Thermally-expandable fire-resistant sheet

The development of a thermally expandable fireproof sheet with a low expansion start temperature and long length, using specific matrix components and adhesives, addresses the challenges of surface roughness and air bubbles, resulting in improved fire resistance and appearance, suitable for fire prevention applications.

WO2024225319A1PCT designated stage expired Publication Date: 2024-10-31SEKISUI CHEMICAL CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016080
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-09-22
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing thermally expandable fireproof sheets with low expansion start temperatures and long lengths face challenges in maintaining a good appearance due to surface roughness and air bubble formation, making it difficult to produce long, high-quality sheets.

Method used

A thermally expandable fireproof sheet containing a matrix component and thermally expandable graphite with an expansion start temperature of 160°C or lower, combined with other inorganic substances and fillers, is developed, allowing for a rolled body with a length of 1 m or more and minimal thickness variation, using specific resin types and adhesives to reduce kneading load and prevent graphite deterioration.

Benefits of technology

The solution enables the production of long, high-quality thermally expandable fireproof sheets with improved fire resistance, reduced gas generation, and excellent appearance, effectively expanding to close gaps in fire prevention equipment during fires.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

A thermally-expandable fire-resistant sheet according to the present invention contains a matrix component and thermally-expandable graphite, has an expansion starting temperature of 160°C or less, an average thickness of 0.5 mm or more, a thickness variation of 10% or less of the average thickness, and is a rolled body having a length of 1 m or more. The present invention makes it possible to provide a thermally-expandable fire-resistant sheet that is long and contains thermally-expandable graphite having a low expansion starting temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Thermally expandable fireproof sheet

[0001] The present invention relates to a thermally expandable fire-resistant sheet.

[0002] In the construction industry, fire-resistant materials are used in fire prevention equipment such as doors and windows. Examples of fire-resistant materials include fire-resistant sheets containing resins blended with inorganic fillers and thermally expandable graphite (see, for example, Patent Document 1). Such fire-resistant sheets expand when heated, and combustion residues form a fire-resistant insulating layer, thereby achieving fire-resistant and insulating performance. Specifically, fire-resistant sheets are installed in gaps between doors and windows and the surrounding frames, such as door frames and window frames. In the event of a fire, the sheets expand in their thickness direction to close the gap and prevent the fire from spreading.

[0003] Japanese Patent Application Laid-Open No. 2017-141463

[0004] In order to rapidly expand in the event of a fire and block the flow path of flammable gas, thermally expandable graphite that begins to expand at low temperatures is often used for fire-resistant sheets. However, when such thermally expandable graphite that expands at low temperatures is used, there is a problem that the surface of the sheet becomes rough during molding, air bubbles are generated, and it is difficult to obtain a long (long) sheet with good appearance. Therefore, an object of the present invention is to provide a thermally expandable fire-resistant sheet that has a low expansion start temperature and is long and has good appearance.

[0005] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by a thermally expandable fire-resistant sheet that contains a matrix component and thermally expandable graphite, has an expansion initiation temperature of 160°C or less, and is in the form of a roll having a length of 1 m or more, and have completed the present invention. That is, the present invention provides the following [1] to [8].

[0006] [1] A thermally expandable fire-resistant sheet containing a matrix component and thermally expandable graphite, having an expansion initiation temperature of 160°C or less, an average thickness of 0.5 mm or more, a thickness variation of 10% or less of the average thickness, and a length of 1 m or more in the form of a roll. [2] The thermally expandable fire-resistant sheet according to [1] above, further containing at least one selected from the group consisting of thermally expandable inorganic substances other than thermally expandable graphite and inorganic fillers. [3] The thermally expandable fire-resistant sheet according to [2] above, having a content of thermally expandable graphite of 3 to 300 parts by mass and a content of inorganic filler of 2 to 200 parts by mass per 100 parts by mass of the matrix component. [4] The thermally expandable fire-resistant sheet according to any one of [1] to [3] above, having an expansion ratio of 5 times or more when heated at 200°C for 30 minutes. [5] The heat-expandable fire-resistant sheet according to any one of [1] to [4] above, which has an elution rate of 3% or less after immersion in pure water at 60°C for one week. [6] The heat-expandable fire-resistant sheet according to any one of [1] to [5] above, wherein the matrix component does not contain a phosphorus component. [7] The heat-expandable fire-resistant sheet according to any one of [1] to [6] above, which has a substrate or an adhesive layer on at least one surface. [8] Fire protection equipment, at least a part of which is equipped with a heat-expandable fire-resistant sheet cut from the roll according to any one of [1] to [7] above.

[0007] According to the present invention, it is possible to provide a heat-expandable fire-resistant sheet that has a low expansion initiation temperature, a good appearance, and is long.

[0008] The present invention will be described in detail below. [Thermal-expandable fire-resistant sheet] The thermal-expandable fire-resistant sheet of the present invention contains a matrix component and thermally expandable graphite, has an expansion initiation temperature of 160°C or less, and is a rolled body having an average thickness of 0.5 mm or more, a thickness variation of 10% or less of the average thickness, and a length of 1 m or more. The thermal-expandable fire-resistant sheet of the present invention will be described in detail below.

[0009] <Matrix Component> The thermally expandable fire-resistant resin sheet of the present invention contains a matrix component. Thermally expandable graphite, which will be described later, and thermally expandable inorganic materials other than thermally expandable graphite and inorganic fillers, which are blended as needed, are dispersed in the matrix component. The matrix component is not particularly limited, and thermoplastic resins, thermosetting resins, rubbers, etc. can be used. The matrix component may be formed from one type of component or multiple components.

[0010] Examples of thermoplastic resins include polyvinyl chloride resin, polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer resin, vinyl acetate resin, vinyl acetate copolymer resin, fluororesin, phenol resin, polycarbonate resin, acrylic resin, polystyrene resin, and polyacrylonitrile resin.

[0011] Examples of thermosetting resins include polyurethane resins, phenolic resins, epoxy resins, urea resins, melamine resins, unsaturated polyester resins, and polyimides.

[0012] Examples of rubber include natural rubber, isoprene rubber, butadiene rubber, 1,2-polybutadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, chlorinated butyl rubber, ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), styrene-based thermoplastic elastomer, chlorosulfonated polyethylene, acrylic rubber, epichlorohydrin rubber, silicone rubber, fluororubber, and urethane rubber.

[0013] In the present invention, the matrix component is preferably an extrusion molding resin, a dry-to-solidify adhesive, a moisture-curing reaction adhesive, a hot-melt adhesive, or a thermosetting reaction adhesive. When the matrix component is one of these specific resin components, the appearance is good and it is easy to obtain a long thermally expandable fire-resistant sheet of 1 m or more in length.

[0014] (Extrusion Resin) The extrusion resin is a resin that can be used to obtain a thermally expandable fire-resistant sheet by extrusion molding. By using the extrusion resin as a matrix component in a thermally expandable composition for obtaining a thermally expandable fire-resistant sheet, the thermally expandable composition can be extruded to obtain a thermally expandable fire-resistant sheet. By appropriately controlling the viscosity of the thermally expandable composition during extrusion molding, the load during kneading can be reduced and deterioration of the thermally expandable graphite can be suppressed. Therefore, gas generation due to deterioration of the thermally expandable graphite can be suppressed, and a thermally expandable fire-resistant sheet with good appearance can be obtained. Examples of the extrusion resin include thermoplastic resins and rubber. Thermoplastic resins and rubbers are as described above. Rubber is preferred as the extrusion resin, and among these, one or more selected from the group consisting of chloroprene rubber, styrene-butadiene rubber, and styrene-based thermoplastic elastomers are preferred.

