Method for producing (METH)acryloyl group-containing organopolysiloxane

The method of reacting organopolysiloxanes with halogen-containing organic groups and (meth)acrylates using phase transfer catalysts addresses the challenges of viscosity and efficiency in producing (meth)acryloyl group-containing organopolysiloxanes, resulting in improved synthesis and application suitability.

WO2024225074A1PCT designated stage expired Publication Date: 2024-10-31SHIN ETSU CHEMICAL CO LTD

Patent Information

Application Number
PCT/JP2024/014796
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional methods for producing (meth)acryloyl group-containing organopolysiloxanes face issues with handling due to increased viscosity and poor reaction efficiency, particularly in introducing (meth)acryloyl groups into siloxane compounds using epoxy-modified organopolysiloxanes or hydroxyethyl acrylate reactions.

Method used

Reacting an organopolysiloxane with a halogen-containing organic group and (meth)acrylate in the presence of a phase transfer catalyst, such as quaternary ammonium salts or crown ethers, to efficiently introduce (meth)acryloyl groups, allowing for better control of reaction conditions and raw material availability.

Benefits of technology

This method enables the efficient synthesis of (meth)acryloyl-modified organopolysiloxanes with improved handling and reaction efficiency, suitable for radiation-curable coatings and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014796_31102024_PF_FP_ABST
    Figure JP2024014796_31102024_PF_FP_ABST
Patent Text Reader

Abstract

[Problem] A purpose of the present invention is to provide a method for producing a new (meth)acryloyl group-containing organopolysiloxane that has easy control of reaction conditions, good availability of raw materials, and favorable reaction efficiency. [Solution] A method for producing a (meth)acryloyl group-containing organopolysiloxane, the method including a step for obtaining a (meth)acryloyl group-containing organopolysiloxane by reacting (A) an organopolysiloxane selected from the group consisting of a halogen-containing organopolysiloxane (a-1) represented by the average compositional formula (1) below and a halogen-containing organopolysiloxane (a-2) represented by the average compositional formula (2) below (in formula (1), R1 are each independently a halogen-containing alkyl group having 1-11 carbon atoms, R2 are each independently a group selected from a substituted or unsubstituted monovalent hydrocarbon group having 1-11 carbon atoms, an alkoxy group having 1-11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers satisfying a≥1, b≥0, and 20≥a+b≥3) (in formula (2), R3 and R3' are each independently a group selected from the choices of R1 and R2, at least one among R3 and R3' is a group represented by R1, and c, d, e, and f are numbers satisfying c≥2, d≥0, e≥0, f≥0, 2≤c+d+e+f≤1,000), and (B) (meth)acrylic acid metal salt in the presence of (C) a phase transfer catalyst selected from a quaternary ammonium salt having at least one monovalent hydrocarbon group having 4-20 carbon atoms, a crown ether, and a phosphonium compound.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing (meth)acryloyl group-containing organopolysiloxane

[0001] The present invention relates to a method for producing a (meth)acryloyl group-containing organopolysiloxane.

[0002] The technique of applying energy to a liquid resin composition to cure it is a widespread technology and is used in many fields, such as for producing coatings and molded products. The energy required for this curing is heat or radiation such as ultraviolet light. In the case of heat curing, a heat-activated catalyst is blended into the base resin, and a cured product is obtained by applying heat. In the case of radiation curing, a composition blended with a photoinitiator that is activated by ultraviolet light or other radiation is cured by irradiating it with radiation.

[0003] Typical functional groups used for radiation curing include (meth)acryloyl groups, mercapto groups, and epoxy groups. (Meth)acryloyl groups form crosslinks through radical polymerization reactions, while mercapto groups undergo radical ene-thiol reactions in the presence of alkenyl groups. Epoxy groups undergo cationic polymerization in the presence of acids.

[0004] Various resins are used for this type of radiation curing, one of which is silicone. Silicone is a general term for organopolysiloxanes with a main chain of continuous siloxane bonds and organic groups such as methyl groups on the side chains. Silicones have excellent heat resistance, cold resistance, chemical resistance, electrical insulation, and mold releasability, and can be made into various forms such as oil, rubber, and resin. Radiation-curable silicones are used as raw materials for cured products such as silicone rubber, silicones for release paper, and silicones for hard coatings.

[0005] Organopolysiloxanes containing (meth)acryloyl groups as radiation-polymerizable groups are used in release coatings, hard coats, and surface tension adjusters. A cured product can be obtained by blending a photopolymerization initiator with this base material and irradiating it with radiation while purging with nitrogen in a chamber to efficiently react the radicals generated by radiation.

[0006]

[0003] Several studies have been conducted on methods for producing such organopolysiloxanes containing (meth)acryloyl groups. In Patent Document 1, an organopolysiloxane containing (meth)acryloyl groups is produced by using an epoxy-modified organopolysiloxane as a raw material and reacting (meth)acrylic acid with an epoxy group. However, in this case, hydroxyl groups are generated as the epoxy ring opens, which increases the viscosity of the product, leaving a problem in terms of handling.

