Resin composition
The resin composition with aluminum nitride fillers and silicone resin addresses the limitations of conventional heat dissipation materials by achieving high thermal conductivity and low thermal resistance, facilitating efficient heat dissipation and thin film formation in electronic components.
Patent Information
- Application Number
- PCT/JP2024/015815
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-04-23
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional resin compositions used for heat dissipation in electronic components face limitations in achieving high thermal conductivity and thin film formation due to the use of large thermally conductive fillers, which restricts their ability to efficiently dissipate heat and reduce thermal resistance.
A resin composition incorporating aluminum nitride-based thermally conductive fillers with a specific particle size distribution and polyhedral shape, combined with a silicone resin and platinum-based catalyst, enhances filling properties and thermal conductivity, allowing for easy formation of thin films with improved dischargeability and reduced thermal resistance.
The resin composition achieves high thermal conductivity (6.0 W/m·K or more) and low thermal resistance, enabling efficient heat dissipation and easy manufacturing of electronic components with thin film formation, while maintaining excellent discharge properties.
Smart Images

Figure JP2024015815_31102024_PF_FP_ABST
Abstract
Description
resin composition
[0001] The present invention relates to a resin composition containing a thermally conductive filler.
[0002] As electronic devices become more sophisticated, the density and packaging of semiconductor elements is increasing, making it increasingly important to efficiently dissipate heat generated by the electronic components that make up the electronic devices.
[0003] For example, in semiconductor devices, heat dissipation materials are used to efficiently dissipate heat generated by electronic components. Heat dissipation materials are materials that reduce the thermal resistance of the path through which heat generated by semiconductor elements is released to a heat sink or housing, and come in a variety of forms, such as sheets, gels, and greases.
[0004] A typical example of a heat dissipation member is a resin composition in which a heat-conductive filler such as aluminum nitride is filled into a silicone resin having excellent heat resistance (see, for example, Patent Documents 1 and 2).
[0005] Resin compositions used as such heat dissipation members are required to have high thermal conductivity in order to efficiently dissipate heat. Known methods for increasing thermal conductivity include increasing the filling rate of thermally conductive fillers or combining multiple thermally conductive fillers with different average particle sizes to efficiently form a heat path.
[0006] Furthermore, in order to efficiently dissipate heat from electronic components, it is also effective to shorten the path from the electronic component, which is the heat source, to the heat sink or housing as much as possible, that is, to reduce the thermal resistance by making the resin composition thinner.
[0007] It is known that in order to obtain high thermal conductivity, thermally conductive fillers with different average particle sizes are combined to improve filling. However, in the conventional combinations of thermally conductive fillers, thermally conductive fillers with large particle sizes are used, which limits the thinning of the resin composition.
[0008] For example, Patent Document 1 discloses a resin composition with excellent thermal conductivity, which contains a specific ratio of thermally conductive inorganic particles of 100 μm to 500 μm and thermally conductive inorganic particles of 0.01 μm to less than 100 μm. In the examples of Patent Document 1, a resin composition with a relatively high thermal conductivity of 6.4 to 11.1 W / mK is obtained. However, because a large amount of large filler with a particle size of 100 μm or more is used, it is not possible to form the resin composition into a film thickness of 100 μm or less, and there are limitations to how thin the resin composition can be made.
[0009] On the other hand, when attempting to prepare a resin composition without using a filler with a large particle size in order to make the resin composition thinner, the combination of thermally conductive fillers with different average particle sizes is limited, making it difficult to obtain high filling properties. Therefore, in practice, it is necessary to reduce the blending ratio of the thermally conductive filler to improve dischargeability and fluidity, which limits the improvement in thermal conductivity.
[0010] For example, Patent Document 2 discloses a thermally conductive silicone composition (resin composition) that has high thermal conductivity, good compressibility to 10 μm or less (enabling thin film formation), and excellent dischargeability within a specific viscosity range. However, the thermal conductivity of the thermally conductive silicone composition disclosed in the examples of Patent Document 2 is at most 2.0 W / m K, and further improvement in thermal conductivity is desired.
[0011] WO2022 / 130665 JP 2020-169231 A
[0012] As described above, in conventional technologies, when increasing the filler packing density to achieve high thermal conductivity, it is necessary to use a filler with a large particle size, making it difficult to form thin films. Furthermore, filler compositions intended to form thin films do not allow for practically high amounts of thermally conductive filler, limiting the improvement in thermal conductivity. Therefore, there is room for improvement from the perspective of thinning the resin composition to reduce thermal resistance and improve the heat dissipation properties of electronic components. Therefore, an object of the present invention is to provide a resin composition that can easily produce electronic components with excellent heat dissipation properties.
[0013] The present inventors conducted extensive research to achieve the above-mentioned object. As a result, they discovered that by using a thermally conductive filler containing particles of a specific shape, the filler's packing ability and thermal conductivity can be improved, and therefore, even in a resin composition that can be made into a thin film without using a filler with a large particle size, it is easy to discharge from a syringe and has high thermal conductivity. Further investigation surprisingly revealed that, even when the thickness and thermal conductivity of the resin compositions are the same, when a resin composition with excellent dischargeability from a syringe is used, the thermal resistance is significantly lower than when a resin composition with poor dischargeability is used. This led to the completion of the present invention.
[0014] That is, the present invention is a resin composition comprising a resin and an aluminum nitride-based thermally conductive filler, characterized in that the resin composition has a thermal conductivity of 6.0 W / m·K or more as measured by a hot disk method, a discharge rate of 10 g / min or more when filled into a syringe having an inner diameter of a 2 mm tip discharge part and discharged at a discharge pressure of 0.62 MPa, and a thickness of 100 μm or less as measured after 0.02 ml of the resin composition is sandwiched between two 10 mm x 10 mm silicon chips and a force of 50 N is applied for 60 seconds.
[0015] In the aluminum nitride thermally conductive filler, in a volumetric particle size distribution measured by a laser diffraction scattering method, the proportion of particles having a particle diameter of 100 μm or less is preferably 90% or more of all particles, the proportion of particles having a particle diameter of 5 μm or more and 100 μm or less is 40 to 90% of all particles, and the proportion of particles having a particle diameter of 0.05 μm or more and less than 5 μm is preferably 5 to 60%, and in a scanning electron microscope image taken at 500x magnification, 50% or more of the particles in the particle diameter range of 5 μm to 50 μm or less are polyhedral particles having at least two flat surfaces. Furthermore, the polyhedral particles are preferably aluminum nitride particles.
[0016] The resin is preferably a silicone resin, and the silicone resin contains a polyorganosiloxane containing an average of two or more alkenyl groups bonded to silicon atoms per molecule, and a polyorganosiloxane having an average of two or more hydrosilyl groups per molecule. It is also preferable that the resin composition further contains a platinum-based catalyst.
[0017] The resin composition can be used as a heat dissipation member, and an example of the present invention is an electronic component that includes a heat dissipation member containing the resin composition and a substrate having a heat-generating portion, and is arranged so that the heat dissipation member is in contact with the heat-generating portion.
[0018] That is, the present invention relates to the following [1] to [7]: [1] A resin composition containing a resin and an aluminum nitride-based thermally conductive filler, characterized in that the resin composition has a thermal conductivity of 6.0 W / m K or more as measured by a hot disk method, a discharge rate of 10 g / min or more when filled into a syringe having an inner diameter of a 2 mm tip discharge part and discharged at a discharge pressure of 0.62 MPa, and a thickness of 100 μm or less as measured when 0.02 ml of the resin composition is sandwiched between two 10 mm x 10 mm silicon chips and a force of 50 N is applied for 60 seconds.
[0019] [2] The resin composition according to [1], wherein the thermally conductive filler has a particle size distribution on a volume basis measured by a laser diffraction scattering method, in which 90% or more of all particles have a particle size in the range of 100 μm or less, and in the volumetric particle size distribution, 40 to 90% of all particles have a particle size of 5 μm or more and 100 μm or less, and 5 to 60% of all particles have a particle size of 0.05 μm or more and less than 5 μm, and in a scanning electron microscope image taken at 500x magnification, 50% or more of the particles in the particle size range of 5 μm or more and 50 μm or less are polyhedral particles having at least two flat surfaces.
[0020] [3] The resin composition according to [2], wherein the polyhedral particles are aluminum nitride particles.
[0021] [4] The resin composition according to any one of [1] to [3], wherein the resin is a silicone resin.
[0022] [5] The silicone resin contains a polyorganosiloxane having an average of two or more alkenyl groups bonded to silicon atoms per molecule, and a polyorganosiloxane having an average of two or more hydrosilyl groups per molecule, and further contains a platinum-based catalyst. [4] The resin composition according to.
[0023] [6] A heat dissipation member comprising the resin composition according to any one of [1] to [5].
