Double metal cyanide catalyst prepared using hydrogen hexacyanocobaltate

The two-step process for producing a DMC catalyst with a specific composition addresses the challenges of reproducibility and activity in conventional DMC catalyst production, resulting in efficient and high-quality polyether-polyol and poly(ether-co-carbonate) polyol synthesis by minimizing by-product formation and enhancing catalyst activity.

WO2024225546A1PCT designated stage expired Publication Date: 2024-10-31AJOU UNIV IND ACADEMIC COOP FOUND
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/018813
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-26
Filing Date
2023-11-21
Publication Date
2024-10-31

Smart Images

  • Figure KR2023018813_31102024_PF_FP_ABST
    Figure KR2023018813_31102024_PF_FP_ABST
Patent Text Reader

Abstract

The present application relates to a double metal cyanide catalyst with a Zn-OR group, and a double metal cyanide catalyst with a zinc acetate group.
Need to check novelty before this filing date? Find Prior Art

Description

Double metal cyanide catalyst manufactured using hydrogen hexacyanocobaltate

[0001] The present invention relates to a DMC (double metal cyanide complex) catalyst used as a catalyst for manufacturing polyether-polyol, a raw material for polyurethane, and as a copolymerization catalyst for CO2 / epoxide.

[0002] DMC (double metal cyanide complex) catalysts are widely used commercially for the ring-opening polymerization of propylene oxide (PO). Materials produced using DMC catalysts, namely polyether polyols, are produced at a scale of approximately 10 million tons annually and are used as polyurethane materials. DMC catalysts are not only active in epoxide homo-ring-opening polymerization but also reactive in CO2 / epoxide copolymerization, making them effective for CO2-utilizing reactions.

[0003] Typically, a DMC catalyst is manufactured by reacting K3Co(CN)6 and an excess of ZnCl2 in an aqueous solution (or a H2O / tBuOH mixed solvent) according to the following reaction scheme 1 to form a precipitate and isolating it.

[0004] [Reaction Formula 1]

[0005]

[0006] In this regard, multiple washing processes using a mixed H2O / tBuOH solvent and a single tBuOH solvent are necessary to completely remove the byproduct KCl to achieve high activity. During the washing process, not only KCl but also ZnCl2 is lost, so a significantly excess of ZnCl2 is added to produce the product compared to the amount required by the reaction formula.

[0007] The DMC catalyst manufactured through the conventional process described above is generally known to have a composition of Zn3[(CN)6Co]·a(ZnCl2)·x(H2O)·y(tBuOH)·z(Ligand), and depending on the amount of ZnCl2 added, the degree of washing, and even the mixing method, materials having different a, x, y, and z values ​​are obtained, and the a, x, y, and z values ​​significantly affect the catalytic activity and selectivity. That is, manufacturing a DMC catalyst by reacting K3Co(CN)6 and ZnCl2 has many problems in terms of reproducibility, reliability, and ease.

[0008] To overcome these problems, a method for producing a DMC catalyst using H3Co(CN)6 has been attempted. In one example of U.S. Patent Publication No. 7,022,641, a method for producing a DMC catalyst by reacting H3[Co(CN)6], ZnO, and ZnCl2 according to the following reaction scheme 2 is disclosed.

[0009] [Reaction Formula 2]

[0010]

[0011] The above reaction scheme 2 has the advantage that since H2O is produced as a by-product, there is no need for a tedious washing process (centrifugation or filtration process) to remove the KCl by-product. That is, in an aqueous solution containing a small amount (4 wt%) of trimethylolpropane, H3[Co(CN)6], After reacting ZnO and ZnCl2, the solvent was removed by vacuum distillation to obtain a DMC catalyst. The composition of the DMC catalyst obtained at this time is that all of the zinc components added are included in the DMC catalyst because it did not go through a filtration process, and therefore, Zn formed through the neutralization process of H3[Co(CN)6] and ZnO 1.5It is presented as a mixture of 0.33 equivalents of ZnO remaining after reacting with Co(CN)6, 1.7 equivalents of ZnCl2, the used solvent H2O, and the additionally added ligand [trimethylolpropane or poly(propylene glycol)], and showed a low conversion rate of 6% in PO polymerization, showing very low activity.

[0012] As shown in the following reaction scheme 3, H3[Co(CN)6] A method for preparing a DMC catalyst by reacting 2 equivalents of ZnCl2 with methanol was reported (Journal of Polymer Science, Part A: Polymer Chemistry 2013, 51, 4811; Kr 10-2015-0010602).

[0013] [Reaction Formula 3]

[0014]

[0015] Specifically, when high-purity H3Co(CN)6 is produced and reacted with 2 equivalents of ZnCl2, HCl is produced as a byproduct, which can be easily removed together with methanol by vacuum depressurization, allowing for the easy production of a DMC catalyst without a cleaning process. However, toxic HCl is produced as a byproduct during the production process, and its activity in polymerization reactions is low, making it insufficient for commercial use.

[0016] It has also been disclosed that a DMC catalyst can be easily prepared without a filtration process by reacting high-purity H3Co(CN)6 with 2 to 4 equivalents of Zn(2-ethylhexanoate)2 in methanol and then removing the methanol by vacuum decompression (Scheme 4; Journal of CO2 Utilization 53 (2021) 101755; Kr 10-2021-0092753). The DMC catalyst prepared in this way also has low activity, which is insufficient for commercial use.

[0017] [Reaction Formula 4]

[0018]

[0019] In the late 1990s, an upgraded DMC catalyst capable of producing polyols with an unsaturation level (i.e., mmol of -OCH2CH=CH2 terminal groups per gram of polymer produced) of as low as 0.005 meq / g was developed, which facilitated commercialization. The upgraded DMC was reported to be due to the use of ZnCl2 containing ZnO impurities (US Patent 5,783,513), and later showed a characteristic 640 cm in the infrared (IR) spectrum. -1 By observing the signal, it was suggested that the upgraded DMC has a Zn-OH group (US Patent 6,063,897).

[0020] In EP 1510534 B1, H3[Co(CN)6] was prepared in an aqueous solution in which tert-butanol, isopropanol, or 1-methoxy-2-propanol was dissolved as a ligand at a concentration of 1.3 mol / L (9.7 wt%, 7.9 wt%, 12 wt%). It is known that a method of manufacturing a DMC catalyst is disclosed by reacting Zn(OH)2 and ZnCl2 in a molar ratio of 1:2:8, filtering and separating the precipitate, dispersing it again in a solvent, treating it with polypropylene glycol, and filtering it again. It was confirmed through IR analysis that the obtained DMC catalyst has a Zn-OH group, and the composition of the obtained DMC catalyst does not contain ZnCl2 (i.e., it is all washed out during the filtration process) [Zn 2+ ] x [(CN)6Co 3- ] y[OH]·(L) (2x + 1 = y; L is isopropanol, sec-butanol (sec-BuOH), or tert-butanol (tert-BuOH)).

[0021] The present invention is intended to solve the problems of the above-mentioned conventional technology, (NC)6Co 3- , (AcO)Zn + , and Zn 2+ Contains components, and additionally ClZn + and / or (RO)Zn + (R is C1-C 20 Alkyl ether or C1-C 20 The purpose of the present invention is to provide a double metal cyanide (DMC) catalyst containing an alkyl component.

[0022] In addition, the present invention aims to provide a method for producing the above DMC catalyst.

[0023] In addition, the present invention aims to provide a method for producing polyether polyol using the above DMC catalyst.

[0024] In addition, the present invention aims to provide a method for producing poly(ether-co-carbonate) polyol using the above DMC catalyst.

[0025] However, the technical tasks to be achieved by the embodiments of the present invention are not limited to the technical tasks described above, and other technical tasks may exist.

[0026] As a technical means for achieving the above-mentioned technical task, the first aspect of the present invention aims to provide a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 1:

[0027] [Chemical Formula 1]

[0028] [ClZn + ] (1-p) [(RO)Zn + ] p [Zn 2+][(NC)6Co 3- ]

[0029] (In the above chemical formula 1,

[0030] p is between 0.1 and 1.0,

[0031] R is C1-C 20 Alkyl ether or C1-C 20 (Alkyl).

[0032] According to one embodiment of the present invention, the p value in the chemical formula 1 may be 0.25 to 0.75, but is not limited thereto.

[0033] According to one embodiment of the present invention, in the chemical formula 1, R may be tert-Bu, but is not limited thereto.

[0034] According to one embodiment of the present invention, in the chemical formula 1, R may be MeOC3H6, but is not limited thereto.

[0035] In addition, the second aspect of the present invention provides a method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 1, comprising: a first step of mixing H3Co(CN)6 and ZnCl2 in a 1-methoxy-2-propanol solvent containing 30 wt% or less of water to form a precipitate and filtering the precipitate; a second step of reacting the precipitate obtained in the first step with lithium phenoxide (PhOLi) in a ROH solvent containing 50 wt% or less of water and then filtering the precipitate to remove byproduct LiCl and obtain a solid compound; and a third step of drying the solid compound obtained in the second step by vacuum depressurization;

[0036] [Chemical Formula 1]

[0037] [ClZn + ] (1-p) [(RO)Zn + ] p [Zn 2+ ][(NC)6Co3- ]

[0038] (In the above chemical formula 1,

[0039] p is between 0.1 and 1.0,

[0040] R is C1-C 20 Alkyl ether or C1-C 20 (Alkyl).

[0041] According to one embodiment of the present invention, the molar ratio of H3Co(CN)6 and ZnCl2 in the first step may be 1:2, but is not limited thereto.

[0042] According to one embodiment of the present invention, the molar ratio of H3Co(CN)6 introduced in the first step and PhOLi introduced in the second step may be 1:0.25 to 1:0.75, but is not limited thereto.

[0043] According to one embodiment of the present invention, the reaction temperature of the first step may be 50°C to 80°C, but is not limited thereto.

[0044] According to one embodiment of the present invention, the vacuum drying temperature of the third step may be from 20°C to 100°C, but is not limited thereto.

[0045] In addition, the third aspect of the present invention aims to provide a method for producing a polyether polyol, comprising the steps of: producing a double metal cyanide (DMC) catalyst by the method according to the second aspect of the present invention; and polymerizing propylene oxide in the presence of a polyol starter using the DMC catalyst.

[0046] According to one embodiment of the present invention, the polyol starter may be, but is not limited to, polypropylene glycol having a molecular weight of 300 to 800.

[0047] Also, the fourth aspect of the original is (NC)6Co 3- , (AcO)Zn + , and Zn2+ Contains components, and additionally ClZn + and / or (RO)Zn + (R is C1-C 20 Alkyl ether or C1-C 20 A double metal cyanide (DMC) catalyst containing an alkyl component is provided.

[0048] According to one embodiment of the present invention, the (AcO)Zn + The components were observed at 1618, 1583, 1554, 1463, 1443, and 1355 cm in the ATR-FTIR spectrum. -1 It may be measured in, but is not limited to,

[0049] According to one embodiment of the present invention, R may be, but is not limited to, tert-butyl.

[0050] According to one embodiment of the present invention, (tert-BuO)Zn + The component is detected at 640 cm in the ATR-FTIR spectrum. -1 It may be measured in the vicinity, but is not limited thereto.

[0051] According to one embodiment of the present invention, the double metal cyanide (DMC) catalyst is (NC)6Co 3- , (AcO)Zn + , Zn 2+ and (tert-BuO)Zn + Ingredients may include, but are not limited to:

[0052] According to one embodiment of the present invention, the (NC)6Co 3- , (AcO)Zn + , Zn 2+ and (tert-BuO)Zn + A double metal cyanide (DMC) catalyst comprising a component may have a composition represented by the following chemical formula 2, but is not limited thereto:

[0053] [Chemical Formula 2]

[0054] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [Zn 2+ ] a [(NC)6Co 3- ]

[0055] (In the above chemical formula 2,

[0056] p is 0.1 to 1.2;

[0057] q is 0.01 to 0.9;

[0058] p + q is 0.9 to 1.2;

[0059] (p + q + 2a is 3).

[0060] According to one embodiment of the present invention, p may be from 0.3 to 0.98; and q may be from 0.01 to 0.75, but is not limited thereto.

[0061] According to one embodiment of the present invention, p may be 0.90 to 0.98; and q may be 0.01 to 0.10, but is not limited thereto.

[0062] According to one embodiment of the present invention, the double metal cyanide (DMC) catalyst is (NC)6Co 3- , (AcO)Zn + , Zn 2+ , (tert-BuO)Zn + and ClZn + Ingredients may include, but are not limited to:

[0063] According to one embodiment of the present invention, the (NC)6Co 3- , (AcO)Zn + , Zn 2+ , (tert-BuO)Zn + and ClZn + A double metal cyanide (DMC) catalyst comprising a component may have a composition represented by the following chemical formula 3, but is not limited thereto:

[0064] [Chemical Formula 3]

[0065] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [ClZn + ] r [Zn 2+ ] a [(NC)6Co 3- ]

[0066] (In the above chemical formula 3,

[0067] p is 0.3 to 0.8;

[0068] q is 0.2 to 0.5;

[0069] r is 0.05 to 0.5;

[0070] p + q + r is 0.9 to 1.2;

[0071] (p + q + r + 2a is 3).

[0072] According to one embodiment of the present invention, p may be 0.4 to 0.8; q may be 0.2 to 0.5; and r may be 0.1 to 0.3, but is not limited thereto.

[0073] Also, the fifth aspect of the present invention is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound consisting of the components, lithium acetate (AcOLi) and acetic acid in a tert-butanol (tert-BuOH) solvent containing less than 30 wt% of water, is prepared by reacting the ClZn + Provided is a method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 2, which comprises the steps of adding 1 equivalent and 1 to 0.4 equivalents of each component, reacting them, filtering to obtain a solid compound, and removing the residual solvent by vacuum depressurization:

[0074] [Chemical Formula 2]

[0075] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [Zn 2+ ] a [(NC)6Co 3- ]

[0076] (In the above chemical formula 2,

[0077] p is 0.1 to 1.2;

[0078] q is 0.01 to 0.9;

[0079] p + q is 0.9 to 1.2;

[0080] (p + q + 2a is 3).

