R A / R B "(Meth)acrylic" is a general term for "methacrylic" and "acrylic," and also includes (meth)acryloyl and (meth)acrylate. Unless otherwise specified, "to" indicating a range of values includes the values before and after it as the lower and upper limits.
[0013] [Abrasive] The abrasive of the present disclosure (hereinafter also referred to as the present abrasive) comprises abrasive grains, an anionic polymer, an acidic compound selected from a phosphoric acid compound and an organic acid compound, and water, wherein the anionic polymer is a copolymer comprising a hydrophobic monomer and an anionic monomer, the anionic polymer has an acid value of 20 mg KOH / g to 400 mg KOH / g, the hydrophobic monomer has a partition coefficient (log D) of 0 to 4, and the anionic monomer comprises at least one selected from unsaturated monocarboxylic acids and salts thereof, and wherein, when the acidic compound with the highest molar concentration is designated as a first acidic compound, the pKa of the first acidic compound and the pH of the abrasive satisfy the relationship shown in formula (1): |pKa - pH| ≦ 1.5 (1) where, when the first acidic compound has two or more acid dissociation constants, the pKa represents the acid dissociation constant closest to the pH.
[0014] By using this abrasive in CMP of a polishing surface including a silicon oxide film in STI, for example, a high polishing rate for the silicon oxide film is maintained while polishing of the stopper film is suppressed, a high selectivity between the silicon oxide film and the stopper film can be obtained, and polishing with high flatness can be achieved. In addition, this abrasive has excellent storage stability, and changes in pH and viscosity are suppressed even when stored for a long period of time.
[0015] The stopper film may be, for example, a compound containing one or more elements selected from silicon, carbon, hafnium, zirconium, cobalt, ruthenium, molybdenum, titanium, tantalum, and copper, or a nitride or oxide containing one or more of these elements. More specifically, examples include elemental metals such as copper, cobalt, ruthenium, molybdenum, titanium, and tantalum; nitrides such as titanium nitride, tantalum nitride, and silicon nitride; oxides such as zirconia and hafnium oxide; polysilicon, amorphous silicon, hafnium silicate, zirconium silicate, and silicon carbide. Among these, silicon nitride or polysilicon is preferred because it can provide a higher selectivity.
[0016] This polishing agent contains at least abrasive grains, an anionic polymer, an acidic compound, and water, and may further contain other components as long as the effects of this embodiment are achieved. Each component that can be contained in this polishing agent will be described below.
[0017] <Abrasive grains> In the present polishing agent, the abrasive grains can be appropriately selected from those used as abrasive grains for CMP. Examples of the abrasive grains include at least one selected from the group consisting of silica particles, alumina particles, zirconia particles, cerium compound particles (e.g., ceria particles, cerium hydroxide particles), titania particles, germania particles, and core-shell type particles having these as core particles. Examples of the silica particles include colloidal silica and fumed silica. Examples of the alumina particles include colloidal alumina.
[0018] The core-shell particles are composed of a core particle (e.g., silica particle, alumina particle, zirconia particle, cerium compound particle, titania particle, or germania particle) and a thin film covering the surface of the core particle. The thin film may be made of at least one oxide selected from the group consisting of silica, alumina, zirconia, ceria, titania, germania, iron oxide, manganese oxide, zinc oxide, yttrium oxide, calcium oxide, magnesium oxide, lanthanum oxide, and strontium oxide. The thin film may also be composed of a plurality of nanoparticles made of these oxides.
[0019] The particle size of the core particle is preferably 0.01 μm to 0.5 μm, more preferably 0.03 μm to 0.3 μm. The particle size of the nanoparticles is only required to be smaller than the particle size of the core particle, and is preferably 1 nm to 100 nm, more preferably 5 nm to 80 nm.
[0020] Among the above-mentioned abrasive grains, silica particles, alumina particles, or cerium compound particles are preferred because of their excellent insulating film removal rate, and cerium compound particles are more preferred. When the surface to be polished contains an insulating film (particularly a silicon oxide film), ceria particles are even more preferred because of their high removal rate. In the case of core-shell type particles, the thin film preferably contains silica, alumina, or a cerium compound, and more preferably contains ceria. One type of abrasive grain can be used alone, or two or more types can be used in combination.
[0021] The content of ceria relative to the total mass of the abrasive grains is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 100% by mass. If the content of ceria relative to the total mass of the abrasive grains is 70% by mass or more, the polishing rate, particularly for insulating films, is easily improved.
[0022] The ceria particles can be appropriately selected from known ones and can be used, and examples thereof include ceria particles produced by the methods described in JP-A-11-12561, JP-A-2001-35818, and JP-A-2010-505735. Specific examples include ceria particles obtained by adding an alkali to an aqueous solution of cerium (IV) ammonium nitrate to produce a cerium hydroxide gel, which is then filtered, washed, and fired; ceria particles obtained by crushing high-purity cerium carbonate, then crushing and classifying it; and ceria particles obtained by chemically oxidizing a cerium (III) salt in a liquid.
[0023] Although the ceria particles may contain impurities other than ceria, the content of ceria in one ceria particle is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and most preferably 100% by mass (without impurities). If the content of ceria in the ceria particles is 80% by mass or more, the polishing rate of the insulating film is likely to be improved.
[0024] The average particle size of the abrasive grains is preferably 0.01 μm to 0.5 μm, and more preferably 0.03 μm to 0.3 μm. If the average particle size is 0.5 μm or less, the mechanical effect on the polished surface is reduced, thereby suppressing the occurrence of polishing defects such as scratches on the polished surface. Furthermore, if the average particle size is 0.01 μm or more, aggregation of the abrasive grains is suppressed, resulting in excellent storage stability of the abrasive and an excellent polishing rate. Note that since the abrasive grains exist in the liquid as aggregated particles (secondary particles) formed by aggregation of primary particles, the above average particle size is the average secondary particle size. The average secondary particle size is measured using a particle size distribution analyzer such as a laser diffraction / scattering type using a dispersion liquid in which the abrasive grains are dispersed in a dispersing medium such as pure water.
[0025] The lower limit of the abrasive content is preferably 0.01% by mass, more preferably 0.05% by mass, even more preferably 0.1% by mass, and particularly preferably 0.15% by mass, relative to the total mass of the abrasive. If the abrasive content is equal to or greater than the lower limit, an excellent polishing rate for the surface to be polished can be obtained. On the other hand, the upper limit of the abrasive content is preferably 10.0% by mass, more preferably 8.0% by mass, even more preferably 5.0% by mass, particularly preferably 2.0% by mass, particularly more preferably 1.0% by mass, extremely preferably 0.8% by mass, and most preferably 0.5% by mass, relative to the total mass of the abrasive. If the abrasive content is equal to or less than the upper limit, aggregation of the abrasive can be suppressed, and an increase in the viscosity of the abrasive can be suppressed, resulting in excellent handleability.