[0007] Patent Document 2 proposes a method of introducing acryloyl groups into siloxanes by reacting hydroxyethyl acrylate with methoxy-containing siloxanes and heating the mixture, accompanied by the distillation of methanol. However, the product obtained by this method contains hydrolyzable silicon-oxygen-carbon bonds, leaving problems in terms of storage stability.

[0008] Patent Document 3 discloses a method for introducing a (meth)acryloyl group into a siloxane compound by reacting a siloxane compound having a Cl-containing organic group with an alkali metal salt of (meth)acrylic acid in the presence of tetramethylammonium chloride. Although this is an effective production method, the low activity of tetramethylammonium chloride poses a problem of poor reaction efficiency depending on the type of siloxane compound having a Cl-containing organic group.

[0009] JP 2018-521188 A JP 2016-209874 A JP 2021-17424 A

[0010] As mentioned above, conventional methods for producing (meth)acryloyl group-containing organopolysiloxanes have had problems with handling and reaction efficiency. Therefore, an object of the present invention is to provide a novel method for producing (meth)acryloyl group-containing organopolysiloxanes that allows for easy control of reaction conditions, good availability of raw materials, and good reaction efficiency.

[0011] As a result of extensive research conducted by the present inventors in order to achieve the above object, they have discovered that a (meth)acryloyl-modified organopolysiloxane can be efficiently synthesized by reacting an organopolysiloxane having a halogen-containing organic group with a (meth)acrylate salt in the presence of a phase transfer catalyst.

[0012] That is, the present invention provides (A) an organopolysiloxane selected from the group consisting of a halogen-containing organopolysiloxane (a-1) represented by the following average composition formula (1) and a halogen-containing organopolysiloxane (a-2) represented by the following average composition formula (2): (In the formula, R 1 are each independently a halogen-containing alkyl group having 1 to 11 carbon atoms, and R 2 are each independently a group selected from a substituted or unsubstituted monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers that satisfy a ≧ 1, b ≧ 0, and 20 ≧ a + b ≧ 3. (In the formula, R 3 and R 3 ' are each independently the above R 1 and R 2 and R 3 and R 3 At least one of the R 1 wherein c, d, e, and f are numbers that satisfy the conditions c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000), and (B) a metal (meth)acrylate in the presence of (C) a phase transfer catalyst selected from the group consisting of a quaternary ammonium salt having at least one monovalent hydrocarbon group having 4 to 20 carbon atoms, a crown ether, and a phosphonium compound, to obtain the (meth)acryloyl group-containing organopolysiloxane.

[0013] The present invention further provides the above-mentioned production method, which further satisfies at least one of the following constituent requirements [1] to [9]: [1] The R of the halogen-containing organopolysiloxane (a-2) represented by the average composition formula (2) is 1is bonded to is 1 to 100% of the total number of silicon atoms. [2] A method for producing the (meth)acryloyl group-containing organopolysiloxane, characterized in that component (B) is blended in an amount of 1 to 3 moles per mole of halogen atoms in component (A), and further component (C) is blended in an amount of 0.05 to 10 parts by mass per 100 parts by mass of component (A). [3] A method for producing the (meth)acryloyl group-containing organopolysiloxane, wherein the (B) metal (meth)acrylate is an alkali metal salt. [4] A method for producing the (meth)acryloyl group-containing organopolysiloxane, wherein the (C) phase transfer catalyst is a compound represented by the following formula (3): R 4 4 N + X - (3) (wherein, R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms, provided that R 4 At least one of X is a linear or branched monovalent hydrocarbon group having 4 to 20 carbon atoms, and - [5] A method for producing the (meth)acryloyl group-containing organopolysiloxane, wherein the phase transfer catalyst (C) is a quaternary ammonium salt represented by the above formula (3), and the halide ion is Br - or Cl - [6] The method for producing the (meth)acryloyl group-containing organopolysiloxane, wherein R 1 are each independently an alkyl group having 1 to 7 carbon atoms and a halogen atom at the end. 3 At least one of the R 1 [8] In the average composition formula (2), 1≦d≦998, and R 3 At least one of the R 1 and the R 1are each independently a C1 to C5 alkyl group having a halogen atom at its terminal. [9] The method for producing the (meth)acryloyl group-containing organopolysiloxane, further comprising blending (D) a polymerization inhibitor in an amount of 0.01 to 1 part by mass per 100 parts by mass of the total of the components (A) and (B).

[0014] According to the production method of the present invention, the desired (meth)acryloyl group-containing organopolysiloxane can be obtained efficiently by a desalting reaction using inexpensive raw materials.

[0015] The present invention will be described in detail below.

[0016] [Component (A)] Component (A) is at least one organopolysiloxane selected from the group consisting of halogen-containing organopolysiloxane (a-1) represented by the following average composition formula (1) and halogen-containing organopolysiloxane (a-2) represented by the following average composition formula (2): (In the formula, R 1 are each independently a halogen-containing alkyl group having 1 to 11 carbon atoms, and R 2 are each independently a group selected from a substituted or unsubstituted monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers that satisfy a ≧ 1, b ≧ 0, and 20 ≧ a + b ≧ 3. (In the formula, R 3 and R 3 ' are each independently the above R 1 and R 2 and R 3 and R 3 At least one of the R 1 wherein c, d, e, and f are numbers satisfying c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000).

