Joining material and method for producing joined body
The bonding method using a specially formulated silver or copper-based bonding material with controlled viscosity and particle size distribution addresses alignment and void issues in conductive part bonding, improving joint conductivity and strength.
Patent Information
- Application Number
- PCT/JP2024/015612
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
Existing bonding methods for conductive parts using silver or copper materials often result in insufficient fixation and alignment issues due to dry or semi-dry bonding materials, leading to voids and reduced conductivity, strength, and thermal performance in the bonded joints.
A bonding material comprising metal particles with specific size distribution and viscosity, applied to one conductive component without drying, and then dried and fired with the second component to form a joint, ensuring proper alignment and minimizing voids.
This method effectively suppresses void formation at the bonded interface, enhancing the electrical conductivity, thermal conductivity, and strength of the joint while maintaining high handleability of the bonding material.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Bonding material and method for manufacturing bonded body
[0001] The present invention relates to a bonding material and a method for manufacturing a bonded body. This application claims priority to Japanese Patent Application No. 2023-071341, filed on April 25, 2023, the contents of which are incorporated herein by reference.
[0002] Silver and copper have high thermal conductivity and high melting points, making them promising raw materials for joining conductive parts together as an alternative to solder. In particular, silver and copper are highly anticipated as packaging materials for power semiconductors, which have high heat density.
[0003] As a method for joining conductive parts using a bonding material containing silver, for example, a method has been disclosed in which a bonding material containing silver nanoparticles is applied to the members to be joined, the bonding material is heated to perform pre-firing, the members to be joined are separately placed on the heated bonding material, and the heated bonding material placed between the members to be joined is subjected to main firing at a temperature higher than the heating temperature, thereby forming a bond and joining the members to be joined (see Patent Document 1).
[0004] International Publication No. 2012 / 070262
[0005] However, in the bonding method described in Patent Document 1, the bonding material is in a dry or semi-dry state during pre-firing, and the bonded members (conductive components) are placed on top of it, which causes a problem that the bonded members placed later are not sufficiently fixed by the pre-firing bonding material. In this case, if any force is applied to the laminate, for example, when transporting the laminate of the bonded members and the pre-firing bonding material before the main firing, the positions of the bonded members placed on the pre-firing bonding material may be shifted.
[0006] In contrast, if a bonding material is applied to one conductive component, and then the other conductive component is placed on the bonding material without drying it, and then the bonding material is dried and fired, the conductive components will not shift in position. However, in this case, voids will occur between the subsequently placed conductive component and the undried bonding material. Even in a bonded body of conductive components obtained by drying and firing the bonding material in this state, voids may remain at the bonded portion. In a bonded body with many such voids, the electrical and thermal conductivity at the bonded portion, as well as the strength of the bonded portion, will be reduced. Until now, no bonding material or method for manufacturing a bonded body that can solve these problems has been known.
[0007] The present invention provides a bonding material for forming a joint that joins conductive parts together, in which one conductive part is placed on top of undried bonding material provided on the other conductive part, and the bonding material is then dried and fired to form the joint, thereby providing a bonding material that can suppress the generation of voids in the joint even when a bonded body of conductive parts is produced.
[0008] To solve the above problems, the present invention employs the following configurations. [1] A bonding material for bonding conductive parts, comprising metal particles containing metal particles (a) and a solvent for dispersing the metal particles, wherein the bonding material has a viscosity of 70 Pa·s or more as measured in accordance with JIS Z 3285:2017, and the metal particles (a) have a 50% cumulative volumetric particle diameter D50 of greater than 0.15 μm and less than 0.8 μm as measured by laser diffraction / scattering particle size distribution measurement. [2] The bonding material according to [1], wherein the metal particles (a) are silver particles. [3] The bonding material according to [1] or [2], wherein the bonding material has a thixotropy index according to JIS Z 3285:2017 in the range of 0.55 to 0.95. [4] The bonding material according to any one of [1] to [3], wherein the metal particles include metal particles (b) different from the metal particles (a), and the particle diameter D50 of the metal particles (b) at 50% cumulative volume, as measured by laser diffraction / scattering particle size distribution measurement, is 0.15 μm or less or 0.8 μm or more. [5] The bonding material according to any one of [1] to [4], wherein the solvent further contains a resin component that is a curable resin, a non-curable resin, or a thermoplastic resin, and the ratio of the content of the resin component to the content of the metal particles in the bonding material is less than 0.01 mass%. [6] The bonding material according to any one of [1] to [4], wherein the solvent does not contain a resin component that is a curable resin, a non-curable resin, or a thermoplastic resin. [7] A method for manufacturing a bonded body in which a conductive first component and a conductive second component are bonded via a conductive bonding part, the method comprising the steps of: attaching the bonding material according to any one of [1] to [6] to a first surface of the first component or a second surface of the second component; stacking the first component and the second component with the attached bonding material interposed therebetween to produce a laminate; drying the bonding material in the laminate to form a dried bonding material; and firing the dried bonding material at a temperature higher than the temperature at which the bonding material was dried to form the bonded part from the dried bonding material.
[0009] According to the present invention, there is provided a bonding material for forming a joint that joins conductive parts together, which is formed by placing one conductive part on top of undried bonding material that has been placed on the other conductive part, and then drying and firing the bonding material to form the joint, thereby capable of suppressing the generation of voids in the joint even when a bonded body of conductive parts is produced.
[0010] 2B. FIG. 2C is a cross-sectional view schematically illustrating an example of a bonded body to which a manufacturing method according to an embodiment of the present invention is applied; FIG. 2D is a cross-sectional view schematically illustrating an example of a manufacturing method for a bonded body according to an embodiment of the present invention, and is a view for illustrating an adhesion step; FIG. 2E is a cross-sectional view schematically illustrating another example of a manufacturing method for a bonded body according to an embodiment of the present invention, and is a view for illustrating an adhesion step; FIG. 3A is a cross-sectional view schematically illustrating a lamination step following the step of FIG. 3B; FIG. 3B is a view for illustrating a drying step following the step of FIG. 3C; and FIG. 3E is a view for illustrating a bonded body after the step of FIG.
[0011] Bonding Material A bonding material according to one embodiment of the present invention is a bonding material for bonding conductive components, comprising metal particles containing metal particles (a) and a solvent for dispersing the metal particles, wherein the bonding material has a viscosity of 70 Pa·s or greater as measured in accordance with JIS Z 3285:2017, and a particle diameter (sometimes referred to herein as "D50") of the metal particles (a) at 50% cumulative volume as measured by laser diffraction / scattering particle size distribution measurement is greater than 0.15 μm and less than 0.8 μm. Because the bonding material of this embodiment is paste-like, contains metal particles (a) as a main component with a D50 within a specific range, and has a viscosity within a specific range, even when a bonded body between conductive components is manufactured by placing one conductive component on top of the undried bonding material, drying the bonding material, and firing the bonding material to form a bond, voids can be suppressed at the bonded portion. This is because, as described above, when a conductive part is placed on the wet bonding material, the generation of voids between the bonding material and the conductive part is suppressed, which increases the conductivity and strength of the bonded part.
[0012] Viscosity The viscosity of the bonding material, measured in accordance with JIS Z 3285:2017, is 70 Pa·s or more, and may be, for example, any one of 90 Pa·s or more, 120 Pa·s or more, and 145 Pa·s or more. When the viscosity is equal to or greater than the lower limit, the effect of suppressing the generation of voids in the bonded portion described above is enhanced. On the other hand, the viscosity is preferably 180 Pa·s or less. When the viscosity is equal to or less than the upper limit, the fluidity of the bonding material is enhanced, and the handling of the bonding material is improved. In one embodiment, the viscosity may be, for example, any one of 70 to 180 Pa·s, 90 to 180 Pa·s, 120 to 180 Pa·s, and 145 to 180 Pa·s. However, these are just examples of the viscosities.