[0026] The zeta potential (surface potential) of the abrasive grains in the polishing agent is preferably negative (less than 0 mV), more preferably -200 mV to -10 mV, even more preferably -150 mV to -20 mV, and particularly preferably -100 mV to -30 mV. When the zeta potential of the abrasive grains is within the above range, the dispersion stability of the abrasive grains and the flatness of the silicon oxide film after polishing can be improved. The zeta potential of the abrasive grains can be measured, for example, using a dynamic light scattering zeta potential measuring device (e.g., manufactured by Beckman Coulter, Inc., product name: DelsaNano C). The zeta potential of the abrasive grains can be adjusted using an anionic polymer, acidic compound, additive, etc., as described below.
[0027] <Anionic Polymer> In this polishing compound, the anionic polymer is a copolymer containing a hydrophobic monomer having a partition coefficient (log D) of 0 to 4 and an anionic monomer containing at least one selected from unsaturated monocarboxylic acids and salts thereof, and has an acid value of 20 mg KOH / g to 400 mg KOH / g. Use of this specific anionic polymer suppresses polishing of the stopper film, thereby achieving a high selectivity between the silicon oxide film and the stopper film. The composition of the anionic polymer is described below.
[0028] (Hydrophobic Monomer) In the present disclosure, a hydrophobic monomer refers to a monomer that dissolves in 100 g of water at 20° C. (hereinafter also referred to as "solubility") in an amount of 10 g or less. The anionic polymer is selected from hydrophobic monomers and used from those having a partition coefficient (log D) of 0 to 4. When the anionic polymer contains a structural unit derived from the hydrophobic monomer, polishing of the stopper film is further suppressed. The partition coefficient of the hydrophobic monomer is preferably 0 to 3.
[0029] In the present disclosure, the partition coefficient (log D) of a hydrophobic monomer represents the partition coefficient of a molecule between an aqueous phase and a lipophilic phase. Specifically, the hydrophobic monomer to be measured, water (a buffer solution), and an organic solvent (n-octanol) are placed in a container and thoroughly shaken, followed by phase separation. The amount of the hydrophobic monomer in each phase is quantified, and the concentration Co in the organic solvent and the concentration Cw in water are determined, respectively, and the common logarithm of the concentration ratio (Co / Cw) is calculated. The partition coefficient (log D) in the present disclosure is determined using a buffer solution as the aqueous phase and a pH of about 5.5. For monomers with known partition coefficients, literature values may be referenced. The lower limit of the log D of the hydrophobic monomer is 0, preferably 0.5, and more preferably 1.0, from the viewpoint of improving the selectivity. The upper limit of the log D of the hydrophobic monomer is 4, preferably 3.5, and more preferably 3.0, from the viewpoint of improving the polishing rate of the silicon oxide film.
[0030] The solubility of the hydrophobic monomer is preferably 7 g or less, more preferably 5 g or less, even more preferably 3 g or less, and particularly preferably 2 g or less. The solubility parameter (SP value) of the hydrophobic monomer is preferably 10.5 or less, more preferably 10.2 or less, even more preferably 10.0 or less, even more preferably 9.8 or less, and particularly preferably 9.6 or less.
[0031] As the hydrophobic monomer, a monomer having no ionic group or hydrophilic group is preferred, and a compound represented by the following formula (2) is more preferred. However, R 1 is a hydrogen atom or a methyl group, R 11 represents a hydrocarbon group which may have O or Si between carbon atoms and in which a hydrogen atom may be substituted with a halogen atom, and L 1 is a single bond or a divalent linking group.
[0032] In the above formula (2), R 11 is a substituent that exhibits hydrophobicity, and is a hydrocarbon group that may have O or Si between carbon atoms and in which a hydrogen atom may be substituted with a halogen atom. 11 Examples of the hydrocarbon group in (I) include an alkyl group, an aryl group, and an aralkyl group. The alkyl group may be linear, branched, or cyclic. The alkyl group preferably has 1 to 18 carbon atoms, and more preferably 1 to 12 carbon atoms. Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, various pentyl groups, various hexyl groups, various octyl groups, various decyl groups, a cyclopentyl group, a cyclohexyl group, a cyclooctyl group, a cyclododecyl group, a bornyl group, and an adamantyl group. Examples of the aryl group include a phenyl group, a biphenyl group, a naphthyl group, a tolyl group, and a xylyl group. The aryl group preferably has 6 to 24 carbon atoms, and more preferably 6 to 12 carbon atoms. Examples of the aralkyl group include a benzyl group, a phenethyl group, a naphthylmethyl group, and a biphenylmethyl group. The number of carbon atoms in the aralkyl group is preferably 7 to 20, and more preferably 7 to 14. 11When R has an aromatic ring, the hydrogen atom of the aromatic ring may have a substituent such as a linear or branched alkyl group having 1 to 4 carbon atoms. 11 The hydrocarbon group in the formula (I) may further have O or Si between carbon atoms, and a hydrogen atom may be substituted with a halogen atom. Examples of the hydrocarbon group having O or Si between carbon atoms include -(CH 2 CH 2 O) x -, -(CH 2 O) x - and alkylene oxides such as -CH 2 Si(R 12 ) 2 -CH 2 Here, x represents the number of repeating units, and is preferably an integer of 1 to 18. 12 are each independently a hydrogen atom or a methyl group. 11 The hydrogen atoms of the hydrocarbon groups in the above structures may be substituted with halogen atoms. Examples of halogen atoms include F, Cl, Br, and I. 11 is preferably a hydrocarbon group that does not contain O, Si, or halogen atoms, from the viewpoint of hydrophobicity and availability.
[0033] L 1 is an unsaturated double bond and R 11 is a single bond or a divalent linking group connecting 1 Examples of the alkylene group include alkylene groups having 1 to 8 carbon atoms, -(CH 2 CH 2 O) x -, -(CH 2 O) x -, -CONH-, -COO-, -C(=O)-, etc. Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group. 1 is preferably a single bond, —CONH—, or —COO— because of ease of availability.