[0024] [7] An electronic component comprising the heat dissipation member according to [6] and a base material having a heat generating portion, the heat dissipation member being arranged so as to be in contact with the heat generating portion.
[0025] The present invention provides a resin composition that has high thermal conductivity, is easily discharged from a syringe, and can be formed into a thin film. By using such a resin composition as a heat dissipation material for electronic components, it is possible to significantly reduce thermal resistance, and because the resin composition has high thermal conductivity, it is possible to efficiently cool heat-generating parts of electronic devices. Furthermore, because the resin composition has excellent dischargeability, it is possible to improve the efficiency of manufacturing electronic components.
[0026] In one embodiment of the aluminum nitride powder of the present invention, a scanning electron microscope image of polyhedral particles in the particle diameter range of 5 to 50 μm was taken at a magnification of 500 times.
[0027] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and can be implemented with any modifications within the scope of the gist of the present invention.
[0028] [Resin Composition] The resin composition of the present invention contains a resin and an aluminum nitride-based thermally conductive filler, and is characterized by having a thermal conductivity of 6.0 W / m·K or more as measured by the hot disk method, a discharge rate of 10 g / min or more when filled into a syringe with an inner diameter of a 2 mm tip and discharged at a discharge pressure of 0.62 MPa, and a thickness of 100 μm or less measured after 0.02 ml of the resin composition is sandwiched between two 10 mm x 10 mm silicon chips and a force of 50 N is applied for 60 seconds. Using the resin composition as a heat dissipation material can achieve extremely low thermal resistance. Additionally, electronic components that can efficiently cool heat-generating components in electronic devices can be efficiently manufactured.
[0029] The resin composition has a thermal conductivity of 6.0 W / m·K or more, which means that it has high thermal conductivity and can provide high heat dissipation performance when used as a heat dissipation component. This makes it possible to efficiently cool heat-generating parts of electronic devices. The thermal conductivity of the resin composition is preferably 8.0 W / m·K or more, and more preferably 10.0 W / m·K or more. There is no particular upper limit to the thermal conductivity, and the higher the better, but it is generally 20.0 W / m·K or less.
[0030] The thermal conductivity of the resin composition is measured by a hot disc method. Specifically, the resin composition is hot-pressed at 100°C to obtain a sheet having a thickness of 7 mm, and the thermal conductivity of the sheet is measured using a hot disc thermophysical property measuring device.
[0031] The resin composition has a discharge rate of 10 g / min or more when filled into a syringe with an inner diameter of 2 mm at the tip of the discharge port and discharged at a discharge pressure of 0.62 MPa. This characteristic allows for a reduction in thermal resistance, even when the thermal conductivity and thickness of the resin composition phase are kept the same, compared to when a resin composition with a lower discharge rate is used. The reason for this is unclear, but the inventors believe it to be as follows.
[0032] Generally, thermal resistance R is expressed by the formula R = L / TC + Rc, where L is the thickness of the resin composition layer, TC is the thermal conductivity of the resin composition, and Rc is the contact thermal resistance between the substrate and the resin composition. In the present invention, the decrease in thermal resistance is not caused by the value of L / TC, and is therefore thought to be due to the contact thermal resistance between the substrate and the resin composition. It is presumed that the resin composition is smoothly applied to the substrate during the manufacture of electronic components, resulting in uniform and gap-free lamination, which improves adhesion between the substrate and the resin composition and reduces the contact thermal resistance.
[0033] That is, if the resin composition has poor syringe dischargeability, when the resin composition is discharged from a syringe and applied to a substrate during the manufacture of electronic components, a large amount of pressure is applied to the resin composition, making it difficult to uniformly extrude it during dispensing. Therefore, it is presumed that the resin composition is not uniformly applied to the substrate surface, or that minute gaps are generated between the substrate and the resin composition, making it difficult to form a thermal path between the substrate and the resin composition, and that the contact thermal resistance cannot be sufficiently reduced. On the other hand, the resin composition of the present invention has excellent syringe dischargeability, which allows the resin composition to be uniformly applied to the substrate surface, and further, it is presumed that the generation of minute gaps between the substrate and the resin composition is easily suppressed, thereby sufficiently reducing the contact thermal resistance.
[0034] In addition, the high ejection properties make it possible to improve the efficiency of manufacturing electronic components.
[0035] The discharge rate is preferably 15.0 g / min or more, more preferably 30.0 g / min or more. If the discharge rate is too high, it may be difficult to control the discharge rate during production, so the discharge rate is preferably 500.0 g / min or less.
[0036] The discharge amount is measured by filling the resin composition into a syringe having an inner diameter of a tip discharge part of 2 mm, and discharging the resin composition at 25° C. under a discharge pressure of 0.62 MPa.
[0037] The resin composition has a thickness (corresponding to the bond line thickness, hereinafter sometimes referred to as "BLT") of 100 μm or less, measured after 0.02 ml of the resin composition is sandwiched between two 10 mm x 10 mm silicon chips and a force of 50 N is applied for 60 seconds. This characteristic indicates that the resin composition can be easily formed into a thin film of 100 μm or less (that it can be thinned). Furthermore, this characteristic allows the resin composition to be formed into a thin film by a simple operation during the manufacture of electronic components, making it easy to arrange the resin composition in thin film form on electronic components simply and inexpensively. The BLT is preferably 70 μm or less, and more preferably 60 μm or less. This makes it easy to arrange the resin composition in thin film form on electronic components to reduce thermal resistance and to improve manufacturing efficiency when the resin composition is arranged in thin film form during the manufacture of electronic components. In particular, since the resin composition of the present invention has a BLT of 100 μm or less, it is possible to suppress adverse effects on the substrate and to perform thin film molding even with a simple device with a low pressure of about 0.5 MPa, which is a great advantage in that it is possible to produce heat dissipation members easily and inexpensively. Although there is no particular restriction on the lower limit of the BLT, if an attempt is made to thin the resin composition, restrictions will arise on the thermally conductive filler that can be used, making it difficult to achieve both high thermal conductivity and high dischargeability. Therefore, the lower limit of the BLT is preferably 10 μm or more, more preferably 20 μm or more, and particularly preferably 30 μm or more.
[0038] The BLT is measured by sandwiching 0.02 ml of the resin composition between two 10 mm x 10 mm silicon chips and applying a force of 50 N for 60 seconds. Specifically, the resin composition is measured onto a silicon chip, and another silicon chip is placed on top of it to sandwich the resin composition between the two silicon chips. A sample is obtained by crushing with a force of 50 N for 60 seconds using a push-pull gauge (manufactured by Imada Co., Ltd., SVH-1000N). The thickness of the sample is then measured with a micrometer (manufactured by Mitutoyo Corporation, high-precision digimatic micrometer MDH-25MB), and the thickness of the resin composition (BLT) is calculated by subtracting the thickness of the silicon chips that were previously measured.
[0039] [Resin] The resin used in the resin composition of the present invention (i.e., the resin constituting the resin composition of the present invention) is not particularly limited, and known resins can be used without particular limitation. Examples of the resin include thermosetting resins such as epoxy resins, epoxy resins into which a mesogen group has been introduced (epoxy resins having a mesogen group), unsaturated polyester resins, polyimide resins, and phenolic resins, thermoplastic resins such as polyethylene, polypropylene, polyamide, polycarbonate, and polyphenylene sulfide, rubbers such as ethylene propylene rubber and styrene butadiene rubber, and silicone resins.
[0040] Among these resins, it is preferable to use a silicone resin as the resin in the resin composition of the present invention. Silicone resins have high heat resistance, allowing them to perform stably for long periods of time when used in heat dissipation components. However, due to their structure, intermolecular forces are weak, and compared to other resins such as epoxy resins, heat conduction between silicone resin molecules is poor. Therefore, when using silicone resins, it has been necessary to incorporate a large amount of thermally conductive filler in order to achieve particularly high thermal conductivity. Therefore, with silicone resin compositions using silicone resins, it has been difficult to achieve both high thermal conductivity and high syringe ejection properties. However, the present invention achieves both high thermal conductivity and high syringe ejection properties, which makes it easy to reduce thermal resistance, and therefore is particularly effective.
[0041] The silicone resin may be a curable silicone resin or a non-curable silicone resin.
[0042] Examples of curable silicone resins include addition reaction type silicone resins and condensation reaction type silicone resins. When a hydrolyzable filler such as aluminum nitride is used as the thermally conductive filler, it is desirable to use an addition reaction type silicone resin.
[0043] The addition reaction type silicone resin can be, for example, a mixture of polyorganosiloxane (a) having alkenyl group and polyorganosiloxane (b) having hydrosilyl group, or a mixture of which a part or all of the mixture is crosslinked by hydrosilylation reaction using a catalyst.That is, the silicone resin can be a mixture containing polyorganosiloxane (a) having alkenyl group and polyorganosiloxane (b) having hydrosilyl group, or can be a crosslinked product of the mixture.