[0081] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOCH2CH(Me)OH], but is not limited thereto.

[0082] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of components may be prepared by reacting H3Co(CN)6 and ZnCl2 in a molar ratio of 1:2, but is not limited thereto.

[0083] Also, the sixth aspect of the present invention is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound consisting of ClZn, lithium acetate (AcOLi) and acetic acid in a tert-butanol (tert-BuOH) solvent containing less than 30 wt% of water+ A method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 3 is provided, which comprises the steps of adding 0.95 to 0.5 equivalents and 0.95 to 0.5 equivalents of each component, reacting them, filtering them to obtain a solid compound, and removing the remaining solvent by vacuum depressurization:

[0084] [Chemical Formula 3]

[0085] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [ClZn + ] r [Zn 2+ ] a [(NC)6Co 3- ]

[0086] (In the above chemical formula 3,

[0087] p is 0.3 to 0.8;

[0088] q is 0.2 to 0.5;

[0089] r is 0.05 to 0.5;

[0090] p + q + r is 0.9 to 1.2;

[0091] (p + q + r + 2a is 3).

[0092] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOCH2CH(Me)OH], but is not limited thereto.

[0093] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+A double metal cyanide (DMC) compound composed of components may be prepared by reacting H3Co(CN)6 and ZnCl2 in a molar ratio of 1:2, but is not limited thereto.

[0094] In addition, the seventh aspect of the present invention provides a method for producing a polyether polyol, comprising the steps of: preparing a double metal cyanide (DMC) catalyst according to any one of the fifth to sixth aspects of the present invention; and polymerizing propylene oxide in the presence of a polyol starter using the DMC catalyst.

[0095] According to one embodiment of the present invention, the polyol starter may be, but is not limited to, polypropylene glycol having a molecular weight of 300 to 800.

[0096] In addition, the eighth aspect of the present invention provides a method for producing a poly(ether-co-carbonate) polyol, comprising the steps of: preparing a double metal cyanide (DMC) catalyst according to any one of the fifth and sixth aspects of the present invention; and copolymerizing propylene oxide and CO2 in the presence of a polyol starter using the DMC catalyst.

[0097] According to one embodiment of the present invention, the polyol starter may be, but is not limited to, polypropylene glycol having a molecular weight of 300 to 800.

[0098] The above-described problem-solving methods are merely exemplary and should not be construed as limiting the present invention. In addition to the exemplary embodiments described above, additional embodiments may be included in the drawings and detailed description of the invention.

[0099] The DMC catalyst according to the present invention is (RO)Zn + (In the formula, R is C1-C 20 Alkyl ether or C1-C 20Since it contains an alkyl component, it has the advantage of minimizing the formation of a monool chain having an allyl ether (-OCH2CH=CH2) terminal while minimizing the generation of harmful impurities with a molecular weight of 100,000 or more when manufacturing a polyol by polymerizing propylene oxide.

[0100] In addition, the DMC catalyst according to the present invention is (AcO)Zn + When manufacturing a polyol by polymerizing propylene oxide, including the component, it has a low degree of unsaturation and produces less high molecular weights of 100,000 or more, so that a polyol with a narrow molecular weight distribution can be manufactured with high activity, and when manufacturing a polyol by copolymerizing propylene oxide and CO2, it has the advantage of being able to increase the CO2 content while minimizing the formation of cyclic carbonate, which is a byproduct, with high activity.

[0101] However, the effects that can be obtained from this center are not limited to the effects described above, and other effects may exist.

[0102] Figure 1 shows SEM images and XRD patterns of DMC compounds prepared by reacting H3Co(CN)6 and 2.0 eq ZnCl in 10:1 MeOC3H6OH / H2O for a) 1 hour, b) 15 hours, and c) 7 days, d) DMC compounds prepared by reacting H3Co(CN)6 with 1.0 eq ZnCl2 and 1.5 eq ZnO in 5:1 MeOC3H6OH / H2O for 15 hours, and e) DMC compounds prepared by reacting H3Co(CN)6 with 1.0 eq ZnCl2 and 1.5 eq ZnO in 10:1 MeOC3H6OH / H2O.

[0103] Figure 2a shows [ClZn] in which the solvent was replaced with tert-butanol. + ][Zn 2+ ][(NC)6Co 3- ][tBuOH] ([DMC-Cl][tBuOH]) IR spectrum, and 2b is [(tBuO)Zn obtained by reacting 1.0 equivalent of PhOLi with [DMC-Cl][MeOC3H6OH] compound in 88:12 tBuOH / H2O solvent. + ] [Zn2+ ][(NC)6Co 3- ] is the IR spectrum of the catalyst, 2c is the IR spectrum of the catalyst prepared using a deuterated solvent (88:12 tBuOD / D2O), 2d is the IR spectrum of the catalyst of 2c after exposure to water vapor, and 2e is the IR spectrum of the (tBuO)2Zn compound.

[0104] Figure 3 [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOC3H6OH] ([DMC-Cl][MeOC3H6OH]) compound was reacted with 0.25, 0.50, 0.75, and 1.0 equivalents of PhOLi to obtain [(MeOC3H6O)Zn + ] p [ClZn + ] (1-p) [Zn 2+ ][(NC)6Co 3- ] (p = 0.25, 0.50, 0.75, 1.0) shows the IR spectrum.

[0105] Figure 4a is a SEM image and XRD pattern of the [DMC-Cl][MeOC3H6OH] compound, and Figures 4b to 4e are SEM images and XRD patterns of [(MeOC3H6O)Zn] obtained by reacting 0.25, 0.50, 0.75, and 1.0 equivalents of PhOLi with the [DMC-Cl][MeOC3H6OH] compound, respectively. + ] p [ClZn + ] (1-p) [Zn 2+ ][(NC)6Co 3- ] shows the SEM image and XRD pattern of [DMC-(OC3H6OMe / Cl) (p / 1-p)] (p = 0.25, 0.50, 0.75, 1.0).

[0106] Figure 5 shows SEM images and XRD patterns of a) DMC-(OtBu / Cl)(0.5 / 0.5), b) [DMC-Cl][tBuOH], and c) DMC-OtBu prepared using the [DMC-Cl][MeOC3H6OH] compound.

[0107] Figure 6 is [(MeOC3H6O)Zn + ][Zn 2+ ][(NC)6Co 3- ] (DMC-OC3H6OMe) shows the structure of the DMC catalyst revealed by analyzing the XRD signal using the Rietveld Refinement method.

[0108] FIGS. 7a to 7c are ATR-FTIR spectra of DMC catalysts according to Comparative Example 2, Comparative Example 3 and Example 1 of the present disclosure, 7d is an ATR-FTIR spectrum of DMC catalyst according to Comparative Example 4, 7e is an ATR-FTIR spectrum of DMC catalyst according to Example 6-1, and 7f is an ATR-FTIR spectrum of DMC catalyst according to Example 6-4.

[0109] FIG. 8a is an ATR-FTIR spectrum of DMC including AcO units prepared by reacting DMc-OtBu with pure AcOH, 8b is an ATR-FTIR spectrum of DMC including AcO units prepared by reacting K3Co(CN)6 with 2.0 eq (AcO)2Zn in 4 M AcOH / H2O, and 8c to 8g are ATR-FTIR spectra of DMC catalysts according to Examples 6-1 to 6-5 of the present disclosure, respectively.

[0110] FIG. 9a is a SEM image and XRD pattern of a DMC catalyst including Zn-OAc units prepared by reacting [DMC-OtBu] with pure AcOH, FIG. 9b is a SEM image and XRD pattern of a DMC catalyst including Zn-OAc units prepared by reacting [DMC-Cl][MeOC3H6OH] with 1:1 AcOLi / AcOH (DMC-OAc), and FIG. 9c is a SEM image and XRD pattern of a DMC catalyst including Zn-OAc units prepared by reacting K3Co(CN)6 with 2.0 eq (AcO)2Zn in 4 M AcOH / H2O according to a conventional method.

[0111] Figures 10a to 10e are SEM images and XRD patterns of DMC catalysts according to Examples 6-1 to 6-5 of the present application, respectively, and Figure 10f is a SEM image and XRD pattern of DMC catalyst according to Comparative Example 4 of the present application.

[0112] Fig. 11a is a SEM image and XRD pattern of a DMC catalyst according to Example 6-1 of the present application, and Figs. 11b to 11f are SEM images and XRD patterns of a DMC catalyst according to Examples 7-1 to 7-5 of the present application, respectively.

[0113] FIG. 12a is an ATR-FTIR spectrum of a DMC catalyst according to Example 6-1 of the present application, and FIGS. 12b to 12f are ATR-FTIR spectra of a DMC catalyst according to Examples 7-1 to 7-5 of the present application, respectively.

[0114] FIG. 13a is a GPC curve of a polyether polyol manufactured using a DMC catalyst according to an example and a comparative example of the present disclosure, and FIG. 13b is a GPC curve of a poly(ether-co-carbonate) polyol manufactured using a DMC catalyst according to an example and a comparative example of the present disclosure.

[0115] FIG. 14a is a GPC curve of a polyether polyol manufactured using a DMC catalyst according to one embodiment of the present disclosure, and FIG. 14b is a GPC curve of a poly(ether-co-carbonate) polyol manufactured using a DMC catalyst according to one embodiment of the present disclosure.

[0116] FIG. 15a is a GPC curve of a polyether polyol manufactured using a DMC catalyst according to an example and a comparative example of the present disclosure, and FIG. 15b is a GPC curve of a poly(ether-co-carbonate) polyol manufactured using a DMC catalyst according to an example and a comparative example of the present disclosure.

[0117] Figures 16a and 16b are GPC curves showing the effect of removing catalyst residue using magnesium silicate / polyacrylic acid / water on polyether polyols prepared using a DMC catalyst (DMC-(OAc / OtBu / Cl)(0.59 / 0.38 / 0.15)) according to Example 7-3 of the present disclosure and a DMC catalyst (benchmark DMC) according to Comparative Example 1, respectively.

[0118] Figure 17 is an ATR-FTIR spectrum of a DMC catalyst according to a) Example 6-2 of the present application (DMC-(OAC / OtBu)(0.95 / 0.08)), b) Example 6-1 of the present application (DMC-(OAC / OtBu)(0.97 / 0.02)) heated at 60°C under vacuum, and c) Example 6-1 of the present application (DMC-(OAC / OtBu)(0.97 / 0.02)).

[0119] Figure 18 is a dispersion image of a polyol obtained from PO / CO2 copolymerization using a DMC catalyst according to a) Example 6-2 of the present invention (DMC-(OAc / OtBu)(0.95 / 0.08)), b) Comparative Example 6 (Zn2[Co(CN)6](CH3COO)·4H2O), and c) Example 6-1 (DMC-(OAC / OtBu)(0.97 / 0.02)).

[0120] Below, with reference to the attached drawings, an embodiment of the present invention is described in detail so that a person having ordinary knowledge in the technical field to which the present invention pertains can easily carry out the present invention.

[0121] However, the present invention can be implemented in various different forms and is not limited to the embodiments described herein. In order to clearly explain the present invention in the drawings, parts irrelevant to the description have been omitted, and similar parts have been designated with similar drawing reference numerals throughout the specification.

[0122] Throughout this specification, when a part is said to be "connected" to another part, this includes not only cases where it is "directly connected" but also cases where it is "electrically connected" with another element in between.

[0123] Throughout this specification, when it is said that a member is located “on,” “above,” “upper,” “lower,” “lower” or “lower” another member, this includes not only cases where the member is in contact with the other member, but also cases where another member exists between the two members.

[0124] Throughout this specification, whenever a part is said to "include" a component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.

[0125] The terms "about," "substantially," and the like, as used herein, are used to mean at or near the numerical value when manufacturing and material tolerances inherent to the meanings referred to are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures that contain precise or absolute numerical values ​​to aid understanding of the present disclosure. Furthermore, throughout the present disclosure, the terms "step of ~" or "step of ~" do not mean "step for ~."

[0126] Throughout this specification, the term "combination thereof" included in the expressions in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expressions in the Makushi format, and means including one or more selected from the group consisting of said components.

[0127] Throughout this specification, references to “A and / or B” mean “A or B, or A and B.”

[0128] Hereinafter, the present invention's double metal cyanide (DMC) catalyst, its preparation method, and its preparation method for polyether polyol and poly(ether-co-carbonate) polyol using the same will be described in detail with reference to embodiments, examples, and drawings. However, the present invention is not limited to these embodiments, examples, and drawings.

[0129]

[0130] As a technical means for achieving the above-mentioned technical task, the first aspect of the present invention provides a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 1:

[0131] [Chemical Formula 1]

[0132] [ClZn + ] (1-p) [(RO)Zn + ] p [Zn 2+ ][(NC)6Co 3- ]

[0133] (In the above chemical formula 1,

[0134] p is between 0.1 and 1.0,

[0135] R is C1-C 20 Alkyl ether or C1-C 20 (Alkyl).

[0136] Typically, DMC catalysts are prepared by reacting K3Co(CN)6 and an excess of ZnCl2 to form a precipitate as described in the background art above, and are known to have a composition of Zn3[(CN)6Co]·a(ZnCl2)·x(H2O)·y(tert-BuOH)·z(Ligand) (USP 5,783,513; USP 5,789,626; Eur. Polym. J. 2011, 47, 2152). The DMC catalyst provided in the present invention is prepared by reacting 1-methoxy-2-propanol solvent and (RO)Zn + It differs from conventional DMC catalysts in terms of its components.

