Thermally conductive composition, two-component curable thermally conductive material, supply form of two-component curable thermally conductive material, and battery module
The thermally conductive composition with a specific viscosity ratio and structural viscosity imparting agent addresses sedimentation and handleability issues by maintaining high viscosity at low shear and reducing it under high shear, ensuring efficient thermal conductivity and uniform composition.
Patent Information
- Application Number
- PCT/JP2024/016292
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Thermally conductive compositions with epoxy compounds and fillers face issues like filler sedimentation and phase separation during storage, leading to quality deterioration and poor handleability due to low viscosity and separation of components.
A thermally conductive composition with a viscosity ratio of 60 or more, comprising an epoxy compound, a thermally conductive filler, and a structural viscosity imparting agent, which suppresses filler sedimentation and improves handleability by forming a loose bond that breaks under shear stress, allowing for easy application and curing.
The composition effectively prevents filler sedimentation during storage and enhances handleability by maintaining a high viscosity at low shear rates and reducing viscosity under high shear, ensuring uniform composition and improved thermal conductivity.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Thermally conductive composition, two-component curing thermally conductive material, supply form of two-component curing thermally conductive material, and battery module
[0001] The present invention relates to a thermally conductive composition, a two-component curing thermally conductive material, a supply form of the two-component curing thermally conductive material, and a battery module.
[0002] A thermally conductive composition containing a thermally conductive filler is filled between a heat generating element and a heat sink, and then cured to form a cured product, which is used as a thermally conductive member that transfers heat generated by the heat generating element to the heat sink. Because the thermally conductive composition is fluid, it can fill any gap between the heat generating element and the heat sink, reliably filling the gap even if the gap between the heat generating element and the heat sink is not uniform. This allows the composition to be used as a gap filler in battery modules, etc. Furthermore, a thermally conductive member formed from the thermally conductive composition can be placed between a battery cell, which is a heat generating element, and a module housing, which is a heat sink, to dissipate heat from the battery cell to the outside, and can also be placed between battery cells to secure them and maintain their separation. Such thermally conductive compositions are generally desired to have workability, allowing them to be discharged from a cartridge or syringe at a sufficient speed, storage stability, preventing settling of the thermally conductive filler during storage, compressibility (handling ease), allowing them to be pressed against an object of use such as a battery cell without stress, and sufficient thermal conductivity and adhesiveness after curing.
[0003] Patent Document 1 describes an invention relating to a thermally conductive composition having high thermal conductivity, which comprises a trifunctional or higher epoxy resin (epoxy compound) that does not have an aromatic skeleton, a liquid bifunctional or lower epoxy compound, a curing agent, a silane compound that does not have any functional groups other than alkoxy groups, and a specific thermally conductive filler.
[0004] Japanese Patent Application Laid-Open No. 2022-116587
[0005] In a thermally conductive composition containing an epoxy compound and a thermally conductive filler, as in the invention described in Patent Document 1, if a low-viscosity epoxy compound is used to improve workability and handleability, there are problems such as sedimentation of the thermally conductive filler during storage or liquid phase separation of the epoxy compound, resulting in a decrease in quality. Therefore, the object of the present invention is to provide a thermally conductive composition containing a curable compound selected from an epoxy compound and an epoxy curing agent, and a thermally conductive filler, which can suppress sedimentation of the thermally conductive filler during storage and has excellent handleability during use.
[0006] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, they have found that the above-mentioned problems can be solved by a thermally conductive composition containing at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent, wherein the thermally conductive composition has a viscosity ratio of at least a certain level under specific conditions measured with a rheometer, and thus completed the present invention. Specifically, the present invention provides the following [1] to
[14] .
[0007] [1] A thermally conductive composition comprising at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent, wherein the viscosity ratio (η1 / η3) between the viscosity η1 measured with a rheometer at 25°C and a shear rate of 0.0001 (1 / s) and the viscosity η3 measured at 25°C and a shear rate of 0.0251 (1 / s) is 60 or more. [2] The thermally conductive composition according to [1] above, wherein the viscosity η2 measured at 25°C and a shear rate of 25.1 (1 / s) is 125 Pa s or less. [3] The thermally conductive composition according to [1] or [2] above, wherein the structural viscosity imparting agent is a compound having a melting point above 25°C. [4] The thermally conductive composition according to any one of [1] to [3] above, wherein the structural viscosity imparting agent is an ester compound having a melting point above 25°C and not more than 120°C. [5] The thermally conductive composition according to any one of [1] to [4] above, wherein the curable compound is an epoxy compound. [6] The thermally conductive composition according to any one of [1] to [4] above, wherein the curable compound is an epoxy curing agent. [7] The thermally conductive composition according to [6] above, wherein the epoxy curing agent is an amine compound. [8] A two-component curing thermally conductive material comprising a first part consisting of the thermally conductive composition according to [5] above and a second part consisting of the thermally conductive composition according to [6] above. [9] A supply form of a two-component curing thermally conductive material comprising a first container filled with a first part consisting of a thermally conductive composition containing an epoxy compound, a thermally conductive filler, and a structural viscosity imparting agent, and a second container filled with a second part consisting of a thermally conductive composition containing an epoxy curing agent, a thermally conductive filler, and a structural viscosity imparting agent, wherein each of the first and second parts has a viscosity ratio (η1 / η3) of 60 or more between the viscosity η1 measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) and the viscosity η3 measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s).
[10] A thermally conductive member that is a cured product of the thermally conductive composition described in any of [1] to [7] above.
[11] A thermally conductive member that is a cured product of the two-component curing thermally conductive material described in [8] above.
[12] A battery module comprising: a gap filler made of the thermally conductive member according to
[10] or
[11] above, a plurality of battery cells, and a module housing for storing the plurality of battery cells, the gap filler being disposed inside the module housing.
[13] A method for producing a thermally conductive composition, comprising the steps of: preparing a mixture containing at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent; heating the mixture; and cooling the mixture to adjust the viscosity ratio (η1 / η3) of the mixture measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) to the viscosity η3 of the mixture measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s) to be 60 or more.
[14] A method for producing a supply form of a thermally conductive composition, the method comprising the steps of: preparing a mixture containing at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent; filling the mixture into a container; heating the mixture; and cooling the mixture to adjust the viscosity ratio (η1 / η3) of the mixture measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) to the viscosity η3 of the mixture measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s) to be 60 or more.
[0008] According to the present invention, it is possible to provide a thermally conductive composition that can suppress sedimentation of a thermally conductive filler during storage and that is easy to handle during use.
[0009] 1 is a schematic diagram showing a container set according to an embodiment; FIG. 2 is a schematic diagram showing a container set according to an embodiment; FIG. 3 is a perspective view showing a typical configuration of a battery module according to the present invention; FIG. 4 is a perspective view showing a typical configuration of a battery cell included in the battery module; FIG. 5 is a perspective view showing a battery assembly having a cell-to-pack structure;
[0010] [Thermal Conductive Composition] The thermally conductive composition of the present invention will be described in detail below. The thermally conductive composition of the present invention includes at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent. The thermally conductive composition of the present invention has a viscosity ratio (η1 / η3) of 60 or more between the viscosity η1 measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) and the viscosity η3 measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s).
[0011] <Viscosity Ratio> The thermally conductive composition of the present invention has a viscosity ratio (η1 / η3) measured with a rheometer of 60 or more. If the viscosity ratio (η1 / η3) is less than 60, the thermally conductive filler is likely to settle during storage of the thermally conductive composition, which tends to deteriorate the handleability during use. Note that the handleability during use refers to a physical property equivalent to the compressibility evaluated in the examples described below. From the viewpoint of suppressing the settling of the thermally conductive filler during storage and improving the handleability during use, the viscosity ratio (η1 / η3) of the thermally conductive composition measured with a rheometer is preferably 70 or more, more preferably 80 or more, even more preferably 100 or more, and even more preferably 140 or more. The upper limit of the viscosity ratio (η1 / η3) is not particularly limited, but is, for example, 500. The adjustment of the viscosity ratio (η1 / η3) will be described in detail later, but when the thermally conductive composition contains a structural viscosity imparting agent and undergoes a heating and cooling treatment to form loose bonds (internal structure) due to cohesive forces, which will be described later, the viscosity ratio (η1 / η3) measured with a rheometer becomes 60 or more. In this specification, the range indicated by "to" means a range from a specified numerical value or more to a specified numerical value or less, which is stated before and after "to".
[0012] Although the reason why adjusting the viscosity ratio (η1 / η3) as described above can suppress sedimentation of the thermally conductive filler during storage of the thermally conductive composition and improve handleability during use is unclear, it is presumed as follows. Both viscosities η1 and η3 represent the viscosity in the low shear rate region. When the viscosity ratio (η1 / η3) of the thermally conductive composition is 60 or higher, the change in viscosity relative to changes in shear rate in the low shear rate region becomes large. In other words, the slope of the graph showing the relationship between shear rate (horizontal axis) and viscosity (vertical axis) becomes steep. This means that the viscosity of the thermally conductive composition increases in the storage state, i.e., when the shear rate is extremely low, which is thought to suppress sedimentation of the thermally conductive filler. Furthermore, when the thermally conductive composition is used after storage, the shear rate becomes relatively high, for example, due to application of the thermally conductive composition using a dispenser or compression of the applied product. In this case, the viscosity of the thermally conductive composition effectively decreases as the shear rate increases, which is thought to result in excellent handleability.
