Ruthenium complex, method for producing silyl group-containing compound, silyl group-containing polymer mixture, curable composition, and cured product
The use of a ruthenium complex with a specific ligand in hydrosilylation reactions improves the efficiency and selectivity of silyl group introduction, addressing the limitations of existing methods and enhancing the mechanical properties of the cured products.
Patent Information
- Application Number
- PCT/JP2024/015650
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-09-01
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-31
AI Technical Summary
The existing methods for hydrosilylation reactions using metal catalysts, such as Karstedt's catalyst, face limitations due to side reactions like isomerization and hydrogenation, which reduce the efficiency of introducing silyl groups into allyl group-containing compounds, especially for high molecular weight compounds, resulting in lower modulus and tensile strength of the cured products.
A ruthenium complex with a specific ligand having a carbon-carbon double bond and an electron-withdrawing group is used as a catalyst in the hydrosilylation reaction, allowing for efficient introduction of silyl groups into allyl group-containing compounds regardless of their molecular weight, thereby reducing side reactions and improving the properties of the cured products.
This approach enhances the selectivity and efficiency of silyl group introduction, leading to higher modulus and tensile strength of the cured products, even for high molecular weight compounds, and reduces the formation of by-products like 1-propenyl groups.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Ruthenium complex, method for producing silyl group-containing compound, silyl group-containing polymer mixture, curable composition, and cured product
[0001] The present invention relates to a ruthenium complex, a method for producing a silyl group-containing compound, a silyl group-containing polymer mixture, a curable composition, and a cured product.
[0002] Organic polymers containing silicon atoms, particularly organic polymers containing silyl groups (hereinafter referred to as "hydrolyzable silyl groups") that have hydroxyl groups or hydrolyzable groups on the silicon atoms and can form siloxane bonds, are known as moisture-reactive polymers. These polymers cure through a hydrolysis reaction to form flexible rubber-like cured products, and are therefore used in many industrial products, such as sealants, adhesives, coating materials, paints, and pressure-sensitive adhesives.
[0003] A commonly known method for obtaining such silyl group-containing organic polymers is the hydrosilylation reaction of an allyl group-containing organic polymer with a hydrosilane compound in the presence of a metal catalyst. However, a common problem with hydrosilylation of allyl group-containing compounds using a metal catalyst is the occurrence of side reactions such as isomerization to 1-propenyl groups (internal olefins) and hydrogenation during the reaction. When the widely used Karstedt catalyst (platinum divinyldisiloxane complex) is used in the hydrosilylation reaction of allyl group-containing organic polymers, the above-mentioned side reactions proceed at a rate of approximately 20%, limiting the rate of silyl group introduction. As a result, the resulting rubber-like cured product obtained by curing a curable composition containing a hydrolyzable silyl group-containing organic polymer leaves room for improvement in terms of modulus, tensile strength, etc.
[0004] On the other hand, in addition to platinum catalysts such as Karstedt's catalyst, metal catalysts that exhibit good activity in hydrosilylation are known, one of which is a ruthenium catalyst. Patent Document 1 reports that the reaction of an allyl ether compound with a hydrosilane compound in the presence of a specific ruthenium complex can efficiently produce the corresponding silylated product. However, when the allyl ether compound has a high molecular weight, the side reaction rate increases, resulting in a decrease in selectivity for the silylated product, and therefore the production of the silylated product was limited to a molecular weight of 3,000 or less.
[0005] Japanese Patent Application Laid-Open No. 2021-11456
[0006] An object of the present invention is to provide a ruthenium complex that can efficiently introduce a silyl group into an allyl group-containing compound in a hydrosilylation reaction thereof, regardless of the molecular weight of the allyl group-containing compound, and a method for producing the silyl group-containing compound.
[0007] As a result of extensive research, the present inventors have found that by carrying out the hydrosilylation reaction of an allyl group-containing compound in the presence of a ruthenium catalyst having a specific compound as a ligand, a silylated product can be efficiently produced, regardless of the molecular weight of the allyl group-containing compound.Furthermore, they have found that by adding a specific compound in advance to the hydrosilylation reaction of an allyl group-containing compound using a known ruthenium catalyst, a silylated product can also be efficiently produced, regardless of the molecular weight of the allyl group-containing compound.This finding led to the present invention.
[0008] That is, the present invention relates to a ruthenium complex (A) having a compound (B) as a ligand, wherein compound (B) has at least one carbon-carbon double bond in one molecule, and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it. The present invention also relates to a hydrosilylation reaction catalyst containing the ruthenium complex (A). The present invention also relates to a method for producing a silyl group-containing compound (E), which includes the step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), and the hydrosilylation reaction catalyst and conducting a hydrosilylation reaction. Furthermore, the present invention also relates to a method for producing a silyl group-containing compound (E), which includes a step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), a ruthenium compound (A') that does not have compound (B) as a ligand, and compound (B) to cause a hydrosilylation reaction, wherein compound (B) has at least one carbon-carbon double bond in one molecule and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it. The present invention also relates to a polymer mixture containing a hydrolyzable silyl group-containing polymer and the ruthenium complex (A); a curable composition containing the polymer mixture and a curing catalyst; and a cured product obtained by curing the curable composition.
[0009] According to the present invention, there are provided a ruthenium complex that can efficiently introduce silyl groups into an allyl group-containing compound, regardless of the molecular weight of the allyl group-containing compound, when used as a catalyst in the hydrosilylation reaction between an allyl group-containing compound and a hydrosilane compound, and a hydrosilylation reaction catalyst containing the ruthenium complex. Furthermore, according to the present invention, there is provided a method for producing a silyl group-containing compound that can efficiently introduce silyl groups into the allyl group-containing compound and a hydrosilane compound in the hydrosilylation reaction. Furthermore, there are provided a hydrolyzable silyl group-containing polymer mixture into which silyl groups have been introduced with high efficiency, which is obtained by the production method of the present invention, and a curable composition containing the same. Furthermore, there is provided a cured product obtained by curing the curable composition.
[0010] Embodiments of the present invention are described in detail below. Ruthenium complex (A) according to one embodiment of the present invention has compound (B) as a ligand, and compound (B) has at least one carbon-carbon double bond per molecule, and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it. Compared to known ruthenium catalysts, such ruthenium complex (A) exhibits higher selectivity when used as a catalyst for the hydrosilylation reaction of an allyl group-containing compound with a hydrosilane compound, suppresses the by-production of 1-propenyl groups or hydrogenated products (propyl groups), and enables the efficient production of the corresponding silylated product, even if the silylated product is a high-molecular-weight product having a number-average molecular weight exceeding 3,000. Hereinafter, "ruthenium complex (A)" and "compound (B)" are described in detail.
[0011] <Ruthenium Complex (A)> The ruthenium complex (A) according to one embodiment of the present invention is a ruthenium complex having a compound (B) as a ligand. The specific type of the ruthenium complex (A) is not particularly limited, except that it has a compound (B) as a ligand. The type of compound (B) that the ruthenium complex (A) has as a ligand may be one type or two or more types.
[0012] (Method for Producing Ruthenium Complex (A)) Ruthenium complex (A) can be produced by a method similar to a known production method. Examples of raw materials for ruthenium complex (A) include anhydrides and hydrates of compounds selected from ruthenium chloride (III), ruthenium bromide (III), and ruthenium iodide (III). A specific method for producing ruthenium complex (A) is, for example, adding compound (B) to an ethanol solution of ruthenium chloride (III) hydrate, heating under reflux, filtering, and then drying. When ruthenium chloride (III) hydrate is used as the raw material, heating under reflux may be performed in the presence of a basic compound such as sodium carbonate or sodium bicarbonate to neutralize the hydrogen chloride generated during heating under reflux. When reacting ruthenium chloride (III) hydrate with compound (B), it is preferable to use compound (B) in an amount of 1 molar equivalent or more relative to the raw ruthenium compound from the viewpoint of the reaction rate.
[0013] Furthermore, ruthenium complex (A) may have, as a ligand, compound (B) together with compound (B'), which does not fall under compound (B). Compound (B') is a compound that can be coordinated to ruthenium complex (A), but is a compound that does not fall under compound (B). Compound (B') that can serve as a ligand is not particularly limited, and examples thereof include a 2,5-norbornadiene ligand, a 1,5-cyclooctadiene ligand, a p-cymene ligand, a mesitylene ligand, a benzene ligand, a carbonyl ligand, an isocyanide ligand, and an arene ligand.
[0014] When ruthenium complex (A) has both compound (B) and compound (B') as ligands, it is preferable that the proportion of compound (B) in all ligands of ruthenium complex (A) is as high as possible, since this can provide better selectivity. The proportion of compound (B) in all ligands is preferably 1 to 100 mol%, more preferably 50 to 100 mol%, even more preferably 70 to 100 mol%, and even more preferably 90 to 100 mol%.
[0015] Ruthenium complex (A) having compound (B) as a ligand can also be obtained by adding compound (B) to a system containing ruthenium compound (A') that does not have compound (B) as a ligand, thereby converting ruthenium compound (A') into ruthenium complex (A), by the method described below.
[0016] <Compound (B)> Compound (B) according to one embodiment of the present invention is a compound capable of coordinating to a ruthenium complex. Compound (B) has at least one carbon-carbon double bond in one molecule, and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it.
[0017] Examples of the basic skeleton containing a carbon-carbon double bond in compound (B) include a norbornadiene skeleton, a cyclooctadiene skeleton, a benzene ring skeleton, a benzoquinone skeleton, etc. More specific examples include a 2,5-norbornadiene skeleton, a 1,5-cyclooctadiene skeleton, a p-cymene skeleton, a mesitylene skeleton, a benzene ring skeleton, a benzoquinone skeleton, etc. A norbornadiene skeleton or a benzene ring skeleton is preferred.
[0018] Examples of the electron-withdrawing group include halogeno groups such as a fluoro group, a chloro group, a bromo group, and an iodo group, as well as a cyano group, an aldehyde group, and a nitro group. When a single molecule contains multiple electron-withdrawing groups, the electron-withdrawing groups may be different types. Compound (B) may contain one or more electron-withdrawing groups in a single molecule, but preferably contains two or more, more preferably two to four, and particularly preferably two or three.
[0019] Furthermore, the type of electron-withdrawing group is preferably a halogeno group, more preferably a fluoro group, a bromo group, or an iodo group, even more preferably a bromo group or an iodo group, and particularly preferably a bromo group. In particular, compound (B) preferably has one or more electron-withdrawing groups selected from a fluoro group, a bromo group, and an iodo group per molecule, more preferably two or more. Furthermore, compound (B) preferably has one or more electron-withdrawing groups selected from a bromo group and an iodo group per molecule. In this case, compound (B) may further have a fluoro group in addition to a bromo group and / or an iodo group. These electron-withdrawing groups are preferably directly bonded to the carbon atom forming the carbon-carbon double bond of compound (B). In particular, when compound (B) has a benzene ring skeleton, these electron-withdrawing groups are preferably directly bonded to the benzene ring.
