Surface protective film and optical laminate

The surface protection film with polyethylene terephthalate and specific adhesive properties addresses rainbow unevenness issues in optical inspections by maintaining optimal retardation, Nz coefficient, and slow axis variation, ensuring accurate and efficient optical assessments.

WO2024225103A1PCT designated stage expired Publication Date: 2024-10-31NITTO DENKO CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015043
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-26
Filing Date
2024-04-15
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Conventional surface protection films on optical members, such as polarizing plates, cause rainbow unevenness during optical inspections, leading to inaccurate defect detection and reduced efficiency, especially near the four corners with large polar angles affecting viewing angle characteristics.

Method used

A surface protection film with a base material of polyethylene terephthalate and an adhesive layer composed of acrylic, urethane, or silicone, having a front retardation R0 of 2000 nm or less, an Nz coefficient of 1.40 or less, and a slow axis variation of 0.6 or less, which suppresses rainbow unevenness during optical inspections.

Benefits of technology

The specified surface protection film effectively prevents rainbow unevenness near the four corners with large polar angles, ensuring accurate optical inspections and improved viewing angle characteristics by maintaining the film's properties within defined ranges for front retardation, Nz coefficient, and slow axis variation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015043_31102024_PF_FP_ABST
    Figure JP2024015043_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a surface protective film attached to an optical member and capable of suppressing rainbow mura during optical inspection through the surface protective film, particularly rainbow mura in the vicinity of four corners at a large polar angle, where viewing angle characteristics are affected. Also provided is an optical laminate including such a surface protective film. The surface protective film according to an embodiment of the present invention has a substrate and an adhesive layer, wherein the front retardation R0 is 2000 nm or less, the Nz coefficient is 1.40 or less, and the variation σ of the slow axis is 0.60 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Surface protection film and optical laminate

[0001] The present invention relates to a surface protection film and to an optical laminate including such a surface protection film.

[0002] Surface protective films are provided on the surfaces of optical devices such as displays and imaging devices, electronic devices, and film and glass materials that are components of these devices, for the purpose of surface protection, imparting impact resistance, etc. Typical surface protective films include those that are temporarily attached before use during device assembly, processing, transportation, etc., and are peeled off before use of the device (those used as processing materials), and those that remain attached to the device surface even during use of the device (those intended for permanent adhesion) (see, for example, Patent Document 1).

[0003] Both surface protection films used as processing materials and surface protection films intended for permanent adhesion have an adhesive layer on the main surface of a film substrate, and are attached to the surface of an adherend to be protected via this adhesive layer (see, for example, Patent Document 2).

[0004] Optical components including polarizing plates in liquid crystal display devices and the like are generally subjected to optical inspections such as lighting tests for the purpose of evaluating rainbow unevenness and the like. However, conventionally, when optical inspection of an optical laminate in which a surface protective film is bonded to an optical component including a polarizing plate is performed through the surface protective film, rainbow unevenness and the like may occur due to the anisotropy of the surface protective film, which may cause a decrease in the accuracy of the optical inspection. As a result, even if there is no problem with the optical component itself, the optical component may be determined to be defective in the optical inspection before shipping, which causes a problem of reduced efficiency from manufacturing to shipping of the optical component and the image display device and the like including the optical component.

[0005] Patent No. 3518677 Patent No. 6249617

[0006] An object of the present invention is to provide a surface protective film to be attached to an optical component, which can suppress rainbow unevenness during optical inspection through the surface protective film, particularly rainbow unevenness near the four corners where the polar angles are large and which affect the viewing angle characteristics, and also to provide an optical laminate including such a surface protective film.

[0007] [1] A surface protection film according to an embodiment of the present invention is a surface protection film having a substrate and a pressure-sensitive adhesive layer, and has a front retardation R0 of 2000 nm or less, an Nz coefficient of 1.40 or less, and a slow axis variation σ of 0.6 or less. [2] In the surface protection film according to the above [1], the material of the substrate is polyethylene terephthalate. [3] In the surface protection film according to the above [1] or [2], the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer may be at least one selected from the group consisting of acrylic pressure-sensitive adhesives, urethane pressure-sensitive adhesives, and silicone pressure-sensitive adhesives. [4] An optical laminate according to an embodiment of the present invention includes the surface protection film according to any one of the above [1] to [3] and an optical member. [5] In the optical laminate according to the above [4], the optical member may include a polarizing plate.

[0008] According to the present invention, it is possible to provide a surface protective film to be attached to an optical component, which can suppress rainbow unevenness during optical inspection through the surface protective film, particularly rainbow unevenness near the four corners where the polar angle is large and which affects the viewing angle characteristics. Also, it is possible to provide an optical laminate including such a surface protective film.

[0009] 1 is a schematic cross-sectional view showing an embodiment of a surface protective film of the present invention; 2 is a schematic cross-sectional view showing an embodiment of an optical laminate of the present invention; 3 is a schematic explanatory view illustrating an angle formed by a slow axis and a length direction (TD direction).

[0010] When the expression "mass" appears in this specification, it may be read as "weight", which has been conventionally and commonly used as a unit of weight, and conversely, when the expression "weight" appears in this specification, it may be read as "mass", which has been conventionally used as an SI unit of weight.

[0011] In this specification, the "angle formed by the slow axis with respect to the length direction (TD direction)" refers to the angle formed in the counterclockwise direction with respect to the length direction (TD direction).

[0012] In this specification, the term "(meth)acrylic" means "acrylic and / or methacrylic", the term "(meth)acrylate" means "acrylate and / or methacrylate", the term "(meth)allyl" means "allyl and / or methallyl", and the term "(meth)acrolein" means "acrolein and / or methacrolein".

[0013] <<Surface Protection Film>> A surface protection film according to an embodiment of the present invention has a substrate and a pressure-sensitive adhesive layer. The surface protection film according to an embodiment of the present invention preferably includes a substrate and a pressure-sensitive adhesive layer.

[0014] The surface protection film according to the embodiment of the present invention may have any other appropriate layer other than the substrate and the pressure-sensitive adhesive layer, as long as the effect of the present invention is not impaired. Examples of such other layers include an easy-adhesion layer, an easy-slip layer, an antiblocking layer, an antistatic layer, an antireflection layer, and an oligomer blocking layer.

[0015] The surface protection film according to the embodiment of the present invention may be provided with a release liner on the surface of the PSA layer opposite the substrate, in order to protect the PSA layer, etc. This release liner is typically peeled off when the surface protection film according to the embodiment of the present invention is used.

[0016] The surface protection film according to the embodiment of the present invention may contain any suitable additives, such as antioxidants, UV absorbers, light stabilizers, nucleating agents, fillers, pigments, surfactants, and antistatic agents, as long as the additives do not impair the effects of the present invention.

[0017] In one embodiment of the surface protection film of the present invention, as shown in FIG. 1, a surface protection film 100 comprises a substrate 10 and a pressure-sensitive adhesive layer 20 .

[0018] The surface protective film according to an embodiment of the present invention has a front retardation R0 of 2000 nm or less, an Nz coefficient of 1.40 or less, and a slow axis variation σ of 0.60 or less. The surface protective film according to an embodiment of the present invention has a front retardation R0, an Nz coefficient, and a slow axis variation σ all within the ranges specified in the present invention, thereby achieving the effect of the present invention of suppressing rainbow unevenness during optical inspection through the surface protective film, particularly rainbow unevenness near the four corners where the polar angle is large and which affects the viewing angle characteristics. In this way, suppressing rainbow unevenness near the four corners where the polar angle is large and which affects the viewing angle characteristics can improve the appearance near the four corners where the polar angle is large when viewed from directly in front. If at least one of the front retardation R0, the Nz coefficient, and the slow axis variation σ falls outside the ranges specified in the present invention, the effect of the present invention may not be achieved. In addition, the front retardation R0, Nz coefficient, and slow axis variation σ of the surface protection film according to the embodiment of the present invention are all measured after peeling off the release liner if a release liner is previously provided on the surface of the pressure-sensitive adhesive layer of the surface protection film opposite the substrate.

[0019] The present invention typically relates to a technology that, when selecting a surface protection film to be attached to an optical component, if the front retardation R0, the Nz coefficient, and the variation σ of the slow axis are measured and all fall within the ranges specified in the present invention, it is possible to suppress rainbow unevenness during optical inspection through the surface protection film, particularly rainbow unevenness near the four corners where the polar angle is large and which affects the viewing angle characteristics. Furthermore, since the front retardation R0, the Nz coefficient, and the variation σ of the slow axis can all be easily measured and calculated, this technology provides a technical means for appropriately selecting a surface protection film that has excellent inspectability during optical inspection.