[0013] In the present invention, since it is important to adjust the viscosity ratio (η1 / η3) as described above, the individual values of the viscosities η1 and η3 are not particularly limited, but from the viewpoint of suppressing sedimentation of the thermally conductive filler, the viscosity η1 is, for example, 50,000 Pa s or more, preferably 100,000 Pa s or more, more preferably 500,000 Pa s or more, and even more preferably 1,000,000 Pa s or more. The upper limit of the viscosity η1 is not particularly limited, but is, for example, 5,000,000 Pa s.
[0014] Furthermore, the viscosity η2 of the thermally conductive composition measured with a rheometer at a measurement temperature of 25°C and a shear rate of 25.1 (1 / s) is preferably 125 Pa s or less, more preferably 100 Pa s or less, and even more preferably 80 Pa s or less, from the viewpoint of increasing compressibility and improving handleability. The lower limit of η2 is not particularly limited, but is, for example, 10 Pa s.
[0015] The viscosities η1, η2, and η3 of the thermally conductive composition are values measured using a rheometer at 25°C. When measuring using a rheometer, the thermally conductive composition is heated and then cooled to room temperature (25°C) to evaluate the composition without considering the influence of shear when the sample is set in the measuring jig. The heating temperature is set to a temperature equal to or higher than the melting point of the structural viscosity imparting agent, preferably equal to or lower than the melting point of the structural viscosity imparting agent + 50°C. The heating temperature may be set appropriately within the range of, for example, 35 to 170°C. Details of the rheometer measurement conditions are described in the Examples. The viscosities η1, η2, and η3 of the thermally conductive composition, as well as the viscosity ratio (η1 / η3), can be adjusted by the type and amount of the structural viscosity imparting agent and the thermally conductive filler, which will be described later.
[0016] <Structural Viscosity Imparting Agent> The thermally conductive composition of the present invention contains a structural viscosity imparting agent. The structural viscosity imparting agent is preferably a compound that is solid at room temperature (25°C). The viscosity can be increased by blending the structural viscosity imparting agent with a curable compound described below and placing the compound under specific conditions. Specifically, the structural viscosity imparting agent has the function of increasing the viscosity in the low shear region compared to the state before heating by blending the structural viscosity imparting agent with a curable compound, mixing the mixture, and then heating and cooling the mixture. The structural viscosity imparting agent is preferably a compound with a melting point above 25°C, more preferably a compound with a melting point of 40°C or higher, and even more preferably a compound with a melting point of 45°C or higher. The structural viscosity imparting agent is preferably a compound with a melting point of 120°C or lower, more preferably a compound with a melting point of 100°C or lower, and even more preferably a compound with a melting point of 85°C or lower.
[0017] By mixing a curable compound and a structural viscosity imparting agent at room temperature, heating the mixture above the melting point of the structural viscosity imparting agent, and then cooling it to room temperature, loose bonds (internal structure) are formed in the mixture. These loose bonds are formed by the cohesive force of the structural viscosity imparting agent and are not destroyed by gravity. This is thought to prevent the thermally conductive filler from settling during storage. During use, the mixture is subjected to a certain level of shear, which destroys the loose bonds, lowering the viscosity and improving workability, such as application and compressibility. In other words, the internal structure is formed by the cohesive force of the structural viscosity imparting agent, thereby increasing the viscosity in the low-shear region. Note that cohesive force here refers to the mutual attraction between compounds of similar structures. These loose bonds are formed during cooling from a state heated above the melting point. Furthermore, the loose bonds are destroyed by shear stress. Therefore, the loose bond is destroyed when shear stress is generated after cooling, and can be reformed by heating and cooling. In order to exhibit the above function, it is preferable that the structural viscosity imparting agent does not separate from the curable compound for a certain period of time when it is heated to a liquid state.
[0018] The thermally conductive composition of the present invention can be easily adjusted to the above-described viscosity or viscosity ratio by containing a structural viscosity imparting agent. Any structural viscosity imparting agent having the above-described functions can be used without particular limitation. Specific examples of the structural viscosity imparting agent include an ester compound that is solid at 25°C (hereinafter also referred to as ester compound X) or an alcohol compound that is solid at 25°C, and among these, an ester compound that is solid at 25°C is more preferred. The melting point of the ester compound X is preferably above 25°C, more preferably 40°C or higher, and even more preferably 45°C or higher. The melting point of the ester compound X is preferably 120°C or lower, more preferably 100°C or lower, and even more preferably 85°C or lower. When the structural viscosity imparting agent is an ester compound X having such a melting point, it becomes easier to adjust the viscosity ratio (η1 / η3) to the desired range described above, which can suppress sedimentation of the thermally conductive filler during storage and facilitate the production of a thermally conductive composition that is easy to handle during use. The melting point of ester compound X can be determined from the peak temperature of the endothermic curve of the ester compound in a measurement using a differential scanning calorimeter (DSC). Specifically, the thermally conductive composition of the present invention containing ester compound X is measured using a differential scanning calorimeter (DSC), and the peak temperature of the endothermic curve accompanying the melting of the ester compound is taken as the melting point of ester compound X.
[0019] The ester compound X is a compound having an ester group, and may be a monoester having one ester group, or a diester or the like having two or more ester groups, but is preferably a monoester or a diester. The number of carbon atoms in the ester compound X is not particularly limited as long as the ester compound X is solid at 25°C, but is, for example, 20 or more, preferably 25 or more, more preferably 28 or more, and preferably 150 or less, more preferably 100 or less, and even more preferably 50 or less.
[0020] The ester compound X is preferably an ester of a fatty acid and an alcohol. The carbon number of the fatty acid is preferably 2 to 30, more preferably 10 to 24. The carbon number of the fatty acid refers to the total number of carbon atoms, including the carbonyl carbon of the carboxyl group. The alcohol may be an alcohol having one hydroxyl group, or an alcohol having two or more hydroxyl groups. The carbon number of the alcohol is preferably 2 to 30, more preferably 4 to 24. Preferred examples of the ester compound X include cetyl myristate, pentaerythritol distearate, myristyl myristate, myristyl stearate, stearyl stearate, behenyl behenate, glycerin monostearyl ester, and ethylene glycol distearyl ester. Among these, the ester compound X is preferably one or more compounds selected from the group consisting of myristyl myristate, stearyl stearate, and behenyl behenate. One type of ester compound X may be used alone, or two or more types may be used in combination.
[0021] When an alcohol compound that is solid at 25°C is used as the structural viscosity imparting agent, the melting point of the alcohol compound is preferably above 25°C, more preferably 30°C or higher, and even more preferably 40°C or higher. The melting point of the alcohol compound is preferably 120°C or lower, more preferably 80°C or lower, and even more preferably 75°C or lower. When the structural viscosity imparting agent is an alcohol compound having such a melting point, it becomes easier to adjust the viscosity ratio (η1 / η3) to the desired range described above, sedimentation of the thermally conductive filler during storage can be suppressed, and a thermally conductive composition that is easy to handle during use can be obtained.
[0022] The alcohol compound is a compound having a hydroxy group, and may be a monoalcohol having one hydroxy group or a dialcohol having two or more hydroxy groups, but is preferably a monoalcohol. The number of carbon atoms in the alcohol compound is not particularly limited as long as the alcohol compound is solid at 25°C, but is, for example, 14 or more, preferably 16 or more, more preferably 18 or more, and preferably 40 or less, more preferably 36 or less, and even more preferably 30 or less. The number of carbon atoms in the alcohol compound is preferably, for example, 14 to 40, more preferably 16 to 36, and even more preferably 18 to 30. Preferred alcohol compounds include myristyl alcohol, cetanol, stearyl alcohol, nonadecyl alcohol, arachidyl alcohol, heneicosanol, behenyl alcohol, lignoceryl alcohol, ceryl alcohol, montanyl alcohol, myricyl alcohol, 1-dotriacontanol, and geddyl alcohol. One type of alcohol compound may be used alone, or two or more types may be used in combination. As for the structural viscosity imparting agent, between the ester compound X and the alcohol compound, the ester compound X is preferred from the viewpoint of excellent storage stability.
[0023] The content of the structural viscosity imparting agent in the thermally conductive composition is preferably 0.5 parts by mass or more, more preferably 3 parts by mass or more, even more preferably 6 parts by mass or more, and preferably 25 parts by mass or less, more preferably 20 parts by mass or less, relative to 100 parts by mass of the curable compound. The content of the structural viscosity imparting agent in the thermally conductive composition is preferably 0.5 to 20 parts by mass, more preferably 3 to 20 parts by mass, even more preferably 6 to 20 parts by mass, relative to 100 parts by mass of the curable compound.
[0024] <Curable Compound> The thermally conductive composition of the present invention contains a curable compound, which is at least one selected from an epoxy compound and an epoxy curing agent. The curable compound is a liquid compound at room temperature (25°C). The epoxy curing agent is used to cure the epoxy compound, and the epoxy compound and the epoxy curing agent react and cure when mixed. Therefore, as will be described in detail later, it is preferable to separate the epoxy compound and the epoxy curing agent, store them in separate thermally conductive compositions, and mix the separate thermally conductive compositions when used. A thermally conductive composition containing an epoxy compound can be mixed with a thermally conductive composition containing an epoxy curing agent to produce a thermally conductive composition with appropriate adhesive strength.
[0025] (Epoxy Compound) The epoxy compound may be any compound having one or more epoxy groups. The epoxy compound may be a polyfunctional epoxy compound having two or more epoxy groups, or a monofunctional epoxy compound having one epoxy group.
