Aluminum-diamond composite, method for producing aluminum-diamond composite, and semiconductor package

The aluminum-diamond composite with a laminated structure and uniform diamond particle distribution addresses the thermal conductivity challenges in semiconductor packages, achieving enhanced heat dissipation through the manufacturing method utilizing a V-type mixer.

WO2024225342A1PCT designated stage expired Publication Date: 2024-10-31DENKA CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016149
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2024-04-24
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Existing aluminum-diamond composites for heat dissipation in semiconductor packages face challenges in achieving high thermal conductivity due to uneven distribution and variation in diamond particle sizes, which affects their thermal performance.

Method used

An aluminum-diamond composite with a laminated structure, where diamond particles of different sizes are uniformly dispersed within an aluminum phase, and a manufacturing method using a V-type mixer to achieve a specific ratio of coarse to fine particles, resulting in a densely packed composite with reduced particle distribution variation.

Benefits of technology

The solution enhances thermal conductivity by ensuring high uniformity and density of diamond particles within the aluminum phase, leading to improved heat dissipation capabilities in semiconductor packages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016149_31102024_PF_FP_ABST
    Figure JP2024016149_31102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an aluminum-diamond composite comprising a laminate structure including a composite layer, which contains an aluminum phase and a plurality of diamond particles having different sizes from each other, and a pair of aluminum layers sandwiching the composite layer, wherein: in a cut surface obtained by cutting along a lamination direction, the plurality of diamond particles include coarse particles having an area of 2000 μm2 or more and fine particles having an area less than 2000 μm2; and an average value α of the ratio of the total area of the coarse particles to the total area of the plurality of diamond particles in a region up to 200 μm from a boundary line between the pair of aluminum layers and the composite layer toward the inside of the composite layer is 65-80%.
Need to check novelty before this filing date? Find Prior Art

Description

Aluminum-diamond composite, method for producing aluminum-diamond composite, and semiconductor package

[0001] The present disclosure relates to aluminum-diamond composites, methods for making aluminum-diamond composites, and semiconductor packages.

[0002] An aluminum-diamond composite is a composite material made of diamond, which has high thermal conductivity, and aluminum, which has a high thermal expansion coefficient, and is used in a variety of materials such as heat sinks. Patent Document 1 discloses an aluminum-diamond composite heat dissipation part. Patent Document 2 discloses a semiconductor package using such a composite.

[0003] JP 2014-107468 A International Publication No. 2015 / 182576

[0004] An aluminum-diamond composite is formed by dispersing diamond particles in an aluminum phase. Therefore, it is believed that the thermal conductivity of the composite can be improved by adjusting the size, number, and distribution of diamond particles in the aluminum phase. The present disclosure provides an aluminum-diamond composite having sufficiently high thermal conductivity, and a method for producing the same. The present disclosure provides a semiconductor package that is equipped with such an aluminum-diamond composite and has excellent heat dissipation properties.

[0005] One aspect of the present disclosure provides the following aluminum-diamond composite:

[0006] [1] An aluminum-diamond composite having a laminated structure including a composite layer containing an aluminum phase and a plurality of diamond particles having different sizes, and a pair of aluminum layers sandwiching the composite layer, wherein, in a cut surface obtained by cutting along the lamination direction, the plurality of diamond particles have a size of 2000 μm or less. 2 Coarse particles having an area of ​​2000 μm or more 2and fine particles having an area of ​​less than 100 μm, wherein an average value α of the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles in a region extending from the boundary line between the pair of aluminum layers and the composite layer to 200 μm inside the composite layer is 65 to 80%.

[0007] In the aluminum-diamond composite of [1] above, in a predetermined region of the cut surface, the average area ratio α of the coarse diamond particles to the total area of ​​the coarse and fine diamond particles is 65 to 80%. Such an aluminum-diamond composite has high thermal conductivity because the diamond particles, which have high thermal conductivity, are densely dispersed in the aluminum phase.

[0008] The aluminum-diamond composite of the above [1] may be any one of the following [2] to [4].

[0009] [2] The aluminum-diamond composite according to [1], wherein the average value β of the ratio of the number of the coarse particles to the number of the plurality of diamond particles in the region is 2.0% or less. [3] The aluminum-diamond composite according to [1] or [2], wherein the region includes a first region that is a region extending from a boundary between one of the pair of aluminum layers and the composite layer to 200 μm inward of the composite layer, and a second region that is a region extending from a boundary between the other of the aluminum layers and the composite layer to 200 μm inward of the composite layer, and wherein the absolute value of the difference between the average value β1 of the ratio of the number of the coarse particles to the number of the plurality of diamond particles in the first region and the average value β2 of the ratio of the number of the coarse particles to the number of the plurality of diamond particles in the second region is 0.6% or less. [4] The aluminum-diamond composite according to any one of [1] to [3], wherein the region includes a first region that is a region extending from the boundary line between one of the pair of aluminum layers and the composite layer to 200 μm inward of the composite layer, and a second region that is a region extending from the boundary line between the other of the aluminum layers and the composite layer to 200 μm inward of the composite layer, and the absolute value of the difference between the average value α1 of the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles in the first region and the average value α2 of the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles in the second region is 6.0% or less.

[0010] The aluminum-diamond composite of [2] has an average particle ratio β of 2.0% or less in the region of the cut surface of the aluminum-diamond composite, which is the ratio of the number of coarse particles to the number of diamond particles. Such an aluminum-diamond composite has an even higher thermal conductivity.

[0011] In the aluminum-diamond composite of [3], the absolute value of the difference between the average particle number ratio β1 in the first region and the average particle number ratio β2 in the second region is 0.6% or less. Such an aluminum-diamond composite has a higher thermal conductivity because the variation in the distribution of coarse particles is sufficiently reduced.

[0012] In the aluminum-diamond composite of [4], the absolute value of the difference between the average area ratio α1 in the first region and the average area ratio α2 in the second region is 6.0% or less. Such an aluminum-diamond composite has a sufficiently reduced variation in the distribution of coarse particles, and therefore has a higher thermal conductivity.

[0013] One aspect of the present disclosure provides the following method for producing an aluminum-diamond composite.

[0014] [5] A method for producing an aluminum-diamond composite, comprising: a mixing step of mixing coarse and fine diamond particles of different sizes using a V-type mixer to obtain a mixture containing a plurality of diamond particles; and a heating step of heating the mixture while sandwiched between aluminum foils to obtain a layered structure comprising a composite layer containing an aluminum phase and the mixture, and a pair of aluminum layers sandwiching the composite layer.