[0020] The structure of compound (B) is a combination of the above-described basic skeleton and an electron-withdrawing group. The specific type of compound (B) is not particularly limited, and examples thereof include 2-bromonorbornadiene, 2,3-dibromonorbornadiene, 1,4-dibromobenzene and its structural isomers, 1-bromo-4-iodobenzene and its structural isomers, 1,3,5-tribromobenzene and its structural isomers, 1,2,4,5-tetrabromobenzene and its structural isomers, hexabromobenzene, 1-bromo-3,5-difluorobenzene and its structural isomers, 1-bromo-3,5-dichlorobenzene and its structural isomers, 1-bromo-3,5-diiodobenzene and its structural isomers, 1-bromo-3-chloro-5-fluorobenzene and its structural isomers, 1,4-diiodobenzene and its structural isomers, 1,3,5-triiodobenzene and its structural isomers, 1,2 , 4,5-tetraiodobenzene and its structural isomers, hexaiodobenzene, 1,3-difluoro-5-iodobenzene and its structural isomers, 1,3-dichloro-5-iodobenzene and its structural isomers, 1,3-dibromo-5-iodobenzene and its structural isomers, 1,3-dibromo-5-chlorobenzene and its structural isomers, 1-chloro-3,5-diiodobenzene and its structural isomers, 1-fluoro-3,5-dibromobenzene and its structural isomers, 1-fluoro-3,5-diiodobenzene and its structural isomers, 1-chloro-3-fluoro-5-iodobenzene and its structural isomers, 1-bromo-3-chloro-5-iodobenzene and its structural isomers, 1-bromo-3-fluoro-5-iodobenzene and its structural isomers. Among these, from the viewpoint of suppressing by-products, compound (B) is preferably 2,3-dibromonorbornadiene, 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,3,5-tribromobenzene, 1,4-diiodobenzene, or hexabromobenzene, and particularly preferably 2,3-dibromonorbornadiene, 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,4-diiodobenzene, or 1,3,5-tribromobenzene.As the compound (B), one type may be used alone, or two or more types may be used in combination.
[0021] A method for producing a silyl group-containing compound (E) according to one embodiment of the present invention includes a step of subjecting an allyl group-containing compound (C) and a hydrosilane compound (D) to a hydrosilylation reaction in the presence of a ruthenium complex (A) as a hydrosilylation reaction catalyst. The ruthenium complex (A) is as described above. The "silyl group-containing compound (E)," "allyl group-containing compound (C)," "hydrosilane compound (D)," and "reaction conditions" will be described in detail below.
[0022] <Silyl Group-Containing Compound (E)> The specific structure of the silyl group-containing compound (E) according to this embodiment is not particularly limited, as long as it is a compound in which a propylene group derived from the allyl group-containing compound (C) is bonded to a silicon atom derived from the hydrosilane compound (D). The silyl group-containing compound (E) has a silyl group represented by the following general formula (1): -SiR a X b Formula (1)
[0023] R in general formula (1) represents a substituted or unsubstituted monovalent hydrocarbon group having 1 to 20 carbon atoms. When general formula (1) contains multiple Rs, they may be the same or different. The hydrocarbon group may be saturated or unsaturated, and may be aliphatic, alicyclic, or aromatic. The hydrocarbon group preferably has 1 to 10 carbon atoms, more preferably 1 to 8 carbon atoms, even more preferably 1 to 6 carbon atoms, even more preferably 1 to 3 carbon atoms, and particularly preferably 1 or 2 carbon atoms. When the hydrocarbon group has a substituent, the substituent is not particularly limited, and examples thereof include halogeno groups such as a chloro group, alkoxy groups such as a methoxy group, and amino groups such as an N,N-diethylamino group.
[0024] Examples of R include unsubstituted alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, tert-butyl, n-hexyl, 2-ethylhexyl, and n-dodecyl; substituted alkyl groups such as chloromethyl, methoxymethyl, and N,N-diethylaminomethyl; unsaturated hydrocarbon groups such as vinyl, isopropenyl, and allyl; cycloalkyl groups such as cyclohexyl; aryl groups such as phenyl, toluoyl, and 1-naphthyl; and aralkyl groups such as benzyl. A substituted or unsubstituted alkyl group is preferred, and a methyl group, an ethyl group, a chloromethyl group, or a methoxymethyl group is more preferred, and a methyl group or a methoxymethyl group is particularly preferred. When a plurality of Rs are present, they may be the same or different.
[0025] X in general formula (1) represents a hydroxyl group or a hydrolyzable group. When general formula (1) contains multiple Xs, they may be the same or different. The hydrolyzable group is not particularly limited and may be a known hydrolyzable group, such as a hydrogen atom, a halogen atom, an alkoxy group, an acyloxy group, a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, or an alkenyloxy group. Among these, an alkoxy group, an acyloxy group, a ketoximate group, and an alkenyloxy group are preferred. Because of their mild hydrolysis and ease of handling, an alkoxy group is more preferred, a methoxy group and an ethoxy group are even more preferred, and a methoxy group is particularly preferred. When multiple Xs are present, they may be the same or different.
[0026] In general formula (1), a represents any one of 0, 1, 2, and 3, and b represents any one of 0, 1, 2, and 3. a+b is 3 or less, and is preferably 3. When the silyl group is a hydrolyzable silyl group, b represents any one of 1, 2, and 3, and is preferably 2 or 3 from the viewpoint of curability.
[0027] The molecular weight of the silyl group-containing compound (E) is not particularly limited, and it may be a low-molecular-weight compound or a polymer. In the production method using known technology (Patent Document 1), low-molecular-weight silyl group-containing compounds can be produced with few by-products, but high-molecular-weight silyl group-containing compounds have reduced selectivity to the silylated product. For example, in Experimental Example 2-10 using a silyl group-containing organic polymer with a molecular weight of approximately 1,400, 8% of the by-product isomer (1-propenyl group) was produced, and the yield of the silylated product was only 92%. In contrast, the method disclosed in the present invention uses a high-molecular-weight allyl group-containing compound (C) as a raw material, and exhibits high selectivity even when producing silyl group-containing organic polymers with number-average molecular weights exceeding 3,000, 10,000, or even 20,000, enabling the production of silylated products with few by-products (1-propenyl group or hydrogenated product). Therefore, the catalyst and the production method of the present invention are particularly suitable for the production of silyl group-containing compounds (E), particularly silyl group-containing organic polymers (E a The silyl group-containing organic polymer (E a In particular, when the organic polymer containing a hydrolyzable silyl group is a hydrolyzable silyl group-containing organic polymer, it can be used as a curable resin for adhesives, sealants, elastic coating agents, pressure-sensitive adhesives, etc., and is therefore industrially useful. The curable composition containing the hydrolyzable silyl group-containing organic polymer according to the present invention exhibits superior curability, and further, the rubber-like cured product obtained after curing can exhibit higher modulus, tensile strength, etc.
[0028] (Silyl group-containing organic polymer (E a ) the polymer skeleton of the silyl group-containing organic polymer (E a ) has a polymer backbone (also referred to as a main chain structure) and polymer chain ends bonded to the polymer backbone. The polymer backbone is a structure in which a plurality of monomer units are formed successively by bonding a plurality of monomers through addition, condensation, or the like. The monomer species contained in the polymer backbone may be one type, or a mixture of a plurality of types may be bonded.
[0029] The polymer chain end refers to a portion located at the end of the polymer skeleton. aThe number of polymer chain ends in the polymer chain of the copolymer (C) is two if the polymer backbone is entirely linear, three or more if the polymer backbone is entirely branched, and can average between two and three if the polymer backbone is a mixture of linear and branched chains.
[0030] Silyl group-containing organic polymer (E a The silyl group contained in the silyl group-containing organic polymer (E) may be present in the polymer backbone and / or at the polymer chain terminal. Two or more silyl groups may be present at one polymer chain terminal. a When the silyl group contained in the silyl group-containing organic polymer (E) is a hydrolyzable silyl group, it can be used as a curable resin for adhesives, sealing materials, elastic coating agents, pressure-sensitive adhesives, etc., and the hydrolyzable silyl group is a In the following description of the curable resin, the curable composition, and the cured product, these are referred to as the silyl group-containing organic polymer (E a ) is a hydrolyzable silyl group.
[0031] Silyl group-containing organic polymer (E aThe polymer skeleton (also referred to as the main chain structure) of the copolymer (C10-C12) is not particularly limited, and various main chain structures can be used. Specific examples include polyoxyalkylene polymers such as polyoxyethylene, polyoxypropylene, polyoxybutylene, polyoxytetramethylene, polyoxyethylene-polyoxypropylene copolymers, and polyoxypropylene-polyoxybutylene copolymers; hydrocarbon polymers such as ethylene-propylene copolymers, polyisobutylene, copolymers of isobutylene and isoprene, and hydrogenated polyolefin polymers obtained by hydrogenating these polyolefin polymers; and polyolefins obtained by condensation of dibasic acids such as adipic acid with glycols or ring-opening polymerization of lactones. Examples of suitable ester polymers include (meth)acrylic acid ester polymers obtained by radical polymerization of (meth)acrylic acid ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and stearyl (meth)acrylate; vinyl copolymers obtained by radical polymerization of monomers such as (meth)acrylic acid ester monomers, vinyl acetate, acrylonitrile, and styrene; polysulfide polymers; polyamide polymers; polycarbonate polymers; and diallyl phthalate polymers. In the above description, (meth)acrylic refers to acrylic and / or methacrylic.
[0032] Among these, saturated hydrocarbon polymers such as polyisobutylene, hydrogenated polyisoprene, and hydrogenated polybutadiene, polyoxyalkylene polymers, and (meth)acrylic acid ester polymers are preferred because they have relatively low glass transition temperatures and the resulting cured products have excellent cold resistance. Only one of these may be used, or two or more may be used in combination.
[0033] Silyl group-containing organic polymer (E a When the organic polymer having a hydrolyzable silyl group is a polyoxyalkylene polymer or a (meth)acrylic acid ester polymer, the latter being particularly preferred because they have high moisture permeability, excellent deep curing properties when made into a one-component curable composition, and excellent adhesive properties. Polyoxyalkylene polymers are more preferred, and polyoxypropylene is even more preferred.
[0034] The polyoxyalkylene polymer is preferably a polymer having a repeating unit represented by -R-O- (wherein R is a linear or branched alkylene group having 1 to 14 carbon atoms). R is more preferably a linear or branched alkylene group having 2 to 4 carbon atoms. Specific examples of the repeating unit represented by -R-O- include -CH 2 O-, -CH 2 CH 2 O-, -CH 2 CH (CH 3 ) O—, —CH 2 CH(C 2 H 5 ) O—, —CH 2 C(CH 3 ) (CH 3 ) O—, —CH 2 CH 2 CH 2 CH 2 The main chain structure of the polyoxyalkylene polymer may be composed of only one type of repeating unit, or may be composed of two or more types of repeating units.
[0035] In particular, the silyl group-containing organic polymer (E a When the above-mentioned organic polymer having a hydrolyzable silyl group is used as a curable resin for a sealant, adhesive, or the like, a polyoxypropylene-based polymer having oxypropylene repeating units in an amount of 50% by weight or more, more preferably 80% by weight or more, of the polymer skeleton is preferred because it is amorphous and has a relatively low viscosity.
[0036] The main chain structure of the polyoxyalkylene polymer may be linear or may have a branched chain. When the polymer has a branched chain, the number of branches is preferably 1 to 6 (i.e., 3 to 8 terminal groups), more preferably 1 to 4 (i.e., 3 to 6 terminal groups), and most preferably 1 (i.e., 3 terminal groups). The presence of a branched chain can provide the effect of improving the restorability of the cured product. It can also be expected to have the effect of reducing the water absorption of the cured product.
[0037] The polyoxyalkylene polymer is preferably one obtained by ring-opening polymerization of a cyclic ether compound in the presence of an initiator using a polymerization catalyst.
[0038] Examples of cyclic ether compounds include ethylene oxide, propylene oxide, butylene oxide, tetramethylene oxide, and tetrahydrofuran. These cyclic ether compounds may be used alone or in combination of two or more. Among the cyclic ether compounds, propylene oxide is particularly preferred because it can produce an amorphous polyether polymer with a relatively low viscosity.