[0026] When the thermally conductive composition contains an epoxy compound, it preferably contains at least a polyfunctional epoxy compound. By containing a polyfunctional epoxy compound, crosslinking can be appropriately formed, making it easier to increase adhesive strength. It is more preferable that the thermally conductive composition further contains a monofunctional epoxy compound in addition to the polyfunctional epoxy compound. By further containing a monofunctional epoxy compound, the thermally conductive composition can prevent the crosslink density after curing from becoming too high, making it easier to increase elongation. In addition, the use of a monofunctional epoxy compound makes it easier to reduce the viscosity of the thermally conductive composition before curing.
[0027] When a polyfunctional epoxy compound and a monofunctional epoxy compound are used in combination, the mass ratio of the monofunctional epoxy compound to the polyfunctional epoxy compound (monofunctional / polyfunctional) is preferably 10 / 90 or more and 90 / 10 or less, more preferably 15 / 85 or more and 75 / 25 or less, and even more preferably 25 / 75 or more and 50 / 50 or less.
[0028] Examples of polyfunctional epoxy compounds include bifunctional and trifunctional compounds, with bifunctional epoxy compounds being preferred. Specific examples of polyfunctional epoxy compounds include, but are not limited to, phenol novolac epoxy compounds, resorcinol epoxy compounds, epoxy compounds having a bisphenol skeleton, epoxy compounds having a naphthalene skeleton, epoxy compounds having a fluorene skeleton, epoxy compounds having a biphenyl skeleton, epoxy compounds having a bi(glycidyloxyphenyl)methane skeleton, epoxy compounds having a xanthene skeleton, epoxy compounds having an anthracene skeleton, and epoxy compounds having a pyrene skeleton, and other epoxy compounds having an aromatic ring. Other examples include epoxy compounds having an alicyclic skeleton, such as epoxy compounds having a dicyclopentadiene skeleton and epoxy compounds having an adamantane skeleton. Furthermore, aliphatic epoxy compounds such as butanediol diglycidyl ether and neopentyl glycol diglycidyl ether are also useful. Hydrogenated or modified versions of the above-listed epoxy compounds can also be used as epoxy compounds.
[0029] Examples of the epoxy compounds having a bisphenol skeleton include epoxy compounds having a bisphenol A, bisphenol F, or bisphenol S bisphenol skeleton. Examples of the resorcinol epoxy compounds include resorcinol diglycidyl ether. Examples of the epoxy compounds having a naphthalene skeleton include 1,2-diglycidylnaphthalene, 1,5-diglycidylnaphthalene, 1,6-diglycidylnaphthalene, 1,7-diglycidylnaphthalene, 2,7-diglycidylnaphthalene, triglycidylnaphthalene, and 1,2,5,6-tetraglycidylnaphthalene. Examples of the epoxy compound having a fluorene skeleton include 9,9-bis(4-glycidyloxyphenyl)fluorene, 9,9-bis(4-glycidyloxy-3-methylphenyl)fluorene, 9,9-bis(4-glycidyloxy-3-chlorophenyl)fluorene, 9,9-bis(4-glycidyloxy-3-bromophenyl)fluorene, 9,9-bis(4-glycidyloxy-3-fluorophenyl)fluorene, 9,9-bis(4-glycidyloxy-3-methoxyphenyl)fluorene, 9,9-bis(4-glycidyloxy-3,5-dimethylphenyl)fluorene, 9,9-bis(4-glycidyloxy-3,5-dichlorophenyl)fluorene, and 9,9-bis(4-glycidyloxy-3,5-dibromophenyl)fluorene.
[0030] Examples of the epoxy compound having a biphenyl skeleton include 4,4'-diglycidylbiphenyl and 4,4'-diglycidyl-3,3',5,5'-tetramethylbiphenyl. Examples of the epoxy compound having a bi(glycidyloxyphenyl)methane skeleton include 1,1'-bi(2,7-glycidyloxynaphthyl)methane, 1,8'-bi(2,7-glycidyloxynaphthyl)methane, 1,1'-bi(3,7-glycidyloxynaphthyl)methane, 1,8'-bi(3,7-glycidyloxynaphthyl)methane, 1,1'-bi(3,5-glycidyloxynaphthyl)methane, 1,8'-bi(3,5-glycidyloxynaphthyl)methane, 1,2'-bi(2,7-glycidyloxynaphthyl)methane, 1,2'-bi(3,7-glycidyloxynaphthyl)methane, and 1,2'-bi(3,5-glycidyloxynaphthyl)methane.
[0031] Examples of the epoxy compound having a xanthene skeleton include 1,3,4,5,6,8-hexamethyl-2,7-bis-glycidylmethoxy-9-phenyl-9H-xanthene, etc. Examples of the epoxy compound having an anthracene skeleton include those having one or more anthracene skeletons and two or more epoxy groups or glycidyl groups in one molecule.
[0032] Examples of the epoxy compound having a pyrene skeleton include those having one or more pyrene skeletons and two or more epoxy groups or glycidyl groups in one molecule. Examples of the epoxy compound having a dicyclopentadiene skeleton include dicyclopentadiene dioxide and a phenol novolac epoxy compound having a dicyclopentadiene skeleton. Examples of the epoxy compound having an adamantane skeleton include 1,3-bis(4-glycidyloxyphenyl)adamantane and 2,2-bis(4-glycidyloxyphenyl)adamantane.
[0033] Among the above-mentioned polyfunctional epoxy compounds, from the viewpoint of improving adhesive strength and mechanical strength, epoxy compounds having an aromatic ring are preferred, among which epoxy compounds having a phenyl group are more preferred, and among which bisphenol-type epoxy compounds, which are epoxy compounds having a bisphenol skeleton, are even more preferred. The polyfunctional epoxy compounds may be used alone or in combination of two or more.
[0034] As the monofunctional epoxy compound, aliphatic monofunctional epoxy compounds are preferred from the viewpoint of high raw material safety, and specific examples include glycidyl ethers of aliphatic alcohols. Here, the aliphatic alcohol may be one having a branched structure or one having a linear structure, but linear structures are preferred from the viewpoint of improving elongation. Furthermore, the aliphatic alcohol may have, for example, approximately 4 to 24 carbon atoms, but from the viewpoint of improving elongation, preferably has 10 to 20 carbon atoms. Furthermore, from the viewpoint of improving elongation, saturated aliphatic alcohols are preferred. Specific examples of glycidyl ethers of aliphatic alcohols include butyl glycidyl ether, decyl glycidyl ether, lauryl glycidyl ether, myristyl glycidyl ether, cetyl glycidyl ether, and stearyl glycidyl ether. The monofunctional epoxy compound may be other than those mentioned above, and examples include monofunctional epoxy compounds having a glycidyl group but not an ether group, such as 1,2-epoxybutane and propylene oxide. As the monofunctional epoxy compound, it is preferable to use an aliphatic monofunctional epoxy compound from the viewpoint of improving elongation, and it is particularly preferable to use a glycidyl ether of an aliphatic alcohol.
[0035] As the monofunctional epoxy compound, a monofunctional epoxy compound having an aromatic ring may be used. Examples of the monofunctional epoxy compound having an aromatic ring include phenyl glycidyl ethers such as alkylphenyl glycidyl ethers represented by phenyl glycidyl ether, 4-t-butylphenyl glycidyl ether, cresyl glycidyl ether, and nonylphenyl glycidyl ether, 1-glycidylnaphthalene, and 2-glycidylnaphthalene. As the monofunctional epoxy compound having an aromatic ring, an epoxy compound having a phenyl group is more preferred. The monofunctional epoxy compounds may be used alone or in combination of two or more.
[0036] The epoxy compound preferably contains an epoxy compound having an aromatic ring, particularly a phenyl group. The epoxy compound having an aromatic ring such as a phenyl group may be a monofunctional epoxy compound or a polyfunctional epoxy compound. The aromatic ring, particularly the phenyl group, forms a stacking structure after curing, making it easier for the epoxy compound to form a pseudo-crosslinked structure in the cured product. This makes it easier to increase mechanical strength and adhesive strength. The epoxy compound preferably contains a polyfunctional epoxy compound, and the polyfunctional epoxy compound preferably has an aromatic ring, particularly a phenyl group.
[0037] The epoxy compound to be used may have a molecular weight of, for example, 2000 or less, preferably 1000 or less, and more preferably 500 or less. By using an epoxy compound with a molecular weight of a certain value or less, the viscosity of the thermally conductive composition can be reduced, and it is also possible to highly fill the thermally conductive filler. The molecular weight of the epoxy compound is, for example, 100 or more, preferably 150 or more, more preferably 200 or more, and even more preferably 250 or more. By setting the molecular weight of the epoxy compound to a certain value or more, it is possible to prevent the crosslink density from becoming higher than necessary, and it is easy to achieve good elongation.
[0038] The epoxy equivalent of the epoxy compound is preferably 1000 g / eq or less, more preferably 500 g / eq or less, even more preferably 375 g / eq or less, and is preferably 100 g / eq or more, more preferably 125 g / eq or more, even more preferably 140 g / eq or more.
[0039] The epoxy compound is preferably liquid at room temperature (25°C). From the viewpoint of reducing viscosity, the lower the viscosity of the epoxy compound at 25°C, the better. For example, it may be 50 Pa·s or less, and preferably 10 Pa·s or less. The viscosity of the epoxy compound at 25°C is not particularly limited, but may be, for example, 0.5 mPa·s or more, or 1 mPa·s or more. The viscosity of the polyfunctional epoxy compound at 25°C may be, for example, 50 Pa·s or less, preferably 10 Pa·s or less, or 1 mPa·s or more, but in practice, it is preferably 10 mPa·s or more, and more preferably 100 mPa·s or more.
