Method for producing (METH)acryloyl group-containing organopolysiloxane
The reaction of halogen-containing organopolysiloxane with (meth)acrylic acid and a basic alkali metal salt in the presence of a phase transfer catalyst addresses the challenges of handling and cost in conventional methods, achieving efficient and cost-effective production of (meth)acryloyl group-containing organopolysiloxane for radiation-curable coatings.
Patent Information
- Application Number
- PCT/JP2024/014798
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-12
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional methods for producing (meth)acryloyl group-containing organopolysiloxanes face challenges in terms of handling, cost, and reaction efficiency, with issues such as increased viscosity and the use of specialized and costly alkali metal salts.
A method involving the reaction of a halogen-containing organopolysiloxane with (meth)acrylic acid and a basic alkali metal salt in the presence of a phase transfer catalyst, such as quaternary ammonium salts, to efficiently synthesize (meth)acryloyl-modified organopolysiloxane with controlled reaction conditions and reduced costs.
This method allows for the production of (meth)acryloyl group-containing organopolysiloxane with high reaction efficiency and controlled conditions, reducing costs and improving handling properties, making it suitable for radiation-curable coatings and other applications.
Smart Images

Figure JP2024014798_31102024_PF_FP_ABST
Abstract
Description
Method for producing (meth)acryloyl group-containing organopolysiloxane
[0001] The present invention relates to a method for producing a (meth)acryloyl group-containing organopolysiloxane.
[0002] The technique of applying energy to a liquid resin composition to cure it is a widespread technology and is used in many fields, such as for producing coatings and molded products. The energy required for this curing is heat or radiation such as ultraviolet light. In the case of heat curing, a heat-activated catalyst is blended into the base resin, and a cured product is obtained by applying heat. In the case of radiation curing, a composition blended with a photoinitiator that is activated by ultraviolet light or other radiation is cured by irradiating it with radiation.
[0003] Typical functional groups used for radiation curing include (meth)acryloyl groups, mercapto groups, and epoxy groups. (Meth)acryloyl groups form crosslinks through radical polymerization reactions, while mercapto groups undergo radical ene-thiol reactions in the presence of alkenyl groups. Epoxy groups undergo cationic polymerization in the presence of acids.
[0004] Various resins are used for this type of radiation curing, one of which is silicone. Silicone is a general term for organopolysiloxanes with a main chain of continuous siloxane bonds and organic groups such as methyl groups on the side chains. Silicones have excellent heat resistance, cold resistance, chemical resistance, electrical insulation, and mold releasability, and can be made into various forms such as oil, rubber, and resin. Radiation-curable silicones are used as raw materials for cured products such as silicone rubber, silicones for release paper, and silicones for hard coatings.
[0005] Organopolysiloxanes containing (meth)acryloyl groups as radiation-polymerizable groups are used in release coatings, hard coats, and surface tension adjusters. A cured product can be obtained by blending a photopolymerization initiator with this base material and irradiating it with radiation while purging with nitrogen in a chamber to efficiently react the radicals generated by radiation.
[0006]
[0003] Several studies have been conducted on methods for producing such organopolysiloxanes containing (meth)acryloyl groups. In Patent Document 1, an organopolysiloxane containing (meth)acryloyl groups is produced by using an epoxy-modified organopolysiloxane as a raw material and reacting (meth)acrylic acid with an epoxy group. However, in this case, hydroxyl groups are generated as the epoxy ring opens, which increases the viscosity of the product, leaving a problem in terms of handling.
[0007] Patent Document 2 proposes a method of introducing acryloyl groups into siloxanes by reacting hydroxyethyl acrylate with methoxy-containing siloxanes and heating the mixture, accompanied by the distillation of methanol. However, the product obtained by this method contains hydrolyzable silicon-oxygen-carbon bonds, leaving problems in terms of storage stability.
[0008] Patent Document 3 discloses a method for introducing a (meth)acryloyl group into a siloxane compound by reacting a siloxane compound having a Cl-containing organic group with an alkali metal salt of (meth)acrylic acid in the presence of tetramethylammonium chloride. While this is a promising production method, the low activity of tetramethylammonium chloride poses a problem of poor reaction efficiency depending on the type of siloxane compound having a Cl-containing organic group. In addition, the alkali metal salt of (meth)acrylic acid requires special production and is not a general-purpose material, which also increases costs and poses a supply issue.
[0009] JP 2018-521188 A JP 2016-209874 A JP 2021-017424 A
[0010] As mentioned above, conventional methods for producing (meth)acryloyl group-containing organopolysiloxanes have problems with handling, cost, etc. Therefore, an object of the present invention is to provide a novel method for producing (meth)acryloyl group-containing organopolysiloxanes that allows for relatively easy control of reaction conditions, good reaction efficiency, and reduced costs.
[0011] As a result of extensive research conducted by the present inventors in order to achieve the above-mentioned object, they have found that a (meth)acryloyl-modified organopolysiloxane can be synthesized efficiently and at low cost by reacting an organopolysiloxane having a halogen-containing organic group, (meth)acrylic acid, and a basic alkali metal salt in the presence of a phase transfer catalyst.
[0012] That is, the present invention provides (A) an organopolysiloxane selected from the group consisting of a halogen-containing organopolysiloxane (a-1) represented by the following average composition formula (1) and a halogen-containing organopolysiloxane (a-2) represented by the following average composition formula (2): (In the formula, R 1 are each independently a halogen-containing alkyl group having 1 to 11 carbon atoms, and R 2 are each independently a group selected from a substituted or unsubstituted monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers that satisfy a ≧ 1, b ≧ 0, and 20 ≧ a + b ≧ 3. (In the formula, R 3 and R 3 ' are each independently the above R 1 and R 2 and R 3 and R 3 At least one of the R 1 and c, d, e, and f are numbers that satisfy the conditions c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000.) The present invention provides a method for producing a (meth)acryloyl group-containing organopolysiloxane, comprising the step of reacting (B-1) (meth)acrylic acid and (B-2) a basic alkali metal salt or a solution thereof in the presence of (C) a phase transfer catalyst selected from a quaternary ammonium salt having at least one monovalent hydrocarbon group having 4 to 20 carbon atoms, a crown ether, and a phosphonium compound to obtain the (meth)acryloyl group-containing organopolysiloxane.
