Double-sided pressure-sensitive adhesive tape for fixing polishing pads

The double-sided adhesive tape, featuring a block copolymer and specific tackifying resins, addresses the issues of adhesive layer instability and peeling by providing high shear strength and slurry resistance, ensuring effective and residue-free fixation of polishing pads in challenging polishing environments.

WO2024225315A1PCT designated stage expired Publication Date: 2024-10-31SEKISUI CHEMICAL CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016071
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Double-sided adhesive tapes used for fixing polishing pads in semiconductor and glass substrate polishing processes face challenges with adhesive layer shifting or peeling due to temperature increases from friction, strong shearing forces, and exposure to acidic or alkaline slurry liquids, leading to inadequate adhesion and resistance.

Method used

A double-sided adhesive tape with a base material having a first adhesive layer composed of a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound, combined with specific tackifying resins that provide high shear strength, slurry resistance, and adhesion to rough surfaces, while maintaining flexibility and preventing adhesive residue.

Benefits of technology

The adhesive tape achieves enhanced shear strength, slurry resistance at high temperatures, and improved adhesion to rough surfaces, ensuring stable fixation of polishing pads during the polishing process without leaving residue.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention pertains to a double-sided pressure-sensitive adhesive tape for fixing polishing pads, the tape comprising a substrate, a first pressure-sensitive adhesive agent layer provided on one surface of the substrate, and a second pressure-sensitive adhesive agent layer provided on the other surface of the substrate. The first pressure-sensitive adhesive agent layer contains: a base polymer; a tackifying resin (T1) that does not include a hydroxyl group or has a hydroxyl value less than 20 mgKOH / g; and a tackifying resin (T2) having a hydroxyl value of 20-120 mgKOH / g. The base polymer contains a block copolymer (A) of a monovinyl-substituted aromatic compound and a conjugated diene compound. In the first pressure-sensitive adhesive agent layer, the percentage content of the base polymer is not less than 40.0 mass% but less than 53.0 mass%. In the first pressure-sensitive adhesive agent layer, the contained amount of the tackifying resin (T1) with respect to 100 parts by mass of the base polymer is 50-100 parts by mass, and the contained amount of the tackifying resin (T2) with respect to 100 parts by mass of the base polymer is 40-80 parts by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Double-sided adhesive tape for fixing polishing pads

[0001] The present invention relates to a double-sided adhesive tape for fixing a polishing pad.

[0002] In processes for polishing semiconductor wafers, liquid crystal glass substrates, and the like to a predetermined thickness (e.g., chemical-mechanical-polishing (CMP) processes), polishing is performed using a polishing cloth or a polishing pad fixed to the platen of a polishing machine. Double-sided adhesive tape is usually used to fix the polishing cloth or polishing pad to the platen of the polishing machine. This double-sided adhesive tape for fixing the polishing cloth is required to have sufficient adhesive strength to prevent the polishing cloth from peeling off during polishing, and to be able to be re-detached from the platen without leaving any adhesive residue when replacing the used polishing cloth.

[0003] As an example of a double-sided adhesive tape for fixing an abrasive cloth, Patent Documents 1 and 2 describe a double-sided adhesive tape for fixing an abrasive material, which has a specific heat-activated adhesive on one side of a plastic film support and a removable adhesive layer on the other side of the plastic film support, with the heat-activated adhesive layer being the bonding surface with the abrasive material.

[0004] JP-A-6-145611 JP-A-6-172721

[0005] The performance requirements for double-sided pressure-sensitive adhesive tapes for fixing polishing pads have been increasing year by year. For example, during polishing, frictional heat causes temperature rises and strong shear forces, which can easily cause the adhesive layer to slip or peel. In particular, in recent years, the use of strongly acidic or strongly alkaline slurry solutions during polishing has led to the adhesive layer being easily deteriorated by the influence of acids or alkalis, making it more likely to slip or peel. However, if high adhesive strength is imparted to the adhesive layer, for example by adding a tackifier resin, in order to prevent slippage or peeling, the adhesive layer becomes hard and it becomes difficult to adhere to polishing pads with rough surfaces. Therefore, there is a need for double-sided pressure-sensitive adhesive tapes for fixing polishing pads that achieve higher levels of resistance to slippage or peeling when exposed to strong shear forces and strongly acidic or strongly alkaline slurry solutions at high temperatures, as well as adhesion to rough surfaces.

[0006] An object of the present invention is to provide a double-sided pressure-sensitive adhesive tape for fixing a polishing pad, which has excellent shear strength and slurry resistance at high temperatures, and also has excellent adhesion to rough surfaces.

[0007] The present disclosure 1 relates to a pressure-sensitive adhesive having a substrate, a first pressure-sensitive adhesive layer on one side of the substrate, and a second pressure-sensitive adhesive layer on the other side thereof, the first pressure-sensitive adhesive layer containing a base polymer, a tackifier resin (T1) that does not contain a hydroxyl group or has a hydroxyl value of less than 20 mgKOH / g, and a tackifier resin (T2) that has a hydroxyl value of 20 mgKOH / g or more and 120 mgKOH / g or less, the base polymer being a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound.

[0013] The double-sided pressure-sensitive adhesive tape for fixing a polishing pad includes a compound (A), wherein the first pressure-sensitive adhesive layer has a base polymer content of 40.0% by mass or more and less than 53.0% by mass, the first pressure-sensitive adhesive layer contains 50 parts by mass or more and 100 parts by mass or less of the tackifier resin (T1) per 100 parts by mass of the base polymer, and the first pressure-sensitive adhesive layer contains 40 parts by mass or more and 80 parts by mass or less of the tackifier resin (T2) per 100 parts by mass of the base polymer.

[0014] Disclosure 2 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of Disclosure 1, wherein the tackifier resin (T1) has a softening point of 80°C or higher.

[0015] Disclosure 3 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of Disclosure 1 or 2, wherein the tackifier resin (T2) has a softening point of 80°C or higher.

[0016] Disclosure 4 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of Disclosure 1, 2, or 3, wherein the tackifier resin (T2) contains a terpene phenol resin. Disclosure 5 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad according to Disclosure 1, 2, 3, or 4, which contains a coumarone resin as the tackifier resin (T2). Disclosure 6 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad according to Disclosure 1, 2, 3, 4, or 5, which contains, as the block copolymer (A), a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 25% by mass or more and 80% by mass or less. Disclosure 7 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad according to Disclosure 6, which contains, as the block copolymer (A), a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 50% by mass or more and 80% by mass or less.Disclosure 8 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad according to Disclosure 7, wherein the first pressure-sensitive adhesive layer contains, as the block copolymer (A), only a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 50% by mass or more and 80% by mass or less. Disclosure 9 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad according to Disclosure 1, 2, 3, 4, 5, 6, 7, or 8, wherein the second pressure-sensitive adhesive layer comprises a base polymer, a tackifier resin (T3) that does not contain a hydroxyl group or has a hydroxyl value of less than 20 mgKOH / g, and a tackifier resin (T4) that has a hydroxyl value of 20 mgKOH / g or more and 120 mgKOH / g or less, the base polymer comprises a block copolymer (B) of a monovinyl-substituted aromatic compound and a conjugated diene compound, the second pressure-sensitive adhesive layer has a base polymer content of 50.0% by mass or more and 70.0% by mass or less, and the content of the tackifier resin (T3) per 100 parts by mass of the base polymer in the second pressure-sensitive adhesive layer is 5 parts by mass or more and 60 parts by mass or less, and the content of the tackifier resin (T4) per 100 parts by mass of the base polymer is 1 part by mass or more and 50 parts by mass or less. Disclosure 10 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of Disclosure 9, wherein the second pressure-sensitive adhesive layer contains, as the block copolymer (B), a block copolymer having a styrene content of 10% by mass or more and 25% by mass or less and a diblock content of 25% by mass or more and 70% by mass or less. Disclosure 11 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of Disclosure 10, wherein the second pressure-sensitive adhesive layer contains, as the block copolymer (B), only a block copolymer having a styrene content of 10% by mass or more and 25% by mass or less and a diblock content of 25% by mass or more and 70% by mass or less. Disclosure 12 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of Disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, or 11, wherein the second pressure-sensitive adhesive layer contains a base polymer, and the base polymer contains a (meth)acrylic copolymer. Disclosure 13 is a double-sided adhesive tape for fixing a polishing pad according to Disclosures 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12, wherein the first adhesive layer is a surface that is bonded to the polishing pad, and the second adhesive layer is a surface that is bonded to the platen of a polishing machine.The present disclosure 14 is the double-sided pressure-sensitive adhesive tape for fixing a polishing pad according to the present disclosure 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, or 13, wherein the substrate comprises a polyolefin film, a polyester film, or a foam. The present invention will be described in detail below.

[0008] The present inventors have investigated a double-sided adhesive tape for bonding a polishing pad to the platen of a polishing machine, and have investigated a pressure-sensitive adhesive layer containing a block copolymer of a monovinyl-substituted aromatic compound and a conjugated diene compound as a base polymer, which can be used as the bonding surface for the polishing pad. The present inventors have further investigated tackifier resins to be added to such pressure-sensitive adhesive layers. As a result, the present inventors have found that by adjusting the base polymer content to a specific level and using, among the tackifier resins, a tackifier resin having a relatively low hydroxyl value within a specific range and a tackifier resin having a relatively high hydroxyl value within a specific range, each in specific amounts, it is possible to improve shear strength (especially shear strength at high temperatures), slurry resistance at high temperatures, and adhesion to rough surfaces. This has led to the completion of the present invention.