[0017] R 1are each independently an alkyl group having 1 to 11 carbon atoms, preferably an alkyl group having 1 to 7 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms, which has a halogen at its terminal.

[0018] R 2 are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, or a hydroxyl group-containing organic group. Examples of the monovalent hydrocarbon group having 1 to 11 carbon atoms include alkyl groups such as methyl, ethyl, propyl, and butyl, cycloalkyl groups such as cyclohexyl, and aryl groups such as phenyl and tolyl. Examples of the alkoxy group having 1 to 11 carbon atoms include methoxy, ethoxy, isopropoxy, and butoxy. Examples of the hydroxyl group-containing organic group include hydroxymethyl, hydroxyethyl, hydroxypropyl, and hydroxybutyl. R 2 is preferably a methyl group, an ethyl group, a methoxy group, an ethoxy group, or a hydroxyl group-containing organic group.

[0019] In the above average composition formula (2), R 3 and R 3 ' are, independently of each other, R 1 and R 2 and R 3 and R 3 At least one of the R 1 Preferably, R 3 At least one of the R 1 Therefore, preferably, in the average composition formula (2), 1≦d≦998, and R 3 At least one of R ' is an alkyl group having 1 to 7 carbon atoms and a halogen atom at the terminal, more preferably an alkyl group having 1 to 5 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms. 3 is R 2 That is, a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, or a hydroxyl group-containing organic group, and more preferably, R 3is an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group, or a hydroxyl group-containing organic group.

[0020] In the above average composition formula (2), the ratio of the number of halogen-containing alkyl groups having 1 to 11 carbon atoms (i.e., R 1 The ratio of the number of silicon atoms to which halogen-containing alkyl groups having 1 to 11 carbon atoms are bonded is preferably 1 to 100%, more preferably 3 to 75%, more preferably 5 to 50%, and even more preferably 5 to 30%. In particular, if the number of silicon atoms to which halogen-containing alkyl groups having 1 to 11 carbon atoms are bonded is less than 1%, the curability when cured by radiation may be insufficient.

[0021] R 1 Examples of R include halogen alkyl groups such as chloromethyl, chloroethyl, chloropropyl, chlorobutyl, chloropentyl, chlorohexyl, chlorooctyl, bromomethyl, bromoethyl, bromopropyl, bromobutyl, bromopentyl, bromohexyl, bromooctyl, iodomethyl, iodoethyl, iodopropyl, iodobutyl, iodopentyl, iodohexyl, and iodooctyl. From the viewpoint of ease of reaction, the substitution position of the halogen atom is preferably primary or secondary, and more preferably primary. Furthermore, from the viewpoint of ease of availability of raw materials for the functional group, the halogen-containing organic group preferably has 1 to 5 carbon atoms. Furthermore, the halogen-containing organic group is preferably a chloroalkyl group or a bromoalkyl group, and a chloroalkyl group is particularly preferred. Among these, a chloromethyl group, a chloroethyl group, and a chloropropyl group are preferred. The halogen-containing alkyl group having 1 to 11 carbon atoms, preferably 1 to 5 carbon atoms, may be linear or branched. R 1 is represented, for example, by the following structure: In the following formula, the positions indicated by dotted lines are bonds to the silicon atoms of the organopolysiloxane.

[0022] In the average composition formula (1), a and b are numbers that satisfy a≧1, b≧0, and 20≧a+b≧3; preferably, a is a number from 1 to 15, b is a number from 0 to 15, and a+b is a number from 3 to 15, and more preferably, a is a number from 1 to 10, b is a number from 0 to 10, and a+b is a number from 3 to 10. Preferably, the organopolysiloxane has a viscosity at 25°C of 1 to 2,000 mPa s, and more preferably a viscosity of 2 to 1,000 mPa s. The viscosity is a value measured using a BM-type rotational viscometer at 25°C.

[0023] Examples of organopolysiloxanes represented by average composition formula (1) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein g is 1 to 20, h is 0 to 19, i is 0 to 19, and 20≧g+h+i≧3)

[0024] In the average composition formula (2), c, d, e, and f are numbers that satisfy the following conditions: c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000. Preferably, c is a number from 2 to 32, d is a number from 0 to 998, d is preferably a number from 1 to 998, e is a number from 0 to 10, f is a number from 0 to 10, and c+d+e+f is 2 to 1,000. More preferably, c is a number from 2 to 20, d is a number from 1 to 798, e is a number from 0 to 6, f is a number from 0 to 6, and c+d+e+f is 3 to 800. More preferably, c is 2, and d is a number from 1 to 600. Even more preferably, c is 2, and d is a number from 1 to 400. As described above, [R 3 'R 3 'SiO 2/2 ] d R bonded to the silicon atom of 3 At least one of the R 1 Preferably, the alkyl group (R 1 The ratio of silicon atoms to which the hydroxyl group (C) is bonded falls within the above range, and the organopolysiloxane has a viscosity at 25°C of 5 to 10,000 mPa s, and more preferably 10 to 5,000 mPa s. The viscosity is measured using a BM-type rotational viscometer.

[0025] Examples of organopolysiloxanes represented by average composition formula (2) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein j is 0 to 997, k is 1 to 998, and l is 0 to 100, and 1≦j+k≦998 or 0≦j+i≦998 is satisfied.)