[0013] The present invention further provides the above-mentioned production method, which further satisfies at least one of the following constituent requirements [1] to [9]: [1] The R 1 is bonded to 1 to 100% of the total number of silicon atoms. [2] A method for producing the (meth)acryloyl group-containing organopolysiloxane, characterized in that the amount of component (B-1) is 1 to 3 moles per mole of halogen atoms in component (A), and the amount of component (B-2) is 1 to 3 moles of alkali metal in component (B-2) per mole of halogen atoms in component (A), and further, component (C) is blended in an amount of 0.05 to 50 parts by mass per 100 parts by mass of component (A). [3] A method for producing the (meth)acryloyl group-containing organopolysiloxane, characterized in that the (B-2) basic alkali metal salt is a potassium salt. [4] A method for producing the (meth)acryloyl group-containing organopolysiloxane, characterized in that the (C) phase transfer catalyst is a compound represented by the following formula (3): R 4 4 N + X - (3) (wherein, R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms, provided that R 4 At least one of X is a linear or branched monovalent hydrocarbon group having 4 to 20 carbon atoms, and - [5] The method for producing the (meth)acryloyl group-containing organopolysiloxane, wherein the phase transfer catalyst (C) is a quaternary ammonium salt represented by the above formula (3), and the halide ion is Br - or Cl - [6] The method for producing the (meth)acryloyl group-containing organopolysiloxane, wherein R 1 are each independently an alkyl group having 1 to 7 carbon atoms and a halogen atom at the end.3 At least one of the R 1 [8] In the average composition formula (2), 1≦d≦998, and R 3 At least one of the R 1 and the R 1 are each independently a C1 to C5 alkyl group having a halogen atom at its terminal. [9] The method for producing the (meth)acryloyl group-containing organopolysiloxane, further comprising blending (D) a polymerization inhibitor in an amount of 0.01 to 1 part by mass per 100 parts by mass of the total of the components (A) and (B).
[0014] The production method of the present invention provides a novel method for producing (meth)acryloyl group-containing organopolysiloxanes, which allows for relatively easy control of reaction conditions and allows for cost reduction.
[0015] The present invention will be described in detail below.
[0016] [Component (A)] Component (A) is at least one organopolysiloxane selected from the group consisting of halogen-containing organopolysiloxane (a-1) represented by the following average composition formula (1) and halogen-containing organopolysiloxane (a-2) represented by the following average composition formula (2): (In the formula, R 1 are each independently a halogen-containing alkyl group having 1 to 11 carbon atoms, and R 2 are each independently a group selected from a substituted or unsubstituted monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers that satisfy a ≧ 1, b ≧ 0, and 20 ≧ a + b ≧ 3. (In the formula, R 3 and R 3 ' are each independently the above R 1 and R 2 and R 3 and R 3 At least one of the R 1and c, d, e, and f are numbers satisfying the following conditions: c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000.
[0017] R 1 are each independently an alkyl group having 1 to 11 carbon atoms, preferably an alkyl group having 1 to 7 carbon atoms, more preferably an alkyl group having 1 to 5 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms, which has a halogen at its terminal.
[0018] R 2 are each independently a substituted or unsubstituted monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, or a hydroxyl group-containing organic group. Examples of the monovalent hydrocarbon group having 1 to 11 carbon atoms include alkyl groups such as methyl, ethyl, propyl, and butyl, cycloalkyl groups such as cyclohexyl, and aryl groups such as phenyl and tolyl. Examples of the alkoxy group having 1 to 11 carbon atoms include methoxy, ethoxy, isopropoxy, and butoxy. Examples of the hydroxyl group-containing organic group include hydroxymethyl, hydroxyethyl, hydroxypropyl, and hydroxybutyl. R 2 is preferably a methyl group, an ethyl group, a methoxy group, an ethoxy group, or a hydroxyl group-containing organic group.
[0019] In the above average composition formula (2), R 3 and R 3 ' are, independently of each other, R 1 and R 2 and R 3 and R 3 At least one of the R 1 Preferably, R 3 At least one of the R 1 Therefore, preferably, in the average composition formula (2), 1≦d≦998, and R 3 At least one of R ' is an alkyl group having 1 to 7 carbon atoms and a halogen atom at the terminal, more preferably an alkyl group having 1 to 5 carbon atoms, and even more preferably an alkyl group having 1 to 3 carbon atoms. 3 is R2 That is, a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, or a hydroxyl group-containing organic group, and more preferably, R 3 is an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group, or a hydroxyl group-containing organic group.
[0020] In the above average composition formula (2), the ratio of the number of halogen-containing alkyl groups having 1 to 11 carbon atoms (i.e., R 1 The ratio of the number of silicon atoms to which halogen-containing alkyl groups having 1 to 11 carbon atoms are bonded is preferably 1 to 100%, more preferably 3 to 75%, more preferably 5 to 50%, and even more preferably 5 to 30%. If the number of silicon atoms to which halogen-containing alkyl groups having 1 to 11 carbon atoms are bonded is less than 1%, the curability when cured by radiation may be insufficient.