[0009] The double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention comprises a substrate, a first pressure-sensitive adhesive layer on one side of the substrate, and a second pressure-sensitive adhesive layer on the other side. The first pressure-sensitive adhesive layer contains a base polymer. The base polymer in the first pressure-sensitive adhesive layer comprises a block copolymer (A) (hereinafter, sometimes simply referred to as "block copolymer (A)") of a monovinyl-substituted aromatic compound and a conjugated diene compound. By including the block copolymer (A) as the base polymer of the first pressure-sensitive adhesive layer, the shear strength of the first pressure-sensitive adhesive layer is sufficiently high. Furthermore, since the block copolymer (A) has relatively low polarity, by including the block copolymer (A) as the base polymer of the first pressure-sensitive adhesive layer, a slurry liquid is less likely to penetrate into the first pressure-sensitive adhesive layer, thereby improving the slurry resistance of the first pressure-sensitive adhesive layer at high temperatures. Furthermore, by including the block copolymer (A) as the base polymer of the first pressure-sensitive adhesive layer, sufficient flexibility is obtained, and the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention has improved adhesion to rough surfaces.

[0010] The block copolymer (A) may be any block copolymer having rubber elasticity at room temperature and having a hard segment portion made of the monovinyl-substituted aromatic compound and a soft segment portion made of the conjugated diene compound. The block copolymer (A) also includes a hydrogenated product of the block copolymer of the monovinyl-substituted aromatic compound and the conjugated diene compound.

[0011] Examples of the monovinyl-substituted aromatic compounds include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, 2,4-dimethylstyrene, 2,4-diisopropylstyrene, 4-t-butylstyrene, 5-t-butyl-2-methylstyrene, vinylethylbenzene, divinylbenzene, trivinylbenzene, divinylnaphthalene, t-butoxystyrene, vinylbenzyldimethylamine, (4-vinylbenzyl)dimethylaminoethyl ether, N,N-dimethylaminoethylstyrene, N,N-dimethylaminomethylstyrene, 2-ethylstyrene, 3-ethylstyrene, 4-ethylstyrene, 2-t-butylstyrene, 3-t-butylstyrene, 4-t-butylstyrene, vinylxylene, vinylnaphthalene, vinylpyridine, diphenylethylene, and tertiary amino group-containing diphenylethylene. Specific examples of the tertiary amino group-containing diphenylethylene include 1-(4-N,N-dimethylaminophenyl)-1-phenylethylene. Among these, styrene is preferred because of its industrial availability. These monovinyl-substituted aromatic compounds may be used alone or in combination of two or more.

[0012] The preferred lower limit of the hard segment content in the block copolymer (A) (when the monovinyl-substituted aromatic compound is styrene, this may be referred to as the "styrene content") is 10% by mass, and the preferred upper limit is 20% by mass. When the hard segment content is 10% by mass or more, sufficient cohesive force is exerted, resulting in sufficiently high shear strength and high-temperature slurry resistance. When the hard segment content is 20% by mass or less, the first pressure-sensitive adhesive layer can be prevented from becoming too hard, resulting in sufficient adhesive strength of the first pressure-sensitive adhesive layer, and the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to a rough surface can be further improved. The more preferred lower limit of the hard segment content is 12% by mass, and the more preferred upper limit is 19% by mass. In this specification, the hard segment content refers to the content of the monovinyl-substituted aromatic compound.

[0013] Examples of the conjugated diene compound include isoprene, 1,3-butadiene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 1,3-heptadiene, 2-phenyl-1,3-butadiene, 3-methyl-1,3-pentadiene, and 2-chloro-1,3-butadiene. Of these, isoprene and butadiene are preferred, and isoprene is more preferred, from the viewpoint of the balance between slurry properties and adhesion to rough surfaces. These conjugated diene compounds may be used alone or in combination of two or more.

[0014] Examples of the block copolymer (A) include styrene-isoprene-styrene (SIS) block copolymer, styrene-butadiene-styrene (SBS) block copolymer, styrene-butadiene-butylene-styrene (SBBS) block copolymer, styrene-ethylene-butylene-styrene (SEBS) block copolymer, styrene-ethylene-propylene-styrene (SEPS) block copolymer, and hydrogenated styrene-butylene rubber (HSBR). Among these, a styrene-isoprene-styrene (SIS) block copolymer is preferred from the viewpoint of providing sufficient flexibility for achieving adhesion to rough surfaces. Furthermore, the block copolymer (A) preferably contains a hydrogenated product, as this further improves the shear strength of the first pressure-sensitive adhesive layer. These block copolymers may be used alone, or two or more types may be used in combination.

[0015] The block copolymer (A) may contain, in addition to a triblock copolymer of the hard segment portion and the soft segment portion, a diblock copolymer of the hard segment portion and the soft segment portion. The preferred lower limit of the diblock content in the block copolymer (A) is 25% by mass, and the preferred upper limit is 80% by mass. A diblock content of 25% by mass or more provides sufficient flexibility, thereby further improving the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to rough surfaces. A diblock content of 80% by mass or less provides sufficient cohesive strength in the first pressure-sensitive adhesive layer, thereby further enhancing the shear strength and slurry resistance at high temperatures of the first pressure-sensitive adhesive layer. A more preferred lower limit of the diblock content is 50% by mass, a more preferred upper limit is 79% by mass, an even more preferred lower limit is 55% by mass, and an even more preferred upper limit is 78% by mass. In this specification, the diblock content refers to the content of the diblock copolymer.

[0016] The first pressure-sensitive adhesive layer preferably contains, as the block copolymer (A), a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 25% by mass or more and 80% by mass or less. In this case, sufficient flexibility is exhibited, thereby further improving the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to rough surfaces. Furthermore, the first pressure-sensitive adhesive layer further enhances shear strength and slurry resistance at high temperatures. More preferably, the first pressure-sensitive adhesive layer contains, as the block copolymer (A), a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 50% by mass or more and 80% by mass or less. It is even more preferable that the first pressure-sensitive adhesive layer contains, as the block copolymer (A), only a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 50% by mass or more and 80% by mass or less.

[0017] The weight-average molecular weight of the block copolymer (A) preferably has a lower limit of 20,000 and a higher limit of 600,000. When the weight-average molecular weight of the block copolymer (A) is 20,000 or more, the heat resistance of the first pressure-sensitive adhesive layer is enhanced, and the shear strength at high temperatures is further improved. When the weight-average molecular weight of the block copolymer (A) is 600,000 or less, the compatibility of the block copolymer (A) with other components is further improved. The weight-average molecular weight of the block copolymer (A) more preferably has a lower limit of 50,000 and a higher limit of 500,000. In this specification, the term "weight-average molecular weight" refers to the weight-average molecular weight measured as a polystyrene-equivalent molecular weight by gel permeation chromatography (GPC). When measuring the weight-average molecular weight by GPC, a column such as LF-804 (manufactured by Showa Denko KK) can be used.

[0018] Examples of the block copolymer (A) include styrene-isoprene-styrene (SIS) block copolymers such as Quintac TM 3450, Quintac TM 3433N, Quintac TM 3520, Quintac TM3270, Quintac TM 3620, Quintac TM 3421, Quintac TM Examples of styrene-ethylene-butylene-styrene (SEBS) block copolymers include DYNARON 8300P and DYNARON 8600P (both manufactured by ENEOS Materials Corporation), and examples of styrene-ethylene-propylene-styrene (SEPS) block copolymers include SEPTON 2063 (manufactured by Kuraray Co., Ltd.).

[0019] The first pressure-sensitive adhesive layer has a base polymer content of 40.0% by mass or more and less than 53.0% by mass. When the base polymer content in the first pressure-sensitive adhesive layer is within the above range, the cohesive strength and flexibility are well balanced, and the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention has improved adhesion to rough surfaces. Furthermore, the shear strength of the first pressure-sensitive adhesive layer is sufficiently high.

[0020] The first pressure-sensitive adhesive layer contains a tackifier resin (T1) that does not contain hydroxyl groups or has a hydroxyl value of less than 20 mgKOH / g, and a tackifier resin (T2) that has a hydroxyl value of 20 mgKOH / g or more and 120 mgKOH / g or less. The inclusion of a tackifier resin in the first pressure-sensitive adhesive layer results in a sufficiently high shear strength of the first pressure-sensitive adhesive layer. Furthermore, the first pressure-sensitive adhesive layer contains, among other tackifier resins, a tackifier resin (T1) that satisfies the relatively low hydroxyl value within the above range and a tackifier resin (T2) that satisfies the relatively high hydroxyl value within the above range. This improves the slurry resistance of the first pressure-sensitive adhesive layer at high temperatures, and the softness of the first pressure-sensitive adhesive layer improves the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to rough surfaces. This is presumably due to the following reasons.

[0021] Typically, when a slurry liquid penetrates into the pressure-sensitive adhesive layer at high temperatures (around 60°C), ionic substances contained in the slurry liquid undergo molecular migration to the interface between the pressure-sensitive adhesive layer and the adherend, and the ionic substances are adsorbed onto the surface of the adherend, causing the pressure-sensitive adhesive layer to slip or peel off. In the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention, since the first pressure-sensitive adhesive layer contains the tackifier resin (T2) with a relatively high polarity, it is thought that the tackifier resin (T2) undergoes molecular migration to the interface between the first pressure-sensitive adhesive layer and the adherend at high temperatures (around 60°C), forming a layer containing a large amount of tackifier resin at the interface. This layer is thought to prevent the ionic substances contained in the slurry liquid from being adsorbed onto the surface of the adherend, improving the slurry resistance of the first pressure-sensitive adhesive layer at high temperatures. Furthermore, when the tackifier resin is the only tackifier resin, the first pressure-sensitive adhesive layer has improved slurry resistance at high temperatures, but the polarity of the layer containing a large amount of the tackifier resin (T2) is too high, which increases the cohesive force of the pressure-sensitive adhesive layer and hardens the pressure-sensitive adhesive layer, thereby reducing adhesion to rough surfaces. In the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention, the first pressure-sensitive adhesive layer contains the tackifier resin (T1) in addition to the tackifier resin (T2), so that the polarity of the layer containing a large amount of the tackifier resin (T2) can be adjusted to an appropriate range, thereby improving the slurry resistance of the first pressure-sensitive adhesive layer at high temperatures and softening the first pressure-sensitive adhesive layer, thereby improving adhesion to rough surfaces.