[0020] Regardless of the type of substrate or adhesive layer constituting the surface protective film according to an embodiment of the present invention, the front retardation R0, the Nz coefficient, and the slow axis variation σ are all within the ranges specified in the present invention, thereby achieving the effect of the present invention of suppressing rainbow unevenness during optical inspection through the surface protective film, particularly rainbow unevenness near the four corners where the polar angle is large and affects the viewing angle characteristics. As such, any type of substrate or adhesive layer constituting the surface protective film according to an embodiment of the present invention can be selected. However, it is preferable to use, for example, the substrate or adhesive layer described below, in that the front retardation R0, the Nz coefficient, and the slow axis variation σ are all likely to fall within the ranges specified in the present invention. When the front retardation R0, the Nz coefficient, and the slow axis variation σ are measured for a surface protective film constructed using the substrate or adhesive layer described below, all of them are likely to fall within the ranges specified in the present invention, making it easier to appropriately select a surface protective film with excellent inspectability during optical inspection.

[0021] The surface protective film according to an embodiment of the present invention has a front retardation R0 of 2000 nm or less. From the viewpoint of further exhibiting the effects of the present invention, the front retardation R0 is preferably 0 nm to 1975 nm, more preferably 10 nm to 1950 nm, even more preferably 100 nm to 1925 nm, particularly preferably 500 nm to 1900 nm, and most preferably 650 nm to 1850 nm. In an embodiment of the present invention, by setting the front retardation R0 within the above range, and by adjusting the Nz coefficient and the variation σ of the slow axis, the effect of the present invention can be exhibited, that is, rainbow unevenness during optical inspection through the surface protective film can be suppressed, particularly in the vicinity of the four corners where the polar angle is large and which affects the viewing angle characteristics. A method for calculating the front retardation R0 will be described later.

[0022] The surface protective film according to an embodiment of the present invention has an Nz coefficient of 1.40 or less. From the viewpoint of further enhancing the effects of the present invention, the Nz coefficient is preferably 0.10 to 1.38, more preferably 0.50 to 1.36, even more preferably 0.70 to 1.35, and particularly preferably 0.90 to 1.34. The Nz coefficient is an index of the ratio of in-plane birefringence to thickness birefringence, and theoretically, viewing angle dependence is considered to be small near 0.50. However, in an embodiment of the present invention, by setting the Nz coefficient within the above range, and by adjusting the front retardation R0 and the variation σ of the slow axis, the effect of the present invention can be achieved, namely, suppressing rainbow unevenness during optical inspection through the surface protective film, particularly rainbow unevenness near the four corners where the polar angle is large and which affects the viewing angle characteristics. A method for calculating the Nz coefficient will be described later.

[0023] The surface protective film according to an embodiment of the present invention has a slow axis variation σ of 0.60 or less. The slow axis variation σ is the standard deviation of the angle between the slow axes at 12 in-plane points and the longitudinal direction (MD direction). In an embodiment of the present invention, by setting the slow axis variation σ within the above range, and by adjusting the front retardation R0 and the Nz coefficient, the effect of the present invention can be achieved, in that rainbow unevenness during optical inspection through the surface protective film can be suppressed, particularly in the vicinity of the four corners where the polar angle is large and which affects the viewing angle characteristics. A method for calculating the slow axis variation σ will be described later.

[0024] <<Substrate>> The substrate may be a substrate made of a single layer, or may be a substrate made of a laminated structure of two or more layers.

[0025] The thickness of the substrate may be any appropriate thickness as long as it does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the thickness of the substrate is preferably 5 μm to 1000 μm, more preferably 10 μm to 800 μm, even more preferably 20 μm to 600 μm, and particularly preferably 30 μm to 400 μm.

[0026] In order to further exhibit the effects of the present invention, the front retardation R0 of the substrate is preferably 2000 nm or less, more preferably 0 nm to 1975 nm, even more preferably 100 nm to 1950 nm, still more preferably 300 nm to 1925 nm, particularly preferably 500 nm to 1900 nm, and most preferably 650 nm to 1850 nm.

[0027] In order to further exhibit the effects of the present invention, the substrate has an elastic modulus in the TD direction E TD and the elastic modulus in the MD direction E MD is preferably 2.0 GPa or more, more preferably 2.5 GPa or more, even more preferably 3.0 GPa or more, particularly preferably 3.5 GPa or more, and most preferably 4.0 GPa or more. TD and the elastic modulus in the MD direction E MD The higher the modulus of elasticity E in the TD direction of the substrate, the more improved the heat resistance and mechanical properties are, and the more suppressed the shrinkage caused by heating during processing, resulting in excellent quality and appearance. TD and the elastic modulus in the MD direction E MD The higher the upper limit of the stress, the better, but in reality it is, for example, 10 GPa or less.

[0028] In order to further exhibit the effects of the present invention, the substrate has an elastic modulus in the TD direction E TD and the elastic modulus in the MD direction E MD The absolute value of the difference between TD -E MD |) is preferably 2.0 GPa or more, more preferably 2.5 GPa or more, and even more preferably 3.0 GPa or more. This is because the elastic modulus E TD and the elastic modulus in the MD direction E MD The absolute value of the difference between TD -E MD If |) is within the above range, the crystals can be aligned in the TD direction or MD direction, the mechanical properties can be improved, and the uniformity of the slow axis of the obtained surface protection film can be improved, so that rainbow unevenness during optical inspection can be suppressed. TD and the elastic modulus in the MD direction E MD The absolute value of the difference betweenTD -E MD The higher the upper limit of |), the better, but in reality, it is, for example, 9 GPa or less. TD and the elastic modulus in the MD direction E MD The measurement method will be described later.

[0029] Any appropriate material may be used as the substrate material as long as it does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, plastic is a preferred example of such a material.

[0030] Any appropriate plastic may be used as the plastic as long as it does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, a thermoplastic resin is preferably used as such a plastic.

[0031] Examples of thermoplastic resins include polyester, acrylic resin, urethane resin, polycarbonate, triacetyl cellulose (TAC), polyolefin (olefin homopolymer, copolymer of olefin and other monomer), polyamide (nylon), wholly aromatic polyamide (aramid), polyimide (PI), polyvinyl chloride (PVC), polyvinyl acetate, and cyclic olefin polymer.

[0032] The thermoplastic resin is preferably a polyester, which can more effectively exhibit the effects of the present invention. Examples of polyester include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT), and polyethylene terephthalate (PET) is preferred, which can more effectively exhibit the effects of the present invention.

[0033] Any suitable substrate may be used as the substrate as long as it does not impair the effects of the present invention, such as a stretched thermoplastic resin substrate or a crystalline PET (polyethylene terephthalate) substrate having a front retardation R0 of R0≦2000 nm.

[0034] <One Preferred Embodiment A of the Substrate> One preferred embodiment A of the substrate is a stretched thermoplastic resin substrate. Hereinafter, the thermoplastic resin substrate to be stretched may be referred to simply as a "thermoplastic resin substrate", and the stretched thermoplastic resin substrate may be referred to as a "stretched thermoplastic resin substrate".

[0035] Any appropriate thickness may be adopted as the thickness of the stretched thermoplastic resin substrate of embodiment A as long as it does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the thickness of the stretched thermoplastic resin substrate is preferably 1 μm to 100 μm, more preferably 2 μm to 80 μm, even more preferably 3 μm to 70 μm, and particularly preferably 5 μm to 60 μm.

[0036] The stretched thermoplastic resin substrate has a front retardation R0 of preferably R0≦2000 nm, more preferably R0≦1700 nm, even more preferably R0≦1400 nm, even more preferably R0≦1200 nm, still more preferably R0≦1000 nm, particularly preferably R0≦800 nm, and most preferably R0≦700 nm. When the front retardation R0 of the stretched thermoplastic resin substrate is within the above range, the effects of the present invention can be more effectively exhibited.

[0037] The lower limit of the front retardation R0 of the stretched thermoplastic resin substrate is preferably as small as possible, but in reality, it is preferably 100 nm or more depending on factors such as material selection.