[0039] Specific examples of the initiator include alcohols such as butanol, ethylene glycol, propylene glycol, propylene glycol monoalkyl ether, butanediol, hexamethylene glycol, neopentyl glycol, diethylene glycol, dipropylene glycol, triethylene glycol, glycerin, trimethylolmethane, trimethylolpropane, pentaerythritol, and sorbitol; and hydroxyl group-terminated polyoxyalkylene polymers having a number average molecular weight of 300 to 4,000, such as polyoxypropylene diol, polyoxypropylene triol, polyoxyethylene diol, and polyoxyethylene triol.
[0040] Examples of synthesis methods for polyoxyalkylene polymers include, but are not limited to, polymerization methods using an alkali catalyst such as KOH, polymerization methods using a transition metal compound-porphyrin complex catalyst such as the complex obtained by reacting an organoaluminum compound with porphyrin disclosed in JP-A-61-215623, polymerization methods using a composite metal cyanide complex catalyst disclosed in JP-B-46-27250, JP-B-59-15336, U.S. Pat. Nos. 3,278,457, 3,278,458, 3,278,459, 3,427,256, 3,427,334, and 3,427,335, polymerization methods using a catalyst made of a polyphosphazene salt exemplified in JP-A-10-273512, and polymerization methods using a catalyst made of a phosphazene compound exemplified in JP-A-11-060722. A polymerization method using a composite metal cyanide complex catalyst is more preferred for reasons such as production costs and the fact that a polymer with a narrow molecular weight distribution can be obtained.
[0041] Silyl group-containing organic polymer (E a ) may be a polyoxyalkylene polymer containing other bonds such as urethane bonds and urea bonds in the polymer skeleton.
[0042] Silyl group-containing organic polymer (E a The molecular weight distribution (Mw / Mn) of the silyl group-containing organic polymer (E) is not particularly limited, but is preferably 1.6 or less, more preferably 1.4 or less, even more preferably 1.3 or less, and particularly preferably 1.2 or less. Within the above range, the polymer has a relatively low viscosity and is easy to handle. a The molecular weight distribution of the copolymer can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.
[0043] Silyl group-containing organic polymer (E aThe number average molecular weight of the silyl group-containing organic polymer (E), as polystyrene-equivalent molecular weight measured by GPC, is preferably more than 3,000, more preferably more than 10,000, and even more preferably more than 20,000. When the number average molecular weight is large, the cured product exhibits high elongation and excellent mechanical properties. It is preferably 8,000 to 100,000, more preferably 8,000 to 50,000, and particularly preferably 8,000 to 35,000. When the number average molecular weight is within these ranges, the cured product exhibits excellent mechanical properties, good curability, and has an easy-to-handle viscosity and excellent workability. a ) can be obtained.
[0044] Silyl group-containing organic polymer (E a The molecular weight of the silyl group-containing organic polymer (E) can also be expressed as the molecular weight of the end group, which is calculated by directly measuring the end group concentration of a polymer precursor before the introduction of a silyl group by titration analysis based on the principles of the hydroxyl value measurement method specified in JIS K 1557-1 and the iodine value measurement method specified in JIS K 0070, and taking into consideration the structure of the organic polymer (the degree of branching determined by the polymerization initiator used). a The molecular weight converted into end groups of the silyl group-containing organic polymer (E) was determined by preparing a calibration curve of the number average molecular weight determined by general GPC measurement of the polymer precursor and the molecular weight converted into end groups. a It is also possible to obtain the number average molecular weight by converting the number average molecular weight determined by GPC of the above-mentioned copolymer into the molecular weight calculated as the terminal group.
[0045] <Allyl Group-Containing Compound (C)> The allyl group-containing compound (C) according to this embodiment contains an allyl group (CH 2 =CH-CH 2 The silyl group-containing organic polymer (E) is not particularly limited as long as it has a silyl group-containing group and can form a silyl group-containing compound (E) by a hydrosilylation reaction with the hydrosilane compound (D). a The allyl group-containing compound (C) may be an allyl group-containing organic polymer, similar to the silyl group-containing organic polymer (E). a ) and therefore the description thereof will be omitted.
[0046] <Hydrosilane Compound (D)> The hydrosilane compound (D) according to this embodiment is not particularly limited, but preferably has a structure represented by formula (2): SiR a X b H 4-a-b Formula (2)
[0047] In general formula (2), R, X, a, and b are as described above for general formula (1). Specific examples of such hydrosilane compound (D) include trimethoxysilane, triethoxysilane, triphenoxysilane, tris(2-propenyloxy)silane, triacetoxysilane, dimethoxymethylsilane, diethoxymethylsilane, dimethoxyethylsilane, (chloromethyl)dimethoxysilane, (chloromethyl)diethoxysilane, (methoxymethyl)dimethoxysilane, (methoxymethyl)diethoxysilane, (N,N-diethylaminomethyl)dimethoxysilane, and (N,N-diphenylsilane). Examples of such silanes include (ethylaminomethyl)diethoxysilane, diphenoxymethylsilane, methylsilane, dimethylsilane, trimethylsilane, ethylsilane, diethylsilane, triethylsilane, methyldiethylsilane, dimethylethylsilane, chlorodimethylsilane, dichloromethylsilane, phenylsilane, diphenylsilane, triphenylsilane, phenylmethylsilane, phenyldimethylsilane, diphenylmethylsilane, ethylphenylsilane, diethylphenylsilane, and ethyldiphenylsilane.
[0048] Silyl group-containing organic polymer (E a When a hydrolyzable silyl group-containing organic polymer suitable for adhesives, sealants, and the like is to be obtained as the hydrosilane compound (D), trimethoxysilane and dimethoxymethylsilane are particularly preferred as the hydrosilane compound (D) in terms of curability and physical properties after curing.
[0049] <Reaction Conditions> The amount of the hydrosilane compound (D) used (charged amount) in the reaction step is, in terms of the amount of substance, preferably 1 molar equivalent or more, more preferably 3 molar equivalents or more, and more preferably 5 molar equivalents or more, relative to the allyl groups in the allyl group-containing compound (C). Furthermore, the amount is usually 20 molar equivalents or less, and preferably 10 molar equivalents or less. Within the above range, silyl groups can be introduced with high efficiency while suppressing production costs. Furthermore, within the above range, the silyl group-containing organic polymer (E) after production can be easily and efficiently introduced. a ) can be kept low, and a polymer with good workability can be obtained.
[0050] The amount (charge amount) of the ruthenium complex (A) used in the reaction step is, in weight ratio relative to the allyl group-containing compound (C), usually 0.01 ppm or more, preferably 0.1 ppm or more, more preferably 1 ppm or more, and usually 10% or less, preferably 1% or less, more preferably 0.1% or less. Within this range, silyl groups can be introduced with high efficiency.
[0051] The reaction step may be carried out using a solvent or without a solvent. When a solvent is used, the type of solvent is not particularly limited, and it is preferably a compound that does not react with the raw materials or catalyst. Specific examples include hydrocarbon solvents such as hexane, and halogenated solvents such as dichloromethane. The solvent is preferably dehydrated and deoxygenated before use.
[0052] The reaction temperature in the reaction step can be appropriately determined taking into consideration the reactivity (reaction rate) and the heat resistance temperature of the reaction vessel, etc., but is usually 0°C or higher, preferably 20°C or higher, more preferably 40°C or higher, and usually 200°C or lower, preferably 150°C or lower. The higher the reaction temperature, the shorter the reaction time and the more effectively side reactions can be suppressed. The reaction time is also not particularly limited and may be about 5 minutes to 12 hours, or about 10 minutes to 5 hours.
[0053] The reaction step is preferably carried out under an inert atmosphere such as nitrogen or argon.
[0054] Furthermore, during the hydrosilylation reaction, in addition to adding the ruthenium complex (A) to the reaction system, further adding and mixing the compound (B) is preferable because this can improve the silylation rate. One possible factor behind this improvement in the silylation rate is that, for example, when the amount of compound (B) used during the synthesis of the ruthenium complex (A) is insufficient and ruthenium chloride (III) is partially contained in the ruthenium complex (A), the ruthenium chloride (III) reacts with the added compound (B) to convert it to the ruthenium complex (A). Therefore, it is preferable that the ruthenium complex (A) and the compound (B) come into contact with each other before the start of the hydrosilylation reaction. For example, one preferred embodiment includes a method in which the ruthenium complex (A) and the compound (B) are added and mixed while stirring the allyl group-containing compound (C) charged in a reaction vessel at a predetermined temperature, and then the hydrosilane compound (D) is added. The time interval between the addition of the ruthenium complex (A) and the compound (B) and the addition of the hydrosilane compound (D) is not particularly limited, and may be appropriately determined in consideration of the desired introduction rate of silyl groups, the time required for production, and the like.
[0055] A method for producing a silyl group-containing compound (E) according to one embodiment of the present invention also includes a step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), a ruthenium compound (A') that does not have compound (B) as a ligand, and compound (B) to carry out a hydrosilylation reaction. This production method, unlike the above-described production method, does not require the use of a pre-synthesized ruthenium complex (A). Instead, the ruthenium compound (A') and compound (B) are mixed in a reaction vessel to form a ruthenium complex (A) in the system, which then functions as a catalyst, thereby efficiently producing a silylated compound. The allyl group-containing compound (C), hydrosilane compound (D), and compound (B) are as described above. The order in which the allyl group-containing compound (C), hydrosilane compound (D), ruthenium compound (A'), and compound (B) are mixed is not particularly limited, and they can be mixed in any order. Hereinafter, the "ruthenium compound (A')" and "reaction conditions" will be described in detail.
[0056] <Ruthenium Compound (A')> The ruthenium compound (A') used in one embodiment of the present invention is not particularly limited, except that it does not have compound (B) as a ligand. As the ruthenium compound (A'), ruthenium(III) chloride hydrate and a ruthenium complex having compound (B') as a ligand that does not fall under compound (B) can be used. Examples of types of compound (B') include a 2,5-norbornadiene ligand, a 1,5-cyclooctadiene ligand, a p-cymene ligand, a mesitylene ligand, a benzene ligand, a carbonyl ligand, an isocyanide ligand, and an arene ligand.
[0057] From the viewpoint of suppressing by-products, the ruthenium compound (A') is preferably a ruthenium complex having a ligand selected from a 2,5-norbornadiene ligand, a benzene ligand, and a p-cymene ligand.
[0058] <Reaction Conditions> The preferred conditions for the amount (charge amount) of the hydrosilane compound (D) used in the reaction step, the type of solvent used in the reaction step, and the reaction temperature are the same as those set forth in the embodiment of the "step of subjecting an allyl group-containing compound (C) and a hydrosilane compound (D) to a hydrosilylation reaction in the presence of a ruthenium complex (A)." The preferred amount (charge amount) of the ruthenium compound (A') used is the same as the above-mentioned amount (charge amount) of the ruthenium complex (A). This production method includes a step of mixing the ruthenium compound (A') and the compound (B) in a reaction vessel to produce the ruthenium complex (A) in the system. Therefore, for example, it is preferred to add the ruthenium compound (A') and the compound (B) to the allyl group-containing compound (C) charged in the reaction vessel while stirring at a predetermined temperature, and then add the hydrosilane compound (D). The time interval between the addition of the ruthenium compound (A′) and the compound (B) and the addition of the hydrosilane compound (D) is not particularly limited and may be appropriately determined in consideration of the desired introduction rate of silyl groups and the production time.
[0059] The amount of compound (B) added is not particularly limited, and is usually 0.01 ppm or more, preferably 0.1 ppm or more, more preferably 1 ppm or more, and usually 10% or less, preferably 1% or less, more preferably 0.1% or less, by weight, relative to the allyl group-containing compound (C).
[0060] According to the above-described method for producing the silyl group-containing compound (E), a mixture containing the silyl group-containing compound (E) and the ruthenium complex (A) can be obtained. In particular, the silyl group-containing organic polymer (E a A polymer mixture containing a hydrolyzable silyl group-containing polymer and a ruthenium complex (A) as the polymer component (B) can be mixed with a curing catalyst to form a curable composition.