[0022] The tackifier resin (T1) does not contain hydroxyl groups or has a hydroxyl value of less than 20 mgKOH / g. When the tackifier resin (T1) has a hydroxyl value of less than 20 mgKOH / g, the first pressure-sensitive adhesive layer becomes soft, improving the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to a rough surface and improving the shear strength of the first pressure-sensitive adhesive layer. The hydroxyl value of the tackifier resin (T1) is preferably less than 5 mgKOH / g, and from the viewpoint of the shear strength of the first pressure-sensitive adhesive layer, it is most preferable that the hydroxyl value of the tackifier resin (T1) is 0 mgKOH / g, i.e., the tackifier resin (T1) does not contain hydroxyl groups. In this specification, the hydroxyl value of a tackifier resin refers to the number of milligrams of potassium hydroxide required to neutralize acetic acid bonded to hydroxyl groups when 1 g of the tackifier resin is acetylated, and is defined as a value measured based on the potentiometric titration method specified in JIS K 0070:1992.

[0023] The preferred lower limit of the softening point of the tackifier resin (T1) is 80°C. When the softening point of the tackifier resin (T1) is 80°C or higher, the first pressure-sensitive adhesive layer becomes softer, and the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to a rough surface is further improved. Furthermore, the heat resistance of the first pressure-sensitive adhesive layer is further increased, and the shear strength at high temperatures is further improved. The preferred lower limit of the softening point of the tackifier resin (T1) is 100°C, an even more preferred lower limit is 105°C, and an even more preferred lower limit is 110°C. There is no particular preferred upper limit of the softening point of the tackifier resin (T1), but the substantial upper limit is about 160°C. In this specification, the softening point of the tackifier resin is the temperature at which a solid resin begins to soften and deform, and is defined as a value measured based on the softening point test method (ring and ball method) specified in JIS K 5902, JIS K 2207, etc.

[0024] Specific examples of the tackifier resin (T1) include petroleum resins, terpene resins, styrene resins, and hydrogenated versions thereof. Among these, petroleum resins and terpene resins are preferred from the viewpoint of good compatibility with the base polymer. These tackifier resins (T1) may be used alone or in combination of two or more.

[0025] Examples of the petroleum resins include aliphatic (C5) petroleum resins, aromatic (C9) petroleum resins, C5 / C9 copolymer petroleum resins, and alicyclic petroleum resins. Examples of the terpene resins include α-pinene polymers, β-pinene polymers, dipentene polymers, and modified terpene resins, which are modified versions of these polymers. Examples of modifications of the modified terpene resins include phenol-modification, styrene-modification, hydrogenation-modification, and hydrocarbon-modification. More specific examples of the modified terpene resins include styrene-modified terpene resins and hydrogenated terpene resins. Examples of the styrene resins include styrene homopolymers, α-methylstyrene homopolymers, α-methylstyrene-styrene copolymers, styrene-aliphatic polymers, α-methylstyrene-styrene-aliphatic copolymers, and phenol-modified styrene resins.

[0026] In the first pressure-sensitive adhesive layer, the content of the tackifier resin (T1) relative to 100 parts by mass of the base polymer is at least 50 parts by mass, and at most 100 parts by mass. When the content of the tackifier resin (T1) is at least 50 parts by mass, the shear strength of the first pressure-sensitive adhesive layer is sufficiently high when used in combination with the tackifier resin (T2). When the content of the tackifier resin (T1) is at most 100 parts by mass, the first pressure-sensitive adhesive layer becomes soft, improving the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to a rough surface. The preferred lower limit of the content of the tackifier resin (T1) is 60 parts by mass, the preferred upper limit is 90 parts by mass, the more preferred lower limit is 70 parts by mass, and the more preferred upper limit is 80 parts by mass. When the tackifier resin (T1) contains two or more types of tackifier resins, the content of the tackifier resin (T1) refers to the total content of the two or more types of tackifier resins.

[0027] The lower limit of the hydroxyl value of the tackifier resin (T2) is 20 mgKOH / g, and the upper limit is 120 mgKOH / g. When the hydroxyl value of the tackifier resin (T2) is 20 mgKOH / g or more, the slurry resistance at high temperatures of the first pressure-sensitive adhesive layer is improved, and the shear strength is also improved. When the hydroxyl value of the tackifier resin (T2) is 120 mgKOH / g or less, the compatibility of the tackifier resin (T2) with other components in the first pressure-sensitive adhesive layer, such as the base polymer, is improved. The lower limit of the hydroxyl value of the tackifier resin (T2) is preferably 30 mgKOH / g, and the upper limit is preferably 100 mgKOH / g, more preferably 50 mgKOH / g, and more preferably 80 mgKOH / g.

[0028] The preferred lower limit of the softening point of the tackifier resin (T2) is 80°C. When the softening point of the tackifier resin (T2) is 80°C or higher, the first pressure-sensitive adhesive layer becomes softer, and the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to a rough surface is further improved. In addition, the heat resistance of the first pressure-sensitive adhesive layer is further improved, and the shear strength at high temperatures is further improved. The more preferred lower limit of the softening point of the tackifier resin (T2) is 120°C, an even more preferred lower limit is 130°C, and an even more preferred lower limit is 140°C. In addition, there is no particular preferred upper limit of the softening point of the tackifier resin (T2), but the substantial upper limit is about 180°C.

[0029] Examples of the tackifier resin (T2) include coumarone resins, terpene phenol resins, rosin resins, rosin derivative resins, etc. These tackifier resins (T2) may be used alone or in combination of two or more.

[0030] The coumarone resin may be, for example, a resin containing coumarone and indene as monomer components constituting the resin skeleton (main chain). Examples of monomer components that can constitute the resin skeleton other than coumarone and indene include styrene, α-methylstyrene, methylindene, vinyltoluene, etc.

[0031] The terpene phenolic resin refers to a polymer containing a terpene residue and a phenol residue. The term "terpene phenolic resin" encompasses both a copolymer of a terpene and a phenolic compound (terpene-phenol copolymer resin) and a phenol-modified terpene resin obtained by modifying a terpene homopolymer or copolymer (terpene resin, typically an unmodified terpene resin) with phenol. The terpene constituting the terpene phenolic resin is not particularly limited, but monoterpenes such as α-pinene, β-pinene, and limonene are preferred. Limonene includes d-, l-, and d / l-forms (dipentene).

[0032] More specifically, examples of the rosin resin include unmodified rosins (raw rosins) such as gum rosin, wood rosin, and tall oil rosin, as well as modified rosins obtained by modifying these unmodified rosins. Modifications of the modified rosins include, for example, hydrogenation, disproportionation, and polymerization. More specifically, examples of the modified rosins include hydrogenated rosin, disproportionated rosin, polymerized rosin, and other chemically modified rosins.

[0033] More specifically, examples of the rosin derivative resin include rosin ester resins obtained by esterifying the rosin resin with alcohols, unsaturated fatty acid-modified rosin resins obtained by modifying the rosin resin with unsaturated fatty acids, and unsaturated fatty acid-modified rosin ester resins obtained by modifying the rosin ester resin with unsaturated fatty acids. Other examples of the rosin derivative resin include rosin alcohol resins obtained by reducing the carboxyl groups in the unsaturated fatty acid-modified rosin resins or unsaturated fatty acid-modified rosin ester resins. Furthermore, examples of the rosin derivative resin include metal salts of the rosin resins or rosin derivative resins (especially rosin ester resins) and rosin phenolic resins. Rosin phenolic resins can be obtained by adding phenol to the rosin resin or rosin derivative resin in the presence of an acid catalyst and then thermally polymerizing the resulting mixture.

[0034] The tackifier resin (T2) preferably contains at least one tackifier resin selected from the group consisting of a terpene phenol resin and a coumarone resin. When the tackifier resin (T2) contains the terpene phenol resin, the slurry resistance of the first pressure-sensitive adhesive layer at high temperatures is further improved.

[0035] When the tackifier resin (T2) contains the coumarone resin, the tackifier resin (T2) interacts with the hard segment moieties in the base polymer, further stabilizing the physical crosslinking between the hard segment moieties. Therefore, when the tackifier resin (T2) contains the coumarone resin, the heat resistance and bulk strength of the first PSA layer are increased, and the shear strength at high temperatures is further improved.

[0036] It is more preferable that the tackifier resin (T2) contains both the coumarone resin and the terpene phenol resin, since this can improve both the shear strength and the slurry resistance at high temperatures of the first pressure-sensitive adhesive layer while maintaining a balance between them.