[0038] The thermoplastic resin substrate preferably has a water absorption rate within a predetermined range so as to further exhibit the effects of the present invention. The water absorption rate of the thermoplastic resin substrate is preferably 0.2% or more, more preferably 0.3% or more. A thermoplastic resin substrate having such a water absorption rate can absorb water during underwater stretching, as described below, and the water acts as a plasticizer to plasticize the substrate. As a result, the stretching stress can be significantly reduced, allowing for stretching at a high magnification, and the stretchability of the thermoplastic resin substrate can be superior to that during in-air stretching, as described below. Stretching such a thermoplastic resin substrate can result in a substrate with excellent optical properties, thereby further exhibiting the effects of the present invention. On the other hand, the water absorption rate of the thermoplastic resin substrate is preferably 3.0% or less, more preferably 1.0% or less. A thermoplastic resin substrate having such a water absorption rate has excellent dimensional stability, thereby preventing problems such as deterioration in the appearance of a stretched thermoplastic resin substrate obtained by stretching such a thermoplastic resin substrate, and can also prevent the substrate from breaking during the underwater stretching process, as described below. The water absorption rate is a value determined in accordance with JIS K 7209.

[0039] The thermoplastic resin substrate preferably has a glass transition temperature (Tg) within a predetermined range in order to further exhibit the effects of the present invention. The glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 170 ° C. or less. By using such a thermoplastic resin substrate, excellent stretchability can be exhibited. Furthermore, in consideration of the plasticization of the thermoplastic resin substrate by water and the successful underwater stretching, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 120 ° C. or less. On the other hand, the glass transition temperature (Tg) of the thermoplastic resin substrate is preferably 60 ° C. or more. By using such a thermoplastic resin substrate, defects such as deformation of the thermoplastic resin substrate (for example, the occurrence of unevenness, sagging, wrinkles, etc.) can be prevented. The glass transition temperature (Tg) is a value determined in accordance with JIS K 7121.

[0040] As the material for the thermoplastic resin substrate, a material having a water absorption rate and a glass transition temperature within the above range is preferable, in order to further exhibit the effects of the present invention. The water absorption rate can be adjusted, for example, by introducing a modifying group into the material. The glass transition temperature can be adjusted, for example, by introducing a modifying group into the material or by heating using a crystallizing material.

[0041] As the material for the thermoplastic resin substrate, polyethylene terephthalate (PET)-based resin is preferred, from the viewpoint of being able to more effectively exhibit the effects of the present invention, more preferably amorphous (non-crystallized) polyethylene terephthalate (PET)-based resin, and even more preferably amorphous (hard to crystallize) polyethylene terephthalate (PET)-based resin. Specific examples of amorphous polyethylene terephthalate (PET)-based resins include copolymers further containing isophthalic acid as a dicarboxylic acid and copolymers further containing cyclohexanedimethanol as a glycol.

[0042] The thickness of the thermoplastic resin substrate (thickness before stretching) is preferably 10 μm to 500 μm, more preferably 20 μm to 400 μm, even more preferably 30 μm to 300 μm, and particularly preferably 50 μm to 200 μm, in order to further exhibit the effects of the present invention.

[0043] Stretching of a thermoplastic resin substrate is typically underwater stretching (wet stretching) using a water bath as the stretching bath. By employing underwater stretching, if the thermoplastic resin substrate has the aforementioned water absorption, the water can act as a plasticizer and plasticize the substrate. As a result, the stretching stress can be significantly reduced, enabling stretching at a high magnification, and the stretchability of the thermoplastic resin substrate can be superior to that of air-stretching, as described below. Therefore, a substrate with excellent optical properties can be obtained, thereby further demonstrating the effects of the present invention. Furthermore, underwater stretching allows the thermoplastic resin substrate to be stretched at a high magnification at a temperature lower than the glass transition temperature.

[0044] The stretching direction of the thermoplastic resin substrate is preferably the lateral direction (short side direction) of the long thermoplastic resin substrate.

[0045] Any appropriate method can be used for the underwater stretching as long as it does not impair the effects of the present invention. Examples of such stretching methods include fixed-end stretching and free-end stretching (for example, a method in which a laminate is passed between rolls with different peripheral speeds for uniaxial stretching). Stretching may be performed in one stage or multiple stages. When performing multiple stages, the stretching ratio (maximum stretching ratio) is the product of the stretching ratios in each stage.

[0046] The stretching temperature for underwater stretching (liquid temperature of the stretching bath) can be any appropriate temperature within a range that does not impair the effects of the present invention. In order to further exhibit the effects of the present invention, the temperature is preferably 30°C or higher, more preferably 40°C to 90°C, even more preferably 45°C to 85°C, and particularly preferably 50°C to 80°C. If the temperature of the stretching bath is too low, there is a risk that good stretching will not be possible, even taking into account the plasticization of the thermoplastic resin substrate by water.

[0047] The stretching time for the underwater stretching can be any appropriate time within a range that does not impair the effects of the present invention, and is preferably 15 seconds to 5 minutes in order to further exhibit the effects of the present invention.

[0048] The maximum stretching ratio in underwater stretching is preferably 5.0 times or more relative to the original length of the thermoplastic resin substrate. In this specification, the "maximum stretching ratio" refers to the stretching ratio just before the substrate breaks, and refers to a value 0.2 lower than the stretching ratio at which the substrate breaks, which is determined separately. In addition, the maximum stretching ratio can be higher when the film is stretched underwater than when it is stretched only by dry stretching.

[0049] The stretching of the thermoplastic resin substrate may be performed by combining the above-described underwater stretching with air stretching (dry stretching). Any appropriate air stretching method may be used as long as the effects of the present invention are not impaired. By combining underwater stretching with air stretching, the thermoplastic resin substrate can be stretched while suppressing its orientation. As the orientation of the thermoplastic resin substrate improves, the stretching tension increases, making stable stretching difficult or causing the thermoplastic resin substrate to break. Therefore, by stretching the thermoplastic resin substrate while suppressing its orientation, it is possible to stretch at a higher magnification. As a result, a substrate with better optical properties can be obtained, thereby further enhancing the effects of the present invention.

[0050] The method of in-air stretching may be fixed-end stretching or free-end stretching (for example, a method of uniaxially stretching a laminate by passing it between rolls with different peripheral speeds), as in the case of the underwater stretching described above. Stretching may be carried out in one stage or in multiple stages. When stretching is carried out in multiple stages, the stretching ratio is the product of the stretching ratios in each stage. The stretching direction is preferably approximately the same as the stretching direction in the underwater stretching described above.

[0051] The stretching temperature for the in-air stretching can be any appropriate temperature within a range that does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the stretching temperature for the in-air stretching is preferably 95°C to 150°C.

[0052] The stretching time for the in-air stretching can be any appropriate time within a range that does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the stretching time for the in-air stretching is preferably 15 seconds to 5 minutes.

[0053] The draw ratio for the in-air stretching can be any appropriate ratio within a range that does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the draw ratio for the in-air stretching is preferably 3.5 times or less.

[0054] The maximum stretching ratio when air-stretching and underwater stretching are combined is preferably 5.0 times or more, more preferably 5.5 times or more, and even more preferably 6.0 times or more, relative to the original length of the thermoplastic resin substrate.

[0055] As a stretched thermoplastic resin substrate as one preferred embodiment A of the substrate, for example, the stretched thermoplastic resin substrate described in JP-A-2012-73580 may be adopted.

[0056] <One Preferred Embodiment B of the Substrate> One preferred embodiment B of the substrate is a crystalline PET (polyethylene terephthalate) substrate having a front retardation R0 of R0≦2000 nm.

[0057] The thickness of the crystalline PET substrate of embodiment B may be any appropriate thickness as long as it does not impair the effects of the present invention. In terms of being able to further exhibit the effects of the present invention, the thickness of the crystalline PET substrate is preferably 10 μm to 500 μm, more preferably 15 μm to 300 μm, even more preferably 25 μm to 200 μm, particularly preferably 30 μm to 100 μm, and most preferably 30 μm to 80 μm.

[0058] The crystalline PET substrate of embodiment B has a front retardation R0 of R0≦2000 nm, preferably R0≦1975 nm, more preferably R0≦1950 nm, even more preferably R0≦1925 nm, particularly preferably R0≦1900 nm, and most preferably R0≦1850 nm. When the front retardation R0 of the crystalline PET substrate of embodiment B is within the above range, the effects of the present invention can be more effectively exhibited.

[0059] The lower limit of the front retardation R0 of the crystalline PET substrate as embodiment B is preferably 100 nm or more, more preferably 600 nm or more, even more preferably 1000 nm or more, particularly preferably 1300 nm or more, and most preferably 1500 nm or more.

[0060] The crystalline PET substrate may be a stretched substrate.

