Film-shaped sealant and circuit device

The use of a film-like sealant with specific viscosity characteristics addresses the inefficiencies of conventional sealing methods by enabling simultaneous mounting and sealing of electronic components during the reflow solder mounting process, enhancing resistance and alignment.

WO2024225084A1PCT designated stage expired Publication Date: 2024-10-31DEXERIALS CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/014893
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-04-09
Filing Date
2024-04-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional methods for surface mounting of chips using solder paste require separate sealing processes, which are inefficient and do not allow for simultaneous sealing of entire chips, especially in miniaturized and complex mounting configurations, leading to issues with corrosion, vibration resistance, and thermal shock resistance.

Method used

A film-like sealant with a melt viscosity of 25 to 70 Pa·s at 220°C, composed of a film-forming component, thermosetting monomer, and curing agent or polymerization initiator, is used to seal electronic components during the reflow solder mounting process, enabling simultaneous mounting and sealing of components of varying sizes on a substrate.

Benefits of technology

This approach allows for efficient and simultaneous sealing of entire electronic components during the reflow process, improving corrosion resistance, vibration resistance, and thermal shock resistance, while preventing solder particle washaway and ensuring proper alignment and bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024014893_31102024_PF_FP_ABST
    Figure JP2024014893_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a film-shaped sealant with which mounting of an electronic component, e.g., a chip, on a substrate can be performed simultaneously with en bloc sealing of the entire electronic component in a reflow step in a solder reflow mounting process. A film-shaped sealant 4 comprises a film-forming component, a thermosetting monomer, and a curing agent or polymerization initiator and has a melt viscosity at 220°C of 25-70 Pa·s. A circuit device 10 includes a component 2 for mounting which has been mounted on a circuit board 1 and sealed with a cured object 4A formed from the film-shaped sealant 4.
Need to check novelty before this filing date? Find Prior Art

Description

Film-like sealant and circuit device

[0001] This application claims priority from Japanese Patent Application No. 2023-71296 filed in Japan on April 25, 2023, and Japanese Patent Application No. 2024-63029 filed in Japan on April 9, 2024, both of which are incorporated herein by reference.

[0002] Conventionally, in surface mounting of chips by reflow soldering using solder paste or the like, after soldering by reflow soldering, the chip (e.g., semiconductor element) is sealed to prevent solder corrosion and to improve soldering strength, vibration resistance, and thermal shock resistance. For example, when flip-chip mounting or the like is performed, the bottom of the chip is sealed, and sometimes the entire chip including the bottom of the chip is sealed.

[0003] On the other hand, shorter mounting times are required due to demands for shorter takt time in mounting and for reasons such as chip miniaturization. Furthermore, with regard to sealing, sealing of smaller areas is required, particularly for the lower parts of chip components. For example, a method using an underfill film can be cited as a technique for simultaneously performing solder mounting and sealing the lower parts of the chip (see, for example, Patent Documents 1 and 2). Furthermore, Patent Documents 3 and 4 describe methods for sealing the entire chip, including the lower parts, after mounting.

[0004] The techniques described in Patent Documents 1 and 2 simultaneously perform solder mounting and sealing of the bottom of the chip, but do not seal the entire chip, so if the entire chip is to be sealed, a separate sealing process is required. Also, the techniques described in Patent Documents 3 and 4 can seal the entire chip, but they seal after solder mounting, so a sealing process is required in addition to the reflow process.

[0005] JP 2018-184605 A JP 2020-065063 A JP 2012-054363 A JP 2015-216229 A

[0006] The present technology has been proposed in light of the above-described conventional situation, and provides a film sealant that can simultaneously mount electronic components such as chips on a substrate and seal the entire electronic component at the same time during the reflow step of a reflow solder mounting process.

[0007] As a result of extensive research, the inventors of the present application focused on the viscosity of the film sealant at the melting point of the bonding material that bonds the substrate and the electronic component, and found that the above-mentioned problems can be solved by using a film sealant whose melt viscosity at the melting point (e.g., the liquidus temperature of the solder) of the bonding material that bonds the substrate and the electronic component is within a predetermined range.

[0008] The film sealant according to the present technology contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity at 220°C of 25 to 70 Pa·s.

[0009] The film-like sealant according to the present technology includes a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity of 25 to 70 Pa·s at 220°C. A second resin layer is laminated on the first resin layer.

[0010] The present technology relates to a film-like sealant for sealing electronic components mounted on a substrate, which contains a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity of 25 to 70 Pa·s at the melting point of the bonding material that bonds the substrate and the electronic components.

[0011] The present technology provides a film-like sealant for sealing electronic components mounted on a substrate, the film-like sealant comprising a first resin layer made of a film-like sealant containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and having a melt viscosity of 25 to 70 Pa·s at the melting point of a bonding material that bonds the substrate and the electronic components, and a second resin layer laminated on the surface of the first resin layer opposite to the surface that contacts the electronic components.

[0012] In the circuit device according to the present technology, electronic components mounted on a substrate are sealed with the cured product of the film sealant described above.

[0013] According to the present technology, it is possible to provide a film sealant that can simultaneously mount electronic components such as chips on a substrate and seal the entire electronic component at the same time in the reflow step of a reflow solder mounting process.

[0014] Furthermore, according to the present technology, when a film sealant is used in which a first resin layer and a second resin layer are laminated, even if a substrate is mounted with a plurality of components of different sizes, for example, chips (semiconductor elements) and electronic components that are smaller than chips (chip resistors, etc.), these components can be mounted and sealed all at once during reflow.

[0015] FIG. 1 is a cross-sectional view showing an example of a circuit device in which electronic components mounted on a substrate are sealed with a cured product of the film sealant according to the present disclosure. FIG. 2 is a graph showing the relationship between time and temperature, illustrating an example of reflow conditions. FIG. 3 is a cross-sectional view showing an example of a film sealant according to a second embodiment. FIG. 4 is a cross-sectional view illustrating a method of placing mounting components on a circuit board in an example of a method for manufacturing a circuit device. FIG. 5 is a cross-sectional view illustrating a method of applying a film sealant to the periphery of a mounting component in an example of a method for manufacturing a circuit device. FIG. 6 is a cross-sectional view illustrating a method of applying a film sealant to the periphery of a mounting component in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed on a circuit board. FIG. 7 is a cross-sectional view illustrating a method of performing a reflow treatment on a circuit board on which mounting components of different sizes are mounted in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed on a circuit board. FIG. 8 is a cross-sectional view illustrating a method of performing a reflow treatment on a circuit board on which mounting components of different sizes are mounted. FIG. 9 is a cross-sectional view illustrating a method for performing a reflow treatment on a circuit board on which mounting components of different sizes are mounted. FIG. 10(A) is a cross-sectional view illustrating a method for applying a film sealant having a first resin layer and a second resin layer laminated on the periphery of a plurality of mounting components of different sizes in an example of a manufacturing method for a circuit device in which mounting components of different sizes are mixed on a circuit board. FIG. 10(B) is a cross-sectional view illustrating a method for performing a reflow treatment on a circuit board on which mounting components of different sizes are mounted. FIG. 10(C) is a cross-sectional view illustrating a state in which the entire mounting components are collectively sealed at the same time as mounting the plurality of mounting components on the circuit board. FIG. 11 is a plan view illustrating an example of the configuration of a test mounting component used in sealing property evaluation (2). FIG. 12 is a cross-sectional view illustrating an example of a state in which a film sealant is placed on a test mounting component used in sealing property evaluation (2). Figure 13(A) is a plan view showing an example of a test circuit device after sealing evaluation (2) was performed using film sealant (1), and Figure 13(B) is a cross-sectional view of AA' in Figure 13(A).

[0016] <Film-like Sealant> As a first embodiment, a film-like sealant according to the present technology is a film-like sealant for sealing electronic components mounted on a substrate, and includes a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and has a melt viscosity of 25 to 70 Pa s at the melting point of the bonding material that bonds the substrate and the electronic components. By using such a film-like sealant, it is possible to simultaneously mount electronic components such as chips on a substrate and seal the entire electronic components at the same time in the reflow step of a reflow solder mounting process.

[0017] As will be described later, in a second embodiment of the film sealant according to the present technology, a second resin layer may be laminated on a first resin layer made of a film sealant that includes a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and has a melt viscosity of 25 to 70 Pa s at 220° C. For example, the second resin layer may be laminated on the surface of the first resin layer opposite to the surface that contacts the electronic component.

