Manufacturing method of silicon powder using waste silicon sludge, silicon powder for manufacturing secondary battery anode material, and manufacturing system of silicon powder

The method of pulverizing and drying waste silicon sludge under inert conditions addresses the inefficiencies in recycling silicon sludge, producing high-purity silicon powder that maintains stability and performance for secondary batteries.

WO2024225523A1PCT designated stage expired Publication Date: 2024-10-31INNOX ECOM CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/006515
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-28
Filing Date
2023-05-12
Publication Date
2024-10-31

AI Technical Summary

Technical Problem

Waste silicon sludge from the photovoltaic and semiconductor industries is typically discarded due to lack of suitable recycling methods, with existing processes being inefficient, costly, or generating hazardous by-products, and the recovered silicon powder often deteriorates over time due to moisture and organic content, affecting its usability in secondary batteries.

Method used

A method involving pulverization of waste silicon sludge in an air atmosphere followed by drying under an inert gas atmosphere to remove moisture and organic components, using a fluidized bed grinding device and airflow drying with argon or nitrogen, to produce high-purity silicon powder with controlled particle size distribution, preventing agglomeration and maintaining physical properties.

Benefits of technology

This method enables the efficient mass production of high-purity silicon powder that suppresses shrinkage and agglomeration, maintaining physical properties during long-term storage and ensuring reliable performance as an anode material for secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023006515_31102024_PF_FP_ABST
    Figure KR2023006515_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a manufacturing method of a silicon powder using waste silicon sludge, a silicon powder for manufacturing a secondary battery anode material, and a manufacturing system of a silicon powder and, more specifically, to a method capable of efficiently manufacturing a silicon powder with excellent quality, a silicon powder, and a manufacturing system usable therefor, wherein waste silicon sludge, generated in the solar power industry and semiconductor wafer production process, is recovered and upcycled as a useful resource, leading to a silicon powder, which can then be used as an anode material for an energy storage device.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing silicon powder using waste silicon sludge, silicon powder for producing secondary battery negative electrode material, and silicon powder production system

[0001] The present invention relates to a method for manufacturing silicon powder using waste silicon sludge, silicon powder for manufacturing a secondary battery anode material, and a system for manufacturing silicon powder. More specifically, the present invention relates to a method for efficiently manufacturing high-quality silicon powder that can be used as anode material for energy storage devices by manufacturing silicon powder through recovery and recycling (upcycling) of waste silicon sludge generated in the solar power industry and semiconductor wafer production process as a useful resource, and to silicon powder and a manufacturing system that can be used therefor.

[0002] Waste silicon sludge, typically generated in the solar power industry and semiconductor wafer production processes, is simply discarded due to lack of suitable applications. Currently, the main recycling methods known include chemically treating the metal components contained in the waste silicon sludge to dry it, creating low-quality silicon ingots for recycling, or simply drying it and using it as a raw material for refractory materials.

[0003] However, since waste silicon sludge can be purified to increase its purity through refinery, many attempts and methods have been proposed to utilize it in other industries, such as the energy storage industry, rather than sorting and recycling it in the solar power industry.

[0004] Patent No. 10-2261429 proposes a method of removing cutting oil, treating with acid, filtering, and then producing silicon oxide or a silicon / carbon composite. However, the process is complex for industrialization, and a large amount of waste liquid, a by-product of the process, is generated, making mass production difficult.

[0005] Patent Publication No. 10-2021-0058397 discloses a method for manufacturing an active material for an energy storage cathode by dispersing silicon (silicon) sludge in alcohol, separating it by specific gravity, mixing and stirring with a carbon precursor, and spray drying the mixture. Patent Registration No. 10-1650184 discloses a method for manufacturing silicon aggregates by ultrasonic treatment and then recovering silicon particles. However, in this case, there is a problem that the cost of the process, such as a separate heat treatment, increases.

[0006] Meanwhile, waste silicon sludge requires technology to remove organic residues left after cutting, as diamond cutters, lubricants, and coolants are used. Furthermore, the moisture content of recently discharged waste silicon sludge is not consistent and varies widely, necessitating efficient moisture removal.

[0007] Therefore, unlike existing production equipment and process technologies, it is necessary to develop a technology that can overcome the above limitations and efficiently mass-produce silicon powder that can be used as an anode material for energy storage devices by recycling waste silicon sludge.

[0008]

[0009] In addition, silicon powders recovered and purified from waste silicon sludge may exhibit shrinkage, agglomeration, and coagulation of the powder, and their physical properties may deteriorate due to trace amounts of metal and moisture in the silicon powder during long-term storage. Accordingly, when silicon powders recovered and purified from waste silicon sludge are used in the manufacture of secondary battery anode materials, the silicon powders may exhibit reduced dispersibility and increased irreversibility due to issues such as volume expansion.

[0010] Accordingly, a new solution is required to resolve the issues of long-term storage and deterioration of physical properties of silicon powder recovered and purified from waste silicon sludge.

[0011] The purpose of the present invention is to provide a method for manufacturing silicon powder using waste silicon sludge, which can efficiently mass-produce high-purity silicon powder from which foreign substances such as organic components and moisture are removed so that waste silicon sludge can be recycled and used as an anode material for energy storage devices (e.g., secondary batteries).

[0012]

[0013] In addition, another object of the present invention is to provide a novel silicon powder that suppresses shrinkage, agglomeration and clumping of the powder while not causing any deterioration in physical properties even during long-term storage.

[0014]

[0015] In addition, another object of the present invention is to provide a silicon powder manufacturing system capable of efficiently mass-producing high-purity silicon powder from which foreign substances such as organic components and moisture have been removed so that waste silicon sludge can be recycled and used as a cathode material for energy storage devices (e.g., secondary batteries).

