Film adhesive agent with dicing film, electronic component using same and manufacturing method therefor

The film adhesive with a dicing film, featuring a specific elastic modulus ratio and composition, addresses chip flying issues during the dicing process by ensuring high transparency and stability, enhancing the manufacturing of electronic components like image sensors.

WO2024225161A1PCT designated stage expired Publication Date: 2024-10-31FURUKAWA ELECTRIC CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/015428
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-18
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing film adhesives used in the dicing process for electronic components, such as image sensors, suffer from chip flying issues due to reduced particulate additives for improved transparency, leading to instability during the dicing process.

Method used

A film adhesive with a dicing film is developed, where the storage elastic modulus of both the film adhesive and the dicing film at 60°C satisfy E1×E2≧7.0, incorporating an epoxy resin and phenoxy resin with a filler content of 10% or less and average particle size of 500 nm or less, and a thermal cationic polymerization initiator, ensuring high transparency and rigidity.

Benefits of technology

The solution effectively suppresses chip flying during the dicing process while maintaining high transparency and productivity, enabling the production of electronic components with improved optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015428_31102024_PF_FP_ABST
    Figure JP2024015428_31102024_PF_FP_ABST
Patent Text Reader

Abstract

This film adhesive agent with a dicing film has: a dicing film having a base and an adhesive layer; and a film adhesive agent disposed on the adhesive layer. A storage elastic modulus E1 (MPa) of the film adhesive agent at 60°C and a storage elastic modulus E2 (MPa) of the dicing film at 60°C satisfy E1 × E2 ≥ 7.0, and the light transmittance of the cured product of the film adhesive agent is 60% or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Film-like adhesive with dicing film, electronic components using the same, and manufacturing method thereof

[0001] The present invention relates to a film-like adhesive with a dicing film, an electronic component using the same, and a method for producing the same.

[0002] Imaging devices such as digital still cameras and digital video cameras incorporate image sensors (imaging elements), such as CMOS (Complementary Metal Oxide Semiconductor) image sensors and CCD (Charge Coupled Device) image sensors. Image sensors convert incident light into electrical signals via photoelectric conversion using a photodiode, which then processes the signals to form a digital image. A color filter, microlens, or the like is optionally disposed on the surface of the photodiode, and a transparent protective film, such as a glass plate, is typically disposed on the surface. Such transparent protective films are fixed via film adhesives or the like. Adhesives used to bond and fix transparent protective films to image sensors are required to be transparent enough to transmit light at least after a curing reaction. Film adhesives with various compositions are known and are widely used not only in image sensors but also in the manufacture of electronic devices and their components. For example, film adhesives are used as die attach films in the manufacturing process of semiconductor chips.

[0003] It has been proposed to use a film adhesive that exhibits sufficiently high transparency at least after a curing reaction as a laminate structure with a dicing film (a film adhesive with a dicing film) in the manufacture of electronic components. For example, Patent Document 1 describes a method for manufacturing electronic components, including a first step of obtaining a laminate in which a transparent film member, a film adhesive that exhibits sufficiently high transparency after a curing reaction, and a dicing film are laminated in this order; a second step of dicing the transparent film member and the film adhesive together to obtain a transparent film chip with an adhesive layer on the dicing film; a third step of removing the dicing film from the adhesive layer and thermocompressing the adhesive layer-attached transparent film chip to other components constituting the electronic component via the adhesive layer; and a fourth step of thermally curing the adhesive layer. Examples of the transparent film member include a glass substrate and a transparent resin. The transparent film chip with an adhesive layer obtained by dicing the transparent film member into the desired shape as described above can be incorporated into an electronic component via the cured product of the adhesive layer, for example, as a protective film for a photodiode. In addition, the above-mentioned film-like adhesive with dicing film can also be used as a dicing die attach film in the semiconductor chip manufacturing process, for dicing a semiconductor wafer and applying adhesive to the semiconductor chips that have been separated by dicing.

[0004] International Publication No. 2023 / 026584

[0005] In the above-mentioned dicing process, there is a considerable risk of chips separated by dicing peeling off from the film-like adhesive during dicing (chip flying). Through extensive research, the inventors have found that reducing the amount of particulate additives such as fillers to increase the transparency of the film-like adhesive makes chip flying more likely to occur during the dicing process. An object of the present invention is to provide a film-like adhesive with a dicing film that exhibits sufficiently high transparency at least after the curing reaction and can effectively suppress chip flying during the dicing process. Another object of the present invention is to provide a method for manufacturing electronic components using this film-like adhesive with a dicing film.

[0006] The above-mentioned problems of the present invention are solved by the following means. [1] A film-like adhesive with a dicing film, comprising a dicing film having a substrate and a pressure-sensitive adhesive layer, and a film-like adhesive disposed on the pressure-sensitive adhesive layer, wherein the storage modulus E1 (MPa) of the film-like adhesive at 60°C and the storage modulus E2 (MPa) of the dicing film at 60°C satisfy E1 × E2 ≧ 7.0, and the cured product of the film-like adhesive has a light transmittance of 60% or more. [2] The film-like adhesive with a dicing film according to [1], wherein the film-like adhesive contains an epoxy resin and a phenoxy resin. [3] The film-like adhesive with a dicing film according to [1] or [2], wherein the film-like adhesive contains a filler, and the content of the filler is 10 mass% or less of the total solid content of the film-like adhesive. [4] The film-like adhesive with a dicing film according to [3], wherein the average particle size (d50) of the filler is 500 nm or less. [5] The film-like adhesive with a dicing film according to any one of [1] to [4], wherein the film-like adhesive contains a curing agent, and the curing agent is a thermal cationic polymerization initiator. [6] The film-like adhesive with a dicing film according to any one of [1] to [5], wherein E1 is 0.1 to 1.0 MPa and E2 is 10 to 70 MPa. [7] A method for producing an electronic component, comprising: a first step of obtaining a laminate in which a transparent film-like member and the film-like adhesive with a dicing film according to any one of [1] to [6] are laminated in this order; a second step of dicing the transparent film-like member and the film-like adhesive together to obtain a transparent film-like chip with an adhesive layer on the dicing film; a third step of removing the dicing film from the adhesive layer and thermocompression-bonding the transparent film-like chip with an adhesive layer to another member constituting an electronic component via the adhesive layer; and a fourth step of thermally curing the adhesive layer. [8] The method for manufacturing an electronic component according to [7], wherein the electronic component is an image sensor. [9] The method for manufacturing an electronic component according to [8], wherein the electronic component has a structure in which the transparent film-like chip is incorporated as a protective film for a photodiode.

[0007] In the present invention, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. In the present invention, the term "... compound" means "a compound having the... skeleton." For example, "dicyandiamide compound" means not only dicyandiamide itself, but also forms in which at least a portion of the hydrogen atoms of dicyandiamide have been substituted.

[0008] The film adhesive with dicing film of the present invention exhibits sufficiently high transparency at least after the curing reaction, and can effectively suppress chip flying when applied to a dicing process. Furthermore, according to the method for producing an electronic component of the present invention, chip flying of the transparent film chip obtained in the dicing process can be effectively suppressed, and as a result, electronic components in which the transparent film chip is incorporated via a transparent cured product of the film adhesive can be obtained with high productivity.