[0026] [Component (B)] Component (B) is a metal (meth)acrylate salt, which is a reaction agent for introducing a (meth)acryloyl group into component (A). Component (B) is preferably a metal (meth)acrylate salt represented by the following general formula (4). Component (B) is more preferably an alkali metal salt.

[0027] In formula (4), R 5 is a hydrogen atom or a methyl group, and M m+ is a metal ion. Examples of the metal ion include potassium ion, sodium ion, calcium ion, and zinc ion. Among them, from the viewpoint of the ease with which the desalination reaction proceeds, M m+ is preferably an alkali metal ion, more preferably a potassium ion, and m is an integer of 1 to 2, preferably 1.

[0028] The amount of component (B) to be reacted is preferably 1 to 3 moles, preferably 1 to 2 moles, and more preferably 1.01 to 1.5 moles per mole of halogen atoms in the organopolysiloxane (A). If the amount of component (B) is less than the above lower limit, the rate of introduction of (meth)acryloyl groups by the desalting reaction decreases. If the amount is more than the above upper limit, the rate of introduction of (meth)acryloyl groups by the desalting reaction increases, but the amount of component (B) is too high, which may result in a decrease in pot yield or an increase in the viscosity of the reaction mixture, making it difficult to handle.

[0029] [Component (C)] Component (C) is a phase transfer catalyst selected from quaternary ammonium salts having at least one monovalent hydrocarbon group having 4 to 20 carbon atoms, crown ethers, and phosphonium compounds, and is preferably a quaternary ammonium salt represented by the following general formula (3): R 44 N + X - (3) (wherein, R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms. 4 At least one of X is a linear or branched monovalent hydrocarbon group having 4 to 20 carbon atoms. - is a halide ion.)

[0030] R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 18 carbon atoms, and more preferably 1 to 16 carbon atoms. 4 At least one of R is a linear or branched hydrocarbon group having 4 to 20 carbon atoms, preferably 4 to 18 carbon atoms, and more preferably 4 to 16 carbon atoms. 4 Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, n-butyl, isopropyl, t-butyl, pentyl, hexyl, and octyl groups, cycloalkyl groups such as cyclohexyl, and phenyl groups. Among these, from the viewpoint of the efficiency of the desalting reaction, R 4 is preferably a straight-chain alkyl group, and more preferably an n-butyl group, an n-pentyl group, or an n-hexyl group.

[0031] R 4 However, the reason why the reaction efficiency improves when the alkyl group is a butyl group, pentyl group, hexyl group, or other alkyl group is thought to be that the presence of an alkyl group with a long chain length improves the compatibility with silicone of the ammonium (meth)acrylate salt that is generated by the ion exchange reaction between the quaternary ammonium salt, which is the phase transfer catalyst, and the metal (meth)acrylate salt, making it easier to promote the reaction.

[0032] X - is a halide ion, and from the viewpoint of availability, Br - or Cl - is preferred.

[0033] Examples of the phase transfer catalyst represented by formula (3) include compounds represented by the following structures:

[0034] The amount of component (C) blended is 0.05 to 10 parts by mass, preferably 0.1 to 7.5 parts by mass, and more preferably 0.3 to 5 parts by mass, per 100 parts by mass of component (A). If the amount is less than the lower limit, the reaction may not proceed sufficiently. If the amount exceeds the upper limit, the curability when cured by radiation may decrease. Furthermore, only one type of phase transfer catalyst may be used, or two or more types may be selected from the above.

[0035] [Component (D)] Component (D) is a polymerization inhibitor, an additive that inhibits self-polymerization of (B) metal (meth)acrylate without reacting with component (A) during the reaction. The polymerization inhibitor is not limited as long as it has the effect of inhibiting radical polymerization, and examples thereof include alkylphenols such as those listed below.

[0036] p-Methoxyphenol, 2,6-di-t-butylhydroxytoluene, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, 4,4'-dioxydiphenol, 1,1'-bis(4-hydroxyphenyl)-cyclohexane, 3-methyl-4-isopropylphenol, 2,4,5-tri-hydroxybutyrophenone, 2,6-di-t-butylphenol, 2,5-di-t-amylhydroquinone, 2,5-di-t-butylhydroquinone, 4-hydroxymethyl-2,6-di-t-butylphenol, 2,6-di-t-butyl-α-dimethylamino-p-cresol, 4,4-bis(2,6-di-butylphenol), 2, 2'-methylene-bis(4-ethyl-6-t-butylphenol), 2,2'-methylene(2,6-di-t-butylphenol), 4,4'-methylene(2,6-di-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thio-bis(6-t-butyl-3-methylphenol), bis(3-methyl-4-hydroxy-5-t-butylbenzyl)sulfide, 4,4'-thio-bis(6-t-butyl-o-cresol), and 2,2'-thio-bis(4-methyl-6-t-butylphenol).

[0037] Amine-based polymerization inhibitors can also be used, such as those listed below.

[0038] Alkylated diphenylamines, N,N'-diphenyl-p-phenylenediamine, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 1,4-dihydroxy-2,2,6,6-tetramethylpiperidine, 1-hydroxy-4-benzoyloxy-2,2,6,6-tetramethylpiperidine.