[0061] In the polymer mixture, the content of the ruthenium complex (A) corresponds to the amount (charge amount) of the ruthenium complex (A) or ruthenium compound (A') used. Specifically, the content of the ruthenium complex (A) is, in weight ratio, usually 0.01 ppm or more, preferably 0.1 ppm or more, and more preferably 1 ppm or more, and usually 10% or less, preferably 1% or less, and more preferably 0.1% or less, based on the weight of the hydrolyzable silyl group-containing polymer.
[0062] <Curable composition> A silyl group-containing organic polymer (E a When the silyl group-containing organic polymer (E) is a hydrolyzable silyl group-containing organic polymer, a curable composition containing the silyl group-containing organic polymer can be formed. In addition, a curable product can be obtained by curing the curable composition. a As the polymer backbone of the above-mentioned copolymer, a polyoxyalkylene polymer is more preferred, and polyoxypropylene is even more preferred, as described above.
[0063] The curable composition containing the hydrolyzable silyl group-containing organic polymer obtained by the above-described production method exhibits a short skinning time and good curability compared to hydrolyzable silyl group-containing organic polymers produced using conventionally known hydrosilylation reaction catalysts such as Karstedt's catalyst. Furthermore, the cured product obtained by curing the curable composition exhibits a high modulus and high strength.
[0064] (Curing Catalyst) The curable composition according to this embodiment preferably contains a curing catalyst for the purpose of promoting the reaction of hydrolyzing and condensing the hydrolyzable silyl group, that is, the curing reaction.
[0065] As the curing catalyst, a conventionally known one can be used, and specifically, an organic tin compound, a metal carboxylate, an amine compound, a carboxylic acid, an alkoxy metal, an inorganic acid, a mixture thereof, etc. can be used.
[0066] Specific examples of organic tin compounds include dibutyltin dilaurate, dibutyltin dioctanoate, dibutyltin bis(butyl maleate), dibutyltin diacetate, dibutyltin oxide, dibutyltin bis(acetylacetonate), a reaction product of dibutyltin oxide with a silicate compound, a reaction product of dibutyltin oxide with a phthalate ester, dioctyltin diacetate, dioctyltin dilaurate, dioctyltin bis(ethyl maleate), dioctyltin bis(octyl maleate), dioctyltin bis(acetylacetonate), dioctyltin distearate, dioctyltin oxide, and a reaction product of dioctyltin oxide with a silicate compound. In view of the growing concern about the environment in recent years, dioctyltin compounds are preferred.
[0067] Specific examples of metal carboxylates include tin carboxylate, bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, potassium carboxylate, calcium carboxylate, etc. The carboxylic acid group can be a combination of the following carboxylic acids with various metals.
[0068] Specific examples of the amine compound include amines such as octylamine, 2-ethylhexylamine, laurylamine, stearylamine, piperidine, 4-methylpiperidine, and hexamethyleneimine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5,4,0]undecene-7 (DBU), and 1,5-diazabicyclo[4,3,0]nonene-5 (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanide, 1-o-tolylbiguanide, and 1-phenylbiguanide; and ketimine compounds.
[0069] Specific examples of carboxylic acids include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.
[0070] Specific examples of alkoxy metals include titanium compounds such as tetrabutyl titanate, titanium tetrakis(acetylacetonate), titanium ethylacetoacetate, and diisopropoxytitanium bis(ethylacetoacetate); aluminum compounds such as aluminum tris(acetylacetonate) and diisopropoxyaluminum ethylacetoacetate; and zirconium compounds such as zirconium tetrakis(acetylacetonate).
[0071] Other curing catalysts that can be used include fluorine anion-containing compounds, photoacid generators, and photobase generators.
[0072] The curing catalyst may be a combination of two or more different catalysts. For example, the combination of the amine compound and a carboxylic acid or the amine compound and an alkoxy metal may provide an effect of improving reactivity.
[0073] The amount of the curing catalyst to be blended is determined by the amount of the silyl group-containing organic polymer (E aThe amount of the curing catalyst is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 15 parts by weight, and particularly preferably 0.01 to 10 parts by weight, per 100 parts by weight of the curable composition. Furthermore, some curing catalysts may ooze onto the surface of the cured product after the curable composition has cured, or may contaminate the surface of the cured product. In such cases, by using 0.01 to 3.0 parts by weight of the curing catalyst, it is possible to maintain good surface condition of the cured product while ensuring curability.
[0074] The curable composition according to this embodiment may contain other additives, such as silicon compounds, adhesion promoters, plasticizers, solvents, diluents, silicates, fillers, anti-sagging agents, antioxidants, light stabilizers, UV absorbers, physical property adjusters, tackifier resins, epoxy group-containing compounds, photocurable substances, oxygen-curable substances, surface property improvers, epoxy resins, other resins, flame retardants, and foaming agents. Furthermore, various additives may be added to the curable composition according to this embodiment as needed to adjust the physical properties of the composition or the cured product. Examples of such additives include curability adjusters, radical inhibitors, metal deactivators, antiozonants, phosphorus-based peroxide decomposers, lubricants, pigments, and mildew inhibitors.
[0075] (Filler) The curable composition according to the present embodiment may contain various fillers, such as heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, clay, talc, titanium oxide, fumed silica, precipitated silica, crystalline silica, fused silica, silicic anhydride, hydrated silicic acid, carbon black, ferric oxide, fine aluminum powder, zinc oxide, activated zinc white, PVC powder, PMMA powder, glass fiber, and filament.
[0076] The amount of filler used is a The amount is preferably 1 to 300 parts by weight, more preferably 10 to 250 parts by weight, per 100 parts by weight of the hydroxybenzoate.
[0077] Organic or inorganic balloons may be added to the composition to reduce its weight (lower its specific gravity). The balloons are hollow spherical fillers, and examples of the materials for the balloons include inorganic materials such as glass, shirasu, and silica, and organic materials such as phenolic resin, urea resin, polystyrene, and saran.
[0078] The amount of balloons used is determined by the silyl group-containing organic polymer (E a The amount is preferably 0.1 to 100 parts by weight, more preferably 1 to 20 parts by weight, per 100 parts by weight of the organic solvent.
[0079] (Adhesion imparting agent) The curable composition according to the present embodiment may contain an adhesion imparting agent. Examples of the adhesion imparting agent that may be added include a silane coupling agent and a reaction product of a silane coupling agent.
[0080] Specific examples of the silane coupling agent include amino group-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxysilane, and γ-isopropyltriethoxysilane; Examples of suitable adhesion promoters include isocyanate group-containing silanes such as cyanatepropylmethyldimethoxysilane, α-isocyanatomethyltrimethoxysilane, and α-isocyanatomethyldimethoxymethylsilane; mercapto group-containing silanes such as γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; and epoxy group-containing silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Condensates of various silane coupling agents, such as condensates of amino group-containing silanes and condensates of amino group-containing silanes with other alkoxysilanes, and reaction products of various silane coupling agents, such as reaction products of amino group-containing silanes and epoxy group-containing silanes and reaction products of amino group-containing silanes and (meth)acrylic group-containing silanes, can also be used. The adhesion promoters may be used alone or in combination.
[0081] The amount of the silane coupling agent used is a The amount is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the inorganic filler.
[0082] (Plasticizer) A plasticizer may be added to the curable composition according to this embodiment. Specific examples of plasticizers include phthalate ester compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate ester compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; non-phthalate ester compounds such as 1,2-cyclohexanedicarboxylic acid diisononyl ester; aliphatic polycarboxylic acid ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and acetyl tributyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters; phosphate ester compounds; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; and epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate.
[0083] Furthermore, a polymer plasticizer can be used. Specific examples of the polymer plasticizer include vinyl polymers; polyester plasticizers; polyether polyols such as polyethylene glycol and polypropylene glycol having a number average molecular weight of 500 or more, and polyethers such as derivatives in which the hydroxy groups of these polyether polyols are converted into ester groups, ether groups, etc.; polystyrenes; polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, polychloroprene, etc. The plasticizers may be used alone or in combination of two or more.
[0084] The polymer plasticizer may not have a reactive silyl group, but may have a reactive silyl group. When it has a reactive silyl group, it acts as a reactive plasticizer and can prevent the plasticizer from migrating from the cured product. When it has a reactive silyl group, it is preferable that the number of reactive silyl groups is 1 or less, more preferably 0.8 or less, on average per molecule. When a plasticizer having a reactive silyl group, particularly an oxyalkylene polymer having a reactive silyl group, is used, its number average molecular weight is 1 or less than that of the silyl group-containing organic polymer (E a ) is preferably lower.
[0085] The amount of plasticizer used is a The amount is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, per 100 parts by weight of the hydroxybenzoate.
[0086] (Solvent, Diluent) A solvent or diluent can be added to the curable composition according to this embodiment. The solvent and diluent are not particularly limited, but aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, ethers, etc. can be used. When using a solvent or diluent, in view of the problem of air pollution when the composition is used indoors, the boiling point of the solvent is preferably 150°C or higher, more preferably 200°C or higher, and particularly preferably 250°C or higher. The above solvents or diluents may be used alone or in combination of two or more.
[0087] (Anti-sagging agent) If necessary, an anti-sagging agent may be added to the curable composition according to this embodiment in order to prevent sagging and improve workability. The anti-sagging agent is not particularly limited, and examples thereof include polyamide waxes; hydrogenated castor oil derivatives; and metal soaps such as calcium stearate, aluminum stearate, and barium stearate. These anti-sagging agents may be used alone or in combination of two or more.
[0088] The amount of the sagging prevention agent used is a The amount is preferably 0.1 to 20 parts by weight per 100 parts by weight of the hydroxybenzoate.
[0089] (Antioxidant) An antioxidant (antiaging agent) can be used in the curable composition according to this embodiment. The use of an antioxidant can improve the weather resistance of the cured product. Examples of antioxidants include hindered phenols, monophenols, bisphenols, and polyphenols. Examples include Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, and Irganox 1520 (all manufactured by BASF); SONGNOX 1076 (manufactured by SONGWON), and BHT. Similarly, hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, TINUVIN 292, CHIMASSORB 944LD, and CHIMASSORB 119FL (all manufactured by BASF); Adeka STAB LA-57, Adeka STAB LA-62, Adeka STAB LA-67, Adeka STAB LA-63, and Adeka STAB LA-68 (all manufactured by ADEKA Corporation); Sanol LS-2626, Sanol LS-1114, and Sanol LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and Nocrac CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. Other antioxidants that can be used include SONGNOX 4120, Nauguard 445, and OKABEST CLX050. Specific examples of antioxidants are also described in Japanese Patent Application Laid-Open Nos. 4-283259 and 9-194731.
[0090] The amount of antioxidant used is a The amount is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the inorganic filler.
[0091] (Light Stabilizer) A light stabilizer can be used in the curable composition according to this embodiment. The use of a light stabilizer can prevent photo-oxidative degradation of the cured product. Examples of light stabilizers include benzotriazole-based, hindered amine-based, and benzoate-based compounds, with hindered amine-based compounds being particularly preferred.
[0092] The amount of the light stabilizer used is aThe amount is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the inorganic filler.
[0093] (Ultraviolet Absorber) An ultraviolet absorber can be used in the curable composition according to this embodiment. Use of an ultraviolet absorber can improve the surface weather resistance of the cured product. Examples of ultraviolet absorbers include benzophenone-based, benzotriazole-based, salicylate-based, substituted acrylonitrile-based, and metal chelate-based compounds, with benzotriazole-based compounds being particularly preferred, and examples thereof include those commercially available under the names Tinuvin P, Tinuvin 213, Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 571, Tinuvin 1600, and Tinuvin B75 (all manufactured by BASF).