[0015] Examples of the styrene-based thermoplastic elastomer include styrene-butadiene-styrene (SBS), polystyrene-poly(ethylene-propylene) (SEP), polystyrene-poly(ethylene-butylene)-polystyrene (SEBS), polystyrene-poly(ethylene-propylene)-polystyrene (SEPS), polystyrene-poly(ethylene-ethylene / propylene)-polystyrene (SEEPS), styrene-isoprene-styrene (SIS), etc. Among these, SBS or SEP is preferred.

[0016] (Dry-Solidifying Adhesive) Examples of dry-solidifying adhesives include solvent-based adhesives, emulsion-based adhesives, and synthetic rubber latex-based adhesives. When using these adhesives, the thermally expandable composition for obtaining the thermally expandable fire-resistant sheet is in a liquid state, which reduces the load during kneading and suppresses deterioration of the thermally expandable graphite. As a result, gas generation due to deterioration of the thermally expandable graphite is suppressed, and a long thermally expandable fire-resistant sheet with good appearance can be obtained.

[0017] Solvent-based adhesives exist as solids in the thermally expandable fire-resistant sheet, but are dissolved in an organic solvent in the thermally expandable composition used to obtain the thermally expandable fire-resistant sheet. Therefore, when using such a solvent-based adhesive, the thermally expandable composition contains an organic solvent. Furthermore, solidification is possible by volatilizing the organic solvent. Examples of solvent-based adhesives include vinyl acetate resins, vinyl acetate copolymer resins, rubbers, acrylic resins, polyesters, and silicone resins. The silicone resin adhesive is preferably an unmodified silicone resin adhesive. In this specification, examples of vinyl acetate copolymer resins include copolymers of vinyl acetate and monomers copolymerizable with vinyl acetate (e.g., α-olefins, (meth)acrylic acid esters, etc.), such as vinyl acetate-(meth)acrylic acid ester copolymers. The term (meth)acrylic acid encompasses both acrylic acid and methacrylic acid. Examples of the rubber-based adhesive include chloroprene, butadiene, styrene-butadiene, butadiene-acrylonitrile, isobutylene-isoprene, and ethylene-propylene, with chloroprene being preferred.Of the solvent-based adhesives, chloroprene, acrylic resins, and silicone resins (unmodified) are preferred.

[0018] The emulsion-type adhesive exists as a solid in the thermally expandable fire-resistant sheet, but is dispersed in a dispersant, preferably water, in the thermally expandable composition used to obtain the thermally expandable fire-resistant sheet. When an emulsion-type adhesive is used, the thermally expandable composition contains a dispersant such as water. Examples of emulsion-type adhesives include vinyl acetate resin-based, vinyl acetate copolymer resin-based, acrylic resin-based, aqueous polymer-isocyanate-based, and polyurethane-based adhesives, with vinyl acetate copolymer resin-based and polyurethane-based adhesives being preferred.

[0019] The synthetic rubber latex adhesive exists as a solid in the heat-expandable fire-resistant sheet, but is dispersed in a dispersant, preferably water, in the heat-expandable composition for obtaining the heat-expandable fire-resistant sheet. When a synthetic rubber latex adhesive is used, the heat-expandable composition contains a dispersant such as water. Examples of synthetic rubber latex adhesives include chloroprene, butadiene, styrene-butadiene, butadiene-acrylonitrile, isobutylene-isoprene, and ethylene-propylene, with chloroprene being preferred.

[0020] When a dry-to-solidify adhesive is used, the thermally expandable composition contains water or an organic solvent. When a solvent-based pressure-sensitive adhesive is used, the solid content of the thermally expandable composition is, for example, 10 to 90 mass %, and preferably 30 to 70 mass %.

[0021] (Moisture-Curing Adhesive) A moisture-curing adhesive is an adhesive that cures with moisture in the air. A thermally expandable composition containing a moisture-curing adhesive can be cured with moisture and can be kneaded at low temperatures, which particularly reduces the load during kneading and effectively suppresses deterioration of the thermally expandable graphite. As a result, gas generation due to deterioration of the thermally expandable graphite is suppressed, and a long thermally expandable fire-resistant sheet with an extremely good appearance can be obtained.

[0022] Examples of moisture-curing reaction adhesives include cyanoacrylate-based, modified silicone resin-based, and silylated urethane-based adhesives, with modified silicone resin-based and silylated urethane-based adhesives being preferred, and modified silicone resin-based adhesives being more preferred.

[0023] (Modified silicone resin system) Examples of the modified silicone resin moisture-curing reaction adhesive include polymers having crosslinkable silyl groups (crosslinkable silyl group-containing polymers). As the crosslinkable silyl group-containing polymer, at least one selected from crosslinkable silyl group-containing polyoxyalkylene polymers, crosslinkable silyl group-containing acrylic polymers, and crosslinkable silyl group-containing acrylic-modified polyoxyalkylene polymers is preferred. Note that the modified silicone resin moisture-curing reaction adhesive is a compound that does not have a urethane bond or a urea bond in the main chain, unlike the silylated urethane system described below.

[0024] The crosslinkable silyl group-containing polyoxyalkylene polymer is preferably a polymer containing a crosslinkable silyl group in the molecule and having a polyoxyalkylene in the main chain, more preferably a polymer having a polyoxyalkylene in the main chain and a crosslinkable silyl group at the main chain terminal. The polyoxyalkylene is preferably polyoxypropylene.

[0025] The crosslinkable silyl group-containing acrylic-modified polyoxyalkylene polymer is preferably a polymer containing a crosslinkable silyl group in the molecule and having a (meth)acrylic-modified polyoxyalkylene in the main chain, more preferably a polymer having a (meth)acrylic-modified polyoxyalkylene in the main chain and having a crosslinkable silyl group at the main chain terminal. The (meth)acrylic-modified polyoxyalkylene is preferably a (meth)acrylic-modified polyoxypropylene.

[0026] The crosslinkable silyl group-containing acrylic polymer may be a polymer having an acrylic polymer in the main chain skeleton and having one or more crosslinkable silyl groups in the molecule. Here, the acrylic polymer may be a conventionally known one, and is not particularly limited as long as it is an acrylic polymer obtained by polymerizing or copolymerizing one or more acrylic monomers selected from (meth)acrylic acid, (meth)acrylic acid ester, (meth)acrylonitrile, (meth)acrylamide, etc.

[0027] Examples of crosslinkable silyl groups include groups in which one or more reactive groups are bonded to a silicon atom.The reactive groups are selected from halogen atoms, hydrogen atoms, hydroxyl groups, alkoxy groups, acyloxy groups, ketoximate groups, amide groups, acid amide groups, mercapto groups, ketoxime groups, alkenyloxy groups, and aminooxy groups, and when there are multiple reactive groups, the reactive groups may be the same or different groups.Among these, the reactive group is preferably an alkoxy group, and more preferably a methoxy group.That is, the crosslinkable silyl group is preferably an alkoxysilyl group.Examples of alkoxysilyl groups include trialkoxysilyl groups such as trimethoxysilyl groups, triethoxysilyl groups, triisopropoxysilyl groups, and triphenoxysilyl groups, dialkoxysilyl groups such as dimethoxymethylsilyl groups and diethoxymethylsilyl groups, and monoalkoxysilyl groups such as methoxydimethylsilyl groups and ethoxydimethylsilyl groups. Among these, a trialkoxysilyl group or a dialkoxysilyl group is preferred, and a trimethoxysilyl group or a dimethoxymethylsilyl group is more preferred.