[0015] The method for producing an aluminum-diamond composite described in [5] above includes a mixing step in which coarse and fine diamond particles are mixed using a V-type mixer. In this method for producing an aluminum-diamond composite that includes a mixing step, the coarse and fine diamond particles are mixed with high uniformity, making it possible to obtain an aluminum-diamond composite with high thermal conductivity.

[0016] The aluminum-diamond composite of [5] above may be any one of [6] to [8] below.

[0017] [6] In a cut surface obtained by cutting the aluminum-diamond composite along the lamination direction, the plurality of diamond particles have a diameter of 2000 μm 2 The coarse particles having an area of ​​2000 μm or more, 2and the fine particles have an area of ​​less than 1 / 2 mm, and an average value α of the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles in a region from the boundary line between the pair of aluminum layers and the composite layer to 200 μm into the composite layer is 65 to 80%. [7] The method for producing an aluminum-diamond composite according to [5] or [6], which includes rotating the V-type mixer at a rotation speed of 15 to 50 rpm for 5 to 30 minutes in the mixing step. [8] The method for producing an aluminum-diamond composite according to any one of [5] to [7], wherein the ratio of the volume of the plurality of diamond particles to the total volume of the V-type mixer in the mixing step is 10 to 50%.

[0018] In the method for producing an aluminum-diamond composite described above in [6], the average area ratio α of the coarse particles to the total area of ​​the coarse and fine diamond particles in the region of the cut surface of the aluminum-diamond composite is 65 to 80%. In this method for producing an aluminum-diamond composite, the diamond particles, which have high thermal conductivity, are densely dispersed in the aluminum phase, making it possible to obtain an aluminum-diamond composite with high thermal conductivity.

[0019] The method for producing an aluminum-diamond composite according to [7] above includes rotating the V-type mixer at a rotation speed of 15 to 50 rpm for 5 to 30 minutes in the mixing step. This method for producing an aluminum-diamond composite allows the diamond particles to be mixed with higher uniformity, resulting in an aluminum-diamond composite with higher thermal conductivity.

[0020] In the method for producing an aluminum-diamond composite described above in [8], the ratio of the volume of the plurality of diamond particles to the total volume of the V-type mixer is 10 to 50%. In this method for producing an aluminum-diamond composite, the diamond particles can be mixed with higher uniformity, thereby obtaining an aluminum-diamond composite with higher thermal conductivity.

[0021] One aspect of the present disclosure provides the following semiconductor package.

[0022] [9] A semiconductor package comprising a heat dissipation member containing the aluminum-diamond composite described in any one of [1] to [4] above, or an aluminum-diamond composite obtained by the manufacturing method described in any one of [5] to [8] above, and a semiconductor element bonded to the heat dissipation member.

[0023] The semiconductor package of [9] above includes a heat dissipation member containing the aluminum-diamond composite, and therefore has high thermal conductivity.

[0024] The present disclosure can provide an aluminum-diamond composite having sufficiently high thermal conductivity, and a method for producing the same. The present disclosure can provide a semiconductor package that includes such an aluminum-diamond composite and has excellent heat dissipation properties.

[0025] FIG. 1 is a diagram showing an example of a cross section of an aluminum-diamond composite in the lamination direction. FIG. 2 is an enlarged view of a portion of the boundary between the first aluminum layer and the first region in a cross section of an aluminum-diamond composite in the lamination direction. FIG. 3 is a diagram showing an example of a block formation step in a method for manufacturing an aluminum-diamond composite. FIG. 4 is a diagram showing an example of a heating step in a method for manufacturing an aluminum-diamond composite. FIG. 5 is a diagram showing an example of a semiconductor package using a heat dissipation member including an aluminum-diamond composite. FIG. 6 is an SEM photograph of a cross section of No. 1 of an aluminum-diamond composite in Example 1. FIG. 7 is an SEM photograph of a cross section of No. 2 of an aluminum-diamond composite in Example 1. FIG. 8 is an SEM photograph of a cross section of No. 3 of an aluminum-diamond composite in Example 1. FIG. 9 is an SEM photograph of a cross section of No. 4 of an aluminum-diamond composite in Example 1.

[0026] Embodiments of the present disclosure are described below. However, the following embodiments are merely examples for explaining the present disclosure and are not intended to limit the present disclosure to the following content. The upper or lower limit of a numerical range specified in this specification may be replaced with any value shown in the examples. Furthermore, the individually described upper and lower limit values ​​may be arbitrarily combined. Unless otherwise specified, the materials or components exemplified in this specification may be used alone or in combination of two or more. In the description, identical elements or elements having the same function are denoted by the same reference numerals, and redundant explanations are omitted. Furthermore, unless otherwise specified, the positional relationships, such as up, down, left, and right, used in the description are based on the positional relationships shown in the drawings. The symbol "to" used in a numerical range indicates a numerical range that includes the upper and lower limit values. For example, "X to Y" indicates a numerical range "greater than or equal to X and less than or equal to Y."

[0027] 1 shows a cross section obtained by cutting an aluminum-diamond composite according to one embodiment along the layering direction. The aluminum-diamond composite 100 comprises a first aluminum layer 20, a composite layer 10, and a second aluminum layer 30, in this order.

[0028] There are no particular limitations on the shape of the aluminum-diamond composite 100 as long as it is plate-like. The thickness of the aluminum-diamond composite 100 may be 1.0 to 3.0 mm, or 1.2 to 2.5 mm.

[0029] The composite layer 10 includes an aluminum phase and a plurality of diamond particles of different sizes. The diamond particles may be natural diamond, synthetic diamond, or a mixture of both. The composite layer 10 also includes large coarse particles and small fine particles. The average particle size of the coarse particles may be 100-250 μm or 140-210 μm. The average particle size of the fine particles may be 5-30 μm or 10-25 μm. The diamond particles may be high-purity or may contain a binder such as silica. The average particle sizes of the diamond particles, coarse particles, and fine particles can be measured using a laser diffraction / scattering particle size distribution analyzer in accordance with ISO 13320:2009. An example of a laser diffraction / scattering particle size distribution analyzer is the "LS-13 320" (device name) manufactured by Beckman Coulter. In a volume-based particle size distribution (cumulative distribution) shown with the horizontal axis representing particle size [μm] on a logarithmic scale and the vertical axis representing frequency [volume %], the particle size when the cumulative value from small particle sizes reaches 50% of the total is the above-mentioned average particle size (D50).

[0030] As the diamond particles, diamond particles having a β-type silicon carbide layer formed on the surface can also be used. Such diamond particles are preferable to those made of metal carbides having low thermal conductivity (e.g., aluminum carbide (Al 4 C 3 )) can be suppressed, and the thermal conductivity of the aluminum-diamond composite 100 can be improved.