[0094] The amount of the ultraviolet absorber used is a The amount is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the inorganic filler.
[0095] (Physical Property Modifier) A physical property modifier may be added to the curable composition according to this embodiment as needed to adjust the tensile properties of the resulting cured product. The physical property modifier is not particularly limited, but examples include alkylalkoxysilanes such as phenoxytrimethylsilane, methyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, and n-propyltrimethoxysilane; arylalkoxysilanes such as diphenyldimethoxysilane and phenyltrimethoxysilane; alkylisopropenoxysilanes such as dimethyldiisopropenoxysilane, methyltriisopropenoxysilane, and γ-glycidoxypropylmethyldiisopropenoxysilane; trialkylsilylborates such as tris(trimethylsilyl)borate and tris(triethylsilyl)borate; silicone varnishes; and polysiloxanes. The use of the physical property modifier can increase the hardness of the curable composition according to this embodiment when cured, or, conversely, decrease the hardness and increase the elongation at break. The physical property modifiers may be used alone, or two or more types may be used in combination.
[0096] In particular, compounds that upon hydrolysis produce compounds having monovalent silanol groups in the molecule have the effect of reducing the modulus of the cured product without increasing the stickiness of the surface of the cured product. Compounds that produce trimethylsilanol are particularly preferred. Examples of compounds that upon hydrolysis produce compounds having monovalent silanol groups in the molecule include silicon compounds that are derivatives of alcohols such as hexanol, octanol, phenol, trimethylolpropane, glycerin, pentaerythritol, and sorbitol and that produce silane monool upon hydrolysis. Specific examples include phenoxytrimethylsilane and tris((trimethylsiloxy)methyl)propane.
[0097] The amount of the physical property adjuster used is a The amount is preferably 0.1 to 10 parts by weight, more preferably 0.5 to 5 parts by weight, per 100 parts by weight of the inorganic filler.
[0098] (Tackifying Resin) A tackifying resin can be added to the curable composition according to the present embodiment for the purpose of improving adhesion or adhesion to a substrate, or as otherwise required. The tackifying resin is not particularly limited, and any commonly used tackifying resin can be used.
[0099] Specific examples include terpene resins, aromatic modified terpene resins, hydrogenated terpene resins, terpene-phenol resins, phenol resins, modified phenol resins, xylene-phenol resins, cyclopentadiene-phenol resins, coumarone-indene resins, rosin resins, rosin ester resins, hydrogenated rosin ester resins, xylene resins, low molecular weight polystyrene resins, styrene copolymer resins, styrene block copolymers and hydrogenated products thereof, petroleum resins (e.g., C5 hydrocarbon resins, C9 hydrocarbon resins, C5C9 hydrocarbon copolymer resins, etc.), hydrogenated petroleum resins, DCPD resins, etc. These may be used alone or in combination of two or more.
[0100] The amount of the tackifier resin used is aThe amount is preferably 2 to 100 parts by weight, more preferably 5 to 50 parts by weight, and even more preferably 5 to 30 parts by weight, per 100 parts by weight of the hydroxybenzoate.
[0101] (Compound containing an epoxy group) In the curable composition according to this embodiment, a compound containing an epoxy group can be used. The use of a compound having an epoxy group can improve the restorability of the cured product. Examples of compounds having an epoxy group include epoxidized unsaturated fats and oils, epoxidized unsaturated fatty acid esters, alicyclic epoxy compounds, compounds shown as epichlorohydrin derivatives, and mixtures thereof. Specific examples include epoxidized soybean oil, epoxidized linseed oil, bis(2-ethylhexyl)-4,5-epoxycyclohexane-1,2-dicarboxylate (E-PS), epoxy octyl stearate, and epoxy butyl stearate. The epoxy compound can be used in the curable composition according to this embodiment, such as the silyl group-containing organic polymer (E a It is recommended to use it in the range of 0.5 to 50 parts by weight per 100 parts by weight of the solvent.
[0102] (Photocurable Substance) A photocurable substance can be used in the curable composition according to this embodiment. When a photocurable substance is used, a film of the photocurable substance is formed on the surface of the cured product, improving the stickiness and weather resistance of the cured product. Many compounds of this type are known, such as organic monomers, oligomers, resins, and compositions containing them. Representative examples include unsaturated acrylic compounds, which are monomers or oligomers having one or more acrylic or methacrylic unsaturated groups, or mixtures thereof, polyvinyl cinnamates, and azido resins.
[0103] The amount of the photocurable material used is the silyl group-containing organic polymer (E a The amount is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the inorganic filler.
[0104] (Oxygen-Curable Substance) An oxygen-curable substance can be used in the curable composition according to this embodiment. Examples of oxygen-curable substances include unsaturated compounds that can react with oxygen in the air, which react with oxygen in the air to form a cured film near the surface of the cured product, preventing stickiness of the surface and adhesion of dirt and dust to the surface of the cured product. Specific examples of oxygen-curable substances include drying oils such as tung oil and linseed oil, and various alkyd resins obtained by modifying such compounds; acrylic polymers, epoxy resins, and silicone resins modified with drying oils; and liquid polymers such as 1,2-polybutadiene, 1,4-polybutadiene, and polymers of C5 to C8 dienes obtained by polymerizing or copolymerizing diene compounds such as butadiene, chloroprene, isoprene, and 1,3-pentadiene. These substances may be used alone or in combination of two or more.
[0105] The amount of oxygen-curing material used is a It is preferable to use the oxygen-curable substance in an amount of 0.1 to 20 parts by weight, and more preferably 0.5 to 10 parts by weight, per 100 parts by weight of the curable material. As described in JP-A-3-160053, it is preferable to use the oxygen-curable substance in combination with a photo-curable substance.
[0106] (Epoxy Resin) The curable composition according to the present embodiment can be used in combination with an epoxy resin. A composition containing an epoxy resin is particularly suitable as an adhesive, particularly as an adhesive for exterior wall tiles. Examples of the epoxy resin include bisphenol A epoxy resins and novolac epoxy resins.
[0107] The epoxy resin and the silyl group-containing organic polymer (E a The proportion of the silyl group-containing organic polymer (E a ) / epoxy resin = 100 / 1 to 1 / 100.
[0108] When an epoxy resin is added, a curing agent for curing the epoxy resin can be used in combination with the curable composition according to this embodiment. There are no particular limitations on the epoxy resin curing agent that can be used, and any commonly used epoxy resin curing agent can be used.
[0109] When a curing agent for an epoxy resin is used, the amount used is preferably in the range of 0.1 to 300 parts by weight per 100 parts by weight of the epoxy resin.
[0110] <<Preparation of Curable Composition>> The curable composition according to this embodiment can be prepared as a one-component composition in which all of the ingredients are mixed in advance and stored in a sealed container, and the composition is cured by moisture in the air after application, or as a two-component composition in which ingredients such as a curing catalyst, a filler, a plasticizer, and water are mixed separately as a curing agent, and the ingredients are mixed with the organic polymer composition before use. From the viewpoint of workability, the one-component composition is preferred.
[0111] When the curable composition is a one-component type, all of the components are blended in advance, and therefore it is preferable to dehydrate and dry the components containing water before use, or to dehydrate them under reduced pressure during blending and kneading. In addition to the dehydration and drying method, the storage stability can be further improved by adding an alkoxysilane compound such as methyltrimethoxysilane, phenyltrimethoxysilane, n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, or γ-glycidoxypropyltrimethoxysilane.
[0112] <Uses> The curable composition according to this embodiment can be used as a pressure-sensitive adhesive, a sealing material for buildings, ships, automobiles, roads, etc., an adhesive, a waterproofing material, a waterproof coating material, a mold release agent, an anti-vibration material, a vibration-damping material, a sound-proofing material, a foam material, a paint, or a spray material. The cured product obtained by curing the curable composition according to this embodiment has excellent flexibility and adhesiveness, and therefore can be suitably used as a sealant or adhesive.
[0113] Furthermore, the curable composition according to this embodiment can be used in a wide range of applications, including electrical and electronic component materials such as solar cell rear surface sealing materials, electrical and electronic components such as insulating coating materials for electric wires and cables, electrical insulating materials for devices, acoustic insulating materials, elastic adhesives, binders, contact adhesives, spray-type sealants, crack repair materials, tiling adhesives, adhesives for asphalt waterproofing materials, powder coatings, casting materials, medical rubber materials, medical pressure-sensitive adhesives, medical adhesive sheets, medical device sealants, dental impression materials, food packaging materials, and joint sealants for exterior materials such as sizing boards. These compounds can be used in a variety of applications, including adhesives, coatings, non-slip coatings, buffer materials, primers, conductive materials for electromagnetic wave shielding, thermally conductive materials, hot melt materials, potting agents for electrical and electronic applications, films, gaskets, concrete reinforcing materials, temporary adhesives, various molding materials, and liquid sealants for rust prevention and waterproofing of wired glass and laminated glass edge (cut portions), automobile parts, large vehicle parts such as trucks and buses, train car parts, aircraft parts, marine parts, electrical parts, and various machine parts. Taking automobiles as an example, they can be used in a wide variety of applications, including adhesive attachment of plastic covers, trim, flanges, bumpers, window mounting, interior components, exterior components, etc. Furthermore, because they can adhere to a wide range of substrates, such as glass, porcelain, wood, metal, and resin moldings, either alone or with the aid of a primer, they can also be used as various types of sealing and adhesive compositions. The curable composition according to this embodiment can also be used as an adhesive for interior panels, exterior panels, tile adhesives, stone veneers, ceiling finishing adhesives, floor finishing adhesives, wall finishing adhesives, vehicle panels, electrical, electronic, and precision equipment assembly adhesives, adhesives for bonding leather, textile products, fabrics, paper, boards, and rubber, reactive post-crosslinking pressure-sensitive adhesives, direct glazing sealants, double-glazing sealants, SSG construction sealants, or building working joint sealants, civil engineering and bridge materials, and can also be used as adhesive materials such as adhesive tapes and adhesive sheets.