[0021] R 1 Examples of the halogen-containing organic group include halogen alkyl groups such as chloromethyl, chloroethyl, chloropropyl, chlorobutyl, chloropentyl, chlorohexyl, chlorooctyl, bromomethyl, bromoethyl, bromopropyl, bromobutyl, bromopentyl, bromohexyl, bromooctyl, iodomethyl, iodoethyl, iodopropyl, iodobutyl, iodopentyl, iodohexyl, and iodooctyl. From the viewpoint of ease of reaction, the substitution position of the halogen atom is preferably primary or secondary, and more preferably primary. As the halogen-containing organic group, a chloroalkyl group or a bromoalkyl group is preferred from the viewpoint of ease of availability of raw materials for the functional group, and a chloroalkyl group is particularly preferred. Among these, a chloromethyl group, a chloroethyl group, and a chloropropyl group are preferred. The halogen-containing alkyl group having 1 to 11 carbon atoms, preferably 1 to 5 carbon atoms, may be linear or branched. R 1 is represented, for example, by the following structure: In the following formula, the positions indicated by dotted lines are bonds to the silicon atoms of the organopolysiloxane.
[0022] In the average composition formula (1), a and b are numbers that satisfy a≧1, b≧0, and 20≧a+b≧3; preferably, a is a number from 1 to 15, b is a number from 0 to 15, and a+b is a number from 3 to 15, and more preferably, a is a number from 1 to 10, b is a number from 0 to 10, and a+b is a number from 3 to 10. Preferably, the organopolysiloxane has a viscosity at 25°C of 1 to 2,000 mPa s, and more preferably a viscosity of 2 to 1,000 mPa s. The viscosity is a value measured using a BM-type rotational viscometer at 25°C.
[0023] Examples of organopolysiloxanes represented by average composition formula (1) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (In the formula, g is 1 to 20, h is 0 to 19, i is 0 to 19, and 20≧g+h+i≧3.)
[0024] In the average composition formula (2), c, d, e, and f are numbers that satisfy the following conditions: c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000. Preferably, c is a number from 2 to 32, d is a number from 0 to 998, d is preferably a number from 1 to 998, e is a number from 0 to 10, f is a number from 0 to 10, and c+d+e+f is 2 to 1,000. More preferably, c is a number from 2 to 20, d is a number from 1 to 798, e is a number from 0 to 6, f is a number from 0 to 6, and c+d+e+f is 3 to 800. More preferably, c is 2, and d is a number from 1 to 600. Even more preferably, c is 2, and d is a number from 1 to 400. As described above, [R 3 'R 3 'SiO 2/2 ] d R bonded to the silicon atom of 3 At least one of the R 1 Preferably, the alkyl group (R 1 The ratio of silicon atoms to which the hydroxyl group (C) is bonded falls within the above range, and the organopolysiloxane has a viscosity at 25°C of 5 to 10,000 mPa s, and more preferably 10 to 5,000 mPa s. The viscosity is measured using a BM-type rotational viscometer.
[0025] Examples of organopolysiloxanes represented by average composition formula (2) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein j is 0 to 997, k is 1 to 998, and l is 0 to 100, and 1≦j+k≦998 or 0≦j+i≦998 is satisfied.)
[0026] [Component (B)] Component (B) comprises (B-1) (meth)acrylic acid and (B-2) a basic alkali metal salt or a solution thereof, and generates a metal (meth)acrylate represented by the following general formula (4) through a neutralization reaction in the reaction system. This metal (meth)acrylate functions as a reaction reagent for introducing a (meth)acryloyl group into component (A).
[0027] In formula (4), R 5 is a hydrogen atom or a methyl group, and M + is an alkali metal ion. Examples of alkali metal ions include potassium ion, sodium ion, and lithium ion. Among these, M is preferred from the viewpoint of ease of proceeding with the desalination reaction. + is preferably a potassium ion.
[0028] Examples of the component (B-2) include potassium hydroxide, potassium bicarbonate, potassium carbonate, sodium hydroxide, sodium bicarbonate, sodium carbonate, lithium hydroxide, lithium bicarbonate, and lithium carbonate. Among these, potassium hydroxide, potassium bicarbonate, and potassium carbonate are preferred from the viewpoint of the ease of proceeding of the desalting reaction after neutralization to form a (meth)acrylate salt. These may be used in a solid state or in a solution such as an aqueous solution. For example, an aqueous potassium hydroxide solution may be used. The concentration of the solution is not particularly limited, and a general concentration may be used.
[0029] The amounts of component (B-1) and component (B-2) are preferably such that 1 to 3 moles, preferably 1 to 2 moles, and more preferably 1.01 to 1.5 moles of component (B-1) are reacted per mole of halogen atoms in the organopolysiloxane (A). Furthermore, 1 to 3 moles, preferably 1 to 2.6 moles, and more preferably 1.01 to 2.2 moles of alkali metal contained in component (B-2) are reacted per mole of halogen atoms in the organopolysiloxane (A). If the amount of component (B) is less than the lower limit, the rate of introduction of (meth)acryloyl groups via the desalting reaction decreases. If the amount is greater than the upper limit, the rate of introduction of (meth)acryloyl groups via the desalting reaction increases, but the amount of component (B) is too high, which may result in a decrease in pot yield or an increase in the viscosity of the reaction mixture, making it difficult to handle.
[0030] [Component (C)] Component (C) is a phase transfer catalyst selected from quaternary ammonium salts having at least one monovalent hydrocarbon group having 4 to 20 carbon atoms, crown ethers, and phosphonium compounds, and is preferably a quaternary ammonium salt represented by the following general formula (3): R 4 4 N + X - (3) (wherein, R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms. 4 At least one of X is a linear or branched monovalent hydrocarbon group having 4 to 20 carbon atoms. - is a halide ion)
[0031] R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 18 carbon atoms, and more preferably 1 to 16 carbon atoms. 4 At least one of R is a linear or branched hydrocarbon group having 4 to 20 carbon atoms, preferably 4 to 18 carbon atoms, and more preferably 4 to 16 carbon atoms. 4Examples of R include alkyl groups such as methyl, ethyl, propyl, n-butyl, isopropyl, t-butyl, pentyl, hexyl, and octyl groups, cycloalkyl groups such as cyclohexyl, and phenyl groups. Among these, from the viewpoint of the efficiency of the desalting reaction, R 4 is preferably a straight-chain alkyl group, and more preferably an n-butyl group, an n-pentyl group, or an n-hexyl group.