[0037] In the first pressure-sensitive adhesive layer, the lower limit of the content of the tackifier resin (T2) relative to 100 parts by mass of the base polymer is 40 parts by mass, and the upper limit is 80 parts by mass. When the content of the tackifier resin (T2) is 40 parts by mass or more, the shear strength of the first pressure-sensitive adhesive layer is sufficiently high, and the slurry resistance at high temperatures is improved. When the content of the tackifier resin (T2) is 80 parts by mass or less, the first pressure-sensitive adhesive layer becomes soft, and the adhesion of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention to a rough surface is improved. The lower limit of the content of the tackifier resin (T2) is preferably 42 parts by mass, and the upper limit is preferably 60 parts by mass, more preferably 45 parts by mass, and even more preferably 55 parts by mass. Note that when the tackifier resin (T2) contains two or more types of tackifier resins, the content of the tackifier resin (T2) refers to the total content of the two or more types of tackifier resins.

[0038] The first pressure-sensitive adhesive layer may contain another tackifier resin having a hydroxyl value of more than 120 mgKOH / g. The preferred upper limit of the content of the other tackifier resin in the first pressure-sensitive adhesive layer relative to 100 parts by mass of the base polymer is 5 parts by mass. If the content of the other tackifier resin is 5 parts by mass or less, the first pressure-sensitive adhesive layer becomes softer and its adhesion to rough surfaces is further improved. The preferred upper limit of the content of the other tackifier resin is 2.5 parts by mass, and even more preferred upper limit is 0.1 parts by mass. It is particularly preferred that the first pressure-sensitive adhesive layer does not contain the other tackifier resin, as this would result in poor compatibility with the tackifier resin (T1) and the base polymer of the first pressure-sensitive adhesive layer, preventing sufficient performance.

[0039] The first pressure-sensitive adhesive layer may further contain additives such as a filler, an antioxidant, an antioxidant, and a colorant.

[0040] The thickness of the first pressure-sensitive adhesive layer is not particularly limited, with a preferred lower limit of 20 μm and a preferred upper limit of 100 μm. When the thickness of the first pressure-sensitive adhesive layer is within the above range, the adhesive strength of the first pressure-sensitive adhesive layer is sufficient, and the shear strength and slurry resistance of the first pressure-sensitive adhesive layer at high temperatures are sufficiently improved. The more preferred lower limit of the thickness of the first pressure-sensitive adhesive layer is 25 μm, and the more preferred upper limit is 85 μm.

[0041] The second pressure-sensitive adhesive layer may be the same pressure-sensitive adhesive layer as the first pressure-sensitive adhesive layer described above, but it is preferable to use a different pressure-sensitive adhesive layer. By using a pressure-sensitive adhesive layer different from the first pressure-sensitive adhesive layer, the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention can be more suitably used for fixing a polishing pad. In this case, it is preferable that the first pressure-sensitive adhesive layer is the surface to be bonded to a polishing cloth, abrasive, polishing pad, etc., and the second pressure-sensitive adhesive layer is the surface to be bonded to the platen of a polishing machine.

[0042] When the second pressure-sensitive adhesive layer has a different composition from that of the first pressure-sensitive adhesive layer as described above, the second pressure-sensitive adhesive layer can contain a pressure-sensitive adhesive used in ordinary pressure-sensitive adhesive tapes, such as an acrylic resin-based pressure-sensitive adhesive, a rubber-based pressure-sensitive adhesive, a silicone-based pressure-sensitive adhesive, a urethane-based pressure-sensitive adhesive, etc. Among these, from the viewpoints of slurry resistance, adhesion to a surface plate, and removability, it is preferable that the second pressure-sensitive adhesive layer contains a rubber-based pressure-sensitive adhesive.

[0043] The second pressure-sensitive adhesive layer preferably contains a base polymer. Examples of the base polymer in the second pressure-sensitive adhesive layer include block copolymers, (meth)acrylic copolymers, silicone polymers, and urethane polymers. Among these, block copolymers are preferred. In this specification, (meth)acrylic refers to acrylic or methacrylic.

[0044] The base polymer in the second pressure-sensitive adhesive layer preferably contains a block copolymer (B) (hereinafter sometimes simply referred to as "block copolymer (B)") of a monovinyl-substituted aromatic compound and a conjugated diene compound. When the base polymer of the second pressure-sensitive adhesive layer contains the block copolymer (B), the shear strength of the second pressure-sensitive adhesive layer at high temperatures is more sufficiently increased. Furthermore, since the block copolymer (B) has relatively low polarity, when the base polymer of the second pressure-sensitive adhesive layer contains the block copolymer (B), a slurry liquid is less likely to penetrate into the second pressure-sensitive adhesive layer, thereby further improving the slurry resistance of the second pressure-sensitive adhesive layer at high temperatures. Furthermore, when the base polymer of the second pressure-sensitive adhesive layer contains the block copolymer (B), the adhesion of the second pressure-sensitive adhesive layer is suppressed compared to when the second pressure-sensitive adhesive layer contains natural rubber, and removability is further improved.

[0045] Examples of the monovinyl-substituted aromatic compound and the conjugated diene compound used in the block copolymer (B) include the same compounds as those used in the block copolymer (A) described above.

[0046] The preferred lower limit of the hard segment content in the block copolymer (B) (sometimes referred to as the "styrene content" when the monovinyl-substituted aromatic compound is styrene) is 10% by mass, and the preferred upper limit is 25% by mass. When the hard segment content is 10% by mass or more, increased adhesion of the second pressure-sensitive adhesive layer is further suppressed, and removability is further improved. When the hard segment content is 25% by mass or less, the second pressure-sensitive adhesive layer can be prevented from becoming too hard, and the adhesive strength of the second pressure-sensitive adhesive layer is sufficient, resulting in sufficiently high shear strength and slurry resistance at high temperatures of the second pressure-sensitive adhesive layer. A more preferred lower limit of the hard segment content is 12% by mass, and a more preferred upper limit is 20% by mass.

[0047] The block copolymer (B) may contain, in addition to a triblock copolymer of the hard segment portion and the soft segment portion, a diblock copolymer of the hard segment portion and the soft segment portion. The preferred lower limit of the diblock content in the block copolymer (B) is 25% by mass, and the preferred upper limit is 70% by mass. A diblock content of 25% by mass or more can prevent the second pressure-sensitive adhesive layer from becoming too hard, resulting in sufficient adhesive strength and more sufficiently high slurry resistance of the second pressure-sensitive adhesive layer. A diblock content of 70% by mass or less can further suppress increased adhesion of the second pressure-sensitive adhesive layer, further improving removability. A more preferred lower limit of the diblock content is 30% by mass, and a more preferred upper limit is 60% by mass.

[0048] The second pressure-sensitive adhesive layer preferably contains, as the block copolymer (B), a block copolymer having a styrene content of 10% by mass or more and 25% by mass or less and a diblock content of 25% by mass or more and 70% by mass or less. In this case, the pressure-sensitive adhesive layer can be prevented from becoming too hard, the adhesion of the second pressure-sensitive adhesive layer can be further suppressed, and removability can be further improved. Furthermore, the second pressure-sensitive adhesive layer has sufficiently high shear strength and slurry resistance at high temperatures. More preferably, the second pressure-sensitive adhesive layer contains, as the block copolymer (B), only a block copolymer having a styrene content of 10% by mass or more and 25% by mass or less and a diblock content of 25% by mass or more and 70% by mass or less.

[0049] The weight-average molecular weight of the block copolymer (B) is not particularly limited, but a preferred lower limit is 20,000 and a preferred upper limit is 600,000. If the weight-average molecular weight of the block copolymer (B) is 20,000 or more, the heat resistance of the second pressure-sensitive adhesive layer is increased, and the shear strength at high temperatures is further improved. If the weight-average molecular weight of the block copolymer (B) is 600,000 or less, the compatibility of the block copolymer (B) with other components is further improved. A more preferred lower limit of the weight-average molecular weight of the block copolymer (B) is 50,000 and a more preferred upper limit is 500,000.

[0050] Examples of the block copolymer (B) include the same as the block copolymer (A) described above.

[0051] When the base polymer in the second pressure-sensitive adhesive layer contains the block copolymer (B), the base polymer content of the second pressure-sensitive adhesive layer preferably has a lower limit of 50.0% by mass and a higher limit of 70.0% by mass. By having the base polymer content within the above range, the adhesion of the second pressure-sensitive adhesive layer is further suppressed, and the removability is further improved. Furthermore, the shear strength of the second pressure-sensitive adhesive layer at high temperatures is sufficiently high. The base polymer content is more preferably 55.0% by mass and a higher limit of 68.0% by mass.

[0052] From the viewpoints of adhesion to a surface plate and removability, the base polymer in the second pressure-sensitive adhesive layer may contain a (meth)acrylic copolymer. The (meth)acrylic copolymer preferably has a structural unit derived from a (meth)acrylic acid alkyl ester. Examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, n-hexyl (meth)acrylate, isohexyl (meth)acrylate, cyclohexyl (meth)acrylate, n-heptyl (meth)acrylate, isoheptyl (meth)acrylate, and 2-(meth)acrylic acid alkyl ester. Examples of the alkyl (meth)acrylate include ethylhexyl, n-octyl (meth)acrylate, isooctyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, n-decyl (meth)acrylate, isodecyl (meth)acrylate, isobornyl (meth)acrylate, n-dodecyl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, and behenyl (meth)acrylate. These alkyl (meth)acrylates may be used alone or in combination of two or more.

[0053] The (meth)acrylic copolymer may optionally contain a structural unit derived from another copolymerizable polymerizable monomer other than the (meth)acrylic acid alkyl ester. Examples of the other copolymerizable polymerizable monomer include a polar functional group-containing monomer. These other copolymerizable polymerizable monomers may be used alone or in combination of two or more.