[0034] The hydrophobic monomer may be used alone or in combination of two or more. From the viewpoint of dispersibility in the abrasive, the hydrophobic monomer may be a combination of a monomer having a ring structure and a monomer not having a ring structure.
[0035] Specific examples of hydrophobic monomers include alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-dodecyl (meth)acrylate, and stearyl (meth)acrylate; (meth)acrylates having a ring structure such as 1-methylcyclopentyl acrylate, cyclohexyl (meth)acrylate, and benzyl (meth)acrylate; Examples of the vinyl monomer include styrene, methylstyrene, vinyltoluene, p-t-butylstyrene, chloromethylstyrene, vinyl chloride, vinylidene chloride, vinyl fluoride, and vinylidene fluoride. Among these, it is preferable to contain an alkyl(meth)acrylate, and more preferable to contain an alkyl(meth)acrylate having an alkyl group having 1 to 6 carbon atoms.
[0036] (Anionic Monomer) In the present disclosure, the anionic monomer includes at least one selected from unsaturated monocarboxylic acids and salts thereof (hereinafter also referred to as unsaturated carboxylic acids, etc.). When the anionic polymer has a structural unit derived from the unsaturated monocarboxylic acid, the carboxy group is adsorbed to the stopper film, and the anionic polymer acts as a protective film for the stopper film.
[0037] As the anionic monomer, a monomer having no ionic group or hydrophilic group is preferred, and a compound represented by the following formula (3) is more preferred. However, R 2 , R 3 , and R 4are each independently a hydrogen atom or a hydrocarbon group, 5 is a group having a carboxy group or a salt thereof.
[0038] R 2 ~R 4 Examples of the hydrocarbon group in R include an alkyl group, an aryl group, and an aralkyl group. Specific examples of the alkyl group, the aryl group, and the aralkyl group are those shown in the above R 11 In this polishing compound, in view of the interaction between the carboxyl group and the stopper film, R 2 ~R 4 The hydrocarbon group in is preferably an alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 6 carbon atoms, and among these, a methyl group or an ethyl group is preferred, with a methyl group being more preferred.
[0039] R 5 The group having a carboxy group or a salt thereof in 2 -R 21 It is preferable that the above L 2 is an unsaturated double bond and R 21 is a single bond or a divalent linking group connecting 2 Examples of the alkylene group include an alkylene group having 1 to 8 carbon atoms, a phenylene group, and —(CH 2 CH 2 O) x -R 22 -, -(CH 2 O) x -R 22 --, --CONH-R 22 -, -COO-R 22 -, etc., where x is an integer of 1 to 18, and R 22 is preferably a single bond or an alkylene group having 1 to 8 carbon atoms. 2 and R 22 Examples of the alkylene group in L include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group, and each may have a halogen atom as a substituent. 2 is preferably a single bond, an alkylene group, or a phenylene group from the viewpoint of easy availability of the monomer.
[0040] R21 is a carboxy group or a salt thereof. When the carboxy group is a salt, examples of the counter cation include an alkali metal ion, an alkaline earth metal ion, and an ammonium ion.
[0041] In formula (3), R 2 ~R 5 A preferred combination of (I) R 2 is hydrogen or a methyl group, R 3 ~R 4 is a hydrogen atom, R 5 (II) R is a combination of carboxy groups, etc. (acrylic acid, methacrylic acid); 2 and R 3 is a hydrogen atom, R 4 is hydrogen or an alkyl group, R 5 Ga-L 2 -R 21 , L 2 is a combination of alkylene groups (unsaturated fatty acids); (III) R 2 ~R 4 is a hydrogen atom, R 5 Ga-L 2 -R 21 , L 2 and the combination of a phenylene group (vinyl benzoic acid).
[0042] Specific examples of the anionic monomer represented by formula (3) include (meth)acrylic acid, vinylbenzoic acid, 2-carboxyethyl (meth)acrylate, unsaturated fatty acids, etc. The anionic monomers can be used alone or in combination of two or more.
[0043] The anionic monomer may also contain an anionic monomer other than the unsaturated monocarboxylic acid, as long as the effects of this embodiment are achieved. Examples of such anionic monomer include allyl sulfonic acid, methallyl sulfonic acid, 2-(meth)acryloyloxyethyl acid phosphate, maleic acid (maleic anhydride), fumaric acid, itaconic acid, citraconic acid, and mesaconic acid. The proportion of such anionic monomer is preferably 5 mol % or less, more preferably 2 mol % or less, and even more preferably 1 mol % or less, based on the total amount of anionic monomers. It is particularly preferable that the anionic monomer is substantially free of such anionic monomer.
[0044] (Other Monomers) The anionic polymer may contain other monomers in addition to the hydrophobic monomer and the anionic monomer, as long as the effects of this embodiment are achieved. Examples of other monomers include (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N,N-dibutyl(meth)acrylamide, N-tert-butylacrylamide, N-phenyl(meth)acrylamide, and (meth)acrylamide derivatives such as N-benzyl(meth)acrylamide. The proportion of the other monomers is preferably 5 mol % or less, more preferably 1 mol % or less, and even more preferably 0.5 mol % or less, based on the total of all monomers constituting the anionic polymer.
[0045] (Physical Properties of Anionic Polymer) In the present polishing compound, the anionic polymer has an acid value of 20 mgKOH / g to 400 mgKOH / g. Using an anionic polymer with an acid value of 400 mgKOH / g or less improves the selectivity between the silicon oxide film and the stopper film. Using an anionic polymer with an acid value of 20 mgKOH / g or more facilitates adsorption of the anionic polymer to the abrasive grains, suppressing agglomeration of the abrasive grains, while improving the solubility of the anionic polymer, thereby suppressing aggregation of the anionic polymers themselves. From the viewpoint of suppressing agglomeration of the abrasive grains, the lower limit of the acid value of the anionic polymer is preferably 50 mgKOH / g, more preferably 100 mgKOH / g, and even more preferably 150 mgKOH / g. From the viewpoint of improving the selectivity, the upper limit of the acid value of the anionic polymer is preferably 350 mgKOH / g, more preferably 300 mgKOH / g, and even more preferably 280 mgKOH / g. The acid value represents the mass (mg) of potassium hydroxide required to neutralize the acidic components contained in 1 g of the solid content of the polymer, and is a value measured by the method described in JIS K 0070:1992.