[0040] On the other hand, the viscosity of the monofunctional epoxy compound at 25°C may be, for example, 10 Pa·s or less, preferably 1 Pa·s or less, more preferably 100 mPa·s or less, and may be, for example, 0.5 mPa·s or more, 1 mPa·s or more, or 3 mPa·s or more. Note that when the epoxy compound contains both a polyfunctional epoxy compound and a monofunctional epoxy compound, the viscosity of the monofunctional epoxy compound is preferably lower than the viscosity of the polyfunctional epoxy compound. Note that the viscosities of the epoxy compound and the amine compound described below are measured using an E-type viscometer at 10 rpm and 25°C.
[0041] (Epoxy curing agent) The epoxy curing agent is not particularly limited as long as it is a compound capable of curing an epoxy compound, and examples thereof include amine compounds, thiol compounds, acid anhydride compounds, epoxy curing catalysts, etc. Among these, amine compounds are preferred from the viewpoints of ease of adjusting the reactivity with the epoxy compound, and of ease of maintaining a low compressive load at the initial stage of curing and of lengthening the usable time when an epoxy compound is used in combination with a polyfunctional acrylate compound as described below.
[0042] [Amine Compound] The amine compound is a compound having an amino group. The number of amino groups in the amine compound is not particularly limited, but is preferably two or more. By making the number of amino groups two or more, the amine compound can appropriately react with the epoxy compound and cure. The number of amino groups is not particularly limited, but is, for example, 10 or less, preferably 6 or less, and more preferably 4 or less. By making the number of amino groups a certain level or less as described above, the curing reaction is prevented from proceeding too quickly, making it easier to extend the usable time. Furthermore, from the viewpoint of rapid curing, the number of amino groups is preferably three or more. Furthermore, the number of amino groups in the amine compound is preferably two or more and ten or less, more preferably three or more and six or less, and even more preferably three or more and four or less, in terms of the balance between usable time and rapid curing.
[0043] The amino group of the amine compound may be a primary amino group or a secondary amino group. However, from the viewpoints of reactivity and curing speed, it is preferable that the amine compound has a primary amino group. The amine compound preferably has one or more primary amino groups per molecule, more preferably two or more, and even more preferably three or more. When the amine compound has many primary amino groups, rapid curing properties can be achieved. The number of primary amino groups per molecule of the amine compound is, for example, 6 or less, preferably 5 or less, and more preferably 4 or less. Furthermore, in terms of the balance between usable time and rapid curing properties, the number of primary amino groups per molecule of the amine compound is preferably 2 or more and 6 or less, more preferably 3 or more and 5 or less, and even more preferably 3 or more and 4 or less. Note that the amine compound having a primary amino group may have only a primary amino group, or may have a primary amino group and a secondary or higher amino group.
[0044] The viscosity of the amine compound is preferably 20 Pa s or less. When the viscosity is 20 Pa s or less, the viscosity before curing is low, and workability can be improved. The viscosity of the amine compound is preferably 15 Pa s or less, more preferably 12 Pa s or less, even more preferably 5 Pa s or less, and even more preferably 2 Pa s or less. The viscosity of the amine compound is not particularly limited, but is, for example, 0.005 Pa s or more, preferably 0.01 Pa s or more, more preferably 0.025 Pa s or more, and even more preferably 0.05 Pa s or more.
[0045] It is preferable to use an amine compound having an oxyalkylene structure. When an amine compound having an oxyalkylene structure is used, due to its molecular structure, the compressive load at the initial stage of curing is moderately low, and the compressive load is easily maintained at a low state for a relatively long period of time, making it easier to extend the usable time. The oxyalkylene structure preferably has an oxyalkylene structure having approximately 2 to 5 carbon atoms, and more preferably an oxypropylene structure. Examples of the oxyalkylene structure include polyoxyalkylene structures having two or more consecutive oxyalkylene structures, and specific examples include polyoxyethylene structures, polyoxypropylene structures, polyoxybutylene structures, polyoxytetramethylene structures, oxyethylene-oxypropylene copolymer structures, and oxypropylene-oxybutylene copolymer structures. Among these, it is preferable for the amine compound to have a polyoxypropylene structure, an oxyethylene-oxypropylene copolymer structure, or an oxypropylene-oxybutylene copolymer structure, and of these, a polyoxypropylene structure is preferred.
[0046] Examples of amine compounds having an oxyalkylene structure include aliphatic amines, specifically polyoxyethylene diamine, poly(oxyethylene / oxypropylene)diamine, poly(oxypropylene)diamine, poly(oxybutylene / oxypropylene)diamine, polyethylene glycol bis(propylamine), trimethylolpropane poly(oxypropylene)triamine, glyceryl poly(oxypropylene)triamine, and other polyoxyalkylene polyamines. Among these, poly(oxypropylene)diamine, glyceryl poly(oxypropylene)triamine, and trimethylolpropane poly(oxypropylene)triamine are preferred, with trimethylolpropane poly(oxypropylene)triamine being more preferred.
[0047] Furthermore, the amine compound not having an oxyalkylene structure may be an aliphatic amine, an aromatic ring-containing amine, or an amidoamine. Specific examples of aliphatic amines include, but are not limited to, branched or linear alkanediamines such as 1,3-diaminopropane, 2-methyl-1,5-diaminopentane, trimethylhexamethylenediamine, 2-methylpentamethylenediamine, and diethylaminopropylamine, and alicyclic polyamines such as 1,3-bis(aminomethyl)cyclohexane, 1,4-bis(aminomethyl)cyclohexane, cyclohexanediamine, methylcyclohexanediamine, and isophoronediamine. Any type of amidoamine may be used as long as it has a low viscosity. The aromatic ring-containing amine may be an amine in which the amino group is not directly bonded to the aromatic ring, such as m-xylylenediamine or a reaction product of m-xylylenediamine and styrene, or an aromatic amine in which the amino group is directly bonded to the aromatic ring. As the amine compound having no oxyalkylene structure, in order to appropriately increase the curing rate and to enable a certain compressive load to be exerted in the initial stage of curing, aromatic ring-containing amines in which the amino group is not directly bonded to the aromatic ring, such as a reaction product of m-xylylenediamine and styrene, or aliphatic diamines are preferred.
[0048] Among the above-mentioned amine compounds, from the viewpoint of fast curing property and ensuring a certain compressive load in the initial stage of curing, aliphatic amines and aromatic ring-containing amines in which the amino group is not directly bonded to the aromatic ring are preferred, and polyoxyalkylene polyamines are more preferred among them. The amine compounds may be used alone or in combination of two or more.
[0049] The molecular weight of the amine compound is not particularly limited, but may be, for example, 5,000 or less, preferably 3,000 or less, more preferably 1,000 or less, and even more preferably 600 or less. Using an amine compound with a molecular weight below a certain value can reduce the viscosity of the thermally conductive composition and enable a high loading of the thermally conductive filler. Furthermore, the molecular weight of the amine compound should be, for example, 100 or more, preferably 110 or more, more preferably 200 or more, and even more preferably 300 or more. By maintaining the molecular weight of the amine compound above a certain value, the compressive load at the initial stage of curing is appropriately reduced, and the crosslink density can be prevented from becoming excessively high, making it easier to improve elongation and adhesive strength. It is preferable that the amine compound be liquid at room temperature (25°C). The molecular weight of the amine compound and the above-mentioned epoxy compounds can be measured, for example, using a mass spectrometer (GC-MS or LC-MS).
[0050] The active hydrogen equivalent of the amine compound is not particularly limited, but is, for example, 15 g / eq or more, preferably 25 g / eq or more, more preferably 40 g / eq or more, and is, for example, 1000 g / eq or less, preferably 600 g / eq or less, more preferably 300 g / eq or less, and even more preferably 150 g / eq or less.
[0051] [Epoxy Curing Agent Other Than Amine Compound] The thermally conductive composition of the present invention may contain an epoxy curing agent other than an amine compound. Examples of the epoxy curing agent other than an amine compound include a thiol compound, an acid anhydride compound, and an epoxy curing catalyst.
[0052] The thiol compound is not particularly limited, but examples thereof include trimethylolpropane tris(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolethane tris(3-mercaptobutyrate), etc. These may be used alone or in combination of two or more.
[0053] Examples of acid anhydride compounds include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, and succinic anhydride. These may be used alone or in combination of two or more. When an acid anhydride compound is used, it is preferable to use it in combination with an epoxy curing catalyst, which will be described later.
[0054] Examples of epoxy curing catalysts include imidazole-based curing catalysts, organophosphorus-based curing catalysts, amine-based curing catalysts, and tin catalysts. When using an epoxy curing catalyst, it is preferable to use it in combination with a plasticizer, i.e., to dilute it in a plasticizer before use. The plasticizer is preferably one that is liquid at room temperature (25°C). Specific examples of plasticizers include hydrocarbon oils such as ester oils and paraffin oils.
[0055] The thermally conductive composition of the present invention contains an epoxy compound or an epoxy curing agent as a curable compound, as described above. The content of the curable compound in the thermally conductive composition is not particularly limited, but is preferably 3 to 80 mass %, more preferably 5 to 50 mass %, and even more preferably 8 to 20 mass %, based on the total amount of the thermally conductive composition.