[0028] (Silylated urethane-based) A silylated urethane-based moisture-curing reaction adhesive is a polymer having at least one of a urethane bond and a urea bond in the main chain and having a crosslinkable silyl group. The crosslinkable silyl group is preferably present at the end of the main chain. The crosslinkable silyl group is the same as that described for the modified silicone resin-based moisture-curing reaction adhesive described above. Furthermore, the main chain of the silylated urethane-based moisture-curing reaction adhesive preferably has a polyoxyalkylene in the skeleton and at least one of a urethane bond and a urea bond. The polyoxyalkylene is preferably polyoxypropylene.

[0029] (Curing Catalyst) The moisture-curing reaction adhesive is preferably cured using a curing catalyst. Examples of the curing catalyst include dibutyltin dilaurate, dibutyltin oxide, dibutyltin diacetate, dibutyltin phthalate, bis(dibutyltin laurate) oxide, dibutyltin bis(acetylacetonate), dibutyltin bis(monoester maleate), tin octoate, dibutyltin octoate, dioctyltin oxide, dibutyltin bis(triethoxysilicate), bis(dibutyltin bistriethoxysilicate) oxide, dibutyltin oxybisethoxysilicate, and organic tin compounds such as 1,1,3,3-tetrabutyl-1,3-dilauryloxycarbonyl-distannoxane, and organic titanium compounds such as tetra-n-butoxytitanate and tetraisopropoxytitanate. These curing catalysts may be used alone or in combination of two or more. The content of the curing catalyst is preferably 1 to 10 parts by mass, more preferably 1 to 5 parts by mass, per 100 parts by mass of the matrix component.

[0030] (Hot-melt adhesive) A hot-melt adhesive is an adhesive that has no fluidity at room temperature but becomes fluid when heated, and is sometimes called a hot-melt adhesive. Furthermore, a heated hot-melt adhesive solidifies when cooled again. When a hot-melt adhesive is used in a thermally expandable composition for obtaining a thermally expandable fire-resistant sheet, the viscosity of the composition can be reduced by heating, reducing the load during kneading and suppressing the deterioration of the thermally expandable graphite. Therefore, gas generation due to the deterioration of the thermally expandable graphite is suppressed, and a long thermally expandable fire-resistant sheet with a good appearance can be obtained.

[0031] Examples of hot-melt adhesives include vinyl acetate resins, vinyl acetate copolymer resins, ethylene-vinyl acetate copolymer resins, rubbers, acrylic resins, polyurethanes, polystyrenes, polyolefins, polyesters, and polyamides. Examples of rubbers include chloroprene, butadiene, styrene-butadiene, butadiene-acrylonitrile, isobutylene-isoprene, and ethylene-propylene. Furthermore, the polystyrene-based adhesive is a polymer containing a styrene-based monomer, and may be a copolymer of a styrene-based monomer and an aliphatic monomer. Among these, ethylene-vinyl acetate copolymer resins or polystyrene-based adhesives are preferred. When using hot-melt adhesives, a tackifying resin may be used in combination. Examples of tackifying resins include rosin-based, terpene-based, petroleum resin-based, and coumarone resin-based.

[0032] (Thermosetting reaction type adhesive) The thermosetting reaction type adhesive is an adhesive that cures at any temperature. A thermally expandable composition containing a thermosetting reaction type adhesive can be cured by heat at a temperature lower than the expansion initiation temperature of the thermally expandable graphite, and since it can be kneaded at a low temperature, the load during kneading is particularly easy to reduce, and deterioration of the thermally expandable graphite can be effectively suppressed. Therefore, gas generation due to deterioration of the thermally expandable graphite is suppressed, and a long thermally expandable fire-resistant sheet with an extremely good appearance can be obtained.

[0033] Examples of thermosetting reaction adhesives include epoxy resin-based, polyurethane resin-based, silicone resin-based, acrylic resin-based, and polyester resin-based adhesives. Among these, epoxy resin-based adhesives are preferred. When using a thermosetting reaction adhesive, a curing agent or a catalyst may be used in combination with the epoxy resin. Examples of curing agents include amine-based, acid anhydride-based, phenolic resin-based, and amide-based curing agents. Examples of catalysts include amine salt-based, imidazole-based, and phosphine phosphonium salt-based. More preferably, by using a curing agent and a catalyst in combination, the temperature required for the thermosetting reaction can be reduced, and a long thermally expandable fire-resistant sheet with a good appearance can be obtained.

[0034] In the present invention, the content of the matrix component is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, based on the total amount of the thermally expandable fire-resistant sheet.

[0035] <Thermal Expandable Graphite> The thermal expandable fire-resistant sheet of the present invention contains thermal expandable graphite. Thermal expandable graphite is a conventionally known substance that expands when heated. When heated, it expands to form large-volume voids, thereby suppressing the spread of fire and extinguishing the fire if the fire-resistant sheet catches fire. Thermal expandable graphite is produced by treating powder of natural flaky graphite, pyrolytic graphite, kish graphite, or the like with an inorganic acid and a strong oxidizing agent to produce a graphite intercalation compound. This is a type of crystalline compound that maintains the layered structure of carbon. Examples of inorganic acids include concentrated sulfuric acid, nitric acid, and selenic acid. Examples of strong oxidizing agents include concentrated nitric acid, persulfates, perchloric acid, perchlorates, permanganates, dichromates, dichromates, and hydrogen peroxide. The thermal expandable graphite obtained by the acid treatment described above may be further neutralized with ammonia, aliphatic lower amines, alkali metal compounds, alkaline earth metal compounds, or the like.

[0036] The particle size of the thermally expandable graphite is preferably 20 to 200 mesh. When the particle size of the thermally expandable graphite is within this range, it expands to easily create large-volume voids, thereby improving fire resistance. It also improves dispersibility in resins. The average aspect ratio of the thermally expandable graphite is preferably 2 or more, more preferably 5 or more, and even more preferably 10 or more. There is no particular upper limit to the average aspect ratio of the thermally expandable graphite, but from the viewpoint of preventing cracking of the thermally expandable graphite, it is preferably 1,000 or less. When the average aspect ratio of the thermally expandable graphite is 2 or more, it expands to easily create large-volume voids, thereby improving flame retardancy. The average aspect ratio of the thermally expandable graphite is determined by measuring the maximum dimension (major axis) and minimum dimension (minor axis) of each of 10 pieces of thermally expandable graphite, and then averaging the values ​​obtained by dividing the maximum dimension (major axis) by the minimum dimension (minor axis). The major axis and minor axis of the thermally expandable graphite can be measured using, for example, a field emission scanning electron microscope (FE-SEM).