[0039] The amount of polymerization inhibitor is 0.01 to 1 part by mass, preferably 0.02 to 0.5 parts by mass, and more preferably 0.03 to 0.3 parts by mass, per 100 parts by mass of the combined total of components (A) and (B). If the amount of component (D) is greater than the above upper limit, the curability of the resulting radiation-curable organopolysiloxane composition containing the radically polymerizable organopolysiloxane may be reduced. If the amount of component (D) is less than the above lower limit, there is a risk of (meth)acrylic acid polymerizing during production, resulting in increased viscosity or gelation. Furthermore, only one type of polymerization inhibitor may be used, or two or more types may be selected and used from the above.

[0040] [Solvent] The desalting reaction of the present invention may be carried out either solvent-free or in an organic solvent, but is preferably carried out in an organic solvent from the viewpoint of ease of reaction progression. As the organic solvent, it is preferable to select and use one or more types from high-polarity solvents, and more preferably to select and use one or more types from each of high-polarity solvents and low-polarity solvents. The amount of solvent is preferably 0 to 200 parts by mass, more preferably 0 or 1 to 150 parts by mass, per 100 parts by mass of component (A).

[0041] In this reaction, the addition of a highly polar solvent allows the reaction to proceed efficiently. Regarding the type of highly polar solvent, if a protic solvent is used, there is a possibility that the halogen atoms may react with the solvent, so it is preferable to use an aprotic solvent. Furthermore, it is preferable to use a solvent with a high boiling point so that it can be used as a solvent even at high reaction temperatures. While the detailed mechanism of the reaction is not clear, it is believed that the addition of a highly polar solvent improves the solubility of the metal (meth)acrylate salt in the organic phase, accelerating the reaction between the halogen-containing silicone, which is an organic substance, and the metal (meth)acrylate salt, which is an inorganic salt. The amount of highly polar solvent is preferably 0 or 1 to 50 parts by weight, more preferably 5 to 45 parts by weight, and even more preferably 10 to 40 parts by weight per 100 parts by weight of component (A).

[0042] Examples of the aprotic highly polar solvent include ether solvents such as diethyl ether, tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, and dipropylene glycol dimethyl ether, ester solvents such as ethyl acetate and butyl acetate, nitrogen-containing solvents such as N,N-dimethylformamide, acetonitrile, and N-methyl-2-pyrrolidone, and mixed solvents thereof. These can be used alone or in appropriate combination of two or more.

[0043] In this reaction, a purification operation is carried out after completion of the reaction, and the addition of a low-polarity solvent can facilitate this purification operation. Examples of purification operations include water washing, filtration, stripping, distillation, etc., which can be carried out alone or in appropriate combination of two or more. Furthermore, if the acrylic group content is high, thickening or gelation can be suppressed by diluting the product with a low-polarity solvent.

[0044] Examples of low-polarity solvents include aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, heptane, octane, isooctane, cyclohexane, methylcyclohexane, and isoparaffin, hydrocarbon solvents such as industrial gasoline, petroleum benzine, and solvent naphtha, and mixed solvents thereof. These solvents can be used alone or in appropriate combinations of two or more. The amount of low-polarity solvent is preferably 0 to 200 parts by mass, more preferably 0 or 1 to 150 parts by mass, per 100 parts by mass of component (A).

[0045] [Desalting Reaction] In the present invention, the halogen atoms contained in component (A) and the acryloyl oxide moieties of component (B) are desalted in the presence of component (C), which serves as a catalyst, to obtain the target organopolysiloxane. The reaction is outlined below. Specific examples of the ≡Si-R-X in the formula are those explained in the section on component (A) above. X represents a halogen.

[0046] More specifically, the reaction temperature can be 50 to 150°C, preferably 60 to 145°C, and more preferably 70 to 140°C. If the reaction temperature is lower than the lower limit, the reaction may not proceed sufficiently. If the reaction temperature is higher than the upper limit, there is a risk of viscosity increase and gelation due to polymerization of the (meth)acrylic acid ester of component (B). The reaction time may be in the range of 1 to 72 hours, but is not limited thereto. The reaction atmosphere may be a nitrogen atmosphere or air, or a mixed gas such as nitrogen containing a small amount of oxygen may be used. The amount of oxygen in this case is 0.1 to 20%, preferably 0.5 to 18%, and more preferably 1 to 15%, by volume.

[0047] After the reaction is complete, the resulting salts are removed by washing with water or filtration, and the product is then obtained by dehydrating with sodium sulfate or removing low-molecular-weight components by vacuum stripping. The temperature during stripping may be 20°C to 130°C and the vacuum may be 1 to 200 mmHg (0.133 kPa to 26.664 kPa), but this is not a limitation.

[0048] The (meth)acryloyl group-containing organopolysiloxane obtained in the present invention is represented by the following average composition formula (5) or (6). (In the formula, R 6 are each independently a (meth)acryloyl group-containing alkyl group having 1 to 11 carbon atoms, and R 7 are each independently a group selected from a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and n and o are numbers that satisfy n≧1, o≧0, and 20≧n+o≧3. (In the formula, R 8 and R 8 ' are, independently of each other, R 6 and R 7 and R 8 and R 8 At least one of ' is R 6 In addition, p, q, r, and s are numbers that satisfy p≧2, q≧0, r≧0, s≧0, and 2≦p+q+r+s≦1,000.