[0056] <Multifunctional Acrylate Compound> The thermally conductive composition of the present invention preferably contains a multifunctional acrylate compound. The multifunctional acrylate compound is a compound having two or more functional groups (i.e., the number of (meth)acryloyl groups). In the present invention, the thermally conductive composition contains a multifunctional acrylate compound, which reacts rapidly with an amine compound, has fast curing properties, and imparts a certain level of adhesive strength at the initial stage of curing. As the multifunctional acrylate compound, various (meth)acrylates can be used, and preferably an ester of a multifunctional diol and (meth)acrylic acid is preferred. Furthermore, in this specification, the term "(meth)acryloyl group" refers to either an acryloyl group or a methacryloyl group, and "(meth)acrylate" refers to either an acrylate or a methacrylate, and the same applies to other similar terms.
[0057] Examples of bifunctional polyfunctional acrylate compounds include 1,3-butanediol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, 2-n-butyl-2-ethyl-1,3-propanediol di(meth)acrylate, dimethyloltricyclodecane di(meth)acrylate, ethylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, triptyline, Examples of the di(meth)acrylate include pyrene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, ethylene oxide-added bisphenol A di(meth)acrylate, propylene oxide-added bisphenol A di(meth)acrylate, ethylene oxide-added bisphenol F di(meth)acrylate, dimethyloldicyclopentadienyl di(meth)acrylate, ethylene oxide-modified isocyanuric acid di(meth)acrylate, 2-hydroxy-3-(meth)acryloyloxypropyl (meth)acrylate, carbonate diol di(meth)acrylate, polyether diol di(meth)acrylate, polyester diol di(meth)acrylate, polycaprolactone diol di(meth)acrylate, and polybutadiene diol di(meth)acrylate.
[0058] Furthermore, examples of polyfunctional acrylate compounds having three or more functional groups include alkylene oxide-added trimethylolpropane tri(meth)acrylates such as trimethylolpropane tri(meth)acrylate, glycerin tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, ethylene oxide-added trimethylolpropane tri(meth)acrylate, and propylene oxide-added trimethylolpropane tri(meth)acrylate, caprolactone-modified trimethylolpropane tri(meth)acrylate, and ethylene oxide-added isocyanuric acid tri(meth)acrylate. tetra(meth)acrylate, propylene oxide-added glycerin tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, alkylene oxide-added pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol octa(meth)acrylate, tetrapentaerythritol deca(meth)acrylate, tripentaerythritol hepta(meth)acrylate, and tetrapentaerythritol nona(meth)acrylate.
[0059] The number of functional groups of the polyfunctional acrylate compound is preferably 3 or more, more preferably 4 or more, and even more preferably 6 or more. As the number of functional groups of the polyfunctional acrylate compound increases, the rapid curing property is improved and the adhesive strength at the initial stage of curing tends to increase. The upper limit of the number of functional groups of the polyfunctional acrylate compound is not particularly limited, but may be, for example, 10 or less, or 8 or less.
[0060] The molecular weight of the polyfunctional acrylate compound is preferably a certain value or less in order to enhance the rapid curing property and to reduce the viscosity of the thermally conductive composition before curing. The molecular weight of the specific polyfunctional acrylate compound may be, for example, 5,000 or less, preferably 3,000 or less, more preferably 1,000 or less, and even more preferably 700 or less. Furthermore, the molecular weight of the polyfunctional acrylate compound is, for example, 150 or more, preferably 200 or more, more preferably 250 or more, and even more preferably 450 or more. By setting the molecular weight of the polyfunctional acrylate compound to a certain value or more, the compressive load at the initial stage of curing is appropriately reduced, and the crosslinking density can be prevented from becoming excessively high, making it easier to improve elongation and adhesive strength. The polyfunctional acrylate compound is preferably liquid at room temperature (25°C) in order to easily reduce the viscosity of the thermally conductive composition before curing.
[0061] The functional group equivalent of the polyfunctional acrylate compound is not particularly limited, but is preferably 500 g / eq or less, more preferably 300 g / eq or less, even more preferably 150 g / eq or less, and is preferably 75 g / eq or more, more preferably 80 g / eq or more, even more preferably 85 g / eq or more.
[0062] In the thermally conductive composition, the ratio of the number of functional groups of the polyfunctional acrylate compound to the number of functional groups of the epoxy compound may be approximately 0.1 or more and 2.5 or less, but is preferably 0.3 or more and 1.5 or less, more preferably 0.6 or more and 1.2 or less, and even more preferably 0.75 or more and 1.1 or less. When the ratio of the number of functional groups of the polyfunctional acrylate compound is set within a predetermined range, the amine compound and the polyfunctional acrylate compound are cured preferentially in the initial stage, resulting in fast curing properties, while the reaction between the amine compound and the epoxy compound is suppressed, so that the compressive load in the initial stage of curing is maintained low and the usable time can be extended.
[0063] The content of the polyfunctional acrylate compound is preferably 10 parts by mass or more, more preferably 20 parts by mass or more, even more preferably 40 parts by mass or more, and preferably 100 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 60 parts by mass or less, relative to 100 parts by mass of the curable compound. When the content of the polyfunctional acrylate compound is equal to or greater than these lower limits, rapid curing properties are easily exhibited, and adhesive strength at the initial stage of curing can be increased. When the content of the polyfunctional acrylate compound is equal to or less than these upper limits, excessive initial curing is prevented, and the initial compressive load can be easily maintained low.
[0064] When the thermally conductive composition contains a polyfunctional acrylate, it may further contain water. The inclusion of water, for example, promotes the reaction between the polyfunctional acrylate and the amine compound, making it easier to achieve rapid curing. The water content is not particularly limited, but may be, for example, about 0.3% by mass or more and 2.0% by mass or less based on the total amount of the thermally conductive composition.
[0065] <Thermal Conductive Filler> The thermally conductive composition of the present invention contains a thermally conductive filler. The inclusion of a thermally conductive filler improves the thermal conductivity of the thermally conductive composition and the thermally conductive member obtained from the thermally conductive composition. Examples of thermally conductive fillers include metals, metal oxides, metal nitrides, metal hydroxides, carbon materials, and oxides, nitrides, and carbides other than metals. The thermally conductive filler may be spherical or in the form of an irregular powder. Examples of metals used in thermally conductive fillers include aluminum, copper, and nickel. Examples of metal oxides include aluminum oxide (e.g., alumina), magnesium oxide, and zinc oxide. Examples of metal nitrides include aluminum nitride. Examples of metal hydroxides include aluminum hydroxide. Examples of carbon materials include spherical graphite and diamond. Examples of oxides, nitrides, and carbides other than metals include quartz, boron nitride, and silicon carbide. Among these, aluminum oxide and aluminum hydroxide are preferred as the thermally conductive filler, with aluminum hydroxide being more preferred. The thermally conductive filler may be used alone or in combination of two or more kinds.
[0066] The average particle size of the thermally conductive filler is preferably 0.1 to 200 μm, more preferably 0.3 to 120 μm, and even more preferably 0.5 to 100 μm. It is preferable to use a small-particle thermally conductive filler with an average particle size of 0.1 μm or more and 5 μm or less in combination with a large-particle thermally conductive filler with an average particle size of more than 5 μm and 200 μm or less. The filling rate can be increased by using thermally conductive fillers with different average particle sizes. The average particle size of the thermally conductive filler can be measured by observation using an electron microscope or the like. More specifically, the particle sizes of 50 random thermally conductive fillers can be measured using, for example, an electron microscope or optical microscope, and the average (arithmetic mean) of the measurements can be used as the average particle size.
[0067] The content of the thermally conductive filler is preferably 150 to 3,000 parts by mass, more preferably 300 to 2,000 parts by mass, and even more preferably 500 to 1,000 parts by mass, per 100 parts by mass of the curable compound. By ensuring that the content of the thermally conductive filler is equal to or greater than the above-mentioned lower limit, a certain level of thermal conductivity can be imparted to the thermally conductive composition and the thermally conductive member. By ensuring that the content of the thermally conductive filler is equal to or less than the above-mentioned upper limit, the thermally conductive filler can be appropriately dispersed. Furthermore, it is possible to prevent the viscosity of the thermally conductive composition from becoming unnecessarily high.
[0068] <Anti-settling Agent> The thermally conductive composition of the present invention may contain an anti-settling agent, as long as the viscosity ratio (η1 / η3) does not deviate from the desired range. The inclusion of an anti-settling agent facilitates the prevention of settling of the thermally conductive filler during storage. Examples of anti-settling agents include waxes such as amide wax and hydrogenated castor oil wax, and silicas such as fumed silica. Among these, amide wax is preferred, and fatty acid amide wax is more preferred, because it prevents settling of the thermally conductive filler during storage while improving the compressibility of the thermally conductive composition. Fatty acid amide wax is a compound having a long-chain fatty acid group and an amide group in its molecule. The content of the anti-settling agent is not particularly limited, but is preferably 0.01% by mass or more, more preferably 0.05% by mass or more, and preferably 3% by mass or less, more preferably 1% by mass or less, based on the total amount of the thermally conductive composition. The content of the anti-settling agent is preferably 0.01 to 3 mass %, more preferably 0.05 to 1 mass %, based on the total amount of the thermally conductive composition.
[0069] <Dispersant> The thermally conductive composition of the present invention may contain a dispersant. Examples of dispersants include polymeric dispersants. Examples of polymeric dispersants include polymeric compounds having functional groups. Examples of polymeric compounds include acrylic, vinyl, polyester, polyurethane, polyether, epoxy, polystyrene, amino, and silicone compounds. Examples of functional groups include carboxyl groups, phosphate groups, sulfonic acid groups, carboxylate ester groups, phosphate ester groups, sulfonate ester groups, hydroxyl groups, amino groups, quaternary ammonium bases, and amide groups. Dispersants other than polymeric dispersants may also be used, such as alkoxysilane compounds. The content of the dispersant in the thermally conductive composition is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 3 parts by mass, per 100 parts by mass of the curable compound.