[0018] 1 is a cross-sectional view showing an example of a circuit device in which an electronic component mounted on a substrate is sealed with a cured film sealant according to the present technology. The circuit device 10 includes a circuit board 1 as a substrate and a mounting component 2 as an electronic component, joined together by a solder joint 3A derived from a solder paste 3. The solder joint 3A is provided between an electrode pad 1a of the circuit board 1 and an electrode bump 2a of the mounting component 2. In the circuit device 10, the periphery of the mounting component 2 is sealed with a sealing portion 4A formed by curing a film sealant 4 according to the present technology. The periphery of the mounting component 2 includes the periphery of the solder joint 3A (including the side surfaces of the solder joint 3A and the space S surrounded by the solder joints 3A, the mounting component 2, and the circuit board 1), the periphery (side surfaces) of the electrode bump 2a, and the periphery of the mounting component 2 (top surface 2b, side surface 2c, and bottom surface 2d). In this way, in the circuit device 10, the periphery of the mounting component 2 is covered with the sealing portion 4A so that there is substantially no gap between the circuit board 1 and the mounting component 2.

[0019] Generally, there are recommended reflow conditions for each bonding material. For example, there are methods that adjust the reflow conditions to match the melting point of the bonding material, and methods that do not change the reflow conditions regardless of the melting point of the bonding material. First, when adjusting the reflow conditions to match the melting point of the bonding material, if the melting point of the bonding material is too low, the reflow conditions will be lower, which may hinder the melting of the film sealant 4 and result in insufficient sealing. On the other hand, if the melting point of the bonding material is too high, the reflow conditions will be higher, which may cause the lower-viscosity film sealant 4 to wash away the bonding material (e.g., solder particles in the solder paste 3), hindering bonding or causing the solder particles to scatter. Second, if the reflow conditions are not changed regardless of the melting point of the bonding material, if the melting point of the bonding material is too low, excessive heat will be applied, which may reduce the thermal fatigue resistance of the bonding material and reduce the long-term durability of the bonded portion. On the other hand, if the melting point of the bonding material is too high, bonding tends to be difficult.

[0020] In the present technology, the temperature at which the film sealant 4 exhibits a melt viscosity of 25 to 70 Pa·s preferably coincides with the melting point of the bonding material (e.g., the solder in the solder paste 3) that bonds the circuit board 1 and the mounting components 2. When using the film sealant 4 according to the present technology, it is preferable to use a bonding material having a melting point (liquidus temperature) of, for example, about 220°C as the bonding material that bonds the circuit board 1 and the mounting components 2. As a specific example, it is preferable to use a solder paste 3 that uses a solder (e.g., SAC-305 (Ag 3.0%-Cu 0.5%-Sn (balance)) that has a liquidus temperature of 220°C. Assuming that such a bonding material is used, it is preferable to use the film sealant 4 according to the present technology that includes a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and that has a melt viscosity of 25 to 70 Pa·s at 220°C.

[0021] Hereinafter, assuming the use of a solder paste 3 using solder with a liquidus temperature of 220°C, as an example of the film-like sealant 4 according to the present technology, a film-like sealant containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and having a melt viscosity of 25 to 70 Pa s at 220°C will be described.

[0022] FIG. 2 is a graph showing the relationship between time and temperature to explain an example of reflow conditions. The area within the box marked P in FIG. 2 represents the preheat region (hereinafter referred to as the preheat region P). Solder paste 3 typically contains a solvent and flux as volatile components. The preheat region P refers to the process in which the solvent in the solder paste 3 is volatilized and the flux cleans the oxide film on the solder surface and the bonded components. The area within the box marked R in FIG. 2 represents the reflow region (hereinafter referred to as the reflow region R). The reflow region R refers to the process in which the flux removes the oxide film on the solder particle surfaces, melts the solder paste 3, and self-aligns and bonds the electrode pads 1a of the circuit board 1 and the electrode pads 2a of the mounting component 2. A in FIG. 2 represents the preheat start point (e.g., 150-180°C). B in FIG. 2 represents the preheat end point (e.g., 170-200°C). In region a in Figure 2, it is preferable to increase the temperature at a rate of 2 to 4°C / sec. The time between A and B in Figure 2 is preferably 90±30 seconds. In region b in Figure 2, it is preferable to increase the temperature at a rate of 2 to 3°C / sec. C in Figure 2 represents the peak temperature (e.g., 230 to 250°C). D in Figure 2 represents the holding time at 220°C or higher, and this holding time is preferably 30 to 60 seconds. The horizontal dashed line between 220°C and 250°C in Figure 2 represents the heat resistance temperature of general substrates and electronic components.

[0023] In the preheating region P in FIG. 2 , the solvent in the solder paste 3 begins to volatilize. Meanwhile, since the melt viscosity of the film sealant 4 at 220°C is 25 to 70 Pa·s, in the preheating region P, the film sealant 4 remains in a film form, or becomes liquid but maintains its film form. In particular, in the low-temperature region near A in the preheating region P, the film sealant 4 does not melt and remains in a film form, so most of the volatilized solvent escapes through the gaps in the film sealant 4, but it may also escape via the film sealant 4. In this way, in the preheating region P, the solvent in the solder paste 3 volatilizes, and the volatilized solvent is discharged through the gaps between the circuit board 1 and the film sealant 4, or from the inside to the outside of the film sealant 4 via the film sealant 4.

[0024] 2, the solder in the solder paste 3 begins to melt, and the circuit board 1 and the mounting component 2 are self-aligned. Also, in the reflow region R, the flux in the solder paste 3 begins to volatilize, and the volatilized flux is discharged from the inside to the outside of the liquid film sealant 4. Then, in the reflow region R, the film sealant 4 begins to melt, and the periphery of the mounting component 2 is covered with a sealing portion 4A as shown in FIG.

[0025] In this way, because the film sealant 4 has a melt viscosity of 25 to 70 Pa·s at 220°C, the melting of the solder paste 3 and the alignment of the circuit board 1 and the mounting components 2 occur first, followed by the melting of the film sealant 4, so that the alignment of the circuit board 1 and the mounting components 2 is less likely to be hindered by the film sealant 4. Therefore, by using the film sealant 4 according to the present technology, the mounting components 2 can be mounted and the entire mounting components 2 can be sealed at the same time in the reflow step of the reflow solder mounting process.

[0026] The film-shaped sealant 4 has a melt viscosity of 70 Pa s or less at 220°C, which sufficiently reduces the viscosity of the film-shaped sealant 4 and prevents the film-shaped sealant 4 from clinging to the circuit board 1 or the mounting component 2, making it difficult for the film-shaped sealant 4 to penetrate into the lower part of the mounting component 2 (space S shown in Figure 1).As a result, the periphery of the mounting component 2 can be sealed at the same time as the mounting component 2 is mounted.

[0027] Furthermore, since the film sealant 4 has a melt viscosity of 25 Pa·s or more at 220°C, it is possible to, for example, prevent the particulate solder that makes up the solder paste 3 from being washed away before the solder paste 3 melts, and to prevent a shortage of solder particles necessary for connecting the circuit board 1 and the mounting component 2. As a result, it is possible to seal the periphery of the mounting component 2 at the same time as mounting the mounting component 2.

[0028] The film sealant 4 has a melt viscosity at 220°C of 25 to 70 Pa·s, and may be 26 Pa·s or more, 31 Pa·s or more, 41 Pa·s or more, 43 Pa·s or more, 44 Pa·s or more, 56 Pa·s or more, 64 Pa·s or more, or may be 26 to 64 Pa·s. The melt viscosity of the film sealant at 220°C can be adjusted, for example, by the content of the film-forming component or the thermosetting monomer.

[0029] <Film-forming component> The film-forming component is appropriately selected so that the film-like sealing agent 4 melts and becomes liquid at around 220°C and exhibits a melt viscosity of 25 to 70 Pa·s at 220°C. The film-forming component may have a melt viscosity of 30 Pa·s or more, 40 Pa·s or more, or 45 Pa·s or more at 220°C. The film-forming component may also have a melt viscosity of 300 Pa·s or less, 200 Pa·s or less, 100 Pa·s or less, 80 Pa·s or less, or 70 Pa·s or less at 220°C. The film-forming component may have a melt viscosity of 25 to 70 Pa·s, or 30 to 50 Pa·s at 220°C.

[0030] Examples of the film-forming component include thermoplastic elastomers having a styrene-ethylene-propylene-styrene structure, thermoplastic elastomers having a styrene-ethylene-ethylene-propylene-styrene structure, thermoplastic elastomers having a styrene-ethylene-butylene-styrene structure, acrylic polymers, phenoxy resins, epoxy resins, and urethane resins. Specific examples include Kuraity LA2250 and LA4285 (methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymers, manufactured by Kuraray Co., Ltd.), Nanostrength M51 (methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymers, manufactured by Arkema Co., Ltd.), Nanostrength D51N (modified methyl methacrylate-polybutyl acrylate block copolymers, manufactured by Arkema Co., Ltd.), Septon 2000 series (elastomers having a styrene-ethylene-propylene-styrene structure), and Septon 4000 series (elastomers having a styrene-ethylene-ethylene-propylene-styrene structure, manufactured by Kuraray Co., Ltd.).