[0046] In the anionic polymer, the ratio of the hydrophobic monomer to the anionic monomer may be appropriately adjusted so that the acid value falls within the above range. For example, the ratio of the hydrophobic monomer is preferably 10 mol% or more, more preferably 20 mol% or more, even more preferably 30 mol% or more, and particularly preferably 40 mol% or more, based on the total of all monomers constituting the anionic polymer. By adjusting the hydrophobic monomer to 10 mol% or more, polishing of the stopper film can be further suppressed. Furthermore, in the anionic polymer, the ratio of the hydrophobic monomer is preferably 95 mol% or less, more preferably 90 mol% or less, even more preferably 85 mol% or less, and particularly preferably 80 mol% or less, based on the total of all monomers. By adjusting the hydrophobic polymer to 95 mol% or less, the solubility of the anionic polymer is improved, and aggregation of abrasive grains and aggregation of the anionic polymer are suppressed.
[0047] The anionic polymer may be a random polymer in which the hydrophobic monomers and the anionic monomers are randomly arranged, or may be a block polymer having a block of anionic polymer and a block of anionic monomer.
[0048] The solubility of the anionic polymer in water is 5 mg / 100 g-H at 25° C. in view of storage stability. 2 Preferably 0 or more, 10 mg / 100 g-H 2 O or more is more preferable.
[0049] The weight average molecular weight Mw of the anionic polymer is preferably 1,000 to 100,000 from the viewpoint of dispersion stability of the anionic polymer. The lower limit of the weight average molecular weight Mw of the anionic polymer is preferably 2,000, more preferably 2,500, and even more preferably 3,000. The upper limit of the weight average molecular weight Mw of the anionic polymer is preferably 50,000, more preferably 40,000, even more preferably 30,000, even more preferably 25,000, particularly preferably 20,000, and extremely preferably 17,500. The weight average molecular weight (Mw) is determined by gel permeation chromatography (GPC) as a value converted into standard polystyrene.
[0050] The anionic polymer may be a commercially available product or may be synthesized. For example, in the case of a random polymer, a hydrophobic monomer and an anionic monomer are mixed, and an initiator is further added, followed by polymerization by a known polymerization method such as solution polymerization, bulk polymerization, or various radical polymerizations. Among these, solution polymerization is preferred because it is easy to adjust the weight-average molecular weight of the copolymer. In the case of a block polymer, for example, an anionic block may be synthesized first, and then a hydrophobic monomer may be polymerized onto the anionic block. In the production method, the order of polymerization of the anionic block and the hydrophobic block may be reversed. Alternatively, the anionic block and the hydrophobic block may be synthesized separately, and then the anionic block and the hydrophobic block may be coupled.
[0051] From the viewpoint of the effect of suppressing polishing of the stopper film, the content of the anionic polymer is preferably 0.02 mass % to 0.5 mass %, more preferably 0.05 mass % to 0.45 mass %, even more preferably 0.08 mass % to 0.4 mass %, and particularly preferably 0.1 mass % to 0.35 mass %, relative to the total mass of the abrasive.
[0052] <Acidic Compound> The polishing agent contains an acidic compound selected from a phosphoric acid compound and an organic acid compound. By including the acidic compound, the polishing rate for the stopper film can be suppressed while maintaining the polishing rate for the silicon oxide film. The molecular weight of the acidic compound is preferably 1,000 or less.
[0053] Specific examples of phosphoric acid compounds include phosphoric acid, phosphorous acid, phosphonic acid, phosphinic acid, and their ammonium salts, alkali metal salts, etc. Examples of organic acid compounds include compounds having a carboxy group, a sulfo group, a phospho group, and their ammonium salts, alkali metal salts, etc. Among these, organic acid compounds having a carboxy group are preferred.
[0054] Examples of organic acid compounds having a carboxy group include alkyl monocarboxylic acids such as formic acid, acetic acid, and propionic acid; carboxylic acids having a heterocycle such as 2-pyridinecarboxylic acid, 3-pyridinecarboxylic acid, 4-pyridinecarboxylic acid, 2,3-pyridinedicarboxylic acid, 2,4-pyridinedicarboxylic acid, 2,5-pyridinedicarboxylic acid, 2,6-pyridinedicarboxylic acid, 3,4-pyridinedicarboxylic acid, 3,5-pyridinedicarboxylic acid, pyrazinecarboxylic acid, 2,3-pyrazinedicarboxylic acid, 2-quinolinecarboxylic acid, pyroglutamic acid, picolinic acid, DL-pipecolic acid, 2-furancarboxylic acid, 3-furancarboxylic acid, tetrahydrofuran-2-carboxylic acid, and tetrahydrofuran-2,3,4,5-tetracarboxylic acid; carboxylic acids having an alicyclic ring such as cyclopentanecarboxylic acid, cyclohexanecarboxylic acid, cycloheptanecarboxylic acid, and cyclohexylcarboxylic acid; Carboxylic acids having an amino group, such as alanine, glycine, glycylglycine, aminobutyric acid, N-acetylglycine, N,N-di(2-hydroxyethyl)glycine, N-(tert-butoxycarbonyl)glycine, proline, trans-4-hydroxy-L-proline, phenylalanine, sarcosine, hydantoic acid, creatine, N-[tris(hydroxymethyl)methyl]glycine, glutamic acid, and aspartic acid; carboxylic acids having a hydroxyl group, such as lactic acid, malic acid, citric acid, tartaric acid, glycolic acid, gluconic acid, salicylic acid, 2-hydroxyisobutyric acid, glyceric acid, 2,2-bis(hydroxymethyl)propionic acid, and 2,2-bis(hydroxymethyl)butyric acid; carboxylic acids having a ketone group (keto acids), such as pyruvic acid, acetoacetic acid, and levulinic acid; Dicarboxylic acids such as oxalic acid, malonic acid, succinic acid, fumaric acid, maleic acid, glutaric acid, adipic acid, and phthalic acid are examples of the organic acid compound having a carboxy group. Of the above, dicarboxylic acids are particularly preferred.
[0055] The acidic compounds can be used singly or in combination of two or more. When using one acidic compound alone, the acidic compound may be referred to as the first acidic compound. When using two or more acidic compounds in combination, the compound with the highest molar concentration among the multiple acidic compounds may be referred to as the first acidic compound. The proportion of the first acidic compound is preferably 30 mol% or more, more preferably 50 mol% or more, and even more preferably 70 mol% or more, based on the total amount of the acidic compounds.
[0056] The acid dissociation constant pKa of the first acidic compound is preferably 4 to 9, more preferably 4.5 to 7, and even more preferably 5 to 6.5. By using an acidic compound having an acid dissociation constant of 4 to 9 as the first acidic compound, it becomes easier to prepare a polishing agent that satisfies the relationship of formula (1) described below, and it is easy to improve the selectivity. When the acidic compound has two or more acid dissociation constants, it is sufficient that at least one of the acid dissociation constants is 4 to 9. The acid dissociation constant may be measured by neutralization titration, or literature values may be referenced.
