Ceramic sintered body
The ceramic sintered body with a balanced composition of Al, Ti, Fe, and Si/Ca/Mg achieves semiconductivity and mechanical strength, addressing the limitations of conventional materials by optimizing mass ratios and firing conditions, resulting in a strong and conductive black ceramic.
Patent Information
- Application Number
- PCT/JP2024/016579
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
Conventional ceramic sintered bodies with increased Ti and Fe content for semiconductivity compromise mechanical strength, making it challenging to achieve both semiconductivity and excellent mechanical strength simultaneously.
A ceramic sintered body composition comprising Al, Ti, Fe, and at least one of Si, Ca, and Mg, with specific mass ratios and firing conditions to balance resistivity and mechanical strength, allowing for a black color and semiconductivity while maintaining high mechanical strength.
The ceramic sintered body achieves a balance of semiconductivity and mechanical strength, with a volume resistivity between 1.0×10^4 Ωcm and 1.0×11 Ωcm, and a three-point bending strength of 260 MPa or more, suitable for applications requiring both properties.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Sintered ceramic
[0001] The present disclosure relates to a ceramic sintered body.
[0002] Conventionally, as disclosed in Patent Document 1, there has been known a ceramic sintered body used for a mounting substrate, a member for an exposure processing apparatus, a light-shielding material, a heat-absorbing material, etc. Such a ceramic sintered body is, for example, black in color and has a composite oxide containing a plurality of metal elements such as Ti and Fe.
[0003] Japanese Patent Application Publication No. 1-42359
[0004] A ceramic sintered body according to one aspect of the embodiment contains Al, Ti, Fe, and at least one of Si, Ca, and Mg, and the Al is 2 O 3 The Ti and Fe are contained in an amount of 67 mass % or more in terms of TiO 2 Conversion and Fe 2 O 3 The total content is 10 mass % or more and 30 mass % or less in terms of TiO 2 / (TiO 2 +Fe 2 O 3 ) is 5% or more and 20% or less, and at least one of the Si, the Ca and the Mg is selected from the group consisting of SiO 2 The total content of the SiO2 equivalent, CaO equivalent, and MgO equivalent is 0.5 mass % or more and 3.0 mass % or less, and the volume resistivity is 1.0 × 10 4 Ωcm or more and 1.0×10 11 It is Ωcm or less.
[0005] Hereinafter, embodiments of the ceramic sintered body disclosed in the present application will be described in detail. However, the present invention is not limited to the embodiments described below.
[0006] Conventionally, as disclosed in Patent Document 1, there has been known a ceramic sintered body used for a mounting substrate, a member for an exposure processing apparatus, a light-shielding material, a heat-absorbing material, etc. Such a ceramic sintered body is, for example, black in color and has a composite oxide containing a plurality of metal elements such as Ti and Fe.
[0007] However, when the above-mentioned ceramic sintered body is to be made semiconductive, the contents of Ti and Fe increase, which causes a problem of a decrease in mechanical strength.
[0008] Therefore, it is desired to solve the above problems and realize a black ceramic sintered body that is semiconductive and has excellent mechanical strength.
[0009] The ceramic sintered body of the present disclosure contains Al, Ti, and Fe. The ceramic sintered body of the present disclosure further contains at least one of Si, Ca, and Mg. The ceramic sintered body of the present disclosure contains a plurality of metal oxides.
[0010] The ceramic sintered body of the present disclosure is black. * and b * is greater than or equal to -2.0 and less than or equal to 2.0. * and b * is CIE1976(L * a * b * ) color space. * and b * can be adjusted by the composition of the metal oxide contained in the ceramic sintered body of the present disclosure as well as the firing temperature and firing time.
[0011] The ceramic sintered body of the present disclosure is Al 2 O 3 The ceramic sintered body of the present disclosure contains 67 mass % or more of Al, calculated as Al, and may further contain 75 mass % or more of Al. 2 O 3 The Al content may be adjusted depending on the contents of other components described below.
[0012] In addition, the ceramic sintered body of the present disclosure contains TiO 2 Conversion and Fe 2 O 3 The total amount of Ti and Fe is 10 mass % or more and 30 mass % or less in terms of TiO 2 Conversion and Fe 2 O3 The total amount of Ti and Fe may be 20% by mass or more and 25% by mass or less in terms of converted amounts.
[0013] TiO 2 Conversion and Fe 2 O 3 By containing 10 mass % or more of Ti and Fe in total, the resistivity of the ceramic sintered body can be reduced. 2 Conversion and Fe 2 O 3 By including 30 mass % or less of Ti and Fe in total, the mechanical strength of the ceramic sintered body can be maintained at a good level.