[0031] The content of the film-forming component in the film-shaped sealant 4 can be appropriately selected within a range in which the film-shaped sealant 4 exhibits a melt viscosity of 25 to 70 Pa·s at 220°C, and can be, for example, 40% by weight or more, 50% by weight or more, 60% by weight or more, 70% by weight or more, or 75% by weight or more. The content of the film-forming component in the film-shaped sealant 4 can be 90% by weight or less, 85% by weight or less, or even 80% by weight or less. The content of the film-forming component in the film-shaped sealant 4 can be, for example, in the range of 65 to 85% by weight, or can also be in the range of 70 to 80% by weight.

[0032] The film-forming component may be used alone or in combination of two or more. When two or more film-forming components are used in combination, it is preferable that the total amount thereof satisfies the above range. When two or more film-forming components are used in combination, it is preferable that a film-forming component having a melt viscosity of 30 to 50 Pa·s at 220°C is included. For example, the content of the film-forming component having a melt viscosity of 30 to 50 Pa·s at 220°C relative to the total amount of the film-forming components in the film-like sealant is preferably 50% by weight or more, may be 60% by weight or more, may be 70% by weight or more, may be 80% by weight or more, may be 90% by weight or more, may be 95% by weight or more, may be 99% by weight or more, or may be 100% by weight.

[0033] <Thermosetting Monomer> The thermosetting monomer is appropriately selected so that the film sealant 4 melts and becomes liquid at around 220°C and exhibits a melt viscosity of 25 to 70 Pa·s at 220°C. Various thermosetting monomers, such as acrylic resins and epoxy resins, can be used as the thermosetting monomer. As the thermosetting monomer, (meth)acrylate monomers are preferred because they have a significant viscosity-reducing effect even with a small amount added, and because increasing the number of functional groups increases crosslink density and improves heat resistance. Furthermore, as described above, when using a solder paste 3 containing solder with a liquidus temperature of 220°C as a joining material, if the curing temperature is too low, the viscosity of the resin increases when the solder paste 3 melts, making it more difficult for the mounting components 2 to move, which tends to make alignment between the circuit board 1 and the mounting components 2 difficult. Therefore, it is preferable to use an acrylic resin, which has a higher curing temperature than an epoxy resin.

[0034] As the (meth)acrylate monomer, it is preferable to use at least one of a bifunctional (meth)acrylate monomer and a polyfunctional (meth)acrylate monomer, because even a small amount of the (meth)acrylate monomer facilitates denser crosslinking. Specific examples of the (meth)acrylate monomer include 1,6-hexanediol diacrylate and trimethylolpropane triacrylate.

[0035] The content of the (meth)acrylate monomer in the film sealant 4 can be appropriately selected within a range in which the film sealant 4 exhibits a melt viscosity of 25 to 70 Pa·s at 220°C, and can be, for example, 1 wt% or more, 2 wt% or more, 3 wt% or more, 4 wt% or more, or 5 wt% or more. The content of the (meth)acrylate monomer in the film sealant can be, for example, 10 wt% or less, 8 wt% or less, 7 wt% or less, or 6 wt% or less. The content of the (meth)acrylate monomer in the film sealant can be, for example, in the range of 1 to 10 wt%, or 3 to 6 wt%.

[0036] The (meth)acrylate monomer may be used alone or in combination of two or more. When two or more (meth)acrylate monomers are used in combination, it is preferable that the total amount thereof falls within the above range.

[0037] <Curing Agent or Polymerization Initiator> The film sealant 4 contains a curing agent for the thermosetting monomer or a polymerization initiator for initiating a reaction between thermosetting monomers. The curing agent or polymerization initiator can be selected appropriately depending on the type of thermosetting monomer. For example, when an acrylic resin is used as the thermosetting monomer, it is preferable to use a thermal radical polymerization initiator as the polymerization initiator. Furthermore, when an epoxy resin is used as the thermosetting monomer, it is preferable to use, for example, a phenolic resin or an acid anhydride as the curing agent. For example, an imidazole compound or a tertiary amine compound, which mainly acts as a curing catalyst, can also be used as the curing agent for the epoxy resin.

[0038] The thermal radical polymerization initiator generates radicals upon heating and initiates polymerization of the (meth)acrylate monomer. For example, in a reflow solder mounting process, it is preferable that the curing of the thermosetting monomer not begin as soon as possible while the temperature is raised from room temperature to approximately 200 to 220°C at a rate of 2 to 3°C / min, and that the curing reaction of the thermosetting monomer then begins at 250 to 260°C. In the reflow step of the reflow solder mounting process, for example, if the thermosetting monomer begins to cure in the preheat region P shown in FIG. 2, the viscosity of the molten film sealant 4 increases, making it difficult for the mounting component 2 to move, preventing self-alignment and potentially hindering the solder connection between the circuit board 1 and the mounting component 2.

[0039] Therefore, it is preferable that the thermal radical polymerization initiator have as high a reaction initiation temperature as possible, for example, a 10-hour half-life temperature of 140°C to 170°C. Examples of thermal radical polymerization initiators include peroxides having a 10-hour half-life temperature of 140°C to 170°C. Specific examples include aromatic hydroperoxides and aliphatic hydroperoxides having a 10-hour half-life temperature of 140°C to 170°C. Examples of commercial thermal radical polymerization initiators include Perbutyl H (10-hour half-life temperature: 166.5°C), Percumyl H (10-hour half-life temperature: 157.9°C), Perocta H (10-hour half-life temperature: 152.9°C), and Percumyl P (10-hour half-life temperature: 145.1°C, all manufactured by NOF Corporation).

[0040] The curing agent or polymerization initiator may be used alone or in combination of two or more. For example, when the film sealant 4 contains an acrylic resin as a thermosetting monomer, it is preferable to contain a thermal radical polymerization initiator as a polymerization initiator. A thermal radical polymerization initiator and a photopolymerization initiator may be used in combination, or a thermal radical polymerization initiator may be used alone.

[0041] The content of the curing agent or polymerization initiator in the film sealant 4 can be, for example, 0.01 wt % or more relative to the total amount of the film-forming components and thermosetting monomer in the film sealant 4. The content of the curing agent or polymerization initiator in the film sealant 4 can be, for example, 2 wt % or less relative to the total amount of the film-forming components and thermosetting monomer in the film sealant 4. For example, when the film sealant 4 contains an acrylic resin as the thermosetting monomer, the content of the polymerization initiator relative to the total amount of the film-forming components and thermosetting monomer can be in the range of 0.1 to 1 wt %. When two or more types of curing agents or polymerization initiators are used in combination, it is preferable that the total amount thereof satisfies the above range.

[0042] <Surfactant> The film sealant 4 may further contain components other than the above-described components as long as the effects of the present technology are not impaired. For example, the film sealant 4 may further contain a surfactant to more efficiently break bubbles generated by outgassing due to the solvent in the solder paste 3 during reflow, to adjust the permeability of the film sealant 4 around the mounting component 2, particularly to the area below the mounting component 2 (the space S shown in FIG. 1 ), and to further increase adhesive strength. The surfactant can be appropriately selected taking into account heat resistance, reactivity with the thermosetting monomer, degassing ability, and the like. Examples of surfactants that can be used include BYK354 and BYK322 (both manufactured by BYK Japan).

[0043] When the film sealant 4 contains a surfactant, the content of the surfactant in the film sealant 4 can be, for example, 1 wt % or more, and may be 10 wt % or more. Furthermore, the content of the surfactant in the film sealant 4 can be, for example, 30 wt % or less, and may be 20 wt % or less. The surfactant may be used alone, or two or more types may be used in combination. When two or more types of surfactants are used in combination, it is preferable that the total amount thereof satisfies the above range.

[0044] <Other Resins> The film sealant 4 may further contain a resin (hereinafter also referred to as "other resin") other than the film-forming component and the thermosetting monomer for purposes such as adjusting the viscosity of the film-forming component, adjusting the elastic modulus of the film sealant 4, or further increasing the adhesive strength of the film sealant 4. The other resin may be any material that melts and liquidizes the film sealant 4 at around 220°C and has a melt viscosity of 25 to 70 Pa·s at 220°C. There are no particular structural limitations on the other resin. For example, styrene-based or terpene phenol-based resins can be used to further increase the elastic modulus of the film sealant 4 at room temperature. An example of a product of the other resin is YS Polystar T160 (terpene phenol resin, softening point: 160°C, manufactured by Yasuhara Chemical Co., Ltd.).