[0032] R 4 However, the reason why the reaction efficiency improves when the alkyl group is a butyl group, pentyl group, hexyl group, or other alkyl group is thought to be that the presence of an alkyl group with a long chain length improves the compatibility with silicone of the ammonium (meth)acrylate salt generated by the ion exchange reaction between the quaternary ammonium salt, which is the phase transfer catalyst, and the metal (meth)acrylate salt, making it easier to promote the reaction.
[0033] X - is a halide ion, and from the viewpoint of availability, Br - or Cl - is preferred.
[0034] Examples of the phase transfer catalyst represented by formula (3) include compounds represented by the following structures:
[0035] The amount of component (C) blended is 0.05 to 50 parts by mass, preferably 0.1 to 45 parts by mass, and more preferably 0.3 to 40 parts by mass, per 100 parts by mass of component (A). If the amount is less than the lower limit, the reaction may not proceed sufficiently. If the amount exceeds the upper limit, the curability when cured by radiation may decrease. Furthermore, only one type of phase transfer catalyst may be used, or two or more types may be selected from the above.
[0036] [Component (D)] Component (D) is a polymerization inhibitor, an additive that inhibits self-polymerization of (B) metal (meth)acrylate without reacting with component (A) during the reaction. The polymerization inhibitor is not limited as long as it has the effect of inhibiting radical polymerization, and examples thereof include alkylphenols such as those listed below.
[0037] p-Methoxyphenol, 2,6-di-t-butylhydroxytoluene, 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, 4,4'-dioxydiphenol, 1,1'-bis(4-hydroxyphenyl)-cyclohexane, 3-methyl-4-isopropylphenol, 2,4,5-tri-hydroxybutyrophenone, 2,6-di-t-butylphenol, 2, 5-di-t-amylhydroquinone, 2,5-di-t-butylhydroquinone, 4-hydroxymethyl-2,6-di-t-butylphenol, 2,6-di-t-butyl-α-dimethylamino-p-cresol, 4,4-bis(2,6-di-butylphenol), 2,2'-methylene-bis(4-ethyl-6-t-butylphenol), 2,2'-methylene(2,6-di-t-butylphenol), 4,4'-methylene(2,6-di-t-butylphenol), 4,4'-butylidene(3-methyl-6-t-butylphenol), 4,4'-thio-bis(6-t-butyl-3-methylphenol), bis(3-methyl-4-hydroxy-5-t-butylbenzyl)sulfide, and 4,4'-thio-bis(6-t-butyl-o-cresol), 2,2'-thio-bis(4-methyl-6-t-butylphenol).
[0038] Amine-based polymerization inhibitors can also be used, such as those listed below.
[0039] Alkylated diphenylamines, N,N'-diphenyl-p-phenylenediamine, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidine, 4-benzoyloxy-2,2,6,6-tetramethylpiperidine, 1,4-dihydroxy-2,2,6,6-tetramethylpiperidine, and 1-hydroxy-4-benzoyloxy-2,2,6,6-tetramethylpiperidine.
[0040] The amount of polymerization inhibitor is 0.01 to 1 part by mass, preferably 0.02 to 0.5 parts by mass, and more preferably 0.03 to 0.3 parts by mass, per 100 parts by mass of the combined total of components (A) and (B). If the amount of component (D) is greater than the above upper limit, the curability of the resulting radiation-curable organopolysiloxane composition containing the radically polymerizable organopolysiloxane may be reduced. If the amount of component (D) is less than the above lower limit, there is a risk of (meth)acrylic acid polymerizing during production, resulting in increased viscosity or gelation. Furthermore, only one type of polymerization inhibitor may be used, or two or more types may be selected and used from the above.
[0041] [Solvent] The desalting reaction of the present invention may be carried out either solvent-free or in an organic solvent, but is preferably carried out in an organic solvent from the viewpoint of ease of reaction progression. As the organic solvent, it is preferable to select and use one or more types from high-polarity solvents, and more preferably to select and use one or more types from each of high-polarity solvents and low-polarity solvents. The amount of solvent is preferably 0 to 700 parts by mass, more preferably 0 or 1 to 500 parts by mass, and more preferably 10 to 500 parts by mass per 100 parts by mass of component (A).
[0042] In this reaction, the addition of a highly polar organic solvent allows the reaction to proceed efficiently. Regarding the type of highly polar solvent, if a protic solvent is used, there is a possibility that the halogen atoms may react with the solvent, so it is preferable to use an aprotic solvent. Furthermore, it is preferable to use a solvent with a high boiling point so that it can be used as a solvent even at high reaction temperatures. Although the detailed mechanism of the reaction has not been clarified, it is believed that the addition of a highly polar solvent improves the solubility of the metal (meth)acrylate salt in the organic phase, accelerating the reaction between the halogen-containing silicone, which is an organic substance, and the metal (meth)acrylate salt, which is an inorganic salt. The amount of highly polar solvent is preferably 0 or 1 to 50 parts by weight, more preferably 5 to 45 parts by weight, and even more preferably 10 to 40 parts by weight per 100 parts by weight of component (A).
[0043] Examples of the aprotic highly polar solvent include ether solvents such as diethyl ether, tetrahydrofuran, dioxane, diethylene glycol dimethyl ether, and dipropylene glycol dimethyl ether, ester solvents such as ethyl acetate and butyl acetate, nitrogen-containing polar solvents such as N,N-dimethylformamide, acetonitrile, and N-methyl-2-pyrrolidone, and mixed solvents thereof. These can be used alone or in appropriate combination of two or more.
[0044] In this reaction, a purification operation is carried out after completion of the reaction, and the addition of a low-polarity solvent can facilitate this purification operation. Examples of purification operations include water washing, filtration, stripping, distillation, etc., which can be carried out alone or in appropriate combination of two or more. Furthermore, if the acrylic group content is high, thickening or gelation can be suppressed by diluting the product with a low-polarity solvent.