[0137] In one embodiment of the US patent (US 7,022,641 B2) mentioned in the above background art, a method for producing a DMC catalyst by reacting H3[Co (CN)6], ZnO, and ZnCl2 is disclosed, and the composition of the obtained material is Zn formed through the neutralization process of H3[(CN)6Co] and ZnO without any filtration or washing process. 1.5 [Co(CN)6], the remaining 0.33 equivalents of ZnO after reaction, 1.7 equivalents of ZnCl2, the used solvent H2O, and the additionally added ligand [trimethylolpropane or poly(propylene glycol)] are presented as a mixture (Scheme 2). The DMC catalyst of the chemical formula 1 provided by the present invention is ClZn + Ingredients and (RO)Zn + (In the formula, R is C1-C 20 Alkyl ether or C1-C 20 It is different from the DMC catalyst provided in the above-mentioned US patent example because it has an alkyl component. In addition, the DMC catalyst disclosed in the above-mentioned US patent shows a 6% lower conversion rate in PO polymerization, and is also different in terms of efficiency from the highly active DMC catalyst disclosed in the present invention.

[0138] H3[Co(CN)6] mentioned in the European patent (EP 1510534 B1) mentioned in the above background technology [Zn] obtained by reacting Zn(OH)2 and ZnCl2 in water solvent 2+ ] x [(CN)6Co 3- ] y [HO - ]·(solvent) (2x + 1 = y) The catalyst of the composition is limited to the solvent contained in isopropanol, sec-butanol (sec-BuOH) or tert-butanol (tert-BuOH), so the catalyst provided by the present invention is (RO)Zn + (In the formula, R is C1-C 20Alkyl ether or C1-C 20 alkyl) components and ClZn + It is different from the catalyst provided by the above invention in terms of the components contained therein.

[0139] A method for producing a DMC catalyst using ZnCl2 containing 0.2 to 2.0 wt% of ZnO according to a conventional method (reaction scheme 1) has been disclosed. While the DMC catalyst produced in this manner has the advantage of being able to produce a polyol with a very low degree of unsaturation, it has been reported that it produces a gel-like polymer byproduct with a molecular weight of 100,000 or more at a level of 2 to 3%, making it inconvenient to use in a polyol production process and also causing problems in using it for producing polyurethane foam (US 6,063,897 A). Since then, issues regarding the formation of this by-product have been raised in various literature, and attempts have been made to elucidate the formation mechanism of this by-product, and the need for the development of a catalyst that can suppress the formation of high molecular weight by-products with a molecular weight of 100,000 or more has emerged (ChemCatChem 2015, 7 (6), 928-935; Catalysts 2020, 10 (9), 1066; US Patent 6083420).

[0140] The DMC catalyst provided in the above-mentioned U.S. patent (US 6,063,897 A) has the advantage of being able to produce a polyol with a very low degree of unsaturation, but has the disadvantage of producing a polymer byproduct with a molecular weight of 100,000 or more in the form of a gel, and its composition has not been reported, but it is highly likely to contain tert-BuOH because it is a catalyst manufactured using a conventional method (reaction formula 1). The DMC catalyst provided in the present invention is (RO)Zn + (In the formula, R is C1-C 20 Alkyl ether or C1-C 20 It is characterized by containing an alkyl component.

[0141] The DMC catalyst of the above chemical formula 1 is manufactured by a two-step reaction shown in the following reaction scheme 5.

[0142] [Reaction Formula 5]

[0143]

[0144] (MeOC3H6O)Zn using controlled amounts of PhOLi (p = 0.75, 0.50, and 0.25 eq per feed [DMC-Cl][MeOC3H6OH]) + Ingredients and ClZn + A DMC catalyst containing all components could be prepared (Scheme 5). Cl detected in the filtrate - The amount of PhOLi supplied was consistent with the amount of PhOLi supplied in all cases (1.07, 1.00, and 1.08 eq per feed, respectively), and the Cl / Co atomic ratio detected via SEM-EDS was consistent with the Cl remaining in the solid. - The amounts (0.20, 0.56, and 0.89, respectively) were approximately equal. In the ATR-FTIR spectrum, 624 cm -1 ν of Zn-OR The silver gradually increased as the amount of injected PhOLi increased (Fig. 3). 1 H NMR spectra indicate that the isolated catalysts contain approximately the same amount of RO moiety in all cases (1.06, 1.17, and 1.33 eq, respectively). Based on these results, the isolated solid is designated as [ClZn + ] (1-p) [(MeOC3H6O)Zn + ] p [Zn 2+ ][(NC)6Co 3- ][MeOC3H6OH] (1-p) was assigned to. However, the XRD pattern and morphology observed in the SEM image appeared to be a mixture of [DMC-Cl][MeOC3H6OH] and DMC-OC3H6OMe rather than indicating the formation of a completely new phase (Fig. 4).

[0145] Also ClZn+ and (tBuO)Zn + DMC catalyst containing all components in a 1:1 ratio ([(tBuO)Zn + ] 0.5 [ClZn + ] 0.5 [Zn 2+ ][(NC)6Co 3- ][tBuOH] 0.37 ; referred to as DMC-OtBu / Cl(0.5 / 0.5)) was prepared by reacting 0.5 eq of PhOLi with [DMC-Cl][MeOC3H6OH] in 88:12 tBuOH / H2O. Unfortunately, excess Cl ions exceeding the input amount of PhOLi were washed away with the filtrate (1.25 eq per feed). Surprisingly, this occurrence proved to be beneficial for the polymerization process. The XRD pattern of the resulting DMC-(OtBu / Cl)(0.5 / 0.5) was different from those of DMC-OtBu and [DMC-Cl][MeOC3H6OH]. The SEM images were similar but did not appear to be a simple combination of the two (Fig. 5).

[0146] In the first step of the above reaction scheme 5, 1-methoxy-2-propanol, 2-methoxyethanol, 1-ethoxy-2-propanol, or 2-ethoxyethanol containing 30 wt% or less of water can be used as a solvent. However, when 1-methoxy-2-propanol containing 30 wt% or less of water is used, the a value is controlled to be close to 1, that is, within the range of 1.0 to 1.1, and particles having a plate-like shape are formed, thereby exposing many active sites and maximizing catalytic activity, which is preferable. In addition, by controlling the reaction time and the amount of water, the size of the formed particle plates can be controlled, thereby maximizing activity and facilitating the filtration process (Fig. 1). The obtained solid compound had some crystallinity, allowing observation of XRD signals, but the structure could not be interpreted through the signals.

[0147] The DMC compound obtained in the first step contains a certain amount of 1-methoxy-2-propanol used in the first step. 1 This can be seen through H NMR spectrum analysis. That is, when the obtained solid compound is added to a D2O solution containing 4 M NaOD, the solid is completely destroyed and a transparent solution is obtained. 1,6-hexanediol is quantitatively added as a standard substance to this solution. 1 When H NMR is measured, a signal corresponding to 1-methoxy-2-propanol is observed together with a standard substance, and the amount of 1-methoxy-2-propanol contained in the obtained solid compound can be quantified through the integral value. The amount of 1-methoxy-2-propanol contained in the obtained solid compound varies depending on the degree of drying, and the contained 1-methoxy-2-propanol can be desorbed when performing the second step, so its amount or structure does not significantly affect the composition and activity of the final chemical formula 1.

[0148] In the above chemical formula 1, the p value can be controlled by the amount of PhOLi injected. That is, the solid compound obtained in the first step is dispersed in a 1-methoxy-2-propanol solvent, and then the DMC compound obtained in the first step, i.e., [ClZn + ] a [Zn 2+ ] b [(NC)6Co 3- ][menstruum] c ClZn containing (a = 1.0 to 1.1; b = (3 - a) / 2) + When reacted by adding less than the component content, LiCl and PhOH equivalent to the amount of PhOLi added are eluted into the solvent phase, and ClZn + (RO)Zn as much as the amount of PhOLi added +A DMC catalyst converted into a component is generated. The generated DMC catalyst is filtered and dried to obtain the DMC catalyst of the above chemical formula 1. The amount of LiCl eluted corresponding to the amount of PhOLi introduced was confirmed by measuring the amount of AgCl produced by adding an excess amount of AgNO3 to the filtrate. That is, when PhOLi was added in amounts of 0.25, 0.50, 0.75, and 1.0 eq relative to the H3Co(CN)6 introduced in the first step and reacted, the Cl detected in the filtrate - The amounts were 0.27, 0.50, 0.80, and 0.97 eq compared to the H3Co(CN)6 input in the first stage. In addition, Cl was detected to have no Zn component in the filtrate. - This Li + It was inferred that it was paired with ClZn. The Cl / Co molar ratio measured through SEM-EDS analysis of the obtained DMC catalyst + (RO)Zn as much as the amount of PhOLi added + It can be confirmed that the Cl / Co mole ratio was converted into a component. That is, the Cl / Co mole ratio measured in the DMC compound obtained in the first step before reacting with PhOLi was 1.06, but the Cl / Co mole ratio measured after reacting 0.25, 0.50, 0.75, and 1.0 eq of PhOLi with respect to H3Co(CN)6 introduced in the first step was 0.89, 0.50, 0.20, and 0.025, respectively, which is equivalent to the ClZn present in the reactant. + The amount of PhOLi added in the ingredient amount is approximately equal to the limit value.

[0149] ZnCl + The component is (tBuO)Zn + The IR spectrum of the catalyst converted into a component is 3296 cm -1 640 cm with the OH stretching vibration signal of H2O -1Additional signals were observed nearby (Fig. 2b). When the catalyst was prepared using a deuterated solvent (tBuOD containing 12 wt% deuterated water (D2O), the OD stretching vibration signal at 2449 cm in the IR spectrum -1 Moved to 640 cm -1 The signal is 618 cm -1 It was confirmed that the signal shifted to 3296 cm (Fig. 2c). When the catalyst was exposed to water vapor, it shifted back to 3296 cm -1 , 640cm -1 It can be confirmed that it returns to (Fig. 2d). Through these results, [(tBuO)Zn + ][Zn 2+ ][(NC)6Co 3- ] in Zn-OR stretching vibration (ν Zn-OR ) signal. This fact indicates that the IR spectrum of (tBuO)2Zn is 610 cm -1 This can be proven by clearly observing it in (Fig. 2e). 610~640cm -1 ν in the range Zn-OR The fluctuation is due to the hydrogen bonding of water molecules. In the catalyst manufactured using 1-methoxy-2-propanol as a solvent, the 640 cm before PhOLi reaction was observed. -1 No signal was observed nearby, but after PhOLi reaction, a Zn-OR stretching vibration signal was observed, and the signal size increased according to the amount of PhOLi injected (Fig. 3).

[0150] In the above chemical formula 1, the p value is equal to 0.25 to 0.75, i.e., ClZn + A large portion of the composition is (RO)Zn +It is preferable to convert it into a component, as it can produce a polyol with a low degree of unsaturation. In the polyurethane manufacturing industry, a polyol with a low degree of unsaturation is usually preferred. The unsaturation measured in the polyol produced in the present invention is ClZn included in the DMC catalyst. + It was recognized that there is a proportional correlation with the components. That is, [ClZn + ] (1-p) [(RO)Zn + ] p [Zn 2+ ][(NC)6Co 3- ] was manufactured and PO polymerization was performed. When the p value was sequentially increased from 0 to 0.25, 0.50, 0.75, and 1.0, the unsaturation value was sequentially decreased from 0.024 meq / g to 0.018, 0.014, 0.006, and 0.003.

[0151] The obtained catalyst was dissolved in a D2O solution containing 4 M NaOD and then measured. 1 No signal related to PhO was observed in H NMR, indicating that PhOLi is ClZn + The component is (RO)Zn + It was determined that the byproduct PhOH was converted into a component and removed by dissolving in the filtrate. Water was Zn 2+ When coordinated, the acidity increases, the PKa value decreases from 14 to 7~9, and PhOLi, which has a PKa value of about 10, acts as a base to form Zn 2+ Inducing dehydrogenation reaction of water coordinated to (RO)Zn + Forming components and PhOH, Li + is ClZn + Cl contained in the ingredients - It is explained that it is dissolved and removed in solution.

[0152] After PhOLi treatment, a plate-like particle shape similar to that before treatment was observed in SEM, but ClZn + The component is reduced and (RO)Zn +As the composition increases, it is observed that the edges change into a sharp, plate-like shape, and in fact, ClZn + All components are (RO)Zn + The material converted into components showed very well-separated signals in XRD (Fig. 4).

[0153] ClZn + All components are (RO)Zn + DMC catalyst obtained by converting into a component, namely [(MeOC3H6O)Zn + ][Zn 2+ ][(NC)6Co 3- ](DMC-OC3H6OMe) was analyzed using the Rietveld Refinement method, and its structure was interpreted for the first time (Fig. 6).

[0154] ClZn as described above + As the composition increases, the degree of unsaturation increases, which is undesirable, but on the other hand, ClZn + As the component is included, the molecular weight distribution is narrowed and also ClZn + As the amount of components increases, the molecular weight distribution also has the advantage of becoming narrower (Fig. 15).

[0155]

[0156] In addition, the second aspect of the present invention comprises a first step of mixing H3Co(CN)6 and ZnCl2 in a 1-methoxy-2-propanol solvent containing 30 wt% or less of water to form a precipitate and filtering the precipitate to obtain the precipitate; and the precipitate obtained in the first step is mixed with ROH (wherein R is C1-C) containing 50 wt% or less of water. 20 Alkyl ether or C1-C 20The present invention provides a method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 1, comprising: a second step of reacting lithium phenoxide (PhOLi) in an alkyl solvent, filtering the reacted product to remove the byproduct LiCl, and obtaining a solid compound; and a third step of drying the solid compound obtained in the second step under reduced pressure under vacuum.