[0014] In addition, the ceramic sintered body of the present disclosure contains TiO 2 / (TiO 2 +Fe 2 O 3 ) is 5% or more and 20% or less, and further, TiO 2 / (TiO 2 +Fe 2 O 3 ) may be 15% or more and 20% or less.
[0015] TiO 2 / (TiO 2 +Fe 2 O 3 ) is 5% or more, the resistivity of the ceramic sintered body can be reduced. 2 / (TiO 2 +Fe 2 O 3 ) is 20% or less, the ceramic sintered body can exhibit a good black color.
[0016] In addition, the ceramic sintered body of the present disclosure is 2 The composition may contain at least one of Si, Ca, and Mg in a total amount of 0.5 mass % or more and 3.0 mass % or less in terms of Si, Ca, and MgO.
[0017] SiO 2By containing at least one of Si, Ca, and Mg in a total amount of 0.5 mass % or more in terms of SiO, CaO, and MgO, the resistivity of the ceramic sintered body can be reduced. 2 By containing at least one of Si, Ca and Mg in a total amount of 3.0 mass % or less in terms of Si, Ca, and MgO, the low reflectance of the ceramic sintered body can be well maintained.
[0018] Furthermore, the ceramic sintered body of the present disclosure has a volume resistivity of 10 4 Ωcm or more and 10 11 Ωcm or less, and further, the volume resistivity is 10 10 This allows for a ceramic sintered body suitable for applications requiring semiconductivity to be obtained.
[0019] In the ceramic sintered body of the present disclosure, the grain boundary phase mainly plays a role in reducing the volume resistivity. In the ceramic sintered body of the present disclosure, the volume resistivity tends to decrease as the average crystal grain size increases. This is presumably because the network of the grain boundary phase becomes thicker as the average crystal grain size increases.
[0020] Furthermore, the ceramic sintered body of the present disclosure has a three-point bending strength of 260 MPa or more as a specific mechanical strength, and may further have a three-point bending strength of 300 MPa or more, thereby obtaining a ceramic sintered body suitable for applications requiring high physical strength.
[0021] Generally, the smaller the average crystal grain size, the higher the mechanical strength. Considering the balance between mechanical strength and volume resistivity, the average crystal grain size may be in the range of 5 μm or more and 7 μm or less. The average crystal grain size can be controlled by appropriately adjusting the firing temperature and firing time. The average crystal grain size may also be measured by the cord method.
[0022] Furthermore, by having a composition within the above-mentioned range, the ceramic sintered body of the present disclosure can be realized as a black ceramic sintered body having semiconductivity and excellent mechanical strength.
[0023] Furthermore, by having a composition within the above-described range, the ceramic sintered body of the present disclosure can exhibit semiconductivity even when fired in a non-reducing atmosphere, which allows for easy production of a semiconductive ceramic sintered body, thereby reducing the production cost of the ceramic sintered body.
[0024] Furthermore, the ceramic sintered body of the present disclosure may have a reflectance of 15% or less, and may further have a reflectance of 10% or less, thereby obtaining a ceramic sintered body suitable for applications requiring low reflectance.
[0025] The ceramic sintered body of the present disclosure also has a * and b * may be not less than −2.0 and not more than 2.0. This makes it possible to obtain a ceramic sintered body that is particularly suitable for applications requiring a black color.
[0026] The metal elements contained in the ceramic sintered body of the present disclosure can be quantified using an ICP (Inductively Coupled Plasma) optical emission spectrometer. The content of each metal element obtained by the measurement is converted into a metal oxide to obtain the content of each metal element. Specifically, for example, Al is Al 2 O 3 Ti is TiO 2 , Fe is Fe 2 O 3 , Si is SiO 2 In addition, when the ceramic sintered body contains other metal elements, the amounts are converted into representative metal oxides of the respective elements.
[0027] Next, an example of a method for producing a ceramic sintered body according to the present disclosure will be described.
[0028] Particulate or powdered Al 2 O 3 , TiO 2 and Fe 2 O 3 and SiO as a sintering aid. 2 At least one of CaO and MgO is added. The particle size of each raw material powder may be, for example, 0.1 μm to 5 μm.
[0029] The resulting slurry is granulated using a spray dryer, and a molded body of a desired shape is produced using the granules. The molded body can be produced by a known method such as press molding.
[0030] The firing temperature during firing may be, for example, 1350° C. or higher and 1550° C. or lower. The firing time may be, for example, about 2 hours. The firing atmosphere may be air.