[0044] In addition, an alkoxysilyl group-containing compound (c) or dimethylpolysiloxane can also be used as the silicone resin. For example, when an alkoxysilyl group-containing compound (c) is used as the silicone resin, the silicone resin may consist solely of the alkoxysilyl group-containing compound (c), or may be a mixture of a polyorganosiloxane (a) having an alkenyl group, a polyorganosiloxane (b) having a hydrosilyl group, and an alkoxysilyl group-containing compound (c), or may be a crosslinked product of the mixture. In addition, the dimethylpolysiloxane that can be used as the silicone resin may also be an alkoxysilyl group-containing compound (c), such as a dimethylpolysiloxane in which one end of the molecular chain is blocked with an alkoxysilyl group. In a preferred and exemplary embodiment of the present invention, the silicone resin is a mixture of a polyorganosiloxane (a) having an alkenyl group, a polyorganosiloxane (b) having a hydrosilyl group, and an alkoxysilyl group-containing compound (c), or a crosslinked product of the mixture.
[0045] Alkenyl-containing polyorganosiloxane (a) The alkenyl-containing polyorganosiloxane (a) may be, for example, a polyorganosiloxane having an average composition formula R x j R y k SiO 〔4-(j+k)〕 / 2The polyorganosiloxane (a) may be used alone or in combination of two or more (i.e., the polyorganosiloxane (a) may be used alone or in combination of two or more).
[0046] R x is an alkenyl group. The alkenyl group is preferably a group having 2 to 8 carbon atoms, and examples thereof include a vinyl group, an allyl group, a 1-butenyl group, and a 1-hexenyl group, and a vinyl group is preferred.
[0047] The number of alkenyl groups bonded to silicon atoms in one molecule of the polyorganosiloxane (a) is preferably 1 or more on average, more preferably 2 or more on average. In other words, the polyorganosiloxane (a) contains, in one molecule, preferably 1 or more alkenyl groups bonded to silicon atoms on average, more preferably 2 or more on average. In addition, the alkenyl group may be bonded to a silicon atom at the end of the molecular chain, to a silicon atom in the middle of the molecular chain, or to both. However, from the viewpoint of the curing speed when curing this composition as described below, the physical properties of the resulting cured product, etc., it is preferable that the alkenyl group be bonded to at least a silicon atom at the end of the molecular chain, particularly to a silicon atom at both ends of the molecular chain.
[0048] R y R is a substituted or unsubstituted monovalent hydrocarbon group that does not contain an aliphatic unsaturated bond. y The number of carbon atoms in R is preferably 1 to 12, more preferably 1 to 10. yExamples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, hexyl, octyl, decyl, and dodecyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cyclobutyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, phenylethyl, and phenylpropyl; groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as chlorine, fluorine, and bromine, or with a cyano group, for example, halogenated hydrocarbon groups such as chloromethyl, trifluoropropyl, chlorophenyl, bromophenyl, dibromophenyl, tetrachlorophenyl, fluorophenyl, and difluorophenyl; and cyanoalkyl groups such as α-cyanoethyl, β-cyanopropyl, and γ-cyanopropyl. Among these, alkyl groups and aryl groups are preferred, and methyl and phenyl groups are more preferred.
[0049] j and k are positive numbers satisfying 0<j<3, 0<k<3, and 1<j+k<3, preferably 0.0005≦j≦1, 1.5≦k<2.4, and 1.5<j+k<2.5, and more preferably 0.001≦j≦0.5, 1.8≦k≦2.1, and 1.8<j+k≦2.2.
[0050] The molecular structure of the polyorganosiloxane (a) may be any of linear, branched, cyclic, and three-dimensional network structures, and the polyorganosiloxane (a) may be a mixture of these.
[0051] The viscosity of the polyorganosiloxane (a) at 23° C. is preferably 0.01 to 100 Pa·s, from the viewpoint that a composition having desired physical properties can be obtained with good workability.
[0052] Hydrosilyl Group-Containing Polyorganosiloxane (b) The hydrosilyl group-containing polyorganosiloxane (b) may be, for example, a polyorganosiloxane having an average composition formula R z m H n SiO [4-(m+n)] / 2The polyorganosiloxane (b) may be a polyorganosiloxane represented by the formula: One type of polyorganosiloxane may be used, or two or more types of polyorganosiloxanes may be used.
[0053] R z R is a substituted or unsubstituted monovalent hydrocarbon group that does not contain an aliphatic unsaturated bond. z Examples of the alkyl group include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, hexyl, cyclohexyl, and octyl; aryl groups such as phenyl and tolyl; aralkyl groups such as benzyl and phenylethyl; and groups in which some or all of the hydrogen atoms of these groups have been substituted with halogen atoms such as fluorine, chlorine, and bromine, or with cyano groups, such as chloromethyl, bromoethyl, trifluoropropyl, and cyanoethyl. Among these, from the standpoints of ease of synthesis, cost, and the like, alkyl groups are preferred, and methyl groups are more preferred.
[0054] m and n are numbers satisfying 0.5≦m≦2, 0<n≦2, 0.5<m+n≦3, preferably 0.6≦m≦1.9, 0.01≦n≦1.0, 0.6<m+n≦2.8. The hydrosilyl groups preferably have an average of two or more per molecule. In other words, the polyorganosiloxane (b) preferably has an average of two or more hydrosilyl groups per molecule.
[0055] The amount of the polyorganosiloxane (b) used is such that the number of hydrosilyl groups in the polyorganosiloxane (b) is 0.1 to 2.0, preferably 0.2 to 1.5, per alkenyl group bonded to a silicon atom of the polyorganosiloxane (a), from the viewpoint that a composition having desired physical properties and whose physical properties are unlikely to change over time can be easily obtained.
[0056] Alkoxysilyl Group-Containing Compound (c) As the alkoxysilyl group-containing compound (c), a compound having at least an alkoxysilyl group represented by the following formula (I) in one molecule is preferred, since it allows a composition with excellent workability to be easily obtained.
[0057] -SiR11 3-z (OR 12 ) z (I) (wherein R 11 is an alkyl group having 1 to 6 carbon atoms, preferably a methyl group, and R 12 is an alkyl group having 1 to 6 carbon atoms, preferably a methyl group, and z is 1, 2, or 3. Examples of compounds having an alkoxysilyl group represented by formula (I) include compounds represented by the following formula (1):
[0058] In the following formula (1), the repeating unit having the number of repeating units a, the repeating unit having the number of repeating units b, and the repeating unit having the number of repeating units c do not necessarily have to be arranged as shown in the following formula (1). For example, a repeating unit having the number of repeating units c may be present between the repeating unit having the number of repeating units a and the repeating unit having the number of repeating units b.
[0059]
[0060] (In formula (1), R 1 is a group having an alkoxysilyl group having 1 to 4 carbon atoms, and R 2 is a group having a siloxane unit represented by the following formula (2) or a monovalent hydrocarbon group having 6 to 18 carbon atoms, and R 3 are each independently a monovalent hydrocarbon group having 1 to 6 carbon atoms or a hydrogen atom, each X is independently a divalent hydrocarbon group having 2 to 10 carbon atoms or a group containing an ester bond and having 2 to 10 carbon atoms, a and b are each independently an integer of 1 or greater, c is an integer of 0 or greater, and a+b+c is an integer of 4 or greater.
[0061]
[0062] (In formula (2), R 4are each independently a monovalent hydrocarbon group having 1 to 12 carbon atoms, Y is a group having an alkoxysilyl group or an aliphatic unsaturated group having 1 to 4 carbon atoms, and d is an integer of 2 to 500, preferably an integer of 4 to 400, more preferably an integer of 10 to 200, and particularly preferably an integer of 10 to 60.) In addition to the compound represented by formula (1) above, examples of the alkoxysilyl group-containing compound (c) include compounds represented by formula (3) below.
[0063] R 21 e R 22 f Si(OR 23 ) 4-(e+f) (3) (In formula (3), R 21 are independently alkyl groups having 6 to 15 carbon atoms, and R 22 are independently unsubstituted or substituted monovalent hydrocarbon groups having 1 to 12 carbon atoms (excluding alkyl groups having 6 to 12 carbon atoms), and R 23 are independently an alkyl group having 1 to 6 carbon atoms, e is an integer of 0 to 3, preferably 1, f is an integer of 0 to 2, and e+f is an integer of 1 to 3. 21 Examples of R include a hexyl group, an octyl group, a nonyl group, a decyl group, a dodecyl group, and a tetradecyl group. 21 It is preferable that the alkyl group has 6 to 15 carbon atoms, since the alkoxysilyl group-containing compound becomes liquid at room temperature and is easy to handle.