[0045] Examples of low-polarity solvents include aromatic hydrocarbon solvents such as toluene and xylene, aliphatic hydrocarbon solvents such as hexane, heptane, octane, isooctane, cyclohexane, methylcyclohexane, and isoparaffin, hydrocarbon solvents such as industrial gasoline, petroleum benzine, and solvent naphtha, and mixed solvents thereof. These solvents can be used alone or in appropriate combinations of two or more. The amount of low-polarity solvent is preferably 0 to 700 parts by mass, more preferably 0 or 1 to 500 parts by mass, more preferably 10 to 500 parts by mass, and even more preferably 20 to 500 parts by mass per 100 parts by mass of component (A).
[0046] In this reaction-based production method, components (B-1) and (B-2) undergo a neutralization reaction in the reaction system to produce a metal (meth)acrylate. The halogen atoms contained in component (A) and the acryloyl oxide moiety of the metal (meth)acrylate undergo a desalination reaction in the presence of component (C), which serves as a catalyst, to produce the target organopolysiloxane. The reaction can be summarized as follows:
[0047] [Neutralization Reaction] In the production method of this reaction, the step of producing a metal (meth)acrylate in the reaction system by the neutralization reaction of (B-1) and (B-2) is outlined below.
[0048] [Desalting Reaction] In this production method, the halogen atoms contained in component (A) and the acryloyl oxide moieties of component (B) generated in the reaction system are desalted using the catalyst component (C) to obtain the target organopolysiloxane. The reaction outline is shown below. Specific examples of ≡Si-R-X in the formula are those explained in the section on component (A) above. X represents a halogen. In this production method, the neutralization reaction and desalting reaction can be carried out by charging component (A), component (B-1), component (B-2), and component (C) all at once to a reaction system in the presence of an optional polymerization inhibitor and solvent. Alternatively, components (B-1) and (B-2) may be stirred before adding components (A) and (C) to the reaction system. This allows the neutralization reaction to proceed first, thereby efficiently introducing (meth)acryloyl groups. For example, an aqueous solution of (B-1) (meth)acrylic acid and (B-2) a basic alkali metal salt is stirred in the amounts described above, preferably in the presence of a polymerization inhibitor. The stirring temperature and time can be adjusted appropriately, for example, 1 to 2 hours at room temperature. Next, the reaction system is charged with (A) an organopolysiloxane, (C) a phase transfer catalyst, and optional polymerization inhibitors and solvents, and the reaction is allowed to proceed, thereby obtaining the desired organopolysiloxane.
[0049] More specifically, the reaction temperature can be 50 to 150°C, preferably 60 to 145°C, and more preferably 70 to 140°C. If the reaction temperature is lower than the lower limit, the reaction may not proceed sufficiently. If the reaction temperature is higher than the upper limit, there is a risk of viscosity increase and gelation due to polymerization of the (meth)acrylic acid ester of component (B). The reaction time may be in the range of 1 to 72 hours, but is not limited thereto. The reaction atmosphere may be a nitrogen atmosphere or air, or a mixed gas such as nitrogen containing a small amount of oxygen may be used. The amount of oxygen in this case is 0.1 to 20%, preferably 0.5 to 18%, and more preferably 1 to 15%, by volume.
[0050] After the reaction is complete, the resulting salts are removed by washing with water or filtration, and the product is then obtained by dehydrating with sodium sulfate or removing low-molecular-weight components by vacuum stripping. The temperature during stripping may be 20°C to 130°C and the vacuum may be 1 to 200 mmHg (0.133 kPa to 26.664 kPa), but this is not a limitation.
[0051] The (meth)acryloyl group-containing organopolysiloxane obtained in the present invention is represented by the following average composition formula (5) or (6). (In the formula, R 6 are each independently a (meth)acryloyl group-containing alkyl group having 1 to 11 carbon atoms or a terminal hydroxyl group-containing alkyl group having 1 to 11 carbon atoms, and R 7 are each independently a group selected from a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and n and o are numbers that satisfy n≧1, o≧0, and 20≧n+o≧3. (In the formula, R 8 and R 8 ' are, independently of each other, R 6 and R 7 and R 8 and R 8 At least one of ' is R 6 In addition, p, q, r, and s are numbers that satisfy p≧2, q≧0, r≧0, s≧0, and 2≦p+q+r+s≦1,000.
[0052] In the formula R 6 is an alkyl group having 1 to 11 carbon atoms and a (meth)acryloyl group at its terminal (hereinafter collectively referred to as a (meth)acryloyl group-containing group), or an alkyl group having 1 to 11 carbon atoms and a hydroxy group at its terminal (hereinafter collectively referred to as a hydroxy group-containing group). The alkyl group is preferably an alkyl group having 1 to 5 carbon atoms, and more preferably an alkyl group having 1 to 3 carbon atoms.
[0053] In the formula R 7 are each independently a group selected from a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and are 2 The examples given above apply.
[0054] In the formula R 8 and R 8 ' is the above R 6 or R 7 Preferably, the number of silicon atoms to which the (meth)acryloyl group-containing groups are bonded is 1 to 100%, more preferably 3 to 75%, even more preferably 5 to 50%, and even more preferably 5 to 30% of the total number of silicon atoms. More preferably, R 8 At least one of ' is R 6 In the average composition formula (6), p, q, r, and s are numbers that satisfy p≧2, q≧0, r≧0, s≧0, and 2≦p+q+r+s≦1,000. Preferably, p is a number from 2 to 32, q is a number from 0 to 998, r is a number from 0 to 10, s is a number from 0 to 10, and p+q+r+s is a number from 2 to 1,000, more preferably, p is a number from 2 to 20, q is a number from 1 to 798, r is a number from 0 to 6, s is a number from 0 to 6, and p+q+r+s is a number from 3 to 800. More preferably, p is 2, and q is a number from 1 to 600. Even more preferably, p is 2, q is a number from 1 to 400, and [R 8 'R 8 'SiO 2/2 ] d R bonded to the silicon atom of 8 At least one of ' is R 6 It is good to be.