[0031] The thickness of the composite layer 10 may be 0.5 to 2.5 mm, may be 0.8 to 2.2 mm, or may be 1.0 to 1.8 mm.

[0032] The mass ratio of coarse particles to the total mass of diamond particles in the composite layer 10 may be 60 mass% or more, 70 mass% or more, or 90 mass% or less. The mass ratio of coarse particles may be, for example, 60 to 90 mass%, or 70 to 90 mass%. The mass ratio of fine particles to the total mass of diamond particles may be 40 mass% or less, 30 mass% or less, or 10 mass% or more. The mass ratio of fine particles may be, for example, 10 to 30 mass%, or 10 to 40 mass%. When the diamond particles have such a mass ratio of coarse particles and fine particles, the diamond particles are dispersed in the aluminum phase with high uniformity, and the thermal conductivity of the aluminum-diamond composite 100 can be improved.

[0033] The aluminum phase only needs to contain aluminum as a main component, and may also contain metals other than aluminum. Examples of metals other than aluminum include silicon, magnesium, and copper. By including such metals, the aluminum phase can be sufficiently infiltrated into the voids of the diamond particles, resulting in a denser composite layer 10.

[0034] The aluminum-diamond composite 100 has a first aluminum layer 20 and a second aluminum layer 30 sandwiching the composite layer 10. By having such aluminum layers, the main surfaces 100a, 100b of the aluminum-diamond composite 100 can be made smooth, improving plating properties.

[0035] The thickness of the first aluminum layer 20 and the second aluminum layer 30 may be 10 to 100 μm, or 20 to 80 μm. When the thickness of the first aluminum layer 20 and the second aluminum layer 30 is within this range, the thermal conductivity of the aluminum-diamond composite 100 can be increased while improving the plating properties of the surface.

[0036] The lower limit of the aluminum content in the first aluminum layer 20 and the second aluminum layer 30 may be, for example, 80 mass%, 82 mass%, 84 mass%, or 86 mass%, and the upper limit of the aluminum content may be, for example, 100 mass%, 98 mass%, 96 mass%, 94 mass%, 92 mass%, or 90 mass%.

[0037] The aluminum-diamond composite 100 may have plating layers on the main surfaces 100a, 100b. The plating layers may have a nickel plating layer and a gold plating layer in this order from the aluminum-diamond composite 100 side. In this case, the average thickness of the nickel plating layer may be 0.5 to 6.5 μm, and the average thickness of the gold plating layer may be 0.5 μm or more. By keeping the average thickness of the nickel plating layer within the above range, it is possible to suppress the occurrence of defects such as pinholes in the plating layer, and to more sufficiently suppress the occurrence of peeling of the plating film and cracks, even in the high-temperature environment when the plated component is used.

[0038] A common plating method can be used to form the plating layer. Examples of plating methods include electrolytic plating and electroless plating. When nickel plating is performed on the first aluminum layer 20 and the second aluminum layer 30, a pretreatment may be performed in which at least a portion of the main surfaces 100a, 100b of the aluminum-diamond composite 100 is replaced with zinc or the like. By performing such a pretreatment, the adhesion of the plating layer can be further improved.

[0039] When nickel plating is performed to form a nickel plating layer, an amorphous nickel alloy plating film having a thickness of 0.5 to 6.5 μm may be formed on the surface of the nickel plating layer. In this case, even if diamond particles are exposed on the surface of the aluminum-diamond composite, the occurrence of pinholes and the like can be suppressed. The means for forming the amorphous nickel alloy plating may be an electroless plating method. In this case, the amorphous nickel alloy plating may be an alloy plating containing nickel and phosphorus (P), for example, 5 to 15 mass %.

[0040] Furthermore, with an increase in the bonding temperature and an increase in the temperature load during actual use, the amorphous nickel alloy plating crystallizes, causing microcracks due to the volume change at that time, and the cracks may then extend due to the subsequent temperature load. Therefore, the nickel alloy plating layer may have a thickness of, for example, 0.5 to 2 μm.

[0041] When used in applications where brazing material is used for joining at high temperatures, it is desirable to provide a gold plating layer on the outermost surface of the plated part. The thickness of the gold plating layer may be, for example, 0.01 μm or more from the viewpoint of ensuring a sufficiently strong bond. The thickness of the gold plating layer may be, for example, 4.0 μm or less from the viewpoint of reducing costs.

[0042] In the cut surface of the aluminum-diamond composite 100 shown in Figure 1, the composite layer 10 is divided into three band-shaped regions by a first imaginary line VL1 extending parallel to the main surface 100a and a second imaginary line VL2 extending parallel to the main surface 100b. The three band-shaped regions are arranged in the order of a first region 80, a central region 85, and a second region 90 from the first aluminum layer 20 toward the second aluminum layer 30. The first imaginary line VL1 is drawn at a position 200 μm toward the interior of the composite layer 10 from a first boundary line 82 between the first aluminum layer 20 and the composite layer 10. The second imaginary line VL2 is drawn at a position 200 μm toward the interior of the composite layer 10 from a second boundary line 92 between the second aluminum layer 30 and the composite layer 10.

[0043] The first region 80 defined by the first boundary line 82 and the first virtual line VL1 is a strip-shaped region extending 200 μm from the first boundary line 82 between the first aluminum layer 20 and the composite layer 10 toward the interior of the composite layer 10. The second region 90 defined by the second boundary line 92 and the second virtual line VL2 is a strip-shaped region extending 200 μm from the second boundary line 92 between the second aluminum layer 30 and the composite layer 10 toward the interior of the composite layer 10. The central region 85 is a strip-shaped region defined by the first virtual line VL1 and the second virtual line VL2. That is, the central region 85 is located between the first region 80 and the second region 90. The presence of the central region 85 is not essential, and the first virtual line VL1 and the second virtual line VL2 may overlap. That is, the thickness of the composite layer 10 may be 400 μm or more. The thickness of the composite layer 10 (the length in the stacking direction) may be 1000 μm or more, or 3000 μm or more.

[0044] The cut surface of the aluminum-diamond composite 100 can be obtained by cutting along the stacking direction (direction perpendicular to the main surfaces 100a, 100b) of the first aluminum layer 20, composite layer 10, and second aluminum layer 30. The cutting may be performed by water jet processing, laser processing, or the like, or may be performed manually by an operator. There are no particular restrictions on the cutting position, and it may be anywhere as long as it is a portion comprising the first aluminum layer 20, composite layer 10, and second aluminum layer 30. However, in order to obtain the average values ​​α and β described below, it is preferable to observe four or more cut surfaces.