[0009] FIG. 1 is a cross-sectional view showing a schematic structure of a film-like adhesive with a release film prepared in the examples.

[0010] [Film-like adhesive with dicing film] The film-like adhesive with dicing film of the present invention comprises a dicing film having a substrate and a pressure-sensitive adhesive layer, and a film-like adhesive disposed on the pressure-sensitive adhesive layer. Furthermore, the storage modulus E1 (MPa) of the film-like adhesive at 60°C and the storage modulus E2 (MPa) of the dicing film at 60°C satisfy E1 x E2 ≥ 7.0, and the light transmittance of the film-like adhesive after curing is 60% or more. When the storage moduli E1 and E2 satisfy the above relationship, the rigidity of the entire film-like adhesive with dicing film of the present invention is ensured even when the film-like adhesive with dicing film of the present invention is locally heated by frictional heat of the blade during dicing (it may be heated to about 60°C), and chip flying can be effectively suppressed. In addition, since the film-like adhesive exhibits high transparency after the curing reaction, it exhibits excellent optical properties as an adhesive when incorporating transparent film-like members into electronic components, etc. In order to control the combined storage modulus of the dicing film and film-like adhesive, even if a film-like adhesive layer with a relatively small storage modulus is used by reducing the amount of microparticle additive blended, it is believed that the storage modulus of the dicing film as a whole can be appropriately controlled, making it possible to suppress vibrations and the like during dicing.

[0011] In the present invention, the storage modulus E1 (MPa) of the film adhesive at 60 ° C. and the storage modulus E2 (MPa) of the dicing film at 60 ° C. are preferably E1 × E2 ≧ 10.0, more preferably E1 × E2 ≧ 11.0, even more preferably E1 × E2 ≧ 12.0, and particularly preferably E1 × E2 ≧ 15.0, from the viewpoint of suppressing chip flying. The upper limit is not particularly limited, but is usually 50.0 ≧ E1 × E2, and 40.0 ≧ E1 × E2 is practical. Therefore, 50.0 ≧ E1 × E2 ≧ 7.0 is preferred, 50.0 ≧ E1 × E2 ≧ 10.0 is more preferred, 50.0 ≧ E1 × E2 ≧ 11.0 is even more preferred, 50.0 ≧ E1 × E2 ≧ 12.0 is even more preferred, and 40.0 ≧ E1 × E2 ≧ 15.0 is particularly preferred.

[0012] The storage modulus E1 of the film-like adhesive at 60°C is not particularly limited as long as the relationship between E1 and E2 is satisfied. E1 is preferably 0.1 to 1.5 MPa, more preferably 0.1 to 1.0 MPa, even more preferably 0.2 to 1.0 MPa, even more preferably 0.3 to 0.9 MPa, and even more preferably 0.3 to 0.8 MPa. The storage modulus E2 of the dicing film at 60°C is not particularly limited as long as the relationship between E1 and E2 is satisfied. E2 is preferably 10 to 80 MPa, more preferably 10 to 70 MPa, even more preferably 20 to 70 MPa, even more preferably 25 to 60 MPa, and even more preferably 30 to 50 MPa.

[0013] The storage modulus E1 of the film-like adhesive at 60°C can be controlled by the type and content of the components (resin, curing agent, filler, etc.) constituting the film-like adhesive. The storage modulus E2 of the dicing film at 60°C can be controlled by the type and content of the components (resins constituting the adhesive layer and substrate) constituting the dicing film, the thickness of the adhesive layer and substrate, etc. Since the substrate is usually thicker than the adhesive layer, E2 tends to be greatly influenced by the characteristics of the substrate. From this perspective, the storage modulus E3 of the substrate of the dicing film at 60°C is preferably 10 to 80 MPa, more preferably 10 to 70 MPa, even more preferably 20 to 70 MPa, even more preferably 30 to 60 MPa, and even more preferably 30 to 50 MPa. The storage modulus E1 of the film-like adhesive at 60°C and the storage modulus E2 of the dicing film at 60°C can each be determined by the method described in the Examples. The storage modulus E3 of the substrate at 60°C can also be determined in accordance with the method for determining the storage modulus E2 of the dicing film at 60°C.

[0014] The film-like adhesive constituting the film-like adhesive with dicing film of the present invention has a light transmittance of 60% or more after curing. A light transmittance of 60% or more after curing ensures transparency after curing, and can exhibit optical properties suitable for bonding transparent film-like members, etc. Here, in the present invention, "light transmittance of 60% or more" means a light transmittance of 60% or more at a wavelength of 400 nm. The light transmittance at a wavelength of 400 nm represents the light transmittance at wavelengths in the entire visible light range. "Cured film-like adhesive" refers to a cured product obtained by treating a film-like adhesive at 150°C for 1 hour. In the present invention and specification, when the term "film-like adhesive" is used to describe the properties of a film-like adhesive, it refers to a film-like adhesive before thermal curing. Specifically, this refers to a film-like adhesive that has not been exposed to temperatures above the temperature at which the epoxy resin thermally cures after preparation. Preferably, the film-like adhesive has not been exposed to temperatures above 25°C after preparation. The above explanation is provided to clarify the characteristics of the film-like adhesive, and the film-like adhesive with dicing film of the present invention is not limited to film-like adhesives that are not exposed to temperatures of 25°C or higher. The light transmittance of the cured product of the film-like adhesive is preferably 70% or higher, more preferably 80% or higher, and even more preferably 85% or higher. The light transmittance of the cured product of the film-like adhesive is preferably 70 to 95%, more preferably 80 to 92%, and even more preferably 85 to 90%. The light transmittance of the cured product of the film-like adhesive is determined by the method described in the Examples. The light transmittance of the cured product of the film-like adhesive can be controlled by the type and content of the components of the film-like adhesive (resin, curing agent, filler, etc.). The particle size of the filler, as well as the content, can affect the light transmittance. The transparency of the film-like adhesive before curing is not limited and may be transparent or opaque. Therefore, the light transmittance of the film-like adhesive before curing may be 60% or higher or less than 60% at a wavelength of 400 nm.

[0015] The film-like adhesive with a dicing film of the present invention will be described in more detail below.

[0016] <Dicing Film> The dicing film constituting the film-like adhesive with dicing film of the present invention has a substrate and a pressure-sensitive adhesive layer. The materials and composition of the substrate and pressure-sensitive adhesive layer are not particularly limited as long as they satisfy E1 and E2 above when combined with the film-like adhesive after being laminated to form a dicing film.

[0017] - Substrate - The substrate can be made of various resin materials. Among them, those made of a resin material selected from polyolefin resin and polyvinyl chloride resin are preferred. It is also preferred that these resin materials have a crosslinked structure. The bond that contributes to the formation of the crosslinked structure may be a covalent bond, a bond based on ionic interaction, or a hydrogen bond.