[0064] R 22Examples of the alkyl groups include alkyl groups such as methyl, ethyl, propyl, isopropyl, butyl, isobutyl, and tert-butyl; cycloalkyl groups such as cyclopentyl, cyclohexyl, and cyclobutyl; aliphatic unsaturated groups such as vinyl and allyl; aryl groups such as phenyl, tolyl, xylyl, and naphthyl; aralkyl groups such as benzyl, 2-phenylethyl, 2-methyl-2-phenylethyl, and phenylpropyl; and groups in which some or all of the hydrogen atoms of these hydrocarbon groups have been replaced with halogen atoms such as chlorine, fluorine, and bromine. Examples of such groups include halogenated hydrocarbon groups such as chloromethyl, trifluoropropyl, 3,3,3-trifluoropropyl, 2-(nonafluorobutyl)ethyl, 2-(heptadecafluorooctyl)ethyl, chlorophenyl, bromophenyl, dibromophenyl, tetrachlorophenyl, fluorophenyl, and difluorophenyl groups, and cyanoalkyl groups such as α-cyanoethyl, β-cyanopropyl, and γ-cyanopropyl groups, with methyl and ethyl groups being preferred.
[0065] R 23 Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, a butyl group, a pentyl group, and a hexyl group, and preferably a methyl group or an ethyl group.
[0066] In the formula (3), examples of the compound in which e is 1 include C6H 13 Si(OCH3)3, C 10 H 21 Si(OCH3)3, C 12 H 25 Si(OCH3)3, C 12 H 25 Si(OC2H5)3,C 10 H 21 Si(CH3)(OCH3)2,C 10 H 21 Si(C6H5)(OCH3)2,C 10 H 21 Si(CH3)(OC2H5)2,C 10 H 21 Si(CH=CH2)(OCH3)2,C 10 H 21Examples include Si(CH2CH2CF3)(OCH3)2.
[0067] Examples of the alkoxysilyl group-containing compound (c) include the compounds represented by the above formula (1) and the compounds represented by the above formula (3), as well as dimethylpolysiloxanes in which one molecular chain terminal is blocked with an alkoxysilyl group, as represented by the following formula (4):
[0068]
[0069] (In formula (4), R 31 is —O— or —CH2CH2—. 32 are independently unsubstituted or substituted monovalent hydrocarbon groups, and specifically, R 22 Among these, alkyl groups and aryl groups are preferred, and methyl groups and phenyl groups are more preferred. 33 are independently an alkyl group having 1 to 6 carbon atoms, preferably a methyl group, an ethyl group, a propyl group, a butyl group, or a hexyl group. g is an integer of 5 to 100, preferably an integer of 5 to 70, and particularly preferably an integer of 10 to 50, and p is an integer of 1 to 3, preferably 2 or 3.) The alkoxysilyl group-containing compound (c) also includes compounds in which one or more methyl groups in the formula (4) are substituted with monovalent hydrocarbon groups other than methyl groups.
[0070] Examples of the substituent include groups having 1 to 10 carbon atoms, and specific examples thereof include alkyl groups such as an ethyl group, a propyl group, a butyl group, a hexyl group, and an octyl group; cycloalkyl groups such as a cyclopentyl group and a cyclohexyl group; aryl groups such as a phenyl group and a tolyl group; aralkyl groups such as a 2-phenylethyl group and a 2-methyl-2-phenylethyl group; and halogenated hydrocarbon groups such as a 3,3,3-trifluoropropyl group, a 2-(nonafluorobutyl)ethyl group, a 2-(heptadecafluorooctyl)ethyl group, and a p-chlorophenyl group.
[0071] The alkoxysilyl group-containing compound (c) may be used alone, or may be used in a mixture with the alkenyl group-containing polyorganosiloxane (a) and the hydrosilyl group-containing polyorganosiloxane (b). When the resin composition is used in a mixture with the alkenyl group-containing polyorganosiloxane (a) and the hydrosilyl group-containing polyorganosiloxane (b), the amount of the alkoxysilyl group-containing compound (c) is preferably 5 to 50 parts by mass, more preferably 10 to 40 parts by mass, relative to 100 parts by mass of the total amount of the alkenyl group-containing polyorganosiloxane (a) and the hydrosilyl group-containing polyorganosiloxane (b).
[0072] Catalyst: The catalyst for crosslinking the polyorganosiloxane (a) having alkenyl groups and the polyorganosiloxane (b) having hydrosilyl groups by hydrosilylation reaction can be, for example, any known platinum-based catalyst. Examples of the platinum-based catalyst include platinum black, platinic chloride, chloroplatinic acid, reaction products of chloroplatinic acid and monohydric alcohols, complexes of chloroplatinic acid with olefins or vinylsiloxanes, and platinum bisacetoacetate. One or more of the catalysts can be used.
[0073] The amount of the catalyst used in terms of platinum element may be the amount necessary for crosslinking, and may be appropriately adjusted according to the desired curing rate, etc., but is usually the total amount of the polyorganosiloxanes (a) and (b). It is preferably 0.1 to 1000 mass ppm.
[0074] [Aluminum nitride-based thermally conductive filler] The aluminum nitride-based thermally conductive filler contained in the resin composition of the present invention is not particularly limited as long as the effects of the present invention are not impaired. Specifically, it is preferred that, in a volumetric particle size distribution measured by a laser diffraction scattering method, the proportion of particles having a particle diameter of 100 μm or less among all particles is 90% or more, that in the volumetric particle size distribution, the proportion of particles having a particle diameter of 5 μm or more and 100 μm or less among all particles is 40 to 90%, and that the proportion of particles having a particle diameter of 0.05 μm or more and less than 5 μm among all particles is 5 to 60%, and that in a scanning electron microscope image taken at a magnification of 500x, 50% or more of the particles in the particle diameter range of 5 μm or more and 50 μm or less are polyhedral particles having at least two flat surfaces. That is, the aluminum nitride-based thermally conductive filler contained in the resin composition of the present invention preferably comprises particles (Pf) containing 90% or more of particles (Pf1) having a particle diameter in the range of 100 μm or less, with the amount of all particles being 100%, when the volume-based particle size distribution is measured by a laser diffraction scattering method, the particles (Pf) contain 40 to 90% of particles (Pf1A) having a particle diameter of 5 μm or more and 100 μm or less, and 5 to 60% of particles (Pf1B) having a particle diameter of 0.05 μm or more and less than 5 μm, and also contain particles (Pf1A-1) having a particle diameter of 5 μm or more and 50 μm or less, and in a scanning electron microscope image taken at a magnification of 500 times, the particles (Pf1A-1) preferably contain 50% or more of polyhedral particles having at least two flat surfaces. By using such a thermally conductive filler, it is possible to easily prepare a resin composition having the thermal conductivity of 6.0 W / m·K or more, the discharge rate of 10 g / min or more, and the thickness of the resin composition of 100 μm or less.
[0075] The aluminum nitride-based thermally conductive filler of the present invention is one in which the proportion of aluminum nitride in the total amount of the thermally conductive filler is 40% by volume or more. That is, the aluminum nitride-based thermally conductive filler of the present invention contains 40% by volume or more of aluminum nitride. Aluminum nitride has high thermal conductivity, making it easy to obtain a resin composition with high thermal conductivity. The proportion of aluminum nitride in the total amount of the thermally conductive filler is preferably 50% by volume or more, more preferably 60% by volume or more. The thermally conductive filler may consist solely of aluminum nitride, or, as described below, may further contain, in addition to aluminum nitride, a filler other than aluminum nitride (e.g., aluminum oxide, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, diamond, etc.). In a preferred and exemplary embodiment of the present invention, the thermally conductive filler contains aluminum nitride and aluminum oxide.
[0076] In the thermally conductive filler, in the volume-based particle size distribution measured by a laser diffraction scattering method, the proportion of particles having a particle diameter of 100 μm or less (i.e., the "particles (Pf1)") among all particles is 90% or more, so that the proportion of fillers having a particle diameter of more than 100 μm contained in the resin composition can be reduced. If a resin composition contains a large amount of large fillers, the fillers will become an obstacle when thinning the resin composition, making it difficult to efficiently thin the resin composition, and in some cases, thinning the resin composition itself may be impossible. The proportion of particles having a particle diameter of 100 μm or less (i.e., the "particles (Pf1)") in the thermally conductive filler is preferably 97% or more, and most preferably 100%.