[0045] When the film sealant 4 contains other resins, the content of the other resins in the film sealant 4 can be, for example, 1% by weight or more, and may be 20% by weight or more. Furthermore, the content of the other resins in the film sealant 4 can be, for example, 50% by weight or less, and may be 40% by weight or less. The other resins may be used singly or in combination of two or more. When two or more types of other resins are used in combination, it is preferable that the total amount thereof satisfies the above range.

[0046] The film sealant 4 may further contain a filler, a lubricant, an antioxidant, and the like within a range that does not impair the effects of the present technology.

[0047] The thickness of the film sealant 4 is not particularly limited and can be appropriately selected depending on the purpose, and can be, for example, in the range of 50 to 200 μm. The thickness of the film sealant 4 can also be, for example, in the range of 50 to 300 μm, or in the range of 200 to 300 μm.

[0048] In the above explanation, an example of the film sealant 4 when using a solder paste 3 that uses solder with a liquidus temperature of 220°C has been described, but the present invention is not limited to this example and various modifications can be made depending on the liquidus temperature of the solder paste 3. For example, when using a solder paste 3 that uses solder with a liquidus temperature lower than 220°C, an epoxy resin may be used as the thermosetting monomer, or a thermal radical polymerization initiator with a low reaction initiation temperature (for example, a 10-hour half-life temperature lower than 140°C to 170°C) may be used.

[0049] [Second embodiment] Fig. 3 is a cross-sectional view showing an example of a film sealant according to a second embodiment. A film sealant 20 according to the second embodiment includes a first resin layer 21 made of the film sealant according to the first embodiment described above, and a second resin layer 22 laminated thereon. As will be described in detail later, the product of the rigidity of the first resin layer 21 and a predetermined coefficient is preferably smaller than the rigidity of the second resin layer 22. By using such a film sealant 20, as will be described in detail later, on a circuit board on which relatively large components such as chips (e.g., semiconductor elements) and relatively small components such as chip resistors are mixed, the components that require sealing can be collectively sealed without the small components such as chip resistors being displaced due to a change in shape of the film sealant during reflow.

[0050] The first resin layer 21 has the same preferred ranges as the above-described film sealant 4, except for the shear modulus G' at 150° C. and the film thickness, which will be described later.

[0051] The resin constituting the second resin layer 22 can be selected from any resin, and examples thereof include epoxy resin, acrylic resin, polyimide resin, etc. When an epoxy resin or an acrylic resin is used as the resin constituting the second resin layer 22, a cured product obtained by curing a resin composition containing a monomer of each resin by irradiating it with ultraviolet light or by heat curing it can be used.

[0052] Examples of the epoxy resin include epoxy resins having a naphthalene skeleton, bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, alicyclic epoxy resins (e.g., dicyclopentadiene type epoxy resins, 3,4-epoxycyclohexylmethyl(3,4-epoxy)cyclohexanecarboxylate), siloxane type epoxy resins, biphenyl type epoxy resins, glycidyl ester type epoxy resins, and glycidyl amine type epoxy resins. These may be used alone or in combination of two or more.

[0053] Examples of acrylic resins include monofunctional (meth)acrylate monomers, polyfunctional (meth)acrylate monomers, and (meth)acrylate resins. These may be used alone or in combination. A monofunctional (meth)acrylate monomer refers to a (meth)acrylate monomer having one (meth)acryloyl group. A polyfunctional (meth)acrylate monomer refers to a (meth)acrylate monomer having two or more (meth)acryloyl groups. The (meth)acrylate resin may be a polymer or an oligomer. Specific examples of monofunctional (meth)acrylate monomers include isobornyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate. Specific examples of polyfunctional (meth)acrylate monomers include tricyclodecane dimethanol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, and trimethylolpropane tri(meth)acrylate. Specific examples of the (meth)acrylate resin include (meth)acrylates having a polyurethane skeleton and (meth)acrylates having a polyisoprene skeleton.

[0054] In addition to the epoxy resin, acrylic resin, and polyimide resin, the second resin layer 22 may further contain other components as needed, such as plasticizers and rubbers that are not directly involved in the reaction.

[0055] The first resin layer 21 and the second resin layer 22 constituting the film sealant 20 preferably satisfy the following formula 1: (shear modulus G' (Pa) of the first resin layer 21 at 150°C) x (film thickness (μm) of the first resin layer 21) x 9 < (tensile modulus E' (Pa) of the second resin layer 22 at 150°C) x (film thickness (μm) of the second resin layer 22).

[0056] The film sealant 20 satisfies Equation 1, in other words, the product of the rigidity of the first resin layer 21 and a predetermined coefficient is smaller than the rigidity of the second resin 22. Therefore, in mounting and sealing using the film sealant 20, even on a circuit board that has a mixture of relatively large components such as chips and relatively small components such as chip resistors, the tiny components such as chip resistors do not shift position due to changes in the shape of the film sealant during reflow, and the mounting components that require sealing can be sealed all at once.

[0057] The reason for focusing on the shear modulus G' of the first resin layer 21 and the tensile modulus E' of the second resin layer 22 at a specific temperature (150°C) in Equation 1 is as follows. The displacement of minute components (relatively small mounting components) mounted on a circuit board due to the flow of the film sealant during reflow is thought to be caused, for example, by a change in the modulus of elasticity of the film sealant up to the preheat region P in FIG. 2 , particularly near the preheat start point A (e.g., 150 to 180°C). Therefore, attention was focused on 150°C, which corresponds to the preheat start point. Furthermore, while the tensile modulus E' is difficult to measure when the measurement target has low elasticity (approximately 1.0E+04 Pa or less), the shear modulus G' can be measured at low elasticity but is difficult to measure at high elasticity. Therefore, the shear modulus G' of the first resin layer 21 and the tensile modulus E' of the second resin layer 22, which can be measured at 150° C., were compared.

[0058] The shear modulus G' of the first resin layer 21 at 150°C is not particularly limited as long as it satisfies Formula 1, although it depends on the thickness of the first resin layer 21 or the second resin layer 22, and can be, for example, 3.8E+03 Pa or more and 2.9E+04 Pa or less. The shear modulus G' of the first resin layer 21 at 150°C can be measured by the method described in the examples below. The film thickness of the first resin layer 21 is not particularly limited as long as it satisfies Formula 1, and can be, for example, in the range of 200 to 300 μm.

[0059] The tensile modulus E' of the second resin layer 22 at 150°C is not particularly limited as long as it satisfies Formula 1, although it depends on the thickness of the first resin layer 21 or the second resin layer 22. For example, from the viewpoint of more effectively suppressing the fluidity of the first resin layer 21 during reflow, it can be, for example, 6.0E+05 Pa or more and 4.0E+09 Pa or less. The tensile modulus E' of the second resin layer 22 can be measured by the method described in the Examples below. The film thickness of the second resin layer 22 is not particularly limited as long as it satisfies Formula 1, and can be, for example, in the range of 50 to 100 μm.

[0060] <Method for manufacturing film sealant> [First embodiment] Next, a method for manufacturing the film sealant 4 according to the present technology will be described. The method for manufacturing the film sealant 4 is not particularly limited, and the film sealant 4 can be obtained, for example, by weighing out predetermined components (e.g., the above-mentioned film-forming components, thermosetting monomer, curing agent or polymerization initiator, and organic solvent), dissolving or dispersing them by stirring, mixing, kneading, or the like to prepare a resin varnish, applying the resin varnish to a substrate film that has been subjected to a release treatment, and removing the organic solvent by heating.

[0061] The organic solvent is preferably one that has the property of being able to uniformly dissolve or disperse each component. Examples include dimethylformamide, dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, diethylene glycol dimethyl ether, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate, butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. One type of organic solvent may be used alone, or two or more types may be used in combination.

[0062] The stirring, mixing, or kneading in preparing the resin varnish can be carried out using, for example, a mixer, a kneading machine, a three-roll mill, a ball mill, a bead mill, or a homodisper, and the resin varnish can be applied to the substrate film using, for example, a knife coater, a roll coater, or an applicator.

[0063] The substrate film to which the resin varnish is applied is not particularly limited as long as it has heat resistance that can withstand the heating conditions when volatilizing the organic solvent. For example, the substrate film may be a polyolefin film such as a polypropylene film or a polymethylpentene film, a polyester film such as a polyethylene terephthalate film or a polyethylene naphthalate film, a polyimide film, or a polyetherimide film. The substrate film may be a single-layer film or a multilayer film. When the substrate film is a multilayer film, the layers may be made of different materials or the same material.