[0057] The polishing agent used herein is one in which the pKa of the first acidic compound and the pH of the polishing agent satisfy the relationship of formula (1): |pKa-pH|≦1.5 (1) However, when the first acidic compound has two or more acid dissociation constants, the pKa represents the acid dissociation constant that is closest to the pH.
[0058] By using a polishing agent in which the absolute value of the difference between pKa and pH is 1.5 or less, a high selectivity between a silicon oxide film and a stopper film can be obtained, and the polishing agent has excellent storage stability, suppressing changes in pH and viscosity even when stored for a long period of time. The inventors have inferred that the first acidic compound, which has the highest concentration among the acidic compounds, has a significant influence on the above-mentioned effect, and therefore it is appropriate to refer to the pKa value of the first acidic compound. To further improve the selectivity of the polishing agent, |pKa - pH| is preferably 1.2 or less, more preferably 1.0 or less, even more preferably 0.9 or less, even more preferably 0.8 or less, particularly preferably 0.7 or less, extremely preferably 0.6 or less, and most preferably 0.5 or less.
[0059] Methods for preparing an abrasive that satisfies formula (1) include, for example, a method of adjusting the pKa by selecting the first acidic compound, a method of adjusting the concentration of the first acidic compound, and a method of adjusting the pH by adding an acidic compound other than the first acidic compound or another pH adjuster.
[0060] The proportion of the acidic compound in the abrasive is preferably 0.001% by mass to 2.0% by mass, more preferably 0.005% by mass to 1.0% by mass, and even more preferably 0.01% by mass to 0.3% by mass, based on the total mass of the abrasive.
[0061] <Water> The polishing compound contains water as a medium for dispersing abrasive grains. The type of water is not particularly limited, but it is preferable to use pure water, ultrapure water, ion-exchanged water, etc., taking into consideration the effects on other components, prevention of impurity contamination, and effects on pH, etc.
[0062] <Nonionic Polymer> The present abrasive may also contain a nonionic polymer. From the viewpoint of lubricity, the nonionic polymer is preferably a nonionic polymer having an ether bond, and more preferably a nonionic polymer containing an ether bond in the main chain. Specific examples of nonionic polymers include polyethylene glycol, polyglycerin, and water-soluble nylon. When a nonionic polymer is used, its content can be 0.005% by mass to 2.0% by mass, preferably 0.01% by mass to 1.5% by mass, and more preferably 0.01% by mass to 0.3% by mass, based on the total mass of the present abrasive. If the content of the nonionic polymer is within the above range, the wettability of the abrasive with respect to the polished surface is improved, increasing the contact frequency of the abrasive grains, thereby improving the removal rate of the silicon oxide film.
[0063] <Additives> The polishing compound may further contain various additives. Examples of such additives include pH adjusters, dispersants, anti-aggregating agents, lubricants, viscosity imparting agents, viscosity modifiers, and preservatives, and two or more additives may be contained. Note that the above-mentioned phosphoric acid compounds and organic acid compounds may also be included in pH adjusters, but in this disclosure they are not considered to be included in pH adjusters.
[0064] (pH Adjuster) A pH adjuster may be contained to adjust the pH to a predetermined value. The pH adjuster may be appropriately selected from acidic compounds other than phosphoric acid compounds and organic acid compounds, basic compounds, amphoteric compounds such as amino acids, and salts thereof.
[0065] Examples of acidic compounds other than phosphoric acid compounds and organic acid compounds include inorganic acids and their salts. Examples of inorganic acids include nitric acid, sulfuric acid, and hydrochloric acid, and ammonium salts, sodium salts, and potassium salts thereof may also be used. When using an inorganic acid, it is preferable to use it in a range in which the molar concentration in the polishing agent is not higher than the molar concentration of the first acidic compound.
[0066] Examples of basic compounds include ammonia, sodium hydroxide, potassium hydroxide, ammonium hydroxide, potassium carbonate, sodium carbonate, ammonium carbonate; quaternary ammonium hydroxides such as tetramethylammonium hydroxide and tetraethylammonium hydroxide; and amino alcohols such as monoethanolamine, diethanolamine, and triethanolamine. Examples of amphoteric compounds include glycine, alanine, and phenylalanine.
[0067] The pH adjuster may be used alone or in combination of two or more. The pH of the polishing compound is preferably 4 to 9. The lower limit of the pH is more preferably 4.5, even more preferably 5, and particularly preferably 6. The upper limit of the pH is preferably 8.5, more preferably 8, even more preferably 7.5, and particularly preferably 7. By adjusting the pH within the above range, agglomeration of the abrasive grains can be suppressed and the selectivity can be improved. The content of the pH adjuster may be appropriately adjusted to achieve the above pH. As an example, the content of the pH adjuster may be 0.005% by mass to 2.0% by mass of the entire polishing compound, preferably 0.01% by mass to 1.5% by mass, and more preferably 0.01% by mass to 0.3% by mass.
[0068] (Dispersant) The abrasive may contain a dispersant to improve the dispersibility of the abrasive grains. Examples of dispersants include anionic surfactants, cationic surfactants, nonionic surfactants, and amphoteric surfactants, and one or more of these can be used. Anionic surfactants are preferably polymers having a carboxy group or an ammonium carboxylate salt, and polyacrylic acid or a polyacrylate is preferred. Examples of cationic surfactants include diallyldimethylammonium chloride polymers, diallyldimethylammonium chloride-sulfur dioxide copolymers, diallyldimethylammonium chloride-acrylamide copolymers, diallyldimethylammonium chloride-maleic acid copolymers, and maleic acid-diallyldimethylammonium ethyl sulfate-sulfur dioxide copolymers. The weight-average molecular weight of the surfactant is preferably 10,000 to 100,000, from the viewpoint of polishing the surface to be polished at a higher speed.
[0069] When a dispersant is used, the content thereof is preferably 0.0001% by mass to 0.3% by mass, more preferably 0.001% by mass to 0.2% by mass, and even more preferably 0.01% by mass to 0.15% by mass, relative to the total mass of the abrasive, from the viewpoint of polishing the surface to be polished at a higher speed.