[0018] Examples of the polyolefin resin include α-olefin homopolymer or copolymer resins such as polyethylene, polypropylene, ethylene-propylene copolymer, polybutene-1, poly-4-methylpentene-1, ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid alkyl ester copolymer (ethylene-ethyl acrylate copolymer, ethylene-methyl acrylate copolymer, ethylene-methyl methacrylate copolymer, etc.), ethylene-(meth)acrylic acid copolymer, and ionomer resin, as well as mixtures thereof.

[0019] In particular, ionomer resins, which are synthetic resins that utilize the cohesive force of metal ions to form polymer aggregates, are preferred. Examples include ionomer resins obtained by crosslinking ethylene-(meth)acrylic acid binary copolymers or ethylene-(meth)acrylic acid-(meth)acrylic acid alkyl ester terpolymers with metal ions. These resins are suitable for the expanding process in terms of uniform expandability. The metal ions contained in the ionomer resins are not particularly limited, but examples include zinc ions and sodium ions. Zinc ions are preferred due to their low elution and low contamination. Generally, ionomer resins have a greater restoring force against tension than resins without metal ions, and experience greater shrinkage stress when heat is applied to the expanded state after the expanding process. Therefore, ionomer resins are preferred in that they allow for a heat shrink process in which slack generated in the tape after the expanding process is removed by thermal shrinkage, and the tape is tensioned to stably maintain the spacing between individual wafer chips.

[0020] In addition to the above-mentioned ionomer resins, thermoplastic crosslinked resins obtained by crosslinking a resin selected from low-density polyethylene with a specific gravity of 0.910 or more but less than 0.930, ultra-low-density polyethylene with a specific gravity of less than 0.910, and ethylene-vinyl acetate copolymer are also suitable. Examples of crosslinking methods include irradiating the above-mentioned resins with energy beams such as electron beams. Such thermoplastic crosslinked resins have a certain degree of uniform extensibility because crosslinked and non-crosslinked regions coexist within the resin. Furthermore, since such thermoplastic crosslinked resins contain almost no chlorine atoms in the molecular chain structure, incineration of used tapes does not generate chlorinated aromatic hydrocarbons such as dioxins and their analogs, thereby minimizing the environmental impact. By appropriately adjusting the amount of energy beams irradiated onto the above-mentioned polyethylene or ethylene-vinyl acetate copolymer, resins with sufficient uniform extensibility can be obtained.

[0021] The substrate may be a single layer or multiple layers, and is preferably an ionomer resin of an ethylene-(meth)acrylic acid copolymer.

[0022] The thickness of the substrate is not particularly limited, but is preferably 50 to 200 μm, more preferably 60 to 160 μm, and even more preferably 70 to 150 μm.

[0023] -Adhesive Layer- The adhesive layer constituting the adhesive tape of the present invention is not particularly limited, as long as it has sufficient retention to prevent peeling between the laminate of the transparent film-like member (adherend) and the film-like adhesive described below during the dicing process and allows peeling of the adhesive-attached transparent film-like chip during pickup. The adhesive constituting the adhesive layer is not particularly limited as long as it exhibits the above-mentioned properties, and general adhesives used in dicing film applications, such as acrylic adhesives and rubber-based adhesives, can be used as appropriate. Among these, energy ray-curable adhesives are preferred. Energy ray-curable adhesives can be cured before the pickup process to facilitate pickup. Here, energy rays refer to light rays such as ultraviolet rays or ionizing radiation such as electron beams. The adhesive constituting the adhesive layer can be any adhesive commonly used as an adhesive for dicing adhesive tapes, without any particular restrictions. For the components, properties, and manufacturing method of the pressure-sensitive adhesive, see, for example, Japanese Patent No. 6928852, paragraphs

[0039] to

[0076] , Japanese Patent No. 6989561, paragraphs

[0033] to

[0052] , and Japanese Patent Laid-Open No. 2023-13022, paragraphs

[0031] to

[0057] .

[0024] The adhesive constituting the adhesive layer is preferably an acrylic adhesive containing a (meth)acrylic resin as a base polymer, and more preferably an acrylic adhesive containing at least one of a (meth)acrylic acid alkyl ester and (meth)acrylic acid as a constituent. The (meth)acrylic acid alkyl ester preferably further has a radiation-curable group introduced into its side chain, and more preferably has a (meth)acrylic acid ester having an isocyanate group added thereto. The adhesive may further contain a radiation-curable oligomer, such as a urethane (meth)acrylate oligomer.

[0025] The pressure-sensitive adhesive layer may contain a curing agent, such as a polyisocyanate compound, and a photopolymerization initiator.

[0026] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is preferably 2 to 35 μm, more preferably 5 to 30 μm, and even more preferably 5 to 20 μm.

[0027] <Film-like Adhesive> The film-like adhesive constituting the film-like adhesive with dicing film of the present invention will be described. A typical film-like adhesive can be used as long as it satisfies the above E1 and E2 when combined with the dicing film and the cured product of the film-like adhesive has a light transmittance of 60% or more. The film-like adhesive preferably contains an epoxy resin and a polymer component, more preferably an epoxy resin and a urethane resin, or an epoxy resin and a phenoxy resin, and even more preferably an epoxy resin and a phenoxy resin. The film-like adhesive may contain a filler. However, from the viewpoint of improving light transmittance, when the film-like adhesive contains a filler, the content of the filler is preferably 30% by mass or less, more preferably 20% by mass or less, even more preferably 10% by mass or less, and even more preferably 5% by mass or less of the total solid content of the film-like adhesive. The film-like adhesive usually contains a curing agent. In a preferred embodiment of the present invention, the film-like adhesive preferably contains an epoxy resin, a polymer component, and a curing agent. In this case, a filler may be contained as described above. Each component will be described.

[0028] -Epoxy Resin- The epoxy resin is a thermosetting resin having epoxy groups and an epoxy equivalent of 1000 g / eq or less. The epoxy resin may be liquid, solid, or semi-solid. In the present invention, "liquid" refers to a resin having a softening point below 25°C, "solid" refers to a resin having a softening point of 60°C or higher, and "semi-solid" refers to a resin having a softening point between the softening points of the liquid and solid (25°C or higher and lower than 60°C). The epoxy resin used in the present invention preferably has a softening point of 100°C or lower, from the viewpoint of obtaining a film-like adhesive that can achieve a low melt viscosity in a suitable temperature range (e.g., 60 to 120°C). In the present invention, the softening point is a value measured by a softening point test (ring and ball method) (measurement conditions: in accordance with JIS-K7234 1986).

[0029] In the epoxy resin used in the present invention, from the viewpoint of increasing the crosslink density of the thermoset, the epoxy equivalent is preferably 150 to 800 g / eq. In the present invention, the epoxy equivalent refers to the number of grams (g / eq) of resin containing 1 gram equivalent of epoxy groups. The weight average molecular weight of the epoxy resin is usually preferably less than 10,000, more preferably 5,000 or less. There is no particular restriction on the lower limit, but a value of 300 or more is practical. The weight average molecular weight is a value determined by GPC (Gel Permeation Chromatography) analysis.