[0055] The (meth)acryloyl group-containing group is the above-mentioned R1 In the following formula, the dotted line indicates the bond to the silicon atom of the polysiloxane. The hydroxyl group-containing group is defined as R 1 The terminal halogen atom of the halogen-containing group represented by the formula (I) is substituted with a hydroxy group.
[0056] R 9 is a hydrogen atom or a methyl group.
[0057] In the average composition formula (5), n ≥ 1, o ≥ 0, and 20 ≥ n + o ≥ 3. Preferably, the organopolysiloxane has a viscosity at 25°C of 1 to 2,000 mPa s, more preferably 2 to 1,000 mPa s. The viscosity is a value measured with a BM-type rotational viscometer at 25°C.
[0058] Examples of organopolysiloxanes represented by the average composition formula (5) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein t is 1 to 20, u is 0 to 19, and v is 0 to 19; 20≧t+u+v≧3)
[0059] In the average composition formula (6), p≧2, q≧0, r≧0, s≧0, and 2≦p+q+r+s≦1,000. Preferably, the amount of (meth)acryloyl group-containing organic groups satisfies the above range, and the organopolysiloxane has a viscosity at 25°C of 5 to 10,000 mPa·s, more preferably 10 to 5,000 mPa·s. The (meth)acryloyl group-containing organopolysiloxane obtained by the above production method of the present invention can have a low viscosity. Preferably, it can have a viscosity of 5 to 3,000 mPa·s, more preferably 5 to 2,000 mPa·s, even more preferably 8 to 1,500 mPa·s, even more preferably 10 to 1,000 mPa·s, and particularly preferably 15 to 700 mPa·s. The viscosity is a value measured using a BM-type rotational viscometer.
[0060] Examples of organopolysiloxanes represented by the average composition formula (6) include compounds represented by the following structures: In the formula, Me represents a methyl group and Ph represents a phenyl group. (wherein w is 0 to 997, x is 1 to 998, and y is 0 to 100; 1≦w+x≦998, and 0≦w+y≦998)
[0061] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, parts are parts by mass.
[0062] [(Meth)acryloyl group introduction rate] The (meth)acryloyl group introduction rate in the desalting reaction in the Examples and Comparative Examples was calculated as follows: The (meth)acryloyl group introduction rate in the present invention was calculated as follows: 1Using H-NMR, it was determined that the sum of the integrals of the protons (δ = 3.49) of methylene groups bonded to halogen atoms in the organopolysiloxane containing an alkyl group having a halogen atom (the starting material), the protons (δ = 3.59) of methylene groups bonded to hydroxy groups formed as the reaction progresses and the halogen atoms are substituted with hydroxy groups, and the protons (δ = 4.11) of methylene groups bonded to (meth)acryloyloxy groups formed as the halogen atoms are substituted with (meth)acryloyloxy groups, remained unchanged before and after the reaction, and therefore this value was used as the reference. For example, if the sum of the integrals of the methylene group protons bonded to halogen atoms (δ = 3.49), the methylene group protons bonded to hydroxy groups (δ = 3.59), and the methylene group protons bonded to (meth)acryloyloxy groups (δ = 4.11) is taken as 1.00, and the introduction rate of (meth)acryloyl groups by the desalting reaction is 100%, the integral of the methylene group protons bonded to (meth)acryloyloxy groups (δ = 4.11) will be 1.00. From this, the introduction rate of (meth)acryloyl groups was calculated using the following formula: (meth)acryloyl group introduction rate = [integral value of the methylene group protons bonded to (meth)acryloyloxy groups (δ = 4.11) / 1.00] x 100 (%)
[0063] Example 1 An organopolysiloxane (viscosity at 25°C) represented by the following average composition formula (A-1) was added to a separable flask equipped with a stirrer, a thermometer, and a Dean-Stark apparatus. A mixture containing 100.00 g of a hydroxypropyl methylcellulose (200 mPa s), 5.49 g of (B-1a) acrylic acid (an amount that was 1.04 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-1)), 10.54 g of (B-2a) potassium carbonate (an amount that was 1.04 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-1)), 0.67 g of (C-1) tetrabutylammonium bromide, 0.05 g of (D-1) 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenyl acrylate, and 21.43 g of N,N-dimethylformamide as a solvent was added, and the mixture was heated and stirred at a temperature such that the reaction system reached 120°C for 5 hours to effect a reaction. To this reaction mixture was added 35.71 g of toluene, and the salt was removed by washing with water. After that, the toluene and other components were removed by vacuum stripping at 100°C for 2 hours at 15 mmHg, yielding an organopolysiloxane represented by the following average compositional formula (X-1). The target product was a brown, transparent product, and the acryloyl group introduction rate was 90%. (The ratio of the number of silicon atoms bonded to halogen-containing groups to the total number of silicon atoms is 5.7%)
[0064] Example 2 The procedure of Example 1 was repeated, except that the amount of (C-1) was increased to 2.00 g and 21.43 g of N,N-dimethylformamide was omitted, to obtain an organopolysiloxane represented by the average composition formula (X-1). The target product was a brown, transparent product, and the acryloyl group introduction rate was 74%.