[0045] The cut surface of the aluminum-diamond composite 100 is obtained by processing using a cross-section polisher (manufactured by JEOL Ltd.). By observing such a cut surface using a scanning electron microscope (SEM), average values ​​such as α and β can be obtained. The magnification of the SEM may be 50 to 100 times, or may be 60 to 90 times.

[0046] 2 is an enlarged cross-sectional view of the boundary between the first aluminum layer 20 and the first region 80 in the cross section shown in FIG. 1 . The first boundary line 82 is a tangent line parallel to the main surface 100a, tangent to the outer edge A of the diamond particle 84 closest to the first aluminum layer 20 among the diamond particles 84 dispersed in the aluminum phase 86 of the composite layer 10. The first boundary line 82 may be tangent to the outer edges of multiple diamond particles 84 as long as it is parallel to the main surface 100a. The second boundary line 92, like the first boundary line 82, is a tangent line parallel to the main surface 100b, tangent to the outer edge of the diamond particle 84 closest to the second aluminum layer 30 among the diamond particles 84 in the composite layer 10. The first boundary line 82 and the second boundary line 92 may be drawn by image analysis or visually drawn on an SEM photograph.

[0047] Among the plurality of diamond particles in the first region 80 and the second region 90 of the cut surface, 2000 μm 2 Those with an area of ​​2000 μm or more are coarse particles, 2 Those having an area of ​​less than 1 / 2 are considered to be fine particles. The areas and numbers of coarse and fine particles are measured in the first region 80 and second region 90 of four or more cut surfaces, and the average values ​​α and β are determined using the following procedure. The area and number of diamond particles in the cut surface can be determined by image analysis. For image analysis, for example, "ImageJ" can be used. When a diamond particle exists across the first region 80 and the central region 85, the portion included in the first region 80 is considered to be the area of ​​the diamond particle. Whether the particle is a fine particle or a coarse particle is determined based on this area. A diamond particle existing across the first region 80 and the central region 85 is also considered to be one particle included in the first region 80. The same applies to the second region 90.

[0048] For each of the four or more cut surfaces, the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles 84 in the first region 80 and the second region 90 is determined. The average value α (weighted average) of this ratio for the four or more cut surfaces is 65 to 80%. The average value α may be 70 to 78%, or 72 to 77%. With such an average value α, the diamond coarse particles are sufficiently densely dispersed in the aluminum phase, and the thermal conductivity of the aluminum-diamond composite 100 can be sufficiently high.

[0049] The absolute value of the difference between the average value α1 in the first region 80 and the average value α2 in the second region 90 may be 6.0% or less, 2.5% or less, or 0.5% or less. If the absolute value of the difference between the average value α1 in the first region 80 and the average value α2 in the second region 90 is within the above range, the diamond particles are dispersed with sufficiently high uniformity throughout the composite layer 10, thereby further improving the thermal conductivity of the aluminum-diamond composite 100. Furthermore, the absolute value of the difference between the above average values ​​α1 and α2 may be 0% or more.

[0050] For each of the four or more cut surfaces, the ratio of the number of coarse particles to the number of diamond particles in the first region 80 and the second region 90 is determined. The average value β (weighted average) of the ratios for the four or more cut surfaces may be 2.0% or less, or may be 1.5% or less. With such an average value β, fine particles are dispersed between the coarse diamond particles, improving the density and further improving the thermal conductivity of the aluminum-diamond composite 100. The average value β may also be 1.0% or more.

[0051] The absolute value of the difference between the average value β1 in the first region 80 and the average value β2 in the second region 90 may be 0.6% or less, or may be 0.3% or less. If the absolute value of the difference between the average value β1 in the first region 80 and the average value β2 in the second region 90 is within the above range, the diamond particles are dispersed with high uniformity throughout the composite layer 10, and the thermal conductivity of the aluminum-diamond composite 100 can be further improved. Furthermore, the absolute value of the difference between the average values ​​β1 and β2 may be 0% or more.

[0052] The aluminum-diamond composite 100 has excellent thermal conductivity because the diamond particles are densely packed in the aluminum phase. The thermal conductivity of the aluminum-diamond composite 100 at 25°C may be 500 W / (m·K) or more, or may be 550 W / (m·K) or more. The thermal conductivity at 25°C may be 650 W / (m·K) or less, or may be 600 W / (m·K) or less. The thermal conductivity can be measured by a laser flash method. For example, an "LF / TCM-8510B" (trade name, manufactured by Rigaku Denki Co., Ltd.) or the like can be used to measure the thermal conductivity.

[0053] A method for producing an aluminum-diamond composite according to one embodiment includes a mixing step in which coarse and fine diamond particles are mixed using a V-type mixer to obtain a mixture, and a heating step in which the obtained mixture is heated while sandwiched between aluminum foils.

[0054] The coarse and fine diamond particles used as raw materials can be those described above. In the mixing step, the coarse and fine diamond particles are fed into a V-type mixer. By using a V-type mixer, the average value α can be set to 65 to 80%. Furthermore, the average value β can be set to 2.0% or less. The mass ratio of the coarse particles to the total mass of the diamond particles fed may be 60% by mass or more, 70% by mass or more, or 90% by mass or less. The numerical range of the mass ratio of the coarse particles to the total mass of the diamond particles fed may be, for example, 60 to 90% by mass, or 70 to 90% by mass. Furthermore, the mass ratio of the fine particles to the total mass of the diamond particles may be 40% by mass or less, 30% by mass or less, or 10% by mass or more. The numerical range of the mass ratio of the fine particles to the total mass of the diamond particles may be, for example, 10 to 30% by mass, or 10 to 40% by mass. A mixture in which the mass ratio of coarse particles to fine particles falls within the above range can contain the coarse particles and fine particles with sufficiently high uniformity, thereby increasing the thermal conductivity of the aluminum-diamond composite.

[0055] The total volume of the V-type mixer is, for example, 0.1 to 5.0 m 3 0.5 to 3.0 m 3 may be used. The V-type mixer may be, for example, "V-10" (trade name, manufactured by Tokuju Machinery Co., Ltd.). The volume ratio of the diamond particles introduced to the total volume of the V-type mixer may be 10 to 50%, 15 to 40%, or 20 to 40%. By introducing the diamond particles at such a volume ratio, the efficiency of mixing is improved, and the difference between the average values ​​α1 and α2, and the difference between the average values ​​β1 and β2 can be sufficiently reduced. This makes it possible to obtain a mixture with even higher uniformity, and to further increase the thermal conductivity of the aluminum-diamond composite.