[0077] In the volume-based particle size distribution of the thermally conductive filler, the proportion of particles having a particle diameter of 5 μm or more and less than 100 μm (i.e., the "particles (Pf1A)") among all particles is 40 to 90%, and the proportion of particles having a particle diameter of 0.05 μm or more and less than 5 μm (i.e., the "particles (Pf1B)") among all particles is 5 to 60%. By including particles of different particle diameters, a structure close to a close-packed structure is easily obtained when the filler is efficiently filled into the resin, and high thermal conductivity and high dischargeability are easily obtained. In the volume-based particle size distribution, the proportion of particles having a particle diameter of 5 μm or more and less than 100 μm (i.e., the "particles (Pf1A)") among all particles is more preferably 45 to 80%, and even more preferably 47 to 70%. In the volume-based particle size distribution, the proportion of particles having a particle diameter of 0.05 μm or more and less than 5 μm (i.e., the “particles (Pf1B)”) in the total particles is more preferably 20 to 55%, and even more preferably 30 to 53%.
[0078] The volumetric particle size distribution measured by the laser diffraction scattering method in the present invention is obtained by dispersing a thermally conductive filler in a solution in which a 5% aqueous solution of sodium pyrophosphate has been added to 90 ml of water, dispersing the resulting dispersion using a homogenizer, and measuring the volumetric particle size distribution using a laser diffraction particle size analyzer (for example, the "MICROTRAC-MT3300EXII" manufactured by Microtrac-Bell Co., Ltd.) When a mixture of multiple fillers is used as the thermally conductive filler, the particle size distribution of each filler may be measured, and then the volumetric particle size distribution may be calculated by combining the fillers.
[0079] In the thermally conductive filler, in a scanning electron microscope image taken at 500x magnification, 50% or more of the particles having a particle size of 5 μm or more and 50 μm or less (i.e., the "particles (Pf1A-1)") are polyhedral particles having at least two flat surfaces. This allows high thermal conductivity to be achieved even if large particles having a particle size of more than 100 μm are not used or if the amount of such particles is extremely small. The reason for this is unclear, but the inventors speculate as follows. In other words, if large particles having a particle size of more than 100 μm are not used or if the amount of such particles is extremely small in order to enable thinning, it would be difficult to achieve both high thermal conductivity and high dischargeability by using fillers of different particle sizes to improve filling. However, by having such polyhedral particles having two flat surfaces, the contact area between particles is increased, making it easier to form heat conduction paths, thereby improving thermal conductivity. In addition, other particles roll on the smooth, flat surfaces of the polyhedral particles, which reduces flow resistance overall, improving fluidity and resulting in high dischargeability.
[0080] The proportion of polyhedral particles (Pf1A-1mp) having a particle size of 5 μm or more and 50 μm or less in the thermally conductive filler is the proportion of the total area of polyhedral particles (Pf1A-1mp) having a particle size in the range of 5 to 50 μm relative to the total area of all particles having a particle size in the range of 5 to 50 μm, as identified in the scanning electron microscope image (i.e., the total area of all the "particles (Pf1A-1)").
[0081] Here, particles having a particle diameter in the range of 5 to 50 μm as identified in a scanning electron microscope image refer to primary particles having a major axis in the range of 5 to 50 μm in an image of the thermally conductive filler of the present invention observed with a scanning electron microscope.
[0082] FIG. 1 shows a scanning electron microscope image taken at 500x magnification of polyhedral particles in the particle diameter range of 5 to 50 μm in one embodiment of the thermally conductive filler of the present invention.
[0083] Polyhedral particle 11 has a polyhedral shape with a plurality of flat surfaces a arranged randomly, and is an aluminum nitride particle having at least two flat surfaces a. Polyhedral particle 12 is also an aluminum nitride particle having at least two flat surfaces a. In Figure 1, there are a plurality of polyhedral particles other than polyhedral particle 11 and polyhedral particle 12.
[0084] In a scanning electron microscope image taken at a magnification of 500x, the proportion of polyhedral particles having at least two flat surfaces among particles having a particle diameter of 5 μm or more and 50 μm or less is preferably 55% or more, more preferably 60% or more, even more preferably 65% or more, still more preferably 70% or more, and particularly preferably 80% or more.
[0085] In the aluminum nitride-based thermally conductive filler, it is preferable that the oxygen content of particles having a particle size in the range of 5 to 50 μm (i.e., the "particles (Pf1A-1)") is 0.5 mass% or less. In aluminum nitride powder, the lower the oxygen content, the higher the thermal conductivity tends to be. As described above, in the present invention, the inclusion of polyhedral particles having a particle size of 5 to 50 μm is one of the reasons why high thermal conductivity can be imparted to the resin composition, and therefore, reducing the oxygen content of particles falling within this range (i.e., reducing the oxygen content of polyhedral particles) is effective for increasing the thermal conductivity of the resin composition.
[0086] The oxygen content of particles having a particle size in the range of 5 to 50 μm (i.e., the “particles (Pf1A-1)”) can be determined by separating particles in the range by sieving and measuring the total oxygen content thereof by a high-temperature pyrolysis method.
[0087] The aluminum nitride-based thermally conductive filler may contain particles other than aluminum nitride particles. Examples of such particles include particles with high thermal conductivity, such as aluminum oxide, boron nitride, magnesium oxide, zinc oxide, silicon carbide, silicon nitride, and diamond. In particular, aluminum nitride is easily oxidized, making it difficult to manufacture when its particle size is small. Therefore, it is preferable to blend other particles as part or all of the particles having a particle size of 0.05 μm or more and less than 5 μm. In particular, from the viewpoint of thermal conductivity and handleability, it is preferable to use aluminum oxide as part or all of the particles having a particle size of 0.05 μm or more and less than 5 μm (i.e., the "particles (Pf1B)").
[0088] When the aluminum nitride-based thermally conductive filler of the present invention contains aluminum nitride particles and aluminum oxide particles, the proportion of aluminum oxide particles in the entire thermally conductive filler is preferably 1 to 30% by volume, and more preferably 5 to 20% by volume. Furthermore, the proportion of aluminum oxide particles in particles having a particle diameter of 0.05 μm or more and less than 5 μm (i.e., the "particles (Pf1B)") is preferably 10 to 60% by volume, and more preferably 20 to 50% by volume. Here, in the case of a thermally conductive filler consisting of aluminum nitride particles and aluminum oxide particles, the densities of aluminum nitride and aluminum oxide are each 3.26 g / cm. 3 and 4.0 g / cm 3 In this case, the proportion of aluminum oxide particles in the entire thermally conductive filler is preferably equivalent to 1.2 to 34% by mass, and more preferably equivalent to 6.1 to 23% by mass. Furthermore, the proportion of aluminum oxide particles in particles having a particle diameter of 0.05 μm or more and less than 5 μm (i.e., the "particles (Pf1B)") is preferably equivalent to 12 to 65% by mass, and more preferably equivalent to 23 to 55% by mass.
[0089] [Method for producing thermally conductive filler] As described above in the section "Aluminum nitride-based thermally conductive filler", the aluminum nitride-based thermally conductive filler contained in the resin composition of the present invention has the following characteristics: in a volume-based particle size distribution measured by a laser diffraction scattering method, the proportion of particles having a particle size in the range of 100 μm or less (i.e., the "particles (Pf1)") among all particles is 90% or more; in the volume-based particle size distribution, the proportion of particles having a particle size of 5 μm or more and 100 μm or less (i.e., the "particles (Pf1A)") among all particles is 40 to 90%; and the proportion of particles having a particle size of 0.05 μm or more and less than 5 μm (i.e., the "particles (Pf1B)") among all particles is 5 to 60%; and in a scanning electron microscope image taken at a magnification of 500 times, 50% or more of the particles having a particle size in the range of 5 μm or more and 50 μm or less (i.e., the "particles (Pf1A-1)") are polyhedral particles having at least two flat surfaces; i.e., It is preferable that, when a volume-based particle size distribution is measured by a laser diffraction scattering method, the particles (Pf) contain 90% or more particles (Pf1) having a particle diameter in the range of 100 μm or less, with the amount of all particles being 100%, the particles (Pf) contain 40 to 90% particles (Pf1A) having a particle diameter of 5 μm or more and 100 μm or less, and 5 to 60% particles (Pf1B) having a particle diameter of 0.05 μm or more and less than 5 μm, and also contain particles (Pf1A-1) having a particle diameter of 5 μm or more and 50 μm or less, and that, in a scanning electron microscope image taken at a magnification of 500 times, the particles (Pf1A-1) contain 50% or more polyhedral particles having at least two flat surfaces.
[0090] Such a thermally conductive filler can be easily obtained by mixing a known powder having a desired particle size with a powder containing polyhedral particles of the desired particle size. For example, it can be produced by mixing, in a predetermined ratio, aluminum nitride powder containing polyhedral particles and having an average particle size of 5 μm to 100 μm, aluminum oxide powder having an average particle size of 0.05 μm to less than 5 μm, and other powders as needed.