[0054] Examples of the polar functional group-containing monomer include hydroxyalkyl (meth)acrylate, glycerin dimethacrylate, glycidyl (meth)acrylate, 2-methacryloyloxyethyl isocyanate, (meth)acrylic acid, itaconic acid, maleic anhydride, crotonic acid, maleic acid, and fumaric acid. Of these, (meth)acrylic acid is preferred from the viewpoint of the balance between adhesiveness and cohesive strength. Specific examples of the hydroxyalkyl (meth)acrylate include 2-hydroxyethyl (meth)acrylate.

[0055] The weight-average molecular weight (Mw) of the (meth)acrylic copolymer preferably has a lower limit of 200,000 and an upper limit of 1,400,000. When the weight-average molecular weight of the (meth)acrylic copolymer is 200,000 or more, a good balance between adhesive strength and cohesive strength is achieved. When the weight-average molecular weight of the (meth)acrylic copolymer is 1,400,000 or less, a good balance between adhesive strength and cohesive strength is achieved. A more preferred lower limit of the weight-average molecular weight of the (meth)acrylic copolymer is 250,000, a more preferred upper limit is 1,300,000, an even more preferred lower limit is 280,000, and an even more preferred upper limit is 1,200,000. In this specification, the weight-average molecular weight (Mw) is the weight-average molecular weight calculated in terms of standard polystyrene by GPC (gel permeation chromatography). Specifically, it can be measured by the following method, etc. That is, the obtained acrylic copolymer solution is diluted with tetrahydrofuran (THF), and the obtained diluted solution is filtered through a filter. The obtained filtrate is supplied to a gel permeation chromatograph (Waters, "2690 Separations Model", etc.), and GPC measurement is performed under conditions of a sample flow rate of 1 mL / min and a column temperature of 40°C to measure the polystyrene-equivalent molecular weight of the (meth)acrylic copolymer, and this molecular weight is taken as the weight average molecular weight (Mw) of the (meth)acrylic copolymer. Examples of the column used include GPC KF-806L (Showa Denko KK), and examples of the detector include a differential refractometer.

[0056] The (meth)acrylic copolymer can be obtained by subjecting a monomer mixture comprising the (meth)acrylic acid alkyl ester, the other copolymerizable polymerizable monomer, etc., to a radical reaction in the presence of a polymerization initiator. As a method for subjecting the monomer mixture to a radical reaction, i.e., a polymerization method, a conventionally known method can be used, such as solution polymerization (boiling point polymerization or constant temperature polymerization), emulsion polymerization, suspension polymerization, bulk polymerization, etc.

[0057] When the base polymer in the second pressure-sensitive adhesive layer contains the block copolymer (B), the second pressure-sensitive adhesive layer preferably contains a tackifier resin (T3) that does not contain hydroxyl groups or has a hydroxyl value of less than 20 mgKOH / g, and a tackifier resin (T4) that has a hydroxyl value of 20 mgKOH / g or more and 120 mgKOH / g or less. By containing a tackifier resin in the second pressure-sensitive adhesive layer, the shear strength of the second pressure-sensitive adhesive layer at high temperatures is sufficiently high. Furthermore, by containing, among the tackifier resins, a tackifier resin (T3) that satisfies the relatively low hydroxyl value within the above range and a tackifier resin (T4) that satisfies the relatively high hydroxyl value within the above range, the slurry resistance of the second pressure-sensitive adhesive layer at high temperatures is further improved, and the increase in adhesion is suppressed, resulting in further improved removability. This is presumably due to the following reasons.

[0058] Typically, when a slurry liquid penetrates into the pressure-sensitive adhesive layer at high temperatures (around 60°C), ionic substances contained in the slurry liquid undergo molecular migration to the interface between the pressure-sensitive adhesive layer and the adherend, and the ionic substances are adsorbed onto the surface of the adherend, causing the pressure-sensitive adhesive layer to slip or peel off. In the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention, since the second pressure-sensitive adhesive layer contains the tackifier resin (T4) with a relatively high polarity, it is thought that the tackifier resin (T4) undergoes molecular migration to the interface between the second pressure-sensitive adhesive layer and the adherend at high temperatures (around 60°C), forming a layer containing a large amount of tackifier resin at the interface. This layer is thought to prevent the ionic substances contained in the slurry liquid from being adsorbed onto the surface of the adherend, further improving the slurry resistance of the second pressure-sensitive adhesive layer at high temperatures. Furthermore, when the tackifier resin is the tackifier resin (T4) alone, the second pressure-sensitive adhesive layer has improved slurry resistance at high temperatures, but the layer containing a large amount of the tackifier resin (T4) has too high a polarity, which tends to promote adhesion and reduce removability. In the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention, the second pressure-sensitive adhesive layer contains the tackifier resin (T3) in addition to the tackifier resin (T4), so that the polarity of the layer containing a large amount of the tackifier resin (T4) can be adjusted to an appropriate range, thereby further improving the slurry resistance at high temperatures of the second pressure-sensitive adhesive layer, suppressing adhesion promotion, and further improving removability.

[0059] The tackifier resin (T3) preferably does not contain a hydroxyl group or has a hydroxyl value of less than 20 mgKOH / g. When the tackifier resin (T3) has a hydroxyl value of less than 20 mgKOH / g, the adhesion of the second pressure-sensitive adhesive layer is suppressed, removability is further improved, and the shear strength of the second pressure-sensitive adhesive layer at high temperatures is further improved. The hydroxyl value of the tackifier resin (T3) is more preferably less than 5 mgKOH / g, and from the viewpoint of the shear strength of the first pressure-sensitive adhesive layer at high temperatures, the hydroxyl value of the tackifier resin (T3) is most preferably 0 mgKOH / g, i.e., the tackifier resin (T3) does not contain a hydroxyl group.

[0060] The preferred lower limit of the softening point of the tackifier resin (T3) is 110°C. When the softening point of the tackifier resin (T3) is 110°C or higher, the heat resistance of the second pressure-sensitive adhesive layer is further increased, and the shear strength at high temperatures is further improved. The more preferred lower limit of the softening point of the tackifier resin (T3) is 115°C. There is no particular preferred upper limit of the softening point of the tackifier resin (T3), but the substantial upper limit is about 160°C.

[0061] Examples of the tackifier resin (T3) include the same resins as those used in the tackifier resin (T1) described above.

[0062] The tackifier resin (T3) may be two or more types of tackifier resins, and in this case, the tackifier resin (T3) preferably contains the styrene resin. By including the tackifier resin (T3) in the styrene resin, the shear strength of the second pressure-sensitive adhesive layer at high temperatures is further improved. The lower limit of the amount of the styrene resin relative to 100 parts by mass of the base polymer in the second pressure-sensitive adhesive layer is preferably 3 parts by mass, and the upper limit is preferably 40 parts by mass, more preferably 5 parts by mass, and more preferably 30 parts by mass, and even more preferably 10 parts by mass, and even more preferably 20 parts by mass.

[0063] In the second PSA layer, the preferred lower limit of the content of the tackifier resin (T3) relative to 100 parts by mass of the base polymer is 5 parts by mass, and the preferred upper limit is 60 parts by mass. When the content of the tackifier resin (T3) is 5 parts by mass or more, when used in combination with the tackifier resin (T4), the adhesion of the second PSA layer is suppressed, improving removability, while also providing a sufficiently high shear strength at high temperatures. When the content of the tackifier resin (T3) is 60 parts by mass or less, the adhesion of the second PSA layer is suppressed, improving removability. A more preferred lower limit of the content of the tackifier resin (T3) is 20 parts by mass, a more preferred upper limit is 50 parts by mass, an even more preferred lower limit is 30 parts by mass, and an even more preferred upper limit is 40 parts by mass. When the tackifier resin (T3) contains two or more types of tackifier resins, the content of the tackifier resin (T3) refers to the total content of the two or more types of tackifier resins.

[0064] The hydroxyl value of the tackifier resin (T4) preferably has a lower limit of 20 mgKOH / g and a higher limit of 120 mgKOH / g. When the hydroxyl value of the tackifier resin (T2) is 20 mgKOH / g or higher, the second pressure-sensitive adhesive layer has improved slurry resistance at high temperatures and improved shear strength at high temperatures. When the hydroxyl value of the tackifier resin (T4) is 120 mgKOH / g or lower, the compatibility of the tackifier resin (T4) with other components such as the base polymer is improved. The hydroxyl value of the tackifier resin (T4) is more preferably 30 mgKOH / g or lower, more preferably 100 mgKOH / g or higher, even more preferably 50 mgKOH / g or lower, and even more preferably 80 mgKOH / g or higher.

[0065] The preferred lower limit of the softening point of the tackifier resin (T4) is 120°C. When the softening point of the tackifier resin (T4) is 120°C or higher, the heat resistance of the second pressure-sensitive adhesive layer is further increased, and the shear strength at high temperatures is further improved. The more preferred lower limit of the softening point of the tackifier resin (T4) is 140°C. There is no particular preferred upper limit of the softening point of the tackifier resin (T4), but the substantial upper limit is about 180°C.

[0066] Examples of the tackifier resin (T4) include the same resins as those used for the tackifier resin (T2) described above.

[0067] The tackifier resin (T4) preferably contains two or more tackifier resins. In particular, the tackifier resin (T4) more preferably contains a coumarone resin. The coumarone resin interacts with the hard segment moieties in the base polymer of the second pressure-sensitive adhesive layer, further stabilizing the physical crosslinking between the hard segment moieties. Therefore, when the tackifier resin (T4) contains the coumarone resin, the heat resistance and bulk strength of the second pressure-sensitive adhesive layer are enhanced, and the shear strength at high temperatures is further improved. The content of the coumarone resin per 100 parts by mass of the base polymer in the second pressure-sensitive adhesive layer is not particularly limited, but a preferred lower limit is 5 parts by mass, a preferred upper limit is 30 parts by mass, a more preferred lower limit is 10 parts by mass, a more preferred upper limit is 20 parts by mass, a still more preferred lower limit is 12.5 parts by mass, and a still more preferred upper limit is 17.5 parts by mass.