[0056] In the mixing step, the rotation speed of the V-type mixer may be 15 to 50 rpm, or may be 20 to 40 rpm. The rotation time of the V-type mixer may be 5 to 30 minutes, or may be 10 to 20 minutes. By adjusting the rotation speed and rotation time of the V-type mixer within this range, the difference between the average values ​​α1 and α2, and the difference between the average values ​​β1 and β2 can be sufficiently reduced. This makes it possible to obtain a mixture with even higher uniformity, and to further increase the thermal conductivity of the aluminum-diamond composite.

[0057] The heating step will be described below with reference to Figures 3 and 4. Before the heating step, a block formation step may be included in which a structure 101 including a laminated structure 40 in which a first release plate 6a, an aluminum layer 22, a diamond particle mixture layer 21, an aluminum layer 22, and a second release plate 6b are laminated in this order within a space surrounded by two metal plates 60 and a porous material 50, as shown in Figures 3 and 4.

[0058] In Figure 3, the openings in the porous material 50 are through-holes that penetrate in the vertical direction. However, the openings are not limited to through-holes, and may be, for example, recesses having an opening on one main surface side of the porous material 50. Furthermore, from the viewpoint of obtaining a more homogeneous aluminum-diamond composite 100, it is desirable that one opening be provided in the center of the porous material 50, but this is not particularly limited. For example, multiple openings may be provided in one porous material 50, and the positions at which the openings are formed may also be adjusted as appropriate. In the following explanation, an example will be described in which the openings are through-holes, but if the openings are recesses, this may be interpreted as one of the metal plates 60 in Figures 3 and 4 being integral with the porous material 50 and made of the same material.

[0059] The block formation process is a process of providing a laminated structure 40 inside an opening of a porous material 50, which is a frame material placed between two metal plates 60 and serves as a mold for the aluminum-diamond composite 100, by providing a gap S so as to be spaced from the inner peripheral surface 50a of the opening of the porous material 50. The method of providing the laminated structure 40 inside the opening of the porous material 50 is not particularly limited. For example, the porous material 50 may be placed on the metal plate 60, and then the layers constituting the laminated structure 40 may be sequentially laminated, or a method in which a separately formed laminated structure 40 is inserted inside the opening of the porous material 50 may be used. A method of providing the gap S (distance g) between the inner peripheral surface 50a of the opening of the porous material 50 and the outer peripheral surface of the laminated structure 40 may be, for example, a method in which a removable spacer of a predetermined thickness is provided so as to be in contact with the inner peripheral surface 50a of the opening, and the laminated structure 40 is formed or inserted inside the spacer (the space on the opposite side from the porous material 50), and then the spacer is removed. Although Figures 3 and 4 show an example in which one laminated structure 40 is provided, multiple laminated structures 40 may be stacked inside the opening of the porous material 50 along the thickness direction of the porous material 50.

[0060] The distance g between the inner peripheral surface 50a of the opening of the porous material 50 and the outer peripheral surface of the laminated structure 40 can be adjusted according to the thickness of the metal layer to be formed on the side surface of the intended aluminum-diamond composite 100. The distance g between the inner peripheral surface 50a of the opening of the porous material 50 and the outer peripheral surface of the laminated structure 40 may be, for example, 0.05 to 3.50 mm, 0.05 to 2.50 mm, or 0.05 to 1.00 mm.

[0061] Examples of the metal plate 60 include an iron plate and a stainless steel plate.

[0062] The porous material 50 may have heat resistance that allows a molten aluminum-containing metal to be injected or infiltrated into it in the heating step described below. The porous material 50 may be, for example, a porous sintered body made of graphite or boron nitride (e.g., an isotropic graphite mold material, etc.), or a porous body made of alumina fibers. The shape of the openings in the porous material 50 can be adjusted according to the desired shape of the aluminum-diamond composite 100. In the manufacturing method of this embodiment, the shape of the aluminum-diamond composite 100 can be changed by adjusting the shape of the openings in the porous material 50. This allows for greater design freedom than conventional methods using laser processing or other methods for forming.

[0063] The laminated structure 40 formed in the block forming step includes a first release plate 6a, an aluminum layer 22, a mixture layer 21, an aluminum layer 22, and a second release plate 6b in this order.

[0064] The mixture layer 21 can be a mixture of diamond particles obtained in the above-mentioned mixing step. The mixture layer 21 may be composed of, for example, diamond particles alone, or may contain other components. The other components may be, for example, a binder such as silica. When the mixture layer 21 contains other components, the content of the other components may be, for example, 0.5 to 3.0 mass % based on the total amount of the mixture layer 21.

[0065] The aluminum layer 22 may include inorganic fibers, such as alumina fibers, glass fibers, etc. The aluminum layer 22 may be, for example, aluminum foil, aluminum alloy foil, etc.

[0066] The thickness of the aluminum layer 22 may be, for example, 0.01 mm or more, 0.02 mm or more, or 0.03 mm or more. By ensuring that the lower limit of the thickness of the aluminum layer 22 is within the above range, it is possible to more effectively prevent the diamond powder from being exposed on the surface of the aluminum-diamond composite 100. The thickness of the aluminum layer 22 may be, for example, 0.20 mm or less, 0.15 mm or less, 0.10 mm or less, 0.08 mm or less, or 0.06 mm or less. By ensuring that the upper limit of the thickness of the aluminum layer 22 is within the above range, it is possible to sufficiently prevent a decrease in the thermal conductivity of the resulting aluminum-diamond composite 100 in the thickness direction. The thickness can be adjusted within the above range and may be, for example, 0.01 to 0.20 mm or 0.02 to 0.15 mm. The thickness of the aluminum layer 22 can be measured using a micrometer and is the arithmetic average of values ​​measured at five points within the surface. The pair of aluminum layers 22 sandwiching the mixture layer 21 may have different thicknesses or may have the same thickness.

[0067] The first release plate 6a and the second release plate 6b can be plates having a dense structure so that sufficient pressure can be applied when the aluminum-containing metal melt is pressed into the mixture layer 21 and impregnated therein in the heating step described below. The first release plate 6a and the second release plate 6b can be, for example, a stainless steel plate, a ceramic plate, or the like. The main surfaces of the first release plate 6a and the second release plate 6b facing the mixture layer 21 may be coated with a release agent or may be subjected to a release treatment. Examples of such release agents include graphite, boron nitride, and alumina. The first release plate 6a and the second release plate 6b can be, for example, release plates formed by forming a coating layer of alumina sol or the like on the main surfaces facing the mixture layer 21, followed by further application of a release agent. The use of such release plates allows for more stable release, and the main surfaces of the resulting aluminum-diamond composite 100 can be made smoother.