[0091] The mixing may be carried out before compounding with the resin, or may be carried out simultaneously with compounding with the resin. Alternatively, a portion of the powder may be compounded with the resin in advance to obtain a resin composite, and then the remaining powder may be compounded with the resin composite to obtain the resin composition of the present invention. The particle size distribution of the thermally conductive filler may be measured before mixing with the resin. When a thermally conductive filler is obtained by mixing multiple powders, the particle size distribution of each powder may be measured separately, and the particle size distribution results obtained may be combined to obtain the particle size distribution of the thermally conductive filler.
[0092] The thermally conductive filler may be surface-treated as needed to improve compatibility with resins, water resistance, etc. Known methods can be used for the surface treatment. For example, surface treatment can be performed using organosilicon compounds such as silicone oil, silylating agents, and silane coupling agents; acids such as phosphoric acid, phosphates, and fatty acids; polymeric compounds such as polyamide resins; and inorganic substances such as alumina and silica. When preparing a thermally conductive filler by mixing multiple powders, the surface treatment can be performed after mixing, or the powders can be mixed after surface treatment. When mixing after surface treatment, powders with different surface treatments can be mixed, or a surface-treated powder can be mixed with a surface-treated powder.
[0093] When the polyhedral particles are aluminum nitride particles, an example of a method for producing a powder containing the polyhedral particles includes a production method including the following steps 1 and 2.
[0094] Process 1: 0.5-5μm, specific surface area 1.2-16.0m 2 100 parts by mass of a first aluminum nitride powder raw material having an average particle diameter of 3 to 40 μm and a specific surface area of 0.05 to 1.8 m 2 / g, and the ratio (SA2 / SA1) of the specific surface area (SA2) of the first aluminum nitride powder raw material to the specific surface area (SA1) of the second aluminum nitride powder raw material is 0.8 or less, to prepare a raw material mixture. Step 1: A step of heating the raw material mixture to 1750 to 2100°C under the supply of an inert gas.
[0095] <Step 1> Step 1 is a process for obtaining a powder of 0.5 to 5 μm and a specific surface area of 1.2 to 16.0 m 2 100 parts by mass of a first aluminum nitride powder raw material having an average particle diameter of 3 to 40 μm and a specific surface area of 0.05 to 1.8 m 2 / g, and the ratio (SA2 / SA1) of the specific surface area (SA2) of the first aluminum nitride powder raw material to the specific surface area (SA1) of the first aluminum nitride powder raw material is 0.8 or less, to prepare a raw material mixture.
[0096] The raw material mixture contains aluminum nitride particles of different average particle sizes in predetermined blending amounts, and by undergoing the heating step (step 2) described below, aluminum nitride powder containing polyhedral particles with at least two flat surfaces can be obtained.
[0097] The specific surface area of each of the raw material powders can be determined by the BET method using N2 adsorption, for example, with a flow-type automatic surface area measuring device, Flowsorb 2300, manufactured by Shimadzu Corporation.
[0098] It is believed that the presence of an appropriate amount of the second aluminum nitride powder raw material, which has a relatively large average particle size, causes the first aluminum nitride powder raw material, which has a small average particle size, to be incorporated into the second aluminum nitride powder raw material by a sublimation reaction during the heating step, resulting in crystal growth of the second aluminum nitride powder raw material, increasing its particle size. It is believed that this crystal growth results in the formation of the predetermined polyhedral particles. Furthermore, it is believed that the oxygen present in the first aluminum nitride powder is effectively removed by the sublimation reaction, resulting in the polyhedral aluminum nitride particles produced through the heating step having a low oxygen content.
[0099] As described above, by using the first and second aluminum nitride powder raw materials in combination in a predetermined blending amount, the crystal growth proceeds sufficiently and aggregation of particles can also be suppressed.
[0100] The first aluminum nitride powder raw material has an average particle size of 0.5 to 5 μm and a specific surface area of 1.2 to 16.0 m 2 / g, and preferably has an average particle size of 0.7 to 5 μm and a specific surface area of 1.2 to 12.0 m 2 / g.
[0101] The second aluminum nitride powder raw material has an average particle size of 3 to 40 μm and a specific surface area of 0.05 to 1.8 m 2 The average particle size of the second aluminum nitride powder raw material can be appropriately selected depending on the desired average particle size, and is preferably 3 to 20 μm, more preferably 5 to 15 μm.
[0102] The amount of the second aluminum nitride powder raw material blended in the raw material mixture relative to 100 parts by mass of the first aluminum nitride powder raw material is preferably 1 to 20 parts by mass, more preferably 2 to 15 parts by mass, and even more preferably 3 to 10 parts by mass. As described above, by appropriately adjusting the blending amounts of the first and second aluminum powder raw materials, it becomes easier to obtain aluminum nitride powder containing polyhedral particles.
[0103] The raw material mixture may contain an additive for forming a liquid phase or an additive for promoting grain growth during firing. Commonly known additives include oxides of alkali metals, alkaline earth metals, or rare earth elements, with yttrium oxide being a typical example. The content of the additive in the raw material mixture is preferably about 1 to 10 mass %.
[0104] The first and second aluminum nitride powder raw materials can be any commonly used material without any particular restrictions, as long as they have a predetermined average particle size. For example, they may be produced by a reduction nitridation method, or may be produced by a direct nitriding method such as combustion synthesis and then adjusted to a predetermined average particle size through pulverization and classification processes, or may be produced by any other manufacturing method. Among these, the first and second aluminum nitride powder raw materials are preferably produced by a reduction nitridation method, since pulverization and classification processes are not required.
[0105] It is also preferable to use the aluminum nitride powder produced by steps 1 and 2 as a second aluminum nitride powder raw material and perform steps 1 and 2 again to obtain aluminum nitride powder having a larger average particle size.
[0106] <Step 2> Step 2 is a step of heating the raw material mixture prepared in step 1 to 1750 to 2100° C. under the supply of an inert gas.
[0107] By setting the heating temperature to 1750°C or higher, crystal growth of the aluminum nitride particles is promoted, making it easier to obtain aluminum nitride powder containing aluminum nitride particles with flat surfaces. On the other hand, by setting the heating temperature to 2100°C or lower, aggregation due to fusion between particles can be suppressed. From this perspective, the heating temperature is preferably 1750 to 2100°C, more preferably 1800 to 2050°C, and even more preferably 1800 to 2000°C.
[0108] The heating time is not particularly limited, but is preferably 1 to 20 hours, and more preferably 2 to 15 hours. If the heating time is 1 hour or longer, the crystal growth of the aluminum nitride particles proceeds sufficiently, and a smooth, flat surface is likely to be formed. On the other hand, if the heating time exceeds 20 hours, the grain growth does not proceed easily, and there is no advantage in industrial implementation.
[0109] Heating is carried out under an inert gas supply. That is, it is most preferable to heat the raw material mixture by supplying the inert gas into a heating device for containing and heating it, but heating can also be carried out while continuously supplying the inert gas. The raw material mixture is filled into a heating container (hereinafter also referred to as a "setter") and contained in the heating device, and it is preferable to use a carbon setter as the setter. As the inert gas, argon gas or nitrogen gas can be used, with nitrogen gas being preferred. The pressure when heating under the inert gas supply is not particularly limited as long as aluminum nitride powder containing polyhedral particles can be obtained in a manner that fully achieves the effects of the present invention. In a typical and exemplary embodiment of the present invention, the heating is carried out under normal pressure.
[0110] <Other Steps> After step 2, a crushing step may be carried out as needed. Crushing is carried out to loosen the bonds between loosely bonded aluminum nitride particles, and is different from pulverization, in which the aluminum nitride particles are partially crushed. Therefore, even if the crushing step is carried out, the shape of the polyhedral particles is maintained. Crushing may be carried out by a known method, such as a roll crusher mill, a jet mill, a ball mill, a mass colloider, or a jaw crusher.
[0111] An oxidation step may be carried out after step 2, and is preferably carried out after the above-mentioned crushing step. By carrying out the oxidation step, decomposition due to contact with water or the like can be prevented. The oxidation step can be carried out by heating in an air atmosphere. The heating temperature in the oxidation step is not particularly limited, but is preferably 500 to 900°C, more preferably 600 to 800°C. The heating time is not particularly limited, but is preferably 1 to 20 hours, more preferably 5 to 15 hours. The oxygen content of the oxide film formed in the oxidation step is included in the oxygen content of the aluminum nitride-based thermally conductive filler. By carrying out the oxidation step so that the oxygen content is within the range of the oxygen content of the aluminum nitride powder described above, it becomes possible to impart excellent thermal conductivity to the resulting resin composition when filled into a resin.