[0064] The drying conditions for volatilizing the organic solvent from the resin varnish applied to the substrate film are preferably conditions under which the organic solvent is sufficiently volatilized, and can be, for example, conditions of 50 to 200°C and 0.1 to 90 minutes.

[0065] Second Embodiment Next, a description will be given of a method for manufacturing the film sealant 20. The method for manufacturing the film sealant 20 includes, for example, a step of preparing a first resin layer 21, a step of preparing a second resin layer 22, and a step of bonding the first resin layer 21 and the second resin layer 22 together to obtain the film sealant 20.

[0066] In the step of preparing the first resin layer 21, for example, the film sealant 4 (first resin layer 21) is obtained by the same method as in the first embodiment described above.

[0067] In the step of preparing the second resin layer 22, a resin composition for the second resin layer 22 is prepared, and the prepared resin composition is applied to a substrate film that has been subjected to a release treatment, and cured with light (ultraviolet rays) to obtain the second resin layer 22. Alternatively, a commercially available resin film may be used as is as the second resin layer 22. Note that when a commercially available resin film is used as the second resin layer 22, the step of preparing the second resin layer 22 can be omitted.

[0068] The resin composition for the second resin layer 22 includes, for example, a precursor of the above-mentioned epoxy resin or acrylic resin, a photopolymerization initiator, and a plasticizer. Specific examples of resin compositions for the second resin layer 22 that mainly contain an acrylic resin include a resin composition containing a (meth)acrylate resin having a polyurethane skeleton, isobornyl (meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, and a photopolymerization initiator, and a resin composition containing a (meth)acrylate resin having a polyisoprene skeleton, isobornyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, and a photopolymerization initiator. Specific examples of resin compositions for the second resin layer 22 that mainly contain an epoxy resin include a resin composition containing a bisphenol A epoxy resin and a photoacid generator, and a resin composition containing a bisphenol A epoxy resin, an alicyclic epoxy resin, and a photoacid generator.

[0069] The resin composition can be applied to the substrate film using, for example, a bar coater. The substrate film can be any of those listed in the first embodiment.

[0070] In the step of laminating the first resin layer 21 and the second resin layer 22 to obtain the film sealant 20, for example, a laminator can be used to laminate the first resin layer 21 and the second resin layer 22. Note that the step of preparing the first resin layer 21 and the step of preparing the second resin layer 22 may be performed in either order, or may be performed in parallel.

[0071] 1 , a circuit device 10 according to the present technology includes a circuit board 1 as a substrate and a mounting component 2 as an electronic component joined together at a solder joint 3A derived from a solder paste. The mounting component 2 is surrounded by a sealing portion 4A formed by hardening a film sealant 4.

[0072] Examples of the circuit board 1 include known substrates such as semiconductor substrates, flexible circuit boards, rigid wiring boards, and printed wiring boards. Known electrode pads such as copper pads and aluminum pads can be used as the electrode pads 1a of the circuit board 1. The electrode pads 1a can also be replaced with electrodes of other types, such as electrode bumps.

[0073] Various known surface-mount components can be used as the mounting component 2, such as a semiconductor chip, a light-emitting diode, a capacitor chip, a resistor element, etc. Known electrode bumps such as gold bumps and solder bumps can be used as the electrode bumps 2a of the mounting component 2. Other types of electrodes, such as electrode pads, can also be used as the electrode bumps 2a.

[0074] The solder joints 3A are formed by reflowing the solder paste 3, and provide electrical continuity between the electrode bumps 2a of the mounting component 2 and the electrode pads 1a of the circuit board 1.

[0075] The sealing portion 4A is formed by hardening the film sealant 4. As described above, the sealing portion 4A covers the periphery of the mounting component 2, the periphery of the electrode bumps 2a, and the periphery of the solder joints 3A, and also covers part of the surface of the circuit board 1.

[0076] In addition, in the circuit device according to the present technology, the electronic components mounted on the substrate may be sealed with the cured film sealant 20 .

[0077] <Method of Manufacturing Circuit Device> [First embodiment] Next, an example of a method of manufacturing a circuit device 10 according to the present technology will be described. First, solder paste 3 is applied to the electrode pads 1a of the circuit board 1. The solder paste can be applied to the electrode pads 1a by a known method, and can be applied using, for example, a precision dispenser or a screen printing machine.

[0078] 4 is a cross-sectional view illustrating a method for placing a mounting component 2 on a circuit board 1 in one example of a method for manufacturing a circuit device 10. After applying solder paste 3 to the electrode pads 1a of the circuit board 1, the mounting component 2 is placed on the circuit board 1 as shown in FIG. Specifically, the electrode bumps 2a of the mounting component 2 are aligned with the electrode pads 1a of the circuit board 1, and may be lightly pressed as necessary. This brings the electrode bumps 2a of the mounting component 2 into contact with the solder paste 3. The height of the gap between the electrode pads 1a and the electrode bumps 2a is not particularly limited and may be, for example, approximately 10 to 100 μm, or approximately 80 μm.

[0079] FIG. 5 is a cross-sectional view illustrating a method for applying a film sealant 4 to the periphery of a mounting component 2 in an example of a manufacturing method for a circuit device 10. For example, after mounting the mounting component 2 on the circuit board 1, the film sealant 4 is placed on the mounting component 2 so as to cover the mounting component 2, as shown in FIG. 5 . As shown in FIG. 5 , the film sealant 4 placed on the mounting component 2 does not conform to the shape of the mounting component 2, and therefore, spaces exist, for example, between the film sealant 4 and the upper surface 2 b of the mounting component 2, between the film sealant 4 and the side surface 2 c, and between the film sealant 4 and the surface of the circuit board 1. Therefore, as described above, the evaporated solvent easily escapes from the inside to the outside of the film sealant 4 in the preheat region P.

[0080] Next, a reflow process is performed on the solder paste 3 sandwiched between the electrode pads 1a of the circuit board 1 and the electrode bumps 2a of the mounting component 2. In the reflow process, the solder paste 3 is heated to a temperature higher than the melting temperature of the solder particles, and the oxide film on the surface of the solder particles is removed by the flux, causing the solder paste 3 to wet and spread between the electrode pads 1a and the electrode bumps 2a, forming a solder joint 3A. The heat generated during the reflow process hardens the film sealant 4, forming a sealing portion 4A. During the reflow process of the solder paste 3, the solder paste 3 tends to remain on the surface of the electrode pads 1a without spreading beyond the periphery of the electrode pads 1a, allowing the mounting component 2 to self-align with the circuit board 1. The reflow process can be performed at normal pressure. In other words, as described above, the reflow process includes the steps of volatilizing the solvent in the solder paste 3 and expelling the volatilized solvent from the inside of the liquefied film-like sealant 4 to the outside, melting the solder in the solder paste 3 to self-align the circuit board 1 and the mounting component 2, volatilizing the flux in the solder paste 3 and expelling the volatilized flux from the inside of the liquefied film-like sealant 4 to the outside, and melting the film-like sealant 4 to seal the periphery of the mounting component 2 with the sealing portion 4A.

[0081] With this manufacturing method, in the reflow step of the reflow solder mounting process, the mount components 2 are mounted on the circuit board 1 and simultaneously the entire mount components 2 are encapsulated at the same time. As a result, a circuit device 10 is obtained in which the mount components 2 are encapsulated by the encapsulating portion 4A, as shown in Fig. 1. In this way, with the manufacturing method for the circuit device 10 according to the present technology, the reflow treatment of the solder paste 3 and the curing treatment of the film sealant 4 can be performed simultaneously.

[0082] Furthermore, in the manufacturing method for the circuit device 10 according to the present technology, in the reflow step of the solder mounting process by reflow, pressure application by a tool is not required, and the entire mounting component 2 can be sealed simultaneously with mounting the mounting component 2. Furthermore, in the manufacturing method for the circuit device 10 according to the present technology, scattering of solder balls can be suppressed and the solvent (volatile component) of the solder paste 3 can be discharged in the solder mounting process by reflow.

[0083] Second Embodiment FIG. 6 is a cross-sectional view illustrating a method for applying a film sealant to the periphery of a mounting component in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed and mounted on a circuit board.