[0030] Examples of epoxy resin skeletons include phenol novolac, orthocresol novolac, cresol novolac, dicyclopentadiene, biphenyl, fluorene bisphenol, triazine, naphthol, naphthalenediol, triphenylmethane, tetraphenyl, bisphenol A, bisphenol F, bisphenol AD, bisphenol S, and trimethylolmethane. Among these, triphenylmethane, bisphenol A, cresol novolac, and orthocresol novolac are preferred from the viewpoint of obtaining a film-like adhesive with low resin crystallinity and good appearance. These may be used alone or in combination of two or more, with a combination of triphenylmethane and bisphenol A being preferred.

[0031] The content of the epoxy resin is preferably 25 to 80 parts by mass, more preferably 30 to 80 parts by mass, even more preferably 30 to 70 parts by mass, and even more preferably 40 to 70 parts by mass, per 100 parts by mass of the total content of the components constituting the film-like adhesive (specifically, components other than the solvent, i.e., solids). By setting the content within the above preferred range, storage stability and transparency can be improved. Furthermore, by setting the content below the above preferred upper limit, the generation of oligomer components can be suppressed, making it less likely that changes in the film state (film tackiness, etc.) will occur due to slight temperature changes. The content of the epoxy resin is preferably 30 to 70 parts by mass, more preferably 30 to 60 parts by mass, per 100 parts by mass of the total content of the epoxy resin and polymer components.

[0032] -Polymer Component- The polymer component may be any component that, when a film-like adhesive is formed, suppresses film tackiness (the property of a film state being easily changed even by slight temperature changes) at room temperature (25°C) and imparts sufficient adhesiveness and film-forming properties (film-forming properties). Examples of such polymer components include natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resins such as 6-nylon and 6,6-nylon, phenoxy resin, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyamideimide resin, fluororesin, and polyurethane resin. These polymer components may be used alone or in combination of two or more. The polymer component is preferably at least one of phenoxy resin and polyurethane resin.

[0033] The weight-average molecular weight of the polymer component is 10,000 or more. There is no particular upper limit, but a practical value is 5,000,000 or less. The weight-average molecular weight of the polymer component is a value determined in terms of polystyrene by GPC (gel permeation chromatography). Hereinafter, the specific weight-average molecular weight of the polymer component has the same meaning. The glass transition temperature (Tg) of the polymer component is preferably less than 100°C, more preferably less than 90°C. The lower limit is preferably 0°C or more, more preferably 10°C or more. Therefore, the glass transition temperature (Tg) of the polymer component is preferably 0°C or more and less than 100°C. The glass transition temperature of the polymer component is the glass transition temperature measured by a differential scanning calorimeter (DSC) at a heating rate of 0.1°C / min. More specifically, the temperature was raised from -100°C to 100°C at a rate of 0.1°C / min, and the extrapolated glass transition onset temperature according to JIS K7121:2012 "Measurement Method for Transition Temperature of Plastics" was used as the glass transition temperature. Hereinafter, the glass transition temperature values ​​of specific polymer components have the same meaning. In the present invention, among the epoxy resins and polymer components, resins that may have epoxy groups, such as phenoxy resins, are classified as epoxy resins when their epoxy equivalent is 1000 g / eq or less, and as polymer components when their epoxy equivalent is greater than 1000 g / eq.

[0034] (Phenoxy Resin) Phenoxy resin is preferred as a polymer component due to its similar structure to epoxy resins and its good compatibility. The inclusion of phenoxy resin can also exhibit excellent adhesive properties. Phenoxy resin can be obtained by conventional methods. For example, phenoxy resin can be obtained by reacting a bisphenol or biphenol compound with an epihalohydrin such as epichlorohydrin, or by reacting a liquid epoxy resin with a bisphenol or biphenol compound.

[0035] The weight average molecular weight of the phenoxy resin is preferably 10,000 or more, more preferably 10,000 to 100,000. The amount of epoxy groups remaining in the phenoxy resin in small amounts is preferably 5,000 g / eq or more in terms of epoxy equivalent.

[0036] The glass transition temperature (Tg) of the phenoxy resin is preferably less than 100° C., more preferably less than 90° C. The lower limit is preferably 0° C. or higher, more preferably 10° C. or higher. Therefore, the glass transition temperature (Tg) of the phenoxy resin is preferably 0° C. or higher and lower than 100° C.

[0037] (Polyurethane Resin) A polyurethane resin is a polymer having a urethane (carbamic acid ester) bond in the main chain. The polyurethane resin has a structural unit derived from a polyol and a structural unit derived from a polyisocyanate, and may further have a structural unit derived from a polycarboxylic acid. The polyurethane resin may be used alone or in combination of two or more. The Tg of the polyurethane resin is usually 100°C or less, preferably 60°C or less, more preferably 50°C or less, and also preferably 45°C or less.

[0038] There are no particular restrictions on the weight average molecular weight of the polyurethane resin, and those in the range of 5,000 to 500,000 are usually used.

[0039] The polyurethane resin can be synthesized by a conventional method, and is also commercially available. Examples of commercially available products that can be used as the polyurethane resin include Dynaleo VA-9320M, Dynaleo VA-9310MF, and Dynaleo VA-9303MF (all manufactured by Toyochem Co., Ltd.).

[0040] The content of the polymer component per 100 parts by mass of the epoxy resin is preferably 1 to 250 parts by mass, more preferably 10 to 180 parts by mass, and even more preferably 40 to 150 parts by mass. By setting the content within this range, it is possible to adjust the rigidity and flexibility of the film-like adhesive before curing. The film condition becomes good (film tackiness is reduced) and film brittleness can also be suppressed. The content of the polymer component is preferably 30 to 70 parts by mass, more preferably 40 to 70 parts by mass, per 100 parts by mass of the total content of the epoxy resin and polymer component.

[0041] - Curing Agent - The curing agent is a component that affects the control of the light transmittance defined in the present invention. It is preferable to select the curing agent in consideration of the control of the light transmittance.

[0042] Examples of curing agents include amines, acid anhydrides, and polyhydric phenols. From the viewpoint of storage stability of the film-like adhesive, it is preferable to use a latent curing agent. Examples of latent curing agents include dicyandiamide compounds, imidazole compounds, curing catalyst composite polyhydric phenol compounds, hydrazide compounds, boron trifluoride-amine complexes, amine imide compounds, polyamine salts, and modified products and microcapsule-type compounds thereof. These may be used alone or in combination of two or more. Among these, it is preferable to use at least one of dicyandiamide compounds, imidazole compounds, and hydrazide compounds. The latent curing agent may be a thermal cationic polymerization initiator, and may contain a sulfonium cation as the cationic component and SbF as the anionic component. 6 - or PF 6 - A thermal cationic polymerization initiator having the formula:

[0043] The content of the curing agent relative to 100 parts by mass of the epoxy resin is preferably 0.5 to 50 parts by mass, more preferably 1 to 40 parts by mass, even more preferably 1 to 30 parts by mass, still more preferably 1 to 10 parts by mass, and even more preferably 1 to 5 parts by mass, from the viewpoints of exhibiting a sufficient curing rate and ensuring transparency after curing.