[0061] The crystalline PET substrate preferably has a ratio (TD / MD) of the tensile strength in the width direction (TD) to the tensile strength in the length direction (MD) of 1.2 to 3.3, in order to further exhibit the effects of the present invention. Note that the tensile strength is the strength (unit: MPa) measured when a test object is pulled at a speed of 200 mm / min using a tensile tester in accordance with JIS C 2151:2019, as described below, and the test object is broken (fractured).

[0062] <<Adhesive Layer>> The adhesive layer may be a single-layer adhesive layer, or may be a laminated adhesive layer having a structure of two or more layers.

[0063] The thickness of the pressure-sensitive adhesive layer is preferably 0.5 μm to 150 μm, more preferably 1 μm to 100 μm, even more preferably 2 μm to 80 μm, still more preferably 3 μm to 50 μm, particularly preferably 4 μm to 30 μm, and most preferably 5 μm to 25 μm, in order to further exhibit the effects of the present invention.

[0064] The adhesive constituting the adhesive layer is preferably at least one type selected from the group consisting of acrylic adhesives, urethane adhesives, and silicone adhesives.

[0065] The pressure-sensitive adhesive layer is more preferably made of an acrylic pressure-sensitive adhesive.

[0066] The acrylic pressure-sensitive adhesive is formed from an acrylic pressure-sensitive adhesive composition.

[0067] An acrylic pressure-sensitive adhesive can be defined as something formed from an acrylic pressure-sensitive adhesive composition in this way. This is because an acrylic pressure-sensitive adhesive becomes an acrylic pressure-sensitive adhesive when an acrylic pressure-sensitive adhesive composition undergoes a crosslinking reaction due to heating, ultraviolet irradiation, etc., and therefore it is impossible and impractical to directly identify an acrylic pressure-sensitive adhesive by its structure ("impossible / impractical circumstances"). Therefore, the definition of "something formed from an acrylic pressure-sensitive adhesive composition" appropriately identifies an acrylic pressure-sensitive adhesive as a "product."

[0068] The acrylic pressure-sensitive adhesive preferably has a peel strength from an acrylic plate at a tension speed of 300 mm / min and a peel angle of 180° under an environment of 23°C and 50% relative humidity of 0.01 N / 25 mm or more, more preferably 0.03 N / 25 mm or more, even more preferably 0.05 N / 25 mm or more, and particularly preferably 0.07 N / 25 mm or more. The preferred upper limit of the peel strength may vary depending on the application of the surface protection film of the present invention. Typically, for permanent adhesion applications (surface protection films intended for permanent adhesion), there is no upper limit, and a higher value is preferable. For re-peelable applications (e.g., surface protection films used as processing materials), the upper limit is preferably 5 N / 25 mm or less, more preferably 3 N / 25 mm or less, and even more preferably 1 N / 25 mm or less.

[0069] The pressure-sensitive adhesive layer can be formed by any appropriate method. Examples of such methods include a method in which a pressure-sensitive adhesive composition that forms the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is applied to any appropriate substrate, and if necessary, heated or dried, and if necessary, cured to form a pressure-sensitive adhesive layer on the substrate, and a method in which a pressure-sensitive adhesive composition that forms the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer is applied to any appropriate film such as a release liner, and if necessary, heated or dried, and if necessary, cured to form a pressure-sensitive adhesive layer on the film, and then any appropriate substrate is attached to the pressure-sensitive adhesive layer and transferred to form a pressure-sensitive adhesive layer on the substrate.

[0070] Any appropriate means can be used to apply the acrylic pressure-sensitive adhesive composition as long as the effects of the present invention are not impaired. Examples of such application means include roll coating, gravure roll coating, reverse roll coating, kiss roll coating, dip roll coating, bar coating, roll brush coating, spray coating, knife coating, air knife coating, comma coating, direct coating, and die coating.

[0071] The acrylic pressure-sensitive adhesive composition may be heated or dried by any appropriate means as long as the effects of the present invention are not impaired. Examples of such heating or drying means include heating to 60°C to 180°C, or performing an aging treatment at a temperature around room temperature.

[0072] The acrylic pressure-sensitive adhesive composition can be cured by any appropriate means as long as the effects of the present invention are not impaired. Examples of such curing means include heat, ultraviolet irradiation, laser irradiation, α-ray irradiation, β-ray irradiation, γ-ray irradiation, X-ray irradiation, and electron beam irradiation.

[0073] The acrylic pressure-sensitive adhesive composition preferably contains an acrylic polymer and a crosslinking agent, in that the effects of the present invention can be more effectively exhibited.

[0074] The acrylic polymer may be referred to as a base polymer in the field of acrylic pressure-sensitive adhesives. The acrylic polymer may be one type only, or two or more types may be used.

[0075] The content of the acrylic polymer in the acrylic pressure-sensitive adhesive composition is preferably 60% by weight to 99.9% by weight, more preferably 65% ​​by weight to 99.9% by weight, even more preferably 70% by weight to 99.9% by weight, particularly preferably 75% by weight to 99.9% by weight, and most preferably 80% by weight to 99.9% by weight, calculated as solid content.

[0076] As the acrylic polymer, any appropriate acrylic polymer can be used as long as it does not impair the effects of the present invention.

[0077] The weight average molecular weight of the acrylic polymer is preferably 300,000 to 2,500,000, more preferably 350,000 to 2,000,000, even more preferably 400,000 to 1,800,000, and particularly preferably 500,000 to 1,500,000, in terms of being able to further exhibit the effects of the present invention.

[0078] The acrylic polymer is preferably an acrylic polymer formed by polymerization of a composition (M) containing a (meth)acrylic acid alkyl ester (component a) in which the alkyl group in the alkyl ester moiety has 4 to 12 carbon atoms, and at least one selected from the group consisting of a (meth)acrylic acid ester and (meth)acrylic acid having an OH group (component b), in order to further enhance the effects of the present invention. Component a and component b may each independently be a single type or two or more types.

[0079] Examples of (meth)acrylic acid alkyl esters in which the alkyl group in the alkyl ester moiety has 4 to 12 carbon atoms include n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. Among these, n-butyl (meth)acrylate and 2-ethylhexyl (meth)acrylate are preferred, and n-butyl acrylate and 2-ethylhexyl acrylate are more preferred, in terms of the ability to further exhibit the effects of the present invention.

[0080] Examples of (meth)acrylic acid esters having an OH group include (meth)acrylic acid esters having an OH group such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, etc. Among these, hydroxyethyl (meth)acrylate is preferred, and hydroxyethyl acrylate is more preferred, in terms of being able to further exhibit the effects of the present invention.

[0081] As the (meth)acrylic acid, acrylic acid is preferred in that the effects of the present invention can be more effectively exhibited.

[0082] The composition (M) may contain a copolymerizable monomer other than the components a and b. The copolymerizable monomer may be of one type only, or of two or more types.Examples of such copolymerizable monomers include carboxyl group-containing monomers (excluding (meth)acrylic acid) such as itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, and acid anhydrides thereof (for example, acid anhydride group-containing monomers such as maleic anhydride and itaconic anhydride); (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N-methylol(meth)acrylamide, N-methoxymethyl(meth)acrylamide, N-butoxymethyl(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, N-methylol ... Amide group-containing monomers such as acrylamide; amino group-containing monomers such as aminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and t-butylaminoethyl (meth)acrylate; epoxy group-containing monomers such as glycidyl (meth)acrylate and methylglycidyl (meth)acrylate; cyano group-containing monomers such as acrylonitrile and methacrylonitrile; N-vinyl-2-pyrrolidone, (meth)acryloylmorpholine, N-vinylpiperidone, N-vinylpiperazine, N-vinylpyrrole, and N-vinylisopropyl heterocycle-containing vinyl monomers such as midazole, vinylpyridine, vinylpyrimidine, and vinyloxazole; sulfonic acid group-containing monomers such as sodium vinyl sulfonate; phosphate group-containing monomers such as 2-hydroxyethyl acryloyl phosphate; imide group-containing monomers such as cyclohexylmaleimide and isopropylmaleimide; isocyanate group-containing monomers such as 2-methacryloyloxyethyl isocyanate; (meth)acrylic acid esters having an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, and isobornyl (meth)acrylate; (meth)acrylic acid esters having an aromatic hydrocarbon group such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate; vinyl esters such as vinyl acetate and vinyl propionate; aromatic vinyl compounds such as styrene and vinyltoluene; olefins and dienes such as ethylene, butadiene, isoprene, and isobutylene; vinyl ethers such as vinyl alkyl ethers; and vinyl chloride.