[0084] As shown in FIG. 6 , when components of different sizes that require sealing, specifically, a relatively large mounting component 30 (hereinafter simply referred to as mounting component 30) and a relatively small mounting component 31 (hereinafter simply referred to as mounting component 31), are mixed and mounted on a circuit board 32, if the entire mounting component that requires sealing is sealed with a film sealant (e.g., film sealant 4), there is a risk that a small component (mounting component 31) measuring, for example, 1 mm square or less may be displaced due to the flow of film sealant 4 during reflow processing. In FIG. 6 , components 35 that are not to be sealed, in other words, components that are not preferably sealed with a film sealant, are components whose original function or performance may be affected if sealed. Examples of components 35 that are not to be sealed include protective elements that break their elements when heated, electrodes and light-emitting elements provided on a substrate, etc.

[0085] 7 is a cross-sectional view illustrating a method for performing a reflow process on a circuit board on which mounting components of different sizes are mounted, in an example of a manufacturing method for a circuit device in which mounting components of different sizes are mixed and mounted on the circuit board. As shown in FIG. 7 , when a reflow process is performed using a film sealant 4 on solder paste 34a sandwiched between electrode pad 32a of circuit board 33 and electrode bump 30a of mounting component 30, and solder paste 34b sandwiched between electrode pad 32b and electrode bump 31a of mounting component 31, the temperature rise during the reflow process may change the elastic modulus of film sealant 4, causing it to bend. The bent film sealant 4 may then move mounting component 31, potentially resulting in component misalignment (misalignment of mounting component 31) in the direction of the arrow in FIG. 7 . Such component misalignment is difficult to correct by self-alignment, even if solder paste 34b melts.

[0086] Such misalignment of tiny components tends to be particularly noticeable when tiny components are mounted on the edge of a circuit board, or even if not on the edge of the circuit board, when the mounting area of ​​the tiny components hits the edge of the film-type sealant, or when there are no areas on the edge of the film-type sealant where components are not mounted and the components are mounted at a very narrow pitch.

[0087] 8 and 9 are cross-sectional views illustrating a method of performing a reflow process on a circuit board on which mounting components of different sizes are mounted. As shown in Fig. 8, when there are no unmounted portions at the end of the film sealant 4 and components (mounting components 30, 31) are mounted at a narrow pitch, the temperature rise during the reflow process changes the elastic modulus of the film sealant 4, causing the film sealant 4 to bend. The bent film sealant 4 may then move the mounting component 31, potentially resulting in component misalignment (misalignment of the mounting component 31) in the direction of the arrow shown in Fig. 8.

[0088] On the other hand, as shown in Figure 9, if there are areas at the ends of the film-shaped sealant 4 where no components (mounting components 30, 31) are mounted, the elastic modulus of the film-shaped sealant 4 changes as the temperature rises during the reflow process, causing the film-shaped sealant 4 to bend.However, before the film-shaped sealant 4 comes into contact with the mounting components 30, 31, it comes into contact with the circuit board 33, and when it comes into contact with the circuit board 32, the film-shaped sealant 4 no longer moves, so no component misalignment occurs.

[0089] From the above viewpoint, when components (mounting components 30, 31) of different sizes that require sealing are mixed and mounted on the circuit board 32, it is preferable to use the film sealant 20.

[0090] FIG. 10(A) is a cross-sectional view illustrating a method for applying a film sealant having a second resin layer laminated on a first resin layer to the periphery of a plurality of mounting components of different sizes in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed and mounted on a circuit board.

[0091] First, solder paste 34a, 34b is applied to electrode pads 32a, 32b of circuit board 32, and then mounting components 30, 31 are placed on circuit board 32. Specifically, electrode bumps 30a (not shown) of mounting component 30 are aligned with electrode pads 32a of circuit board 32, and electrode bumps 31a (not shown) of mounting component 31 are also aligned with electrode pads 32a of circuit board 32, and may be lightly pressed as needed. Next, for example, after mounting components 30, 31 are placed on circuit board 32, film sealant 20 is placed on mounting components 30, 31 so as to cover mounting components 30, 31, as shown in FIG. 10(A). Film sealant 20 is placed on mounting components 30, 31 so that first resin layer 21 faces mounting components 30, 31.

[0092] Fig. 10(B) is a cross-sectional view illustrating a method for performing reflow processing on a circuit board on which mounting components of different sizes are mounted, in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed on the circuit board. Fig. 10(C) is a cross-sectional view illustrating a state in which all of the mounting components are collectively sealed at the same time as mounting a plurality of mounting components on the circuit board, in an example of a method for manufacturing a circuit device in which mounting components of different sizes are mixed on the circuit board.

[0093] A reflow process is performed on the solder pastes 34a, 34b sandwiched between the electrode pads 32a of the circuit board 32 and the electrode bumps 30a, 31a of the mounting components 30, 31. The reflow process heats the solder pastes 34a, 34b to a temperature higher than the melting temperature of the solder particles, removes oxide films on the surfaces of the solder particles with flux, and causes the solder pastes to wet and spread between the electrode pads 32a, 32b and the electrode bumps 30a, 31a, forming solder joints 34a, 34b. The heat generated during the reflow process hardens the film sealant 20, forming a sealing portion.

[0094] 10(B), during the reflow process of the solder pastes 34a and 34b, the movement of the first resin layer 21 in the film sealant 20 is suppressed by the second resin layer 22, and the curvature of the first resin layer 21 in the film sealant 20 is suppressed due to the temperature rise during the reflow process, thereby suppressing the occurrence of misalignment of the mounting components 30 and 31 (particularly the mounting component 31) due to the curvature of the first resin layer 21. Furthermore, the first resin layer 21 flows after its viscosity becomes sufficiently low, and the flowing first resin layer 21 encapsulates the entire mounting components 30 and 31. The reflow process can be performed in the same manner as in the first embodiment of the method for manufacturing a circuit device. Furthermore, during the reflow process, the solvent in the solder pastes 34a and 34b evaporates in the preheat region P shown in Figure 2, and the volatilized solvent is discharged from the inside to the outside of the film-shaped sealant 20 through the gap between the circuit board 32 and the film-shaped sealant 20, or through the film-shaped sealant 20.

[0095] This manufacturing method allows the entire mounting components 30, 31 to be encapsulated simultaneously with the mounting of the mounting components 30, 31 on the circuit board 32 during the reflow step of the reflow solder mounting process. As a result, as shown in FIG. 10C , a circuit device 33 is obtained in which the mounting components 30, 31 are encapsulated by the encapsulation portion. Thus, this manufacturing method for a circuit device allows the reflow treatment of the solder paste 34 and the curing treatment of the film sealant 20 to be performed simultaneously. Furthermore, this manufacturing method allows the components on the entire surface of the circuit board 32 to be encapsulated without misalignment of the microcomponents (mounting components 31), even in a circuit board 32 on which multiple mounting components of different sizes, such as the mounting components 30 and 31, are mounted.

[0096] Examples of the present technology will be described below. However, the present technology is not limited to these examples. The components of the film sealant used in the examples and comparative examples are as follows.

[0097] [First Resin Layer] <Film-forming Components> Kuraity LA2250: methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, viscosity at 220°C: 47 Pa·s, manufactured by Kuraray Co., Ltd. Nanostrength M51: methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, viscosity at 220°C: 46 Pa·s, manufactured by Arkema Co., Ltd. Nanostrength D51N: modified methyl methacrylate-polybutyl acrylate block copolymer, viscosity at 220°C: 33 Pa·s, manufactured by Arkema Co., Ltd. Kuraity LA4285: methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, viscosity at 220°C: 590 Pa·s, manufactured by Kuraray Co., Ltd. Septon 2002: elastomer having a styrene-ethylene-propylene-styrene structure, viscosity at 220°C: 350 Pa·s, manufactured by Kuraray Co., Ltd.

[0098] <Thermosetting Monomer> NK Ester A-TMPT: Trimethylolpropane triacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd. HDDA: 1,6-hexanediol diacrylate, manufactured by Daicel Allnex Corporation

[0099] <Thermal radical polymerization initiator> Perocta H: 1,1,3,3-tetramethylbutyl hydroperoxide, manufactured by NOF Corporation

[0100] <Other resins> YS Polystar T160: terpene phenol resin, softening point: 160°C, manufactured by Yasuhara Chemical Co., Ltd.