[0016]

[0017] The purpose of the present invention is not limited to the aforementioned purposes, and other unmentioned purposes and advantages of the present invention can be understood through the following description and will be more clearly understood through the embodiments of the present invention. Furthermore, it will be readily apparent that the purposes and advantages of the present invention can be realized by the means and combinations thereof set forth in the claims.

[0018] From the viewpoint of solving the above problem, according to one aspect of the present invention, a method for producing silicon powder can be provided, comprising: (a) a step of pulverizing waste silicon sludge supplied as a raw material in an air atmosphere; and (b) a step of drying the resultant product pulverized in step (a) under an inert gas atmosphere to remove moisture.

[0019] The average particle size of the above-mentioned waste silicon sludge may be greater than 0 cm and less than or equal to 20 cm. The particle size D of the resultant product crushed in step (a) 50 The value can be greater than 0 ㎛ and less than or equal to 50 ㎛.

[0020] The above step (a) may be one in which separation of moisture and hydrocarbon organic components is performed simultaneously with crushing.

[0021] The above step (a) may be performed in a fluidized bed grinding device.

[0022] Before the above step (a), a step of pre-processing and crushing waste silicon sludge supplied as a raw material (a') may be further included.

[0023] The above step (b) can be performed by an airflow drying method, and the airflow drying method can be performed using an inert gas that does not contain oxygen.

[0024] The above inert gas may include at least one of argon (Ar) gas and nitrogen (N2) gas.

[0025] When the moisture content is 0 wt% or more and 3 wt% or less based on 100 wt% of the total weight of the above-mentioned waste silicon sludge, the step (b) may be performed in a low-temperature airflow manner at a temperature of 20°C or more.

[0026] When the moisture content is more than 3 wt% and less than 80 wt% based on 100 wt% of the total weight of the above-mentioned waste silicon sludge, the step (b) may be performed in a high-temperature airflow manner at a temperature of 60°C or higher.

[0027] The moisture content may be 5 wt% or less and the carbon content may be 10 wt% or less based on 100 wt% of the total weight of the above silicon powder.

[0028] According to another aspect of the present invention, a silicon powder manufactured by a method for manufacturing silicon powder according to an aspect of the present invention can be provided.

[0029] The above silicon powder can be used as a negative electrode material for a secondary battery.

[0030]

[0031] Next, from the viewpoint of solving the above problem, according to another aspect of the present invention, silicon powder is obtained from waste sludge generated in the semiconductor and solar cell manufacturing process, and is D 50 The value is 0.1 ~ 2㎛, D 90 It has a particle size distribution with a value of 0.5 to 5㎛.

[0032] Preferably, the silicon powder for manufacturing a secondary battery negative electrode material of the present invention is D 10 The value is 0.01~0.5㎛, D 100 It can have a particle size distribution with a value of 1 to 10 μm.

[0033] In addition, the silicon powder for manufacturing a secondary battery negative electrode material of the present invention may have a moisture content of less than 2 wt%, a total metal content of less than 2 wt%, and a carbon content of less than 5 wt% based on 100 wt% of the total weight.

[0034]

[0035] Next, from the viewpoint of solving the above problem, a silicon powder manufacturing system according to the present invention includes a rotary kiln having a plurality of cases formed with hollow interiors and arranged in a longitudinal direction, a tube arranged to penetrate the interior of the plurality of cases and rotatable in a horizontal direction, and a heating means for heating the tube arranged inside at least one of the plurality of cases.

[0036] Here, the plurality of cases may include a first case having a heating means for heating the tube disposed therein, a second case without a heating means disposed therein, and a third case having a cooling means for cooling the tube disposed therein.

[0037] Preferably, the first case may include a 1-1 case having a heating means for heating the tube to a temperature range of 100 to 200°C, a 1-2 case having a heating means for heating the tube to a temperature range of 200 to 500°C, and a 1-3 case having a heating means for heating the tube to a temperature range of 500 to 1000°C.

[0038] Here, the rotary kiln may further include a raw material supply device that supplies silicon powder raw material and gas to the inside of the tube, and the raw material supply device may include a raw material input unit into which silicon powder raw material is input and stored, a raw material transfer unit that supplies silicon powder raw material stored in the raw material input unit to the tube, and a gas supply unit that supplies gas to the inside of the tube.

[0039] Preferably, the gas may comprise an inert gas.

[0040] In addition, the tube can operate by repeating forward and reverse rotation under any conditions so that the silicon powder raw material inside is not discharged.

[0041] In addition, the manufacturing system of the present invention may further include a drying device configured to dry and crush waste silicon sludge.

[0042] Here, the drying and crushing device may include a dryer for drying waste silicon sludge, a rotary crusher having a rotary blade for crushing waste silicon sludge, and a fluidized bed crusher for crushing waste silicon sludge by collision of fluid flows, including a funnel-shaped guide tube whose diameter becomes narrower from the top to the bottom, and preferably, the guide tube may have a lower portion inclined at an angle of 10 to 20° based on the upper portion.

[0043] Additionally, the drying and grinding device may further include a cyclone particle separator, a fine particle collector and a scrubber.

[0044] The method for producing silicon powder using waste silicon sludge of the present invention has the advantage of being able to efficiently dry waste silicon sludge having various moisture contents and simultaneously remove foreign substances such as organic components, thereby efficiently producing high-quality silicon powder that can be used in secondary batteries, in order to solve the problems and limitations of the prior art described above.

[0045]

[0046] In addition, the silicon powder of the present invention is a silicon powder for use as a negative electrode material for a secondary battery, and the size distribution of the particles is strictly controlled, so that shrinkage, agglomeration, and clumping of the powder are suppressed.

[0047] In addition, the silicon powder for secondary battery negative electrode material of the present invention does not show any deterioration in physical properties even when stored for a long period of time.