[0114] The following items list preferred embodiments of the present disclosure, but the present invention is not limited to them. [Item 1] A ruthenium complex (A) having a compound (B) as a ligand, wherein the compound (B) has at least one carbon-carbon double bond in one molecule, and an electron-withdrawing group is bonded to at least one of the carbon atoms forming the carbon-carbon double bond. [Item 2] The ruthenium complex (A) according to Item 1, wherein the compound (B) has a benzene ring skeleton as the skeleton containing the carbon-carbon double bond. [Item 3] The ruthenium complex (A) according to Item 1, wherein the compound (B) has a norbornadiene skeleton as the skeleton containing the carbon-carbon double bond. [Item 4] The ruthenium complex (A) according to any one of Items 1 to 3, wherein the electron-withdrawing group is at least one selected from the group consisting of a fluoro group, a bromo group, and an iodo group. [Item 5] The ruthenium complex (A) according to Item 2, wherein compound (B) is at least one selected from the group consisting of 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,4-diiodobenzene, and 1,3,5-tribromobenzene. [Item 6] The ruthenium complex (A) according to Item 3, wherein compound (B) is 2,3-dibromonorbornadiene. [Item 7] A hydrosilylation reaction catalyst comprising the ruthenium complex (A) according to any one of Items 1 to 6. [Item 8] A method for producing a silyl group-containing compound (E), comprising the step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), and the hydrosilylation reaction catalyst according to Item 7, and carrying out a hydrosilylation reaction. [Item 9] The production method according to Item 8, wherein compound (B) is further mixed in the hydrosilylation reaction.[Item 10] A method for producing a silyl group-containing compound (E), comprising the step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), a ruthenium compound (A') that does not have compound (B) as a ligand, and compound (B) to carry out a hydrosilylation reaction, wherein compound (B) has at least one carbon-carbon double bond in one molecule, and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it. [Item 11] The production method according to any one of Items 8 to 10, wherein the amount of hydrosilane compound (D) used is 3 molar equivalents or more relative to the allyl groups in the allyl group-containing compound (C). [Item 12] The production method according to any one of Items 8 to 11, wherein the silyl group-containing compound (E) is a polymer with a number average molecular weight of more than 3,000. [Item 13] The production method according to any one of Items 8 to 12, wherein the silyl group-containing compound (E) is a hydrolyzable silyl group-containing polymer. [Item 14] The production method according to Item 13, wherein the silyl group-containing compound (E) is a hydrolyzable silyl group-containing polyoxyalkylene polymer. [Item 15] The production method according to any one of Items 8 to 14, wherein compound (B) has a benzene ring skeleton as the skeleton containing the carbon-carbon double bond. [Item 16] The production method according to any one of Items 8 to 14, wherein compound (B) has a norbornadiene skeleton as the skeleton containing the carbon-carbon double bond. [Item 17] The production method according to any one of Items 8 to 16, wherein the electron-withdrawing group is at least one selected from the group consisting of a fluoro group, a bromo group, and an iodo group. [Item 18] The production method according to Item 15, wherein compound (B) is at least one selected from the group consisting of 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,4-diiodobenzene, and 1,3,5-tribromobenzene. [Item 19] The production method according to Item 16, wherein compound (B) is 2,3-dibromonorbornadiene. [Item 20] The production method according to any one of Items 10 to 19, wherein ruthenium compound (A') has a ligand selected from 2,5-norbornadiene, benzene, and p-cymene.[Item 21] A polymer mixture containing a hydrolyzable silyl group-containing polymer and the ruthenium complex (A) according to any one of items 1 to 6. [Item 22] A curable composition containing the polymer mixture according to item 21 and a curing catalyst. [Item 23] A cured product obtained by curing the curable composition according to item 22.
[0115] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The number average molecular weight in the examples is a GPC molecular weight measured under the following conditions: Solution delivery system: HLC-8420GPC manufactured by Tosoh Corporation Column: TSKgel Super H series manufactured by Tosoh Corporation Solvent: THF (tetrahydrofuran) Molecular weight: Polystyrene equivalent Measurement temperature: 40°C
[0116] The proportion of silyl groups, 1-propenyl groups, or hydrogenated products was calculated using the following nuclear magnetic resonance (NMR) spectrometer: 1 H NMR measurement was performed. Apparatus: AVANCE III HD500 digital instrument (manufactured by BRUKER)
[0117] Example 1 While stirring an ethanol solution containing 0.15 g of ruthenium (III) chloride hydrate (manufactured by Tokyo Chemical Industry Co., Ltd.), which is ruthenium compound (A'), under a nitrogen atmosphere, 0.064 g of sodium carbonate and 0.20 g of 2,3-dibromonorbornadiene (manufactured by Tokyo Chemical Industry Co., Ltd.), which is compound (B), were added under heating and reflux. After stirring under the above conditions for 1 hour, the mixture was filtered and dried under reduced pressure to obtain ruthenium complex (A-1), which is ruthenium complex (A).
[0118] Example 2 To an ethanol solution containing 0.15 g of ruthenium (III) chloride hydrate (manufactured by Tokyo Chemical Industry Co., Ltd.), which is ruthenium compound (A'), 0.064 g of sodium carbonate and 0.36 g of 2,3-dibromonorbornadiene (manufactured by Tokyo Chemical Industry Co., Ltd.), which is compound (B), were added under heating and reflux while stirring under a nitrogen atmosphere. After stirring under the above conditions for 1 hour, the mixture was filtered and dried under reduced pressure to obtain ruthenium complex (A-2), which is ruthenium complex (A).
[0119] Synthesis Example 1 To a hydroxyl-terminated polyoxypropylene polymer (F-1) having a number-average molecular weight of approximately 3,100, 1.1 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-1) were added as a 28% methanol solution. After distilling off the methanol by vacuum evaporation, 1.3 molar equivalents of allyl chloride relative to the hydroxyl groups of the polymer (F-1) were added and the mixture was reacted at 130°C for 1 hour to convert the terminal hydroxyl groups to allyl groups. Unreacted allyl chloride was then distilled off by degassing under reduced pressure. The resulting unpurified allyl-terminated polyoxypropylene was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove metal salts from the polymer. As a result, an allyl-group-containing organic polymer (C-1), which is the allyl-group-containing compound (C), was obtained. The number-average molecular weight of the polymer was 3,100.
[0120] Example 3 To a polymer (C-1) that is an allyl group-containing compound (C), 2,400 ppm of the ruthenium complex (A-1) that is the ruthenium complex (A) obtained in Example 1 and dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-1)) that is a hydrosilane compound (D) were added, and a hydrosilylation reaction was carried out at 70°C. 1 The reaction was continued until it was confirmed by H NMR measurement that the allyl groups in the polymer (C-1) had been completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The proportion of each group relative to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 1.
[0121] Example 4 A hydrosilylation reaction was carried out in the same manner as in Example 3, except that 2,400 ppm of ruthenium complex (A-2), which was the ruthenium complex (A) obtained in Example 2, was used. The results are shown in Table 1.
[0122] Examples 5 to 17 To polymer (C-1), which is the allyl group-containing compound (C), ruthenium complex (A) or each ruthenium compound (A'), and each compound (B) were added as shown in Table 1, and the mixture was stirred at 70°C for 10 minutes. Furthermore, dimethoxymethylsilane, which is hydrosilane compound (D) (5.0 molar equivalents relative to the allyl groups in polymer (C-1)), was added, and the allyl groups in polymer (C-1) were subjected to a hydrosilylation reaction at 70°C. Every hour from the start of the reaction, 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-1) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The proportion of each group relative to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 1.
[0123]
[0124] Comparative Examples 1 to 6 To polymer (C-1), which is the allyl group-containing compound (C), 2,400 ppm of a commercially available Karstedt catalyst (platinum divinyldisiloxane complex (3 wt % isopropanol solution in terms of platinum)) or each ruthenium compound (A'), and dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in polymer (C-1)), which is the hydrosilane compound (D), were added, as shown in Table 2, and the allyl groups in polymer (C-1) were hydrosilylated at 70°C. 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-1) were completely consumed, after which the volatile components were distilled off under reduced pressure to obtain a silyl group-containing polymer. 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 2.
[0125] Comparative Examples 7 to 12 As shown in Table 2, the polymer (C-1) which is the allyl group-containing compound (C) was mixed with the ruthenium compound (A′) [RuCl 2 (nbd)] n2,400 ppm of norbornadiene (nbd) and each compound (B') not corresponding to compound (B) were added, and the mixture was stirred at 70°C for 10 minutes. Further, dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in polymer (C-1)), which is hydrosilane compound (D), was added, and a hydrosilylation reaction of the allyl groups in polymer (C-1) was carried out at 70°C. Every hour from the start of the reaction, 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-1) were completely consumed, after which the volatile components were distilled off under reduced pressure to obtain a silyl group-containing polymer. 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 2.
[0126]
[0127] The following can be seen from Tables 1 and 2. Comparing Examples 3 and 4 with Comparative Examples 1 to 6, it can be seen that, compared to Comparative Examples 1 to 6 which used a Karstedt catalyst or a ruthenium compound (A'), Examples 3 and 4 which used a ruthenium complex (A) having compound (B) as a ligand showed a higher proportion of silyl groups in the resulting polymer and a lower proportion of 1-propenyl groups and hydrogenated products, indicating that silyl groups could be introduced with higher selectivity into the allyl groups of polymer (C-1). Comparing Example 3 with Example 4, which used ruthenium complex (A-2), showed a higher silyl group introduction rate, suggesting that it is preferable to use a larger amount of compound (B) when synthesizing ruthenium complex (A).
[0128] Furthermore, when Example 3 and Example 5, which both used ruthenium complex (A-1), are compared, it is clear that Example 5, in which 2,3-dibromonorbornadiene was added as compound (B) in addition to ruthenium complex (A-1), enabled the introduction of silyl groups with higher selectivity.
[0129] Furthermore, when Examples 6 to 17, in which ruthenium compound (A') was used and compound (B) was further added, were compared with Comparative Examples 2 to 6, in which ruthenium compound (A') was used but compound (B) was not added, it was found that silyl groups were introduced more selectively to the allyl groups of polymer (C-1) in Examples 6 to 17. Thus, a significant increase in the silyl group introduction rate was confirmed even in the simpler method in which compound (B) was added to ruthenium compound (A') and then the hydrosilylation reaction was carried out without using a pre-synthesized ruthenium complex (A).
[0130] Furthermore, the ruthenium compound (A') is [RuCl 2 (nbd)] n In Example 6, 2,3-dibromonorbornadiene was further added as the compound (B), and [RuCl 2 (nbd)] n When compared with Comparative Examples 7 to 12, in which a compound (B') not corresponding to compound (B) was further added using the compound (B), it can be seen that Example 6 was able to introduce silyl groups more selectively to the allyl groups of polymer (C-1). While Comparative Examples 7 to 12 did not show an increase in the silyl group introduction rate compared to Comparative Example 2, a significant increase in the silyl group introduction rate was confirmed in Example 6 compared to Comparative Example 2. This shows that the addition of compound (B) having a specific structure is important for increasing the silyl group introduction rate.
[0131] Synthesis Example 2 Using polyoxypropylene glycol having a number-average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl group-containing organic polymer (F-2) having a number-average molecular weight of 14,500 and hydroxyl groups at both ends. To the hydroxyl group-containing organic polymer (F-2), 1.1 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-2) were added as a 28% methanol solution. After distilling off the methanol by vacuum distillation, 1.3 molar equivalents of allyl chloride relative to the hydroxyl groups of the polymer (F-2) were added and the mixture was reacted at 130°C for 1 hour, after which the allyl chloride was distilled off under reduced pressure. The resulting unpurified allyl-containing organic polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove metal salts from the polymer. As a result, an allyl group-containing organic polymer (C-2), which is the allyl group-containing compound (C), was obtained. The number average molecular weight of the polymer was 14,500.
[0132] Example 18 To a polymer (C-2) that is an allyl group-containing compound (C), 240 ppm of the ruthenium complex (A-2) obtained in Example 2, which is the ruthenium complex (A), was added, and further dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-2)) that is a hydrosilane compound (D) was added, and a hydrosilylation reaction of the allyl groups in the polymer (C-2) was carried out at 90°C. 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-2) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 3.
[0133] Example 19 Polymer (C-2), which is the allyl group-containing compound (C), was used to prepare a ruthenium compound (A') [RuCl 2 (nbd)] n240 ppm of 2,3-dibromonorbornadiene (compound (B)) and 620 ppm of 2,3-dibromonorbornadiene were added, and the mixture was stirred at 90° C. for 10 minutes. Further, dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in polymer (C-2)) (hydrosilane compound (D)) was added, and a hydrosilylation reaction of the allyl groups in polymer (C-2) was carried out at 90° C. Every hour from the start of the reaction, 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-2) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 3.
[0134] Comparative Examples 13 and 14: Polymer (C-2), which is the allyl group-containing compound (C), was reacted with a Karstedt catalyst or a ruthenium compound (A') [RuCl 2 (nbd)] n 240 ppm of methyl silane was added, and then dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-2)) as the hydrosilane compound (D) was added, and a hydrosilylation reaction of the allyl groups in the polymer (C-2) was carried out at 90°C. 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-2) were completely consumed, after which the volatile components were distilled off under reduced pressure to obtain a silyl group-containing polymer. 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 3.