[0013] In this specification, unless otherwise specified, the term "viscosity of the bonding material" refers to the viscosity of the bonding material measured in accordance with the above-mentioned JIS Z 3285:2017.
[0014] Thixotropy Index: The thixotropy index of the bonding material, measured separately from the viscosity measurement in accordance with JIS Z 3285:2017, is preferably 0.55 to 0.95. When the bonding material has a viscosity within the above range and a thixotropy index within this range, the bonding material exhibits more favorable characteristics. Therefore, it is presumed that immediately after placing a conductive component on the wet bonding material, stress is applied to the bonding material, reducing the viscosity of the bonding material, making it easier for air bubbles generated between the wet bonding material and the conductive component to escape. On the other hand, it is presumed that after a certain time has passed since the conductive component was placed on the wet bonding material, the viscosity of the bonding material increases, making it easier to maintain the state in which air bubbles have escaped between the wet bonding material and the conductive component. As a result, it is presumed that the generation of voids between the undried bonding material and the conductive component is further suppressed, and ultimately the generation of voids at the bonding portion is further suppressed.
[0015] The viscosity of the bonding material can be adjusted, for example, by adjusting the type of metal particles (including metal particles (a)) and the solvent, and the content of the metal particles (a) and the solvent. In particular, the viscosity of the bonding material can be easily adjusted by adjusting the D50 of the metal particles (a) and the D10 and D90 described below. This is thought to be because the degree of aggregation of the metal particles affects the viscosity of the bonding material.
[0016] The bonding material of this embodiment will be described below. Note that in the bonding material, the ratio of the total content of one or more components contained in the bonding material, which will be described later, to the total mass of the bonding material does not exceed 100 mass%.
[0017] <<Metal Particles>> In this embodiment, the metal particles contained in the bonding material include at least metal particles (a). As will be described in detail later, the metal particles may further include metal particles (b). The shape of the metal particles (a) is not particularly limited, but is preferably approximately spherical. In this specification, the term "approximately spherical" refers to a spherical or spherical-like shape, not limited to the metal particles (a). More specifically, it refers to a particle shape having an aspect ratio calculated by [particle major axis] / [particle minor axis] of 2 or less. The aspect ratio is preferably 1.6 or less, and more preferably 1.3 or less. The surface of the approximately spherical particles may be composed of only curved surfaces, or may have flat surfaces, or may have corners formed by two flat surfaces connected at a predetermined angle to each other. The surface of the approximately spherical particles may be smooth or may have irregularities. As the metal particles (a), any commercially available spherical or approximately spherical shape can be used as long as it satisfies the above D50 condition.
[0018] The metal species of the metal particles (a) preferably has high thermal conductivity and a high melting point. For example, the thermal conductivity (e.g., bulk thermal conductivity) of the metal species of the metal particles (a) is preferably 350 W / mK or higher, and may be 350 to 450 W / mK. This allows heat to be quickly released, for example, even when the heat generation temperature of a semiconductor or the like in contact with the bonding material becomes high (e.g., 150°C or higher). For example, the melting point of the metal species of the metal particles (a) is preferably 900°C or higher, and may be 900 to 1100°C.
[0019] The metal species of the metal particles (a) contained in the bonding material may be one kind or two or more kinds, and when there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.
[0020] Among these, the metal species of the metal particles (a) is preferably silver or copper, and more preferably silver. That is, the metal particles (a) are preferably silver particles or copper particles, and more preferably silver particles. Note that the metal species of the metal particles (a) is not limited to pure silver or pure copper, and may be a silver alloy or a copper alloy.
[0021] Among the metal particles (a), silver particles include, for example, silver particles obtained by a reduction method and silver particles obtained by an atomization method. The silver particles may be surface-treated products whose surfaces have been chemically treated (treated with chemical substances), or may be surface-untreated products whose surfaces have not been chemically treated. Usually, silver particles obtained by a reduction method are surface-treated products, and silver particles obtained by an atomization method are surface-untreated products.
[0022] <Particle Size Distribution of Metal Particles> In this embodiment, the particle size distribution of the metal particles was measured by laser diffraction / scattering particle size distribution measurement. Hereinafter, the minimum particle size of the metal particles measured by laser diffraction / scattering particle size distribution measurement will be referred to as "Dmin," the particle size at 10% cumulative volume of the metal particles will be referred to as "D10," the particle size at 50% cumulative volume of the metal particles will be referred to as "D50," the particle size at 90% cumulative volume of the metal particles will be referred to as "D90," and the maximum particle size of the metal particles will be referred to as "Dmax."
[0023] The D50 of the metal particles (a) is greater than 0.15 μm and less than 0.8 μm, and is preferably 0.2 to 0.7 μm, and may be, for example, any of 0.2 to 0.5 μm, 0.2 to 0.45 μm, and 0.2 to 0.37 μm, or any of 0.3 to 0.7 μm, 0.38 to 0.7 μm, and 0.45 to 0.7 μm, or any of 0.3 to 0.5 μm and 0.38 to 0.45 μm. Having a D50 in this range enhances the effect of suppressing the generation of voids at the joints.
[0024] The D90 of the metal particles (a) is not particularly limited, but is preferably less than 1.2 μm, more preferably 1.08 μm or less, and may be, for example, 1.0 μm or less or 0.9 μm or less. Having a D90 in this range makes it easier to adjust the viscosity of the bonding material. On the other hand, a D90 of 0.45 μm or more is preferable. Such metal particles (a) are easier to prepare and are readily available. For example, particles with a predetermined D50 and a D90 smaller than 0.45 μm (i.e., particles with a narrow particle size distribution) may be difficult to manufacture. In one embodiment, the D90 may be, for example, 0.45 μm or more but less than 1.1 μm, 0.45 to 1.08 μm, 0.45 to 1.0 μm, or 0.45 to 0.9 μm or less. However, these are just examples of D90.
[0025] The D10 of the metal particles (a) is not particularly limited, but is preferably 0.06 μm or more, and may be, for example, 0.12 μm or more or 0.18 μm or more. Having a D10 in this range makes it easier to adjust the viscosity of the bonding material. On the other hand, D10 is preferably 0.34 μm or less. Such metal particles (a) are easier to prepare and are readily available. This is because, as described above, particles with a narrow particle size distribution may be more difficult to manufacture. In one embodiment, D10 may be, for example, 0.06 to 0.34 μm, 0.12 to 0.34 μm, or 0.18 to 0.34 μm. However, these are just examples of D10.
[0026] In the bonding material, the ratio of the content of the metal particles (a) to the total mass of the bonding material ([content of metal particles (a) in bonding material (parts by mass)] / [total mass of bonding material (parts by mass)]×100) is preferably 88.5 to 95 mass%, and may be, for example, any one of 90 to 95 mass%, 88.5 to 93 mass%, and 90 to 93 mass%. When the ratio is equal to or greater than the lower limit, the bonding portion can be formed more efficiently and the effect of suppressing the generation of voids in the bonding portion described above is further enhanced. When the ratio is equal to or less than the upper limit, the fluidity of the bonding material is further enhanced, and the handling of the bonding material is further enhanced.
[0027] <<Solvent>> The bonding material contains a solvent, which gives the bonding material fluidity and good handleability. The bonding material is typically in a paste or liquid form.
[0028] In this specification, unless otherwise specified, the term "solvent" is a concept that encompasses both a component that is liquid at room temperature and that dissolves a solute, and a component that is liquid at room temperature and that functions as a dispersion medium for dispersing a dispersoid. In this specification, "room temperature" means a temperature that is not particularly cooled or heated, that is, an ordinary temperature, and examples thereof include a temperature of 15 to 25°C.