[0083] As the copolymerizable monomer, a polyfunctional monomer may also be used. A polyfunctional monomer refers to a monomer having two or more ethylenically unsaturated groups in one molecule. As the ethylenically unsaturated group, any appropriate ethylenically unsaturated group may be used as long as it does not impair the effects of the present invention. Examples of such ethylenically unsaturated groups include radically polymerizable functional groups such as a vinyl group, a propenyl group, an isopropenyl group, a vinyl ether group (vinyloxy group), and an allyl ether group (allyloxy group). Examples of polyfunctional monomers include hexanediol di(meth)acrylate, butanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, trimethylolpropane tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, etc. Such polyfunctional monomers may be used alone or in combination of two or more.

[0084] As the copolymerizable monomer, (meth)acrylic acid alkoxyalkyl esters can also be used. Examples of (meth)acrylic acid alkoxyalkyl esters include 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, methoxytriethylene glycol (meth)acrylate, 3-methoxypropyl (meth)acrylate, 3-ethoxypropyl (meth)acrylate, 4-methoxybutyl (meth)acrylate, and 4-ethoxybutyl (meth)acrylate. The (meth)acrylic acid alkoxyalkyl esters may be used alone or in combination of two or more.

[0085] The content of the (meth)acrylic acid alkyl ester (component a) in which the alkyl group in the alkyl ester moiety has 4 to 12 carbon atoms is preferably 30% by weight or more, more preferably 35 to 99% by weight, even more preferably 40 to 98% by weight, and particularly preferably 50 to 95% by weight, relative to the total amount (100% by weight) of the monomer components constituting the acrylic polymer, in terms of being able to further exhibit the effects of the present invention.

[0086] The content of at least one member (component b) selected from the group consisting of a (meth)acrylic acid ester having an OH group and (meth)acrylic acid is preferably 1% by weight or more, more preferably 1 to 30% by weight, even more preferably 2 to 20% by weight, and particularly preferably 3 to 10% by weight, relative to the total amount (100% by weight) of the monomer components constituting the acrylic polymer, in terms of being able to further exhibit the effects of the present invention.

[0087] The composition (M) may contain any appropriate other components as long as the effects of the present invention are not impaired. Examples of such other components include a polymerization initiator, a chain transfer agent, and a solvent. The content of these other components may be any appropriate content as long as the effects of the present invention are not impaired.

[0088] The polymerization initiator may be a thermal polymerization initiator, a photopolymerization initiator (photoinitiator), or the like, depending on the type of polymerization reaction. Only one type of polymerization initiator may be used, or two or more types may be used.

[0089] A thermal polymerization initiator can be preferably used when obtaining an acrylic polymer by solution polymerization. Examples of such a thermal polymerization initiator include 2,2'-azobisisobutyronitrile (AIBN), 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid) dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propanol], 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propanol], 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propanol], 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propanol], 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propanol], 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl] ... azo initiators such as 2,2'-azobis(2-methylpropionamidine)dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate (VA-057, manufactured by Wako Pure Chemical Industries, Ltd.); persulfates such as potassium persulfate and ammonium persulfate, and di(2-ethylhexyl)peroxydicarbonate peroxide-based initiators such as di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butyl peroxydicarbonate, t-butyl peroxyneodecanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butylperoxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane, t-butyl hydroperoxide, and hydrogen peroxide; redox-based initiators combining a peroxide and a reducing agent, such as a combination of a persulfate and sodium hydrogen sulfite, or a combination of a peroxide and sodium ascorbate; substituted ethane-based initiators such as phenyl-substituted ethane; and aromatic carbonyl compounds.

[0090] The photopolymerization initiator can be preferably used when obtaining an acrylic polymer by active energy ray polymerization. Examples of the photopolymerization initiator include a benzoin ether-based photopolymerization initiator, an acetophenone-based photopolymerization initiator, an α-ketol-based photopolymerization initiator, an aromatic sulfonyl chloride-based photopolymerization initiator, a photoactive oxime-based photopolymerization initiator, a benzoin-based photopolymerization initiator, a benzyl-based photopolymerization initiator, a benzophenone-based photopolymerization initiator, a ketal-based photopolymerization initiator, and a thioxanthone-based photopolymerization initiator.

[0091] Examples of benzoin ether-based photopolymerization initiators include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether. Examples of acetophenone-based photopolymerization initiators include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-(t-butyl)dichloroacetophenone. Examples of α-ketol-based photopolymerization initiators include 2-methyl-2-hydroxypropiophenone and 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropan-1-one. Examples of aromatic sulfonyl chloride-based photopolymerization initiators include 2-naphthalenesulfonyl chloride. Examples of photoactive oxime-based photopolymerization initiators include 1-phenyl-1,1-propanedione-2-(o-ethoxycarbonyl)-oxime. Examples of benzoin-based photopolymerization initiators include benzoin. Examples of benzyl-based photopolymerization initiators include benzil. Examples of benzophenone-based photopolymerization initiators include benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexyl phenyl ketone. Examples of ketal-based photopolymerization initiators include benzil dimethyl ketal. Examples of thioxanthone-based photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.

[0092] The amount of the polymerization initiator used can be set to any appropriate amount within a range that does not impair the effects of the present invention.

[0093] The acrylic pressure-sensitive adhesive composition may contain a crosslinking agent. By using a crosslinking agent, the cohesive strength of the acrylic pressure-sensitive adhesive can be improved, and the effects of the present invention can be further exhibited. The crosslinking agent may be one type only, or two or more types.

[0094] Examples of the crosslinking agent include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a silicone-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, a silane-based crosslinking agent, an alkyl etherified melamine-based crosslinking agent, a metal chelate-based crosslinking agent, and a peroxide. In terms of being able to further exhibit the effects of the present invention, at least one crosslinking agent (component c) selected from the group consisting of an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, and a peroxide is preferred.

[0095] The isocyanate crosslinking agent can be a compound having two or more isocyanate groups (including isocyanate-regenerating polar groups in which the isocyanate group is temporarily protected by a blocking agent or oligomerization, etc.) per molecule. Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylene diisocyanate; alicyclic isocyanates such as isophorone diisocyanate; and aliphatic isocyanates such as hexamethylene diisocyanate.

[0096] Examples of the isocyanate crosslinking agent include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate; isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (e.g., manufactured by Tosoh Corporation, trade name: Coronate L), trimethylolpropane / hexamethylene diisocyanate trimer adduct (e.g., manufactured by Tosoh Corporation, trade name: Coronate HL), and isocyanurate of hexamethylene diisocyanate (e.g., manufactured by Tosoh Corporation, trade name: Coronate HX); Examples of the polyisocyanate include a trimethylolpropane adduct of rylene diisocyanate (e.g., manufactured by Mitsui Chemicals, Inc., trade name: Takenate D110N), a trimethylolpropane adduct of xylylene diisocyanate (e.g., manufactured by Mitsui Chemicals, Inc., trade name: Takenate D120N), a trimethylolpropane adduct of isophorone diisocyanate (e.g., manufactured by Mitsui Chemicals, Inc., trade name: Takenate D140N), a trimethylolpropane adduct of hexamethylene diisocyanate (e.g., manufactured by Mitsui Chemicals, Inc., trade name: Takenate D160N), and a trimethylolpropane adduct of tolylene diisocyanate (e.g., manufactured by Mitsui Chemicals, Inc., trade name: Takenate D101E); polyether polyisocyanates, polyester polyisocyanates, and adducts thereof with various polyols; and polyisocyanates multifunctionalized with isocyanurate bonds, biuret bonds, allophanate bonds, etc. Among these, aromatic isocyanates and alicyclic isocyanates are preferred because they can achieve a good balance between deformability and cohesive strength.

[0097] As the epoxy crosslinking agent, a polyfunctional epoxy compound having two or more epoxy groups in one molecule can be used. Examples of the epoxy crosslinking agent include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, 1,6-hexanediol diglycidyl ether, neopentyl glycol diglycidyl ether, ethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, and sorbitol polyglycidyl ether. Examples of epoxy crosslinking agents include glycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether, sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. Examples of commercially available epoxy crosslinking agents include those manufactured by Mitsubishi Gas Chemical Company, Inc. under the trade names "Tetrad C" and "Tetrad X."