[0065] Example 3 Example 1 was repeated, except that 100.00 g of an organopolysiloxane (viscosity at 25°C: 200 mPa s) represented by the following average compositional formula (A-2) was used instead of (A-1) in Example 1, to obtain an organopolysiloxane represented by the following average compositional formula (X-2). The target product was brown and transparent, and the acryloyl group introduction rate was 91%. (The ratio of the number of silicon atoms bonded to halogen-containing groups to the total number of silicon atoms is 5.7%)
[0066] Example 4 Into a separable flask equipped with a stirrer, a thermometer, and a Dean-Stark apparatus, 70.00 g of an organopolysiloxane (viscosity at 25°C: 200 mPa·s) represented by the following average composition formula (A-3), 11.68 g of (B-1a) acrylic acid (an amount equivalent to 1.01 molar equivalent per mole of halogen atoms in the organopolysiloxane (A-3)), and 22.40 g of (B-2a) potassium carbonate (an amount equivalent to 1.01 molar equivalent per mole of halogen atoms in the organopolysiloxane (A-3)) were added. A mixture of (C-1) tetrabutylammonium bromide (amount equivalent to 1.01 molar equivalent per mole of halogen atoms in (A-3)), 0.39 g of (C-1) tetrabutylammonium bromide, 0.04 g of (D-1) 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, and 14.00 g of N,N-dimethylformamide as a solvent was added and the reaction system was heated and stirred for 6 hours at a temperature of 120°C to allow the reaction to proceed. 30.00 g of toluene was added to the reaction mixture, and the salt was removed by washing with water. After that, the toluene and other components were removed by vacuum stripping at 120°C for 3 hours at 18 mmHg, yielding an organopolysiloxane represented by the following average compositional formula (X-3). The target product was a pale pink transparent product, and the acryloyl group introduction rate was 93%. (The ratio of the number of silicon atoms bonded to halogen-containing groups to the total number of silicon atoms is 20%)
[0067] Example 5 Into a separable flask equipped with a stirrer, a thermometer, and a Dean-Stark apparatus was added 20 g of an organopolysiloxane (viscosity at 25°C of 60 mPa·s) represented by the following average composition formula (A-4), 11.07 g of (B-1a) acrylic acid (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-4)), and 21.24 g of (B-2a) potassium carbonate (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-4)). 5 molar equivalents), 0.50 g of (C-1) tetrabutylammonium bromide, 0.05 g of (D-1) 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, 0.01 g of (D-2) N,N'-diphenyl-p-phenylenediamine, 80.00 g of toluene as a solvent, and 8.00 g of N,N-dimethylformamide were charged and reacted for 8 hours with heating and stirring at a temperature such that the reaction system reached 110°C. The reaction mixture was washed with water to remove salts, and then subjected to a vacuum strip at 70°C for 5 hours at 18 mmHg to remove toluene and other components, yielding an organopolysiloxane represented by the following average compositional formula (X-4). The target product was a brown, transparent product, and the acryloyl group introduction rate was 90%.
[0068] Example 6 The procedure of Example 5 was repeated, except that 0.75 g of (C-2) trioctylmethylammonium chloride was used instead of (C-1) tetrabutylammonium bromide, to obtain an organopolysiloxane represented by average composition formula (X-4). The target product was a brown, transparent product, and the methacryloyl group introduction rate was 66%.
[0069] Example 7 Example 5 was repeated, except that the amount of (C-1) was increased to 1.00 g, 8.00 g of N,N-dimethylformamide was omitted, and the reaction time was changed to 13 hours, to obtain an organopolysiloxane represented by average composition formula (X-4). The target product was a brown, transparent product, and the acryloyl group introduction rate was 87%.
[0070] Example 8 Into a separable flask equipped with a stirrer, a thermometer, and a reflux condenser was added 100 g of an organopolysiloxane represented by the average composition formula (A-4) (viscosity at 25°C: 60 mPa·s), 64.3 g of (B-1a) acrylic acid (an amount equivalent to 1.22 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-4)), and 102.7 g of (B-2b) 48% aqueous potassium hydroxide solution (an amount equivalent to 1.22 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-4)). (Amount equivalent to 1.20 molar equivalents relative to the total weight of the hydroxybenzoate), 30.0 g of (C-1) tetrabutylammonium bromide, 0.30 g of (D-1) 2-t-butyl-6-(3-t-butyl-2-hydroxy-5-methylbenzyl)-4-methylphenylacrylate, 0.05 g of (D-2) N,N'-diphenyl-p-phenylenediamine, 0.20 g of (D-3) p-methoxyphenol, and 40.0 g of toluene as a solvent were charged and reacted for 11 hours with heating and stirring at a temperature such that the reaction system reached 100°C. The reaction mixture was washed with water to remove salts, and then subjected to a vacuum strip at 70°C for 5 hours at 18 mmHg to remove toluene and other components, yielding an organopolysiloxane represented by the average compositional formula (X-4). The target product was a brown, transparent product, and the acryloyl group introduction rate was 96%.
[0071] Example 9 Example 5 was repeated, except that 13.22 g of (B-1b) methacrylic acid was used instead of (B-1a) acrylic acid, to obtain an organopolysiloxane represented by the average composition formula (X-4'). The target product was a brown, transparent product, and the methacryloyl group introduction rate was 91%.
[0072] Example 10 Example 5 was repeated, except that 20 g of an organopolysiloxane (viscosity at 25°C: 70 mPa s) represented by the following average compositional formula (A-5) was used instead of (A-4), the amount of (B-1a) acrylic acid was changed to 8.45 g (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-5)), and the amount of (B-2a) potassium carbonate was changed to 16.24 g (an amount equivalent to 1.05 molar equivalents per mole of halogen atoms in the organopolysiloxane (A-5)), to obtain an organopolysiloxane represented by the average compositional formula (X-5). The target product was a brown, transparent product, and the acryloyl group introduction rate was 90%.
[0073] Comparative Example 1 An acrylic-modified silicone was produced using the catalyst tetramethylammonium chloride used in Examples 1 to 3 of Patent Document 3 (JP 2021-017424 A). Example 2 was repeated except that 2.00 g of tetramethylammonium chloride was used instead of (C-1) in Example 2, and an attempt was made to synthesize an organopolysiloxane represented by the average composition formula (X-1). However, after 5 hours of reaction, the acryloyl group introduction rate was 1%, and the reaction could not be completed.
[0074] [Comparative Example 2] An acrylic-modified silicone was produced using the catalyst tetramethylammonium chloride used in Examples 1 to 3 of Patent Document 3 (JP 2021-017424 A). Example 5 was repeated except that 0.50 g of tetramethylammonium chloride was used instead of (C-1) and 8.00 g of N,N-dimethylformamide was omitted, and an attempt was made to synthesize an organopolysiloxane represented by the average composition formula (X-4). However, after 5 hours of reaction, the acryloyl group introduction rate was 5%, and the reaction could not be completed.