[0029] The solvent is not particularly limited as long as it can be removed (vaporized) under heating conditions, and it is preferable that the solvent does not have reactivity with components other than the solvent, such as the metal particles (a) in the bonding material. Examples of the solvent include aromatic hydrocarbons such as toluene, o-xylene, m-xylene, and p-xylene; aliphatic hydrocarbons such as pentane, hexane, cyclohexane, heptane, octane, cyclooctane, nonane, decane, undecane, dodecane, tridecane, tetradecane, pentadecane, and decahydronaphthalene; halogenated hydrocarbons such as dichloromethane and chloroform; alcohols such as hexanol (for example, 1-hexanol), heptanol (for example, 1-heptanol), octanol (for example, 1-octanol), nonanol (for example, 1-nonanol), decanol (for example, 1-decanol), benzyl alcohol, cyclohexanol, and terpineol (also known as terpineol); esters such as ethyl acetate, monomethyl glutarate, and dimethyl glutarate; and esters such as diethyl ether, tetrahydrofuran (THF), and 1,2-dimethoxyethane (dimethyl cellosolve). alcohol ethers (compounds having both a hydroxyl group and an ether bond in one molecule) such as propylene glycol monomethyl ether (also known as 1-methoxy-2-propanol), 3-methoxy-3-methyl-1-butanol, and butyl carbitol (also known as diethylene glycol monobutyl ether); ketones such as acetone, methyl ethyl ketone (MEK), and cyclohexanone; hydroxyketones such as diacetone alcohol (also known as 4-hydroxy-4-methyl-2-pentanone); enones such as isophorone (also known as 3,5,5-trimethylcyclohex-2-en-1-one); nitriles such as acetonitrile; amides such as N,N-dimethylformamide (DMF) and N,N-dimethylacetamide; and alcohol esters (compounds having both a hydroxyl group and an ester bond in one molecule) such as texanol (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate).
[0030] The bonding material may contain only one type of solvent, or two or more types of solvents. When two or more types of solvents are contained, the combination and ratio thereof can be selected arbitrarily.
[0031] In the bonding material, the ratio of the solvent content to the total mass of the bonding material ([solvent content (parts by mass) of bonding material] / [total mass (parts by mass) of bonding material]×100) is preferably 5 to 11.5 mass%, and may be, for example, any one of 5 to 10 mass%, 7 to 11.5 mass%, and 7 to 10 mass%. When the ratio is equal to or greater than the lower limit, the viscosity of the bonding material is lowered, and the handling of the bonding material is improved. When the ratio is equal to or less than the upper limit, the content of metal particles (a) in the bonding material can be increased, the bonding portion can be formed more efficiently, and the effect of suppressing the generation of voids in the bonding portion described above is improved.
[0032] <<Other Components>> The bonding material may or may not contain other components that do not fall under either the metal particles (a) or the solvent, as long as the effects of the present invention are not impaired. The other components are not particularly limited as long as the effects of the present invention are not impaired, and can be selected as desired depending on the purpose.
[0033] The bonding material may contain only one type of other component, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.
[0034] Examples of the other components contained in the bonding material include metal particles (b) other than the metal particles (a) and a resin component. That is, the bonding material may further contain either or both of the metal particles (b) and the resin component.
[0035] <Metal Particles (b)> The metal particles (b) are different from the metal particles (a). In this embodiment, the metal particles (a) and the metal particles (b) being different from each other means, for example, that the metal species, particle size distribution, or shape of the two types of metal particles are different from each other. For example, when the metal species of the metal particles (a) is silver, the metal species of the metal particles (b) may be a metal species other than silver (e.g., copper). When the shape of the metal particles (a) is approximately spherical, the shape of the metal particles (b) may be other than approximately spherical (e.g., plate-like). The particle size distributions of the two types of metal particles being different from each other include cases where the D50s are different from each other and cases where the spreads of the particle size distributions are different from each other. When the D50s are different from each other, the particle size distribution of the mixture obtained by mixing the two types of particles will have two peak particle size portions. Furthermore, even if the D50 of two types of particles is the same, the case where the particle size distribution spreads of the two types of metal particles are different from each other is also included in the "case where the particle size distributions of metal particles (a) and metal particles (b) are different." The case where the particle size distribution spreads of two types of metal particles are different from each other refers to, for example, a case where at least one of Dmin, D10, D90, or Dmax is different from each other. In other words, the case where the particle size distribution spread when two types of particles are mixed is different from the tail spread of the particle size distribution of only one type of particle.
[0036] The metal particles (b) are not particularly limited as long as they satisfy this condition. Examples of the metal species of the metal particles (b) include those similar to those of the metal particles (a). Examples of the shape of the metal particles (b) include substantially spherical, plate-like, and the like. Examples of the metal particles (b) include metal particles having a D50 of 0.15 μm or less or metal particles having a D50 of 0.8 or more.
[0037] In this specification, the term "plate-like" refers to a metal particle having two main surfaces, and the shape of the main surfaces is an approximately polygonal shape such as a substantially triangular shape (a triangular shape or a shape that can be considered to be a triangular shape), a substantially pentagonal shape (a pentagonal shape or a shape that can be considered to be a pentagonal shape), or a substantially hexagonal shape (a hexagonal shape or a shape that can be considered to be a hexagonal shape), or an irregular shape that can be considered to be a polygonal shape with some sides or corners missing. The thickness of the plate (i.e., the width between the two main surfaces, i.e., the thickness of the plate in the direction perpendicular to the main surfaces) is 40 nm or less, and the maximum length of the two main surfaces (in other words, the particle diameter) is 10 to 1000 nm. The aspect ratio of the plate-like metal particles (= [maximum length of the main surfaces (particle diameter)] / [width between the main surfaces]) is 3 or more.
[0038] The metal species of the metal particles (b) contained in the bonding material may be one kind or two or more kinds, and when there are two or more kinds, the combination and ratio thereof can be selected arbitrarily.
[0039] The metal species of the metal particles (b) is preferably silver or copper, and is preferably silver. Note that the metal species of the metal particles (b) is not limited to pure silver or pure copper, and may be a silver alloy or a copper alloy. It is preferable that both the metal particles (a) and the metal particles (b) contained in the bonding material are silver particles.
[0040] In the bonding material, the ratio of the content of the metal particles (b) to the total mass of the bonding material ([content of metal particles (b) in bonding material (parts by mass)] / [total mass of bonding material (parts by mass)]×100) is preferably 1 mass% or less, and may be, for example, 0.5 mass% or less, 0.3 mass% or less, or 0.1 mass% or less. When the ratio is equal to or less than the upper limit, the effect obtained by using the metal particles (a) is further enhanced.
[0041] When the volume-based particle size of the metal particles in the bonding material is measured by laser diffraction / scattering particle size distribution measurement, if multiple peaks are observed in the particle size distribution, the presence of metal particles (b) can be confirmed. If the difference between the D50 of metal particles (b) and the D50 of metal particles (a) is relatively large, multiple peaks can be easily confirmed. When observing the bonding material using an SEM or the like, if metal particles having a shape other than a substantially spherical shape, such as a plate shape, are observed, the presence of metal particles (b) can be confirmed.
[0042] <Resin Component> The resin component can be selected arbitrarily depending on the purpose and is not particularly limited. The resin component may be, for example, either a curable resin or a non-curable resin, or a thermoplastic resin. The resin component may be dissolved in a solvent or dispersed in a solvent. The resin component may be a binder that contributes to bonding between metal particles or between a bonding material and an adherend, or may be spacer particles that are dispersed in a solvent and serve as spacers between metal particles. Note that resins provided on the surfaces of metal particles for chemically treating the surfaces of the metal particles are not included in the resin component of this embodiment.
[0043] It should be noted that it is not essential for the bonding material of this embodiment to contain a resin component (e.g., a binder or spacer particles). The lower the resin component content, the better. In the bonding material, the ratio of the resin component content to the total metal particle content ([resin component content (parts by mass) of the bonding material] / [total metal particle content (parts by mass) of the bonding material] × 100) is preferably less than 0.01% by mass, and may be 0.005% by mass or less. When the resin component is contained in an amount of less than 0.01% by mass, the resin component may reduce the porosity of the bonding material and suppress the occurrence of cracks. However, if the resin component remains in the fired bonding material, the remaining resin component may increase the porosity. For this reason, it is preferable that the resin component content of the bonding material be less than 0.01% by mass, or that the bonding material contain no resin component at all. Therefore, it can be said that the resin component content is preferably 0% by mass or more and less than 0.01% by mass. When the ratio is less than 0.01% by mass or when no resin component is contained, the effect of suppressing the generation of voids is further enhanced.