[0048] In addition, the silicon powder for secondary battery anode materials of the present invention exhibits excellent dispersibility without deterioration in physical properties when used as anode materials. Accordingly, the silicon powder for secondary battery anode materials of the present invention can ensure reliability and reproducibility when used as anode materials.

[0049]

[0050] In addition, the silicon powder manufacturing system of the present invention has the advantage of being able to efficiently dry waste silicon sludge having various moisture contents and simultaneously remove foreign substances such as metal components and organic components, thereby efficiently producing high-quality silicon powder that can be used in secondary batteries, in order to solve the problems and limitations of the conventional technology described above.

[0051]

[0052] In addition to the effects described above, specific effects of the present invention are described below while explaining specific details for carrying out the invention.

[0053] FIG. 1 is a simplified flow chart illustrating a method for manufacturing silicon powder using waste silicon sludge according to one embodiment of the present invention.

[0054] FIG. 2 is a simplified flow chart illustrating a method for manufacturing silicon powder using waste silicon sludge according to another aspect of the present invention.

[0055] FIG. 3 is a cross-sectional view schematically illustrating a rotary kiln included in a silicon powder manufacturing system according to one embodiment of the present invention.

[0056] FIG. 4 is a conceptual diagram schematically illustrating a drying and crushing device included in a silicon powder manufacturing system according to one embodiment of the present invention.

[0057] Figure 5 is a conceptual diagram schematically illustrating a silicon powder manufacturing system according to the present invention.

[0058]

[0059] The above-described purposes, features and advantages are described in detail below, so that a person having ordinary knowledge in the technical field to which the present invention pertains can easily implement the technical idea of ​​the present invention.

[0060] In describing the present invention, if it is determined that a detailed description of a known technology related to the present invention may unnecessarily obscure the gist of the present invention, a detailed description thereof will be omitted.

[0061] Any details not described in this specification that can be sufficiently technically inferred by a person skilled in the art will be omitted.

[0062] As used herein, singular expressions include plural expressions unless the context clearly dictates otherwise. As used herein, terms such as "comprises," "contains," and "has (haves)" should not be construed to necessarily include all components described in the specification, and should be construed to mean that some of the components may not be included, or that additional components may be included.

[0063]

[0064] <Method for producing silicone powder>

[0065]

[0066] First, a method for producing silicon powder using waste silicon sludge according to one embodiment of the present invention will be described in detail.

[0067]

[0068] Referring to FIG. 1, the present invention can provide a method for producing silicon powder using waste silicon sludge, comprising: (a) a step of crushing waste silicon sludge supplied as a raw material in an air atmosphere; and (b) a step of drying the crushed result in step (a) under an inert gas atmosphere to remove moisture.

[0069]

[0070] (a) Step

[0071] Waste silicon sludge coagulates into a so-called filter cake state, and exists as a mixture of coagulants of various sizes. In addition, waste silicon sludge exists in a state containing moisture because it is left outside, and if the moisture is not removed, there is a problem that a silicon dioxide (SiO2) oxide film may form on the silicon surface. Furthermore, metal blades such as diamond cutters used for cutting silicon wafers, and hydrocarbon organic substances such as lubricants and coolants used for cutting remain in the waste silicon sludge, so foreign substances including metal components and carbon-based organic substances also remain in the waste silicon sludge.

[0072] Therefore, in step (a), a process can be performed to separate clumped particles of waste silicon sludge supplied as raw material and to crush silicon sludge particles that are already relatively small into even finer particles.

[0073] The average particle size of the waste silicon sludge, which is the raw material supplied above, may be, for example, in the range of more than 0 cm and less than 20 cm, for example, in the range of more than 0 cm and less than 15 cm, for example, in the range of more than 0 cm and less than 10 cm, but is not necessarily limited thereto, and may exist in a substantially mixed and agglomerated state of various particle sizes.

[0074] Particle size D of the result crushed in the above step (a) 50 The value may be in the range of more than 0 ㎛ and less than or equal to 50 ㎛, for example, more than 0 ㎛ and less than or equal to 30 ㎛, for example, more than 0 ㎛ and less than or equal to 10 ㎛, but is not necessarily limited thereto. The powder pulverized in this way can suppress shrinkage, agglomeration, and coagulation, and can suppress deterioration of physical properties due to oxidation, etc., which may be caused by trace amounts of hydrocarbons, moisture, etc. that may remain in the silicon powder even during long-term storage.

[0075] Above D 50 The value means the particle size (size) value that accounts for 50% of the particle size (size) in the order of smallest particle size in the particle distribution of the entire powder. In the present invention, D 50 The value is based on the value measured by adding 10 to 20 wt% of the sample to be measured based on 100 wt% of IPA solvent, treating it with ultrasonic waves for 10 to 30 minutes, and then analyzing it with a particle size analyzer (Cilas).

[0076] The crushing device that can be used in the above step (a) is not particularly limited as long as it can satisfy the average particle size of the result after the crushing described above, but it is preferable that a process for separating foreign substances such as hydrocarbon organic components including moisture can be performed simultaneously with the crushing.

[0077] For example, in the step (a), it is preferable to use a fluidized bed crusher, and as a more specific example, a cyclone device can be used. Specifically, the waste silicon sludge supplied in the step (a) can be finely broken down through a particle-to-particle collision process in the fluidized bed crusher along with the high-speed gas, and at this time, hydrocarbon organic components, moisture, etc. attached to the silicon sludge fall off in the form of fine particles, so that as a result, the silicon sludge is pulverized and at the same time, there is an advantage in that the foreign substances can be separated.

[0078] Optionally, if the silicon sludge particles, which are the raw material supplied, contain a very excessive amount of moisture, a high-temperature air stream (e.g., below approximately 400°C) may be supplied to the grinding device together with the grinding process in step (a) so that some of the moisture can be removed.