[0037] The expansion start temperature of the thermally expandable graphite is 160°C or lower. When the expansion start temperature of the thermally expandable graphite is 160°C or lower, the expansion start temperature of the thermally expandable fire-resistant sheet can also be easily adjusted to a low temperature, and the thermally expandable graphite expands at the beginning of a fire to form a fire-resistant heat insulating layer, making it easier to maintain good fire resistance for a long period of time. The expansion start temperature of the thermally expandable graphite is preferably 100 to 160°C, more preferably 120 to 150°C. The expansion start temperature of the thermally expandable graphite is measured by the method described in the examples.

[0038] The expansion start temperature of the thermally expandable graphite is preferably lower than the decomposition start temperature of the matrix component. This improves the expandability of the thermally expandable fire-resistant sheet and increases the mechanical strength of the formed fire-resistant heat insulating layer, thereby improving fire resistance. The expansion start temperature of the thermally expandable graphite is preferably at least 5°C lower than the decomposition start temperature of the matrix component, and more preferably at least 10°C lower. Here, the decomposition start temperature means the temperature at which the matrix component decomposes and weight loss begins, and is measured using a thermogravimetric analyzer in a dry air atmosphere at a heating rate of 10°C / min.

[0039] The content of thermally expandable graphite is preferably 3 to 300 parts by mass, more preferably 10 to 200 parts by mass, even more preferably 30 to 100 parts by mass, and even more preferably 30 to 90 parts by mass, per 100 parts by mass of the matrix component. When the content of thermally expandable graphite is equal to or greater than these lower limits, the thermally expandable fire-resistant sheet can be imparted with appropriate fire resistance. Furthermore, when the content of thermally expandable graphite is equal to or less than these upper limits, the amount of gas generated during the production process of the thermally expandable fire-resistant sheet is reduced, making it easier to obtain long products with good appearance.

[0040] <Thermal-Expandable Inorganic Substance Other than Thermally Expandable Graphite> The thermally expandable fire-resistant sheet of the present invention may contain a thermally expandable inorganic substance other than thermally expandable graphite. The thermally expandable inorganic substance expands when heated, and is not particularly limited, and examples thereof include vermiculite, kaolin, mica, metal phosphite, and shirasu balloon. When a thermally expandable inorganic substance is used, the content thereof is preferably 2 to 200 parts by mass, more preferably 10 to 150 parts by mass, and even more preferably 30 to 100 parts by mass relative to 100 parts by mass of the matrix component, from the viewpoint of improving fire resistance.

[0041] <Inorganic Filler> The thermally expandable fire-resistant sheet of the present invention may contain an inorganic filler. The inorganic filler is an inorganic filler other than thermally expandable graphite and thermally expandable inorganic materials. The inorganic filler expands when heated, and when the fireproof heat insulating layer is formed, it increases the heat capacity and suppresses heat transfer, while acting as an aggregate to improve the strength of the expansion residue. The inorganic filler that can be used in the present invention is not particularly limited, and examples thereof include metal oxides such as alumina, zinc oxide, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, antimony oxide, and ferrite; metal carbonates such as calcium carbonate, zinc carbonate, strontium carbonate, and barium carbonate; metal hydroxides such as calcium hydroxide, magnesium hydroxide, aluminum hydroxide, and hydrotalcite; calcium sulfate, gypsum fiber, calcium salts such as calcium silicate; silica, diatomaceous earth, dawsonite, barium sulfate, talc, clay, montmorillonite, bentonite, activated clay, sepiolite, imogolite, sericite, glass fiber, glass beads, aluminum nitride, boron nitride, silicon nitride, carbon black, graphite, carbon fiber, carbon balloons, various metal powders, potassium titanate, magnesium sulfate, lead zirconate titanate, aluminum borate, molybdenum sulfide, silicon carbide, stainless steel fiber, and zinc borate. The inorganic fillers may be used alone or in combination of two or more. Among these, calcium carbonate, iron oxide, and aluminum hydroxide are preferred from the viewpoint of improving the fire resistance of the thermally expandable fire-resistant sheet, and a combination of calcium carbonate and iron oxide or a combination of calcium carbonate and aluminum hydroxide is preferred. The inorganic fillers may be used alone or in combination of two or more. From the viewpoint of improving fire resistance, the content of the inorganic filler is preferably 2 to 200 parts by mass, more preferably 10 to 150 parts by mass, and even more preferably 30 to 100 parts by mass, per 100 parts by mass of the matrix component.

[0042] <Plasticizer> The thermally expandable fire-resistant sheet of the present invention may contain a plasticizer from the viewpoint of improving moldability. Examples of plasticizers include phthalate ester plasticizers such as di-2-ethylhexyl phthalate (DOP), dibutyl phthalate (DBP), diheptyl phthalate (DHP), and diisodecyl phthalate (DIDP); fatty acid ester plasticizers such as di-2-ethylhexyl adipate (DOA), diisobutyl adipate (DIBA), and dibutyl adipate (DBA); epoxidized ester plasticizers such as epoxidized soybean oil; adipate ester plasticizers such as adipate esters and adipic acid polyesters; trimellitate ester plasticizers such as tri-2-ethylhexyl trimellitate (TOTM) and triisononyl trimellitate (TINTM); and process oils such as mineral oil. These plasticizers may be used alone or in combination of two or more. When the heat-expandable fire-resistant sheet contains a plasticizer, the content of the plasticizer is preferably 1 to 60 parts by mass, more preferably 5 to 50 parts by mass, per 100 parts by mass of the matrix component.

[0043] (Other Components) The thermally expandable fire-resistant sheet of the present invention may contain additional components other than those described above, as needed, as long as the object of the present invention is not impaired. The type of these additional components is not particularly limited, and various additives can be used. Examples of such additives include lubricants, anti-shrinkage agents, crystal nucleating agents, colorants (pigments, dyes, etc.), UV absorbers, antioxidants, antiaging agents, flame retardants, flame retardant assistants, antistatic agents, surfactants, vulcanizing agents, dispersants, and surface treatment agents. The amount of additive added can be appropriately selected within a range that does not impair moldability, etc., and the additives may be used alone or in combination of two or more.

[0044] <Long Product> The heat-expandable fire-resistant sheet of the present invention is a rolled product having a length of 1 m or more. The length is the length in the longitudinal direction (MD) of the heat-expandable fire-resistant sheet. The heat-expandable fire-resistant sheet of the present invention contains heat-expandable graphite with a low expansion initiation temperature, but can be made into a long product having a length of 1 m or more and a good appearance. Furthermore, a length of 1 m or more is preferable because it improves productivity and broadens the range of applications. The length of the heat-expandable fire-resistant sheet is preferably 5 m or more, more preferably 20 m or more, even more preferably 50 m or more, and even more preferably 100 m or more. Furthermore, the length of the heat-expandable fire-resistant sheet is usually 500 m or less. In this specification, the MD direction is an abbreviation for machine direction, which corresponds to the flow direction of the composition during application, etc., as described below, and is the longitudinal direction of the sheet. The TD direction is an abbreviation for transverse direction, which is the direction perpendicular to the MD direction.

[0045] Furthermore, the thermally expandable fire-resistant sheet of the present invention can reduce thickness variations even when the length is 1 m or more, and can obtain long products with high dimensional accuracy. In the present invention, it is presumed that by reducing the kneading load when kneading the composition, deterioration of the thermally expandable graphite can be suppressed, thereby suppressing gas generation and reducing thickness variations.