[0157] [Chemical Formula 1]

[0158] [(RO)Zn + ] p [ClZn + ] (1-p) [Zn 2+ ][(NC)6Co 3- ]

[0159] (In the above chemical formula 1,

[0160] p is between 0.1 and 1.0,

[0161] R is C1-C 20 Alkyl ether or C1-C 20 (Alkyl).

[0162] Regarding the method for manufacturing a DMC catalyst according to the second aspect of the present application, detailed descriptions of parts overlapping with the first aspect of the present application have been omitted, but even if the descriptions have been omitted, the contents described in the first aspect of the present application can be equally applied to the second aspect of the present application.

[0163] DMC catalysts are typically manufactured using K3Co(CN)6. The present invention differs from conventional methods in that it manufactures the DMC catalyst using H3Co(CN)6 instead of K3Co(CN)6. In addition, there is no example of manufacturing a DMC catalyst through a two-step reaction scheme as shown in the above reaction scheme 5. In particular, (RO)Zn is manufactured through the amount of PhOLi added in the second step. + Ingredients and ClZn + There are no examples of manufacturing DMC catalysts with precisely controlled amounts.

[0164] In the method for producing a DMC catalyst according to the present invention, any of the compounds in the form of H3Co(CN)6·(CH3OCH2CH2OH) (x = 1.5 to 4) or H3[Co(CN)6]·x[CH3OH] (x = 1.4 to 1.8) and H3Co(CN)6·x[CH3CH2OH] (x = 2.3 to 2.4) prepared according to a method known in the literature (Journal of CO2 Utilization 53 (2021) 101755; Kr 10-2021-0007885), or compounds prepared using an ion exchange resin (Journal of Polymer Science, Part A: Polymer Chemistry 2013, 51, 4811) may be used, but H3Co(CN)6·x(CH3OCH2CH2OH) (x = 1.5 to 4) may be used. 4) It is preferable to use compounds of this form because they have high purity and can be manufactured in large quantities.

[0165] In the first step, the H3Co(CN)6 compound can be dissolved in 1-methoxy-2-propanol containing less than 30 wt% of water, and ZnCl2 can be reacted therewith to produce a precipitate, and this precipitate can be separated by filtration to obtain the DMC compound obtained at this time. [ClZn + ] a [Zn 2+ ] b [(NC)6Co 3- ][1-methoxy-2-propanol] c It has a composition of (a = 1.0 to 1.1; b = (3 - a) / 2; c = 1.0 to 2.0). If an excess of 30 wt% or more of water is used in the first step, the shape of the generated particles is not uniform and the composition is outside the range, which is not desirable.

[0166] [ClZn obtained in step 1 + ] a [Zn 2+ ] b [(NC)6Co 3-][1-methoxy-2-propanol] c ((a = 1.0 to 1.1; b = (3 - a) / 2; c = 1.0 to 2.0)) is reacted with PhOLi to produce LiCl as a by-product, which must be eluted and removed. This is performed in 1-methoxy-2-propanol containing a relatively large amount of water, i.e., less than 50 wt% of water. If a solvent containing more than 50% of water is used, a catalyst having the composition specified in Chemical Formula 1 is not obtained, and the induction time of the catalyst becomes long, which is not desirable.

[0167] Instead of PhOLi, which is introduced in the second stage, other lithium compounds, such as lithium hydroxide, lithium alkoxide, or lithium aryloxide, may be used, but solubility and unit cost should be taken into consideration, and PhO - There is no advantage to be gained by using other forms of lithium compounds that are complex and expensive, as the component is not incorporated into the catalyst but simply acts as a base and is then removed in the form of PhOH.

[0168] In the first step, when the molar ratio of H3Co(CN)6 and ZnCl2 is 1:2, plate-like particles are formed with an a value close to 1 (i.e., 1.0 to 1.10), which is desirable because a highly active catalyst can ultimately be obtained. That is, when the molar ratio of H3Co(CN)6 and ZnCl2 is less than 1:2, a DMC catalyst with an a value of 1.0 or less is generated, resulting in low activity, and when the molar ratio is 1:2 or more, a substance with an a value close to 1.0 precipitates, and most of the remainder does not react and is washed away through the filtration process, making it meaningless to introduce it at a molar ratio of 1:2 or more.

[0169] The p value of chemical formula 1 (i.e., (RO)Zn) finally obtained with the amount of PhOLi injected in the second step described above +The amount of PhOLi added in the second stage, i.e., when the molar ratio of H3Co(CN)6 added in the first stage and PhOLi added in the second stage is 1:0.25 to 1:0.75, (RO)Zn + ClZn, which contains a lot of components + A DMC catalyst having a small component content is obtained, which is desirable because it enables the production of a polyol with a low degree of unsaturation.

[0170] The third step of drying is performed to provide [ClZn + ] (1-p) [(RO)Zn + ] p [Zn 2+ ][(NC)6Co 3- ] can obtain a DMC catalyst of the composition.

[0171] The reaction temperature of the first step may be 50°C to 80°C. If the catalyst is prepared at 50°C or lower, for example, at room temperature, the catalyst activity is low, which is undesirable. If the catalyst is prepared at 80°C or higher, the catalyst discolors to yellow, which is undesirable.

[0172] The vacuum drying temperature of the third step may be 20°C to 100°C. Even if drying is performed at 20°C or lower, that is, at room temperature, a highly active catalyst is obtained, and there is no benefit obtained by vacuum drying at room temperature or lower. If it is performed at 120°C or higher, the solvent is excessively removed, which is not preferable.

[0173]

[0174] In addition, the third aspect of the present invention provides a method for producing a polyether polyol, comprising the steps of producing a double metal cyanide (DMC) catalyst by the method according to the second aspect of the present invention, and polymerizing propylene oxide in the presence of a polyol starter using the DMC catalyst.

[0175] Regarding the method for producing polyether polyol according to the third aspect of the present application, detailed descriptions of parts overlapping with the first aspect and / or the second aspect of the present application are omitted, but even if the descriptions are omitted, the contents described in the first aspect and / or the second aspect of the present application can be equally applied to the third aspect of the present application.

[0176] According to one embodiment of the present invention, the polyol starter may be, but is not limited to, polypropylene glycol having a molecular weight of 300 to 800.

[0177]

[0178] Also, the fourth aspect of the original is (NC)6Co 3- , (AcO)Zn + , and Zn 2+ Contains components, and additionally ClZn + and / or (RO)Zn + (R is C1-C 20 Alkyl ether or C1-C 20 A double metal cyanide (DMC) catalyst containing an alkyl component is provided.

[0179] Previous studies have reported that DMC catalysts containing Zn-OH groups efficiently produce polyols with low unsaturation levels. However, they have the disadvantage of producing very high molecular weight chain impurities, which poses a serious problem in certain applications. To address this issue, the inventors of the present invention prepared a DMC catalyst containing acetate groups by treating a DMC catalyst known to contain Zn-OH groups with acetic acid. Analysis of the IR spectrum indicated that the Zn-OH groups were effectively converted to Zn-OAc.

[0180] Similarly, pure acetic acid [(tBuO)Zn + ][Zn 2+ ][(NC)6Co 3- ] (hereinafter, DMC-OtBu) is treated to obtain the desired composition [(AcO)Zn +][(H2O)Zn 2+ ][(NC)6Co 3- ] (hereinafter, DMC-OAc) was formed. 1 It was confirmed by H NMR and ATR-FTIR spectra (Scheme 6a, Fig. 8a, Fig. 9a). However, the above [(AcO)Zn + ][(H2O)Zn 2+ ][(NC)6Co 3- ] did not show any activity.

[0181] According to one embodiment of the present invention, the (AcO)Zn + The components were observed at 1618, 1583, 1554, 1463, 1443, and 1355 cm in the ATR-FTIR spectrum. -1 It may be measured in, but is not limited to,

[0182] AcOZn + For the purpose of manufacturing a DMC catalyst containing a unit [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOC3H6OH] (hereinafter, [DMC-Cl][MeOC3H6OH]) was treated with 1.0 eq AcOLi in 88:12 tBuOH / H2O. However, this attempt yielded DMC-OtBu. The desired complex, DMC-OAc, was successfully obtained when [DMC-Cl][MeOC3H6OH] was reacted in the presence of 1.0 eq AcOLi and 1.0 eq AcOH (i.e., in a weakly acidic medium). (Scheme 6b). The filtrate contained Cl - 1.1eq and Li + 1.0 eq was detected, and Zn and Co ions were also detected in trace amounts (1.0 and 0.54 mol% per feed). The separated solid was dissolved in a 1:1 mixture of 4 M NaOD / D2O and CD3OD, and 1,6-hexanediol was used as an internal standard. 1When the H NMR spectrum was measured, 0.97 eq AcO signal and 0.02 eq tBuO signal were observed.

[0183] ATR-FTIR spectral analysis results at 1583 and 1463 cm -1 The presence of -C(O)O stretching signals was observed at 1554 and 1443 cm -1 An additional set of small signals was observed (Fig. 8c). The SEM image showed small broken plate-like particles, and the XRD pattern was consistent with DMC-OR and the starting material [ClZn + ][Zn 2+ ][(NC)6Co 3- ] (hereinafter, DMC-Cl) showed a distinct deviation from the pattern (Fig. 9b). Both the SEM image and XRD pattern showed similarity to those observed for Zn2[Co(CN)6](CH3COO)·4H2O synthesized by the reported method by direct reaction of K3Co(CN)6 and 2.0 eq Zn(OAc)2 (Fig. 9c).

[0184] [Reaction Formula 6]

[0185]

[0186] According to one embodiment of the present invention, R may be, but is not limited to, tert-butyl.

[0187] According to one embodiment of the present invention, (tert-BuO)Zn + The component is detected at 640 cm in the ATR-FTIR spectrum. -1 It may be measured in the vicinity, but is not limited thereto.

[0188] According to one embodiment of the present invention, the double metal cyanide (DMC) catalyst is (NC)6Co 3- , (AcO)Zn + , Zn 2+ and (tert-BuO)Zn + Ingredients may include, but are not limited to:

[0189] According to one embodiment of the present invention, the (NC)6Co 3- , (AcO)Zn + , Zn 2+ and (tert-BuO)Zn + A double metal cyanide (DMC) catalyst comprising a component may have a composition represented by the following chemical formula 2, but is not limited thereto:

[0190] [Chemical Formula 2]

[0191] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [Zn 2+ ] a [(NC)6Co 3- ]

[0192] (In the above chemical formula 2,

[0193] p is 0.1 to 1.2;

[0194] q is 0.01 to 0.9;

[0195] p + q is 0.9 to 1.2;

[0196] (p + q + 2a is 3).

[0197] According to one embodiment of the present invention, p may be from 0.3 to 0.98; and q may be from 0.01 to 0.75, but is not limited thereto.

[0198] According to one embodiment of the present invention, p may be 0.90 to 0.98; and q may be 0.01 to 0.10, but is not limited thereto.

[0199] By systematically reducing the amount of AcOH from 1.0 eq to 0.8, 0.7, 0.6, and 0.5 eq while maintaining the fixed amount of AcOLi at 1.0 eq, various (AcO)Zn + / (tBuO)Zn + DMC catalyst having a ratio [i.e., [(AcO)Zn + ]p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ]; referred to as DMC-(OAc / OtBu)(p / q) (p / q = 0.95 / 0.08, 0.68 / 0.31, 0.42 / 0.57 and 0.31 / 0.71)] were obtained. Here, "p" and "q" are 1 The OAc and OtBu contents of the isolated solids, respectively, are shown in the H NMR spectrum. The combined amount of OAc and OtBu is [(NC)6Co 3- ] is about 1.0 eq. It is worth noting that throughout the experiment, all the Cl initially present in the DMC-Cl reactant - (0.98-0.99 eq) and introduced lithium ions (1.00-1.07 eq) were effectively removed and found in the filtrate (Table 2). Trace amounts of zinc (0.3-0.5 mol% relative to the feed) were detected in the filtrate, along with detectable amounts of cobalt. Consequently, only negligible amounts of Cl anions were detected in the SEM-EDS analysis.

[0200] (tBuO)Zn + Addition of a small amount (0.08 eq) of (OAc / OtBu) significantly changes the particle shape. That is, the SEM image of DMC-(OAc / OtBu)(0.95 / 0.08), which shows regular, thin, and narrow slabs, is different from the SEM images of DMC-(OAc / OtBu)(0.97 / 0.02), DMC-OR, and DMC-Cl (Fig. 2 and Figs. 10a-10b). (tBuO)Zn + When the fraction was increased to 0.31 eq and further increased to 0.57 and 0.58 eq, the XRD signal corresponding to DMC-OtBu appeared and gradually intensified. At the same time, the signal corresponding to DMC-(OAc / OtBu)(0.97 / 0.02) showed a gradual decrease. In addition, the particle shape was (tBuO)Zn +As the fraction increased, it gradually transformed from a thin and narrow slab to a wider plate (Figs. 10c-10e). In the ATR-FTIR spectrum of DMC-(OAc / OtBu)(0.95 / 0.08), a small amount of (tBuO)Zn + A notable change was observed when including the unit (i.e., 0.08 eq). 1554 and 1443 cm , which are marked as minor sets in DMC-(OAc / OtBu)(0.97 / 0.02). -1 The signal was found to be significantly increased in intensity to become the main set in DMC-(OAc / OtBu)(0.95 / 0.08) (Figs. 8c-8d).