[0044] Filler: As long as the above-mentioned light transmittance can be achieved, fillers that are commonly used in film-like adhesives can be used without any particular restrictions. The filler is preferably an inorganic filler. Examples of inorganic fillers include ceramics such as silica, clay, gypsum, calcium carbonate, barium sulfate, alumina (aluminum oxide), beryllium oxide, magnesium oxide, silicon carbide, silicon nitride, aluminum nitride, and boron nitride; metals or alloys such as aluminum, copper, silver, gold, nickel, chromium, lead, tin, zinc, palladium, and solder; and various inorganic powders such as carbons such as carbon nanotubes and graphene. Silica is preferred as the filler.

[0045] The particle size (d50) of the filler is not particularly limited, but is preferably 500 nm or less from the viewpoint of improving light transmittance. The particle size is preferably 1 to 500 nm, more preferably 10 to 500 nm, even more preferably 10 to 499 nm, even more preferably 10 to 450 nm, even more preferably 10 to 350 nm, even more preferably 10 to 200 nm, and even more preferably 10 to 100 nm. The particle size (d50) is the so-called median diameter, and refers to the particle size at 50% cumulative when the particle size distribution is measured by a laser diffraction / scattering method and the total volume of the particles in the cumulative distribution is taken as 100%.

[0046] -Other Components- In addition to the epoxy resin, curing agent, polymer component, and filler, the film adhesive may further contain an ion trapping agent (ion capture agent), curing catalyst, viscosity modifier, antioxidant, flame retardant, colorant, and the like, as long as the effects of the present invention are not impaired. For example, other additives described in International Publication No. 2017 / 158994 may be included. From the viewpoint of adhesive reliability, it is preferable that the film adhesive does not contain a colorant such as a dye or pigment. It is also preferable that the film adhesive does not contain a filler. The total content of the epoxy resin and polymer component contained in the film adhesive is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and even preferably 80% by mass or more.

[0047] -Thickness of film adhesive- The thickness of the film adhesive is not particularly limited and can be set appropriately depending on the purpose. The thickness of the film adhesive can be, for example, 1 to 30 μm, preferably 1 to 25 μm, preferably 1 to 20 μm, preferably 2 to 20 μm, preferably 3 to 20 μm, or preferably 4 to 20 μm. The thickness of the film adhesive can be measured using a contact / linear gauge method (desktop contact thickness measurement device).

[0048] <Production of a Film-Like Adhesive with a Dicing Film> The method for producing a film-like adhesive with a dicing film is not particularly limited as long as it results in a laminated structure of a dicing film and a film-like adhesive. For example, a coating liquid containing a pressure-sensitive adhesive is applied to a release-treated release liner and dried to form a pressure-sensitive adhesive layer. The pressure-sensitive adhesive layer is then bonded to a substrate to obtain a laminate in which the substrate, pressure-sensitive adhesive layer, and release liner are laminated in this order. Separately, a film-like adhesive-forming composition is applied to a release film (synonymous with release liner, but for convenience, the term is used interchangeably here) and dried to form a film-like adhesive on the release film. Next, the release liner is peeled off to expose the pressure-sensitive adhesive layer, and the dicing film and the film-like adhesive are bonded together to obtain a film-like adhesive with a dicing film in which the substrate, pressure-sensitive adhesive layer, film-like adhesive, and release film are laminated in this order. The bonding of the dicing film and the die attach film is preferably performed under pressure. In bonding the dicing film and the film-like adhesive, the shape of the dicing film is not particularly limited as long as it can cover the opening of the ring frame, and is preferably circular. The shape of the film-like adhesive is also not particularly limited as long as it can cover the back surface of the wafer, and is preferably circular. The dicing film is preferably larger than the film-like adhesive and has a shape in which the pressure-sensitive adhesive layer is exposed around the adhesive layer. In this way, it is preferable to bond the dicing film and film-like adhesive cut into the desired shape. When using the film-like adhesive with dicing film prepared as described above, the release film is peeled off.

[0049] The formation of a film-like adhesive will now be further explained. A film-like adhesive can be obtained by forming a film using a composition (film-like adhesive-forming composition (varnish)) obtained by mixing the components constituting the film-like adhesive at a temperature at which the epoxy resin does not actually cure. The order of mixing is not particularly limited. For example, resin components such as an epoxy resin and a polymer component may be mixed, optionally with a solvent, followed by mixing with a curing agent. In this case, mixing in the presence of a curing agent may be performed at a temperature at which the epoxy resin does not actually cure, while mixing of the resin components in the absence of a curing agent may be performed at a higher temperature. A film can be formed using the above-mentioned film-like adhesive-forming composition by, for example, applying the film-like adhesive-forming composition to a release-treated substrate (also referred to as a release film or peel film) and drying it as necessary. Any release film can be used as the cover film for the resulting film-like adhesive, and conventional release films can be used as appropriate. Examples include release-treated polypropylene (PP), release-treated polyethylene (PE), and release-treated polyethylene terephthalate (PET). As the coating method, a conventional method can be appropriately adopted, and examples include methods using a roll knife coater, gravure coater, die coater, reverse coater, etc. Drying may be performed by removing the organic solvent from the film-like adhesive-forming composition without substantially curing the epoxy resin, to obtain a film-like adhesive, and can be performed, for example, by maintaining the composition at a temperature of 80 to 150°C for 1 to 20 minutes.

[0050] The film adhesive can be in a form in which the above-mentioned release film or the like is laminated to at least one surface. In this case, the release film does not constitute the film adhesive, but is considered to be laminated to the film adhesive. In other words, when describing the thickness of a film adhesive in a form in which the above-mentioned release film or the like is laminated to at least one surface of the film adhesive, the thickness does not include the thickness of the release film or the like. In other words, the thickness of the film adhesive in the present invention is the thickness of the layer derived from the film adhesive-forming composition.

[0051] From the viewpoint of more reliably suppressing the thermal curing of the epoxy resin, the film adhesive is preferably stored at a temperature of 10° C. or less before use.

[0052] The film-like adhesive with dicing film of the present invention may further be laminated with a release film or the like. By forming the film-like adhesive with dicing film of the present invention into such a laminated film, a transparent film-like member (adherend), such as a transparent protective film, can be adhered to the film-like adhesive side of the laminated film, fixed via a dicing film, and the transparent film-like member can be cut (diced) to the desired size together with the film-like adhesive. As a result, a transparent film-like chip with an adhesive layer cut to the desired size can be obtained on the dicing film. The transparent film-like chip with the adhesive layer is then peeled from the dicing film, and the transparent film-like chip can be incorporated into an electronic component via the adhesive layer. This incorporation into the electronic component is performed by thermocompression bonding or the like, and then the adhesive layer is thermally cured. This curing reaction, for example, involves the reaction of a solid curing agent, thereby increasing the transparency of the adhesive. The thermocompression bonding is performed at a temperature at which the epoxy resin does not actually cure. For example, conditions of 70°C and a pressure of approximately 0.3 MPa can be cited. The thermosetting reaction may be carried out at a temperature equal to or higher than the thermosetting initiation temperature of the film-like adhesive. The thermosetting initiation temperature varies depending on the types of epoxy resin, polymer component, and epoxy curing agent used, and cannot be generalized; however, for example, 100 to 180°C is preferred, and 140 to 180°C is more preferred from the viewpoint of achieving short curing times. If the temperature is below the thermosetting initiation temperature, the thermosetting reaction does not proceed sufficiently, and the strength of the adhesive layer tends to decrease. On the other hand, if the curing reaction temperature is too high, the curing agent and additives in the film-like adhesive tend to volatilize during the curing reaction, causing foaming. Furthermore, the curing treatment time is preferably 10 to 120 minutes, for example. Regarding the above-described embodiment, the present invention provides the following method for manufacturing an electronic component.