[0046] The wound body in the present invention is a heat-expandable fire-resistant sheet having a length of 1 m or more wound into a roll, for example, a heat-expandable fire-resistant sheet having a length of 1 m or more wound around a cylindrical winding core. The winding core may be omitted.

[0047] The heat-expandable fire-resistant sheet of the present invention has an average thickness of 0.5 mm or more and a thickness variation of 10% or less of the average thickness. A heat-expandable fire-resistant sheet with such low thickness variation and high dimensional accuracy facilitates efficient production of long rolled sheets and also provides a good appearance. The average thickness refers to the average value obtained when measuring the thickness at 10 equally spaced points along the length of the heat-expandable fire-resistant sheet. The average thickness is preferably 0.8 mm or more, more preferably 1 mm or more, and preferably 5 mm or less. The thickness is measured at the center of the sheet width. Furthermore, the thickness variation refers to the average of the absolute values ​​A of the differences between the thickness measured at each point and the average thickness measured at 10 equally spaced points along the length of the heat-expandable fire-resistant sheet, as described above. The thickness variation is preferably 0.1 mm or less, more preferably 0.08 mm or less, and even more preferably 0.05 mm or less. From the viewpoint of improving the appearance of the sheet, the thickness variation of the heat-expandable fire-resistant sheet is 10% or less, preferably 5% or less, of the average thickness. The width of the heat-expandable fire-resistant sheet is not particularly limited, but is, for example, 0.005 to 2.0 m.

[0048] The heat-expandable fire-resistant sheet of the present invention preferably has a heat shrinkage rate of 1% or less in both the MD and TD directions, even when the sheet is 1 m or longer, and more preferably 0.5% or less. Such a low heat shrinkage rate suppresses peeling and dimensional inadequacies due to shrinkage, even when heat is applied during the manufacturing process of a rolled sheet. The heat shrinkage rate is calculated by cutting a 100 mm square evaluation sample, heat-treating it at 60°C for 6 hours, and then calculating the heat shrinkage rate from the length before and after heat treatment using the following formula: Heat shrinkage rate (%) = 100 × (length before heat treatment - length after heat treatment) / length before heat treatment. The heat shrinkage rates in the MD and TD directions can be calculated using the above formula from the lengths before and after heat treatment in the MD and TD directions, respectively. Ten or more 100 mm square evaluation samples are prepared at equal intervals along the length of the sheet, and the heat shrinkage rates calculated from the individual evaluation samples are averaged to determine the heat shrinkage rates in the MD and TD directions. The thermal shrinkage rate can be adjusted by adjusting the contents of the various components constituting the heat-expandable fire-resistant sheet.

[0049] <Expansion Start Temperature, Expansion Ratio> The heat-expandable fire-resistant sheet of the present invention has an expansion start temperature of 160°C or less. Having an expansion start temperature of 160°C or less allows it to expand in the early stages of a fire when temperatures are relatively low, forming a fire-resistant heat insulating layer, making it easier to maintain good fire resistance for a long period of time. The expansion start temperature of the heat-expandable fire-resistant sheet is preferably 155°C or less, more preferably 150°C or less, and preferably 120°C or more. The expansion start temperature of the heat-expandable fire-resistant sheet is measured by the method described in the examples.

[0050] Furthermore, the heat-expandable fire-resistant sheet of the present invention preferably has an expansion ratio of 5 times or more when heated at 200°C for 30 minutes. An expansion ratio of 5 times or more makes it easier to close gaps in fire prevention equipment in the event of a fire, improving fire resistance. The expansion ratio when heated at 200°C for 30 minutes is preferably 6 times or more, more preferably 8 times or more. There is no particular upper limit to the expansion ratio, but it is, for example, 50 times. The expansion ratio of the heat-expandable fire-resistant sheet is measured by the method described in the examples.

[0051] <Elution Rate> The heat-expandable fire-resistant sheet of the present invention preferably has an elution rate of 3% or less after immersion in pure water at 60°C for one week. An elution rate of 3% or less can suppress elution of the components constituting the heat-expandable fire-resistant sheet, preventing a decrease in fire resistance, even when the heat-expandable fire-resistant sheet is placed in a high-humidity environment or in contact with water. Furthermore, when the heat-expandable fire-resistant sheet is installed in a fire-prevention equipment, contamination of the fire-prevention equipment and poor appearance can be prevented. The elution rate of the heat-expandable fire-resistant sheet is preferably 2% or less, more preferably 1% or less. The lower the elution rate, the better, with the lower limit being 0%. The elution rate can be adjusted by appropriately selecting each component to be incorporated into the heat-expandable fire-resistant sheet. Specifically, compounds with low solubility in water can be used for the matrix component, heat-expandable graphite, optional inorganic filler, and other additives. The elution rate is measured by the method described in the examples.

[0052] <Phosphorus Component> The matrix component contained in the thermally expandable fire-resistant sheet of the present invention preferably does not contain a phosphorus component. By using a matrix component that does not contain a phosphorus component, the phosphorus content of the thermally expandable fire-resistant sheet can be reduced. Furthermore, it is also preferable that components other than the matrix component contained in the thermally expandable fire-resistant sheet also do not contain a phosphorus component. That is, the thermally expandable fire-resistant sheet preferably does not contain a phosphorus component. The matrix component and the thermally expandable fire-resistant sheet may contain an unavoidable amount of phosphorus as an impurity. That is, in this specification, "not containing a phosphorus component" means that the phosphorus content is 0.1% by mass or less, preferably 0.01% by mass or less. The absence of a phosphorus component improves water resistance, thereby ensuring excellent expansion ratio, residual hardness, and shape retention after expansion even after long-term exposure to water. Here, the phosphorus component refers to a compound containing a phosphorus atom. It is preferable that compounds containing a phosphorus atom are not used as the matrix component, thermally expandable graphite, and the inorganic filler and other additives that are optionally blended.

[0053] <Method for producing thermally expandable fire-resistant sheet> The thermally expandable fire-resistant sheet of the present invention comprises a thermally expandable composition containing a matrix component and thermally expandable graphite, and is obtained by molding the thermally expandable composition by a method such as extrusion or coating, which will be described later. In addition to the matrix component and thermally expandable graphite, the thermally expandable composition may also contain a thermally expandable inorganic material other than the thermally expandable graphite, an inorganic filler, etc.

[0054] The heat-expandable fire-resistant sheet of the present invention can be obtained by extrusion molding a kneaded mixture of a heat-expandable composition, or by applying the kneaded mixture to any object and solidifying or drying the heat-expandable composition after application.

[0055] From the viewpoint of obtaining a wound body having a length of 1 m or more with little variation in thickness and a good appearance, it is preferable to adopt a method of kneading the thermally conductive composition with a low kneading load. When the kneading load is low, deterioration of the thermally expandable graphite is unlikely to occur, and therefore gas generation can be suppressed. Therefore, it is easy to obtain a wound body having a length of 1 m or more with a good appearance.

[0056] Specifically, when the above-mentioned resin for extrusion molding is used as the matrix component, the Mooney viscosity ML(1+4) of the thermally expandable composition at 100°C is preferably 10 to 70, more preferably 30 to 60, from the viewpoint of reducing the kneading load.