[0070] <Other Additives> The thermally conductive composition of the present invention may contain additives other than the above-mentioned settling inhibitor and dispersant. Examples of other additives include a flame retardant, an antioxidant, and a colorant.
[0071] <Supply Form of Thermally Conductive Composition> In the present invention, the thermally conductive composition may be supplied in a form in which the thermally conductive composition is filled in a container, such as a syringe, a cartridge, a pail, or a drum.
[0072] <Method for Producing Thermally Conductive Composition> The method for producing a thermally conductive composition of the present invention includes the steps of preparing a mixture containing a curable compound, a thermally conductive filler, and a structural viscosity imparting agent, heating the mixture, and cooling the mixture. The cooling step adjusts the viscosity ratio (η1 / η3) of the mixture measured with a rheometer at a temperature of 25°C and a shear rate of 0.0001 (1 / s) to the viscosity (η3) of the mixture measured at a temperature of 25°C and a shear rate of 0.0251 (1 / s) by cooling the mixture. That is, the method for producing a thermally conductive composition of the present invention includes, in this order, the steps of preparing a mixture by mixing a curable compound, a thermally conductive filler, a structural viscosity imparting agent, and optional additives, heating the mixture, and cooling the mixture. Through these steps, a thermally conductive composition of the present invention having a viscosity ratio (η1 / η3) adjusted as described above can be obtained.
[0073] In addition, the method for producing a thermally conductive composition in a supply form may include, in the above-described method for producing a thermally conductive composition, a step of filling a container with the mixture containing a curable compound, a thermally conductive filler, and a structural viscosity imparting agent after the step of preparing the mixture. The steps of heating the mixture and cooling the mixture are preferably performed after the mixture is filled in the container.
[0074] The step of preparing the mixture may be carried out by any known mixing method, such as using a known kneader, kneading roll, mixer, or the like. The heating temperature in the step of heating the mixture may be any temperature at or above the temperature at which the structural viscosity imparting agent melts, for example, a temperature at or above the melting point of the structural viscosity imparting agent, and is preferably at least 10°C higher than the melting point of the structural viscosity imparting agent and not higher than 50°C higher than the melting point of the structural viscosity imparting agent. The upper limit of the heating temperature is not particularly limited, but is preferably, for example, 200°C or lower from the viewpoint of suppressing thermal degradation of the structural viscosity imparting agent. Furthermore, when a volatile component is contained, it is preferable to set the temperature as low as possible, for example, 100°C or lower, and particularly 80°C or lower. The heating time is not particularly limited, but is set to a time that allows the entire mixture to be heated depending on the volume of the mixture. For example, it may be 5 to 1000 minutes, preferably 10 to 500 minutes. Heating times above these lower limits facilitate sufficient heating of the mixture to the interior. When the heating time is equal to or less than these upper limit values, if the mixture contains a volatile substance, it is possible to suppress the evaporation of part of the volatile substance. In the step of cooling the mixture, the mixture after the heating is cooled. The cooling is performed until the temperature of the mixture reaches 25°C. The cooling method is not particularly limited, and may be a method of cooling using a cooler or a method of natural cooling, but it is preferable to cool the mixture quickly using a cooler.
[0075] <Two-component curing thermally conductive material> In the present invention, from the viewpoint of storage stability, it is preferable to use a thermally conductive composition to form a two-component curing thermally conductive material. Specifically, a two-component curing thermally conductive material is preferred, which is composed of a first part consisting of a thermally conductive composition containing an epoxy compound, a thermally conductive filler, and a structural viscosity imparting agent, and having a viscosity ratio (η1 / η3) of 60 or more, and a second part consisting of a thermally conductive composition containing an epoxy curing agent, a thermally conductive filler, and a structural viscosity imparting agent, and having a viscosity ratio (η1 / η3) of 60 or more. The thermally conductive compositions of the first and second parts may also contain the above-mentioned settling inhibitor, dispersant, polyfunctional acrylate compound, and other additives. When a polyfunctional acrylate compound is added, it is preferable to add it to the thermally conductive composition of the first part. The mass ratio of the first agent to the second agent (second agent / first agent) is preferably 1 or a value close to 1, specifically preferably 0.9 to 1.1, and more preferably 0.95 to 1.05. In this way, by setting the mass ratio of the first agent to the second agent to a value close to 1, it becomes easy to prepare a mixture of the first agent and the second agent.
[0076] The present invention provides a supply form of a two-component curing thermally conductive material comprising a first container filled with a first part consisting of a thermally conductive composition containing an epoxy compound, a thermally conductive filler, and a structural viscosity imparting agent, and a second container filled with a second part consisting of a thermally conductive composition containing an epoxy curing agent, a thermally conductive filler, and a structural viscosity imparting agent. The first and second containers can also be combined and integrated. The integration of the first and second containers facilitates supply to consumers as a container set. In this specification, the first container filled with the first part and the second container filled with the second part are sometimes collectively referred to as a container set. The first and second components each have a viscosity ratio (η1 / η3) of 60 or more between the viscosity η1 measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) and the viscosity η3 measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s).
[0077] As described above, the thermally conductive composition of the present invention is prepared through the steps of preparing a mixture, heating the mixture, and cooling the mixture. For example, a mixture (thermally conductive composition) containing an epoxy compound, a thermally conductive filler, and a structural viscosity imparting agent is prepared, and the mixture is filled into a first container. The mixture is then heated and cooled to obtain a first container filled with a first agent. Similarly, a mixture (thermally conductive composition) containing an epoxy curing agent, a thermally conductive filler, and a structural viscosity imparting agent is prepared, and the mixture is filled into a second container. The mixture is then heated and cooled to obtain a second container filled with a second agent. The first and second agents filled in the first and second containers, respectively, are prevented from settling, ensuring excellent storage stability. When in use, the first and second agents are discharged from the first and second containers, respectively, and mixed using a static mixer or the like, followed by curing to form a thermally conductive member. When the first and second agents are ejected, a certain shear force is generated, which reduces the viscosity of the first and second agents, making them easier to eject. Furthermore, the coated material formed by ejection is easy to compress and has excellent handleability. For example, after ejecting a mixture of the first and second agents between a heat generating element and a heat dissipating element to form a coated material of a certain thickness, it becomes easy to stretch the coated material thinly with a small load.
[0078] Examples of the first and second containers include syringes, cartridges, pails, and drums. For example, when syringes are used as containers, the two-component curing thermally conductive material is supplied in a form consisting of a first syringe filled with a first component and a second syringe filled with a second component. In this case, the first and second syringes may be arranged in parallel and integrated to form a two-component parallel type. As shown in FIG. 1 , a two-component parallel type syringe 30 is formed by arranging a first syringe 31 constituting the first container and a second syringe 32 constituting the second container in parallel and integrated. The first component 35 and the second component 36 filled in the syringes 31 and 32 may be dispensed and mixed from the syringes as dispensers.
[0079] When cartridges are used, the two-component curing thermally conductive material is supplied in a form consisting of a first cartridge filled with the first component and a second cartridge filled with the second component. In this case, too, the first cartridge and the second cartridge may be arranged in parallel and integrated to form a two-component parallel type.
[0080] The first and second agents may be mixed using a mixer such as a static mixer. For example, as shown in FIG. 1 , the static mixer 38 is connected to the outlet 31A of the first syringe 31 and the outlet 32A of the second syringe 32, and the first agent 35 and the second agent 36 discharged from the respective outlets 31A, 32A can be mixed inside the mixer 38. The mixture obtained by mixing in the mixer 38 may be discharged from the outlet 39 of the mixer 38. Each syringe 31, 32 may have a structure in which the openings of the barrels 33A, 34A, into which the first agent 35 and the second agent 36, respectively, are filled, are closed by lids 33B, 34B. In the syringe 30 shown in FIG. 1 , the first agent 35 and the second agent 36 may be ejected from the respective outlets 31A, 32A after the lids 33B, 34B are removed, and the first agent 35 and the second agent 36 are pushed out by pistons (not shown) inserted through the openings.
[0081] 2, the container set may include a first pail 41 that constitutes the first container and is filled with a first agent 45, and a second pail 42 that constitutes the second container and is filled with a second agent 46. Each pail 41, 42 may include, for example, a container body 43A, 44A that has an opening and is filled with the first agent 45 and the second agent 46, and a lid 43B, 44B that closes the opening of each container body 43A, 44A.
[0082] <Thermal Conductive Member> The present invention can also provide a thermally conductive member. The thermally conductive member is a cured product of the thermally conductive composition described above, or a cured product of a two-component curing thermally conductive material obtained by mixing and curing the first and second components described above. The thermally conductive member of the present invention uses a structural viscosity imparting agent, which provides excellent handleability of the thermally conductive composition as a raw material, thereby improving workability when forming the thermally conductive member. Furthermore, the thermally conductive composition as a raw material has suppressed sedimentation of the thermally conductive filler during storage, resulting in a uniform composition. Therefore, the composition of the formed thermally conductive member is also uniform, resulting in less variation in physical properties.
[0083] The thermal conductivity of the thermally conductive member is preferably 1.0 W / m·K or higher, more preferably 1.5 W / m·K or higher, and even more preferably 2.0 W / m·K or higher. By setting the thermal conductivity at or above these lower limits, good thermal conductivity is achieved. Therefore, when used as a gap material in a battery cell module, for example, heat generated from the battery cells can be efficiently transferred to the module housing via the gap material, preventing excessive increases in the temperature of the battery cells. The higher the thermal conductivity of the thermally conductive member, the better, but in practical use, it is, for example, 15 W / m·K or lower. Thermal conductivity is measured in accordance with ASTM D5470.