[0079] Referring to FIG. 2 according to one embodiment of the present invention, in order to more effectively carry out the pulverization process of step (a), if the waste silicon sludge supplied as a raw material has excessive agglomeration or a large amount of sludge with large particle sizes, a step of (a') preprocessing and pulverizing the waste silicon sludge may be further included before step (a). In this way, a total of two steps of pulverization may be performed including the (a') preprocessing pulverization step and the (a) pulverization step, or only the (a) pulverization step may be performed alone, which may be selected depending on the particle agglomeration state and particle size state of the waste silicon sludge provided as a raw material.

[0080] For example, the above (a') pretreatment grinding step can be performed in a general grinding device, and the average particle size of the pretreatment grinded result can be, for example, in a range of more than 0 cm and less than 15 cm, for example, in a range of more than 0 cm and less than 3 cm, for example, in a range of more than 0 cm and less than 1 cm, but is not necessarily limited thereto.

[0081] The crushing device that can be used in the above step (a') is not particularly limited, but may include, for example, a ball mill, a bead mill, a blade mill, an air mill, a jet mill, a rod mill, a roller mill, a jaw crusher, an impact crusher, a wheeler mill, a hammer mill, etc.

[0082]

[0083] (b) Step

[0084] Step (b) is a drying process performed under an inert gas atmosphere to more effectively remove moisture from the result of step (a).

[0085] According to one embodiment of the present invention, in order to quickly dry the moisture, the step (b) may be performed using a hot air stream drying method that vaporizes and removes moisture using a high-speed flow of high-temperature gas, and an inert gas from which oxygen has been removed may be used in the gas supplied in the air stream drying method to prevent further oxidation. Since the present invention uses an inert gas in the air stream drying method, the drying method can be performed under an inert gas atmosphere.

[0086] According to one embodiment of the present invention, the inert gas in step (b) may include at least one of argon (Ar) gas and nitrogen (N2) gas, and for example, airflow drying may be performed using nitrogen gas.

[0087] Waste silicon sludge is left outside and exists in a moisture-containing state. Since it is discharged from various solar power industries and numerous factories, the moisture content contained in the waste silicon sludge is not constant.

[0088] Meanwhile, since the drying process to remove moisture requires the application of heat energy along with airflow drying, it is desirable to control the temperature during drying differently depending on the moisture content of the waste silicon sludge in order to maximize energy efficiency, which has recently emerged as an important issue.

[0089] According to one embodiment of the present invention, when the moisture content is 0 wt% or more and 3 wt% or less based on 100 wt% of the total weight of the waste silicon sludge, the step (b) may be performed by a low-temperature airflow method, and may be, for example, a temperature of 20°C or more, for example, a temperature of 40°C or more, for example, a temperature of 60°C or more, but is not necessarily limited thereto. In addition, since it is a process for removing moisture, the upper limit of the temperature condition of the low-temperature airflow method is not specifically set, but from the viewpoint of energy efficiency, in order not to use an excessive heat source, it may be, for example, a temperature of 200°C or less, for example, a temperature of 150°C or less, for example, a temperature of 120°C or less, but is not necessarily limited thereto.

[0090] According to one embodiment of the present invention, when the moisture content is more than 3 wt% and less than 80 wt% based on 100 wt% of the total weight of the waste silicon sludge, the step (b) may be performed by a high-temperature airflow method, and may be, for example, a temperature of 80°C or higher, for example, a temperature of 100°C or higher, for example, a temperature of 200°C or higher, for example, a temperature of 300°C or higher, but is not limited thereto. In addition, since it is a process for removing moisture, the upper limit of the temperature condition of the high-temperature airflow method is not specifically set, but from the viewpoint of energy efficiency, in order not to use an excessive heat source, it may be, for example, a temperature of 500°C or lower, for example, a temperature of 400°C or lower, for example, a temperature of 350°C or lower, but is not necessarily limited thereto.

[0091] The airflow drying of step (b) above can supply gas under atmospheric pressure conditions, and the flow rate of the supplied gas can be adjusted depending on the equipment selected.

[0092] The method for manufacturing silicon powder of the present invention can further improve the quality of the silicon powder produced by introducing the dry powder into a hydrogen reduction furnace and performing hydrogen reduction to remove a silicon oxide film existing on the surface of the silicon powder.

[0093] The method for manufacturing the silicon powder of the present invention may be performed in one device in which steps (a) and (b) can be performed continuously, depending on the device for manufacturing the silicon powder. For example, the device may be designed so that the drying step is performed together with the grinding or sequentially in one device manufactured by attaching a grinding device to the top of the cyclone device.

[0094] In the silicon powder obtained through steps (a) and (b) according to the manufacturing method of the present invention, the moisture content may be, for example, 5 wt% or less, for example, 3 wt% or less, for example, 2 wt% or less, based on 100 wt% of the total weight of the silicon powder, and the carbon content may be, for example, 10 wt% or less, for example, 8 wt% or less, for example, 5 wt% or less, so as to exhibit excellent quality.

[0095] The silicon powder of the present invention can be used as a material for an energy storage device, and for example, can be used as a negative electrode material for a secondary battery.

[0096]

[0097] <Silicone powder>

[0098]

[0099] Next, a silicon powder according to another embodiment of the present invention will be described in detail. The silicon powder according to another embodiment of the present invention can preferably be used as a secondary battery negative electrode material.

[0100]

[0101] The silicon powder for a secondary battery negative electrode material of the present invention is a silicon powder obtained from waste sludge generated during the semiconductor and solar cell manufacturing process, and D50 The value is 0.1 ~ 2㎛, D 90 It has a particle size distribution with a value of 0.5 to 5㎛.