[0057] When the above-described extrusion resin is used as the matrix component, it is preferable to extrude the thermally expandable composition to obtain a thermally expandable fire-resistant sheet. In extrusion molding, the thermally expandable composition is melted and extruded using an extruder. The extruder may be a single-screw extruder or a twin-screw extruder. Furthermore, it is preferable for the extruder to have a vent mechanism. This allows gas generated during kneading of the thermally expandable composition to be discharged outside the system, making it easier to obtain a thermally expandable fire-resistant sheet with high thickness accuracy and good appearance. The kneading temperature during extrusion molding should be below the expansion initiation temperature of the thermally expandable graphite, preferably 80 to 160°C, and more preferably 90 to 120°C.

[0058] When a dry-and-solidify adhesive such as a solvent-based adhesive, emulsion-based adhesive, or synthetic rubber latex-based adhesive is used as the matrix component, the thermally expandable composition is preferably kneaded at room temperature (40°C) and a shear rate of 25 s -1 The viscosity measured by a rheometer at 120°C and a shear rate of 25 s is preferably 0.1 to 20 Pa·s, more preferably 2 to 8 Pa·s. When a hot-melt adhesive is used as the matrix component, the viscosity of the thermally expandable composition at 120°C and a shear rate of 25 s is preferably 0.1 to 20 Pa·s, more preferably 2 to 8 Pa·s. -1 The viscosity measured by a rheometer in the above ranges preferably from 0.1 to 200 Pa·s, more preferably from 1 to 100 Pa·s.

[0059] When a dry-and-solidify adhesive is used as the matrix component, it is preferable to apply a mixture obtained by kneading a thermally expandable composition to a desired object to obtain a thermally expandable fire-resistant sheet. The kneading temperature is preferably around room temperature, for example, 20 to 40°C. When a dry-and-solidify adhesive is used, the thermally expandable composition is in a liquid state containing a solvent, so the thermally expandable fire-resistant sheet can be formed by drying the thermally expandable composition after application to remove the solvent. Drying can be carried out by leaving it at around room temperature (about 25°C), but it is preferable to heat it. Heating is preferably carried out at or below the expansion initiation temperature of the thermally expandable graphite, for example, at about 50 to 160°C, preferably about 60 to 120°C.

[0060] When a hot-melt adhesive is used as the matrix component, it is preferable to knead the thermally expandable composition and apply the molten mixture to an object to obtain a thermally expandable fire-resistant sheet. The kneading temperature should be equal to or lower than the expansion initiation temperature of the thermally expandable graphite, preferably 80 to 160°C, and more preferably 90 to 120°C.

[0061] The object to which the thermally expandable composition is applied is not particularly limited, but may be, for example, a release-treated resin film, or when a thermally expandable fire-resistant sheet having a substrate is produced, the substrate may be the object to which the thermally expandable composition is applied.

[0062] <Substrate, Adhesive Layer, Separator> The heat-expandable fire-resistant sheet of the present invention may be used alone, or may be used as a multilayer sheet by attaching other components as appropriate. Specifically, the heat-expandable fire-resistant sheet may have a substrate or an adhesive layer on at least one surface. For example, the heat-expandable fire-resistant sheet may have a substrate on one surface (a multilayer sheet of substrate / heat-expandable fire-resistant sheet), an adhesive layer on one surface (a multilayer sheet of adhesive layer / heat-expandable fire-resistant sheet), or a substrate on one surface and an adhesive layer on the other surface (a multilayer sheet of adhesive layer / heat-expandable fire-resistant sheet / substrate). Furthermore, the heat-expandable fire-resistant sheet may have a separator, for example, a separator may be provided on the surface of the adhesive layer.

[0063] (Substrate) The substrate is in the form of, for example, a woven fabric, a nonwoven fabric, a film, etc., and is formed from a thermoplastic resin, a thermosetting resin, an elastomer resin, etc., among which a thermoplastic resin is preferred. The substrate may also be formed from glass fiber, ceramic fiber, cellulose fiber, polyester fiber, carbon fiber, graphite fiber, thermosetting resin fiber, etc. A preferred form of the substrate is a film. A film having a cavity therein can also be suitably used as the film.

[0064] Specific examples of thermoplastic resins include polyesters such as polyvinyl chloride, polyethylene terephthalate, and polybutylene terephthalate; polyolefins such as polyethylene, polypropylene, poly(1-butene), and polypentene; polyvinyl acetate, polystyrene, acrylic resins, acrylonitrile-butadiene-styrene (ABS) resins, polycarbonate, polyamide, polyphenylene ether, and polyethersulfone. Among these, from the viewpoint of adhesion to the thermally expandable fire-resistant sheet, preferred thermoplastic resins are polyvinyl chloride, polyethylene terephthalate, polyolefins, and polyvinyl acetate. Furthermore, from the viewpoint of flame retardancy, polyvinyl chloride is more preferred. Also preferred is a polyethylene terephthalate film having internal cavities.

[0065] Specific examples of thermosetting resins include epoxy resins, urethane resins, phenolic resins, unsaturated polyesters, alkyd resins, urea resins, and polyimides.

[0066] Specific examples of elastomer resins include isoprene rubber, butadiene rubber, 1,2-polybutadiene rubber, styrene-butadiene rubber, chloroprene rubber, nitrile rubber, butyl rubber, ethylene-propylene rubber, chlorosulfonated polyethylene, acrylic rubber, epichlorohydrin rubber, silicone rubber, fluororubber, urethane rubber, polyisobutylene rubber, and butyl chloride. One or more of the above-mentioned thermoplastic resins, thermosetting resins, and elastomer resins are used.

[0067] The thickness of the substrate is preferably 1 to 20% of the thickness of the multilayer sheet. When the thickness of the substrate is 1% or more of the thickness of the multilayer sheet, the substrate can easily support the heat-expandable fire-resistant sheet. Furthermore, when the thickness of the substrate is 20% or less of the thickness of the multilayer sheet, peeling between the substrate and the heat-expandable fire-resistant sheet and the occurrence of wrinkles in the substrate are suppressed when the multilayer sheet is curved, and the appearance of the multilayer sheet can be maintained in a good condition.

[0068] The thickness of the substrate is, for example, 10 to 500 μm, preferably 20 to 450 μm, and more preferably 30 to 400 μm. By making the thickness of the substrate equal to or greater than these lower limits, the substrate can be provided with the strength to support the thermally expandable fire-resistant sheet. Furthermore, by making the thickness equal to or less than the upper limits, the thickness of the substrate can be prevented from becoming thicker than necessary, making it easier to use the multilayer sheet in fire prevention equipment such as doors.

[0069] (Adhesive Layer) The adhesive layer may be a single layer (hereinafter also referred to as adhesive layer) formed solely from an adhesive, or may be a double-sided adhesive tape in which adhesive layers are provided on both surfaces of a double-sided adhesive tape substrate. However, an adhesive layer is preferred. The adhesive layer of a double-sided adhesive tape is formed by bonding one of the adhesive layers to a heat-expandable fire-resistant sheet or a separator. The adhesive constituting the adhesive layer is not particularly limited, and examples thereof include acrylic adhesives, urethane adhesives, and rubber adhesives. The thickness of the adhesive layer is not particularly limited, but is, for example, 10 to 500 μm, preferably 50 to 200 μm. The substrate for a double-sided adhesive tape is not particularly limited as long as it is a substrate commonly used in double-sided adhesive tapes, and examples thereof include nonwoven fabrics, paper such as Japanese paper, woven fabrics made of natural fibers, synthetic fibers, and the like, resin films made of polyester, polyolefin, soft polyvinyl chloride, hard polyvinyl chloride, acetate, and the like, and flat yarn cloth.