[0031] Ceramic sintered bodies with different compositions were prepared and the volume resistivity, reflectivity, and * , b * As an indicator of mechanical strength, three-point bending strength was measured.
[0032] First, Al 2 O 3 powder and TiO 2 powder and Fe 2 O 3 powder and SiO 2 Powder, CaO powder, and MgO powder were prepared.
[0033] In the sintered ceramics, the oxide of Al (Al 2 O 3 ) equivalent, Fe oxide (Fe 2 O 3 ) equivalent, Ti oxide (TiO 2 ) converted to silicon oxide (SiO 2 The powder was weighed so that the mass ratios of the powder in terms of Ca, CaO, and Mg were the values shown in Table 1.
[0034] Next, water and an optional binder were added to each weighed powder, and the mixture was mixed and stirred. The resulting slurry was then granulated using a spray dryer, and the granules were then molded to obtain a molded body having the desired shape.
[0035] Next, the compacts were fired in a firing furnace in an air atmosphere, i.e., an oxidizing atmosphere, to obtain sintered bodies for each sample. The firing temperature was in the range of 1350°C to 1550°C, and the firing time was 2 hours.
[0036] Next, each sample was measured using XRD to confirm the presence of aluminum oxide (alumina). Also, for each sample, Al, Si, Ca, Mn, Ti, Fe, and Mg were measured using an ICP atomic emission spectrometer to determine the content of each element, and the determined element content was converted to the content of each oxide, and the content of each element shown in Table 1 was calculated. Note that ICP atomic emission spectroscopic analysis may be simply referred to as ICP.
[0037] The volume resistivity of the resulting sintered body was measured by a three-terminal method using a commercially available electrical resistance measuring instrument, for example, a super insulation resistance meter DSM-8104 manufactured by HIOKI. The results are shown in Table 1.
[0038] The reflectance of the resulting sintered body was measured in the visible light range using a color difference meter, for example, CR-13 manufactured by Konica Minolta. The results are shown in Table 1.
[0039] The obtained sintered body was subjected to a CIE1976 (L) test in accordance with JIS Z 8722-2000. * a * b * ) based on color space a * and b * are measured at wavelengths of 400 nm to 700 nm using a spectrophotometer, for example, a CM-700dl manufactured by Konica Minolta, * and b * The measurement results are shown in Table 1. The notation (%) shown in Table 1 is an abbreviation for mass % except for reflectance.
[0040] Furthermore, the three-point bending strength of the obtained sintered body was measured in accordance with JIS R 1601-2008, and the results are shown in Table 1.
[0041] The measured values for each sample shown in Table 1 are measured values for the baked surface except for sample No. 17, which is a measured value for the mirror surface of a sample having the same composition as sample No. 16.
[0042]
[0043] As shown in sample No. 1, TiO 2 Conversion and Fe 2 O 3 When the total amount of Ti and Fe contained is less than 10 mass %, the volume resistivity is 1.0 × 10 11 The resulting ceramic sintered body had a low semiconductivity, exceeding Ωcm.
[0044] Furthermore, as shown in sample No. 6, TiO 2 Conversion and Fe 2 O 3 When the total amount of Ti and Fe contained exceeded 30 mass % in terms of conversion, the three-point bending strength was less than 260 MPa, and the resulting ceramic sintered body had poor mechanical strength.
[0045] Furthermore, as shown in sample No. 7, TiO 2 / (TiO 2 +Fe 2 O 3 ) is less than 5%, the volume resistivity is 1.0 × 10 11 The resulting ceramic sintered body had a low semiconductivity, exceeding Ωcm.
[0046] Furthermore, as shown in sample No. 12, TiO 2 / (TiO 2 +Fe 2 O 3 ) is more than 20%, a * The blackness of the sintered ceramic body was less than 2.0.
[0047] Furthermore, as shown in sample No. 13, SiO 2 When the total of at least one of Si, Ca, and Mg is less than 0.5 mass % in terms of Si, Ca, and Mg, the volume resistivity is 1.0 × 10 11 The resulting ceramic sintered body had a low semiconductivity, exceeding Ωcm.
[0048] Sample No. 18, which contained MgO, had higher strength than Sample No. 19, which did not contain MgO. When the microstructure was examined, the average crystal grain size of Sample No. 18 was 4.6 μm, which was smaller than the average crystal grain size of Sample No. 19, which had an average crystal grain size of 5.1 μm. The average crystal grain sizes of Samples Nos. 2 to 5, 8 to 11, and 14 to 17 were all within the range of 5 μm to 7 μm.