[0102]

[0103] Here, D 50 value, D 90 The values ​​represent the particle size (size) values ​​that account for 50% and 90% of the total powder distribution, respectively, in descending order of particle size (size). The above D 50 Value and D 90 The values ​​can be measured using the Cilas equipment.

[0104]

[0105] The silicon powder for a secondary battery anode material of the present invention is obtained by recovering and purifying waste sludge generated during the semiconductor and solar cell manufacturing process, and in particular, has a controlled particle size distribution.

[0106]

[0107] D of the silicon powder for the secondary battery negative electrode material of the present invention 50 The value is 0.1 ~ 2㎛, D 90 The particle size is controlled to be 0.5 to 5 μm, which suppresses shrinkage, agglomeration, and coagulation of the powder, and can suppress deterioration of physical properties that may occur due to trace amounts of metal and moisture in the silicon powder even during long-term storage. In addition, the silicon powder for secondary battery anode materials with particle size control as described above can ensure reliability and reproducibility when used as a material for secondary battery anode materials.

[0108]

[0109] D of the silicon powder for the secondary battery negative electrode material of the present invention 50 The value is controlled to be 0.1 to 2 μm, preferably 0.3 to 1 μm, and more preferably 0.5 to 0.9 μm.

[0110] In addition, D of the silicon powder for the secondary battery negative electrode material of the present invention 90The value is controlled to 0.5 to 5 μm, preferably 0.8 to 4 μm, and more preferably 1 to 3.5 μm.

[0111] As described above, silicon powder for secondary battery anode materials with controlled size distribution suppresses shrinkage, agglomeration, and coagulation of the powder, and suppresses deterioration of physical properties that may occur due to trace amounts of metal and moisture within the silicon powder even during long-term storage. In addition, silicon powder for secondary battery anode materials with controlled particle size as described above can ensure reliability and reproducibility when used as a material for secondary battery anode materials.

[0112]

[0113] Also preferably, the silicon powder for the secondary battery negative electrode material of the present invention is D 10 The value is 0.01~0.5㎛, D 100 It can have a particle size distribution with a value of 1 to 10 μm.

[0114]

[0115] In addition, the silicon powder for a secondary battery negative electrode material of the present invention is obtained from waste sludge generated during the semiconductor and solar cell manufacturing process as described above, and thus impurities and moisture contained in the raw material are removed.

[0116]

[0117] Accordingly, the silicon powder for a secondary battery negative electrode material of the present invention preferably has a moisture content of less than 2 wt% based on 100 wt% of the total weight through a moisture removal process, and more preferably, the moisture content may be less than 1 wt%.

[0118]

[0119] In addition, the silicon powder for a secondary battery negative electrode material of the present invention may contain trace amounts of metals such as Al, Fe, and Cu in ppm units, but the silicon powder for a secondary battery negative electrode material of the present invention may contain less than 2 wt% of the above metal components, and more preferably less than 1 wt%.

[0120]

[0121] Preferably, the silicon powder of the present invention can be manufactured from the method for manufacturing silicon powder according to one embodiment of the present invention described above.

[0122]

[0123] <Silicon Powder Manufacturing System>

[0124]

[0125] Next, a system for manufacturing silicon powder according to another embodiment of the present invention will be described in detail.

[0126]

[0127] rotary kiln

[0128]

[0129] Referring to FIG. 3, the silicon powder manufacturing system of the present invention includes a rotary kiln (100). First, the rotary kiln (100) included in the manufacturing system of the present invention will be described in detail.

[0130]

[0131] Referring to FIG. 3, the silicon powder manufacturing system of the present invention includes a rotary kiln (100) having a plurality of cases (10) formed with a hollow interior and arranged in a longitudinal direction, a tube (20) arranged to penetrate the interior of the plurality of cases (10) and rotatable in a horizontal direction, and a heating means (H) for heating the tube (20) arranged inside at least one of the plurality of cases (10).

[0132]

[0133] Referring to Fig. 3, the plurality of cases (10) have hollow spaces formed inside and are each arranged in the longitudinal direction, that is, in the horizontal direction.

[0134] In Fig. 3, the plurality of cases (10) are illustrated in a box shape, but the shape of the cases (10) is not particularly limited as long as it has a structure surrounding the tube (20).

[0135] A heating means (H) for heating the tube (20) is arranged inside at least one of the plurality of cases (10). Although not limited thereto, the heating means (H) may be formed in a coil shape that surrounds the tube, as illustrated in FIG. 3.

[0136] As illustrated in FIG. 3, the plurality of cases (10) are arranged in the longitudinal direction and can each apply heat to the tube (20) in a different temperature range. Accordingly, the plurality of cases (10) can provide a temperature gradient in the longitudinal direction of the tube (20).

[0137] Preferably, the plurality of cases (10) may include a first case (11) in which a heating means (H) for heating the tube (20) is disposed inside, and a second case (30) in which no heating means is disposed.

[0138] Here, the first case (11) may include a 1-1 case (12) equipped with a heating means (H) for heating the tube (20) to a temperature range of 100 to 200°C, a 1-2 case (13) equipped with a heating means (H) for heating the tube (20) to a temperature range of 200 to 500°C, and a 1-3 case (14) equipped with a heating means (H) for heating the tube (20) to a temperature range of 500 to 1000°C.

[0139] Accordingly, the plurality of cases (10) can provide a temperature gradient of various temperature ranges to the tube (20).

[0140] In addition, the plurality of cases (10) may further include a third case (not shown) having a cooling means (not shown) for cooling the tubes disposed therein. Here, a device such as a cooling module may be used as the cooling means.

[0141]

[0142] Next, referring to FIG. 3, the rotary kiln (100) of the present invention includes a tube (20) that is arranged to penetrate the interior of the plurality of cases (10) and is rotatable in a horizontal direction.