[0070] (Separator) The separator may be, for example, a separator substrate comprising a separator base material and a release layer provided on at least one surface of the separator base material. The release layer can be formed by subjecting the separator base material to a release treatment. The separator may be positioned so that the surface on which the release layer is provided contacts the adhesive layer. Alternatively, both surfaces of the separator base material may be subjected to a release treatment, and release layers may be provided on both surfaces. The release layer is not particularly limited, but may be composed of, for example, an organic resin. As the organic resin, a known release agent may be used, such as a fluorine-based resin, a long-chain alkyl-containing resin, an alkyd-based resin, a polyolefin-based resin, or a rubber-based elastomer. As the separator base material, a resin film, paper, or the like may be used. The resin film may be formed from a thermoplastic resin, a thermosetting resin, an elastomer resin, or the like. Specific examples of the thermoplastic resin, thermosetting resin, or elastomer resin include those listed for the resin film, but thermoplastic resins are preferred.

[0071] The thickness of the separator is preferably 0.3 to 10% of the thickness of the multilayer sheet. When the thickness of the separator is 0.3% or more of the thickness of the multilayer sheet, the separator is more likely to be prevented from breaking. Furthermore, when the thickness of the separator is 10% or less of the thickness of the multilayer sheet, peeling between the heat-expandable fire-resistant sheet and the separator and the occurrence of wrinkles in the separator are prevented when the multilayer sheet is bent, and the appearance of the multilayer sheet can be maintained in a good condition.

[0072] The thickness of the separator is, for example, 1 to 200 μm, preferably 2 to 150 μm, and more preferably 5 to 100 μm. By making the thickness of the separator equal to or greater than these lower limits, the separator can be provided with sufficient strength to withstand breakage. Furthermore, by making the thickness equal to or less than the upper limits, peeling between the fireproof material and the separator and wrinkles on the separator can be prevented when the multilayer sheet is bent.

[0073] [Fire Prevention Equipment] The present invention can provide fire prevention equipment at least partially equipped with a heat-expandable fire-resistant sheet cut from the above-mentioned roll. Examples of fire prevention equipment include fittings such as windows, shoji screens, doors, sliding doors, and other doors, pillars, walls made of steel concrete, floors, and roofs. The heat-expandable fire-resistant sheet of the present invention is installed in part of such fire prevention equipment and expands in the event of a fire, thereby reducing or preventing the penetration of flames and smoke. In particular, the heat-expandable fire-resistant sheet is preferably used in gaps between windows and window frames, between doors and door frames, and the like.

[0074] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0075] The measurement and evaluation methods for each physical property are as follows. <Expansion Start Temperature of Thermally Expandable Graphite> In a rheometer ("Discovery HR-2", manufactured by TA Instruments), 0.5 g of a sample of thermally expandable graphite was placed on the sample stage and wrapped in aluminum foil to prevent the powder from falling off. The sample was grounded with a 25 mmφ cone plate until the load became 0 [N]. From this state, the sample was heated at a constant heating rate (10°C / min) from a set temperature of 50°C using a Peltier heater, and the point when the load reached 0.1 N was taken as the expansion start temperature.

[0076] <Mooney Viscosity During Kneading> The Mooney viscosity ML(1+4) of the thermally expandable composition at 100° C. during kneading was measured in accordance with JIS K6300.

[0077] <Viscosity during kneading (40°C, 120°C)> The viscosity of the thermally expandable composition during kneading was measured using a rheometer. The rheometer used was a Discovery HR20 manufactured by TA Instruments, and the measurement was performed at temperatures of 40°C and 120°C under the measurement conditions of a shear rate of 25 s -1 It was decided.

[0078] <Expansion Start Temperature of Heat-Expandable Fire-Resistant Sheet> Using a heat-expandable fire-resistant sheet as a sample, the temperature was increased at a rate of 10°C / min using a rheometer ("Discovery HR2" manufactured by TA Instruments), and the temperature at which the normal force rose was measured, and this was taken as the expansion start temperature.

[0079] <Expansion Ratio of Heat-Expandable Fireproof Sheet> The heat-expandable fireproof sheets of each Example and Comparative Example were cut to a predetermined size (thickness 1.5 mm, width 25 mm, length 25 mm). Each heat-expandable fireproof sheet of the predetermined size was placed on the bottom surface of a stainless steel plate (98 mm square, thickness 0.3 mm), and then placed in an electric furnace and heated at 200°C for 30 minutes. The expansion ratio was calculated by dividing the thickness of the heat-expandable fireproof sheet after heating by the thickness of the heat-expandable fireproof sheet before heating.

[0080] <Thickness Variation> The thickness of the heat-expandable fire-resistant sheet was measured at 10 equally spaced points along the longitudinal direction, and the average thickness was calculated by averaging these 10 thicknesses. Next, the absolute value A of the difference between the thickness measured at each of the 10 equally spaced points along the longitudinal direction of the heat-expandable fire-resistant sheet and the average thickness was calculated, and the average of the absolute values ​​A for the 10 points was taken as the thickness variation. The ratio (%) of the thickness variation to the average thickness was then calculated.

[0081] <Appearance> The appearance of the obtained thermally expandable fire-resistant sheet was evaluated according to the following criteria. After producing a long fire-resistant sheet, the fire-resistant sheet was cured at 40°C for one week and then re-unfolded to evaluate. During the unfolding process, the appearance of the sheet was observed to determine whether or not bubbles were observed on the surface. If bubbles of 5 mm or more in the width direction were not observed, it was rated as A, and if bubbles were observed, it was rated as B.

[0082] <Strength> The strength of the obtained thermally expandable fire-resistant sheets was evaluated according to the following criteria. Using a rolled fire-resistant sheet obtained by winding up the long fire-resistant sheet obtained in each Example and Comparative Example, the fire-resistant sheet was re-deployed at 20°C for evaluation. During the unfolding process, the appearance of the sheet was observed to check whether the surface cracked or broke. Evaluation was based on the following criteria. A: The sheet could be unfolded without breaking. B: The sheet broke when unfolded.

[0083] <Elution Rate> A test piece (10 g) prepared by cutting out the obtained thermally expandable fireproof sheet was immersed in 200 g of pure water and left to immerse in a sealed container at 60°C for one week. The test piece was then removed, the pure water was evaporated and dried, and the mass of the precipitate that formed was measured. Using this value, the elution rate was calculated using the following formula and used as an index of water resistance: Elution Rate (%) = [(Mass of Precipitate) / (Mass of Test Piece Before Immersion in Pure Water)] × 100