[0053] A method for manufacturing an electronic component, comprising: a first step of obtaining a laminate in which a transparent film-like member and the film-like adhesive with a dicing film of the present invention are laminated in this order; a second step of dicing the transparent film-like member and the film-like adhesive together to obtain a transparent film-like chip with an adhesive layer on the dicing film; a third step of removing the dicing film from the adhesive layer and thermocompressing the transparent film-like chip with an adhesive layer to other members that constitute the electronic component via the adhesive layer; and a fourth step of thermally curing the adhesive layer.

[0054] The electronic component obtained by the above manufacturing method has a structure in which a transparent film chip is incorporated into the electronic component via a thermoset film adhesive. In the present invention, the term "transparent film chip" refers to a transparent film processed into a desired shape. Typically, a transparent film member such as a glass substrate or transparent resin is cut into a desired shape for incorporation into the electronic component.

[0055] An example of the electronic component is an image sensor (imaging element), in which case the transparent film chip incorporated into the electronic component is preferably a protective film for a photodiode.

[0056] The above is a description of a preferred embodiment of the transparent film-like member, and the present invention is not limited to these embodiments except as specified in the present invention. For example, preferred examples of the electronic component include members used in optical devices such as optical lenses, optical fibers, optical waveguides, optical isolators, and semiconductor lasers.

[0057] The present invention will be described in more detail based on examples and comparative examples, but the present invention is not limited to the following embodiments. In the following description, room temperature means 25°C. Furthermore, "MEK" stands for methyl ethyl ketone, and "PET" stands for polyethylene terephthalate.

[0058] For each of the Examples and Comparative Examples, a film-like adhesive with a release film as shown in FIG. 1 was prepared.

[0059] [Fabrication of Dicing Film] <Preparation of Substrate> (Substrate X) Ethylene-methacrylic acid copolymer zinc ionomer resin (trade name: Himilan 1855, manufactured by DuPont-Mitsui Chemical Co., Ltd.) was melted at 200°C and extruded to produce a 90 μm thick substrate X. One side of substrate X was subjected to corona treatment. (Substrate Y) Ethylene-methacrylic acid copolymer zinc ionomer resin (trade name: Himilan AM7326, manufactured by DuPont-Mitsui Chemical Co., Ltd.) was melted at 200°C and extruded to produce a 90 μm thick substrate Y. One side of substrate Y was subjected to corona treatment. (Substrate Z) Ethylene-methacrylic acid copolymer (trade name: Nucrel N0200H, manufactured by DuPont-Mitsui Chemical Co., Ltd.) was melted at 200°C and extruded to produce a 90 μm thick substrate Z. One side of substrate Z was subjected to corona treatment.

[0060] <Dicing Film A> 65 parts by weight of butyl acrylate, 25 parts by weight of 2-hydroxyethyl acrylate, and 10 parts by weight of acrylic acid were radically polymerized, and then 2-isocyanatoethyl methacrylate was added dropwise while the reaction was continued to obtain an acrylic copolymer with a weight-average molecular weight of 800,000. 3 parts by weight of polyisocyanate as a curing agent and 1 part by weight of 1-hydroxycyclohexylphenyl ketone as a photopolymerization initiator were added to 100 parts by weight of this acrylic copolymer and mixed to obtain a pressure-sensitive adhesive layer composition. The pressure-sensitive adhesive layer composition was then applied to a release-treated release liner to a dry film thickness of 10 μm, and dried at 120°C for 3 minutes to obtain a pressure-sensitive adhesive layer. This pressure-sensitive adhesive layer was then bonded to the corona-treated surface of Substrate X to produce Dicing Film A, which had a substrate and a pressure-sensitive adhesive layer with a release liner.

[0061] Dicing Film B Dicing film B was produced in the same manner as dicing film A, except that substrate Y was used instead.

[0062] Dicing Film C Dicing film C was produced in the same manner as dicing film A, except that substrate Z was used instead.

[0063] [Preparation of film-like adhesive with dicing film] The components used in preparing the film-like adhesive are shown below. <Materials used> (Epoxy resins) 828 (bisphenol A type epoxy resin, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 190 g / eq, specific gravity 1.17) ST-3000 (hydrogenated bisphenol A type epoxy resin, manufactured by Nippon Steel Chemical & Material Co., Ltd.) YDCN-703 (cresol novolac type epoxy resin, manufactured by Tohto Kasei Co., Ltd., epoxy equivalent 210 g / eq, molecular weight 1200, softening point 80°C) (Phenoxy resins) 1256 (phenoxy resin, manufactured by Mitsubishi Chemical Corporation, epoxy equivalent 7500 g / eq) (Urethane resins) Dynaleo VA-9320M (urethane resin solution, weight average molecular weight: 120,000, Tg: 39°C, room temperature elastic modulus: 594 MPa, solvent: MEK / IPA mixed solvent, manufactured by Toyochem Co., Ltd.) (referred to as VA-9320M in the table) (acrylic resin) SG-P3 (acrylic resin, manufactured by Nagase ChemteX Corporation, weight average molecular weight 850,000, glass transition temperature 10°C) (curing agent) 2PHZ-PW (imidazole-based curing agent, manufactured by Shikoku Kasei Co., Ltd.) SI-150 (thermal cationic polymerization initiator, manufactured by Sanshin Chemical Co., Ltd.) (phenolic resin) Milex XLC-LL (phenolic resin, manufactured by Mitsui Chemicals, Inc., hydroxyl equivalent 175 g / eq) (filler) RY-200 (nano silica filler, manufactured by Nippon Aerosil Co., Ltd., particle size (d50): 12 nm, Mohs hardness: 7 Mohs, thermal conductivity: 1 W / m K) S0-C2 (silica filler, manufactured by Adma Fine Co., Ltd., specific gravity 2.2 g / cm 3 , Mohs hardness: 7 Mohs, particle size (d50) 500 nm, specific surface area 6.0 m 2 / g)