[0070] When the above-mentioned additives are used in the present polishing agent, the total content of the additives is preferably 0.01 mass % to 10.0 mass %, and more preferably 0.01 mass % to 5.0 mass %, relative to the total mass of the polishing agent, in order to obtain a polishing agent having a high selectivity between the silicon oxide film and the stopper film.
[0071] The method for preparing this abrasive may be appropriately selected from methods that uniformly disperse or dissolve the abrasive grains, anionic polymer, and optional acidic compound in water as a medium. For example, the abrasive may be prepared by separately preparing a dispersion of abrasive grains and an additive liquid for the abrasive described below and mixing them. This method provides excellent storage stability and transportation convenience for the dispersion liquid and additive liquid for the abrasive. It is preferable to prepare this abrasive just before use by performing the above mixing in a polishing machine.
[0072] [Abrasive Additive Liquid] The abrasive additive liquid of this embodiment is an additive liquid to be mixed with a dispersion of abrasive grains to prepare an abrasive as described above, and is an abrasive additive liquid containing an anionic polymer, an acidic compound selected from a phosphoric acid compound and an organic acid compound, and water, wherein the anionic polymer is a copolymer containing a hydrophobic monomer and an anionic monomer, the anionic polymer has an acid value of 20 mg KOH / g to 400 mg KOH / g, the hydrophobic monomer has a partition coefficient (log D) of 0 to 4, and the anionic monomer contains at least one selected from unsaturated monocarboxylic acids and salts thereof, and when the acidic compound with the highest molar concentration is defined as a first acidic compound, the pKa of the first acidic compound and the pH of the abrasive additive liquid satisfy the relationship shown in formula (1) above. The abrasive additive liquid may optionally contain additives described as other components in the abrasive. Since each of these components is as described above, further description here will be omitted.
[0073] In addition, when the abrasive is prepared by mixing two liquids, an abrasive dispersion liquid and an abrasive additive liquid, the abrasive concentration in the dispersion liquid and the anionic polymer and acidic compound concentration in the abrasive additive liquid may be concentrated 2 to 100 times at the time of use of the abrasive, and then diluted to the desired concentration at the time of use. More specifically, for example, if the abrasive concentration in the dispersion liquid and the anionic polymer and acidic compound concentration in the additive liquid are both concentrated 10 times, 10 parts by mass of the dispersion liquid, 10 parts by mass of the abrasive additive liquid, and 80 parts by mass of water are mixed and stirred to prepare the abrasive.
[0074] By adding the above-mentioned additive liquid for abrasives to a dispersion of abrasive grains, it is possible to obtain a polishing agent that can maintain a high polishing rate for silicon oxide films while suppressing the polishing rate for stopper films to a low level, thereby achieving high selectivity and flatness.
[0075] In the above-mentioned additive liquid for abrasives, the content (concentration) of the anionic polymer is preferably 0.001 to 30 mass %, more preferably 0.01 to 20 mass %, and even more preferably 0.1 to 10 mass % of the total additive liquid. In the above-mentioned dispersion liquid of abrasive grains, the content (concentration) of the abrasive grains is preferably 0.2 to 40 mass %, more preferably 1 to 20 mass %, and even more preferably 5 to 10 mass %.
[0076] [Polishing Method] The polishing method of the present disclosure is a polishing method in which a surface to be polished is brought into contact with a polishing pad while an abrasive is supplied, and polishing is performed by the relative movement of the two, and the polishing method uses the abrasive of the present disclosure as the abrasive, and polishes a surface to be polished containing silicon oxide of a semiconductor substrate.
[0077] Examples of the surface to be polished include a surface of a semiconductor substrate made of silicon dioxide, a blanket wafer in which a stopper film and a silicon oxide film are laminated on the surface of a semiconductor substrate, and a patterned wafer in which these film types are arranged in a pattern. A preferred example of the semiconductor substrate is a substrate for STI. The abrasive of the present disclosure is also effective for polishing to planarize an interlayer insulating film between multilayer wiring in the manufacture of semiconductor devices.
[0078] Examples of silicon oxide films in STI substrates include so-called PE-TEOS films formed by plasma CVD using tetraethoxysilane (TEOS) as a raw material. Examples of silicon oxide films include so-called HDP films formed by high-density plasma CVD. Other examples include HARP films and FCVD films formed by other CVD methods, and SOD films formed by spin coating. Examples of silicon nitride films include those formed by low-pressure CVD or plasma CVD using silane or dichlorosilane and ammonia as raw materials, or those formed by ALD. Examples of polysilicon films include those formed by low-pressure CVD or plasma CVD using silane as a raw material, and then heat-treated to form polycrystalline granules.
[0079] A known polishing apparatus can be used for this polishing method. Fig. 2 is a schematic diagram showing an example of a polishing apparatus. The polishing apparatus 20 shown in Fig. 2 includes a polishing head 22 that holds a semiconductor substrate 21 such as an STI substrate, a polishing platen 23, a polishing pad 24 attached to the surface of the polishing platen 23, and an abrasive supply pipe 26 that supplies an abrasive 25 to the polishing pad 24. While the abrasive 25 is supplied from the abrasive supply pipe 26, the polished surface of the semiconductor substrate 21 held by the polishing head 22 is brought into contact with the polishing pad 24, and the polishing head 22 and the polishing platen 23 are rotated relative to each other to perform polishing.
[0080] The polishing head 22 may move linearly as well as rotaryly. Furthermore, the polishing platen 23 and polishing pad 24 may be approximately the same size as or smaller than the semiconductor substrate 21. In this case, it is preferable to move the polishing head 22 and polishing platen 23 relative to each other so that the entire surface to be polished of the semiconductor substrate 21 can be polished. Furthermore, the polishing platen 23 and polishing pad 24 do not have to be of the type that moves rotary, and may be, for example, of the type that moves in one direction as a belt.
[0081] Although there are no particular limitations on the polishing conditions for such a polishing apparatus 20, applying a load to the polishing head 22 to press it against the polishing pad 24 can increase the polishing pressure and improve the polishing rate. The polishing pressure is preferably about 0.5 to 50 kPa, and more preferably about 3 to 40 kPa from the viewpoints of uniformity of the polishing rate across the polished surface of the semiconductor substrate 21, flatness, and prevention of polishing defects such as scratches. The rotation speed of the polishing platen 23 and the polishing head 22 is preferably about 50 to 500 rpm. The supply amount of the abrasive 25 is appropriately adjusted depending on the composition of the abrasive, the above-mentioned polishing conditions, etc.