[0201] According to one embodiment of the present invention, the double metal cyanide (DMC) catalyst is (NC)6Co 3- , (AcO)Zn + , Zn 2+ , (tert-BuO)Zn + and ClZn + Ingredients may include, but are not limited to:

[0202] According to one embodiment of the present invention, the (NC)6Co 3- , (AcO)Zn + , Zn 2+ , (tert-BuO)Zn + and ClZn + A double metal cyanide (DMC) catalyst comprising a component may have a composition represented by the following chemical formula 3, but is not limited thereto:

[0203] [Chemical Formula 3]

[0204] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [ClZn + ] r [Zn 2+ ] a [(NC)6Co 3- ]

[0205] (In the above chemical formula 3,

[0206] p is 0.3 to 0.8;

[0207] q is 0.2 to 0.5;

[0208] r is 0.05 to 0.5;

[0209] p + q + r is 0.9 to 1.2;

[0210] (p + q + r + 2a is 3).

[0211] According to one embodiment of the present invention, p may be 0.4 to 0.8; q may be 0.2 to 0.5; and r may be 0.1 to 0.3, but is not limited thereto.

[0212] DMC catalysts containing three components, Zn-OAc, Zn-OtBu, and Zn-Cl, were further synthesized by reacting [DMC-Cl][MeOC3H6OH] with substoichiometric amounts of equimolar mixtures of AcOLi and AcOH (0.90, 0.80, 0.70, 0.60, and 0.50 eq). As observed in the preparation of DMC-(OtBu / Cl)(0.5 / 0.5), the excess Cl ions exceeding the AcOLi feed were washed away with the filtrate (1.07, 1.18, 1.29, 1.30, and 1.26 eq per feed AcOLi, respectively) (Table 2).

[0213] All Li introduced + was detected in the filtrate for 0.90, 0.80 and 0.70 eq AcOLi inputs (1.0 eq per AcOLi feed), while slightly lower amounts of Li were detected for 0.60 and 0.50 eq AcOLi inputs (0.83 and 0.93 eq, respectively). +was detected. Therefore, some Zn ions in the form of ZnCl2 were detected in the filtrate (1.7, 4.4, 5.3, 4.9 and 8.5 mol% per supplied ZnCl2, respectively). Cobalt was not detected in the filtrate in any case. The Cl / Co ratio determined by SEM-EDS analysis of the separated solid was - The values ​​were roughly in line with the expected values ​​(0.06, 0.10, 0.15, 0.28, 0.39 compared to the expected 0.04, 0.06, 0.10, 0.22, 0.37, respectively).

[0214] The chemical formula of the isolated solid is logically [(AcO)Zn + ] p [(tBuO)Zn + ] q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ][tBuOH] r (hereinafter referred to as DMC-(OAc / OtBu / Cl)(p / q / r)), where "r" corresponds to the Cl / Co ratio determined through SEM-EDS analysis, while "p" and "q + r" are 1 The OAc and OtBu contents of the isolated solids are shown in the H NMR spectrum, respectively. The "r" value gradually increased from 0.06 to 0.39 with decreasing AcOLi input, while the combined "p + q + r" value was (NC)6Co 3- It remained almost constant at 1.1 eq per unit.

[0215] Due to the presence of these three components, the XRD pattern became broader and more complex, and the SEM image showed wide and thin plates with irregular shapes (Fig. 11). In the ATR-FTIR spectrum (Fig. 12), three sets of -C(O)O stretching signals were observed, with peaks at 1554 and 1443 cm across all instances. -1 A prominent set appeared in . The Zn-OtBu stretching signal was at 642 cm for all cases.-1 It was also clearly shown in .

[0216]

[0217] Also, the fifth aspect of the present invention is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound consisting of the components, lithium acetate (AcOLi) and acetic acid in a tert-butanol (tert-BuOH) solvent containing less than 30 wt% of water, is prepared by reacting the ClZn + Provided is a method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 2, which comprises the steps of adding 1 equivalent and 1 to 0.4 equivalents of each component, reacting them, filtering to obtain a solid compound, and removing the remaining solvent by vacuum depressurization:

[0218] [Chemical Formula 2]

[0219] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [Zn 2+ ] a [(NC)6Co 3- ]

[0220] (In the above chemical formula 2,

[0221] p is 0.1 to 1.2;

[0222] q is 0.01 to 0.9;

[0223] p + q is 0.9 to 1.2;

[0224] (p + q + 2a is 3).

[0225] Regarding the method for manufacturing a DMC catalyst according to the fifth aspect of the present application, detailed descriptions of parts overlapping with the fourth aspect of the present application have been omitted. However, even if the descriptions have been omitted, the contents described in the fourth aspect of the present application can be equally applied to the fifth aspect of the present application.

[0226] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOCH2CH(Me)OH], but is not limited thereto.

[0227] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of components may be prepared by reacting H3Co(CN)6 and ZnCl2 in a molar ratio of 1:2, but is not limited thereto.

[0228]

[0229] Also, the sixth aspect of the present invention is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound consisting of ClZn, lithium acetate (AcOLi) and acetic acid in a tert-butanol (tert-BuOH) solvent containing less than 30 wt% of water + A method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 3 is provided, which comprises the steps of adding 0.95 to 0.5 equivalents and 0.95 to 0.5 equivalents of each component, reacting them, filtering them to obtain a solid compound, and removing the remaining solvent by vacuum depressurization:

[0230] [Chemical Formula 3]

[0231] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [ClZn + ] r [Zn 2+ ] a[(NC)6Co 3- ]

[0232] (In the above chemical formula 3,

[0233] p is 0.3 to 0.8;

[0234] q is 0.2 to 0.5;

[0235] r is 0.05 to 0.5;

[0236] p + q + r is 0.9 to 1.2;

[0237] (p + q + r + 2a is 3).

[0238] Regarding the method for manufacturing a DMC catalyst according to the sixth aspect of the present application, detailed descriptions of parts overlapping with the fourth aspect of the present application have been omitted. However, even if the descriptions have been omitted, the contents described in the fourth aspect of the present application can be equally applied to the sixth aspect of the present application.

[0239] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOCH2CH(Me)OH], but is not limited thereto.

[0240] According to one embodiment of the present invention, the starting material is (NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of components may be prepared by reacting H3Co(CN)6 and ZnCl2 in a molar ratio of 1:2, but is not limited thereto.

[0241]

[0242] In addition, the seventh aspect of the present invention provides a method for producing a polyether polyol, comprising the steps of: preparing a double metal cyanide (DMC) catalyst according to any one of the fifth to sixth aspects of the present invention; and polymerizing propylene oxide in the presence of a polyol starter using the DMC catalyst.

[0243] Regarding the method for producing a polyether polyol according to the seventh aspect of the present application, detailed descriptions of parts overlapping with the fourth to sixth aspects of the present application have been omitted. However, even if the descriptions have been omitted, the contents described in the fourth to sixth aspects of the present application can be equally applied to the seventh aspect of the present application.

[0244] According to one embodiment of the present invention, the polyol starter may be, but is not limited to, polypropylene glycol having a molecular weight of 300 to 800.

[0245]

[0246] In addition, the eighth aspect of the present invention provides a method for producing a poly(ether-co-carbonate) polyol, comprising the steps of: preparing a double metal cyanide (DMC) catalyst according to any one of the fifth and sixth aspects of the present invention; and copolymerizing propylene oxide and CO2 in the presence of a polyol starter using the DMC catalyst.

[0247] Regarding the method for producing a poly(ether-co-carbonate) polyol according to the 8th aspect of the present application, detailed descriptions of parts overlapping with the 4th to 6th aspects of the present application are omitted, but even if the descriptions are omitted, the contents described in the 4th to 6th aspects of the present application can be equally applied to the 5th aspect of the present application.

[0248] According to one embodiment of the present invention, the polyol starter may be, but is not limited to, polypropylene glycol having a molecular weight of 300 to 800.

[0249] Hereinafter, the structure and operation of the present invention will be described in more detail through preferred embodiments of the present invention. However, these are presented as preferred examples of the present invention and should not be construed as limiting the present invention in any way.

[0250]

[0251] [ingredient]

[0252] Zinc chloride (anhydrous, ≥98%), zinc oxide (puriss. pa, ACS reagent, ≥99.0%), potassium hexacyanocobalt(III) (≥97%), nitric acid (puriss. pa, ≥65%), lithium hydroxide monohydrate (ACS reagent, ≥98.0%), lithium acetate dihydrate (BioUltra, ≥99.0% (calculated on dry matter, NT)), phenol (destabilized, ReagentPlus) ® , ≥99%), potassium tert-butoxide (reagent grade, ≥98%), sodium oxide (80%), 1,6-hexanediol (99%), 2-methoxyethanol (99+%), 1-methoxy-2-propanol (≥99.5%), PPG (average Mn ~4,000), PPG (average Mn ~425), PTMEG (average Mn ~2,900, containing 300-500 ppm of BHT as a stabilizer), phenolphthalein solution (0.5 wt%, ethanol:water (1:1))), florisil ® (<200 mesh, fine powder) was purchased from Sigma-Aldrich (St. Louis, MO, USA); PEG 4,000, poly(acrylic acid) (50 wt% solution in water, approximately MW 3,000–5,000) was purchased from Alfa Aesar (Ward Hill, MA, USA); propylene oxide (PO) (>99.0%), tert-butyl alcohol (>99.0%) were purchased from TCI (Tokyo, Japan); sulfuric acid (95.0%), acetic acid (99.5%), sodium hydroxide (beads, >98.0%) were purchased from SAMCHUN (Seoul, Korea); deuterium oxide (99.90%) was purchased from Eurisotope ®was purchased from; CO2 gas (purity 99.999%) was dried by storing in a column of 3Å molecular sieve and alumina at a pressure of 50 bar; PO was dried by stirring over CaH2 and then vacuum-transferred to storage.

[0253] [Specification method]

[0254] 1 H NMR (600 MHz) analysis was performed on a JEOL ECZ 600 instrument; ICP-OES analysis was performed on an iCAP PRO XP DUO (Thermo Fisher science, Waltham, MA, USA); morphological analysis was performed using a SEM (JSM-7900F) at an accelerating voltage of 3 kV (15 kV for EDS); the specimens were coated with platinum using a sputter coater; TEM was examined using a JEM-2100F; XRD patterns were obtained on a Rigaku D / max-2500V / PC using Cu-Kα radiation at 40 kV and 150 mA; FTIR spectra were recorded in the range of 4000–400 cm -1 The TGA data were obtained in ATR mode using a Nicolet iS50 FT-IR spectrometer (Thermo Fisher science, Wal-tham, MA, USA) in the wavenumber range; TGA data were obtained using a NETZSCH STA449F3 Jupiter ® The data were obtained at a heating rate of 10°C / min, N2 flow rate of 20 mL / min in the temperature range of 30-1000°C using; GPC data were obtained in THF at 40°C using Shodex GPC HK-400 series using polystyrene standards.

[0255]

[0256] [Manufacturing Example 1] Preparation of H3Co(CN)6·3.6(MeOCH2CH2OH)

[0257] K3Co(CN)6 (100 g, 300 mmol) was dissolved in distilled water (200 mL) at 50°C. Sulfuric acid (95%, 38 mL, 675 mmol) was then added dropwise over 30 minutes. The mixture was stirred for 3 hours, after which cooled ethanol (500 mL) was added. The resulting mixture was stirred for an additional 30 minutes. The white precipitate was separated by filtration. The solvent in the filtrate was removed using a rotary evaporator to obtain a pale yellow residue, which was then dried under vacuum at 20-25°C for 6 hours to reach a mass of 75.5 g.

[0258] Then, cooled absolute ethanol (250 mL) was added, and the resulting slurry was stirred overnight. The solid was separated by filtration and washed with absolute ethanol (75 mL). The solvent remaining in the separated solid was completely removed using a vacuum line to obtain a pale yellow solid (67.8 g, 68% based on the formula H3[Co(CN)6]·2.4[CH3CH2OH]). For composition analysis of the separated solid, the separated solid (10.0 mg) was dissolved in D2O together with 1,6-hexanediol (13.2 mg) as an internal standard. 1 A H NMR spectrum was recorded. Distinct signals corresponding to ethanol and 1,6-hexanediol were observed separately in the spectrum. The integral of these signals indicated that the chemical formula of the isolated solid was H3[Co(CN)6]·2.4[CH3CH2OH].

[0259] The obtained H3[Co(CN)6]·2.4[CH3CH2OH] (67.8 g, 204 mmol) was dissolved in 2-methoxyethanol (712 g) at 70°C. When the solution was slowly cooled to room temperature and stored for 36 h, transparent quartz-like crystals were deposited. These crystals were separated by decantation, and a small portion was selected for subsequent X-ray crystallographic analysis. Evacuation to remove residual 2-methoxyethanol yielded an opaque solid (60 g). The temperature was recorded in D2O using 1,6-hexanediol as an internal standard. 1Analysis of the H NMR spectrum revealed that the chemical formula of the isolated solid was determined to be H3Co(CN)6·3.6(MeOCH2CH2OH). ICP-OES analysis revealed that the isolated solid contained negligible amounts of K and S (K, 4 ppm; S, 3 ppm).

[0260]

[0261] [Comparative Example 1] Benchmark DMC

[0262] Under the limitations of the analysis, we used a state-of-the-art benchmark DMC catalyst currently used in the industry with only information on the Zn / Co ratio (ca., 2.0) and cobalt content (ca., 10 wt%).

[0263] [Comparative Example 2] [DMC-Cl][MeOC3H6OH]

[0264] ZnCl2 (1.36 g, 10.0 mmol) dissolved in a 10:1 (wt / wt) mixture of MeOC3H6OH / H2O (20 mL) was added H3Co(CN)6·3.6(MeOCH2CH2OH) (2.46 g, 5.00 mmol) prepared in Preparation Example 1 to the same solvent (10 mL) at 70°C. After stirring at 70°C for 15 h, the mixture was filtered, and the collected filter cake was thoroughly washed with 10:1 MeOC3H6OH / H2O (50 mL). The filtrate (78 g) including the washing process was retained for further analysis. The filter cake was transferred to a single-necked flask and dried under vacuum at 20–25°C for 4.5 h, followed by an additional drying step at 80°C for 15 h. Through this process, a white solid (2.22 g, 95%) was isolated. Based on the analysis of the filtrate and the isolated solid (detailed below), the chemical formula of the isolated solid was [ClZn + ][Zn 2+ ][(NC)6Co 3- ] was identified as [MeOC3H6OH].