[0049] In the formula R 6 is an alkyl group having 1 to 11 carbon atoms and having a (meth)acryloyl group at its terminal (hereinafter collectively referred to as a (meth)acryloyl group-containing group). The alkyl group is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.

[0050] In the formula R 7 are each independently a group selected from a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and are 2 The examples given above apply.

[0051] In the formula R 8 and R 8 ' is the above R 6 or R 7 Preferably, the number of silicon atoms to which the (meth)acryloyl group-containing groups are bonded is 1 to 100%, more preferably 3 to 75%, even more preferably 5 to 50%, and even more preferably 5 to 30% of the total number of silicon atoms. More preferably, R 8 At least one of ' is R6 In the average composition formula (6), p, q, r, and s are numbers that satisfy p≧2, q≧0, r≧0, s≧0, and 2≦p+q+r+s≦1,000. Preferably, p is a number from 2 to 32, q is a number from 0 to 998, r is a number from 0 to 10, s is a number from 0 to 10, and p+q+r+s is a number from 2 to 1,000, more preferably, p is a number from 2 to 20, q is a number from 1 to 798, r is a number from 0 to 6, s is a number from 0 to 6, and p+q+r+s is a number from 3 to 800. More preferably, p is 2, and q is a number from 1 to 600. Even more preferably, p is 2, q is a number from 1 to 400, and [R 8 'R 8 'SiO 2/2 ] d R bonded to the silicon atom of 8 At least one of ' is R 6 It is good to be.

[0052] The (meth)acryloyl group-containing group is the above-mentioned R 1 In the following formula, the dotted line indicates the bond to the silicon atom of the polysiloxane.

[0053] R 9 is a hydrogen atom or a methyl group.

[0054] In the average composition formula (5), n ≥ 1, o ≥ 0, and 20 ≥ n + o ≥ 3. Preferably, the organopolysiloxane has a viscosity at 25°C of 1 to 2,000 mPa s, more preferably 2 to 1,000 mPa s. The viscosity is a value measured with a BM-type rotational viscometer at 25°C.

[0055] Examples of organopolysiloxanes represented by the average composition formula (5) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein t is 1 to 20, u is 0 to 19, and v is 0 to 19; 20≧t+u+v≧3)

[0056] In the average composition formula (6), p≧2, q≧0, r≧0, s≧0, and 2≦p+q+r+s≦1,000. Preferably, the amount of (meth)acryloyl group-containing organic groups satisfies the above range, and the organopolysiloxane has a viscosity at 25°C of 5 to 10,000 mPa·s, more preferably 10 to 5,000 mPa·s. The (meth)acryloyl group-containing organopolysiloxane obtained by the above production method of the present invention can have a low viscosity. Preferably, it can have a viscosity of 5 to 3,000 mPa·s, more preferably 5 to 2,000 mPa·s, even more preferably 8 to 1,500 mPa·s, even more preferably 10 to 1,000 mPa·s, and particularly preferably 15 to 700 mPa·s. The viscosity is measured using a BM-type rotational viscometer.

[0057] Examples of organopolysiloxanes represented by the average composition formula (6) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein w is 0 to 997, x is 1 to 998, and y is 0 to 100; 1≦w+x≦998, and 0≦w+y≦998)

[0058] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, parts are parts by mass.

[0059] [(Meth)acryloyl group introduction rate] The (meth)acryloyl group introduction rate in the desalting reaction in the Examples and Comparative Examples was calculated as follows: The (meth)acryloyl group introduction rate in the present invention was calculated as follows: 1Using H-NMR, the sum of the integrals of the methylene group protons (δ = 3.49) bonded to the halogen atoms of the organopolysiloxane containing an alkyl group having a halogen atom, which is the raw material, and the methylene group protons (δ = 4.11) bonded to the (meth)acryloyloxy group produced as the reaction progresses and the halogen atoms are replaced with (meth)acryloyloxy groups, remains unchanged before and after the reaction, and this value was used as the reference. For example, if the sum of the integrals of the methylene group protons (δ = 3.49) bonded to the halogen atoms and the methylene group protons (δ = 4.11) bonded to the (meth)acryloyloxy group is taken as 1.00, then if the introduction rate of (meth)acryloyl groups by the desalting reaction is 100%, the integral of the methylene group protons (δ = 4.11) bonded to the (meth)acryloyloxy group will be 1.00. From this, the introduction rate of (meth)acryloyl groups was determined using the following formula: (Meth)acryloyl group introduction rate=[integral value of protons (δ=4.11) of methylene groups bonded to (meth)acryloyloxy groups / 1.00]×100 (%)