[0044] The resin component contained in the bonding material may be one type only, or two or more types. When two or more types are contained, the combination and ratio thereof can be selected arbitrarily.
[0045] In the bonding material, when the metal particles include metal particles (a) and metal particles (b), the ratio of the resin component content to the total content of the metal particles (a) and the metal particles (b) is [content of resin component in bonding material (parts by mass)] / [total content of metal particles (a) and metal particles (b) in bonding material (parts by mass)] × 100. Even in this case, the resin component content may be less than 0.01% by mass, for example, 0.005% by mass or less. Here, when the bonding material does not contain metal particles (b), the content of metal particles (b) in the bonding material is 0 parts by mass. Similarly, when the bonding material does not contain a resin component, the content of resin component in the bonding material is 0 parts by mass.
[0046] The bonding material may contain, as the other component, a component (X) that does not fall into either the metal particles (b) or the resin component. In this case, the ratio of the content of the other component (X) to the total mass of the bonding material ([content (parts by mass) of the component (X)] / [total mass (parts by mass) of the bonding material] × 100) is preferably 5% by mass or less, and may be, for example, 3% by mass or less or 1% by mass or less. When this ratio is equal to or less than the upper limit, the effect of suppressing the generation of voids at the bonding portion described above is further enhanced. On the other hand, the content ratio of the component (X) is 0% by mass or more.
[0047] In the bonding material, the ratio of the total content of the metal particles (a) and the solvent to the total mass of the bonding material ([total content (parts by mass) of the metal particles (a) and the solvent in the bonding material] / [total mass (parts by mass) of the bonding material]×100) is preferably 95% by mass or more, and may be, for example, 97% by mass or more or 99% by mass or more. When the ratio is equal to or more than the lower limit, the effect of suppressing the generation of voids at the bonding portion described above is further enhanced. On the other hand, the ratio of the total content of the metal particles (a) and the solvent to the total mass of the bonding material is 100% by mass or less.
[0048] As described above, the bonding material according to this embodiment includes metal particles containing metal particles (a) and a solvent for dispersing the metal particles, and the bonding material has a viscosity of 70 Pa·s or more as measured in accordance with JIS Z 3285:2017, and the particle diameter D50 of the metal particles (a) at 50% cumulative volume, as measured by laser diffraction / scattering particle size distribution measurement, is greater than 0.15 μm and less than 0.8 μm. In this configuration, the bonding material has a viscosity of 70 Pa·s or more and a D50 of greater than 0.15 μm and less than 0.8 μm, which makes it possible to suppress the generation of voids at the bonded portion.
[0049] The bonding material also has a thixotropy index in the range of 0.55 to 0.95 in accordance with JIS Z 3285: 2017. This is thought to be because, immediately after placing a conductive part on the wet bonding material, stress is applied to the bonding material, reducing the viscosity of the bonding material, which makes it easier for air bubbles generated between the wet bonding material and the conductive part to escape.
[0050] The metal particles also include metal particles (b) different from the metal particles (a), and the particle diameter D50 of the metal particles (b) at 50% cumulative volume, measured by laser diffraction / scattering particle size distribution measurement, is 0.15 μm or less or 0.8 μm or more.
[0051] The solvent may further contain a resin component that is a curable resin, a non-curable resin, or a thermoplastic resin, and the ratio of the resin component content to the metal particle content in the bonding material may be less than 0.01% by mass. Alternatively, the bonding material may not contain a resin component that is a curable resin, a non-curable resin, or a thermoplastic resin in the solvent. This makes it possible to reduce the porosity of the bonding material and suppress the occurrence of cracks and voids.
[0052] <<Method for manufacturing bonding material>> The bonding material of the present embodiment is obtained by blending metal particles (a), a solvent, and, if necessary, the other components. After blending the components, the resulting material may be used as the bonding material as is, or may be used as the bonding material after, if necessary, performing a known post-treatment or purification operation.
[0053] The order in which the components are mixed is not particularly limited. The method for mixing the components is not particularly limited, and may be appropriately selected from known methods such as a method of mixing by rotating a stirrer or stirring blades, a method of mixing using a mixer, a three-roll mill, a kneader, a bead mill, or the like, and a method of mixing by applying ultrasound.
[0054] The temperature during blending of the components is not particularly limited as long as the components do not deteriorate, but is preferably 0 to 40° C. The blending time for the components is also not particularly limited as long as the components do not deteriorate, but is preferably 10 minutes to 12 hours.
[0055] ◇Method of Manufacturing a Bonded Body A method of manufacturing a bonded body according to one embodiment of the present invention is a method of manufacturing a bonded body configured by joining a conductive first component (sometimes referred to herein simply as a “first component”) and a conductive second component (sometimes referred to herein simply as a “second component”) via a conductive bonding portion (sometimes referred to herein simply as a “bonding portion”), and includes the steps of: attaching a bonding material according to one embodiment to a first surface of the first component or a second surface of the second component (sometimes referred to herein as an “attaching step”); stacking the first component and the second component with the attached bonding material interposed therebetween to produce a laminate (sometimes referred to herein as a “laminating step”); drying the bonding material in the laminate to form a dried bonding material (sometimes referred to herein as a “drying step”); and firing the dried bonding material at a temperature higher than the temperature at which the bonding material was dried to form the bonded portion from the dried bonding material (sometimes referred to herein as a “firing step”).
[0056] The conductive parts such as the first part and the second part are not particularly limited as long as they are conductive. Examples of the conductive parts include metal parts (metal members). The metal parts may be, for example, metal layers formed by sputtering or plating on the surface of a semiconductor chip or semiconductor element such as a silicon chip, or may be metal layers such as electrodes formed on a resin substrate or a ceramic substrate.
[0057] The bonding portion is formed using the bonding material according to the embodiment described above and is a metal sintered body. For example, when the bonding material contains silver particles as the metal particles (a), the metal sintered body is a silver sintered body, and when the bonding material contains copper particles as the metal particles (a), the metal sintered body is a copper sintered body. The bonding portion has electrical conductivity and thermal conductivity and is useful as a substitute for solder.
[0058] In the manufacturing method, all steps can be performed in the atmosphere. When the constituent material of one or both of the first and second components to be joined is a metal that is easily oxidized (e.g., copper), all steps in the manufacturing method can be performed in an inert gas atmosphere. Examples of the inert gas include nitrogen gas and helium gas.
[0059] Hereinafter, the method for manufacturing a bonded body according to the present embodiment will be described with reference to the drawings. First, a bonded body to which the manufacturing method according to the present embodiment is applied will be described.
[0060] <<Jointed Body>> Fig. 1 is a cross-sectional view schematically showing an example of the joined body. The joined body 1 shown here is configured by joining a conductive first component 11 and a conductive second component 12 via a conductive joint 13. A first surface 11a of the first component 11 is in contact with the joint 13. A second surface 12a of the second component 12 is in contact with the joint 13. The joined body 1 is configured by stacking the first component 11, the joint 13, and the second component 12 in this order in the thickness direction. Hereinafter, the stacking direction of the first component 11, the joint 13, and the second component 12 will be referred to as the thickness direction.
[0061] The area of the first surface 11 a of the first component 11 is preferably equal to or greater than the area of the second surface 12 a of the second component 12 .
[0062] The first part 11 has a sheet, plate or block shape.
[0063] The first component 11 preferably contains a metal, and more preferably is made of metal. Examples of metals that form the first component 11 include silver, copper, aluminum, gold, and nickel.