[0068] The tackifier resin (T4) more preferably contains at least one tackifier resin (hereinafter also referred to as "terpene phenolic resin, etc.") selected from the group consisting of terpene phenolic resins, rosin resins, and rosin derivative resins. When the tackifier resin (T4) contains the terpene phenolic resin, etc., the second pressure-sensitive adhesive layer has further improved slurry resistance at high temperatures. Among the terpene phenolic resins, etc., terpene phenolic resins are more preferred because they further improve the slurry resistance of the second pressure-sensitive adhesive layer at high temperatures. The content of the terpene phenolic resin, etc., per 100 parts by mass of the base polymer in the second pressure-sensitive adhesive layer is not particularly limited, but a preferred lower limit is 1 part by mass, a preferred upper limit is 15 parts by mass, a more preferred lower limit is 5 parts by mass, and a more preferred upper limit is 10 parts by mass.

[0069] It is particularly preferable that the tackifier resin (T4) contains both the coumarone resin and the terpene phenol resin, etc., since this can improve both the shear strength at high temperatures and the slurry resistance at high temperatures of the second pressure-sensitive adhesive layer while maintaining a balance between them.

[0070] In the second pressure-sensitive adhesive layer, the content of the tackifier resin (T4) relative to 100 parts by mass of the base polymer is preferably 1 part by mass at the lower limit and 50 parts by mass at the upper limit. When the content of the tackifier resin (T4) is 1 part by mass or more, the shear strength of the second pressure-sensitive adhesive layer at high temperatures is sufficiently increased, and the slurry resistance at high temperatures is further improved. When the content of the tackifier resin (T4) is 50 parts by mass or less, the adhesion of the second pressure-sensitive adhesive layer is suppressed and the removability is further improved. The lower limit of the content of the tackifier resin (T4) is more preferably 3 parts by mass, and the upper limit is more preferably 35 parts by mass, and the even more preferably 5 parts by mass, and the even more preferably 30 parts by mass at the upper limit. Note that when the tackifier resin (T4) contains two or more types of tackifier resins, the content of the tackifier resin (T4) refers to the total content of the two or more types of tackifier resins.

[0071] In the second pressure-sensitive adhesive layer, the preferred lower limit of the total content of the tackifier resin (T3) and the tackifier resin (T4) relative to 100 parts by mass of the base polymer is 20 parts by mass, and the preferred upper limit is 80 parts by mass. When the total content of the tackifier resin (T3) and the tackifier resin (T4) is 20 parts by mass or more, the shear strength of the second pressure-sensitive adhesive layer at high temperatures is sufficiently increased, and the slurry resistance at high temperatures is further improved. When the total content of the tackifier resin (T3) and the tackifier resin (T4) is 80 parts by mass or less, the adhesion of the second pressure-sensitive adhesive layer is suppressed, and the removability is further improved. A more preferred lower limit of the total content of the tackifier resin (T3) and the tackifier resin (T4) is 40 parts by mass, and a more preferred upper limit is 60 parts by mass.

[0072] When the base polymer in the second pressure-sensitive adhesive layer contains the block copolymer (B), the second pressure-sensitive adhesive layer may contain another tackifier resin having a hydroxyl value of more than 120 mgKOH / g. The upper limit of the content of the other tackifier resin in the second pressure-sensitive adhesive layer relative to 100 parts by mass of the base polymer is preferably 5 parts by mass. By having the content of the other tackifier resin be 5 parts by mass or less, the adhesion of the second pressure-sensitive adhesive layer is suppressed and removability is further improved. The upper limit of the content of the other tackifier resin is more preferably 2.5 parts by mass, and even more preferably 0.1 parts by mass. From the viewpoint of poor compatibility with the tackifier resin (T3) and the base polymer and inability to exhibit sufficient performance, it is most preferable that the second pressure-sensitive adhesive layer does not contain the other tackifier resin.

[0073] When the base polymer in the second pressure-sensitive adhesive layer contains the (meth)acrylic copolymer, the second pressure-sensitive adhesive layer preferably contains a crosslinking agent, which causes the (meth)acrylic copolymer to form a crosslinked structure, making it less likely for cohesive failure to occur on the surface plate when the pressure-sensitive adhesive tape is re-peeled.

[0074] Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, and metal chelate-based crosslinking agents. Among these, isocyanate-based crosslinking agents are preferred from the viewpoint of the balance between adhesive strength and cohesive strength. Specific examples of the isocyanate-based crosslinking agent include Takenate D-101E (manufactured by Mitsui Chemicals, Inc.).

[0075] The preferred lower limit of the content of the crosslinking agent relative to 100 parts by mass of the (meth)acrylic copolymer is 0.1 parts by mass, and the preferred upper limit is 5 parts by mass. When the content of the crosslinking agent is 0.1 parts by mass or more, the adhesive is less likely to undergo cohesive failure when re-peeled from the surface plate. When the content of the crosslinking agent is 5 parts by mass or less, peeling due to stress during polishing, etc. is less likely. The more preferred lower limit of the content of the crosslinking agent is 0.2 parts by mass, even more preferred lower limit is 0.3 parts by mass, even more preferred upper limit is 4 parts by mass, and even more preferred upper limit is 3 parts by mass.

[0076] The second pressure-sensitive adhesive layer may further contain additives such as a filler, an antioxidant, an antioxidant, and a colorant.

[0077] The thickness of the second pressure-sensitive adhesive layer is not particularly limited, with a preferred lower limit of 20 μm and a preferred upper limit of 100 μm. When the thickness of the second pressure-sensitive adhesive layer is within the above range, the adhesive strength of the second pressure-sensitive adhesive layer is sufficient, and the shear strength and slurry resistance of the second pressure-sensitive adhesive layer at high temperatures are sufficiently improved. The more preferred lower limit of the thickness of the second pressure-sensitive adhesive layer is 40 μm, and the more preferred upper limit is 85 μm.

[0078] From the viewpoint of ease of application and peeling, the substrate preferably includes a resin film or a foam. Examples of the resin film include polyester film, polyolefin film, polyurethane film, etc. Among these, polyester film is preferred because it is flat, has little thickness variation, and is high in strength, and among polyester films, polyethylene terephthalate film is more preferred. Furthermore, from the viewpoint of ease of processing and water resistance, polyolefin film is preferred. That is, the substrate preferably includes a polyolefin film, polyester film, or a foam. Examples of the foam include polyolefin foam, polyurethane foam, etc.

[0079] The substrate may contain additives such as fillers, ultraviolet absorbers, light stabilizers, and antistatic agents within limits that do not impair the physical properties of the substrate.

[0080] The thickness of the substrate is not particularly limited, but a preferred lower limit is 2 μm, and a preferred upper limit is 2000 μm. If the thickness of the substrate is 2 μm or more, the substrate can be prevented from breaking when the adhesive tape is re-peeled, thereby further improving the removability of the adhesive tape. If the thickness of the substrate is 2000 μm or less, it becomes easy to adjust the pressure when pressing the adhesive tape against the adherend, and sufficient adhesive strength can be obtained. A more preferred lower limit of the thickness of the substrate is 12 μm, and a more preferred upper limit is 1000 μm.

[0081] The double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention may further comprise a separator. By comprising a separator, the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention can be produced in a roll shape, resulting in a tape that is easier to handle.

[0082] The separator is not particularly limited, and examples thereof include release paper and release film obtained by subjecting at least one surface of paper or plastic film to a release treatment using a silicone-based release agent, a long-chain alkyl group pendant graft polymer-based release agent, etc. Examples of the plastic film include polyester film, polyolefin film, polyurethane film, etc. Examples of the paper include glassine paper and kraft paper, etc.

[0083] The thickness of the separator preferably has a lower limit of 10 μm and an upper limit of 200 μm. By having the thickness of the separator within this range, the handleability of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention is further improved, resulting in superior handling during use and transportation. The lower limit of the thickness of the separator is more preferably 20 μm and the upper limit is more preferably 190 μm.

[0084] The double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention can be produced, for example, by the following method when the substrate has pressure-sensitive adhesive layers of the same composition and thickness on both sides of the substrate. First, a pressure-sensitive adhesive solution containing the block copolymer (A), the tackifier resin (T1), and the tackifier resin (T2) is prepared. Next, the pressure-sensitive adhesive solution obtained above is applied to the release-treated surface of a release film, one side of which has been release-treated, and dried to produce a laminate sheet having a pressure-sensitive adhesive layer on the release-treated surface of the release film. Another laminate sheet is produced in the same manner. Next, the pressure-sensitive adhesive layers of the two laminate sheets produced are transferred and laminated onto different surfaces of the substrate, respectively, to produce a pressure-sensitive adhesive tape having a first pressure-sensitive adhesive layer on one side of the substrate and a second pressure-sensitive adhesive layer of the same composition and thickness as the first pressure-sensitive adhesive layer on the other side of the substrate.

[0085] Although the use of the double-sided pressure-sensitive adhesive tape for fixing a polishing pad of the present invention is not particularly limited, because it has excellent shear strength and slurry resistance at high temperatures and excellent adhesion to rough surfaces, it is preferably used to fix a polishing cloth, abrasive, polishing pad, etc. to the platen of a polishing machine in the process of polishing semiconductor wafers, liquid crystal glass substrates, etc. to a predetermined thickness. Examples of such polishing processes include chemical-mechanical-polishing (CMP) processes.