[0098] Examples of peroxides include dibenzoyl peroxide, dicumyl peroxide, di-t-butyl peroxide, di-t-butylperoxy-3,3,5-trimethylcyclohexane, t-butyl hydroperoxide, t-butylcumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxin)hexyne-3, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, 2,5-dimethyl-2,5-mono(t-butylperoxy)hexane, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, di(2-ethylhexyl)peroxydicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxy Examples of commercially available peroxides include neodecanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, t-butylperoxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, t-butylperoxy-2-ethylhexyl carbonate, t-amylperoxyisopropyl carbonate, 3,5,5-trimethylhexanoyl peroxide, t-butylperoxy-2-hexanoate, t-butyl peroxypivalate, and t-hexyl peroxypivalate. Examples of commercially available peroxides include the "Niper BMT" series and "Niper BW" series manufactured by NOF Corporation.

[0099] The content of the crosslinking agent in the acrylic pressure-sensitive adhesive composition may be any appropriate content within a range that does not impair the effects of the present invention. For example, in order to further exhibit the effects of the present invention, the content is preferably 0.01 to 20 parts by weight, more preferably 0.01 to 18 parts by weight, even more preferably 0.01 to 15 parts by weight, and particularly preferably 0.05 to 10 parts by weight, relative to the solid content (100 parts by weight) of the acrylic polymer.

[0100] The acrylic pressure-sensitive adhesive composition may contain any other appropriate components as long as they do not impair the effects of the present invention.Such other components include, for example, polymer components other than acrylic polymers, crosslinking accelerators, crosslinking catalysts, silane coupling agents, tackifying resins (rosin derivatives, polyterpene resins, petroleum resins, oil-soluble phenols, etc.), antioxidants, inorganic fillers, organic fillers, metal powders, colorants (pigments, dyes, etc.), foil-like materials, UV absorbers, antioxidants, light stabilizers, nucleating agents, chain transfer agents, plasticizers, softeners, surfactants, antistatic agents, conductive agents, stabilizers, surface lubricants, leveling agents, corrosion inhibitors, heat stabilizers, polymerization inhibitors, lubricants, solvents, catalysts, etc.

[0101] <<Optical Laminate>> An optical laminate according to an embodiment of the present invention includes a surface protection film according to an embodiment of the present invention and an optical member.

[0102] FIG. 2 shows one embodiment of the optical laminate of the present invention. The optical laminate 1000 includes a surface protection film 100 and an optical member 200 , and the surface protection film 100 has a substrate 10 and a pressure-sensitive adhesive layer 20 .

[0103] The optical laminate according to the embodiment of the present invention may include any other appropriate layer as long as it includes a surface protective film and an optical member, as long as the effects of the present invention are not impaired.

[0104] Examples of other layers include glass, displays, imaging devices, lenses, and (half) mirrors.

[0105] The total thickness of the optical laminate according to the embodiment of the present invention may be any appropriate thickness depending on the type of optical member. Typically, the total thickness of the optical laminate according to the embodiment of the present invention is preferably 10 μm to 1000 μm, more preferably 25 μm to 800 μm, even more preferably 30 μm to 800 μm, particularly preferably 35 μm to 700 μm, and most preferably 40 μm to 500 μm.

[0106] The optical member preferably includes a polarizing plate. The optical member may include any other appropriate member as long as the effect of the present invention is not impaired.

[0107] Examples of other members include an adhesive layer and a brightness enhancement film.

[0108] The thickness of the optical member may be any appropriate thickness depending on the type of the optical member. Typically, the thickness of the optical member is preferably 10 μm to 1000 μm, more preferably 30 μm to 800 μm, even more preferably 50 μm to 700 μm, particularly preferably 100 μm to 600 μm, and most preferably 100 μm to 500 μm.

[0109] The present invention will be specifically described below using examples, but the present invention is not limited to these examples. The test and evaluation methods used in the examples are as follows. The term "parts" means "parts by weight" unless otherwise specified, and the term "%" means "% by weight" unless otherwise specified.

[0110] <Measurement of tensile strength of substrate> In accordance with JIS C 2151:2019, a substrate to be measured was pulled in the width direction (TD direction) or length direction (MD direction) at a speed of 200 mm / min using a tensile tester (manufactured by Shimadzu Corporation, product name "Autograph"), and the strength (unit: MPa) was measured when the substrate to be measured broke (fractured).

[0111] <Measurement of elastic modulus of substrate> Elastic modulus E in the TD direction of the substrate TD , elastic modulus E in the MD direction of the substrate MDwas measured as follows. The surface protection film obtained in each Example and Comparative Example was cut into a piece measuring 10 mm (MD) x 150 mm (TD) to obtain measurement sample (1), and a piece measuring 10 mm (TD) x 150 mm (MD) to obtain measurement sample (2). For the obtained measurement samples (1) and (2), the release liner was peeled from the pressure-sensitive adhesive layer, and then the measurement samples were measured at a temperature of 23°C and a relative humidity of 50% using a precision universal testing machine (Shimadzu Corporation, AUTOGRAPH AG-X plus) with a gripper distance of 100 mm and a pulling speed of 100 mm / min to obtain a TD strain ε (horizontal axis) - stress σ (vertical axis) curve for measurement sample (1), and a MD strain ε (horizontal axis) - stress σ (vertical axis) curve for measurement sample (2). The elastic modulus was calculated from the obtained TD direction strain ε (horizontal axis) - stress σ (vertical axis) curve and MD direction strain ε (horizontal axis) - stress σ (vertical axis) curve using the following formula. The elastic modulus E obtained from the TD direction strain ε (horizontal axis) - stress σ (vertical axis) curve was taken as the TD direction elastic modulus of the substrate, and the elastic modulus obtained from the MD direction strain ε (horizontal axis) - stress σ (vertical axis) curve was taken as the MD direction elastic modulus of the substrate. E = α (GL / Wt) α: slope of the curve calculated by the least squares method using all data between 15N and 25N stresses GL: grip distance (100mm) W: sample width (10mm) t: substrate thickness (mm)

[0112] <Average refractive index N ave The surface protection film obtained in each example and comparative example was cut into a size of 50 mm x 50 mm, the release liner was peeled off from the adhesive layer, and the refractive indexes of the target in the TD and MD directions were measured at a measurement wavelength of 589.3 nm (TE wave / TM wave respectively) using a refractive index film thickness measuring device (Metricon "Model 2010 Prism Coupler") in an environment of 23°C and relative humidity of 50%, and the average value of these was taken as the average refractive index N ave When calculating the Nz coefficient, measurements were taken at four points (intersections of X [mm] = 25, 325 and Y [mm] = 25, 225) at each of the four corners of the surface (350 mm x 250 mm).

[0113] <Front Retardation R0> The substrate obtained in each Production Example or the surface protection film obtained in each Example and Comparative Example was cut into a size of 350 mm × 250 mm, and for the surface protection film, the release liner was peeled off from the pressure-sensitive adhesive layer. The front retardation R0 was measured at 12 in-plane points (intersections of X [mm] = 25, 125, 225, 325, Y [mm] = 25, 125, 225) using a polarization / retardation measurement system (Axometrics, "AxoScan" software (Multi-order-retardance) used) in an environment of 23°C and relative humidity of 50% at a measurement wavelength of 590 nm, and the average value of the 12 points was calculated. When calculating the Nz coefficient, values ​​at four points (intersections of X [mm] = 25, 325 and Y [mm] = 25, 225) at each of the four corners of the surface (350 mm x 250 mm) were used.

[0114] <Variation σ of Slow Axis> The surface protection film obtained in each Example and Comparative Example was cut into a size of 350 mm × 250 mm, the release liner was peeled off from the pressure-sensitive adhesive layer, and the axial angle of the slow axis was measured at 12 in-plane points (intersections of X [mm] = 25, 125, 225, 325, Y [mm] = 25, 125, 225) using a polarization / phase difference measurement system (Axometrics' "AxoScan" software (Multi-order-retardance) used) in an environment of 23°C and relative humidity of 50% at a measurement wavelength of 590 nm, and the standard deviation σ of these 12 points was determined, and this was defined as the variation σ of the slow axis. The axial angle of the slow axis refers to the angle θ that the slow axis forms with the width direction (TD direction) in a counterclockwise direction when the width direction (TD direction) is set to 0°, as shown in FIG. 3 .

[0115] <Rθ (θ=40°)> The surface protection film obtained in each example and comparative example was cut into a size of 350 mm × 250 mm, the release liner was peeled off from the pressure-sensitive adhesive layer, and the retardation value Rθ (θ=40°) was measured at an incident angle θ of 40° (advanced axis tilt) at four points on each of the four corners of the plane (intersections of X [mm]=25, 325, Y [mm]=25, 225) at a measurement wavelength of 590 nm in an environment of 23°C and relative humidity of 50%.