[0064] The first component 11 may be made of one layer (single layer) or may be made of two or more layers. When the first component 11 is made of multiple layers, these multiple layers may be the same or different from one another, and the combination of these multiple layers is not particularly limited. In this specification, not limited to the case of the first component, "multiple layers may be the same or different from one another" means "all layers may be the same, all layers may be different, or only some layers may be the same," and further, "multiple layers are different from one another" means "at least one of the constituent materials and thicknesses of the layers is different from one another."
[0065] When the first component 11 is made up of multiple layers, for example, one or more layers on the bonding portion 13 side of the first component 11 may be layers that improve adhesion to the bonding portion 13.
[0066] There are no particular limitations on the thickness of the first component 11, and the thickness can be set arbitrarily depending on the purpose of the bonded body 1. The thickness of the first component 11 may be, for example, 10 to 10,000 μm.
[0067] When the first component 11 is made up of a plurality of layers, it is preferable that the total thickness of the layers be the thickness of the first component 11 described above.
[0068] Here, the first part 11 is shown to be in the shape of a sheet, a plate, or a block, but the first part 11 may have any other shape, and the shape of the first part 11 can be selected arbitrarily depending on the purpose.
[0069] The second part 12 is in the form of a sheet, a plate, or a block.
[0070] The second component 12 is preferably composed of a metal, and more preferably is made of metal, and examples of the metals that compose the second component 12 include the same metals that compose the first component 11 described above.
[0071] The second component 12 may be made of one layer (single layer) or may be made of two or more layers. When the second component 12 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.
[0072] When the second component 12 is made up of multiple layers, for example, one or more layers on the bonding portion 13 side of the second component 12 may be layers that improve adhesion to the bonding portion 13 .
[0073] The thickness of the second component 12 is not particularly limited and can be set arbitrarily depending on the purpose of the bonded body 1. The thickness of the second component 12 is preferably 0.05 to 10,000 μm, and may be, for example, 0.05 to 500 μm, or may be greater than 500 μm and not greater than 10,000 μm. When the second component 12 is made up of multiple layers, the total thickness of the layers is preferably the thickness of the second component 12 described above.
[0074] Here, the second part 12 is shown to be in the shape of a sheet, a plate, or a block, but the second part 12 may have any other shape, and the shape of the second part 12 can be selected arbitrarily depending on the purpose.
[0075] The joint 13 is in the form of a sheet, a plate, or a block. The joint 13 may be made of one layer (single layer), or may be made of two or more layers. When the joint 13 is made of multiple layers, these multiple layers may be the same or different from each other, and the combination of these multiple layers is not particularly limited.
[0076] It is preferable that the entire surface of the joint portion 13 on the first component 11 side be in contact with the first surface 11 a of the first component 11 .
[0077] The thickness of the bonding portion 13 may be, for example, 10 μm or more and 400 μm or less. Alternatively, the thickness may be any of 100 μm or more, 200 μm or more, and 300 μm or more. The thicker the bonding portion 13, the stronger the bonding portion 13. On the other hand, the thickness of the bonding portion 13 is preferably 400 μm or less. When the thickness of the bonding portion 13 is 400 μm or less, the bonding portion 13 can be formed more easily.
[0078] Here, the joint 13 is shown to be sheet-shaped, plate-shaped, or block-shaped, but the joint 13 may be in any other shape, and the shape of the joint 13 can be selected arbitrarily depending on the purpose.
[0079] The area of the contact region of the surface of the joining portion 13 with the first component 11 (more specifically, the first surface 11a) and the area of the contact region with the second component 12 (more specifically, the second surface 12a) may be the same or different. The area of each of the contact regions is 9 to 2500 mm 2 It is preferable that the length is 9 to 1225 mm. 2 More preferably, for example, 9 to 576 mm 2 , and 9 to 144 mm 2 or 225 to 1225 mm 2 , and 625 to 1225 mm 2 or 225 to 576 mm 2 However, these are just examples of the area of the contact area. When the area of the contact area is in the above range, the bonding strength and heat dissipation between the components 11 and 12 and the joint 13 are improved.
[0080] The area of the second surface 12a of the second component 12 is preferably 50 to 150% of the area of the surface of the joint 13 facing the second component 12. The area of the second surface 12a of the second component 12 that is in contact with the joint 13 is preferably 50 to 100% of the area of the entire second surface 12a. It is preferable that the entire surface of the joint 13 facing the first component 11 be in contact with the first component 11.
[0081] In the joined body 1, one first component 11 and one second component 12 are joined by one joint 13, but the joining form is not limited to this. In the joined body, for example, one first component and two or more second components may be joined by one joint. In this case, the two or more second components may be all the same, all different, or only partially different. In the joined body, for example, one first component and two or more second components may be joined by two or more joints. In this case, the number of second components and the number of joints may be the same or different. In addition, the two or more second components may be all the same, all different, or only partially different. The number of first components and the number of second components illustrated here may be reversed.
[0082] The bonded body to which the manufacturing method of the present embodiment is applied is not limited to that shown in FIG. 1 . For example, the bonded body 1 shown in FIG. 1 may have some components modified, deleted, or added within the scope of the present invention.
[0083] Next, the manufacturing method of this embodiment will be described by taking as an example the case of manufacturing the bonded body shown in FIG.
[0084] 2A to 2E are cross-sectional views for schematically illustrating an example of a method for manufacturing a bonded body according to this embodiment (sometimes referred to in this specification as "manufacturing method (1)"). In each figure, the same components as those shown in figures that have already been described are denoted by the same reference numerals as in the figures that have already been described, and detailed description thereof will be omitted.
[0085] 2A , in the attachment step of the manufacturing method (1), the bonding material 130 is attached to the first surface 11a of the first component 11. Examples of a method for attaching the bonding material 130 to the first component 11 include known methods such as a printing method and a coating method.
[0086] Examples of the printing method include screen printing, flexographic printing, offset printing, dip printing, inkjet printing, dispenser printing, jet dispenser printing, gravure printing, gravure offset printing, and pad printing.
[0087] Examples of the coating method include methods using various coaters such as a spin coater, an air knife coater, a curtain coater, a die coater, a blade coater, a roll coater, a gate roll coater, a bar coater, a rod coater, and a gravure coater; methods using a wire bar; and methods using a coating device such as a slot die.
[0088] When the bonding material 130 is applied to the first component 11, a mask such as a metal mask may be used to apply the bonding material 130 only to the desired locations.
[0089] <<Laminating Step>> After the attaching step of manufacturing method (1), in the laminating step, as shown in Fig. 2B , the first component 11 and the second component 12 are laminated via the attached bonding material 130 to produce a laminated body 101. That is, the laminated body 101 is configured by laminating the first component 11, the bonding material 130, and the second component 12 in this order in the thickness direction. The first component 11 is in contact with the bonding material 130 at its first surface 11a. The second component 12 is in contact with the bonding material 130 at its second surface 12a.
[0090] In the lamination process, when the second component 12 is placed on the undried bonding material 130 , the generation of voids between the bonding material 130 and the second component 12 is suppressed.
[0091] When producing the laminate 101, for example, the second component 12 is placed above the exposed surface of the bonding material 130 (i.e., the surface opposite to the side in contact with the first component 11) at a position spaced apart from the exposed surface, and the second component 12 is dropped from this position to place the second component 12 on the bonding material 130, thereby producing the laminate 101. In this specification, this method of stacking the first component 11, the bonding material 130, and the second component 12 in this manner may be referred to as the "stacking method (i)."
[0092] When producing the laminate 101, for example, the second component 12 may be pressed against the exposed surface of the bonding material 130 (i.e., the surface opposite to the surface in contact with the first component 11) with light pressure, and then the pressure on the second component 12 may be released and the second component 12 may be placed on the bonding material 130, thereby producing the laminate 101. In this specification, this method of stacking the first component 11, the bonding material 130, and the second component 12 may be referred to as the "stacking method (ii)."