[0060] Example 1 A separable flask equipped with a stirrer, a thermometer, and a reflux condenser was charged with 140 g of an organopolysiloxane (viscosity at 25°C: 200 mPa s) represented by the following average compositional formula (A-1), 11.76 g of (B-1) potassium acrylate (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-1)), 1.89 g of (C-1) tetrabutylammonium bromide, 0.07 g of (D-1) 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, and 30 g of N,N-dimethylformamide as a solvent. The mixture was heated and stirred for 7 hours at a temperature such that the reaction system reached 120°C, while blowing 4% oxygen-mixed nitrogen gas into the reaction solution using a glass tube, to effect a reaction. Toluene was added to this reaction mixture, and the salt was removed by washing with water. After that, the toluene and other components were removed by vacuum stripping at 100°C for 4 hours at 15 mmHg, yielding an organopolysiloxane represented by the following average compositional formula (X-1). The target product was a brown, transparent product, and the acryloyl group introduction rate was 97%. (The ratio of the number of silicon atoms bonded to halogen-containing groups to the total number of silicon atoms is 5.7%)

[0061] Example 2 Example 1 was repeated, except that the amount of (C-1) was increased to 4.00 g and 30 g of N,N-dimethylformamide was omitted, to obtain an organopolysiloxane represented by the average composition formula (X-1). The target product was a brown, transparent product, and the acryloyl group introduction rate was 64%.

[0062] Example 3 Example 1 was repeated, except that 140 g of an organopolysiloxane (viscosity at 25°C: 200 mPa s) represented by the following average compositional formula (A-2) was used instead of (A-1) in Example 1, to obtain an organopolysiloxane represented by the following average compositional formula (X-2). The target product was a brown, transparent product, and the acryloyl group introduction rate was 97%. (The ratio of the number of silicon atoms bonded to halogen-containing groups to the total number of silicon atoms is 5.7%)

[0063] Example 4 A separable flask equipped with a stirrer, a thermometer, and a reflux condenser was charged with 70 g of an organopolysiloxane (viscosity at 25°C of 200 mPa s) represented by the following average compositional formula (A-3), 17.86 g of (B-1) potassium acrylate (an amount equivalent to 1.01 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-3)), 0.26 g of (C-1) tetrabutylammonium bromide, 0.05 g of (D-1) 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, and 14 g of N,N-dimethylformamide as a solvent. The mixture was heated and stirred for 3 hours at a temperature such that the reaction system reached 120°C, while blowing 4% oxygen-mixed nitrogen gas into the reaction solution using a glass tube, to effect a reaction. Toluene was added to this reaction mixture, and the salt was removed by washing with water. After that, the toluene and other components were removed by vacuum stripping at 115°C for 3 hours at 18 mmHg, yielding an organopolysiloxane represented by the following average compositional formula (X-3). The target product was a pale pink transparent product, and the acryloyl group introduction rate was 96%. (The ratio of the number of silicon atoms bonded to halogen-containing groups to the total number of silicon atoms is 20%)

[0064] Example 5 Into a separable flask equipped with a stirrer, a thermometer, and a reflux condenser, 200 g of an organopolysiloxane represented by the following average composition formula (A-4) (viscosity at 25°C: 60 mPa·s), 169 g of (B-1) potassium acrylate (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-4)), 1.88 g of (C-1) tetrabutylammonium bromide, and (D-1) 2-t-butylammonium bromide were added. A mixture of 0.40 g of ethyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, 0.04 g of (D-2) N,N'-diphenyl-p-phenylenediamine, 200 g of toluene as a solvent, and 80 g of N,N-dimethylformamide was charged, and the reaction was carried out for 5 hours with heating and stirring at a temperature of 115°C while 4% oxygen-mixed nitrogen gas was blown into the reaction solution through a glass tube. The reaction mixture was washed with water to remove salts, and then subjected to a vacuum strip at 70°C for 5 hours at 7.7 mmHg to remove toluene and other components, yielding an organopolysiloxane represented by the following average compositional formula (X-4). The target product was a brown, transparent product, and the acryloyl group introduction rate was 98%.

[0065] Example 6 The procedure of Example 5 was repeated, except that the amount of (C-1) was increased to 4.00 g and 80 g of N,N-dimethylformamide was omitted, to obtain an organopolysiloxane represented by average composition formula (X-4). The target product was a brown, transparent product, and the acryloyl group introduction rate was 97%.

[0066] Example 7 Example 5 was repeated, except that 6.00 g of (C-2) trioctylmethylammonium chloride was used instead of (C-1), 80 g of N,N-dimethylformamide was omitted, and the reaction time was changed to 7 hours, to obtain an organopolysiloxane represented by average composition formula (X-4). The target product was a brown, transparent product, and the acryloyl group introduction rate was 89%.

[0067] Example 8 Example 5 was repeated, except that 200 g of an organopolysiloxane (viscosity at 25°C: 70 mPa s) represented by the following average compositional formula (A-5) was used instead of (A-4) in Example 5, and the amount of (B-1) potassium acrylate was changed to 129 g (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-5)), to obtain an organopolysiloxane represented by the average compositional formula (X-5). The target product was a brown, transparent product, and the acryloyl group introduction rate was 95%.

[0068] [Comparative Example 1] An acrylic-modified silicone was produced using the catalyst tetramethylammonium chloride used in Examples 1 to 3 of Patent Document 3 (JP 2021-017424 A). Example 2 was repeated except that 4.00 g of tetramethylammonium chloride was used instead of (C-1) in Example 2 above, and an attempt was made to synthesize an organopolysiloxane represented by the average composition formula (X-1). However, after 7 hours of reaction, the acryloyl group introduction rate was 0%, and the reaction did not proceed.