[0112] [Composition of Resin Composition] The content of the thermally conductive filler contained in the resin composition of the present invention is not particularly limited, but the lower limit value is preferably 300 parts by mass or more, more preferably 500 parts by mass or more, and even more preferably 900 parts by mass or more, relative to 100 parts by mass of the resin, and the upper limit value is preferably 5000 parts by mass or less, more preferably 3500 parts by mass or less, and even more preferably 2000 parts by mass or less. When the content of the thermally conductive filler is equal to or greater than these lower limits, it becomes easy to improve the thermal conductivity of the resin composition, and when the content of the aluminum nitride powder is equal to or less than these upper limits, it becomes easy to improve the syringe dischargeability.
[0113] Furthermore, the resin composition of the present invention may contain additives such as a plasticizer, a vulcanizing agent, a curing catalyst, a curing accelerator, a reaction inhibitor, and a mold release agent, as needed.
[0114] [Method for Producing Resin Composition] The method for producing the resin composition of the present invention is not particularly limited, and the resin composition can be produced by mixing the resin, filler, and other components as needed using a known method using a blender, mixer, or the like. During the mixing, the components may be added simultaneously to a mixer or the like and mixed, or the components may be added sequentially to a mixer or the like and mixed. The order of addition is not particularly limited. Furthermore, the mixing may be performed under heating, or in a controlled atmosphere such as an inert gas atmosphere, as needed.
[0115] [Uses of Resin Composition] The resin composition can be used as a heat dissipation member (heat dissipation material) for efficiently dissipating heat generated by electronic components mounted in home appliances, automobiles, (notebook) personal computers, etc. Specific examples thereof include heat dissipation sheets, heat dissipation greases, heat dissipation gels, adhesives, semiconductor encapsulants, and underfills. In other words, the present invention can also be said to provide a heat dissipation member containing the resin composition.
[0116] When the resin composition of the present invention is used as a heat dissipation member, by using the resin composition of the present invention between a substrate having a heat-generating portion such as a semiconductor element and a substrate having a cooling portion such as a heat sink or a housing, the heat generated by the electronic component can be efficiently dissipated. The electronic component of the present invention is an electronic component having the resin composition of the present invention as a heat dissipation member, specifically, an electronic component comprising a heat dissipation member containing the resin composition of the present invention and a substrate having a heat-generating portion, the heat dissipation member being arranged so as to contact the heat-generating portion. In one preferred exemplary aspect of the present invention, the electronic component is an electronic component comprising a heat dissipation member containing the resin composition of the present invention, a substrate having a heat-generating portion, and a substrate having a cooling portion, the heat dissipation member being arranged so as to contact the heat-generating portion, and it is preferable that the heat dissipation member be arranged so as to contact both the heat-generating portion and the cooling portion. In another preferred exemplary embodiment similar to the above embodiment, the electronic component of the present invention comprises a heat dissipation member containing the resin composition of the present invention, a substrate having a heat-generating portion, and a substrate having a cooling portion, the heat dissipation member being arranged so as to contact the substrate having the heat-generating portion, particularly the electronic component being arranged so as to contact both the substrate having the heat-generating portion and the substrate having the cooling portion. As described above, the resin composition of the present invention has a high thermal conductivity (TC), and it is easy to reduce the layer thickness (L) of the resin composition between substrates such as semiconductor elements, heat sinks, and housings, thereby easily reducing the thermal resistance (R). Furthermore, due to its high syringe ejection properties, it is easy to reduce the contact thermal resistance (Rc) at the interface between the resin composition and substrates such as semiconductor elements, heat sinks, and housings, thereby easily achieving an extremely low thermal resistance (R).
[0117] The method for producing electronic components using the resin composition of the present invention is not particularly limited, but examples include applying the resin composition of the present invention filled in a syringe onto one substrate, then placing the other substrate on top and pressing with a force of 0.05 to 0.5 MPa. The resin composition of the present invention has a BLT of 100 μm or less when sandwiched between two 10 mm x 10 mm silicon chips and subjected to a force of 50 N (i.e., 0.5 MPa) for 60 seconds, and therefore does not require high-pressure pressing to thin the resin composition. Therefore, the thickness of the resin composition layer can be easily reduced without using special equipment and without adversely affecting the substrate, thereby enabling the production of electronic components with high production efficiency.
[0118] EXAMPLES The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0119] [Measurement Methods] Various physical properties in the examples and comparative examples were measured by the following methods.
[0120] (1) Particle size distribution measurement For each of AL1 to AL7 and AO1 described below, powder was dispersed in a solution of 5% aqueous sodium pyrophosphate solution added to 90 ml of water, and this was dispersed using a homogenizer. The particle size distribution on a volume basis was measured using a laser diffraction particle size distribution analyzer (MICROTRAC MT3300EXII manufactured by Microtrac-Bell Co., Ltd.). The volume-based particle size distribution of the thermally conductive filler was obtained by calculation based on the above results in accordance with the filler composition to be blended in each resin composition.
[0121] (2) Proportion of Polyhedral Particles SEM photographs (accelerating voltage 15 kV, secondary electron detection) were taken of the aluminum nitride powder at a magnification of 500x using a scanning electron microscope ("TM3030" manufactured by Hitachi High-Technologies Corporation). The SEM photographs were used to confirm the presence or absence of particles having two or more flat surfaces among the aluminum nitride primary particles having a particle diameter (major axis) of 5 μm or more and 50 μm or less. The proportion of polyhedral particles was determined by calculating the proportion of the total area of polyhedral particles to the total area of all aluminum nitride primary particles having a particle diameter of 5 μm or more and 50 μm or less from image analysis of the SEM photographs, and this was taken as the proportion of polyhedral particles. Specifically, this was calculated using the following formula: Proportion of polyhedral particles (%) = [(total area of polyhedral particles) / (total area of all aluminum nitride primary particles having a particle diameter of 5 μm or more and 50 μm or less)] × 100
[0122] (3) Thermal Conductivity of Resin Composition The resin composition was hot-pressed at 100° C. to obtain a sheet having a thickness of 7 mm. The thermal conductivity of the obtained sheet was measured using a hot disc method thermophysical property measuring device (TPS500, manufactured by Kyoto Electronics Manufacturing Co., Ltd.).
[0123] (4) Amount of resin composition discharged from syringe The resin composition was filled into a syringe "PSY-30F" manufactured by Musashi Engineering Co., Ltd. (the inner diameter of the syringe body for storing the sample was 22 mm, and the inner diameter of the tip (tip discharge part) from which the sample was discharged was 2 mm), and then the syringe was left to stand for 6 hours in a thermostatic chamber at 25°C. Thereafter, while the syringe was kept in a thermostatic chamber at 25°C, the resin composition was discharged from the syringe for 1 minute at a discharge pressure of 0.62 Pa, and the amount of resin composition discharged per minute was measured from the amount of resin composition discharged.
[0124] (5) Measurement of BLT: 0.02 ml of the resin composition was sandwiched between two 10 mm x 10 mm silicon chips and a force of 50 N was applied for 60 seconds. Specifically, the resin composition was measured onto a silicon chip, and another silicon chip was placed on top of it, sandwiching the resin composition between the two silicon chips. A sample was obtained by crushing with a force of 50 N for 60 seconds using a push-pull gauge (manufactured by Imada Co., Ltd., SVH-1000N). The thickness of the sample was then measured using a micrometer (manufactured by Mitutoyo Corporation, high-precision digimatic micrometer MDH-25MB). The thickness of the resin composition alone was calculated by subtracting the thickness of the silicon chip, which had been measured previously, from the thickness of the obtained sample, and this was designated as the BLT.
[0125] (6) Evaluation of thermal resistance (BLT) Using the sample for the BLT measurement described above, the thermal resistance value at 25°C was measured by a laser flash method (NETZSCH, LFA467 HyperFlash). The value obtained by subtracting the thermal resistance value of the silicon chip measured in advance was used as the thermal resistance value. 2 ・Less than K / W is marked as "〇", 10mm 2 ・K / W or more was evaluated as "X".
[0126] (7) Evaluation of thermal resistance (100 μm) The resin composition was sandwiched between two silicon chips, and a force of 50 N or less was applied for 60 seconds so that the thickness of the resin composition became 100 μm. Specifically, 0.02 ml of the resin composition was measured on a 10 mm × 10 mm silicon chip, and another 10 mm × 10 mm silicon chip was placed on top of it, and the resin composition was sandwiched between the two silicon chips, and crushed using a push-pull gauge (manufactured by Imada Co., Ltd., SVH-1000N) to obtain a sample. Using this sample, the thermal resistance value was measured by the laser flash method in the same manner as above, and the 20 mm 2 ・Less than K / W is marked as "〇", 25mm 2 ・K / W or more and 20mm 2 ・Less than K / W is "△", 25mm 2 ・K / W or more was evaluated as "X".