[0084] [Applications] The thermally conductive composition, two-component curing thermally conductive material, supply form of the two-component curing thermally conductive material, and thermally conductive members formed therefrom of the present invention can be used in a variety of applications. They can be used in various electronic devices, such as battery assemblies such as lithium-ion battery (LiB) assemblies, power electronic devices, electronic packaging, LEDs, solar cells, and electrical grids. Among these, they are preferably used in battery assemblies, and more preferably in LiB assemblies. Therefore, a preferred embodiment of the present invention provides a battery assembly comprising the above-described thermally conductive member. Battery assemblies such as LiB assemblies are preferably used in automobiles.
[0085] In battery assembly applications, the thermally conductive composition, two-component curing thermally conductive material, supply form of the two-component curing thermally conductive material, and thermally conductive member formed therefrom of the present invention are preferably used as a gap filler in a battery assembly. Furthermore, in one aspect, the thermally conductive composition and thermally conductive member of the present invention are preferably used in a battery module, and more preferably as a gap filler in a battery module. Below, an example in which the thermally conductive member of the present invention is applied to a battery module will be described.
[0086] The thermally conductive member of the present invention can be used as a gap material in a battery module as follows. The battery module of the present invention includes a gap material made of a thermally conductive member, multiple battery cells, and a module housing that houses the multiple battery cells, and the gap material is disposed inside the module housing. The gap material made of a thermally conductive member is filled between the battery cells and between the battery cells and the module housing, and the filled gap material is in close contact with the battery cells and the module housing. As a result, the gap material between the battery cells has the function of maintaining a separation between the battery cells. Furthermore, the gap material between the battery cells and the module housing is in close contact with both the battery cells and the module housing, and has the function of transferring heat generated in the battery cells to the module housing.
[0087] Fig. 3 shows a specific configuration of a battery module. Fig. 4 shows a specific configuration of each battery cell. As shown in Fig. 3, a plurality of battery cells 11 are arranged inside a battery module 10. Each battery cell 11 is laminated and enclosed in a flexible exterior film, and has an overall shape of a flat body that is thin compared to its height and width. As shown in Fig. 4, the positive electrode 11a and negative electrode 11b of such a battery cell 11 are exposed to the outside, and the central portion 11c of the flat surface is formed thicker than the crimped end portion 11d.
[0088] As shown in Fig. 3, the battery cells 11 are arranged so that their flat surfaces face each other. In the configuration of Fig. 3, the gap material 13 is not filled so as to entirely cover the plurality of battery cells 11 housed inside the module housing 12. The gap material 13 is filled so as to fill gaps that exist in a portion (bottom portion) inside the module housing 12. The gap material 13 is filled between the battery cells 11 and between the battery cells 11 and the module housing 12, and is in close contact with the surfaces of the battery cells 11 in these portions and the inner surface of the module housing 12.
[0089] The gap material 13 filled between the battery cells 11 is adhered to the surfaces of both battery cells 11. However, the gap material 13 itself has appropriate elasticity and flexibility, and can mitigate distortion and deformation caused by an external force even when an external force that displaces the spacing between the battery cells 11 is applied. Therefore, the gap material 13 has the function of maintaining the battery cells 11 spaced apart from each other. The gap material 13 filled in the gap between the battery cell 11 and the inner surface of the module housing 12 is also tightly adhered to the surface of the battery cell 11 and the inner surface of the module housing 12. As a result, heat generated inside the battery cell 11 is conducted via the gap material 13 adhered to the surface of the battery cell 11 to the inner surface of the module housing 12, which is in close contact with the other surface of the gap material 13.
[0090] The gap filler 13 may be formed in the battery module 10 by applying a liquid thermally conductive composition or a two-component curing thermally conductive material using a general dispenser and then curing the applied material. In the case of a two-component curing thermally conductive material, for example, the first and second containers described above may be placed in the dispenser and the material may be applied using the dispenser. The two-component curing thermally conductive material is easy to store, and if mixed immediately before use, it is less likely to harden during application with the dispenser and can be quickly cured after application. Application with a dispenser is also preferable because it allows the material to be filled relatively deep within the housing 12 of the battery module 10.
[0091] The gap material 13 covering the battery cells 11 preferably covers 20 to 100% of each battery cell 11 on one side of the battery cell 11, and more preferably covers 20 to 40%. By covering 20% or more, the battery cells 11 can be stably held. Furthermore, by sufficiently covering battery cells that generate a large amount of heat, heat dissipation efficiency is improved. On the other hand, by covering 100% or less, heat generated from the battery cells 11 can be efficiently dissipated. Furthermore, by covering 40% or less, weight increase and deterioration of workability can be prevented. Furthermore, to improve heat dissipation efficiency, it is preferable to cover the side of the battery cells 11 where the electrodes 11a and 11b are located with the gap material 13, and it is more preferable to cover the entire electrodes 11a and 11b with the gap material 13.
[0092] As described above, the battery module 10 can dissipate heat generated from the battery cells 11 to the module housing 12 via the gap material 13. The gap material 13 is also preferably used in a battery pack having a plurality of battery modules 10 therein. A battery pack generally includes a plurality of battery modules 10 and a battery pack housing that houses the plurality of battery modules 10. In the battery pack, the gap material 13 can be provided between the battery modules 10 and the battery pack housing. This allows the heat dissipated to the module housing 12 as described above to be further dissipated to the battery pack housing, enabling effective heat dissipation. Furthermore, since the thermally conductive member of the present invention is used for the gap material 13, excellent workability is achieved when forming the gap material 13.
[0093] In addition, in the above description, examples of the battery assembly have been described as a battery module or a battery pack including a battery module, but the battery assembly may also be applied to a battery assembly that does not include a battery module, and it is also preferable to apply the battery assembly to, for example, a battery assembly having a cell-to-pack structure.
[0094] FIG. 5 shows a schematic diagram of a battery assembly having a cell-to-pack structure. The battery assembly 20 having the cell-to-pack structure includes a plurality of battery cells 21 and a battery pack housing. The plurality of battery cells 21 are bonded to a base member 25 constituting the battery pack housing via a spacer 23 made of a thermally conductive material (a cured product of a thermally conductive composition). The base member 25 may also constitute a cooling plate or the like. The spacer 23 in the battery assembly 20 may be formed in the same manner as the spacer 13 in the battery module described above, for example, using a general dispenser. The thermally conductive composition of the present invention also provides good workability when forming the spacer 23. Furthermore, because the thermally conductive composition of the present invention has excellent compressibility, the battery cells 21 can be bonded to the base member 25 with high workability even in a battery assembly having a cell-to-pack structure.
[0095] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0096] The measurement and evaluation methods in the present examples are as follows.
[0097] [Viscosity] For Examples 1 to 6 and Comparative Examples 1 and 2, the viscosities of the first and second components, which are thermally conductive compositions, were measured as follows. Using a rheometer, the viscosities of each of the first and second components were measured at various shear rates. Using an Anton Paar MCR-302e rheometer, the sample temperature was adjusted to 85°C, which is above the melting point of each structural viscosity imparting agent, using a Peltier plate. After 5 minutes, the sample was cooled to 25°C at a cooling rate of 20°C / min and allowed to stand for 10 minutes. Subsequently, viscosity measurements were performed using a φ25 mm parallel plate while continuously changing the shear rate. The viscosity η1 measured at a shear rate of 0.0001 (1 / s), the viscosity η3 measured at a shear rate of 0.0251 (1 / s), and the viscosity η2 measured at a shear rate of 25.1 (1 / s) were each measured, and the viscosity ratio (η1 / η3) was calculated. Viscosities at other shear rates were also measured as shown in Table 1.
[0098] [Melting Point of Ester Compound in Thermally Conductive Composition] The melting point of the structural viscosity imparting agent in the thermally conductive composition was measured by the following method for Examples 1 to 6. Specifically, 20 mg of the first or second part of the thermally conductive composition was weighed into an aluminum cell, and then the temperature was increased from 25°C to 90°C at a rate of 10°C / min using a Shimadzu DSC-60 under a nitrogen flow.
[0099] [Thermal Conductivity] The thermal conductivity of the first and second thermally conductive compositions was determined by measuring thermal resistance using a measuring device conforming to ASTM D5470-06. Specifically, the thermally conductive composition was placed in a thickness greater than that required for measurement, covering the measurement die on the heating element side. The composition was then sandwiched between heat sinks and compressed under a load of 30 psi until the thermally conductive composition reached a thickness of 1.0 mm, 1.5 mm, or 2.0 mm, and the thermal resistance at each thickness was measured. The thickness can be adjusted using spacers. For these three thermal resistance values, a graph was created with thickness on the horizontal axis and thermal resistance on the vertical axis, and an approximate line between three points was determined using the least squares method. The slope of the approximate line represents the thermal conductivity. Thermal resistance measurements were performed at 80°C using an LW-9389 manufactured by Long Win Science and Technology Corporation. The area of the measurement die was 1 inch x 1 inch.