[0265] Determination of chloride ion content in the filtrate: HNO3 (1 mL, 10 wt% solution) was added to 1 / 10 of the filtrate (7.8 g). Subsequently, excess AgNO3 (0.680 g, 4 eq per ZnCl2 feed) was introduced. This immediately resulted in the formation of a white precipitate (AgCl), which was separated by filtration using a 47 mm filter paper. The weight of the filter paper was measured after drying at 60 °C. After drying at 60 °C for 1 h, the mass of the entire filter paper including AgCl was measured (mass of AgCl, 0.210 g, 2.93 eq Cl per H3Co(CN)6 feed). - ).

[0266] H in the balance + Content measurement: 1 / 5 (15.6 g) of the filtrate was added to phenolphthalein (2.9 mmol-H) as an indicator. + , was titrated using a 0.10 N NaOH standard solution having 2.9 eq per H3Co(CN)6 feed.

[0267] Measurement of Zinc and Cobalt Ion Contents in the Filtrate: One-fifth (15.6 g) of the filtrate was vacuum-dried, and the resulting residue was dissolved in HNO3 (10 wt% solution) to achieve a total mass of 10.0 g. ICP-OES analysis of the resulting solution revealed 252 ppm Zn (1.9 mol% per ZnCl2 feed) and 32 ppm Co (0.55 mol% per H3Co(CN)6 feed).

[0268] Determination of 1-methoxy-2-propanol content in the separated solid: 1.24 g of sodium oxide (20.0 mmol) was slowly added to 10 mL of D2O at room temperature to prepare a 4 M NaOD / D2O solution. The separated DMC (6.83 mg) and the internal standard 1,6-hexanediol (5.76 mg) were dissolved in the prepared mixture of 4 M NaOD / D2O (1 mL) and CD3OD (1 mL). 1H NMR spectra were recorded. Signals corresponding to MeOC3H6OH and the internal standard 1,6-hexanediol were clearly observed. Analysis of the integrated values ​​quantified the MeOC3H6OH content of the isolated solid (formula [ClZn + ][Zn 2+ ][(NC)6Co 3- ][menstruum] c 0.96 eq based on "c" = 0.96 in ).

[0269] Determination of Cl / Co and Zn / Co ratios of the separated solid: While examining the SEM images, EDS analysis showed that the Cl / Co ratio was 1.06 and the Zn / Co ratio was 2.76.

[0270] [Comparative Example 3] [DMC-Cl][tBuOH]

[0271] [DMC-Cl][MeOC3H6OH] (0.100 g, 0.213 mmol) prepared according to Comparative Example 2 was stirred overnight at 70°C in 88:12 tBuOH / H2O (4.62 g). The resulting suspension was filtered, and the filter cake was washed with 88:12 tBuOH / H2O (6.5 g). The filter cake was then discharged at 20-25°C for 4 hours to produce a white solid (97.0 mg, 100%). The isolated solid 1 The chemical formula [ClZn] in the H NMR spectrum + ][Zn 2+ ][(NC)6Co 3- ] was detected, but no signal corresponding to MeOC3H6OH.

[0272] [Comparative Example 4] DMC-OtBu

[0273] LiOH·H2O (0.420 g, 10.0 mmol) and phenol (0.941 g, 10.0 mmol) were combined with H2O (8.64 g) to produce a transparent PhOLi solution (concentration, 1.0 mmol / g). The PhOLi solution (0.226 g, 0.226 mmol) thus prepared was introduced into 10:1 MeOC3H6OH / H2O (4.62 g) and heated to 70°C. Subsequently, [DMC-Cl][MeOC3H6OH] (0.500 g, 1.06 mmol) dissolved in 88:12 tBuOH / H2O (23.1 g) was added to the solution. After stirring at 70°C for 15 hours, the resulting suspension was filtered through a filter paper and washed with 10:1 MeOC3H6OH / H2O (6.5 g). The filter cake was then vacuum dried at 20–25°C for 2 hours. (Yield, 0.452 g (96%)). Chemical formula [(tBuO)Zn + ][Zn 2+ ][(NC)6Co 3- ] Analysis data for verification are disclosed in Table 1.

[0274] [Comparative Example 5] DMC-OAc

[0275] DMC-OtBu (19.7 mg) prepared according to Comparative Example 4 was stirred overnight at 70°C in pure acetic acid, and then vacuum dried at 20-25°C for 2 hours to obtain a white solid (19.7 mg). [(AcO)Zn + ][(H2O)Zn 2+ ][(NC)6Co 3- ] (hereinafter, DMC-OAc) structure 1 It was confirmed by H NMR and ATR-FTIR spectra.

[0276] [Comparative Example 6] Zn2[Co(CN)6](CH3COO)·4H2O

[0277] A DMC catalyst with the chemical formula Zn2[Co(CN)6](CH3COO)·4H2O, known from the paper (Marquez, C.; Simonov, A.; Wharmby, MT; Van Goethem, C.; Vankelecom, I.; Bueken, B.; Krajnc, A.; Mali, G.; De Vos, D.; De Baerdemaeker, T., Layered Zn2[Co(CN)6](CH3COO) double metal cyanide: a two-dimensional DMC phase with excellent catalytic performance. Chemical Science 2019, 10 (18), 4868-4875.), was used.

[0278]

[0279] [Example 1] DMC catalyst (DMC-OC3H6OMe) using 1.0 equivalent of LiOPh

[0280] LiOH·H2O (0.420 g, 10.0 mmol) and phenol (0.941 g, 10.0 mmol) were combined with H2O (8.64 g) to produce a transparent PhOLi solution (concentration, 1.0 mmol / g). The PhOLi solution (0.226 g, 0.226 mmol) thus prepared was introduced into 10:1 MeOC3H6OH / H2O (4.62 g) and heated to 70°C. Subsequently, [DMC-Cl][MeOC3H6OH] (0.106 g, 0.226 mmol) in solid form was added to the solution. After stirring at 70°C for 15 h, the resulting suspension was filtered through a filter paper and washed with 10:1 MeOC3H6OH / H2O (6.5 g). Then, the filter cake was vacuum dried at 20-25℃ for 2 hours to obtain 88.7 mg (chemical formula [(MeOC3H6O)Zn + ][Zn 2+ ][(NC)6Co 3- ] yield of 90%) was obtained. The analytical data for confirming the chemical formula are disclosed in Table 1.

[0281] [Example 2] DMC catalyst using 0.75 equivalents of LiOPh [DMC-(OC3H6OMe / Cl)(0.75 / 0.25)]

[0282] It was prepared in the same manner as Example 1, but using 0.170 mmol of PhOLi. Chemical formula [(MeOC3H6O)Zn + ] 0.75 [ClZn + ] 0.25 [Zn 2+ ][(NC)6Co 3- ] Analysis data for verification are disclosed in Table 1.

[0283] [Example 3] DMC catalyst using 0.50 equivalents of LiOPh [DMC-(OC3H6OMe / Cl)(0.5 / 0.5)]

[0284] It was prepared in the same manner as Example 1, but using 0.113 mmol of PhOLi. Chemical formula [(MeOC3H6O)Zn + ] 0.50 [ClZn + ] 0.50 [Zn 2+ ][(NC)6Co 3- ] Analysis data for verification are disclosed in Table 1.

[0285] [Example 4] DMC catalyst using 0.25 equivalents of LiOPh [DMC-(OC3H6OMe / Cl)(0.25 / 0.75)]

[0286] It was manufactured in the same manner as Example 1, but using 0.057 mmol of PhOLi. Chemical formula [(MeOC3H6O)Zn + ] 0.25 [ClZn + ] 0.75 [Zn 2+ ][(NC)6Co 3- ] Analysis data for verification are disclosed in Table 1.

[0287] [Example 5] DMC-(OtBu / Cl)(0.5 / 0.5)

[0288] It was prepared in the same manner as in Example 1, but using [DMC-Cl][MeOC3H6OH] (0.106 g, 0.226 mmol) dissolved in 88:12 tBuOH / H2O (4.62 g) and a reduced amount of PhOLi (0.113 mmol) (yield, 94.8 mg). Chemical formula [(tBuO)Zn + ] p [ClZn + ] (1-p) [Zn 2+ ][(NC)6Co 3- ] Analysis data for verification are disclosed in Table 1.

[0289] [Table 1] Analysis data collected during the production of DMC catalysts according to Examples 1 to 5 and Comparative Example 4.

[0290]

[0291] [Example 6-1] DMC-(OAc / OtBu)(0.97 / 0.02)

[0292] AcOLi·2H2O (21.8 mg, 0.213 mmol) and acetic acid (12.8 mg, 0.213 mmol) were dissolved in 88:12 tBuOH / H2O (4.62 g). After stirring at 70°C for 5 minutes, [DMC-Cl][MeOC3H6OH] (0.100 g, 0.213 mmol) was added to the solution and stirred for an additional 15 hours. The resulting suspension was then filtered, and the filter cake was washed with 88:12 tBuOH / H2O (6.5 g). After drying in vacuum at 20–25°C for 2 hours, a white solid (86.7 mg) was obtained. Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ] (p / q = 0.97 / 0.02) are disclosed in Table 2.

[0293] [Example 6-2] DMC-(OAc / OtBu)(0.95 / 0.08)

[0294] It was prepared in the same manner as in Example 6-1, but using a reduced amount of AcOH (10.3 mg (0.80 eq)) while keeping the amount of AcOLi constant (21.8 mg, 0.213 mmol, 1.0 eq per reactant [DMC-Cl][MeOC3H6OH]) (yield 87.5 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ] (p / q = 0.95 / 0.08) are disclosed in Table 2.

[0295] [Example 6-3] DMC-(OAc / OtBu)(0.68 / 0.31)

[0296] It was prepared in the same manner as in Example 6-1, but using a reduced amount of AcOH (9.0 mg (0.70 eq)) while keeping the amount of AcOLi constant (21.8 mg, 0.213 mmol, 1.0 eq per reactant [DMC-Cl][MeOC3H6OH]) (yield 87.0 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ] (p / q = 0.68 / 0.31) are disclosed in Table 2.

[0297] [Example 6-4] DMC-(OAc / OtBu)(0.42 / 0.57)

[0298] It was prepared in the same manner as in Example 6-1, but using a reduced amount of AcOH (7.7 mg (0.60 eq)) while keeping the amount of AcOLi constant (21.8 mg, 0.213 mmol, 1.0 eq per reactant [DMC-Cl][MeOC3H6OH]) (yield 93.1 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ] (p / q = 0.42 / 0.57) are disclosed in Table 2.

[0299] [Example 6-5] DMC-(OAc / OtBu)(0.31 / 0.71)

[0300] It was prepared in the same manner as in Example 6-1, but using a reduced amount of AcOH (6.4 mg (0.50 eq)) while keeping the amount of AcOLi constant (21.8 mg, 0.213 mmol, 1.0 eq per reactant [DMC-Cl][MeOC3H6OH]) (yield 90.0 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ] (p / q = 0.31 / 0.71) are disclosed in Table 2.

[0301] [Example 7-1] DMC-(OAc / OtBu / Cl)(0.68 / 0.38 / 0.06)

[0302] It was manufactured in the same manner as Example 6-1, but the amount of AcOLi / AcOH was reduced to 19.6 mg / 11.5 mg (0.90 eq) per reactant [DMC-Cl][MeOC3H6OH] (yield 88.3 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ]q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ] (p / q / r = 0.68 / 0.38 / 0.06) are shown in Table 2.

[0303] [Example 7-2] DMC-(OAc / OtBu / Cl)(0.74 / 0.24 / 0.10)

[0304] It was manufactured in the same manner as Example 6-1, but the amount of AcOLi / AcOH was reduced to 17.4 mg / 10.3 mg (0.80 eq) per reactant [DMC-Cl][MeOC3H6OH] (yield 100 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ] (p / q / r = 0.74 / 0.24 / 0.10) are shown in Table 2.

[0305] [Example 7-3] DMC-(OAc / OtBu / Cl)(0.59 / 0.38 / 0.15)

[0306] It was manufactured in the same manner as Example 6-1, but the amount of AcOLi / AcOH was reduced to 15.2 mg / 9.1 mg (0.70 eq) per reactant [DMC-Cl][MeOC3H6OH] (yield 89.7 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ] (p / q / r = 0.59 / 0.38 / 0.15) are shown in Table 2.

[0307] [Example 7-4] DMC-(OAc / OtBu / Cl)(0.41 / 0.43 / 0.28)

[0308] It was manufactured in the same manner as Example 6-1, but the amount of AcOLi / AcOH was reduced to 13.1 mg / 7.7 mg (0.60 eq) per reactant [DMC-Cl][MeOC3H6OH] (yield 87.7 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ] (p / q / r = 0.41 / 0.43 / 0.28) are shown in Table 2.

[0309] [Example 7-5] DMC-(OAc / OtBu / Cl)(0.34 / 0.39 / 0.39)

[0310] It was manufactured in the same manner as Example 6-1, but the amount of AcOLi / AcOH was reduced to 10.9 mg / 6.4 mg (0.50 eq) per reactant [DMC-Cl][MeOC3H6OH] (yield 90.6 mg). Chemical formula [(AcO)Zn + ] p [(tBuO)Zn + ] q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ] (p / q / r = 0.34 / 0.39 / 0.39) are shown in Table 2.

[0311] [Table 2] Analysis data collected during the preparation of DMC catalysts according to Examples 6-1 to 6-5 and Examples 7-1 to 7-5.