[0064] Example 1 (Preparation of Film-Like Adhesive) 50 parts by mass of epoxy resin (trade name: 828, manufactured by Mitsubishi Chemical Corporation, bisphenol A-type epoxy resin, epoxy equivalent 190 g / eq, specific gravity 1.17) and 50 parts by mass of phenoxy resin (trade name: 1256, manufactured by Mitsubishi Chemical Corporation, bisphenol A-type phenoxy resin, epoxy equivalent 7500 g / eq) were heated and stirred together with MEK in a 1000 ml separable flask at a temperature of 110°C for 2 hours to obtain a resin varnish. Next, this resin varnish was transferred to another flask, and 1 part by mass of curing agent (trade name: 2PHZ-PW, imidazole-based curing agent, manufactured by Shikoku Kasei Co., Ltd.) was added. The mixture was stirred and mixed at room temperature for 1 hour, and then vacuum degassed to obtain a mixed varnish. The resulting mixed varnish was then applied to a 38 μm thick release-treated PET film (release film) and dried by heating at 130°C for 10 minutes to form a film-like adhesive layer measuring 300 mm in length, 300 mm in width, and 20 μm in thickness. The resulting film-like adhesive with release film was stored at 10°C or below. After drying, the epoxy resin was not cured (unless otherwise specified, this also applies to other examples and comparative examples). (Preparation of film-like adhesive with dicing film) Next, the dicing film B with release liner was cut into a circular shape that could be bonded to cover the opening of the ring frame. The film-like adhesive with release film was also cut into a circular shape that could cover the backside of the wafer. The dicing film B cut as described above and exposed by peeling the release liner from the dicing film B with release liner was then bonded to the film-like adhesive with release film cut as described above using a roll press under conditions of a load of 0.4 MPa and a speed of 1.0 m / min to produce a film-like adhesive with dicing film, in which a substrate, a pressure-sensitive adhesive layer, a film-like adhesive, and a release film were laminated in this order. This film-like adhesive with dicing film has a substrate and a pressure-sensitive adhesive layer, and the film-like adhesive is formed on the pressure-sensitive adhesive layer of the dicing film. Furthermore, in this film-like adhesive with dicing film, the dicing film is larger than the film-like adhesive, and there is an exposed portion of the dicing film around the film-like adhesive.

[0065] Example 2 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 1, except that in producing the film-like adhesive of Example 1, 1 part by mass of SI-150 was used instead of 2PHZ-PW as the curing agent, and 3 parts by mass of RY-200 was added to the mixed varnish as a filler.

[0066] Example 3 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 1, except that in the preparation of the film-like adhesive of Example 1, 11 parts by mass of RY-200 was added to the mixed varnish as a filler.

[0067] Example 4 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 2, except that in the preparation of the film-like adhesive of Example 2, 5 parts by mass of S0-C2 was added to the mixed varnish instead of RY-200 as the filler.

[0068] <Example 5> In producing the film-like adhesive with a dicing film of Example 2, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 2, except that dicing film A was used as the dicing film.

[0069] <Example 6> In preparing the film-like adhesive with a dicing film of Example 3, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 3, except that dicing film A was used as the dicing film.

[0070] <Example 7> In preparing the film-like adhesive with dicing film of Example 4, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 4, except that dicing film A was used as the dicing film.

[0071] Example 8 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 5, except that in producing the film-like adhesive of Example 5, 150 parts by mass of a urethane resin solution (VA-9320M) (50 parts by mass of urethane resin) was used as the polymer component instead of the phenoxy resin (1256), the curing agent in the mixed varnish was 1 part by mass of 2PHZ-PW, and 35 parts by mass of RY-200 was added as a filler.

[0072] Example 9 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 5, except that in preparing the film-like adhesive of Example 5, 50 parts by mass of ST-3000 was used instead of 828 as the epoxy resin.

[0073] Example 10 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 5, except that in the preparation of the film-like adhesive of Example 5, 20 parts by mass of RY-200 was added to the mixed varnish as a filler.

[0074] <Example 11> In preparing the film-like adhesive of Example 5, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 5, except that the blending amount of 828 in the resin varnish was 30 parts by mass and the blending amount of 1256 was 70 parts by mass.

[0075] <Example 12> In preparing the film-like adhesive of Example 2, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 2, except that the blending amount of 828 in the resin varnish was 60 parts by mass and the blending amount of 1256 was 40 parts by mass.

[0076] <Comparative Example 1> In producing the film-like adhesive with dicing film of Example 1, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 1, except that dicing film A was used as the dicing film.

[0077] <Comparative Example 2> A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Comparative Example 1, except that in the preparation of the film-like adhesive of Comparative Example 1, 80 parts by mass of S0-C2 was added to the mixed varnish as a filler.

[0078] Comparative Example 3 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 1, except that in producing the film-like adhesive of Example 1, 18 parts by mass of YDCN-703 was used instead of 828 as the epoxy resin, 100 parts by mass of acrylic resin (SG-P3) was used instead of phenoxy resin (1256) as the polymer component, and 1 part by mass of 2PHZ-PW and 15 parts by mass of Milex XLC-LL were used as the curing agents.

[0079] Comparative Example 4 A film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Comparative Example 3, except that in the preparation of the film-like adhesive of Comparative Example 3, the blending amount of YDCN-703 was 50 parts by mass, the blending amount of SG-P3 was 250 parts by mass, 50 parts by mass of Milex XLC-LL was used as the curing agent without blending 2PHZ-PW, and 35 parts by mass of S0-C2 was added to the mixed varnish as a filler.

[0080] <Comparative Example 5> In preparing the film-like adhesive with dicing film of Example 2, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 2, except that dicing film C was used as the dicing film.

[0081] <Comparative Example 6> In preparing the film-like adhesive with dicing film of Example 3, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 3, except that dicing film C was used as the dicing film.

[0082] <Comparative Example 7> In preparing the film-like adhesive with dicing film of Example 4, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 4, except that dicing film C was used as the dicing film.

[0083] <Comparative Example 8> In preparing the film-like adhesive with dicing film of Example 8, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 8, except that dicing film C was used as the dicing film.

[0084] <Comparative Example 9> In preparing the film-like adhesive with dicing film of Example 9, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 9, except that dicing film C was used as the dicing film.

[0085] <Comparative Example 10> In preparing the film-like adhesive with dicing film of Example 10, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 10, except that dicing film C was used as the dicing film.

[0086] <Comparative Example 11> In preparing the film-like adhesive with dicing film of Example 11, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 11, except that dicing film C was used as the dicing film.

[0087] <Comparative Example 12> In preparing the film-like adhesive with dicing film of Example 12, a film-like adhesive with a release film and a film-like adhesive with a dicing film were obtained in the same manner as in Example 12, except that dicing film C was used as the dicing film.

[0088] For the film-like adhesive with release film and dicing films A to C obtained in each of the above examples and comparative examples, the storage modulus of the film-like adhesive at 60°C and the storage modulus of the dicing film at 60°C were determined as follows.

[0089] [Measurement of storage modulus of film-like adhesive] The release film was peeled off from the film-like adhesive with release film obtained in each Example and Comparative Example, and the film-like adhesive was laminated using a laminator at 70°C to a thickness of 0.5 mm. This laminate was cut into a 5 mm width to serve as a measurement sample. Using a dynamic viscoelasticity measuring device RSAIII (manufactured by TA Instruments), the viscoelastic behavior of the film-like adhesive was measured when it was heated from 25°C to 80°C at a heating rate of 5°C / min under tensile conditions of a chuck distance of 20 mm and a frequency of 10 Hz, and the storage modulus E1 at 60°C was determined.