[0143] The above tube (20) may be formed as a cylindrical tube with an empty interior. However, the cross-section of the tube (20) is not necessarily limited to a circle, and may have various shapes such as a triangle, square, and hexagon.

[0144] The raw material of silicon powder moves along the longitudinal direction inside the tube (20). The silicon powder can move along the longitudinal direction inside the tube (20) by rotating the tube (20). To this end, a screw-shaped partition wall may be formed inside the tube (20) to allow the silicon powder to move. In addition, the tube (20) may be arranged at an angle to facilitate the movement of the silicon powder.

[0145] The above tube (20) is arranged to penetrate the interior of the plurality of cases (10). As described above, the plurality of cases (10) can provide a temperature gradient of various temperature ranges to the tube (20). Accordingly, the silicon powder moving along the longitudinal direction inside the tube (20) can be heat-treated in various temperature ranges by the heat supplied from the plurality of cases.

[0146]

[0147] In addition, referring to FIG. 3, the rotary kiln (100) may further include a raw material supply device that supplies silicon powder raw material and gas to the inside of the tube (20).

[0148] Preferably, the raw material supply device may include a raw material input unit (41) into which silicon powder raw material is input and stored, a raw material transfer unit (42) for supplying the silicon powder raw material stored in the raw material input unit (41) to the tube (20), and a gas supply unit (43) for supplying gas into the inside of the tube.

[0149] Here, the gas may include an inert gas, and the inert gas may include at least one of argon (Ar) gas and nitrogen (N2) gas, and for example, nitrogen gas may be used.

[0150]

[0151] Referring to FIG. 3, the silicon powder raw material passing through the tube (20) can be discharged from the discharge port (60), and the remaining gas can be separated by the residual gas separator (50).

[0152]

[0153] In addition, the rotary kiln (100) of the present invention can operate so that the silicon powder raw material inside is not discharged by repeating forward and reverse rotation of the tube (20) under any conditions.

[0154] Here, the above arbitrary condition may be, for example, a condition under which a failure signal of the rotary kiln (100) is generated.

[0155] The operation of the tube (20) as above can be controlled from a control device (not shown) that controls the rotary kiln (100).

[0156]

[0157] Drying and crushing equipment

[0158]

[0159] Next, referring to FIG. 4, the silicon powder manufacturing system of the present invention may further include a drying and crushing device (200) configured to dry and crush waste silicon sludge.

[0160]

[0161] The above drying and crushing device (200) refers to a device configured to dry and crush waste silicon sludge.

[0162] Referring to FIG. 4, the drying and crushing device (200) may include a dryer for drying waste silicon sludge, a rotary crusher having a rotary blade for crushing waste silicon sludge, and a fluidized bed crusher for crushing waste silicon sludge by collision of fluid flows, including a funnel-shaped guide tube whose diameter becomes narrower from the top to the bottom.

[0163] Here, it is preferable that the lower part of the induction tube has an angle of 10 to 20° with respect to the upper part.

[0164] In addition, the drying and grinding device (200) may further include a cyclone particle separator, a fine particle collector, and a scrubber.

[0165]

[0166] The waste silicon sludge is first fed into a dryer, and the dryer dries the waste silicon sludge with hot air at 200 to 250°C.

[0167] Next, the dried waste silicon sludge is pulverized by the rotary crusher and the fluidized bed crusher. As described above, the waste silicon sludge is first pulverized by the rotating blade of the rotary crusher, and then the waste silicon sludge is pulverized by the fluidized bed crusher. At this time, the fluidized bed crusher is supplied with a high-temperature, high-speed fluid at a speed of 25 to 30 m 3 / hr, and the high temperature, high speed fluid may be nitrogen gas.

[0168]

[0169] The silicon powder discharged from the fluidized bed crusher can pass through the cyclone particle separator, fine particle collector, and scrubber in that order.

[0170] As described above, the silicon powder discharged from the fluidized bed mill is separated by a cyclone particle separator and transferred to a fine particle collector. Fine particles that are difficult to collect by the cyclone particle separator are ultimately collected through a bag filter (not shown), and ultrafine particles that pass through the bag filter can ultimately be collected and discharged by a scrubber.

[0171] At this time, in order to induce smooth airflow and crush silicon particles, it is desirable for the lower part to have an angle of inclination of 10 to 20 degrees based on the upper part, and for example, it can have an angle of inclination of approximately 15 degrees. The silicon in the form of a lump moves along with the airflow of high-temperature nitrogen gas through the upper part of the funnel-shaped tube as described above and falls to the lower part, and the gas reaches the lower part while being compressed to a certain volume through the funnel-shaped tube, and the gas speed increases by up to 20% or more compared to the inflow speed, which can act as a driving force to high-speed rotational wear of the silicon in the form of a lump.

[0172] The lower part of the fluidized bed crusher is configured as a gentle funnel-shaped bottom with an inclined angle with respect to the ground, and is configured so that large lumps of silicon gather in the center, and lumps pouring from the upper part to the lower part can naturally collide and be crushed with the lumps gathered in the center of the lower part.

[0173] Meanwhile, the unseparated lump of silicon filter cake continues to rotate at the bottom of the fluidized bed mill, undergoing drying, rotation, collision, and separation processes until the particles are finally dried and separated.

[0174] However, if too many silicon particles are supplied, there is a problem that rotation stops and they accumulate at the bottom, blocking the flow. Considering these points, the supply speed of silicon raw material for drying is preferably approximately 70 to 120 kg / hr. If the supply speed of silicon raw material exceeds 120 kg / hr, there is a problem that drying quality may deteriorate and silicon lumps may not be properly decomposed and crushed. On the other hand, if the supply speed of raw material is less than 70 kg / hr, the production yield may decrease, which may lead to a decline in mass productivity.