[0116] <Refraction angle β> Calculated using the following formula: sin β = sin θ / N ave

[0117] <Thickness d> The surface protection film obtained in each Example and Comparative Example was cut into a size of 50 mm × 50 mm, the release liner was peeled off from the pressure-sensitive adhesive layer, and the thickness was measured using a refractive index film thickness measuring device (Metricon "Model 2010 Prism Coupler") in an environment of 23°C and relative humidity of 50%. Note that when calculating the Nz coefficient, measurements were made at four points (intersections of X [mm] = 25, 325, Y [mm] = 25, 225) at each of the four corners of the plane (350 mm × 250 mm).

[0118] <Nz coefficient> The Nz coefficient was the average value of the Nz coefficients at four points (intersections of X [mm] = 25, 325, Y [mm] = 25, 225) at each of the four corners of the surface (350 mm × 250 mm). The Nz coefficients at the four points at each of the four corners were calculated using the following formula: nx, ny, nz (nx>ny, nx is the slow axis direction, ny is the fast axis direction, nz is the thickness direction) were calculated by the following formula: ave = (nx+ny+nz) / 3 R0=(nx-ny)×d Rθ=(n eff −ny) × d (n eff is the nx component when Rθ is used.)

[0119] <Iridescent Irregularity> The release liner was peeled from the surface protective film, and the pressure-sensitive adhesive layer of the surface protective film was bonded to a polarizing plate (a) (manufactured by Nitto Denko, product name "SEG1423DU") with the absorption axis direction of the polarizing plate (a) aligned with the MD or TD direction of the substrate of the surface protective film. Next, another polarizing plate (b) (manufactured by Nitto Denko, product name "SEG1423DU") was placed on the substrate side of the surface protective film so as to be in a crossed Nicol position with the polarizing plate bonded to the surface protective film. From below the polarizing plate (b), transmitted light (constant current control power supply settings: Course 0 / Fine 8, brightness 366 cd / m) was illuminated using a large surface light (manufactured by ITEC Systems, product name "LMWG300X400NW-0053") and a UV constant current control power supply (manufactured by ITEC Systems, product name "LPDC1-24150-2R1-0073") was illuminated. 2 ) was visually observed from a height of 590 mm from the center (intersection of X [mm] = 175, Y [mm] = 125) of the crossed Nicol rainbow unevenness evaluation sample (350 mm × 250 mm), and the degree of rainbow unevenness at the four corners (polar angle of the four corners: 20°) was evaluated according to the following criteria: ◯: No rainbow unevenness was observed. Δ: Slight rainbow unevenness was observed. ×: Strong rainbow unevenness was observed.

[0120] <Evaluation of Peel Strength from Acrylic Plate> The surface protection film obtained in each Example and Comparative Example was cut into a size of 25 mm wide and 100 mm long, the release liner was peeled off from the pressure-sensitive adhesive layer, and the cut sample was roll-bonded to an acrylic plate ("Acrylite" manufactured by Mitsubishi Chemical Corporation, thickness: 2 mm, width: 70 mm, length: 100 mm) at a pressure of 0.25 MPa and a feed rate of 0.3 m / min. This sample was allowed to stand for 30 minutes in an environment of a temperature of 23°C and a relative humidity of 50%, and then a peel test was carried out in the same environment at a peel angle of 180° and a pulling rate of 300 mm / min to measure the peel strength from the acrylic plate.

[0121] [Manufacturing Example 1] <Preparation of Substrate (1)> As a thermoplastic resin substrate, an amorphous polyethylene terephthalate film (manufactured by Mitsubishi Chemical Holdings Group, product name "Novaclear", thickness 100 μm) having a water absorption rate of 0.60% and a Tg of 80°C was used. An aqueous solution of a polyvinyl alcohol (PVA) resin (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., product name "GOHSENOL (registered trademark) NH-26") having a polymerization degree of 2600 and a saponification degree of 99.9% was applied at 60°C to one side of the film and dried to form a PVA-based resin layer having a thickness of 7 μm, thereby forming a laminate. The obtained laminate was uniaxially stretched twice in the machine direction (longitudinal direction) between rolls with different peripheral speeds in an oven at 120°C, and then immersed for 30 seconds in an insolubilizing bath (a boric acid aqueous solution obtained by blending 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 30°C, and then immersed for 60 seconds in a dyeing bath (an iodine aqueous solution obtained by blending 0.2 parts by weight of iodine and 2 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 30°C. Next, the laminate was immersed in a crosslinking bath (a boric acid aqueous solution obtained by blending 3 parts by weight of potassium iodide and 3 parts by weight of boric acid per 100 parts by weight of water) at a liquid temperature of 30°C for 30 seconds. Thereafter, the laminate was immersed in a boric acid aqueous solution (a solution obtained by blending 4 parts by weight of boric acid and 5 parts by weight of potassium iodide per 100 parts by weight of water) at a liquid temperature of 60°C, while being uniaxially stretched in the longitudinal direction (machine direction) between rolls operating at different peripheral speeds. The immersion time in the boric acid aqueous solution was 120 seconds, and the laminate was stretched until just before breaking. Thereafter, the laminate was immersed in a cleaning bath (a solution obtained by blending 3 parts by weight of potassium iodide per 100 parts by weight of water) and then dried with hot air at 60°C. In this manner, an optical film laminate having a thin polarizing film formed on a thermoplastic resin substrate and stretched at a maximum ratio of 6.5 was obtained. Here, the "maximum stretching ratio" refers to the stretching ratio just before the laminate breaks. The stretching ratio at which the laminate breaks was separately determined, and a value 0.2 lower than that value was defined as the "maximum stretching ratio." Finally, the thermoplastic resin substrate was removed from the obtained optical film laminate by peeling, and used as substrate (1). The thickness of the substrate (1) used was 40 μm, and the front retardation R0 was 668 nm.

[0122] [Production Example 2] <Preparation of Substrate (2)> Two substrates (1) obtained in Production Example 1 were laminated to obtain a substrate (2) having a thickness of 80 μm and a front retardation R0 of 1321 nm.

[0123] [Manufacturing Example 3] <Preparation of Substrate (3)> A crystalline PET film (manufactured by Toray Industries, Inc., product name "XF60R", thickness = 38 μm, ratio of tensile strength in width direction (TD direction) to tensile strength in length direction (MD direction) (TD / MD) = 1.38) was cut out from a master roll to obtain a crystalline PET film having a front retardation R0 of 1640 nm. This was used as substrate (3).

[0124] [Production Example 4] <Preparation of Substrate (4)> A location different from that used in Production Example 3 was cut out from a master roll of crystalline PET film (manufactured by Toray Industries, Inc., product name "XF60R", thickness = 38 μm, ratio of tensile strength in width direction (TD direction) to tensile strength in length direction (MD direction) (TD / MD) = 1.38), to obtain a crystalline PET film having a front retardation R0 of 1780 nm. This was used as substrate (4).

[0125] [Production Example 5] <Preparation of Substrate (5)> A location different from that in Production Examples 3 and 4 was cut out from a master roll of crystalline PET film (manufactured by Toray Industries, Inc., product name "XF60R", thickness = 38 μm, ratio of tensile strength in width direction (TD direction) to tensile strength in length direction (MD direction) (TD / MD) = 1.38), to obtain a crystalline PET film having a front retardation R0 of 1821 nm. This was used as substrate (5).

[0126] [Manufacturing Example 6] <Preparation of Substrate (6)> A crystalline PET film (manufactured by Toray Industries, Inc., product name "XF60R", thickness = 38 μm, ratio of tensile strength in width direction (TD direction) to tensile strength in length direction (MD direction) (TD / MD) = 1.38) was cut out from a master roll to obtain a crystalline PET film having a front retardation R0 of 1943 nm. This was used as substrate (6).

[0127] [Production Example 7] <Preparation of Substrate (7)> ​​A polyester film (trade name "T100C38", manufactured by Mitsubishi Chemical Corporation, thickness = 38 μm) was cut out from a master roll to obtain a polyester film having a front retardation R0 of 752 nm. This was used as substrate (7).

[0128] [Production Example 8] <Preparation of Substrate (8)> A polyester film (trade name "T100C38", manufactured by Mitsubishi Chemical Corporation, thickness = 38 μm) was cut out at a different location from that in Production Example 7 to obtain a polyester film having a front retardation R0 of 1138 nm. This was used as substrate (8).