[0082] The polishing pad 24 can be made of a material such as nonwoven fabric, polyurethane foam, porous resin, or non-porous resin. To facilitate the supply of abrasive 25 to the polishing pad 24 or to allow a constant amount of abrasive 25 to accumulate on the polishing pad 24, the surface of the polishing pad 24 may be grooved in a grid, concentric circle, spiral, or other pattern. If necessary, a pad conditioner may be brought into contact with the surface of the polishing pad 24 to condition the surface of the polishing pad 24 while polishing.
[0083] According to this polishing method, a high selectivity between the silicon oxide film and the stopper film can be obtained while suppressing polishing scratches, and highly flat polishing can be achieved.
[0084] [Method for Manufacturing Semiconductor Components] In the method for manufacturing semiconductor components according to this embodiment, semiconductor components are obtained by dividing a semiconductor substrate having a surface to be polished that has been polished by the polishing method of the present disclosure into individual pieces.
[0085] The method for manufacturing a semiconductor component of the present disclosure includes a singulation step of singulating a semiconductor substrate having a polished surface polished by the polishing method. The singulation step may include, for example, dicing the semiconductor substrate (e.g., a semiconductor wafer) using a known method such as blade dicing, laser dicing, or plasma dicing to obtain semiconductor chips as semiconductor components. The method for manufacturing a semiconductor component of the present disclosure may further include a bonding step of bonding another member to the polished surface of the semiconductor chip. This step results in a semiconductor component as a bonded assembly. Examples of the other member include a second semiconductor chip, a rewiring layer, etc. The second semiconductor chip may be a semiconductor chip obtained by the manufacturing method of the present disclosure, or may be a semiconductor chip obtained by another method. The bonding step may include, for example, placing another member directly on the polished surface and bonding it directly by fusion bonding, surface activated bonding, or the like, or bonding the polished surface to the other member via an adhesive layer. Examples of the adhesive layer include a metal layer such as solder or copper, a glass layer, or a resin layer such as polyimide or epoxy. The present disclosure can further provide an electronic device including at least one semiconductor component having a surface polished by the polishing method of the present disclosure.
[0086] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these examples. Examples 1 to 8 are examples, and Examples 9 to 14 are comparative examples.
[0087] [Measurement Method] <pH> The pH was measured using a pH meter HM-30R manufactured by DKK-TOA Corporation, with the temperature set to 25±5°C.
[0088] <Average Secondary Particle Diameter> The average secondary particle diameter was measured using a laser scattering / diffraction particle size distribution measuring device (manufactured by Horiba, Ltd., device name: LA-950).
[0089] <Acid value> The acid value was measured according to the method described in JIS K 0070:1992.
[0090] <Weight-average molecular weight (Mw)> Measured by gel permeation chromatography (GPC) under the following conditions: Apparatus: HLC-8320GPC (manufactured by Tosoh Corporation) Column: TSKgel GMPWXL (manufactured by Tosoh Corporation) Detector: RI detector, polarity (+) Eluent: 0.2 M NaNO 3 Aqueous solution Flow rate: 1.0 mL / min Column temperature: 40°C Calculated using standard PEO / PEG
[0091] [Abrasive] <Abrasive Grains> Ceria particles with a particle size of 50 to 150 nm were used as the abrasive grains. The ceria content in the ceria particles was 95% by mass or more. <Anionic Polymers> Anionic polymers having the following composition were prepared. - Anionic polymer (A): A polymer consisting of 70 mol% n-butyl methacrylate (logD is 2.6) and 30 mol% methacrylic acid, with an acid value of 150 mg KOH / g and a weight average molecular weight of 20,000. - Anionic polymer (B): A polymer consisting of 50 mol% n-butyl methacrylate and 50 mol% methacrylic acid, with an acid value of 250 mg KOH / g and a weight average molecular weight of 20,000. Anionic polymer (C): A polymer consisting of 50 mol% n-butyl methacrylate and 50 mol% methacrylic acid, having an acid value of 250 mg KOH / g and a weight-average molecular weight of 15,000. Anionic polymer (D): A homopolymer of methacrylic acid, having an acid value of 650 mg KOH / g and a weight-average molecular weight of 10,000. Anionic polymer (E): A polymer consisting of 10 mol% n-butyl methacrylate and 90 mol% methacrylic acid, having an acid value of 510 mg KOH / g and a weight-average molecular weight of 20,000. Anionic polymer (F): A polymer consisting of 30 mol% decyl methacrylate (log D is 5.9) and 70 mol% methacrylic acid, having an acid value of 300 mg KOH / g and a weight-average molecular weight of 40,000.
[0092] <Preparation of Abrasives> As shown in Table 1, abrasives of Examples 1 to 14 were prepared by mixing abrasive grains, anionic polymers, acidic compounds, other components, and water. The zeta potential of the abrasive grains in each abrasive was -80 mV to -50 mV. The acidic compound was adjusted to a range of 0.01% by mass to 0.3% by mass, taking the pH into consideration. In Table 1, "-" indicates that the acidic compound was not used.
[0093] [Polishing Evaluation] <Polishing Conditions> The performance of the abrasives according to Examples 1 to 14 was evaluated using a fully automatic CMP device FREX300X (manufactured by Ebara Corporation). In the evaluation, a polyurethane pad (manufactured by DuPont IC-1000) was used as the polishing pad, and a diamond pad conditioner (manufactured by 3M, product name: A165) was used for conditioning the polishing pad. The polishing conditions were a polishing pressure of 21 kPa, a polishing platen rotation speed of 100 rpm, and a polishing head rotation speed of 102 rpm. The supply rate of the abrasive was 250 milliliters / minute unless otherwise specified.
[0094] The following were used as the objects to be polished (workpieces to be polished): - A blanket wafer with a silicon dioxide film, in which a silicon dioxide film was formed on a 12-inch silicon substrate by plasma CVD using tetraethoxysilane (TEOS) as a raw material - A blanket wafer with a silicon nitride film, in which a silicon nitride film was formed on a 12-inch silicon substrate by low-pressure CVD using silane and ammonia as raw materials
[0095] <Evaluation Method> A SCREEN VM-3210 film thickness meter was used to measure the film thickness of the formed silicon dioxide film and silicon nitride film. The removal rate of each silicon dioxide film and silicon nitride film was calculated by determining the difference between the film thickness of each blanket wafer before polishing and the film thickness after 1 minute of polishing. The average value (Å / min) of the removal rates obtained from the removal rates at 49 points on the substrate surface was used as the removal rate, and the ratio of the removal rate of the silicon dioxide film to the removal rate of the silicon nitride film (removal rate of silicon dioxide film / removal rate of silicon nitride film) was calculated as the selectivity. The results are shown in Table 1. In the table, silicon oxide films are abbreviated as "TEOS" and silicon nitride films are abbreviated as "SiN."