[0049] Furthermore, as shown in sample No. 20, SiO 2 When the glass contains at least one of Si, Ca, and Mg in a total amount of more than 3.0 mass% in terms of Si, Ca, and Mg, the reflectance is more than 15%, and * and b * The blackness of the sintered ceramic body was less than -2.0, and the blackness was poor.
[0050] Furthermore, the three-point bending strength of sample No. 20 was less than 260 MPa, and the obtained ceramic sintered body had poor mechanical strength.
[0051] In contrast, as shown in Samples Nos. 2 to 5, 8 to 11, and 14 to 19, Al 2 O 3 67 mass % or more of Al converted to TiO 2 Conversion and Fe 2 O 3 The total amount of TiO is 10 mass % or more and 30 mass % or less in terms of TiO 2 / (TiO 2 +Fe 2 O 3 ) is 5% or more and 20% or less Ti and Fe, and SiO 2 The ceramic sintered body contains at least one of Si, Ca, and Mg in a total of 0.5 mass % or more and 3.0 mass % or less in terms of Si, Ca, and Mg, calculated as a CaO equivalent and a MgO equivalent, and has a volume resistivity of 1.0 × 10 4 Ωcm or more and 1.0×10 11 The three-point bending strength was 260 MPa or more.
[0052] Thus, the ceramic sintered body of the present disclosure has good semiconductivity and physical strength. In addition, the ceramic sintered body of the present disclosure has a reflectance of 15% or less, a * and b* was −2.0 or more and 2.0 or less, and exhibited a black color.
[0053] For sample No. 16, a disk having dimensions after firing of 30 mm in thickness and 800 mm in diameter was prepared, and five points on the surface of this disk were cut at equal widths in the diametric direction. * , b * The reflectance was measured. This measurement was carried out on the polished surface. The color tone was measured using a spectrophotometer CM-26dg manufactured by Konica Minolta, Inc., at a measurement wavelength of 360 nm to 740 nm.
[0054] As a result of the measurement, the surface roughness Ra after polishing was about 0.2 to 0.6 μm. * The difference between the maximum and minimum values was 0.28. * The difference between the maximum and minimum values of reflectance was 0.31. The difference between the maximum and minimum values of reflectance was 0.68%. As described above, the ceramic sintered body of the present disclosure has small color tone differences depending on the location, even in large products.
[0055] In addition, the content of Al is Al 2 O 3 When the converted content was 89.5 mass % or less, a ceramic sintered body with low volume resistivity was obtained.
[0056] The present disclosure has been described in detail above, but the present disclosure is not limited to the above-described embodiments, and various modifications, improvements, etc. are possible within the scope that does not deviate from the gist of the present disclosure.
[0057] Further advantages and modifications will readily occur to those skilled in the art. Therefore, the invention in its broader aspects is not limited to the specific details and representative embodiments shown and described above. Accordingly, various modifications may be made without departing from the spirit or scope of the general inventive concept as defined by the appended claims and their equivalents.
Claims
1. A steel sheet comprising Al, Ti, Fe, and at least one of Si, Ca, and Mg, wherein the Al is 2 O 3 The Ti and Fe are contained in an amount of 67 mass % or more in terms of TiO 2 Conversion and Fe 2 O 3 The total content is 10 mass % or more and 30 mass % or less in terms of TiO 2 / (TiO 2 +Fe 2 O 3 ) is 5% or more and 20% or less, and at least one of the Si, the Ca and the Mg is selected from the group consisting of SiO 2 The total content of CaO and MgO is 0.5% by mass or more and 3.0% by mass or less in terms of CaO, CaO and MgO, and the volume resistivity is 1.0×10 4 Ωcm or more and 1.0×10 11 A ceramic sintered body having a resistivity of Ωcm or less.
2. Volume resistivity is 1.0 x 10 10 The ceramic sintered body according to claim 1 , wherein the resistivity is Ωcm or less.
3. The ceramic sintered body according to claim 1 or 2, having a reflectance of 15% or less.
4. a * and b * The ceramic sintered body according to any one of claims 1 to 3, wherein the coefficient of elasticity is -2.0 or more and 2.0 or less.
5. The ceramic sintered body according to any one of claims 1 to 4, having a three-point bending strength of 260 MPa or more.
Citation Information
Patent Citations
Electric cleaner equipped with rotary brush
JP1989022225A
Black alumina ceramic composition
JP1989042359A
Black alumina sintered compact and method of manufacturing the same
JP2008260645A
Alumina sintered compact and substrate holding board formed by alumina sintered compact
JP2011168420A
Semiconductive ceramic sintered compact
JP2013136503A
Cited By
Optical sensor member and optical sensor device
WO2026094787A1