[0127] [Raw materials used] The following raw materials were used. AL1: Aluminum nitride powder containing polyhedral particles with a particle diameter of 5 μm to 50 μm, produced by the method of Synthesis Example 1 below. AL2: Aluminum nitride powder containing polyhedral particles with a particle diameter of 5 μm to 50 μm, produced by the method of Synthesis Example 2 below. AL3: Aluminum nitride powder containing polyhedral particles with a particle diameter of 5 μm to 50 μm, produced by the method of Synthesis Example 3 below. AL4: Commercially available aluminum nitride powder (average particle diameter 1 μm). AL5: Commercially available aluminum nitride powder (average particle diameter 30 μm). AL6: Commercially available aluminum nitride powder (average particle diameter 50 μm). AL7: Commercially available aluminum nitride powder (average particle diameter 120 μm). AL8: Commercially available aluminum nitride powder (average particle diameter 20 μm). AO1: Commercially available aluminum oxide powder (average particle diameter 0.3 μm).
[0128] (Synthesis example 1) Average particle diameter 1.0 μm, specific surface area 2.81 m 2 100 parts by mass of aluminum nitride powder raw material having an average particle diameter of 5.0 μm and a specific surface area of 1.02 m 2 1 / g of aluminum nitride powder raw material was mixed with 5 parts by mass of aluminum nitride powder raw material to prepare a raw material mixture. The raw material mixture was placed in a heating device, nitrogen gas was supplied into the device to create a nitrogen atmosphere, and the mixture was heated at 1950°C for 3 hours. Heating was carried out under normal pressure, and crushing and oxidation treatment were carried out to obtain a powder with an average particle size of 8.0 μm and a specific surface area of 0.60 m. 2 / g of aluminum nitride powder (AL1) was obtained.
[0129] (Synthesis Example 2) Average particle diameter 0.5 μm, specific surface area 15.70 m 2 100 parts by mass of aluminum nitride powder raw material having a particle size of 7.8 μm and a specific surface area of 0.62 m 2 10 parts by mass of aluminum nitride powder raw material with a sintered body of 1000 μm / g was mixed to prepare a raw material mixture. The raw material mixture was placed in a heating device, nitrogen gas was supplied into the device to create a nitrogen atmosphere, and the mixture was heated at 2000°C for 5 hours. Heating was carried out under normal pressure, and crushing and oxidation treatment were carried out to obtain a powder with an average particle size of 18.7 μm and a specific surface area of 0.20 m. 2 / g of aluminum nitride powder (AL2) was obtained.
[0130] (Synthesis Example 3) Average particle diameter 1.0 μm, specific surface area 2.81 m2 100 parts by mass of aluminum nitride powder raw material having a particle size of 17.8 μm and a specific surface area of 0.21 m 2 20 parts by mass of aluminum nitride powder raw material with a sintered body of 10 ... 2 / g of aluminum nitride powder (AL3) was obtained.
[0131] Example 1 A resin, 1,426 parts by mass of a thermally conductive filler relative to 100 parts by mass of the resin, a platinum catalyst (1,2-divinyltetramethyldisiloxane complex of platinum) as a catalyst in an amount of 20 ppm by mass, calculated as platinum element, relative to the resin, and 3,000 ppm by mass of 1-ethynyl-1-cyclohexanol as a reaction inhibitor, relative to the resin, were mixed in a blade-type agitator to prepare a resin composition, and the thermal conductivity, syringe discharge rate, BLT, and thermal resistance of the obtained resin composition were evaluated. The resin is a mixture of polyorganosiloxane (a) having an average of two or more alkenyl groups bonded to silicon atoms per molecule and polyorganosiloxane (b) having an average of two or more hydrosilyl groups per molecule in a mass ratio of 97:3 (for one alkenyl group bonded to a silicon atom in polyorganosiloxane (a) having an alkenyl group, 0.7 hydrosilyl groups in polyorganosiloxane (b) having a hydrosilyl group). To 100 parts by mass of the resulting mixture, 20 parts by mass of decyltrimethoxysilane was added as an alkoxysilyl group-containing compound (c). The thermally conductive filler is a mixture of 44% by mass of AL1, 33% by mass of AL4, and 23% by mass of AO1. The compositions of the thermally conductive filler and resin composition, and the evaluation results of the resulting resin composition are shown in Tables 1 and 2-1.
[0132] (Examples 2 to 4, Comparative Examples 1 to 4) Resin compositions were obtained and evaluated in the same manner as in Example 1, except that the compositions of the thermally conductive filler and resin composition were changed as shown in Tables 1, 2-1, and 2-2. The compositions of the thermally conductive filler and resin composition, and the evaluation results of the obtained resin compositions are shown in Tables 1, 2-1, and 2-2.
[0133]
[0134]
[0135]
[0136] Regarding the evaluation results, the resin compositions of Examples 1 to 4, which had a thermal conductivity of 6.0 W / m·K or more, a syringe discharge rate of 10 g / min or more, and a BLT of 100 μm or less, had extremely low thermal resistance and favorable evaluation results when the resin composition layer thickness was 100 μm. On the other hand, when the resin composition of Comparative Example 4, which had a high thermal conductivity but a syringe discharge rate of less than 10 g / min, was used and the resin composition layer thickness was similarly 100 μm, the thermal resistance was high. Furthermore, when the resin composition of Comparative Example 2, which had a syringe discharge rate of 10 g / min or more but low thermal conductivity, was used and the resin composition layer thickness was similarly 100 μm, the thermal resistance was also high. It should be noted that the resin compositions of Comparative Examples 1 and 3, which had large BLTs, could not be made 100 μm thick. The evaluation of the thermal resistance is an evaluation in which the two silicon chips are treated as the substrate of an electronic component, and the overall thermal resistance including the silicon chips is measured, and only the thermal resistance of the silicon chips is subtracted from it, so the evaluation takes into account both the thermal resistance (L / TC) of the resin composition itself and the contact thermal resistance (Rc). For example, when comparing Example 2 and Comparative Example 4, in which the thermal conductivity of the resin composition is the same but the syringe dischargeability is significantly different, the evaluation results of the thermal resistance are significantly different even though the thermal conductivity and thickness of the resin composition are the same (L / TC is the same), and this is presumed to be because the contact thermal resistance is extremely low in Example 2, which has high syringe dischargeability.
[0137] Furthermore, the resin compositions of Examples 1 to 4 have extremely low thermal resistance at the BLT thickness. This shows that by using the resin composition of the present invention, it is possible to easily form a resin composition layer thinner than 100 μm during the production of electronic components, which has extremely low thermal resistance.
[0138] 11, 12 Multifaceted particle a Flat surface
Claims
1. A resin composition comprising a resin and an aluminum nitride-based thermally conductive filler, characterized in that the resin composition has a thermal conductivity of 6.0 W / m·K or more as measured by a hot disk method, a discharge rate of 10 g / min or more when filled into a syringe having an inner diameter of a 2 mm tip discharge part and discharged at a discharge pressure of 0.62 MPa, and a thickness of 100 μm or less as measured after 0.02 ml of the resin composition is sandwiched between two 10 mm x 10 mm silicon chips and a force of 50 N is applied for 60 seconds.
2. The resin composition according to claim 1, wherein the thermally conductive filler has a particle size distribution on a volume basis measured by a laser diffraction scattering method, in which 90% or more of all particles have a particle size in the range of 100 μm or less, a particle size distribution on a volume basis of 40 to 90% of all particles have a particle size in the range of 5 μm or more and 100 μm or less, and a particle size distribution on a volume basis of 5 to 60% of all particles have a particle size in the range of 0.05 μm or more and less than 5 μm, and a scanning electron microscope image taken at 500x magnification of 50% or more of the particles in the range of 5 μm or more and 50 μm or less are polyhedral particles having at least two flat surfaces.
3. The resin composition according to claim 2, wherein the polyhedral particles are aluminum nitride particles.
4. The resin composition according to claim 1, wherein the resin is a silicone resin.
5. The resin composition according to claim 4, wherein the silicone resin comprises a polyorganosiloxane having an average of two or more alkenyl groups bonded to silicon atoms per molecule, and a polyorganosiloxane having an average of two or more hydrosilyl groups per molecule, and further comprises a platinum-based catalyst.
6. A heat dissipation component comprising the resin composition according to any one of claims 1 to 5.
7. An electronic component comprising the heat dissipation member according to claim 6 and a base material having a heat generating portion, said heat dissipation member being arranged in contact with said heat generating portion.
Citation Information
Patent Citations
Heat-conductive silicone composition, method of manufacturing the same, and semiconductor device
JP2020169231A
Thermally conductive liquid composition
WO2022130665A1
Thermally conductive silicone composition
JP2023062399A
Thermally conductive polysiloxane composition
WO2020262449A1
Composition and filler mixture
WO2023013441A1