[0100] [Settling Inhibition Evaluation] For Examples 1 to 6 and Comparative Examples 1 and 2, the settling inhibition evaluation was performed as follows. The settling inhibition evaluation was performed for each of the first and second parts as follows. 10 cc of each sample was placed in a 15 cc transparent container (cylindrical, 24 mm diameter), and heated at the melting point of the structural viscosity imparting agent +10°C for 30 minutes. The sample was then naturally cooled to 25°C in a 25°C atmosphere and allowed to stand for one day. After that, the sample was left in a 35°C environment for 30 days, after which the condition of the sample was confirmed. The first and second parts of each Example and Comparative Example were evaluated according to the following criteria and recorded as a "settling inhibition evaluation." Furthermore, the worse of the "settling inhibition evaluations" for the first and second parts was recorded as the "settling inhibition evaluation (overall)." (Evaluation Criteria) 5: No visible change. 4: The liquid component was slightly smeared at the edge of the surface. 3: The liquid component was slightly smeared on the surface, but the liquid component did not flow even when tilted. 2 The liquid component was slightly smeared on the surface, and when tilted, the liquid component flowed. 1 The liquid component was separated when viewed from the side.
[0101] [Compressibility Evaluation (Compressibility)] The compressibility evaluation for Examples 1 to 6 and Comparative Examples 1 and 2 was performed as follows. The raw materials for the first and second components listed in the table were each introduced into a first and second syringe, which were two-liquid parallel-type 25 cc syringes, at 16.4 cc each. The first and second components were then heated to the melting point of each structural viscosity imparting agent +10°C and allowed to stand for 15 minutes, after which they were cooled to 25°C and left for 10 minutes. A 2.5 cc sample (a mixture of the first and second components (mass ratio 1:1)) was then ejected onto an aluminum plate using a static mixer. The ejected material was then compressed at a compression rate of 60 mm / min using a 30 mm diameter plunger (compression test jig), and the load value when the gap between the jigs was compressed to 0.380 mm was read and used as the compression load. The temperature during the compression test was 25°C. Based on the compression load value, compressibility was evaluated according to the following criteria. (Evaluation criteria) 5 Less than 250N 4 250N or more but less than 300N 3 300N or more but less than 350N 2 350N or more but less than 400N 1 400N or more
[0102] [Overall Evaluation] For each example and comparative example, the average value of the sedimentation prevention evaluation and the compressibility evaluation was used as the overall evaluation. Specifically, the overall evaluation value was calculated based on the following formula: Overall evaluation = (settling prevention evaluation (overall) + compressibility evaluation) / 2
[0103] In each of the Examples and Comparative Examples, the following components were used. <Epoxy Compounds> - Multifunctional epoxy compound: bisphenol F type epoxy resin, manufactured by Mitsubishi Chemical Corporation, trade name "jER806", molecular weight 330, epoxy equivalent 165 g / eq, number of functional groups 2, viscosity (25°C) 400 mPa·s - Monofunctional epoxy compound: aliphatic glycidyl ether (aliphatic alcohol C12-14), trade name "Epogose ML", manufactured by Yokkaichi Synthetic Co., Ltd., epoxy equivalent 282 g / eq, number of functional groups 1, viscosity (25°C) 7 mPa·s
[0104] <Epoxy curing agent> Amine compound: trimethylolpropane poly(oxypropylene) triamine, manufactured by HUNTSMAN (trade name "T-403"), molecular weight 440, active hydrogen equivalent 73.3 g / eq, number of active hydrogen atoms in amino groups = 6, functional group = 3 × (-NH 2 ), viscosity (25°C) 0.07 Pa・s
[0105] <Polyfunctional acrylate compound> Polyfunctional acrylate compound: dipentaerythritol hexaacrylate, "DPHA" manufactured by Daicel Allnex Corporation
[0106] <Dispersant> Polymer dispersant (acidic group-containing copolymer)
[0107] <Structural viscosity imparting agent (ester compound X solid at 25°C)> Stearyl stearate, melting point 57°C, number of carbon atoms 36 Behenyl behenate, melting point 75°C, number of carbon atoms 44 The melting points were measured by weighing 20 mg of the structural viscosity imparting agent in an aluminum cell, and then using a Shimadzu DSC-60 in a nitrogen stream, raising the temperature from 25°C to 90°C at a rate of 10°C / min.
[0108] <Settling inhibitor> Amide wax: fatty acid amide wax (melting point 122°C) Fumed silica: "AEROSIL 300" from Nippon Aerosil Co., Ltd., hydrophilic, specific surface area 300 m 2 / g
[0109] <Thermal conductive filler> Aluminum hydroxide 1: average particle size 1 μm Aluminum hydroxide 2: average particle size 10 μm Aluminum hydroxide 3: average particle size 50 μm Aluminum hydroxide 4: average particle size 90 μm Aluminum oxide (alumina): average particle size 45 μm
[0110] [Examples 1 to 6, Comparative Examples 1 and 2] First and second agents were prepared according to the formulations shown in Tables 1 to 3, and the viscosity, sedimentation suppression evaluation, and compressibility evaluation were carried out as described above. The results are shown in Tables 1 to 3.
[0111]
[0112]
[0113]
[0114] Each of the thermally conductive compositions of Examples 1 to 6 contained a curable compound, a thermally conductive filler, and a structural viscosity imparting agent, and had a viscosity ratio (η1 / η3) of 60 or greater, satisfying the requirements of the present invention. In each example, the results of the sedimentation suppression evaluation were favorable, indicating that sedimentation of the thermally conductive filler was suppressed during storage. Furthermore, the compressibility evaluation was also favorable, demonstrating excellent handleability. In contrast, the thermally conductive composition of Comparative Example 1 did not contain a structural viscosity imparting agent and had a viscosity ratio (η1 / η3) of less than 60. Therefore, Comparative Example 1 showed a poor result in the sedimentation suppression evaluation and inferior storage stability. The thermally conductive composition of Comparative Example 2, which incorporated fumed silica instead of a structural viscosity imparting agent, showed slightly worse sedimentation suppression than the examples, but significantly inferior compressibility evaluation compared to the examples, indicating inferior handleability.
[0115] DESCRIPTION OF SYMBOLS 10 Battery module 11, 21 Battery cell 12 Battery module housing (module housing) 13, 23 Gap material 20 Battery assembly 25 Base member 30 Syringe 31 First syringe 31A First syringe outlet 32 Second syringe 32A Second syringe outlet 33A, 34A Barrel 33B, 34B Barrel lid 35, 45 First agent 36, 46 Second agent 38 Mixer 39 Mixer outlet 41 First pail 42 Second pail 43A, 44A Container body with opening 43B, 44B Lid for closing the opening of the container body
Claims
1. A thermally conductive composition comprising at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent, wherein the viscosity ratio (η1 / η3) between the viscosity η1 measured by a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) and the viscosity η3 measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s) is 60 or more.
2. The thermally conductive composition according to claim 1, having a viscosity η2 of 125 Pa·s or less, measured at a measurement temperature of 25°C and a shear rate of 25.1 (1 / s).
3. The thermally conductive composition according to claim 1 or 2, wherein the structural viscosity imparting agent is a compound having a melting point of more than 25°C.
4. The thermally conductive composition according to claim 1 or 2, wherein the structural viscosity imparting agent is an ester compound having a melting point of more than 25°C and not more than 120°C.
5. The thermally conductive composition according to claim 1, wherein the curable compound is an epoxy compound.
6. The thermally conductive composition of claim 1, wherein said curable compound is an epoxy curing agent.
7. The thermally conductive composition of claim 6, wherein the epoxy hardener is an amine compound.
8. A two-component curing type thermally conductive material comprising a first part made of the thermally conductive composition according to claim 5 and a second part made of the thermally conductive composition according to claim 6.
9. A supply form of a two-component curing thermally conductive material comprising a first container filled with a first agent consisting of a thermally conductive composition containing an epoxy compound, a thermally conductive filler, and a structural viscosity imparting agent, and a second container filled with a second agent consisting of a thermally conductive composition containing an epoxy curing agent, a thermally conductive filler, and a structural viscosity imparting agent, wherein each of the first and second agents has a viscosity ratio (η1 / η3) of 60 or more between the viscosity η1 measured by a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) and the viscosity η3 measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s).
10. A thermally conductive member which is a cured product of the thermally conductive composition according to claim 1 or 2.
11. A thermally conductive member which is a cured product of the two-component curing type thermally conductive material according to claim 8.
12. A battery module comprising a gap material made of the thermally conductive material according to claim 10, a plurality of battery cells, and a module housing for storing the plurality of battery cells, the gap material being disposed inside the module housing.
13. A method for producing a thermally conductive composition, comprising the steps of: preparing a mixture containing at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent; heating the mixture; and cooling the mixture to adjust the viscosity ratio (η1 / η3) of the mixture measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) to the viscosity of the mixture measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s), to 60 or more.
14. A method for producing a supply form of a thermally conductive composition, comprising the steps of: preparing a mixture containing at least one curable compound selected from the group consisting of epoxy compounds and epoxy curing agents, a thermally conductive filler, and a structural viscosity imparting agent; filling the mixture into a container; heating the mixture; and cooling the mixture to adjust the viscosity ratio (η1 / η3) of the mixture measured with a rheometer at a measurement temperature of 25°C and a shear rate of 0.0001 (1 / s) to the viscosity of the mixture measured at a measurement temperature of 25°C and a shear rate of 0.0251 (1 / s), to 60 or more.
Citation Information
Patent Citations
Thermally conductive composition and electronic apparatus including the same
JP2022116587A
Thermal conductive adhesive
JP1994017024A
Resin composition and laminated structure
JP2011132368A
Resin composition and semiconductor device using the resin composition
JP2018138634A
Thermally conductive potting composition
JP2022533511A
Cited By
Two-component curable composition, method for producing two-component curable composition, and cured product
WO2026225543A1