[0068] The heating step can be carried out by impregnating the above-described structure 101 with a melt of aluminum-containing metal. The temperature of the melt may be 600 to 1500°C, or may be 700 to 1300°C. As a result, the melt of metal is supplied to the inside and surface of the mixture layer 21 via the porous material 50. As a result, as shown in FIG. 4, an aluminum-diamond composite 100 (FIG. 1) is formed in the structure 102, having a composite layer 10 containing aluminum and diamond, a first aluminum layer 20, and a second aluminum layer 30. Furthermore, a metal layer 24 can be formed on the side surface of the aluminum-diamond composite 100. A method for forming the aluminum-diamond composite 100 will be specifically described below.

[0069] In the heating step, in addition to the metal layer 24, a molten material of a metal containing aluminum may penetrate into the interior of the aluminum layer 22 or onto the main surface of the aluminum layer 22 on the mixture layer 21 side, thereby forming the first aluminum layer 20 and the second aluminum layer 30. The aluminum layer 22 itself constitutes a metal-containing layer, and the molten material of a metal containing aluminum penetrates onto the main surface of the aluminum layer 22 on the mixture layer 21 side, thereby firmly bonding the composite layer 10 to the first aluminum layer 20 and the second aluminum layer 30.

[0070] In the heating step, the method for supplying the molten aluminum-containing metal may be, for example, a so-called high-pressure forging method, in which the molten metal is impregnated into the object under high pressure. From the viewpoint of obtaining an aluminum-diamond composite 100 with superior thermal conductivity, it is desirable to use a molten metal forging method. The heating step is carried out, for example, by immersing the structure 101 obtained in the block formation step in a container filled with the molten metal and applying pressure to the molten metal. This allows the molten metal to permeate through the pores of the porous material 50 and be supplied between the inner circumferential surface 50a of the opening of the porous material 50 and the outer circumferential surface of the laminated structure. The molten metal then penetrates into the interior of the mixture layer 21, thereby obtaining the composite layer 10.

[0071] The aluminum-containing metal melt may contain, for example, other metals in addition to aluminum. Examples of other metals include silicon, magnesium, and copper. The other metal preferably contains at least one of silicon and magnesium. By including the above-mentioned metals in the melt, the melting point of the melt can be lowered and the melt viscosity during impregnation can be reduced, allowing the melt to sufficiently penetrate into the voids formed between the diamond powder particles in the mixture layer 21. This action can further improve the density of the composite layer 10 in the resulting aluminum-diamond composite 100. When the melt contains silicon, the melting point can be further lowered, and when the melt contains magnesium, the bond between the composite layer 10 and the aluminum layer can be stronger.

[0072] When the melt contains other metals in addition to aluminum, the content of the other metals may be 2 to 20 mass %, 2 to 15 mass %, or 5 to 15 mass %, based on the total mass of the melt.

[0073] When impregnating the molten material, it is desirable to preheat the structure 101. The lower limit of the heating temperature in preheating may be, for example, 520°C or higher, or 540°C or higher. By setting the lower limit of the heating temperature within the above range, the molten material can be more easily impregnated into the mixture layer 21, and the impregnation of the metal in the heating step can be more stably carried out. The upper limit of the heating temperature may be, for example, 750°C or lower, or 700°C or lower. By setting the upper limit of the heating temperature in preheating within the above range, it is possible to prevent the formation of aluminum carbide (Al 4 C 3 ) can be further suppressed, thereby further improving the thermal conductivity of the aluminum-diamond composite 100. The heating temperature may be adjusted within the above-mentioned range, and can be set to, for example, 520 to 750°C or 540 to 700°C.

[0074] The pressure when the molten material is impregnated into the mixture layer 21 may be, for example, 20 MPa or more, 30 MPa or more, 40 MPa or more, or 50 MPa or more. By setting the lower limit of the pressure when the molten material is impregnated into the mixture layer 21 within the above range, the compounding in the heating step can be carried out more stably, and the thermal conductivity of the resulting aluminum-diamond composite 100 can be further improved. The pressure when the molten material is impregnated into the mixture layer 21 may be, for example, 150 MPa or less, 100 MPa or less, or 80 MPa or less. The pressure when the molten material is impregnated into the mixture layer 21 may be adjusted within the above range, and may be, for example, 20 to 150 MPa.

[0075] After the heating step, the metal plate 60, porous material 50, first release plate 6a, and second release plate 6b are removed from the structure 102, and the aluminum-diamond composite 100 as shown in Figure 1 can be taken out. The aluminum-diamond composite 100 may be cut out from the structure 102 by water jet processing, laser processing, or the like. In order to smooth the surface of the obtained aluminum-diamond composite 100, a surface treatment may be carried out. The surface treatment can be carried out by a processing method employed in ordinary metal processing, for example, polishing, surface grinding, or the like.

[0076] The obtained aluminum-diamond composite 100 may be subjected to an annealing step. In the annealing step, heat treatment is performed at a relatively low temperature after the heating step to reduce distortion that may exist in the composite layer 10, the first aluminum layer 20, the second aluminum layer 30, the metal layer 24, etc. This step makes it possible to produce an aluminum-diamond composite 100 with superior thermal conductivity. The heating temperature in the annealing step may be, for example, 400 to 550°C, or 400 to 500°C. The heating time in the annealing step may be, for example, 10 minutes or more, or 20 minutes or more, and may be 24 hours or less, or 12 hours or less.

[0077] FIG. 5 shows an example of a semiconductor package using a heat dissipation member containing an aluminum-diamond composite 100. The semiconductor package of FIG. 5 can be obtained by bonding a semiconductor element 8 to a heat dissipation member 2, bonding an insulating member 1 and a lid member 5 to each other so as to surround the semiconductor element 8, and bonding the insulating member 1 to the heat dissipation member 2. The semiconductor package is connected to an external terminal (not shown) via a conductor 6. The heat dissipation member 2 and the semiconductor element 8 are bonded via a bonding material 7. The lower surfaces of the heat dissipation member 2 and the insulating member 1 are bonded via a bonding material 3. The upper surface of the insulating member 1 and the lid member 5 are bonded via a bonding material 4. For example, alumina, aluminum nitride, silicon nitride, beryllium oxide, etc. can be used for the insulating member 1. By including an aluminum-diamond composite 100 with high thermal conductivity in the heat dissipation member 2 of such a semiconductor package, a semiconductor package with even improved heat dissipation properties can be obtained.

[0078] Although several embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments. For example, the aluminum-diamond composite 100 may have a metal layer on the side surface of the composite layer 10.

[0079] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited to the following examples.