[0312]

[0313]

[0314] [Experimental Example 1] PO polymerization

[0315] PO polymerization was performed using the DMC catalyst according to the examples and comparative examples, and the results are shown in Table 3 below.

[0316] [Table 3] PO polymerization results of DMC catalyst according to examples and comparative examples a

[0317]

[0318] a Polymerization conditions: DMC (4.0 μmol-Co), PPG starter (M n = 425 Da, 4.25 g), heat to 125°C, feed 5 mL PO for 4 minutes to initiate, wait until PO is almost completely consumed (initiation time), then feed PO continuously (1.25 mL / min) at 130-145°C with spontaneous temperature control. b Mass of polyol produced excluding the supplied starter. c 1 Calculated based on H NMR spectrum (600 MHz). d Measured on GPC eluted with THF and processed using PS standards.

[0319] Most of the prepared catalysts showed high yields (23-34 g) comparable to that of the benchmark DMC (28 g) (Table 3). Among them, DMC-(OAc / OtBu) (0.95 / 0.08) showed the highest yield (32 g), surpassing the benchmark DMC (28 g). The catalysts with the next highest yields were DMC-(OAc / OtBu / Cl) (29-31 g) and DMC-Cl (28 g), and the DMC with a higher proportion of alkoxy groups showed lower yields (23-27 g) along with shorter catalyst lives (23-27 min). In general, the very short initiation times occurred within a few minutes in most cases, except for [DMC-Cl][MeOC3H6OH], DMC-OtBu, and DMC-(OAc / OtBu) (0.31 / 0.71), which required external heating for initiation. DMC-(OAc / OtBu) and DMC-(OAc / OtBu / Cl) with low OtBu contents (< 0.5 eq) emerged as efficient catalysts, showing high yields (30-32 g; 18 kg / g-DMC) and almost negligible induction times of less than 1 min (Examples 6-2, 6-3, and 7-1 to 7-4). The turnover number (TON) and turnover frequency (TOF) demonstrated by these catalysts were remarkably high, reaching 137,000 and 243,000 units per Co per hour, respectively.

[0320] Polyols produced with DMC-Cl exhibited high unsaturation levels (0.022-0.024 meq / g), whereas polyols produced with DMC-OC3H6OMe and DMC-OtBu exhibited very low unsaturation levels, consistent with the benchmark DMC (0.004 meq / g). DMC-(OAc / OtBu) (0.97 / 0.02) exhibited moderate unsaturation levels (0.016 meq / g). Following this trend, in the DMC-(OC3H6OMe / Cl)(p / (1-p)) series, the degree of unsaturation gradually decreased as the Zn-OR portion (i.e., p value) increased, from 0.024 meq / g for [DMC-Cl][MeOC3H6OH] to 0.018, 0.008, and 0.006 meq / g for p = 0.25, 0.50, and 0.75, respectively, and 0.005 meq / g for DMC-(OtBu / Cl) (0.5 / 0.5). Likewise, in the DMC-(OAc / OtBu)(p / q) series, the degree of unsaturation gradually decreased as the Zn-OtBu content increased, from 0.016 meq / g for DMC-(OAc / OtBu)(0.97 / 0.02) to 0.013, 0.010, 0.007, and 0.005 meq / g for p / q = 0.95 / 0.08, 0.68 / 0.31, 0.42 / 0.57, and 0.31 / 0.71, respectively. Importantly, the unsaturation levels of the DMC-(OAc / OtBu / Cl)(p / q / r) series (Examples 7-2 to 7-5) were within the low range of 0.005-0.008 meq / g.

[0321] The formation of high molecular weight impurities (2–3 wt%) is a critical issue in DMC-catalyzed polyol production. In the GPC curve of the polyol synthesized using benchmark DMC, a distinct high molecular weight segment was identified along with a narrow base peak (Fig. 13a). Although the amount of these impurities was not large, the molecular weight increased beyond 100 kDa, up to 1,000 kDa, and the polydispersity (Ð = M ) increased from 1.12 excluding the high molecular weight fraction to 4.88 including the corresponding fraction.w / M n ) increased substantially, which occurred simultaneously with the appearance of gel-like heterocomponents in the produced polyols. [DMC-Cl][MeOC3H6OH] and [DMC-Cl][tBuOH] exhibited particularly favorable abilities to produce polymers with narrow dispersities (Ð = 1.2). In contrast, DMC-OtBu produced polymers with broad dispersities (Ð = 7.2) up to 1,000 kDa, accompanied by the formation of gel-like components. The dispersities increased with increasing OtBu moiety not only in the DMC-(OAc / OtBu) series but also within the DMC-(OAc / OtBu / Cl) series (Figs. 14a and 15a). In particular, DMC-(OAc / OtBu / Cl)(0.74 / 0.24 / 0.10) and DMC-(OAc / OtBu / Cl)(0.59 / 0.38 / 0.15) showed the narrowest dispersion values ​​of 3.08 and 3.32 (1.15 and 1.12 excluding high molecular weight impurity fraction), respectively. tBuOZn + Although a gel-like portion was evident in all DMCs containing the unit, its presence was minimal in DMC-(OAc / OtBu / Cl)(0.59 / 0.38 / 0.15) and was noticeably less pronounced than the benchmark DMC, demonstrating almost equivalent performance, and almost identical performance to the benchmark DMC across other elements (Fig. 13a).

[0322]

[0323] [Experimental Example 2] PO / CO2 Copolymerization

[0324] PO / CO2 copolymerization was performed using the DMC catalyst according to the examples and comparative examples, and the results are shown in Table 4 below.

[0325] [Table 4] PO / CO2 copolymerization results of DMC catalysts according to examples and comparative examples a

[0326]

[0327] aCopolymerization conditions: DMC (11 μmol-Co), PPG starter (M n = 425 Da, 4.25 g), heated to 110°C, charged with CO2 gas to 30 bar, fed 5 mL PO for 4 minutes for initiation, waited until the pressure dropped 32-30 bar (initiation time), continuously fed PO at 0.50 mL / min for 54 minutes with temperature control using external heating, and charged with CO2 to 30 bar every time the pressure dropped to 25 bar. b Mass of polyol produced excluding the supply starter. c 1 (Mass of propylene carbonate) / (Mass of polymer + Mass of propylene carbonate) determined from H NMR spectrum. d 1 (Carbonate bonds) / (ether bonds + carbonate bonds) of polymers excluding cyclic carbonates determined from H NMR spectra. e Measured on GPC eluted with THF and processed using PS standards. f Polymerization temperature 100℃. g Pressure of 40-35 bar. h PO supply rate (1.0 mL / min) doubled and supply time (28 minutes) was halved.

[0328] The prepared DMC catalysts were evaluated in PO / CO2 copolymerization under continuous feeding of PO and CO2 gases (Table 4). In general, the catalytic activity decreased significantly under CO2 pressure, requiring a lower PO feed rate (0.50 vs. 1.25 mL / min) and a larger amount of catalyst (11 vs. 4.0 μmol). Notably, the productivities of the catalysts in these copolymerizations varied considerably, which was in contrast to the marginal productivity changes observed in PO polymerization. DMC-Cl, DMC-OC3H6OMe, and DMC-(OC3H6OMe / Cl)(0.5 / 0.5) showed low activities (yields, 3.1–6.7 g), whereas tBuOZn, including the benchmark catalysts, showed the lowest activity (yields, 3.1–6.7 g). + or AcOZn +Other DMCs containing the unit showed excellent activity, producing 18–28 g of polyol. A dramatic difference in productivity (19 g vs. 6.8 g, respectively) was observed between DMC-(OAc / OtBu)(0.97 / 0.02) and Zn2[Co(CN)6](CH3COO)·4H2O, which is structurally similar to the above DMC-(OAc / OtBu)(0.97 / 0.02). Interestingly, DMC-OAc / OtBu(0.95 / 0.08) and DMC-OAc / OtBu(0.68 / 0.31) showed the highest yields (27–28 g) with short induction times (15 min), demonstrating superiority over the benchmark DMC (yield, 25 g; induction time, 36 min).

[0329] In terms of the dispersion of the produced polymer, DMC-OAc / OtBu (0.95 / 0.08) also showed excellent results, exhibiting a fairly narrow unimodal GPC curve with the lowest Ð = 1.43 (Fig. 13b). However, DMC-OtBu and DMC-(OtBu / Cl) (0.5 / 0.5) showed low dispersions (Ð = 4.04 and 8.81, respectively) despite their excellent activities, and exhibited multimodal features with tailing toward higher molecular weight fractions. In particular, in the DMC-OAc / OtBu series catalysts, tBuOZn + As the fraction increased, the Ð value increased, resulting in significant tailing (Figs. 14b and 15b). The benchmark DMC catalyst also exhibited a high molecular weight tail with a narrow primary peak, similar to that observed in PO polymerization, resulting in a high value of 3.34.

[0330] A major concern in PO / CO2 copolymerization is the formation of cyclic carbonate (i.e., propylene carbonate) byproducts. Low-activity catalysts, such as DMC-Cl, DMC-OC3H6OMe, and DMC-(OC3H6OMe / Cl)(0.5 / 0.5), resulted in significant cyclic carbonate formation (9.2-25 mol%). In contrast, other highly active catalysts produced small amounts of cyclic carbonate (<5 mol%). Among these, DMC-OtBu, DMC-(OAc / OtBu / Cl)(0.59 / 0.38 / 0.15), and DMC-(OAc / OtBu / Cl)(0.74 / 0.24 / 0.10) exhibited exceptionally good performance, demonstrating the ability to limit cyclic carbonate formation to less than 2 wt%.

[0331] Carbon dioxide content (F) of the resulting polymers produced using DMC-OtBu and benchmark DMC CO2 ) was significantly lower (15 mol%). In contrast, except for DMC-(OAc / OtBu)(0.97 / 0.02), (AcO)Zn + DMC containing units is a CO2 mixture (F CO2 , 20-33 mol%), which showed remarkable performance, which is AcOZn + F correlated with increasing ratio CO2 It shows a discernible pattern of increasing levels. Interestingly, DMC-(OAc / OtBu)(0.97 / 0.02) has a substantially higher F of 29 mol%, as evidenced by the compositionally similar Zn2[Co(CN)6](CH3COO)·4H2O. CO2 In contrast to the value, a low F of 13 mol% (Example 6-1) CO2 The values ​​were expressed. The various binding modes of acetate are F CO2 played a significant role in influencing the value (see below).

[0332] In particular, DMC-(OAc / OtBu)(0.95 / 0.08) was distinguished by its excellent properties such as short induction time (15 min), improved productivity (yield, 27 g), narrow dispersity (Ð = 1.43), and the highest CO2 content (F) with minimal formation of cyclic carbonates (4.2 mol%). CO2 = 33 mol%) was obtained. This content could be further improved to 42 mol% by performing polymerization at a low temperature of 100°C (Example 6-2). f ). However, this is when the pressure is 40 to 35 bar (Example 6-2 g ) was not affected by the increase in F. In particular, DMC-(OAc / OtBu)(0.95 / 0.08) was not affected by the increase in F. CO2 Almost the same amount of copolymer (25 g; 5.3 kg / g-DMC) was produced while maintaining the value, and more advantageously, the production of cyclic carbonate was reduced to 3.4 mol% while doubling the PO feed rate and reducing the reaction time by half from 54 to 28 minutes (Example 6-2 h ) As a result, it showed a TOF of 64,000 PO-consumption / h / Co and 20,000 CO2-consumption / h / Co. The CO2 consumption rate achieved is similar to the best performance recorded using a homogeneous catalyst, especially a Salen-Co complex bound with four ammonium salts.

[0333]

[0334] [Experimental Example 3] Polymerization Mechanism

[0335] The initiation and propagation mechanisms in DMC-catalyzed PO polymerization have been a matter of debate. The prevailing hypothesis postulates that alcohol groups in the starter or growing chain externally attack PO bound to the Lewis acidic Zn site (Scheme 7A). According to this hypothesis, (tBuO)Zn + and (AcO)Zn +The unit is expected to remain in a continuous state throughout the polymerization process. Alternatively, the opposite hypothesis suggests that the -OtBu or -OAc group directly participates in initiation and propagation during chain growth by attacking the PO coordinated with the alkoxide or carbonate group. The process can unfold by linking a single Zn site (Scheme 7B) or two adjacent Zn sites (Scheme 7C). In particular, the bimetallic mechanism C has received considerable experimental support in CO2 / PO copolymerization.

[0336] To clarify this issue, the powder form of DMC-(OAc / OtBu / Cl)(0.68 / 0.38 / 0.06) was simply treated with PO gas at 20-25°C under reduced pressure without a starter. This treatment resulted in the formation of a limited amount of low molecular weight polymer (e.g., 240 mg of polymer containing 50 mg of DMC), where 1 The H NMR spectrum showed signals corresponding to the AcO and tBuO end groups (Scheme 7). This finding supports the presence of (AcO)Zn in DMC. + and (tBuO)Zn + Indicates that the unit was directly involved in the initiation process, providing confirmation for mechanism B or C. Nevertheless, the M calculated from the integrated values ​​of the AcO or tBuO terminal groups n The values ​​significantly exceeded those measured by GPC in all three experiments (11 vs. 5.9 kDa, 37 vs. 14 kDa, 40 vs. 19 kDa). This discrepancy suggests the occurrence of another chain growth process, potentially a "catch-up mechanism" A, in addition to mechanisms B or C. In the experiments, a discernible double GPC curve was observed, further supporting the presence of two different growth sites. The GPC curves were separated into two segments. One was M n = 84 kDa and Ð = 2.7 and the other is M n= 11 kDa and Ð = 1.8 (Reaction Scheme 7). The inventors of the present invention have discovered that the former is (RO)Zn + It can be attributed to chains grown at site (B or C), while the latter is Zn by a "catch-up mechanism" (A). 2+ It was assumed that this could be attributed to a chain that grew on the site.