[0135]
[0136] As is clear from Table 3, compared to Comparative Examples 13 and 14, which used the Karstedt catalyst or ruthenium compound (A'), Example 18, which used ruthenium complex (A), and Example 19, which used ruthenium compound (A') and compound (B), showed that silyl groups could be introduced more selectively into the allyl groups of polymer (C-2). Thus, it was confirmed that a high silyl group introduction rate could be achieved by performing a hydrosilylation reaction using the production method of the present invention even on polymer (C) having a number average molecular weight of 14,500.
[0137] Synthesis Example 3 Using polyoxypropylene glycol having a number-average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized with a zinc hexacyanocobaltate glyme complex catalyst to obtain a hydroxyl group-containing organic polymer (F-3) having a number-average molecular weight of 27,600 and hydroxyl groups at both ends. To the hydroxyl group-containing organic polymer (F-3), 1.1 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-3) were added as a 28% methanol solution. After distilling off the methanol by vacuum distillation, 1.3 molar equivalents of allyl chloride relative to the hydroxyl groups of the polymer (F-3) were added and the mixture was reacted at 130°C for 1 hour, after which the allyl chloride was distilled off under reduced pressure. The resulting unpurified allyl group-containing organic polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove metal salts from the polymer. In this manner, an allyl group-containing organic polymer (C-3), which is the allyl group-containing compound (C), was obtained. The number average molecular weight of the polymer was 27,600.
[0138] Example 20 To a polymer (C-3) that is an allyl group-containing compound (C), 240 ppm of the ruthenium complex (A-2) that is the ruthenium complex (A) obtained in Example 2 and dimethoxymethylsilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-3)) that is a hydrosilane compound (D) were added, and a hydrosilylation reaction of the allyl groups in the polymer (C-3) was carried out at 90°C. 1H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-3) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 4.
[0139] Examples 21 to 25 Each ruthenium compound (A') and each compound (B) were added to polymer (C-3), which is the allyl group-containing compound (C), as shown in Table 4, and the mixture was stirred at 90°C for 10 minutes. Furthermore, dimethoxymethylsilane, which is hydrosilane compound (D) (5.0 molar equivalents relative to the allyl groups in polymer (C-3)), was added, and the allyl groups in polymer (C-3) were subjected to a hydrosilylation reaction at 90°C. Every hour from the start of the reaction, 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-3) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 4.
[0140] (Comparative Examples 15 to 17) To polymer (C-3), which is the allyl group-containing compound (C), 240 ppm of a commercially available Karstedt catalyst or each ruthenium compound (A') and dimethoxymethylsilane, which is hydrosilane compound (D) (5.0 molar equivalents relative to the allyl groups in polymer (C-3)), were added, and the allyl groups in polymer (C-3) were hydrosilylated at 90°C. 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-3) were completely consumed, after which the volatile components were distilled off under reduced pressure to obtain a silyl group-containing polymer. 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 4.
[0141]
[0142] As is clear from Table 4, in Examples 20 to 25, silyl groups were introduced more selectively into the allyl groups of the allyl group-containing organic polymer than in Comparative Examples 15 to 17. This confirms that a high silyl group introduction rate can be achieved by carrying out a hydrosilylation reaction using the production method of the present invention even for polymer (C) having a number average molecular weight of 27,600.
[0143] Example 26 The polymer (C-2) which is the allyl group-containing compound (C) obtained in Synthesis Example 2 was treated with a ruthenium compound (A') [RuCl 2 (nbd)] n 240 ppm of 2,3-dibromonorbornadiene (compound (B)), and 620 ppm of 2,3-dibromonorbornadiene were added, and the mixture was stirred at 100° C. for 10 minutes. Further, triethoxysilane (5.0 molar equivalents relative to the allyl groups in polymer (C-2)) (hydrosilane compound (D)) was added, and a hydrosilylation reaction of the allyl groups in polymer (C-2) was carried out at 100° C. Every hour from the start of the reaction, 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-2) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated products was calculated by H NMR measurement. The results are shown in Table 5.
[0144] Comparative Example 18 The polymer (C-2) which is the allyl group-containing compound (C) obtained in Synthesis Example 2 was added with [RuCl 2 (nbd)] n 240 ppm of silyl group-containing polymer was added, and then triethoxysilane (5.0 molar equivalents relative to the allyl groups in the polymer (C-2)) as the hydrosilane compound (D) was added, and the allyl groups in the polymer (C-2) were subjected to a hydrosilylation reaction at 100°C. After the reaction was continued for 5 hours from the start of the reaction, the volatile components were distilled off under reduced pressure to obtain a silyl group-containing polymer. The resulting polymer was 1The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated product was calculated by H NMR measurement. The results are shown in Table 5.
[0145]
[0146] As is clear from Table 5, in Example 26, silyl groups were introduced more selectively to the allyl groups of the allyl group-containing organic polymer than in Comparative Example 18. This confirms that a high silyl group introduction rate can be achieved by carrying out a hydrosilylation reaction using the production method of the present invention even with other types of hydrosilane compounds.
[0147] Example 27 To 1-octene (1.0 g, 8.9 mmol), which is the allyl group-containing compound (C), 2 mg of ruthenium complex (A-2), which is the ruthenium complex (A) obtained in Example 2, was added with stirring at 60°C, and dimethoxymethylsilane (1.4 g, 13.4 mmol), which is the hydrosilane compound (D), was further added, and a hydrosilylation reaction of the allyl group in 1-octene was carried out at 60°C. 1 H NMR measurement confirmed that the allyl groups of 1-octene were completely consumed in 30 minutes, and that the silylated product was produced in a yield of 99% or more. Therefore, it was confirmed that the production method of the present invention can be applied without any problems even when the allyl group-containing compound (C) is a low-molecular-weight compound that is not a polymer.
[0148] Example 28 In an atmosphere of 23°C and 50% relative humidity, 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-1), which is the silyl group-containing compound (E) obtained in Example 19, was mixed with 90 parts by weight of DINP (diisononyl phthalate, manufactured by J-Plus Corporation), 160 parts by weight of Hakuenka CCR (precipitated calcium carbonate, manufactured by Shiraishi Calcium Co., Ltd.), and 100 parts by weight of silyl group-containing organic polymer (E-1). 54 parts by weight of SB (manufactured by Shiraishi Calcium Co., Ltd.: heavy calcium carbonate), 5 parts by weight of Typaque R820 (manufactured by Ishihara Sangyo Kaisha, Ltd.: titanium oxide), 2 parts by weight of Disparlon 6500 (manufactured by Kusumoto Chemical Co., Ltd.: fatty acid amide wax), 1 part by weight of Tinuvin 326 (manufactured by BASF: 2-(3-tert-butyl-2-hydroxy-5-methylphenyl)-5-chlorobenzotriazole), and Tinuvin 770 (manufactured by BASF: bis(2,2,6,6-tetramethyl-4-piperidinyl) To a mixture of these, 1 part by weight of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane (manufactured by Momentive), 5 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd., dibutyltin bis(acetylacetonate)) were added, and the mixture was thoroughly mixed with a spatula, and then uniformly mixed and degassed using a planetary centrifugal mixer to obtain a curable composition.
[0149] (Skinning Time) The obtained curable composition was filled into a mold about 5 mm thick using a spatula under an atmosphere of 23°C and 50% relative humidity, and the time when the surface was smoothed to a flat surface was defined as the curing initiation time. The surface was touched with the spatula, and the time when the composition to be evaluated no longer adhered to the spatula was defined as the skinning time. The results are shown in Table 6.
[0150] (Dumbbell Tensile Properties) The resulting curable composition was filled into a mold and aged for two days at 23°C and 50% relative humidity, followed by two days at 50°C, to produce a sheet-like cured product approximately 3 mm thick. The sheet-like cured product was punched into a No. 3 dumbbell shape and subjected to a tensile strength test at 23°C and 50% relative humidity to measure the modulus at 50% and 100% elongation (M50 and M100). The strength at break (TB) and elongation (EB) were also measured. Measurements were performed using an autograph (AGS-J) manufactured by Shimadzu Corporation at a tensile speed of 200 mm / min. The results are shown in Table 6.
[0151] Example 29 A curable composition was obtained in the same manner as in Example 28, except that 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-2), which was the silyl group-containing compound (E) obtained in Example 20, was used instead of 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-1). Using the obtained curable composition, the skinning time and dumbbell tensile properties were evaluated in the same manner as in Example 28. The results are shown in Table 6.
[0152] Comparative Example 19 A curable composition was obtained in the same manner as in Example 28, except that 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E'-1) obtained in Comparative Example 13 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-1). Using the obtained curable composition, the skinning time and dumbbell tensile properties were evaluated in the same manner as in Example 28. The results are shown in Table 6.
[0153] Comparative Example 20 A curable composition was obtained in the same manner as in Example 28, except that 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E'-2) obtained in Comparative Example 15 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-1). Using the obtained curable composition, the skinning time and dumbbell tensile properties were evaluated in the same manner as in Example 28. The results are shown in Table 6.
[0154]
[0155] As can be seen from Table 6, the hydrolyzable silyl group-containing organic polymer (E-1) obtained by the production method of the present invention exhibited a shorter skinning time and better curing properties than the hydrolyzable silyl group-containing organic polymer (E'-1) produced using the same allyl group-containing organic polymer (C-2) as a raw material and a Karstedt catalyst. Furthermore, the modulus and strength increased, with M100 being approximately 1.6 times and the strength being approximately 1.1 times. Furthermore, the hydrolyzable silyl group-containing organic polymer (E-2) obtained by the production method of the present invention exhibited a shorter skinning time and better curing properties than the hydrolyzable silyl group-containing organic polymer (E'-2) produced using the same allyl group-containing organic polymer (C-3) as a raw material and a Karstedt catalyst. Furthermore, the modulus and strength increased, with M100 being approximately 1.7 times and the strength being approximately 1.3 times.
[0156] Synthesis Example 4 To the hydroxyl group-containing organic polymer (F-3) obtained in Synthesis Example 3, 0.9 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-3) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 1.2 molar equivalents of 3-chloro-2-methyl-1-propene (methallyl chloride) relative to the hydroxyl groups of the polymer (F-3) were added and the mixture was reacted at 130°C for 1 hour to convert the terminal hydroxyl groups to methallyl groups, after which the 3-chloro-2-methyl-1-propene (methallyl chloride) was distilled off under reduced pressure. Thereafter, 0.6 molar equivalents of sodium methoxide relative to the hydroxyl groups of the polymer (F-3) were added as a 28% methanol solution. After removing the methanol by distillation under reduced pressure, 0.7 molar equivalent of 3-chloro-2-methyl-1-propene (methallyl chloride) relative to the hydroxyl groups of the polymer (F-3) was added and the reaction was carried out at 130°C for 1 hour to convert the remaining terminal hydroxyl groups to methallyl groups, and then the 3-chloro-2-methyl-1-propene (methallyl chloride) was distilled off under reduced pressure. The resulting unpurified methallyl group-containing organic polymer was mixed and stirred with n-hexane and water, after which the water was removed by centrifugation. The hexane was then distilled off under reduced pressure from the resulting hexane solution to remove the metal salts in the polymer. In this way, a methallyl group-containing organic polymer (G-1), which is the methallyl group-containing compound (G), was obtained. To the methallyl group-containing organic polymer (G-1), 100 ppm of Karstedt's catalyst and 1,000 ppm of 2,5-di-t-butyl-1,4-benzoquinone were added, and further, dimethoxymethylsilane (1.5 molar equivalents relative to the methallyl groups in the polymer (G-1)) as the hydrosilane compound (D) was added, and the hydrosilylation reaction of the methallyl groups in the polymer (G-1) was carried out at 100°C. 1 H NMR measurement was carried out, and the reaction was continued until the methallyl groups of the polymer (G-1) were completely consumed, after which the volatile components were distilled off under reduced pressure to obtain a silyl group-containing polymer (E'-3).