[0086] From the viewpoint of alignment during lamination, the double-sided adhesive tape for fixing a polishing pad of the present invention is preferably wider than the width of the object to be polished in the polishing process, such as a semiconductor wafer or a glass substrate for liquid crystal displays. Specifically, the preferred lower limit of the width of the double-sided adhesive tape for fixing a polishing pad of the present invention is 300 mm, more preferably 600 mm, and the preferred upper limit is 3000 mm, more preferably 2500 mm.

[0087] According to the present invention, it is possible to provide a double-sided pressure-sensitive adhesive tape for fixing a polishing pad, which has excellent shear strength and slurry resistance at high temperatures, and also has excellent adhesion to rough surfaces.

[0088] The following examples will further illustrate the present invention, but the present invention is not limited to these examples.

[0089] (Adhesives 1 to 21) An SIS copolymer or an SBS copolymer and a tackifier resin shown in Tables 1 and 2 were added to a reactor, and toluene was further added as a solvent so that the total concentration of the SIS copolymer or SBS copolymer and the tackifier resin was 50 mass %, and the mixture was thoroughly stirred to obtain an adhesive-containing solution containing Adhesives 1 to 21.

[0090]

[0091]

[0092] (Adhesives 22-24) (Synthesis of Acrylic Copolymer) Ethyl acetate was added as a solvent to a reactor equipped with a thermometer, a stirrer, and a cooling tube. The atmosphere was then replaced with nitrogen, and the reactor was heated to initiate reflux. After the solvent boiled, a polymerization initiator solution prepared by diluting 0.2 parts by mass of azobisisobutyronitrile 10 times with ethyl acetate was added. An ethyl acetate solution of the monomer mixture shown in Table 3 was then added dropwise from the dropping funnel to the reactor over 2 hours so that the monomer concentration was 30% by mass. After the completion of the dropwise addition, the polymerization reaction was carried out for 4 hours to obtain a solution containing an acrylic copolymer. The resulting acrylic copolymer was diluted 50 times with tetrahydrofuran (THF), and the resulting diluted solution was filtered through a filter (material: polytetrafluoroethylene, pore diameter: 0.2 μm) to prepare a measurement sample. The measurement sample was supplied to a gel permeation chromatograph (Waters Corporation, "2690 Separations Module") and subjected to GPC measurement at a sample flow rate of 1 mL / min and a column temperature of 40°C to measure the polystyrene-equivalent molecular weight of the acrylic copolymer and determine the weight-average molecular weight. The results are shown in Table 3.

[0093] (Preparation of adhesive-containing solution) In the above-mentioned "(Synthesis of acrylic copolymer)", 1 part by mass of Takenate D-101E (manufactured by Mitsui Chemicals, Inc.) as an isocyanate-based crosslinking agent was added to 100 parts by mass of the acrylic copolymer in the solution containing the obtained acrylic copolymer, and in the case of adhesive 24, a tackifier resin shown in Table 3 was further added, and the mixture was thoroughly stirred to obtain an adhesive-containing solution containing adhesives 22 to 24.

[0094] The materials in Table 3 are as follows: BA: n-butyl (meth)acrylate 2EHA: 2-ethylhexyl (meth)acrylate AAc: acrylic acid

[0095]

[0096] (Examples 1, 3, 5-17, 19, Comparative Examples 1-6) A polyethylene terephthalate (PET) film with one release-treated surface was prepared. A pressure-sensitive adhesive solution of the type shown in Tables 4-6 was applied to the release-treated surface of this polyethylene terephthalate film to a dry thickness of 40 μm, and then dried at 110°C for 5 minutes to prepare a laminate sheet (a) having a first pressure-sensitive adhesive layer on the release-treated surface of the polyethylene terephthalate film. A laminate sheet (b) having a second pressure-sensitive adhesive layer on the release-treated surface of the polyethylene terephthalate film was prepared in a similar manner.

[0097] A 25 μm thick polyethylene terephthalate (PET) film was prepared as a substrate. The obtained laminate sheet (a) was laminated on one side of the substrate with the first pressure-sensitive adhesive layer facing the substrate, and the first pressure-sensitive adhesive layer was transferred to the substrate and laminated together. Furthermore, the laminate sheet (b) was laminated on the other side of the substrate with the second pressure-sensitive adhesive layer facing the substrate, and the second pressure-sensitive adhesive layer was transferred to the substrate and laminated together, thereby obtaining a double-sided pressure-sensitive adhesive tape having a first pressure-sensitive adhesive layer (first side of the pressure-sensitive adhesive tape) on one side of the substrate and a second pressure-sensitive adhesive layer (second side of the pressure-sensitive adhesive tape) on the other side.

[0098] (Examples 2 and 4) Double-sided adhesive tapes were produced in the same manner as in Examples 1, 3, 5 to 17, and 19 and Comparative Examples 1 to 6, except that a 60 μm thick biaxially stretchable polypropylene (OPP) film (manufactured by Futamura Chemical Co., Ltd., "FOSAQBT #60") was prepared as the substrate.

[0099] (Example 18) Double-sided pressure-sensitive adhesive tapes were produced in the same manner as in Examples 1, 3, 5 to 17, and 19 and Comparative Examples 1 to 6, except that a 750 μm thick polyurethane foam (PU foam, manufactured by NHK Spring Co., Ltd., "EXT") was prepared as the substrate.

[0100] <Evaluation> The double-sided pressure-sensitive adhesive tapes obtained in the Examples and Comparative Examples were evaluated as follows. The results are shown in Tables 4 to 6.

[0101] (1) 180° Peel Force of the First Surface of the Pressure-Sensitive Adhesive Tape from SUS After the obtained double-sided pressure-sensitive adhesive tape was cut into a flat rectangular shape measuring 25 mm wide x 75 mm long, the release-treated polyethylene terephthalate film on the second surface of the pressure-sensitive adhesive tape was peeled off, and the tape was attached to a 23 μm-thick polyethylene terephthalate film for backing. Further, in an environment of 23°C, the release-treated polyethylene terephthalate film on the first surface of the pressure-sensitive adhesive tape was peeled off, and the tape was pressed against a SUS plate (surface roughness Ra: 0.23 μm) polished with #360 sandpaper using a 2 kg rubber roller, which was moved back and forth at a speed of 300 mm / min, and then allowed to stand for 20 minutes at 23°C and 50% RH to obtain a measurement sample. For the obtained measurement sample, a tensile tester (Shimadzu Corporation, "Universal Testing Machine Autograph AGS-X") was used in accordance with JIS Z0237 to perform a 180 ° peel test of the adhesive tape under conditions of 23 ° C., 50% RH, and a peel speed of 300 mm / min, and the 180 ° peel strength (N / 25 mm) of the first surface of the adhesive tape against SUS was measured. If the obtained 180 ° peel strength against SUS was 35.0 N / 25 mm or more, it was marked "○", if it was 25.0 N / 25 mm or more but less than 35.0 N / 25 mm, it was marked "△", and if it was less than 25.0 N / 25 mm, it was marked "x". The adhesion of the first surface of the adhesive tape to the rough surface was evaluated.

[0102] (2) Slurry Resistance of the First Surface of the Pressure-Sensitive Adhesive Tape (Preparation of Samples Before and After Immersion in Chemical Solution) A test sample before immersion in a chemical solution was prepared in the same manner as in "(1) 180° Peel Force of the First Surface of the Pressure-Sensitive Adhesive Tape from SUS" described above. Semi-Sperse 25 (manufactured by Cabot Microelectronics) was diluted 1:1 with ion-exchanged water to prepare an alkaline chemical solution. The obtained test sample before immersion in the chemical solution was immersed in the alkaline chemical solution for 7 days in an atmosphere at 60°C. Thereafter, the test sample was removed from the alkaline chemical solution, washed with ion-exchanged water, and then dried at 23°C for 1 hour to obtain a test sample after immersion in the chemical solution.

[0103] (Measurement of the rate of change in 180° peel strength) For each test sample before and after immersion in a chemical solution, a 180° peel test of the adhesive tape was performed using a tensile tester (Shimadzu Corporation, "Universal Testing Machine Autograph AGS-X") under conditions of 23°C, 50% RH, and a peel speed of 300 mm / min, and the 180° peel strength (N / 25 mm) of the first surface of the adhesive tape from SUS was measured. Using the obtained 180° peel strength from SUS, the ratio (%) of the 180° peel strength of the first surface of the adhesive tape after immersion in the chemical solution to the 180° peel strength of the first surface of the adhesive tape before immersion in the chemical solution was calculated according to the following formula: Rate of 180° peel strength (%) = {(180° peel strength of the adhesive tape from SUS after immersion in the chemical solution) / (180° peel strength of the adhesive tape from SUS before immersion in the chemical solution)} × 100

[0104] The slurry resistance of the first surface of the adhesive tape was evaluated by assigning "◎" when the obtained 180° peel force ratio was 105.0% or more, "◯" when it was 100.0% or more but less than 105.0%, "△" when it was 90.0% or more but less than 100.0%, and "×" when it was less than 90.0%.