[0084] The components used in the examples and comparative examples are as follows. <Matrix components> Chloroprene: "Skyprene B-31" manufactured by Tosoh Corporation, extrusion molding resin Chloroprene: "Skyprene Y-30S" manufactured by Tosoh Corporation, solvent-based adhesive, solvent (toluene) Chloroprene: "Skyprene LA-710" manufactured by Tosoh Corporation, synthetic rubber latex-based adhesive Styrene-butadiene rubber (SBR), "JSR0202" manufactured by JSR Corporation, extrusion molding resin Styrenic thermoplastic elastomer: styrene-butadiene-styrene (SBS), "TR1086" manufactured by JSR Corporation, extrusion molding resin Styrenic thermoplastic elastomer (TPS): polystyrene-poly(ethylene-propylene) (SEP), "Septon 1020" manufactured by Kuraray Co., Ltd., extrusion molding resin Acrylic resin: "ACRYDIC 57-773-BA" manufactured by DIC Corporation, solvent-based adhesive, solvent (ethyl acetate, butyl acetate)・Silicone resin (unmodified): Shin-Etsu Silicones "KR220L", solvent-based adhesive, solvent (toluene, isopropyl alcohol) ・Modified silicone resin system: polymer having crosslinkable silyl groups, Kaneka Corporation "MS Polymer S-303", moisture-curing reaction type ・Modified silicone resin system: polymer having crosslinkable silyl groups, Toagosei Co., Ltd. "US-6150", moisture-curing reaction type ・Modified silicone resin system: polymer having crosslinkable silyl groups, AGC Corporation "Excestar-S6250", moisture-curing reaction type ・Modified silicone resin system: polymer having crosslinkable silyl groups, Soken Chemical & Engineering Co., Ltd. "SE-09", moisture-curing reaction type ・Modified silicone resin system: polymer having crosslinkable silyl groups, Kaneka Corporation "Silyl EST280", moisture-curing reaction type ・Silylated urethane system: Momentive Performance Materials Japan "SPUR3030"・Ethylene-vinyl acetate copolymer resin (EVA-based), Mitsui Chemicals' "V5774ETWR", hot-melt adhesive ・Polystyrene-based, Mitsui Chemicals' "FTR6100", hot-melt adhesive ・Epoxy resin-based, Mitsubishi Chemical's "jER807", amine-based curing agent, Mitsubishi Chemical's "FL052", catalyst, Shikoku Chemicals' "Curesol 1.2DMZ", heat-curing reaction adhesive

[0085] <Curing catalyst> - "Neostan U220H" manufactured by Nitto Kasei Co., Ltd.

[0086] <Thermal expandable graphite> ・Fuji Graphite Industries Co., Ltd. "EXP-50S150", expansion start temperature 150°C ・Fuji Graphite Industries Co., Ltd. "EXP-50S120", expansion start temperature 120°C

[0087] <Inorganic fillers> Iron oxide Aluminum hydroxide (Shiraishi Calcium Co., Ltd.) Calcium carbonate (Shiraishi Calcium Co., Ltd.)

[0088] [Example 1] The components were introduced into an extruder so as to obtain the composition shown in Table 1, and the kneaded thermally expandable composition was extruded at 110°C to obtain a thermally expandable fire-resistant sheet. The thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm) was subjected to various evaluations. The extruder used had a vent mechanism.

[0089] [Examples 4 to 6, Comparative Example 1] A thermally expandable fire-resistant sheet was obtained in the same manner as in Example 1, except that the composition was changed as shown in Table 1. Various evaluations were carried out on the thermally expandable fire-resistant sheet.

[0090] [Example 2] The components were mixed at 40°C using a stirrer to obtain the composition shown in Table 1, and the mixture was dissolved in toluene to a solids concentration of 40%, yielding a thermally expandable composition. The thermally expandable composition was then applied to a release PET film using a roll coater, and the applied product was dried to evaporate the solvent, forming a thermally expandable fire-resistant sheet on the release PET film. The thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm) was subjected to various evaluations.

[0091] [Example 3] A thermally expandable composition was obtained by mixing the components at 25°C using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then applied to a release PET film using a roll coater, and the applied product was dried at 120°C to evaporate the solvent, forming a thermally expandable fire-resistant sheet on the release PET film. Various evaluations were performed on the thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm).

[0092] [Examples 7 and 8] A thermally expandable fire-resistant sheet was obtained in the same manner as in Example 3, except that the composition and drying temperature were changed to those shown in Table 1. Various evaluations were carried out on the thermally expandable fire-resistant sheet.

[0093] [Example 9] A thermally expandable composition was obtained by mixing the components using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then heated to 110°C to melt and knead, and then applied to a release PET film using a roll coater. The applied product was cooled to room temperature (25°C) and solidified to form a thermally expandable fire-resistant sheet on the release PET film. Various evaluations were performed on the thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm).

[0094] Example 10 A thermally expandable fire-resistant sheet was obtained in the same manner as in Example 9, except that the composition was changed as shown in Table 1. The thermally expandable fire-resistant sheet was subjected to various evaluations.

[0095] [Examples 11 to 18] A thermally expandable composition was obtained by mixing the components at 25°C using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then applied to a release PET film using a roll coater, and the applied product was cured at 50°C to form a thermally expandable fire-resistant sheet on the release PET film. Various evaluations were performed on the thermally expandable fire-resistant sheet (length 20 mm, thickness 1.5 mm, width 10 mm).

[0096] [Example 19] A thermally expandable composition was obtained by mixing the components at 40°C using a stirrer to obtain the composition shown in Table 1. The thermally expandable composition was then applied to a release PET film using a roll coater, and the applied material was thermally cured to form a thermally expandable fire-resistant sheet on the release PET film. Various evaluations were performed on the thermally expandable fire-resistant sheet (length 100 mm, thickness 1.5 mm, width 10 mm).

[0097] Table 1 shows the composition of the thermally expandable fire-resistant sheet and the composition of the solid content of the thermally expandable composition.

[0098] In each example, a long heat-expandable fire-resistant sheet with good appearance was obtained despite the use of heat-expandable graphite with a low thermal expansion onset temperature. In contrast, the heat-expandable fire-resistant sheet of Comparative Example 1 had a large variation in thickness and was inferior in appearance and strength.

Claims

1. A heat-expandable fire-resistant sheet containing a matrix component and heat-expandable graphite, having an expansion start temperature of 160°C or less, an average thickness of 0.5 mm or more, a thickness variation of 10% or less of the average thickness, and a length of 1 m or more in a rolled form.

2. The thermally expandable fire-resistant sheet according to claim 1, further comprising at least one selected from the group consisting of thermally expandable inorganic substances other than thermally expandable graphite and inorganic fillers.

3. The thermally expandable fireproof sheet according to claim 2, wherein the content of thermally expandable graphite is 3 to 300 parts by mass and the content of inorganic filler is 2 to 200 parts by mass per 100 parts by mass of the matrix component.

4. The heat-expandable fire-resistant sheet according to claim 1 or 2, which has an expansion ratio of 5 times or more when heated at 200°C for 30 minutes.

5. The heat-expandable fire-resistant sheet according to claim 1 or 2, which has a dissolution rate of 3% or less after immersion in pure water at 60°C for one week.

6. The thermally expandable fire-resistant sheet according to claim 1 or 2, wherein the matrix component does not contain a phosphorus component.

7. The thermally expandable fire-resistant sheet according to claim 1 or 2, having a substrate or an adhesive layer on at least one surface.

8. A fire protection system having at least a part mounted thereon a thermally expandable fireproof sheet cut out from the roll according to claim 1 or 2.

Citation Information

Patent Citations

  • Fire-resistant resin composition

    JP2017141463A

  • Fire-resistant resin composition

    JP2004043641A

  • Refractory material and wound body thereof

    JP2017141661A

  • Fireproof sheet and wound body thereof

    JP2017155227A

  • Thermally-expandable refractory sheet

    JP2018070879A