[0175]

[0176] Referring to FIG. 5, FIG. 3 illustrates a conceptual diagram of a silicon powder manufacturing system according to the present invention. The silicon powder manufacturing system of the present invention includes the rotary kiln (100) described above, and may preferably include a drying and grinding device (200) for drying and grinding silicon powder raw materials.

[0177] The silicon powder raw material that has passed through the above-described drying and crushing device (200) is moved to the above-described rotary kiln (100) and undergoes heat treatment. The silicon powder raw material that has been heat-treated by the above-described rotary kiln (100) is ultimately purified so that it can be used as a material for a negative electrode of an energy storage device (e.g., a secondary battery).

[0178]

[0179] In addition, preferably, the manufacturing system of the silicon powder of the present invention can be used in the manufacturing method of the present invention described above, and can be used in manufacturing the silicon powder of the present invention described above.

[0180]

[0181] Below, the structure and operation of the present invention will be described in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be construed as limiting the present invention in any way.

[0182]

[0183] <Example>

[0184]

[0185] 1. Manufacturing of silicon powder

[0186]

[0187] (1) Example 1

[0188] As a feedstock, 100 kg of filter cake of silicon powder with a moisture content of 45 wt% was prepared, and crushing was performed at room temperature (23-25°C), at a speed of 30-60 Hz / bead, and at a supply speed of 3-10 kg / min using a roll mill crushing device (manufacturer: Inox Ecom Co., Ltd.) having a 2-axis crushing shaft (wet) and a 1-axis tunnel crushing shaft (wet).

[0189]

[0190] The above-mentioned crushed silicon powder was fed into a cyclone device (manufacturer: Inox Ecom Co., Ltd.). The drying temperature of the dryer was set to 60°C, and hot air nitrogen gas stream drying was performed using nitrogen gas for less than 5 minutes.

[0191]

[0192] The characteristics of the silicon powder manufactured in this way according to Example 1 are as shown in Table 1 below.

[0193]

[0194] (2) Examples 2 to 3, Comparative Examples 1 to 3

[0195] Silicon powder was manufactured in the same manner as in Example 1, but silicon powders of Examples 2, 3, and Comparative Examples 1 to 3 having particle size distributions as shown in Table 1 below were manufactured.

[0196]

[0197] Particle size distribution (㎛)Moisture content (wt%)Metal content (wt%)Carbon content (wt%)D 10 D 50 D 90 D 100Example 10.210.841.513.230.610.050.55 Example 20.290.992.324.800.710.050.76 Example 30.311.312.594.910.760.050.67 Comparative Example 11.202.54.85.170.880.050.66 Comparative Example 21.171.85.16.980.770.050.77 Comparative Example 31.492.76.48.210.770.050.77

[0198]

[0199] The particle size distribution of the silicon powder described in Table 1 above was measured using a Cilas device.

[0200]

[0201] Additionally, the moisture content of the silicon powder was analyzed by measuring the weight change of the sample in a drying oven. The metal content was measured using an ICP-OES instrument, and the carbon content was measured using a carbon analyzer (CS995).

[0202]

[0203] 2. Physical property evaluation

[0204]

[0205] The dispersion stability of the silicon powder according to the above-described examples and comparative examples was evaluated.

[0206]

[0207] Each silicon slurry was prepared using the silicon powders of Examples 1 to 3 and Comparative Examples 1 to 3.

[0208] Specifically, by mixing each silicon powder and NMP, a slurry prepared to have a silicon content of 10 wt% was treated with 20 kHz ultrasonic waves at a power of 500 Watt in a continuous circulation mode for 30 minutes to prepare a silicon slurry using the silicon powders of Examples 1 to 3 and Comparative Examples 1 to 3.

[0209]

[0210] In order to evaluate the dispersion stability of the above silicone slurry, each silicone slurry was stored in a graduated cylinder and observed over time to determine whether layer separation occurred. The height excluding the clear upper liquid layer separated into the upper layer was measured as a % of the initial height. The results of measuring and calculating the height excluding the clear upper liquid layer separated into the upper layer as a % of the initial height are described in Table 2 below.

[0211]

[0212] Example 1 Example 1 Example 1 Comparative Example 1 Comparative Example 1 Comparative Example 1 Height ratio excluding the separated clear upper liquid layer [%] 878687747170

[0213]

[0214] Looking at the test results as above, it can be confirmed that the examples according to the present invention have superior long-term storage safety compared to the comparative examples.

[0215] Therefore, the silicon powder according to the present invention has excellent long-term storage stability, prevents deterioration of physical properties, and can be used for manufacturing a negative electrode material with excellent reversibility.

[0216]

[0217] While the present invention has been described as above, it is clear that the present invention is not limited to the embodiments disclosed herein, and that various modifications can be made by those skilled in the art within the scope of the present invention's technical concept. Furthermore, even if the operational effects according to the configuration of the present invention have not been explicitly described while describing the embodiments of the present invention, it is natural that the effects predictable by the corresponding configuration should also be acknowledged.

[0218]

[0219] [Explanation of symbols]

[0220] 100: Rotary Kiln

[0221] 10: Case

[0222] 11: Case 1

[0223] 12: Case 1-1

[0224] 13: Case 1-2

[0225] 14: Case 1-3

[0226] 20: Tube

[0227] 30: Case 2

[0228] 41: Raw material input section

[0229] 42: Raw material transfer section

[0230] 43: Gas supply section

[0231] 50: Residual gas separator

[0232] 60: outlet

[0233] 200: Drying and crushing device

Claims

1. (a) A step of grinding waste silicon sludge supplied as raw material in an air atmosphere; and (b) a step of drying under an inert gas atmosphere to remove moisture from the resultant product crushed in step (a); Method for manufacturing silicon powder.