[0129] [Production Example 9] <Preparation of Substrate (9)> A polyester film (trade name "T100C38", manufactured by Mitsubishi Chemical Corporation, thickness = 38 μm) was cut out at a location different from that in Production Examples 7 and 8 to obtain a polyester film having a front retardation R0 of 1410 nm. This was used as substrate (9).

[0130] [Manufacturing Example 10] <Preparation of Substrate (10)> Two films cut from a master roll of crystalline PET film (manufactured by Toray Industries, Inc., product name "XF60R", thickness = 38 μm, ratio of tensile strength in width direction (TD direction) to tensile strength in length direction (MD direction) (TD / MD) = 1.38) were laminated to obtain a crystalline PET film having a thickness of 76 μm and a front retardation R0 of 3310 nm. This was used as substrate (10).

[0131] [Production Example 11] <Preparation of Substrate (11)> Two films cut from a master roll of polyester film (manufactured by Mitsubishi Chemical Corporation, product name "T100C38", thickness = 38 μm) were laminated to obtain a polyester film having a thickness of 76 μm and a front retardation R0 of 2888 nm. This was used as substrate (11).

[0132] [Production Example 12] <Preparation of Substrate (12)> Two films cut out from a master roll of polyester film (manufactured by Mitsubishi Chemical Corporation, product name "T100C38", thickness = 38 μm) at positions different from those used in Production Example 11 were laminated to obtain a polyester film having a thickness of 76 μm and a front retardation R0 of 3201 nm, which was used as substrate (12).

[0133] [Manufacturing Example 13] <Preparation of Substrate (13)> Three substrates (1) obtained in Manufacturing Example 1 were laminated, and one film cut from a master roll of crystalline PET film (manufactured by Toray Industries, Inc., product name "XF60R", thickness = 38 μm, ratio of tensile strength in the width direction (TD direction) to tensile strength in the length direction (MD direction) (TD / MD) = 1.38) was laminated. During lamination, since the slow axis direction of the substrate (1) is the MD direction, the substrates were laminated so that the MD direction of the substrate (1) and the TD direction of "XF60R" were aligned (strictly speaking, since the slow axis direction is offset from the MD direction and the TD direction, the slow axis direction was overlapped and laminated). As a result, a laminated film having a thickness of 158 μm and a front retardation R0 of 3853 nm was obtained. This was designated as substrate (13).

[0134] [Production Example 14] <Preparation of Coating Liquid A> Coating Liquid A was prepared by mixing 100 parts by mass of a vinyl group-containing addition silicone (manufactured by Shin-Etsu Chemical Co., Ltd., product name "KS-847T", 30% toluene solution), 3 parts by mass of a platinum catalyst (manufactured by Shin-Etsu Chemical Co., Ltd., product name "CAT-PL-50T"), 15,000 parts by mass of toluene as a dilution solvent, and 1,500 parts by mass of normal hexane.

[0135] [Production Example 15] <Preparation of Release Liner A> Coating Solution A was applied to one side of a 38 μm thick polyethylene terephthalate (PET) film (manufactured by Mitsubishi Chemical Corporation, product name "T100C38", thickness = 38 μm) using a Mayer bar, and then heated at 130°C for 1 minute in a hot air dryer to obtain Release Liner A. The coating amount of Coating Solution A was 0.1 g / m2 in terms of solid content. 2 The surface to be coated with Coating Solution A was the corona-treated surface of the PET film.

[0136] [Production Example 16] <Polymerization of Acrylic Polymer> A reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube was charged with 96.2 parts by mass of 2-ethylhexyl acrylate (2EHA) as monomer components, 3.8 parts by mass of hydroxyethyl acrylate (HEA), and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator, along with 150 parts by mass of ethyl acetate. Nitrogen gas was introduced into the mixture while gently stirring at 23°C to perform nitrogen substitution. The liquid temperature was then maintained at around 65°C, and a polymerization reaction was carried out for 6 hours to prepare an acrylic polymer solution (concentration: 40% by mass). The weight-average molecular weight of the acrylic polymer was 540,000. <Preparation of Acrylic Pressure Sensitive Adhesive> Ethyl acetate was added to the acrylic polymer solution to dilute it to a concentration of 20% by mass. To 500 parts by mass of this solution (solid content 100 parts by mass), 4 parts by mass of an isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 parts by mass (solid content 0.03 parts by mass) of dibutyltin dilaurate (1% by mass solution in ethyl acetate) as a crosslinking catalyst were added and stirred to prepare an acrylic pressure-sensitive adhesive.

[0137] [Example 1] The acrylic pressure-sensitive adhesive obtained in Production Example 16 was applied to the surface of the release liner A obtained in Production Example 15 and dried to form a 10 μm thick pressure-sensitive adhesive layer on the release liner A. The substrate (1) obtained in Production Example 1 was bonded to the obtained pressure-sensitive adhesive layer to obtain a surface protection film (1) with a release liner. Various evaluation results are shown in Table 1.

[0138] [Example 2] A surface protective film (2) with a release liner was obtained in the same manner as in Example 1, except that the substrate (2) obtained in Production Example 2 was attached instead of the substrate (1) obtained in Production Example 1. The various evaluation results are shown in Table 1.

[0139] [Example 3] A surface protective film (3) with a release liner was obtained in the same manner as in Example 1, except that the substrate (3) obtained in Production Example 3 was attached instead of the substrate (1) obtained in Production Example 1. The various evaluation results are shown in Table 1.

[0140] [Example 4] A surface protective film (4) with a release liner was obtained in the same manner as in Example 1, except that the substrate (4) obtained in Production Example 4 was attached instead of the substrate (1) obtained in Production Example 1. The various evaluation results are shown in Table 1.

[0141] [Example 5] A surface protective film (5) with a release liner was obtained in the same manner as in Example 1, except that the substrate (5) obtained in Production Example 5 was attached instead of the substrate (1) obtained in Production Example 1. The various evaluation results are shown in Table 1.

[0142] Comparative Example 1 A surface protective film (C1) with a release liner was obtained in the same manner as in Example 1, except that the substrate (7) obtained in Production Example 7 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0143] Comparative Example 2 A surface protective film (C2) with a release liner was obtained in the same manner as in Example 1, except that the substrate (8) obtained in Production Example 8 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0144] Comparative Example 3 A surface protective film (C3) with a release liner was obtained in the same manner as in Example 1, except that the substrate (9) obtained in Production Example 9 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0145] Comparative Example 4 A surface protective film (C4) with a release liner was obtained in the same manner as in Example 1, except that the substrate (6) obtained in Production Example 6 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0146] Comparative Example 5 A surface protective film (C5) with a release liner was obtained in the same manner as in Example 1, except that the substrate (10) obtained in Production Example 10 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0147] A surface protective film (C6) with a release liner was obtained in the same manner as in Example 1, except that the substrate (11) obtained in Production Example 11 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0148] Comparative Example 7 A surface protective film (C7) with a release liner was obtained in the same manner as in Example 1, except that the substrate (12) obtained in Production Example 12 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0149] Comparative Example 8 A surface protective film (C8) with a release liner was obtained in the same manner as in Example 1, except that the substrate (13) obtained in Production Example 13 was attached instead of the substrate (1) obtained in Production Example 1. The results of various evaluations are shown in Table 1.

[0150]

[0151] The surface protective film and optical laminate of the present invention can be used for any suitable application, and is preferably used in the fields of optical members and electronic members.

Claims

1. A surface protection film having a substrate and an adhesive layer, the surface protection film having a front retardation R0 of 2000 nm or less, an Nz coefficient of 1.40 or less, and a variation σ of a slow axis of 0.60 or less.

2. The surface protection film according to claim 1, wherein the material of the substrate is polyethylene terephthalate.

3. The surface protection film according to claim 1, wherein the adhesive constituting the adhesive layer is at least one type selected from the group consisting of acrylic adhesives, urethane adhesives, and silicone adhesives.

4. An optical laminate comprising the surface protective film according to any one of claims 1 to 3 and an optical member.

5. The optical laminate according to claim 4, wherein the optical member includes a polarizing plate.

Citation Information

Patent Citations

  • Film for polarizer supporting base material

    JP2011008169A

  • Method for producing optical film

    JP2019101075A

  • Surface protection film and optical laminate

    JP2023174542A

  • Surface-protective film

    WO2000044841A1

  • Laminate optical body, optical film, liquid crystal display device using said optical film, and method for manufacturing laminate optical body

    WO2010092926A1