[0069] [Comparative Example 2] An acrylic-modified silicone was produced using the catalyst tetramethylammonium chloride used in Examples 1 to 3 of Patent Document 3 (JP 2021-017424 A). Example 5 was repeated except that 4.00 g of tetramethylammonium chloride was used instead of (C-1) and 80 g of N,N-dimethylformamide was omitted, and an attempt was made to synthesize an organopolysiloxane represented by the average composition formula (X-4). However, after 5 hours of reaction, the acryloyl group introduction rate was 4%, and the reaction could not be completed.

[0070] It is believed that the reaction did not proceed in the methods of the above comparative examples due to the low miscibility between the organopolysiloxane having chloropropyl groups and the organic salt. In contrast, in the production method of the present invention, as shown in Examples 1 to 6, the reaction proceeds sufficiently even with organopolysiloxane having chloropropyl groups.

[0071] Comparative Example 3: An attempt was made to synthesize an organopolysiloxane represented by average composition formula (X-4) by repeating Example 5, except that (C-1) was omitted from Example 5. However, after 5 hours of reaction, the acryloyl group introduction rate was 2%, and the reaction could not be completed.

[0072]

[0073] According to the method of the present invention, it is possible to simply and efficiently synthesize a (meth)acryloyl-modified organopolysiloxane by reacting an organopolysiloxane having a halogen-containing organic group with a (meth)acrylate salt. The (meth)acryloyl-modified organopolysiloxane obtained by the production method of the present invention is useful for radiation-curable coating agents, additives, resins, etc.

Claims

1. (A) An organopolysiloxane selected from the group consisting of halogen-containing organopolysiloxanes (a-1) represented by the following average composition formula (1) and halogen-containing organopolysiloxanes (a-2) represented by the following average composition formula (2): (In the formula, R 1 are each independently a halogen-containing alkyl group having 1 to 11 carbon atoms, R 2 are each independently a substituted or unsubstituted group selected from a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers that satisfy a ≧ 1, b ≧ 0, and 20 ≧ a + b ≧ 3. (In the formula, R 3 and R 3 ' are each independently the above R 1 and R 2 R 3 and R 3 At least one of the above R 1 and c, d, e, and f are numbers that satisfy c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000), and (B) a metal (meth)acrylate is reacted in the presence of (C) a phase transfer catalyst selected from a quaternary ammonium salt having at least one monovalent hydrocarbon group having 4 to 20 carbon atoms, a crown ether, and a phosphonium compound to obtain the (meth)acryloyl group-containing organopolysiloxane.

2. The R of the halogen-containing organopolysiloxane (a-2) represented by the average composition formula (2) 1 2. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein the number of silicon atoms to which are bonded is 1 to 100% based on the total number of silicon atoms.

3. A method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, characterized in that component (B) is blended in an amount of 1 to 3 moles per mole of halogen atoms contained in component (A), and further, component (C) is blended in an amount of 0.05 to 10 parts by mass per 100 parts by mass of component (A).

4. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein the metal salt of (meth)acrylic acid (B) is an alkali metal salt.

5. The phase transfer catalyst (C) is represented by the following formula (3): R 4 4 N + X - (3) (wherein, R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms, provided that R 4 At least one of X is a linear or branched monovalent hydrocarbon group having 4 to 20 carbon atoms, and - 2. The method of claim 1, wherein the quaternary ammonium salt is represented by the formula:

6. The phase transfer catalyst (C) is a quaternary ammonium salt represented by the above formula (3), and the halide ion is Br - Or Cl - 6. The method for producing the (meth)acryloyl group-containing organopolysiloxane according to claim 5, wherein 7. R in the component (A) 1 2. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein each of the groups is independently an alkyl group having 1 to 7 carbon atoms and a halogen atom at the terminal.

8. In the above average composition formula (2), 1≦d≦998, R 3 At least one of the above R 1 2. The method for producing the (meth)acryloyl group-containing organopolysiloxane according to claim 1, wherein the acryloyl group is a group represented by the formula:

9. In the above average composition formula (2), 1≦d≦998, R 3 At least one of the above R 1 wherein R 1 2. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein each of the groups is independently an alkyl group having 1 to 5 carbon atoms and a halogen atom at the terminal.

10. The method for producing a (meth)acryloyl group-containing organopolysiloxane according to any one of claims 1 to 9, wherein in the above step, 0.01 to 1 part by mass of a polymerization inhibitor (D) is further blended per 100 parts by mass of the combined total of components (A) and (B).

Citation Information

Patent Citations

  • Method for preparing gama-(acryloyloxy)-propyl trialkoxy silane monomer

    CN101723965A

  • Propylene acyloxy methacryloxy silane and preparation method of its derivative

    CN104892661A

  • Preparation of organosilanes

    JP1977073826A

  • Preparation of organosilane

    JP1981104890A

  • Preparation of organosilane containing methacryloxy or acryloxy group

    JP1991209388A

Cited By

  • Organopolysiloxane and method for producing same

    WO2026063354A1

  • Curable organopolysiloxane composition, release coating agent, and release film

    WO2026063356A1