[0093] It is estimated that when lamination method (i) is employed, the viscosity of the bonding material 130 is more likely to decrease at the initial stage of contact between the second component 12 and the bonding material 130 than when lamination method (ii) is employed. In this way, when lamination method (i) and lamination method (ii) are compared, it is estimated that the state of the bonding material 130 is different at the initial stage of contact between the second component 12 and the bonding material 130. However, in the manufacturing method, whichever method is employed, the generation of voids is suppressed in the finally formed bonded portion.
[0094] <<Drying Step>> After the lamination step of the manufacturing method (1), in the drying step, the bonding material 130 in the laminate 101 is dried to form a dried bonding material 130′, as shown in Fig. 2C . The drying step volatilizes the solvent in the bonding material 130, so that the dried bonding material 130′ does not contain any solvent or has a significantly reduced solvent content compared to the bonding material 130.
[0095] The dried bonding material 130' is not a metal sintered body and typically does not have the luster characteristic of metal, and this external appearance feature also makes it possible to distinguish it from the target metal sintered body.
[0096] The bonding material 130 can be dried by a known method, and is preferably dried by heating under normal pressure.
[0097] The heating temperature (drying temperature) of the bonding material 130 in the drying process can be adjusted appropriately depending on the type of solvent, but is preferably 70°C or higher, and may be, for example, 100°C or higher. A heating temperature above the lower limit allows the bonding material 130 to dry more quickly. Furthermore, since the solvent can be sufficiently evaporated in the drying process, bumping due to residual solvent can be prevented in the firing process described below, thereby suppressing the generation of voids. On the other hand, the heating temperature is preferably 130°C or lower. A heating temperature below the upper limit suppresses deterioration of the dried bonding material 130' and also suppresses adverse effects caused by gas (volatilized solvent) escaping from the inside of the bonding material 130. Furthermore, for example, if the drying temperature is excessively high, metal particles may neck (fuse) together before the firing process, making it difficult to reduce pores during pressurization. Therefore, the above-mentioned heating temperature is preferred.
[0098] The heating time (drying time) of the bonding material 130 in the drying step can be adjusted appropriately depending on the heating temperature, but is preferably 1 to 40 minutes, and may be, for example, 3 to 30 minutes or 5 to 20 minutes. By setting the heating time within this range, the desired dried bonding material 130' can be formed more efficiently.
[0099] The thickness of the dried bonding material 130' may be, for example, 10 μm or more and 400 μm or less. Alternatively, the thickness may be any of 100 μm or more, 200 μm or more, and 300 μm or more. On the other hand, the thickness of the dried bonding material 130' is preferably 400 μm or less. When the thickness of the dried bonding material 130' is 400 μm or less, it becomes easier to form the dried bonding material 130'.
[0100] 2D , in the firing step after the drying step of the manufacturing method (1), the dried bonding material 130′ in the laminate 101 is fired at a temperature (sometimes referred to as a “firing temperature” in this specification) higher than the temperature at which the bonding material 130 was dried. When the bonding material 130 is dried by heating, the firing temperature of the dried bonding material 130′ (the firing temperature) is set higher than the heating temperature (drying temperature) of the bonding material 130.
[0101] When the dried bonding material 130' is fired, the temperature rise rate of the dried bonding material 130' during heating is not particularly limited, but is preferably 30 to 70°C / min, and may be, for example, 40 to 60°C / min. When the temperature rise rate is in such a range, a metal sintered body (bonding portion 13) having the desired characteristics can be produced more efficiently.
[0102] The firing temperature of the dried bonding material 130′ (the temperature at which the metal particles (a) are sintered) is preferably 180°C or higher, and may be, for example, any one of 200°C or higher, 220°C or higher, and 240°C or higher. When the firing temperature is equal to or higher than the lower limit, a metal sintered body (bonding portion 13) with higher purity can be obtained. On the other hand, the firing temperature of the dried bonding material 130′ is preferably 320°C or lower, and may be, for example, any one of 300°C or lower and 280°C or lower, in order to prevent excessive heating and obtain a metal sintered body (bonding portion 13) with good properties.
[0103] The firing time of the dried bonding material 130' (the time for sintering the metal particles (a)) is preferably 3 to 120 minutes, and may be, for example, 3 to 60 minutes, 50 to 90 minutes, or 80 to 120 minutes. By setting the firing time (sintering time) within this range, a metal sintered body with the desired characteristics can be more efficiently manufactured. In the firing step, it is preferable to fire the dried bonding material 130' at a firing temperature within the above-mentioned numerical range and for a firing time within the numerical range shown here.
[0104] In the firing step, the dried bonding material 130′ is preferably fired (sometimes referred to as “pressure firing” in this specification) while pressurizing the laminate 101 in its thickness direction (in other words, the stacking direction of the first component 11, the dried bonding material 130′, and the second component 12). By pressurizing and firing the dried bonding material 130′ in this manner, a bonded portion with fewer voids can be formed.
[0105] When the laminate 101 is pressed in its thickness direction (in other words, in the stacking direction of the first component 11, the dried bonding material 130′, and the second component 12), the pressure applied to the laminate 101 is a pressure P 1 and the pressure P applied from the second component 12 side. 2 In this specification, "pressurization" means increasing the pressure applied to an object by actively applying force to the object, and for example, simply supporting the object (applying normal force) without actively applying force is not considered pressurization. In the case of pressurization, for example, the position of the pressurizing means changes by itself with acceleration.
[0106] During pressurized firing, heating for firing the dried bonding material 130′ (laminate 101) and pressurizing the dried bonding material 130′ (laminate 101) may be started simultaneously, or heating for firing the dried bonding material 130′ may be started before pressurizing the dried bonding material 130′, or heating for firing the dried bonding material 130′ may be started before pressurizing the dried bonding material 130′.
[0107] The pressure applied to the dried bonding material 130' during pressure firing is preferably 20 MPa or less, and may be, for example, 16 MPa or less. When the pressure is equal to or less than the upper limit, damage such as cracking and deformation of the first component 11 or the second component 12 are further suppressed. On the other hand, the pressure during pressure firing is preferably 1 MPa or more, in order to more effectively obtain the effect of pressing, for example, by reducing voids in the bonding portion. Here, the pressure applied to the dried bonding material 130' (the pressure during pressure firing) is the load applied to the laminate 101 during pressing divided by the area of the region of the dried bonding material 130' that receives this load. The pressure P applied from the first component 11 side 1 and the pressure P applied from the second component 12 side. 2 When both of the pressures P and P are applied to the bonding material 130′, the pressure during pressurized firing per unit area is 1 / Pressure P 1 The area of the first surface 11a receiving the pressure P 2 / Pressure P 2 (area of the second surface 12a that receives the load).
[0108] 2E, the firing step forms the bonding portion 13 from the dried bonding material 130′, thereby obtaining the desired bonded body 1. The bonding portion 13 is a metal sintered body formed from the bonding material 130 via the dried bonding material 130′.
[0109] The use of the bonding material 130 suppresses the generation of voids in the bonding portion 13. As a result, the conductivity and strength of the bonding portion 13 are high.
[0110] So far, we have explained a method for manufacturing a bonded body (manufacturing method (1)) in which the bonding material is attached to a first surface of a first component and a bonded joint is formed from this bonding material. However, the manufacturing method of this embodiment may also be a method for manufacturing a bonded body (sometimes referred to in this specification as "manufacturing method (2)") in which the bonding material is attached to a second surface of a second component and a bonded joint is formed from this bonding material.
[0111] Manufacturing Method (2) FIGS. 3A to 3E are cross-sectional views for schematically illustrating another example of the manufacturing method for the bonded body of this embodiment, that is, the manufacturing method (2).
[0112] 3A , in the attachment step of the manufacturing method (2), the bonding material 130 is attached to the second surface 12 a of the second component 12. The attachment step in the manufacturing method (2) can be performed in the same manner as the attachment step in the manufacturing method (1), except that the bonding material 130 is attached to the second surface 12 a of the second component 12, not the first surface 11 a of the first component 11.