[0101] <Surfactants> BYK354: Polyacrylate surfactant, manufactured by BYK Japan BYK322: Silicone surfactant, manufactured by BYK Japan

[0102] [Second Resin Layer] CN9014NS: bifunctional urethane acrylate, manufactured by Arkema; ​​Acrylate IBX: isobornyl methacrylate, manufactured by Mitsubishi Chemical Corporation; NK Ester DCP: tricyclodecane dimethanol dimethacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.; UC-203M: isoprene methacrylate, manufactured by Kuraray Co., Ltd.; LBR-307: polybutadiene, manufactured by Kuraray Co., Ltd.; Arcon M-100: alicyclic saturated hydrocarbon resin, manufactured by Arakawa Chemical Industries, Ltd.; PI-184: manufactured by Aal Chem; EXA-850CRP: bisphenol A type epoxy resin, manufactured by DIC Corporation; Celloxide 2021P: 3,4-epoxycyclohexylmethyl (3,4-epoxy) cyclohexane carboxylate, manufactured by Daicel Corporation; EPICLON HP7200L: dicyclopentadiene type epoxy resin, manufactured by DIC Corporation CPI-200K: San-Apro Co., Ltd. Kapton 200H: Toray DuPont Co., Ltd. (polyimide resin film)

[0103] <Preparation of Composition for Film-Like Sealant> The components shown in Table 1 were uniformly mixed in the blending ratios (parts by weight) shown in Table 1 to prepare compositions for film-like sealants (first resin layer).

[0104] <Preparation of Composition for Second Resin Layer> A composition for a film-like sealant (second resin layer) was prepared by uniformly mixing the components shown in Table 2 in the blending ratios (parts by weight) shown in Table 2. In Example 15, a commercially available film was used as is.

[0105] <Preparation of Film-Like Sealant (1)> A resin varnish was prepared by mixing a composition for the film-like sealant (first resin layer) with an organic solvent (a mixed solvent of 80% toluene and 20% methyl ethyl ketone). This resin varnish was applied to a release-treated substrate film (polyethylene terephthalate film) using a bar coater, and heated at 100°C for 5 minutes to remove the organic solvent, thereby obtaining a primary film-like sealant with a thickness of 50 μm. Then, the resin varnish was again applied and dried on top of the primary film-like sealant to obtain a film-like sealant with a thickness of 100 μm. Hereinafter, this film-like sealant will be referred to as film-like sealant (1). Film-like sealant (1) was used in the sealing property evaluation (1) described below.

[0106] <Preparation of Film-Like Sealant (2)> A first resin layer was obtained in the same manner as in the preparation of the above-described film-like sealant (1). Furthermore, for Examples 8 to 18, except for Example 15, a resin composition for the second resin layer containing each component shown in Table 2 was applied to a release-treated film using a bar coater and cured with ultraviolet light. In Example 15, a commercially available polyimide resin film was used as is. The obtained first resin layer and second resin layer were bonded together using a laminator to obtain a film-like sealant in which the second resin layer was laminated on the first resin layer. The thickness of each layer is as shown in Table 1. Hereinafter, this film-like sealant will be referred to as film-like sealant (2). Film-like sealant (2) was used in the sealing property evaluation (2) described below. Note that in Examples 1 to 7 and Comparative Examples 1 to 4, film-like sealant (1) was also used in the sealing property evaluation (2).

[0107] <Melt Viscosity of Film-Forming Component and Film-Like Sealant> The melt viscosity of the film-forming component and the film-like sealant at 220° C. was measured using a rheometer (AR-G2 (manufactured by TA Instruments)). The results are shown in Table 1.

[0108] <Shear Modulus G′ of First Resin Layer> The shear modulus G′ of the first resin layer at 150° C. was determined using a rheometer (AR-G2 (manufactured by TA Instruments)) at a frequency of 1 Hz and a temperature rise rate of 10° C. / min. The results are shown in Table 1.

[0109] <Tensile Modulus E′ of Second Resin Layer> The tensile modulus E′ of the second resin layer at 150° C. was determined by measurement using a viscoelasticity measuring device (DMA7100, manufactured by Hitachi High-Tech Science Corporation) at a frequency of 1 Hz and a temperature rise rate of 10° C. / min. The results are shown in Table 1.

[0110] <Sealability Evaluation (1)> <Fabrication of Circuit Device> A test circuit device was fabricated using the following FR-4 grade circuit board as the test circuit board and the following semiconductor element as the test mounting component. Specifically, solder paste ("M705-GRN360-K2-V" (solder particles: Ag 3.0%-Cu 0.5%-Sn (balance)) manufactured by Senju Metal Industry Co., Ltd. was applied to the electrode pads of the test circuit board using a precision dispenser to a thickness of 150 μm. The electrode bumps of the test mounting component were aligned with the electrode pads of the test circuit board to which the solder paste had been applied, and the test mounting component was mounted on the test circuit board by lightly pressing. Next, the above-mentioned film sealant (1) was applied to the test circuit board on which the test mounting component was mounted. The test circuit board was placed on a test circuit board and heated from room temperature to 170°C at a rate of 3°C / sec under atmospheric pressure, and then held at 170°C for 90 seconds. The temperature was then raised to 250°C at 2°C / sec, and then cooled to room temperature at 2°C / sec, performing a reflow process under atmospheric pressure. This soldered the test mounting component to the test circuit board, and sealed the top, sides, and bottom of the test mounting component. As a result, a circuit device 10 sealed with a cured product 4A of the film sealant 4 was obtained, as shown in Figure 1. A UNI-5016A (manufactured by Antom Co., Ltd.) was used as the reflow oven.

[0111] The test circuit board used was an FR-4 grade circuit board (20 × 40 × 0.6 (mm)) with gold-plated copper wiring (1.0 × 7.2 (mm)) on its surface. The test mounting component used was a semiconductor element (5 × 9.5 × 1 (mm)) with electrode bumps (1.0 × 7.2 (mm)). The film sealant was cut to a size of 22 mm × 42 mm.

[0112] The film sealant was used to evaluate whether the periphery (outer periphery and lower part) of the semiconductor element, which was a test mounting component, was sealed. The appearance of the upper and side parts of the semiconductor element was observed with a microscope and visually evaluated. For the lower part of the semiconductor element, the sealed semiconductor element was polished from the top until the internal solder paste part was revealed, and then observed with a microscope. Those in which the periphery of the semiconductor element was sealed were evaluated as ○ (OK), and those in which there was an unsealed part around the semiconductor element were evaluated as × (NG). The results are shown in Table 1.

[0113]

[0114]

[0115] <Sealability Evaluation (2)> Fig. 11 is a plan view showing an example of the configuration of the test mounting component and test circuit board used in sealability evaluation (2). Fig. 12 is a cross-sectional view showing an example of the state in which a film sealant was placed on the test mounting component used in sealability evaluation (2). An FR-4 grade circuit board (5 mm x 20 mm x 0.6 mm) having gold-plated copper wiring 41a and 41b on its surface was used as the test circuit board 41. The component mounting portion on the test circuit board 41 has 2 mm x 1 mm copper wiring (semiconductor element 43 mounting portion) and 0.1 mm x 0.2 mm copper wiring (chip component 42 mounting portion). The test components were a semiconductor element 43 (4 mm × 4 mm × 1 mm) with electrode bumps (2 mm × 1 mm), and a chip resistor 42 measuring 0402 (0.4 mm × 0.2 mm × 0.2 mm) was placed at the end of the substrate 41 as shown in FIG. 11 . The distance from the end of the test circuit substrate 41 to the chip resistor 42 on the end side of the test circuit substrate 41 was 1 mm, the distance between the chip resistors 42 was 0.5 mm, and the distance from the chip resistor 42 on the semiconductor element 43 side to the end of the semiconductor element 43 was 6.1 mm. The method of mounting the test components on the test circuit substrate 41 was the same as in the sealing evaluation (1). The solder paste and its application method were also the same as in the sealing evaluation (1).

[0116] 12, the film sealant was placed on a test circuit board 41 on which a test mounting component was placed. Then, under the same reflow conditions as in sealing evaluation (1), the test mounting component and the test circuit board 41 were soldered together, and the top, sides, and bottom of the test mounting component were sealed. The film sealant was cut into a size of 7 mm x 22 mm.

[0117] The film sealant was then evaluated in the same manner as in sealing evaluation (1) to determine whether the periphery of the test mounting component, i.e., the periphery and bottom of the chip resistor 42 and the semiconductor element 43, were sealed. Specifically, a case in which the periphery of the test mounting component was sealed was evaluated as ○ (OK). A case in which the film sealant spread onto the test circuit board 41 and around the test mounting component but misalignment of the test mounting component (particularly the chip resistor 42) occurred was evaluated as △ (NG). A case in which the film sealant did not spread and there were unsealed areas on the test circuit board 41 or around the test mounting component was evaluated as × (NG). The results are shown in Table 1.