2. In paragraph 1, The average particle size of the above waste silicon sludge is greater than 0 cm and less than 20 cm, Particle size D of the result crushed in the above step (a) 50 The value is greater than 0 ㎛ and less than or equal to 50 ㎛, Method for manufacturing silicon powder.

3. In paragraph 1, The above step (a) is a process in which separation of moisture and hydrocarbon organic components is carried out simultaneously with crushing. Method for manufacturing silicon powder.

4. In paragraph 1, The above step (a) is performed in a fluidized bed grinding device, Method for manufacturing silicon powder.

5. In paragraph 1, Before the above step (a), further comprising a step of pre-processing and crushing waste silicon sludge supplied as a raw material (a'). Method for manufacturing silicon powder.

6. In paragraph 1, The above step (b) is performed by air drying, The above airflow drying method is performed using an inert gas that does not contain oxygen. Method for manufacturing silicon powder.

7. In paragraph 6, The above inert gas includes at least one of argon (Ar) gas and nitrogen (N2) gas. Method for manufacturing silicon powder.

8. In paragraph 1, When the moisture content is 0 wt% or more and 3 wt% or less based on 100 wt% of the total weight of the above-mentioned waste silicon sludge, the step (b) is performed in a low-temperature airflow manner at a temperature of 20°C or more. Method for manufacturing silicon powder.

9. In paragraph 1, When the moisture content is more than 3 wt% and less than 80 wt% based on 100 wt% of the total weight of the above waste silicon sludge, the step (b) is performed in a high-temperature airflow manner at a temperature of 60°C or higher. Method for manufacturing silicon powder.

10. In paragraph 1, The moisture content is 5 wt% or less and the carbon content is 10 wt% or less based on 100 wt% of the total weight of the above silicon powder. Method for manufacturing silicon powder.

11. Silicon powder obtained from waste sludge generated during the semiconductor and solar cell manufacturing process. D 50 The value is 0.1 ~ 2㎛, D 90 Having a particle size distribution of 0.5 to 5㎛ Silicon powder for manufacturing secondary battery negative electrode materials.

12. In paragraph 11, The above silicon powder D 10 The value is 0.01~0.5㎛, D 100 Having a particle size distribution of 1 to 10 μm Silicon powder for manufacturing secondary battery negative electrode materials.

13. In paragraph 11, Based on 100% of total weight Moisture content less than 2% by weight Silicon powder for manufacturing secondary battery negative electrode materials.

14. In paragraph 11, Based on 100% of total weight The total metal content contained is less than 2 wt% Silicon powder for manufacturing secondary battery negative electrode materials.

15. In paragraph 11, Based on 100% of total weight Carbon content less than 5% by weight Silicon powder for manufacturing secondary battery negative electrode materials.

16. A plurality of cases arranged lengthwise with a hollow interior, A tube that is arranged to penetrate the inside of the above plurality of cases and can rotate in a horizontal direction; and A rotary kiln comprising a heating means for heating the tube is arranged inside at least one of the plurality of cases; Manufacturing system for silicon powder.

17. In paragraph 16, The above multiple cases A first case having a heating means for heating the tube disposed therein, and A second case comprising no heating means arranged therein Manufacturing system for silicon powder.

18. In paragraph 17, The above multiple cases A third case including a cooling means for cooling the above tube is disposed inside. Manufacturing system for silicon powder.

19. In Article 17 The first case above A first case having a heating means for heating the above tube to a temperature range of 100 to 200°C, A first-second case having a heating means for heating the above tube to a temperature range of 200 to 500°C, and A case 1-3 comprising a heating means for heating the above tube to a temperature range of 500 to 1000°C. Manufacturing system for silicon powder.

20. In Article 16 The above heating means Formed in a coil shape that wraps around the above tube Manufacturing system for silicon powder.

21. In Article 16 The above rotary kiln Further comprising a raw material supply device for supplying silicon powder raw material and gas to the inside of the above tube, The above raw material supply device A raw material input section where silicon powder raw material is input and stored; A raw material transfer unit that supplies silicon powder raw material stored in the raw material input unit to the tube, and A gas supply unit that supplies gas inside the above tube is included. Manufacturing system for silicon powder.

22. In Article 21 The above gas contains an inert gas. Manufacturing system for silicon powder.

23. In Article 16 The above tube Under any conditions By repeating forward and reverse rotation It operates to prevent the silicon powder raw material inside from being discharged. Manufacturing system for silicon powder.

24. In Article 16 Further comprising a drying and crushing device configured to dry and crush waste silicon sludge. Manufacturing system for silicon powder.

25. In paragraph 24 The above drying and grinding device A dryer for drying waste silicon sludge, A rotary crusher having a rotary blade for crushing waste silicon sludge and A fluidized bed crusher that crushes waste silicon sludge by the collision of fluid flows, including a funnel-shaped guide tube whose diameter narrows from top to bottom. Manufacturing system for silicon powder.

26. In Article 25 The above induction tube The lower part has an angle of 10 to 20 degrees relative to the upper part. Manufacturing system for silicon powder.

27. In Article 25 The above drying and grinding device Further including a cyclone particle separator, a fine particle collector and a scrubber. Manufacturing system for silicon powder.

Citation Information

Patent Citations

  • Method for recovering of silicon particles, and manufacturing of cathode material for secondary battery

    KR101650184B1

  • Multi layer ceramic condenser and electronic component package having the same

    KR1020220151316A

  • Method for manufacturing silicon oxides from waste silicon sludge using spray drying method

    KR102261429B1

  • Rotary kiln

    KR1020160073648A

  • Memory device and operating method thereof

    KR1020200106748A