[0113] <<Lamination Step>> After the attachment step of manufacturing method (2), in the lamination step, as shown in Fig. 3B , the first component 11 and the second component 12 are laminated via the attached bonding material 130 to produce a laminated body 102. That is, the laminated body 102 is configured by laminating the first component 11, the bonding material 130, and the second component 12 in this order in the thickness direction. The first component 11 is in contact with the bonding material 130 at its first surface 11a. The second component 12 is in contact with the bonding material 130 at its second surface 12a.
[0114] In the lamination process, when the first component 11 is placed on the undried bonding material 130 , the generation of voids between the bonding material 130 and the first component 11 is suppressed.
[0115] The laminate 102 is the same as the laminate 101 in manufacturing method (1), except that very small voids may exist between the bonding material 130 and the first component 11, rather than between the bonding material 130 and the second component 12.
[0116] The lamination process in manufacturing method (2) can be performed in the same manner as the lamination process in manufacturing method (1), except that the second part 12 having the bonding material 130 is used instead of the first part 11 having the bonding material 130, and the first part 11 not having the bonding material 130 is used instead of the second part 12 not having the bonding material 130.
[0117] <<Drying Step>> After the lamination step of manufacturing method (2), in the drying step, the bonding material 130 in the laminate 101 is dried to form a dried bonding material 130', as shown in Fig. 3C. The drying step in manufacturing method (2) can be performed in the same manner as the drying step in manufacturing method (1). The dried bonding material 130' formed in manufacturing method (2) is the same as the dried bonding material 130' formed in manufacturing method (1).
[0118] <<Firing Step>> After the lamination step of manufacturing method (2), in the firing step, the dried bonding material 130' in the laminate 102 is fired at a temperature higher than the temperature at which the bonding material 130 was dried, as shown in Fig. 3D. The firing step in manufacturing method (2) can be performed in the same manner as in the firing step in manufacturing method (1). In the firing step in manufacturing method (2), it is also preferable to pressurize and fire the dried bonding material 130'.
[0119] By carrying out the firing step of the manufacturing method (2), as shown in FIG. 3E, the joint 13 is formed from the dried joining material 130′, and the desired joined body 1 is obtained. The joint 13 is a metal sintered body formed from the joining material 130 via the dried joining material 130′. The joined body 1 obtained by the manufacturing method (2) is the same as the joined body 1 obtained by the manufacturing method (1).
[0120] In the case of manufacturing method (2), the use of the bonding material 130 also suppresses the generation of voids in the bonding portion 13. As a result, the conductivity and strength of the bonding portion 13 are high.
[0121] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the examples shown below.
[0122] The metal particles (a) used in the following examples and comparative examples are all silver particles produced by a reduction method.
[0123] Example 1 Production of Bonding Material Metal particles (a)-1 (approximately spherical silver particles) (92 parts by mass) whose metal species, shapes, and particle size distribution are shown in Table 1 and Texanol (8 parts by mass) were weighed into an agate mortar at room temperature and kneaded for 15 minutes. The kneaded mixture was then passed through a triple roll mill three times to obtain the desired paste-like bonding material.
[0124] <<Evaluation of Bonding Material>> Using a micro spiral viscometer ("PCU-02V" manufactured by Malcom), the viscosity of the bonding material was measured at a temperature of 25°C and a rotation speed of 10 rpm (shear rate 6 / s) in accordance with JIS Z 3285:2017. Furthermore, the thixotropy index of the bonding material was measured in accordance with JIS Z 3285:2017. The results are shown in Table 1.
[0125] <<Production of Bonded Body>> An oxygen-free copper plate having a size of 20 mm × 20 mm and a thickness of 1 mm was prepared. A metal mask plate having a thickness of 50 μm was placed on one surface of the oxygen-free copper plate, and a rectangular shape having a size of 5.8 mm × 5.8 mm was printed using the bonding material. In this way, the rectangular bonding material was attached to the surface of the oxygen-free copper plate (attachment process).
[0126] A silicon carbide (SiC) chip having a size of 4.8 mm x 4.8 mm and a thickness of 0.35 mm was prepared, with a 50 nm titanium film, a 100 nm nickel film, and a 100 nm gold film laminated in this order on one side (i.e., the back side) by sputtering. Using a semi-automatic mounter (LPKF "ProtoPlace S"), the backside silicon carbide chip was picked up by suction, and the suction was released about 2 mm above the bonding material on the surface of the oxygen-free copper plate. From this position, the backside silicon carbide chip was dropped onto the bonding material, and the backside silicon carbide chip was placed on the bonding material (lamination method (i)). As a result, a laminate was produced in which the oxygen-free copper plate, the bonding material, and the backside silicon carbide chip were stacked in this order in the thickness direction (lamination process). At this time, the entire exposed surface of the gold film in the backside-coated silicon carbide chip was brought into contact with the bonding material.
[0127] Next, the laminate was heated at 110°C for 10 minutes using a hot air circulation oven to volatilize the Texanol in the bonding material and dry it, forming a dried bonding material in the form of a film having a rectangular planar shape, and the laminate was used as a dried laminate (drying step). Next, a carbon sheet ("PERMA-FOIL (registered trademark)" manufactured by Toyo Tanso Co., Ltd.) was placed as a buffer material on the surface of the silicon carbide chip in the backside-coated silicon carbide chip of the dried laminate.
[0128] Next, using a servo press, the dried laminate with the carbon sheet obtained above was pressed in the thickness direction. Pressurization of the dried bonding material was initiated at a pressure of 15 MPa, and simultaneously heating was initiated at a temperature increase rate of approximately 50°C / min. The dried laminate with the carbon sheet was placed between a pair of press plates in the servo press. The pair of press plates included a first press plate located on the backside silicon carbide chip side of the laminate with the carbon sheet, and a second press plate located on the oxygen-free copper plate side. The first press plate was fixed to the servo press. The second press plate was then moved toward the first press plate, supporting the dried laminate with the carbon sheet with the first press plate, while applying pressure to the dried laminate with the carbon sheet from the oxygen-free copper plate side. That is, pressure was applied to the dried laminate with the carbon sheet from the oxygen-free copper plate side. After the heating temperature (in other words, the temperature of the laminate) reached 250°C, this temperature was maintained for 5 minutes. That is, the dried bonding material was heated and pressed at a temperature of 250°C and a pressure of 15 MPa for 5 minutes. In this way, the dried bonding material was pressurized and fired to form a bonded portion from the dried bonding material (firing process). Next, cooling was initiated by flowing cooling water inside the servo press, and the pressure was released when the temperature of the laminate reached 60°C. This resulted in the desired bonded body. The thickness of the bonded portion in the bonded body was 27 μm.
[0129] <<Evaluation of Bonded Article>> <Evaluation of Effect of Suppressing Void Generation at Bonded Portion> The presence or absence of voids at the bonded portion of the bonded article obtained above was confirmed using an ultrasonic flaw detector (SAT). The results are shown in Table 1.
[0130] <<Production and Evaluation of Bonding Material, Production and Evaluation of Bonded Body>> [Example 2] A bonding material was produced and evaluated, and a bonded body was produced and evaluated in the same manner as in Example 1, except that metal particles (a)-2 (approximately spherical silver particles) (92 parts by mass) were used instead of metal particles (a)-1 (92 parts by mass) as shown in Table 1. The results are shown in Table 1. The thickness of the bonded portion in the bonded body was 26 μm.
[0131] Example 3 <<Production and Evaluation of Bonding Material>> In this example, the bonding material obtained in Example 2 was used, and therefore detailed description of the bonding material will be omitted.
[0132] <<Production of Bonded Body>> A bonding material was attached to the surface of an oxygen-free copper plate in the same manner as in Example 1 (attaching step).