[0105] (3) Shear strength of the first surface of the adhesive tape against SUS The obtained double-sided adhesive tape was cut into a flat square shape measuring 20 mm wide x 20 mm long, the release-treated polyethylene terephthalate film on the second surface of the adhesive tape was peeled off, and the tape was pressure-bonded to the surface of a stainless steel plate (a SUS304 plate that had been washed with ethanol and then wiped dry) by moving a 2 kg rubber roller back and forth once at a speed of 300 mm / min. Further, in an environment of 23°C, the release-treated polyethylene terephthalate film on the first surface of the adhesive tape was peeled off, and the tape was pressure-bonded to the surface of a stainless steel plate (a SUS304 plate that had been washed with ethanol and then wiped dry) by moving a 2 kg rubber roller back and forth once at a speed of 300 mm / min. The tape was then left to stand at 23°C and 50% RH for 24 hours to obtain a test sample. For the obtained test samples, a tensile tester (Shimadzu Corporation, "Universal Testing Machine Autograph AGS-X") was used to measure the shear strength (MPa) of the first surface of the adhesive tape against SUS in an atmosphere of 23 ° C. and 50% RH by peeling the first surface of the adhesive tape at a rate of 10 mm / min in the direction of the shear stress. The shear strength of the first surface of the adhesive tape against SUS was evaluated by assigning "◎" when the shear strength of the first surface of the obtained adhesive tape against SUS was 1.00 MPa or more, "○" when it was 0.80 MPa or more but less than 1.00 MPa, "△" when it was 0.50 MPa or more but less than 0.80 MPa, and "×" when it was less than 0.50 MPa.

[0106] (4) 180° Peel Force of the Second Surface of the Adhesive Tape from SUS In the above-mentioned "(1) 180° Peel Force of the First Surface of the Adhesive Tape from SUS," the first surface of the adhesive tape was attached to a 23 μm thick polyethylene terephthalate film as a backing, and the 180° peel force of the second surface of the adhesive tape from SUS was measured using a stainless steel plate (a SUS304 plate washed with ethanol and then wiped dry). The 180° peel force (N / 25 mm) of the second surface of the adhesive tape from SUS was measured in the same manner as in the above-mentioned "(1) 180° Peel Force of the First Surface of the Adhesive Tape from SUS." The adhesiveness of the second surface of the adhesive tape was evaluated by rating it as "Good" if the obtained 180° peel force from SUS was 10 N / 25 mm or more, and rating it as "Fair" if it was less than 10 N / 25 mm.

[0107] (5) Removability of the Second Surface of the Pressure-Sensitive Adhesive Tape A test sample before heat treatment was obtained in the same manner as in "(4) 180° Peel Force of the Second Surface of the Pressure-Sensitive Adhesive Tape from SUS" described above. The test sample before heat treatment was left to stand in an atmosphere at 60°C for 7 days to obtain a test sample after heat treatment. A 180° peel test of the pressure-sensitive adhesive tape was performed on each test sample before and after heat treatment using a tensile tester (Shimadzu Corporation, "Universal Testing Machine Autograph AGS-X") under conditions of 23°C, 50% RH, and a peel rate of 300 mm / min, and the 180° peel force (N / 25 mm) of the second surface of the pressure-sensitive adhesive tape from SUS was measured. Using the obtained 180° peel force from SUS, the ratio (%) of the 180° peel force of the second surface of the pressure-sensitive adhesive tape after heat treatment to the 180° peel force of the second surface of the pressure-sensitive adhesive tape before heat treatment was calculated using the following formula: Percentage of 180° peel strength (%)={(180° peel strength from SUS after heat treatment) / (180° peel strength from SUS before heat treatment)}×100

[0108] The removability of the second surface of the pressure-sensitive adhesive tape was evaluated by rating it as "◯" when the obtained 180° peel strength ratio was less than 120.0% and rating it as "Δ" when it was 120.0% or more.

[0109] (6) Slurry Resistance of Second Surface of Pressure-Sensitive Adhesive Tape The 180° peel strength (N / 25 mm) of the second surface of the pressure-sensitive adhesive tape after immersion in the chemical solution was measured in the same manner as in the above-mentioned "(2) Slurry Resistance of First Surface of Pressure-Sensitive Adhesive Tape", except that in the above-mentioned "(2) Slurry Resistance of First Surface of Pressure-Sensitive Adhesive Tape", the first surface of the pressure-sensitive adhesive tape was attached to a 23 μm-thick polyethylene terephthalate film as a backing, and the 180° peel strength of the second surface of the pressure-sensitive adhesive tape against SUS was measured.

[0110] The slurry resistance of the second surface of the adhesive tape was evaluated by rating it as follows: when the 180° peel strength against the obtained SUS was 30.0 N / 25 mm or more, it was marked "◎", when it was 5.0 N / 25 mm or more but less than 30.0 N / 25 mm, it was marked "◯", and when it was less than 5.0 N / 25 mm, it was marked "×". Note that even if the rating is "×", the double-sided adhesive tape for fixing a polishing pad of the present invention can be used without any problems depending on the application.

[0111]

[0112]

[0113]

[0114] According to the present invention, it is possible to provide a double-sided pressure-sensitive adhesive tape for fixing a polishing pad, which has excellent shear strength and slurry resistance at high temperatures, and also has excellent adhesion to rough surfaces.

Claims

1. A substrate, a first adhesive layer on one side of the substrate and a second adhesive layer on the other side, the first adhesive layer containing a base polymer, a tackifier resin (T1) that does not contain a hydroxyl group or has a hydroxyl value of less than 20 mg KOH / g, and a tackifier resin (T2) that has a hydroxyl value of 20 mg KOH / g or more and 120 mg KOH / g or less, the base polymer containing a block copolymer (A) of a monovinyl-substituted aromatic compound and a conjugated diene compound, the first adhesive layer containing the base polymer at a rate of 40.0% by mass or more and less than 53.0% by mass, the first adhesive layer containing the tackifier resin (T1) at a rate of 50 parts by mass or more and 100 parts by mass or less relative to 100 parts by mass of the base polymer, and containing the tackifier resin (T2) at a rate of 40 parts by mass or more and 80 parts by mass or less relative to 100 parts by mass of the base polymer.

1. A double-sided adhesive tape for fixing a polishing pad, comprising:

2. The double-sided adhesive tape for fixing a polishing pad according to claim 1, wherein the softening point of said tackifier resin (T1) is 80° C. or higher.

3. The double-sided adhesive tape for fixing a polishing pad according to claim 1 or 2, wherein the softening point of the tackifier resin (T2) is 80° C. or higher.

4. The double-sided adhesive tape for fixing a polishing pad according to claim 1, 2 or 3, wherein the tackifier resin (T2) contains a terpene phenol resin.

5. The double-sided adhesive tape for fixing a polishing pad according to claim 1, 2, 3 or 4, wherein the tackifier resin (T2) contains a coumarone resin.

6. A double-sided adhesive tape for fixing a polishing pad as described in claim 1, 2, 3, 4 or 5, wherein the first adhesive layer contains, as the block copolymer (A), a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 25% by mass or more and 80% by mass or less.

7. A double-sided adhesive tape for fixing a polishing pad as described in claim 6, wherein the first adhesive layer contains as the block copolymer (A) a block copolymer having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 50% by mass or more and 80% by mass or less.

8. A double-sided adhesive tape for fixing a polishing pad as described in claim 7, wherein the first adhesive layer contains as the block copolymer (A) only block copolymers having a styrene content of 10% by mass or more and 20% by mass or less and a diblock content of 50% by mass or more and 80% by mass or less.

9. The double-sided adhesive tape for fixing a polishing pad according to claim 1, 2, 3, 4, 5, 6, 7 or 8, wherein the second adhesive layer contains a base polymer, a tackifier resin (T3) that does not contain a hydroxyl group or has a hydroxyl value of less than 20 mg KOH / g, and a tackifier resin (T4) that has a hydroxyl value of 20 mg KOH / g or more and 120 mg KOH / g or less, the base polymer contains a block copolymer (B) of a monovinyl substituted aromatic compound and a conjugated diene compound, the second adhesive layer has a base polymer content of 50.0% by mass or more and 70.0% by mass or less, the second adhesive layer having a tackifier resin (T3) content of 5 parts by mass or more and 60 parts by mass or less per 100 parts by mass of the base polymer and a tackifier resin (T4) content of 1 part by mass or more and 50 parts by mass or less per 100 parts by mass of the base polymer.

10. A double-sided adhesive tape for fixing a polishing pad as described in claim 9, wherein the second adhesive layer contains as the block copolymer (B) a block copolymer having a styrene content of 10% by mass or more and 25% by mass or less and a diblock content of 25% by mass or more and 70% by mass or less.

11. A double-sided adhesive tape for fixing a polishing pad as described in claim 10, wherein the second adhesive layer contains as the block copolymer (B) only block copolymers having a styrene content of 10% by mass or more and 25% by mass or less and a diblock content of 25% by mass or more and 70% by mass or less.

12. The double-sided adhesive tape for fixing a polishing pad according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10 or 11, wherein the second adhesive layer contains a base polymer, and the base polymer contains a (meth)acrylic copolymer.

13. A double-sided adhesive tape for fixing a polishing pad according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11 or 12, wherein the first adhesive layer is a surface to be bonded to the polishing pad, and the second adhesive layer is a surface to be bonded to the platen of a polishing machine.

14. The double-sided adhesive tape for fixing a polishing pad according to claim 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12 or 13, wherein the substrate comprises a polyolefin film, a polyester film or a foam.

Citation Information

Patent Citations

  • Adhesive composition and adhesive sheet

    JP2015028130A

  • Pressure-sensitive adhesive sheet for fastening polishing pad

    JP2015078348A

  • Polishing pad fixing adhesive sheet

    JP2017105976A

  • Adhesive composition and adhesive sheet

    JP2020073703A

  • Adhesive for fixing abrasive member and adhesive sheet

    JP2021088614A