[0080] (Example 1) Commercially available high-purity diamond powder A (average particle size: 180 μm, manufactured by Saint-Gobain Co., Ltd.) and high-purity diamond powder B (average particle size: 20 μm, manufactured by Saint-Gobain Co., Ltd.) were charged into a V-type mixer (trade name: V-10, manufactured by Tokuju Machine Works Co., Ltd.) so that the mass ratio A:B = 7:3. The volume ratio of diamond particles to the internal volume of the V-type mixer was 17%. The V-type mixer was rotated at a rotation speed of 25 rpm for 10 minutes to mix the diamond powder, and a mixture of diamond powders A and B was obtained. A release plate was produced by coating alumina sol on the surface of a stainless steel plate (SUS430 material) measuring length x width x thickness = 40 mm x 40 mm x 2 mm and baking it at 350 ° C for 30 minutes.

[0081] An isotropic graphite jig with a porosity of 20% was prepared, having an outer shape of length x width x thickness = 60 mm x 60 mm x 8 mm and a through hole of length x width x length = 40 mm x 40 mm x 8 mm in the center. The isotropic graphite jig was placed on a 12 mm thick iron plate with bolt holes at the four corners so that the opening of the through hole was facing upward. A release plate and a 30 μm thick pure aluminum foil (manufactured by UACJ Corporation) were inserted into the through hole from above in this order, and the pure aluminum foil was laminated on the release plate inside the through hole. Furthermore, the diamond powder mixture was filled on this pure aluminum foil to a thickness of 1.24 mm to form a mixture layer, and pure aluminum foil and a release plate were laminated on the mixture layer in this order to form a laminated structure inside the through hole.

[0082] The same procedure was repeated to form six such laminate structures inside the through-holes. Then, a stainless steel plate coated with a graphite-based release agent and measuring 60 mm x 60 mm x 1 mm in length x width x thickness was inserted into the through-holes on top of these laminate structures, and the laminate structures were sandwiched between the pair of stainless steel plates. A 12 mm thick iron plate with bolt holes at the four corners was placed on the isotropic graphite jig to cover the through-holes. The upper and lower iron plates were connected to each other with six M10 bolts and tightened with a torque wrench to a tightening torque of 10 N m in the surface direction, obtaining a single block.

[0083] The obtained block was preheated to a temperature of 650 ° C in an electric furnace and then placed in a preheated press mold with an inner diameter of 300 mm. A molten aluminum alloy containing 12% by mass of silicon and 1% by mass of magnesium at a temperature of 800 ° C was poured into the press mold and pressed at a pressure of 100 MPa for 20 minutes. This resulted in the aluminum alloy being impregnated into the mixture layer to obtain a composite layer containing the aluminum alloy and diamond powders A and B. The block on which the composite layer was formed was cooled to room temperature, then cut along the shape of the release plate with a wet band saw, and the stainless steel plate was peeled off to obtain cut pieces. Thereafter, to remove distortion during impregnation, the cut pieces were subjected to an annealing treatment in which they were heated at a temperature of 400 ° C for 3 hours. Thereafter, the surface of the aluminum layer in the cut pieces was polished with #600 abrasive paper and then buffed. In this way, a laminate comprising a first aluminum layer, a composite layer, and a second aluminum layer in this order was obtained.

[0084] After ultrasonic cleaning of the surface of the laminate, the main surfaces of the first and second aluminum layers were pretreated with a Zn catalyst. The pretreated surfaces of the first and second aluminum layers were sequentially subjected to Ni electroplating, electroless Ni—P plating, and Au electroplating to form a 6 μm-thick (Ni: 2.0 μm + Ni—P: 2.0 μm + Au: 2.0 μm) plating layer on the surface of the aluminum-diamond composite.

[0085] Subsequently, the aluminum-diamond composite of Example 1 was obtained by processing the aluminum-diamond composite into a shape of length×width×thickness=25 mm×25 mm×2 mm using a YAG laser processing machine.

[0086] Examples 2 and 3 Aluminum-diamond composites of Examples 2 and 3 were obtained in the same manner as in Example 1.

[0087] Comparative Example 1 An aluminum-diamond composite of Comparative Example 1 was obtained in the same manner as in Examples 1 to 3, except that the diamond mixture was obtained by manually stirring for 5 minutes by an operator instead of using a V-type mixer.

[0088] (Comparative Example 2) Instead of filling the through-holes of the isotropic graphite jig with a mixture of diamond powders, diamond powder A was placed in the through-holes, and then diamond powder B was placed on top so that the mass ratio was 7:3. Otherwise, the aluminum-diamond composite of Comparative Example 2 was obtained using the same procedures as in Examples 1 to 3.

[0089] [Measurement of Thermal Conductivity] The thermal conductivity of the aluminum-diamond composites of each Example and Comparative Example at 25°C was measured using a laser flash method (product name: LF / TCM-8510B, manufactured by Rigaku Corporation). The results are shown in Tables 2 and 4.

[0090] [Calculation of area ratio and particle number ratio of diamond particles in cross section] The aluminum-diamond composite of each example and each comparative example was cut at four locations along a direction perpendicular to the main surfaces of the first aluminum layer and the second aluminum layer using a YAG laser processing machine to obtain four cut surfaces. The cut surfaces were polished using a cross-section polisher, and each cut surface was observed at 70x magnification using a scanning electron microscope (SEM). Figure 6 is an SEM photograph showing the cut surface of No. 1 of Example 1. Figure 7 is an SEM photograph showing the cut surface of No. 2 of Example 1. Figure 8 is an SEM photograph showing the cut surface of No. 3 of Example 1. Figure 9 is an SEM photograph showing the cut surface of No. 4 of Example 1. As shown in Figures 6 to 9, a composite layer of the aluminum-diamond composite was present, sandwiched between the first aluminum layer and the second aluminum layer. In addition, in the composite layer, coarse and fine diamond particles were dispersed in the aluminum phase.

[0091] The first region was defined as the area from the first boundary line between the first aluminum layer and the composite layer in the obtained SEM image to the area 200 μm into the composite layer. As shown in FIG. 2, the first boundary line is a tangent line that contacts the outer edge A of the diamond particle 84 located closest to the first aluminum layer 20 and is drawn parallel to the main surface of the first aluminum layer 20. The second region was defined as the area from the second boundary line between the second aluminum layer and the composite layer to the area 200 μm into the composite layer. The second boundary line is a tangent line that passes through the outer edge of the diamond particle located closest to the second aluminum layer and is drawn parallel to the main surface of the second aluminum layer.

[0092] Image analysis of the first and second regions of each cut surface was performed using ImageJ. 2 Diamond particles having an area of ​​2000 μm or more are called coarse particles. 2 Diamond particles having an area of ​​less than 1 / 2 mm were defined as fine particles. The areas and numbers of coarse particles and fine particles were measured in each of the first and second regions. The results are shown in Tables 1 and 3.