[0133] A silicon carbide chip having a back surface formed thereon was prepared as in Example 1. Using a semi-automatic mounter ("ProtoPlace S" manufactured by LPKF), the silicon carbide chip having a back surface formed thereon was picked up by suction, and the chip was lightly pressed against the bonding material on the surface of the oxygen-free copper plate, and then the suction was released, thereby placing the silicon carbide chip on the bonding material. This resulted in a laminate consisting of the oxygen-free copper plate, the bonding material, and the silicon carbide chip having a back surface formed thereon, stacked in this order in the thickness direction (lamination process). At this time, the entire exposed surface of the gold film in the silicon carbide chip having a back surface formed thereon was brought into contact with the bonding material. Hereinafter, in this specification, the lamination method in which the silicon carbide chip having a back surface formed thereon is lightly pressed against the bonding material and placed thereon is sometimes referred to as "lamination method (ii)."
[0134] The drying and firing processes were then carried out in the same manner as in Example 1, and the laminate was allowed to cool and the pressure was released to obtain the desired bonded body. That is, this example was the same as Example 2, except that the method of placing the backside-coated silicon carbide chip on the bonding material was changed. The thickness of the bonded portion in the bonded body was 23 μm.
[0135] <<Evaluation of Bonded Structure>> The bonded structure obtained above was evaluated in the same manner as in Example 1. The results are shown in Table 1.
[0136] <<Production and Evaluation of Bonding Material, Production and Evaluation of Bonded Body>> [Example 4] A bonding material was produced and evaluated, and a bonded body was produced and evaluated in the same manner as in Example 3, except that metal particles (a)-3 (approximately spherical silver particles) (92 parts by mass) were used instead of metal particles (a)-2 (92 parts by mass) as shown in Table 1. The results are shown in Table 1. The thickness of the bonded portion in the bonded body was 22 μm.
[0137] Example 5 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 2, except that the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 91 parts by mass, and the blending amount of Texanol was changed from 8 parts by mass to 9 parts by mass, as shown in Table 2. The results are shown in Table 2. The thickness of the bonded portion in the bonded body was 25 μm.
[0138] Example 6 A bonding material was produced and evaluated, and a bonded body was produced and evaluated in the same manner as in Example 1, except that metal particles (a)-4 (approximately spherical silver particles) (92 parts by mass) were used instead of metal particles (a)-1 (92 parts by mass) as shown in Table 2. The results are shown in Table 1. The thickness of the bonded portion in the bonded body was 28 μm.
[0139] Comparative Example 1 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 2, except that the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 87 parts by mass, and the blending amount of Texanol was changed from 8 parts by mass to 13 parts by mass, as shown in Table 2. The results are shown in Table 2. The thickness of the bonded portion in the bonded body was 17 μm.
[0140] Comparative Example 2 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 3, except that the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 87 parts by mass, and the blending amount of Texanol was changed from 8 parts by mass to 13 parts by mass, as shown in Table 2. The results are shown in Table 2. The thickness of the bonded portion in the bonded body was 11 μm.
[0141] Comparative Example 3 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 2, except that, as shown in Table 3, the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 89 parts by mass, the blending amount of Texanol was changed from 8 parts by mass to 11 parts by mass, and the drying temperature was changed from 110°C to 80°C. The results are shown in Table 3. The thickness of the bonded portion in the bonded body was 22 μm.
[0142] Comparative Example 4 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 2, except that the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 89 parts by mass, and the blending amount of Texanol was changed from 8 parts by mass to 11 parts by mass, as shown in Table 3. The results are shown in Table 3. The thickness of the bonded portion in the bonded body was 22 μm.
[0143] Comparative Example 5 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 2, except that, as shown in Table 3, the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 90 parts by mass, the blending amount of Texanol was changed from 8 parts by mass to 10 parts by mass, and the drying temperature was changed from 110°C to 80°C. The results are shown in Table 3. The thickness of the bonded portion in the bonded body was 24 μm.
[0144] Comparative Example 6 A bonding material and a bonded body were produced and evaluated in the same manner as in Example 2, except that the blending amount of metal particles (a)-2 was changed from 92 parts by mass to 90 parts by mass, and the blending amount of Texanol was changed from 8 parts by mass to 10 parts by mass, as shown in Table 3. The results are shown in Table 3. The thickness of the bonded portion in the bonded body was 21 μm.
[0145]
[0146]
[0147]
[0148] As is clear from the above results, in Examples 1 to 6, when manufacturing the bonded body, even if the backside-coated silicon carbide chip (second component) was placed on the undried bonding material, and then the bonding material was dried and fired, the generation of voids at the bonded portion was suppressed. As is clear from Examples 2 and 3, even if the lamination method in the lamination process was changed (whether lamination method (i) or lamination method (ii)), the generation of voids at the bonded portion was suppressed.
[0149] In Examples 1 to 6, the D50 of the metal particles (a) was 0.33 to 0.48 μm, and the viscosity of the bonding material was 70 Pa·s or more (70 to 162.7 Pa·s).
[0150] In Examples 1 to 6, the D90 of the metal particles (a) was 0.75 μm or less (0.58 to 0.75 μm), and the D10 of the metal particles (a) was 0.22 μm or more (0.22 to 0.32 μm), and it was presumed that the bonding material had more preferable properties.
[0151] In contrast, in Comparative Examples 1 to 6, even when the lamination method in the lamination process was changed (whether lamination method (i) or lamination method (ii)), the generation of voids at the joints could not be suppressed. In Comparative Example 1, many streak-like voids occurred at the joints, and in Comparative Example 2, many point-like voids occurred at the joints. In Comparative Examples 1 to 6, the viscosity of the bonding material was 34.8 to 63.4 Pa s.
[0152] The present invention can be used to manufacture conductive junctions, particularly semiconductor devices.
[0153] REFERENCE SIGNS LIST 1... Bonded body, 11... First part, 11a... First surface, 12... Second part, 12a... Second surface, 13... Bonding portion, 130... Bonding material, 130'... Dried bonding material, 101, 102... Laminate
Claims
1. A bonding material for bonding conductive parts, comprising: metal particles containing metal particles (a); and a solvent for dispersing the metal particles, wherein the bonding material has a viscosity of 70 Pa·s or more as measured in accordance with JIS Z 3285:2017; and the metal particles (a) have a 50% cumulative volumetric particle diameter D50 of more than 0.15 μm and less than 0.8 μm as measured by a laser diffraction / scattering particle size distribution measurement.
2. The bonding material according to claim 1, wherein the metal particles (a) are silver particles.
3. The bonding material according to claim 1 or 2, wherein the bonding material has a thixotropy index in accordance with JIS Z 3285:2017 in the range of 0.55 to 0.
95.
4. The bonding material according to claim 1 or 2, wherein the metal particles have metal particles (b) different from the metal particles (a), and the particle diameter D50 of the metal particles (b) at 50% accumulation on a volume basis, as measured by laser diffraction / scattering particle size distribution measurement, is 0.15 μm or less or 0.8 μm or more.
5. The bonding material according to claim 1 or 2, further comprising a resin component in the solvent, which is a curable resin, a non-curable resin, or a thermoplastic resin, and wherein the ratio of the content of the resin component to the content of the metal particles in the bonding material is less than 0.01 mass%.
6. The bonding material according to claim 1 or 2, wherein the bonding material does not contain a resin component in the solvent that is a curable resin, a non-curable resin, or a thermoplastic resin.
7. A method for manufacturing a bonded body in which a conductive first part and a conductive second part are bonded via a conductive joint, comprising the steps of: attaching the bonding material according to claim 1 or 2 to a first surface of the first part or a second surface of the second part; stacking the first part and the second part via the attached bonding material to produce a laminate; drying the bonding material in the laminate to form a dried bonding material; and forming the joint from the dried bonding material by firing the dried bonding material at a temperature higher than the temperature at which the bonding material was dried.
Citation Information
Patent Citations
Water heater
JP2023071341A
Binding material, binding body, and binding method
WO2012070262A1
Silver powder for sintered conductive paste
JP2013119651A
Method for manufacturing bonded body
JP2021055185A
Silver paste and joined body production method
WO2020004342A1