[0096] [Stability Evaluation] The pH of each of the polishing agents of Examples 1 to 14 was measured after storage for 2 weeks at 50° C. The difference in pH between the polishing agent immediately after preparation and the pH after storage is shown in Table 1.
[0097]
[0098] The polishing agents of Examples 1 to 8, which contain abrasive grains, a specific anionic polymer, and a specific acidic compound and satisfy |pKa-pH|≦1.5, were shown to have a high removal rate for silicon oxide films and a suppressed removal rate for silicon nitride films, resulting in a high selectivity. Furthermore, the polishing agents of Examples 1 to 7 were shown to have excellent pH and viscosity stability and to be able to maintain stable performance. The polishing agents of Examples 7 and 8, which further contained a nonionic polymer, exhibited a higher removal rate for silicon oxide films than the polishing agent of Example 4. It is presumed that the combination of a nonionic polymer improved the wettability of the polishing agent with the polished surface, increasing the contact frequency of the abrasive grains and thereby improving the removal rate for silicon oxide films. On the other hand, the polishing agents of Examples 9 and 10, which used an anionic polymer with a high acid value, were shown to not sufficiently suppress the removal rate for silicon nitride films and to result in a reduced selectivity. The polishing agent of Example 11, which did not contain an acidic compound, exhibited a reduced removal rate for silicon oxide films and an insufficient selectivity. Furthermore, it was shown that the polishing agents of Examples 12 to 14, which had a |pKa-pH| of more than 1.5, had problems with storage stability and it was difficult to maintain the performance of the polishing agent. From the above, it was revealed that the polishing agent of this embodiment can suppress the polishing rate of the stopper film while maintaining the polishing rate of the silicon oxide film, thereby obtaining a high selectivity and capable of maintaining this performance for a long period of time.
[0099] According to the present disclosure, high-speed polishing can be achieved, for example, in CMP of a polishing target surface including an insulating film. Therefore, the polishing method of the present disclosure is suitable for polishing insulating films for STI in semiconductor device manufacturing.
[0100] This application claims priority based on Japanese Patent Application No. 2023-74452, filed on April 28, 2023, the disclosure of which is incorporated herein in its entirety.
[0101] 1...silicon substrate, 2...stopper film, 3...trench, 4...silicon oxide film, 20...polishing device, 21...semiconductor substrate, 22...polishing head, 23...polishing surface plate, 24...polishing pad, 25...abrasive, 26...abrasive supply pipe
Claims
1. A polishing agent comprising an abrasive grain, an anionic polymer, an acidic compound selected from a phosphoric acid compound and an organic acid compound, and water, wherein the anionic polymer is a copolymer containing a hydrophobic monomer and an anionic monomer, the anionic polymer has an acid value of 20 mg KOH / g to 400 mg KOH / g, the hydrophobic monomer has a partition coefficient (log D) of 0 to 4, and the anionic monomer comprises at least one selected from unsaturated monocarboxylic acids and salts thereof, and when the acidic compound having the highest molar concentration is defined as a first acidic compound, the pKa of the first acidic compound and the pH of the polishing agent satisfy the relationship of formula (1): |pKa-pH|≦1.5 (1) However, when the first acidic compound has two or more acid dissociation constants, the pKa represents the acid dissociation constant closest to the pH.
2. The abrasive according to claim 1, wherein the abrasive grains comprise at least one selected from the group consisting of silica grains, alumina grains, zirconia grains, cerium compound grains, titania grains, germania grains, composite grains thereof, and core-shell grains.
3. The abrasive according to claim 2, wherein the abrasive grains include cerium compound particles.
4. The abrasive of claim 2, wherein the abrasive grains include ceria particles.
5. The abrasive according to claim 1, wherein the content of the abrasive grains is 0.01% by mass to 10.0% by mass based on the total mass of the abrasive.
6. The polishing agent according to claim 1, wherein the anionic polymer has an acid value of 20 mg KOH / g to 300 mg KOH / g.
7. The polishing agent according to claim 1, wherein the partition coefficient (log D) of the hydrophobic monomer is 0 to 3.
8. The polishing agent of claim 1, wherein the hydrophobic monomer comprises an alkyl (meth)acrylate.
9. The polishing agent according to claim 1, wherein the weight average molecular weight of the anionic polymer is 1,000 to 100,000.
10. The polishing agent according to claim 1, wherein the ratio of the hydrophobic monomer in the anionic polymer is 10 to 95 mol % based on the total monomers constituting the anionic polymer.
11. The abrasive according to claim 1, wherein the content of the anionic polymer is 0.02% by mass to 0.5% by mass based on the total mass of the abrasive.
12. The polishing agent according to claim 1, wherein the pKa is 4 to 9.
13. The abrasive of claim 1, further comprising a nonionic polymer.
14. The polishing agent according to claim 1, having a pH of 4 to 9.
15. A polishing method in which a surface to be polished of a semiconductor substrate is brought into contact with a polishing pad while an abrasive is being supplied, and polishing is performed by the relative movement of the two, wherein the abrasive is an abrasive as defined in any one of claims 1 to 14.
16. A method for producing semiconductor components, comprising the steps of: obtaining semiconductor components by dicing a semiconductor substrate having a surface to be polished by the polishing method according to claim 15 into individual pieces.
17. An additive liquid for an abrasive comprising an anionic polymer, an acidic compound selected from a phosphoric acid compound and an organic acid compound, and water, wherein the anionic polymer is a copolymer containing a hydrophobic monomer and an anionic monomer, the acid value of the anionic polymer is 20 mg KOH / g to 400 mg KOH / g, the partition coefficient (log D) of the hydrophobic monomer is 0 to 4, and the anionic monomer comprises at least one selected from unsaturated monocarboxylic acids and salts thereof, and when the acidic compound having the highest molar concentration among the acidic compounds is defined as a first acidic compound, the pKa of the first acidic compound and the pH of the additive liquid for an abrasive satisfy the relationship of formula (1): |pKa-pH|≦1.5 (1) However, when the first acidic compound has two or more acid dissociation constants, the pKa represents the acid dissociation constant closest to the pH.
Citation Information
Patent Citations
Polishing agent and polishing method, and additive solution for polishing
JP2019087660A
Abrasive and polishing method
JP2022010758A