[0118] 13(A) is a plan view showing an example of a test circuit device after performing a sealing property evaluation (2) using a film sealant (1), and FIG. 13(B) is a cross-sectional view of A-A' in FIG. 13(A). For example, when performing a sealing property evaluation (2) using a film sealant (film sealant (1)) that does not have a second resin layer, as shown in FIG. 8, the temperature rise during the reflow treatment changes the elastic modulus of the film sealant 4, causing the film sealant 4 to bend, and the bent film sealant 4 causes a shift in the chip resistor 42. Then, as shown in FIGS. 13(A) and (B), the film sealant 4 spreads over the test circuit board 41 and around the test mounting components, causing a shift in the chip resistor 42. Thus, a sealability evaluation (2) of △ (NG) refers to, for example, a state in which chip resistor 42 is misaligned, chip resistor 42 is not connected to test circuit board 41, and the hardened film sealant (sealing portion 4B) covers the periphery of the test mounting component. In this case, although test circuit board 41 and semiconductor element 43 are joined by solder joint 44A derived from solder paste 44a, chip resistor 42 is misaligned from position 42P (the position of chip resistor 42 when properly connected), and test circuit board 41 and chip resistor 42 are not sufficiently joined by solder joint 44B derived from solder paste 44b, so chip resistor 42 does not function on test circuit board 41.

[0119] [Results of Sealing Property Evaluation (1)] The results of Examples 1 to 18 showed that the sealing property evaluation was good when a film sealant (1) containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator and having a melt viscosity of 25 to 70 Pa s at 220° C. was used. That is, in Examples 1 to 18, it was found that the entire electronic component could be encapsulated simultaneously with the mounting of electronic components such as chips (semiconductor elements) on a substrate during the reflow step of the reflow solder mounting process.

[0120] Furthermore, the results of Comparative Examples 1 to 4 showed that even in the case of a film-like sealant (1) containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, if the melt viscosity at 220°C does not satisfy the range of 25 to 70 Pa s, the sealability evaluation is not good. That is, in Comparative Examples 1 to 4, it was found that it is difficult to simultaneously mount electronic components such as chips on a substrate and seal the entire electronic component at the same time in the reflow step of the reflow solder mounting process.

[0121] For example, in Comparative Example 3, a film-shaped sealant (1) having a melt viscosity of 102 Pa·s at 220°C was used. Therefore, although the film-shaped sealant (1) melted during the reflow treatment, the viscosity did not decrease sufficiently, and the film-shaped sealant (1) clung to the components (the test circuit board and the test mounting components) and was difficult to penetrate into the lower parts of the test mounting components.

[0122] [Results of Sealing Property Evaluation (2)] From the results of Examples 8, 10, 12 to 15, 17, and 18, it was found that by using the film sealant (2) satisfying the above-mentioned formula 1, even if multiple components of different sizes are placed on a circuit board, they can be sealed all at once at the same time as reflow, and in addition, tiny components do not become displaced due to changes in shape of the film sealant (2) during reflow.

[0123] In Example 9, the thickness of the first resin layer in Example 8 was increased, so that Formula 1 was not satisfied, and misalignment of the chip resistor 42 occurred, but it was possible to mount the semiconductor element 43.

[0124] In Example 11, the tensile modulus E' of the second resin layer was reduced, so that the formula 1 was not satisfied, and the chip resistor 42 was displaced, but the semiconductor element 43 could be mounted.

[0125] In Example 16, the shear modulus G' of the first resin layer was increased, so that the formula 1 was not satisfied, and the chip resistor 42 was displaced, but the semiconductor element 43 could be mounted.

[0126] In Examples 1 to 7, the sealing evaluation (2) was performed using a film-like sealant (1) containing a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and having a melt viscosity of 25 to 70 Pa·s at 220°C, so that although misalignment of the chip resistor 42 occurred, it was possible to mount the semiconductor element 43. In Comparative Examples 1 to 4, the sealing evaluation (2) was performed using a film-like sealant (1) that did not satisfy the melt viscosity of 25 to 70 Pa·s at 220°C, so that the film-like sealant did not spread, and there were unsealed areas on the test circuit board 41 and around the test mounting components.

[0127] REFERENCE SIGNS LIST 1 Circuit board, 1a Electrode pad, 2 Mounting component, 2a Electrode bump, 2b Upper surface, 2c Side surface, 2d Lower surface, 3 Solder paste, 3A Solder joint portion, 4 Film sealant, 4A Sealed portion, 4B Sealed portion, 10 Circuit device, 20 Film sealant, 20A Sealed portion, 21 First resin layer, 22 Second resin layer, 30 Relatively large mounting component, 30a Electrode bump, 31 Relatively small mounting component, 31a Electrode bump, 32 Circuit board, 32a Electrode pad, 32b Electrode pad, 33 Circuit device, 34a Solder paste, 34b Solder paste, 34A Solder joint portion, 34B Solder joint portion 35 Non-sealed component, 41 Test circuit board, 41a Copper wiring, 41b Copper wiring, 42 Chip resistor, 42P Position of chip resistor when properly connected, 43 Semiconductor element, 44a Solder paste, 44b Solder paste 44A Solder joint, 44B Solder joint

Claims

1. A film-like sealant comprising a film-forming component, a thermosetting monomer, and a curing agent or a polymerization initiator, and having a melt viscosity of 25 to 70 Pa·s at 220°C.

2. The film sealant according to claim 1, wherein the thermosetting monomer is a (meth)acrylate monomer.

3. The film-like sealant according to claim 1 or 2, comprising a thermal radical polymerization initiator as the polymerization initiator, the thermal radical polymerization initiator having a 10-hour half-life temperature of 140°C to 170°C.

4. The film-like sealant according to claim 1 or 2, comprising a film-forming component having a melt viscosity of 30 to 50 Pa·s at 220° C.

5. The film-like sealant according to claim 1 or 2, wherein the film-forming component contains at least one member selected from the group consisting of methyl methacrylate-polybutyl acrylate-methyl methacrylate block copolymer, modified methyl methacrylate-polybutyl acrylate block copolymer, elastomers having a styrene-ethylene-propylene-styrene structure, and elastomers having a styrene-ethylene-ethylene-propylene-styrene structure.

6. The film-like sealant according to claim 1 or 2, wherein the thermosetting monomer is a difunctional (meth)acrylate monomer or a polyfunctional (meth)acrylate monomer.

7. The film sealant according to claim 1 or 2, further comprising a surfactant.

8. The film sealant according to claim 1 or 2, further comprising a resin other than the film-forming component and the thermosetting monomer.

9. A film sealant comprising a first resin layer made of the film sealant according to claim 1 or 2 and a second resin layer laminated on the first resin layer.

10. The film sealant according to claim 9, wherein the first resin layer and the second resin layer satisfy the following formula 1. Formula 1: (shear modulus G' (Pa) of the first resin layer at 150°C) x (film thickness (μm) of the first resin layer) x 9 < (tensile modulus E' (Pa) of the second resin layer at 150°C) x (film thickness (μm) of the second resin layer).

11. A film-like sealant for sealing an electronic component mounted on a substrate, comprising: a film-forming component; a thermosetting monomer; and a curing agent or a polymerization initiator, and the melt viscosity at the melting point of a bonding material that bonds the substrate and the electronic component is 25 to 70 Pa·s.

12. A film-like sealant comprising a first resin layer made of the film-like sealant according to claim 11, and a second resin layer laminated on the surface of the first resin layer opposite to the surface that contacts the electronic component.

13. The film sealant according to claim 12, wherein the first resin layer and the second resin layer satisfy the following formula 1. Formula 1: (shear modulus G' (Pa) of the first resin layer at 150°C) x (film thickness (μm) of the first resin layer) x 9 < (tensile modulus E' (Pa) of the second resin layer at 150°C) x (film thickness (μm) of the second resin layer).

14. The film sealant according to claim 11, wherein the bonding material is a solder paste.

15. A circuit device in which electronic components mounted on a substrate are encapsulated with a cured product of the film sealant according to claim 1 or 11.

16. A circuit device in which electronic components mounted on a substrate are encapsulated with the cured film sealant according to claim 9.

17. A circuit device in which electronic components mounted on a substrate are encapsulated with the cured film sealant according to claim 12.

18. The circuit device described in claim 15, wherein the substrate and the electronic component having electrode bumps are joined by a solder joint, and the periphery of the solder joint, the periphery of the electrode bumps, the top surface of the electronic component, the side surfaces of the electronic component, and the bottom surface of the electronic component are covered with a hardened product of the film-like sealant.

Citation Information

Patent Citations

  • Heat curing resin sheet for sealing, electronic component device, and method of manufacturing electronic component device

    JP2008177432A

  • Electronic device manufacturing method and electronic device package manufacturing method

    JP2012129326A

  • Semiconductor device manufacturing method, block laminate and successive laminate

    JP2013065835A

  • Manufacturing method of electronic component module

    JP2013153012A

  • Sealing resin sheet

    JP2016213391A