[0093] Tables 1 and 2 show the total area of ​​diamond particles in each region, the ratio of the total area of ​​coarse particles to that total area, as well as the average values ​​(α1, α2) of that ratio for the first region and the second region, the average value α of that ratio for both the first region and the second region combined, and the absolute value of the difference between the average value α1 of the first region and the average value α2 of the second region.

[0094] Tables 3 and 4 show the number of diamond particles in each cut surface (total X), the ratio of the number of coarse particles to the total X, the average value of the ratio for each of the first and second regions (β1, β2), the average value β of the ratio for both the first and second regions combined, and the absolute value of the difference between the average value β1 of the first region and the average value β2 of the second region.In addition, in Tables 1 to 4, among No. 1 to 4 of one example, those with the same No. indicate the results of the first region and the second region on the same cut surface.

[0095]

[0096]

[0097]

[0098]

[0099] As shown in Tables 2 and 4, the aluminum-diamond composites using the diamond powder mixtures of Examples 1 to 3 had higher thermal conductivities than Comparative Examples 1 and 2. Furthermore, as shown in Table 2, when comparing the average values ​​α of the area ratios of coarse particles in the first and second regions of each aluminum-diamond composite, Examples 1 to 3 were 73.7% to 77.9%. Meanwhile, the average value α of Comparative Example 1 was high at 80.7%, while the average value α of Comparative Example 2 was low at 48.8%. Furthermore, as shown in Table 4, in Examples 1 to 3, the average value β of the ratio of the number of coarse particles to the total number of diamond particles calculated for each region was 2.0% or less. Thus, it was confirmed that the aluminum-diamond composites of Examples 1 to 3 had diamond particles with high thermal conductivity dispersed appropriately within the aluminum phase.

[0100] According to the present disclosure, it is possible to provide an aluminum-diamond composite having sufficiently high thermal conductivity, and a method for producing the same. Furthermore, it is possible to provide a semiconductor package having excellent heat dissipation properties by including such an aluminum-diamond composite.

[0101] 100...aluminum-diamond composite, 100a, 100b...main surface, 20...first aluminum layer, 30...second aluminum layer, 10...composite layer, 80...first region, 85...central region, 90...second region, 82...first boundary line, 92...second boundary line, VL1...first virtual line, VL2...second virtual line, 84...diamond particle, 86...aluminum phase, A...outer edge, 21...mixture layer, 22...aluminum layer, 40...laminated structure, 50...porous material, 60...metal plate, 50a...inner surface, S...gap, g...distance, 24...metal layer, 101, 102...structure, 1...insulating member, 2...heat dissipation member, 3, 4, 7...bonding material, 5...lid material, 6...conductor, 6a...first release plate, 6b...second release plate, 8...semiconductor element.

Claims

1. An aluminum-diamond composite having a laminated structure including a composite layer containing an aluminum phase and a plurality of diamond particles having different sizes, and a pair of aluminum layers sandwiching the composite layer, wherein, in a cut surface obtained by cutting along the lamination direction, the plurality of diamond particles are 2000 μm or less in size. 2 Coarse particles having an area of ​​2000 μm or more and 2 and fine particles having an area of ​​less than 100 μm, wherein an average value α of a ratio of a total area of ​​the coarse particles to a total area of ​​the plurality of diamond particles in a region extending from a boundary line between the pair of aluminum layers and the composite layer to 200 μm inside the composite layer is 65 to 80%.

2. An aluminum-diamond composite as described in claim 1, wherein in said region, an average value β of the ratio of the number of said coarse particles to the number of said plurality of diamond particles is 2.0% or less.

3. The aluminum-diamond composite according to claim 2, wherein the region includes a first region which is a region extending from the boundary between one of the pair of aluminum layers and the composite layer to 200 μm toward the inside of the composite layer, and a second region which is a region extending from the boundary between the other of the aluminum layers and the composite layer to 200 μm toward the inside of the composite layer, and the absolute value of the difference between an average value β1 of the ratio of the number of the coarse particles to the number of the plurality of diamond particles in the first region and an average value β2 of the ratio of the number of the coarse particles to the number of the plurality of diamond particles in the second region is 0.6% or less.

4. The aluminum-diamond composite according to any one of claims 1 to 3, wherein the region includes a first region which is a region extending from the boundary between one of the pair of aluminum layers and the composite layer to 200 μm toward the inside of the composite layer, and a second region which is a region extending from the boundary between the other of the aluminum layers and the composite layer to 200 μm toward the inside of the composite layer, and the absolute value of the difference between the average value α1 of the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles in the first region and the average value α2 of the ratio of the total area of ​​the coarse particles to the total area of ​​the plurality of diamond particles in the second region is 6.0% or less.

5. A method for producing an aluminum-diamond composite, comprising: a mixing step in which coarse and fine diamond particles of different sizes are mixed using a V-type mixer to obtain a mixture containing a plurality of diamond particles; and a heating step in which the mixture is heated while sandwiched between aluminum foil to obtain a layered structure comprising a composite layer containing an aluminum phase and the mixture, and a pair of aluminum layers sandwiching the composite layer.

6. In a cut surface obtained by cutting the aluminum-diamond composite along the lamination direction, the plurality of diamond particles are 2000 μm 2 The coarse particles having an area of ​​2000 μm or more, 2 and the fine particles have an area of ​​less than 100 μm, and an average value α of a ratio of a total area of ​​the coarse particles to a total area of ​​the plurality of diamond particles in a region from a boundary line between the pair of aluminum layers and the composite layer to 200 μm inside the composite layer is 65 to 80%.

7. The method for producing an aluminum-diamond composite according to claim 5 or 6, wherein the mixing step includes rotating the V-type mixer at a rotation speed of 15 to 50 rpm for 5 to 30 minutes.

8. The method for producing an aluminum-diamond composite according to claim 5 or 6, wherein in the mixing step, the ratio of the volume of the plurality of diamond particles to the total volume of the V-type mixer is 10 to 50%.

9. A semiconductor package comprising a heat dissipation member containing the aluminum-diamond composite according to any one of claims 1 to 3, and a semiconductor element bonded to the heat dissipation member.

Citation Information

Patent Citations

  • Aluminum-diamond-based complex heat dissipation component

    JP2014107468A

  • Semiconductor package and method for manufacturing same

    WO2015182576A1

  • Semiconductor light emitting device

    JP2022002266A

  • Heat dissipating component for semiconductor element

    WO2013015158A1

  • Heat dissipation member and electronic device

    WO2023013500A1