[0090] [Measurement of storage modulus of dicing film] Dicing films A to C were each cut into a width of 5 mm to serve as a measurement sample. Using a dynamic viscoelasticity measuring device RSAIII (manufactured by TA Instruments), the viscoelastic behavior of the dicing film was measured when the temperature was raised from 25°C to 80°C at a heating rate of 5°C / min under tensile conditions of a chuck distance of 20 mm and a frequency of 10 Hz, and the storage modulus E2 at 60°C was determined. When the storage modulus of the substrate alone at 60°C was measured, it was found to be almost the same as that of the dicing film.

[0091] The film-like adhesive with dicing film obtained in each of the above Examples and Comparative Examples was evaluated for light transmittance and chipping after curing of the film-like adhesive as follows.

[0092] [Measurement of light transmittance of cured film adhesive] The film adhesive with the dicing film was heated and cured at 150°C for 1 hour, and then the dicing film was peeled off. The parallel ray transmittance of the film adhesive alone was measured over a wavelength range of 200 to 1100 nm using a spectrophotometer (Hitachi High-Technologies Corporation, Spectrophotometer U-4100 Solid State Sample Measurement System), and evaluated using the parallel ray transmittance at a wavelength of 400 nm.

[0093] [Chip Flying Evaluation] The film-like adhesive with dicing film obtained in each Example and Comparative Example was first bonded to one side of a glass wafer (material D263, 10 cm square, 100 μm thick) using a manual laminator (trade name: FM-114, manufactured by Technovision Co., Ltd.) at a temperature of 70°C and a pressure of 0.3 MPa so that the film-like adhesive layer was in contact with the surface. Then, using the same manual laminator at room temperature and a pressure of 0.3 MPa, a dicing frame (trade name: DTF2-8-1H001, manufactured by DISCO Corporation) was bonded to the area of ​​the film-like adhesive where the glass wafer was not bonded. Next, dicing was carried out from the glass wafer side to a size of 2 mm x 2 mm using a dicing machine (trade name: DFD-6340, manufactured by DISCO) equipped with a two-axis dicing blade (Z1: NBC-ZH2050 (27HEDD), manufactured by DISCO; Z2: NBC-ZH127F-SE (BC), manufactured by DISCO). 2,500 chips were obtained by this dicing. In the diced sample, the number of chips that had chipped (peeled off) was counted, and the chipping incidence rate relative to the total number of chips (number of chips that had chipped / total number of chips x 100) was calculated. The obtained chipping incidence rate was evaluated according to the following evaluation criteria. -Evaluation criteria- AA: Chip flying incidence rate is 0% A: Chip flying incidence rate is less than 1% of all chips B: Chip flying incidence rate is 1% or more but less than 3% of all chips C: Chip flying incidence rate is 3% or more of all chips

[0094] The above results are summarized in the table below. In the table below, the values ​​indicating the amount of epoxy resin, polymer component, hardener, and filler are in parts by mass. Blank spaces indicate that the component is not contained. The "Filler content" column indicates the amount of filler contained in the total solid content of the film adhesive.

[0095]

[0096]

[0097] The film-like adhesive with dicing film of Comparative Example 1 does not satisfy the storage modulus relationship E1 × E2 ≧ 7.0. The film-like adhesive with dicing film of Comparative Example 1 experienced chip flying during dicing. The film-like adhesive with dicing film of Comparative Examples 2 to 4 had a light transmittance of 35% or less for the cured film-like adhesive, and did not exhibit sufficient transparency. One possible cause of this is thought to be the excessive amount of filler in Comparative Example 2, and the incompatibility of the acrylic resin with the epoxy resin in Comparative Examples 3 and 4. The film-like adhesive with dicing film of Comparative Examples 5 to 12 does not satisfy the storage modulus relationship E1 × E2 ≧ 7.0. The film-like adhesive with dicing film of Comparative Examples 5 to 12 experienced chip flying during dicing. In contrast, the film-like adhesive with dicing film of Examples 1 to 12, which satisfy the requirements of the present invention, satisfied E1 × E2 ≧ 7.0, and the light transmittance of the cured film-like adhesive was 60% or more. It was found that the use of these film adhesives with dicing films effectively prevented chips from flying off during the dicing process, and also showed sufficiently high transparency after the curing reaction.

[0098] While the present invention has been described in connection with embodiments thereof, we do not intend to limit our invention to any of the details of the description unless otherwise specified, and believe that the claims should be construed broadly without departing from the spirit and scope of the invention as set forth in the appended claims.

[0099] This application claims priority based on Japanese Patent Application No. 2023-074875, filed in Japan on April 28, 2023, the contents of which are incorporated herein by reference.

[0100] REFERENCE SIGNS LIST 10 Dicing film 11 Substrate 12 Pressure-sensitive adhesive layer 20 Film-like adhesive

Claims

1. A film-like adhesive with a dicing film, comprising a dicing film having a substrate and an adhesive layer, and a film-like adhesive disposed on the adhesive layer, wherein the storage modulus E1 (MPa) of the film-like adhesive at 60°C and the storage modulus E2 (MPa) of the dicing film at 60°C satisfy E1 x E2 ≧ 7.0, and the light transmittance of the cured product of the film-like adhesive is 60% or more.

2. The film-like adhesive with dicing film according to claim 1, wherein the film-like adhesive contains an epoxy resin and a phenoxy resin.

3. A film-like adhesive with a dicing film as described in claim 1 or 2, wherein the film-like adhesive contains a filler, and the content of the filler is 10 mass% or less of the total solid content of the film-like adhesive.

4. A film-like adhesive with a dicing film according to claim 3, wherein the particle size (d50) of the filler is 500 nm or less.

5. A film-like adhesive with a dicing film according to any one of claims 1 to 4, wherein the film-like adhesive contains a curing agent, and the curing agent is a thermal cationic polymerization initiator.

6. A film-like adhesive with a dicing film according to any one of claims 1 to 5, wherein E1 is 0.1 to 1.0 MPa and E2 is 10 to 70 MPa.

7. A method for producing an electronic component comprising: a first step of obtaining a laminate in which a transparent film-like member and a film-like adhesive with a dicing film described in any one of claims 1 to 6 are laminated in this order; a second step of dicing the transparent film-like member and the film-like adhesive together to obtain a transparent film-like chip with an adhesive layer on the dicing film; a third step of removing the dicing film from the adhesive layer and thermocompressing the transparent film-like chip with the adhesive layer to other members constituting an electronic component via the adhesive layer; and a fourth step of thermally curing the adhesive layer.

8. The method for manufacturing an electronic component according to claim 7, wherein the electronic component is an image sensor.

9. The method for manufacturing an electronic component according to claim 8, wherein the electronic component has a structure in which the transparent film-like chip is incorporated as a protective film for a photodiode.

Citation Information

Patent Citations

  • Method of manufacturing semiconductor device and dicing-tape integral type adhesive sheet

    JP2010074135A

  • Dicing die-bonding film

    JP2011187571A

  • Dicing tape-integrated film for semiconductor back surface

    JP2011249739A

  • Film for semiconductor device and semiconductor device

    JP2012059768A

  • Method for manufacturing semiconductor device and adhesive film used in the method

    JP2013153071A