[0157] Example 30 Using a 5 L planetary mixer (manufactured by Dalton Co., Ltd.), a one-component curable composition was prepared according to the formulation shown in Table 7. First, 160 parts by weight of Ultra-Pflex (manufactured by Specialty Minerals: colloidal calcium carbonate), 54 parts by weight of Q3T (manufactured by Huber: surface-untreated heavy calcium carbonate), and 20 parts by weight of Ti-Pure R-902+ (manufactured by Chemours: titanium oxide) were dried under reduced pressure at 120°C for 2 hours. Next, 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-3), which is the silyl group-containing compound (E) obtained in Example 22, 90 parts by weight of DINP (diisononyl phthalate manufactured by J-Plus Corporation), 2 parts by weight of Crayvallac SL (fatty acid amide wax manufactured by ARKEMA), 1 part by weight of Tinuvin 328 (ultraviolet absorber manufactured by BASF), and 1 part by weight of Tinuvin 770 (light stabilizer manufactured by BASF) were each charged into a mixer and kneaded for 10 minutes. The resulting mixture was removed and passed through a three-roll mill once to uniformly disperse the mixture, and then charged back into the mixer and dehydrated under reduced pressure for 2 hours. After dehydration under reduced pressure, the mixture was cooled to 50°C or below, and then 3 parts by weight of A-171 (manufactured by Momentive: vinyltrimethoxysilane), 3 parts by weight of A-1120 (manufactured by Momentive: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane), and 2 parts by weight of Neostan U-220H (manufactured by Nitto Kasei Co., Ltd., dibutyltin bis(acetylacetonate)) were added and kneaded for 3 minutes. Subsequently, the mixture was degassed under reduced pressure for 2 minutes, and the resulting mixture was immediately filled into a moisture-proof aluminum cartridge and sealed to obtain a curable composition.
[0158] (Skinning time) The obtained curable composition was filled into a mold about 5 mm thick using a spatula under an atmosphere of 23°C and 50% relative humidity, and the time when the surface was smoothed to a flat surface was defined as the curing initiation time. The surface was touched with the spatula, and the time when the composition to be evaluated no longer adhered to the spatula was defined as the skinning time. The results are shown in Table 7.
[0159] (Dumbbell Tensile Properties) The resulting curable composition was filled into a mold and aged for 3 days at 23°C and 50% relative humidity, and then for 4 days at 50°C to produce a sheet-like cured product approximately 3 mm thick. The sheet-like cured product was punched into a No. 3 dumbbell shape and subjected to a tensile strength test at 23°C and 50% relative humidity to measure the modulus at 50% and 100% elongation (M50 and M100). The strength at break (TB) and elongation (EB) were also measured. Measurements were performed using an autograph (AGS-J) manufactured by Shimadzu Corporation at a tensile speed of 200 mm / min. The results are shown in Table 7.
[0160] (Tear Strength) The obtained curable composition was filled into a 3 mm thick sheet mold at 23°C and 50% relative humidity. After curing for 3 days at 23°C and 50% relative humidity, the composition was aged in a 50°C dryer for 4 days to obtain a sheet-like cured product. The obtained cured product was punched into a dumbbell shape (JIS Type A) for tear testing to obtain a test specimen. Using the obtained test specimen, a tear test (tensile speed 200 mm / min) was performed using an autograph at 23°C and 50% relative humidity to measure the stress at break (TB).
[0161] (Tensile Shear Strength) At 23°C and 50% relative humidity, the above-mentioned curable composition was applied to an aluminum substrate with a bonding area of 25 mm x 25 mm and a thickness of 50 μm. After a 2-minute open time, the substrates were bonded together. The resulting specimens were left at a constant temperature and humidity of 23°C and 50% relative humidity. After 1 hour, 3 hours, and 24 hours, a tensile shear test (tensile speed 50 mm / min) was performed using an autograph to measure the stress at break (TB). The resulting specimens were aged for 3 days at 23°C and 50% relative humidity, and then for 4 days at 50°C, after which a tensile shear test was performed using an autograph to measure the stress at break (TB). The strength development rate at each time point was calculated as follows: Strength development rate (%) = (shear strength at each time) ÷ (shear strength after aging at 23°C and 50% relative humidity for 3 days and then at 50°C for 4 days) × 100 The results are shown in Table 7.
[0162] Comparative Example 21 A curable composition was obtained in the same manner as in Example 30, except that 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E'-2) obtained in Comparative Example 15 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-3). Using the obtained curable composition, the skinning time, dumbbell tensile properties, tear strength, and tensile shear strength were evaluated in the same manner as in Example 30. The results are shown in Table 7.
[0163] Comparative Example 22 A curable composition was obtained in the same manner as in Example 30, except that 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E'-3) obtained in Synthesis Example 4 was used instead of 100 parts by weight of the hydrolyzable silyl group-containing organic polymer (E-3). Using the obtained curable composition, the skinning time, dumbbell tensile properties, tear strength, and tensile shear strength were evaluated in the same manner as in Example 30. The results are shown in Table 7.
[0164]
[0165] As can be seen from Table 7, the hydrolyzable silyl group-containing organic polymer (E-3) obtained by the production method of the present invention exhibited a shorter skinning time and better curing properties than the hydrolyzable silyl group-containing organic polymer (E'-2) produced using a Karstedt catalyst from the same allyl group-containing organic polymer (C-3) as a raw material, and the hydrolyzable silyl group-containing organic polymer (E'-3) produced using a Karstedt catalyst from the methallyl group-containing organic polymer (G-1) as a raw material. It also exhibited better tear strength and tensile shear strength. In a dumbbell tensile test, the hydrolyzable silyl group-containing organic polymer (E-3) exhibited a higher modulus and strength than the hydrolyzable silyl group-containing organic polymer (E'-2), and showed values comparable to those of the hydrolyzable silyl group-containing organic polymer (E'-3).
[0166] Examples 31 to 34 As shown in Table 8, the polymer (C-3) which is the allyl group-containing compound (C) was used in combination with the ruthenium compound (A') [RuCl 2 (nbd)] n100 ppm of methyl silane and 260 ppm of 2,3-dibromonorbornadiene, which is compound (B), were added, and the mixture was stirred for 10 minutes at the reaction temperature shown in Table 8. Furthermore, dimethoxymethylsilane, which is hydrosilane compound (D), was added (in the molar equivalent shown in Table 8 relative to the allyl groups in polymer (C-3)), and a hydrosilylation reaction of the allyl groups in polymer (C-3) was carried out. 1 H NMR measurement was carried out, and the reaction was continued until the allyl groups in the polymer (C-3) were completely consumed, and then the volatile components were distilled off under reduced pressure to obtain a polymer that was a silyl group-containing compound (E). 1 The ratio of each group to the total of silyl groups, 1-propenyl groups, and hydrogenated products was calculated by H NMR measurement. The viscosity of the polymer was measured at 23°C using a viscometer RE85U (manufactured by Toki Sangyo Co., Ltd.). The results are shown in Table 8.
[0167]
[0168] As is clear from Table 8, in all of Examples 31 to 34, silyl groups were introduced with high selectivity. In particular, it can be seen that the greater the molar equivalent of the hydrosilane compound (D) relative to the allyl groups in the polymer (C-3), the higher the silyl group introduction rate and the lower the viscosity of the hydrolyzable silyl group-containing organic polymer. In Example 31, in which 5 molar equivalents of the hydrosilane compound (D) were reacted with the allyl groups in the polymer (C-3), a polymer with the highest silylation rate and the lowest viscosity was obtained among those in Table 8. In Example 32, in which 3 molar equivalents of the hydrosilane compound (D) were reacted with the allyl groups in the polymer (C-3), the silylation rate was lower and the viscosity after silylation was higher than in Example 31. However, a polymer with a lower viscosity was obtained than in Example 33, in which 2 molar equivalents of the hydrosilane compound (D) were reacted with the allyl groups in the polymer (C-3).
Claims
1. A ruthenium complex (A) having a compound (B) as a ligand, in which compound (B) has at least one carbon-carbon double bond in one molecule, and an electron-withdrawing group is bonded to at least one or more of the carbon atoms forming the carbon-carbon double bond.
2. The ruthenium complex (A) according to claim 1, wherein the compound (B) has a benzene ring skeleton as the skeleton containing the carbon-carbon double bond.
3. The ruthenium complex (A) according to claim 1, wherein the compound (B) has a norbornadiene skeleton as the skeleton containing the carbon-carbon double bond.
4. The ruthenium complex (A) according to any one of claims 1 to 3, wherein the electron-withdrawing group is at least one selected from the group consisting of a fluoro group, a bromo group, and an iodo group.
5. The ruthenium complex (A) according to claim 2, wherein the compound (B) is at least one selected from the group consisting of 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,4-diiodobenzene, and 1,3,5-tribromobenzene.
6. The ruthenium complex (A) according to claim 3, wherein the compound (B) is 2,3-dibromonorbornadiene.
7. A hydrosilylation reaction catalyst comprising the ruthenium complex (A) according to claim 1.
8. A method for producing a silyl group-containing compound (E), comprising the step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), and the hydrosilylation reaction catalyst according to claim 7, and carrying out a hydrosilylation reaction.
9. The method according to claim 8, further comprising mixing a compound (B) in the hydrosilylation reaction.
10. A method for producing a silyl group-containing compound (E), comprising the step of mixing an allyl group-containing compound (C), a hydrosilane compound (D), a ruthenium compound (A') not having compound (B) as a ligand, and compound (B) to carry out a hydrosilylation reaction, wherein compound (B) has at least one carbon-carbon double bond in one molecule, and at least one of the carbon atoms forming the carbon-carbon double bond has an electron-withdrawing group bonded to it.
11. The process according to any one of claims 8 to 10, wherein the amount of the hydrosilane compound (D) used is 3 molar equivalents or more relative to the allyl groups contained in the allyl group-containing compound (C).
12. The method according to any one of claims 8 to 10, wherein the silyl group-containing compound (E) is a polymer having a number average molecular weight of more than 3,000.
13. The method according to any one of claims 8 to 10, wherein the silyl group-containing compound (E) is a hydrolyzable silyl group-containing polymer.
14. The process according to claim 13, wherein the silyl group-containing compound (E) is a hydrolyzable silyl group-containing polyoxyalkylene polymer.
15. The method according to any one of claims 8 to 10, wherein compound (B) has a benzene ring skeleton as the skeleton containing the carbon-carbon double bond.
16. The method according to any one of claims 8 to 10, wherein compound (B) has a norbornadiene skeleton as the skeleton containing the carbon-carbon double bond.
17. The method according to any one of claims 8 to 10, wherein the electron-withdrawing group is at least one selected from the group consisting of a fluoro group, a bromo group, and an iodo group.
18. The production method according to claim 15, wherein compound (B) is at least one selected from the group consisting of 1,4-dibromobenzene, 1-bromo-3,5-difluorobenzene, 1-bromo-2,6-difluorobenzene, 1,4-diiodobenzene, and 1,3,5-tribromobenzene.
19. The method according to claim 16, wherein compound (B) is 2,3-dibromonorbornadiene.
20. The process according to claim 10, wherein the ruthenium compound (A') has a ligand selected from 2,5-norbornadiene, benzene, and p-cymene.
21. A polymer mixture comprising a hydrolyzable silyl group-containing polymer and the ruthenium complex (A) according to any one of claims 1 to 3.
22. A curable composition comprising the polymer mixture of claim 21 and a curing catalyst.
23. A cured product obtained by curing the curable composition according to claim 22.
Citation Information
Patent Citations
JP1971027250B1
Receiving device
JP1984015336A
Production of unsaturated group-terminated polyalkylene oxide
JP1986215623A
JP1989060722U
Magnetic recording medium