[0075] It is believed that the reaction did not proceed in the methods of the above comparative examples due to the low miscibility between the organopolysiloxane having chloropropyl groups and the organic salt. In contrast, in the production method of the present invention, as shown in Examples 1 to 10, the reaction proceeds sufficiently even with organopolysiloxane having chloropropyl groups.
[0076] Comparative Example 3: The synthesis of an organopolysiloxane represented by average composition formula (X-4) was attempted by repeating Example 5, except that (C-1) was omitted from Example 5. However, after 5 hours of reaction, the acryloyl group introduction rate was 0%, and the reaction could not be completed.
[0077] Comparative Example 4 The synthesis of an organopolysiloxane represented by average composition formula (X-4) was attempted by repeating Example 5, except that (B-2a) was omitted from Example 5. However, after 5 hours of reaction, the acryloyl group introduction rate was 0%, and the reaction could not be completed.
[0078]
[0079] As described above, the method of the present invention makes it possible to simply and efficiently produce a (meth)acryloyl-modified organopolysiloxane by reacting an organopolysiloxane having a halogen-containing organic group with a (meth)acrylate salt. The (meth)acryloyl-modified organopolysiloxane obtained by the production method of the present invention is useful for radiation-curable coating agents, additives, resins, etc.
Claims
1. (A) An organopolysiloxane selected from the group consisting of halogen-containing organopolysiloxanes (a-1) represented by the following average composition formula (1) and halogen-containing organopolysiloxanes (a-2) represented by the following average composition formula (2): (In the formula, R 1 are each independently a halogen-containing alkyl group having 1 to 11 carbon atoms, R 2 are each independently a substituted or unsubstituted group selected from a monovalent hydrocarbon group having 1 to 11 carbon atoms, an alkoxy group having 1 to 11 carbon atoms, and an organic group having a hydroxyl group, and a and b are numbers that satisfy a ≧ 1, b ≧ 0, and 20 ≧ a + b ≧ 3. (In the formula, R 3 and R 3 ' are each independently the above R 1 and R 2 R 3 and R 3 At least one of the above R 1 and c, d, e, and f are numbers that satisfy c≧2, d≧0, e≧0, f≧0, and 2≦c+d+e+f≦1,000.) A method for producing a (meth)acryloyl group-containing organopolysiloxane, comprising the step of reacting (B-1) (meth)acrylic acid, and (B-2) a basic alkali metal salt or a solution thereof, in the presence of (C) a phase transfer catalyst selected from a quaternary ammonium salt having at least one monovalent hydrocarbon group having 4 to 20 carbon atoms, a crown ether, and a phosphonium compound, to obtain the (meth)acryloyl group-containing organopolysiloxane.
2. The R of the halogen-containing organopolysiloxane (a-2) represented by the average composition formula (2) 1 2. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein the number of silicon atoms to which are bonded is 1 to 100% based on the total number of silicon atoms.
3. A method for producing a (meth)acryloyl group-containing organopolysiloxane as set forth in claim 1, characterized in that the amount of component (B-1) is an amount such that 1 to 3 moles of component (B-1) per mole of halogen atoms in component (A), and the amount of component (B-2) is an amount such that 1 to 3 moles of alkali metal in component (B-2) per mole of halogen atoms in component (A), and further, the amount of component (C) is blended in an amount such that 0.05 to 50 parts by mass per 100 parts by mass of component (A).
4. The method for producing a (meth)acryloyl group-containing organopolysiloxane according to claim 1, wherein the basic alkali metal salt (B-2) is a potassium salt.
5. The phase transfer catalyst (C) is represented by the following formula (3): R 4 4 N + X1 -v (3) (wherein, R 4 are each independently a hydrogen atom or a linear or branched monovalent hydrocarbon group having 1 to 20 carbon atoms, provided that R 4 At least one of X is a linear or branched monovalent hydrocarbon group having 4 to 20 carbon atoms, and - 2. The method of claim 1, wherein the quaternary ammonium salt is represented by the formula:
6. The phase transfer catalyst (C) is a quaternary ammonium salt represented by the above formula (3), and the halide ion is Br - Or Cl - 6. The method for producing the (meth)acryloyl group-containing organopolysiloxane according to claim 5, wherein 7. R in the component (A) 1 2. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein each of the groups is independently an alkyl group having 1 to 7 carbon atoms and a halogen atom at the terminal.
8. In the above average composition formula (2), 1≦d≦998, R 3 At least one of the above R 1 2. The method for producing the (meth)acryloyl group-containing organopolysiloxane according to claim 1, wherein the acryloyl group is a group represented by the formula:
9. In the above average composition formula (2), 1≦d≦998, R 3 At least one of the above R 1 wherein R 1 2. The method for producing an organopolysiloxane containing a (meth)acryloyl group according to claim 1, wherein each of the groups is independently an alkyl group having 1 to 5 carbon atoms and a halogen atom at the terminal.
10. The method for producing a (meth)acryloyl group-containing organopolysiloxane according to any one of claims 1 to 9, wherein in the above step, 0.01 to 1 part by mass of a polymerization inhibitor (D) is further blended per 100 parts by mass of the combined total of components (A) and (B).
Citation Information
Patent Citations
Method for preparing gama-(acryloyloxy)-propyl trialkoxy silane monomer
CN101723965A
Propylene acyloxy methacryloxy silane and preparation method of its derivative
CN104892661A
Preparation of organosilanes
JP1977073826A
Preparation of organosilane
JP1981104890A
Production of ester-containing organosilicone compound
JP1987232439A
Cited By
Organopolysiloxane and method for producing same
WO2026063354A1
Curable organopolysiloxane composition, release coating agent, and release film
WO2026063356A1