[0337] [Reaction Scheme 7] Verifying the mechanism 1 Initiation and propagation mechanism (AC) including H NMR spectra and GPC curves

[0338]

[0339] A striking trend emerged in the experiment: a significant proportion of (RO)Zn + DMC catalysts containing the component exhibited high Ð values ​​with tailing to higher molecular weights while forming undesirable impurities such as gels. The inventors of the present invention have discovered (RO)Zn + Chain transfer process occurring at the site (via the action of external R'OH)Zn + It was suggested that the exchange of RO and R'O at the position occurred at a relatively slow rate, resulting in high values ​​with tailing. ClZn in DMC-Cl + The site remains inactive and Zn 2+ Only the site was operated, resulting in a polymer with a narrow dispersion. When chain growth mechanism B was operated, the DMC catalyst, especially (tBuO)Zn +The DMC catalyst, rich in units, was ultimately converted into a gel-like aggregate composed of fragmented DMC catalysts that attached numerous growing polymer chains. After removal of the catalyst residue using magnesium silicate / polyacrylic acid / water, the gel-like component disappeared, and the Ð value decreased significantly, especially with the removal of high molecular weight tails exceeding 100 kDa (3.32 → 1.41 for DMC-(OAc / OtBu / Cl)(0.59 / 0.38 / 0.15); 4.88 → 1.97 for the benchmark DMC; Figure 16).

[0340] The degree of separation between the asymmetric and symmetric stretching vibrational signals (denoted as Δ) is an indicator of the distinct binding modes of carboxylates. According to the guidelines given in the literature (Zelenak, V.; Vargovα, Z.; Gyoryova, K., Correlation of infrared spectra of zinc(II) carboxylates with their structures. Spectrochimica Acta Part A: Molecular and Biomolecular Spectroscopy 2007, 66 (2), 262-272), the main observed peaks at 1554 and 1443 cm in DMC-(OAc / OtBu)(0.95 / 0.08) and Zn2[Co(CN)6](CH3COO)·4H2O -1 (Δ = 111 cm -1 ) is attributed to the syn-anti bridge binding mode D (Fig. 17a, Fig. 17b), which is further supported by the solved crystal structure of Zn2[Co(CN)6](CH3COO)·4H2O.

[0341] 1583 and 1463 cm, slightly observed in DMC-(OAc / tOBu)(0.95 / 0.08) and mainly observed in DMC-(OAc / OtBu)(0.97 / 0.02). -1 (Δ = 120 cm -1) is due to the chelating bond mode E, which appears slightly in most of the prepared DMC catalysts at 1618 and 1355 cm -1 The remaining set in (Δ = 263 cm -1 ) is due to the single-site or single-atom bridged bonding mode F.

[0342] AcOZn + DMC catalysts containing units (especially those characterized by a predominantly syn-anti bridged bonding mode D, such as Zn2[Co(CN)6](CH3COO)·4H2O and DMC-(OAc / OtBu)(0.95 / 0.08)) are notable for their F CO2 values ​​(29 and 33 mol%, respectively), whereas catalysts characterized primarily by chelating bond mode E, such as DMC-(OAc / OtBu)(0.97 / 0.02), produced polymers with low F CO2 The value (13 mol%) was shown.

[0343] In CO2 / epoxide copolymerization, the bimetallic mechanism has been widely accepted, and the optimal Zn-Zn distance of 4.3–5.0 Å has been proposed. The structural analysis of Zn2[Co(CN)6](CH3COO)·4H2O revealed a Zn-Zn distance of 4.4 Å linked by syn-anti bridge acetates, which is highly suitable for promoting the bimetallic mechanism C. In contrast, the corresponding Zn-Zn distance revealed in the structure of DMC-OC3H6OMe was found to be too short (3.6 Å) to operate the bimetallic mechanism, leading to F CO2 The price has gone down.

[0344] Meanwhile, when heated to 60°C in a vacuum, it was confirmed that the primary acetate binding mode of DMC-(OAc / OtBu)(0.97 / 0.02) was switched from chelate E to syn-anti bridge D (Figs. 17b-17c). This binding mode change resulted in F CO2The value increased significantly from 13 mol% to 32 mol%, with a negligible effect on other performance indicators (Example 6-1 in Table 4). Importantly, the heat treatment did not noticeably affect the XRD pattern or SEM image. Although the heat-treated DMC-(OAc / OtBu)(0.97 / 0.02) and Zn2[Co(CN)6](CH3COO)·4H2O exhibited identical IR patterns, the resulting F CO2 The values ​​(32 and 29 mol%) were shown, respectively, and there was a significant difference in their activities (yield, 16.4 vs. 6.8 g). This activity change could potentially be caused by fragmentation or delamination of the catalyst. DMC-(OAc / OtBu) (0.95 / 0.08), which exhibited high activity, produced a clear and transparent solution in PO / CO2 copolymerization, confirming that the catalyst residue was well dispersed through fragmentation (Fig. 18a). In contrast, Zn2[Co(CN)6](CH3COO)·4H2O, which exhibited low activity, produced a turbid solution that underwent phase separation over time (Fig. 18b), and DMC-(OAc / OtBu) (0.97 / 0.02), which had intermediate activity, produced a slightly turbid solution without phase separation (Fig. 18c).

[0345] Meanwhile, a striking trend was observed regarding carbonate formation. A lower unsaturation level in PO polymerization was correlated with lower cyclic carbonate formation in PO / CO2 copolymerization. Specifically, (RO)Zn +Low unsaturation levels (< 0.010 meq / g) were achieved with DMC-OR and DMC with high component ratios [e.g., DMC-(OC3H6OMe / Cl)(0.75 / 0.25), DMC-(OAc / OtBu)(0.42 / 0.57), and DMC-(OAc / OtBu)(0.31 / 0.71)]. Interestingly, low unsaturation levels were also achieved with the DMC-(OtBu / Cl)(0.5 / 0.5) and DMC-(OAc / OtBu / Cl) series, generally with excess Cl. - was washed out in excess of the supply of PhOLi or AcOLi. -OCH2CH=CH2 terminal groups and the formation of cyclic carbonates were confirmed to be affected by the content of homogeneous Zn components (i.e., ClZn-OR or (AcO)Zn-OR). Specifically, the DMC catalyst was ClZn + or AcOZn + When the unit is included with minimal or no inclusion, leaching of the homogeneous Zn component is minimized, resulting in low unsaturation levels and low cyclic carbonate formation. During the manufacture of the DMC-(OtBu / Cl)(0.5 / 0.5) and DMC-(OAc / OtBu / Cl) series, certain potentially soluble fractions can be washed away, minimizing the generation of a homogeneous Zn component during polymerization.

[0346] The inventors of this invention successfully prepared high-purity H3[Co(CN)6] on a 60 g scale for preparative use and elucidated its X-ray structure. Subsequently, [ClZn + ][Zn 2+ ][(NC)6Co 3- ] well-defined DMCs with a composition of [ClZn + ][Zn 2+ ][(NC)6Co 3- ] by reacting [(RO)Zn with stoichiometric amounts of PhOLi or a 1:1 mixture of AcOLi / AcOH +][Zn 2+ ][(NC)6Co 3- ] (RO = MeOC3H6O, tBuO) and [(AcO)Zn + ][Zn 2+ ][(NC)6Co 3- ] was synthesized. [(MeOC3H6O)Zn + ][Zn 2+ ][(NC)6Co 3- ] atomic-level structure was revealed by Rietveld refinement of synchrotron XRD data. Additionally, [(RO)Zn + ] p [ClZn + ] (1-p) [Zn 2+ ][(NC)6Co 3- ], [(tBuO)Zn + ] p [(tBuO)Zn + ] q [Zn 2+ ][(NC)6Co 3- ], and [(AcO)Zn + ] p [(tBuO)Zn + ] q [ClZn + ] r [Zn 2+ ][(NC)6Co 3- ] was manufactured.

[0347] Analysis of the polymer produced by briefly exposing DMC-(OAc / OtBu / Cl)(0.68 / 0.38 / 0.06) to PO gas showed that Zn 2+ Not only the site, (tBuO)Zn + and (AcO)Zn + Chain growth processes were observed at all sites. Higher proportions of (RO)Zn + DMC catalysts containing units exhibited higher Ð values ​​as the molecular weight increased. This phenomenon is attributed to (RO)Zn + This is due to the chains growing from the unit, which may slow down the chain transfer process. (AcO)Zn +DMC catalysts containing units, especially those characterized by a syn-anti bridge binding mode of mainly acetate, are noteworthy. CO2 Polymers with values ​​were produced. This result is attributed to the presence of an appropriate Zn-Zn distance to promote the bimetallic chain growth mechanism. Among the prepared catalysts, DMC-(OAc / OtBu / Cl) (0.59 / 0.38 / 0.15) showed almost equivalent performance to the benchmark DMC in PO polymerization, with the additional advantage of producing less gel-like impurities. DMC-(OAc / OtBu) (0.95 / 0.08) outperformed the benchmark DMC in PO / CO2 copolymerization by producing polyols with twice the CO2 content.

[0348] Simple modifications or changes of the present invention can be easily implemented by a person having ordinary skill in the art, and all such modifications or changes can be considered to be included in the scope of the present invention.

[0349] The scope of the present invention is indicated by the claims described below rather than the detailed description above, and all changes or modifications derived from the meaning and scope of the claims and their equivalent concepts should be interpreted as being included in the scope of the present invention.

Claims

1. A double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 1: [Chemical Formula 1] [ClZn + ] (1-p) [(RO)Zn + ] p [Zn 2+ ][(NC)6Co 3- ] (In the above chemical formula 1, p is between 0.1 and 1.0, R is C1-C 20 Alkyl ether or C1-C 20 (Alkyl).

2. In paragraph 1, In the above chemical formula 1, the p value is 0.25 to 0.75, DMC catalyst.

3. In paragraph 1, In the above chemical formula 1, R is tert-Bu, DMC catalyst.

4. In paragraph 1, A DMC catalyst, wherein in the above chemical formula 1, R is MeOC3H6. A first step of forming a precipitate by mixing H3Co(CN)6 and ZnCl2 in a 1-methoxy-2-propanol solvent containing less than 5.30 wt% of water, and filtering the precipitate to obtain the precipitate; The precipitate obtained in the above first step is ROH containing less than 50 wt% of water (wherein R is C1-C 20 Alkyl ether or C1-C 20 A second step of reacting lithium phenoxide (PhOLi) in an alkyl) solvent and then filtering to remove the byproduct LiCl and obtain a solid compound; and A third step of drying the solid compound obtained in the second step by vacuum depressurization; including, A method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 1: [Chemical Formula 1] [(RO)Zn + ] p [ClZn + ] (1-p) [Zn 2+ ][(NC)6Co 3- ] (In the above chemical formula 1, p is between 0.1 and 1.0, R is C1-C 20 Alkyl ether or C1-C 20 (Alkyl).

6. In paragraph 5, In the above first step, the molar ratio of H3Co(CN)6 and ZnCl2 is 1:

2. Method for producing DMC catalyst.

7. In paragraph 5, The molar ratio of H3Co(CN)6 introduced in the first step and PhOLi introduced in the second step is 1:0.25 to 1:0.

75. Method for producing DMC catalyst.

8. In paragraph 5, The reaction temperature of the first step is 50°C to 80°C, Method for producing DMC catalyst.

9. In paragraph 5, The vacuum drying temperature of the third step is 20°C to 100°C, Method for producing DMC catalyst.

10. A step of preparing a double metal cyanide (DMC) catalyst by a method according to any one of claims 5 to 9; and A step of polymerizing propylene oxide in the presence of a polyol starter using the above DMC catalyst; including, Method for producing polyether polyol.

11. In paragraph 10, The above polyol starter is polypropylene glycol having a molecular weight of 300 to 800. Method for producing polyether polyol. 12.(NC)6Co 3- , (AcO)Zn + , and Zn 2+ Contains ingredients, Additionally, ClZn + and / or (RO)Zn + (R is C1-C 20 Alkyl ether or C1-C 20 Containing alkyl components, Double metal cyanide (DMC) catalyst.

13. In paragraph 12, The above (AcO)Zn + The components were observed at 1618, 1583, 1554, 1463, 1443, and 1355 cm in the ATR-FTIR spectrum. -1 which is measured in, Double metal cyanide (DMC) catalyst.

14. In paragraph 12, A double metal cyanide (DMC) catalyst wherein R is tert-butyl.

15. In paragraph 14, (tert-BuO)Zn + The component is detected at 640 cm in the ATR-FTIR spectrum. -1 Double metal cyanide (DMC) catalyst, which is measured in the vicinity.

16. In paragraph 12, The above double metal cyanide (DMC) catalyst is (NC)6Co 3- , (AcO)Zn + , Zn 2+ and (tert-BuO)Zn + Contains ingredients, Double metal cyanide (DMC) catalyst.

17. In paragraph 16, Above (NC)6Co 3- , (AcO)Zn + , Zn 2+ and (tert-BuO)Zn + A double metal cyanide (DMC) catalyst comprising a component having a composition represented by the following chemical formula 2: [Chemical Formula 2] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [Zn 2+ ] a [(NC)6Co 3- ] (In the above chemical formula 2, p is 0.1 to 1.2; q is 0.01 to 0.9; p + q is 0.9 to 1.2; (p + q + 2a is 3).

18. In paragraph 17, The above p is 0.3 to 0.98; The above q is 0.01 to 0.75, Double metal cyanide (DMC) catalyst.

19. In paragraph 18, The above p is 0.90 to 0.98; The above q is 0.01 to 0.10, Double metal cyanide (DMC) catalyst.

20. In paragraph 12, The above double metal cyanide (DMC) catalyst is (NC)6Co 3- , (AcO)Zn + , Zn 2+ , (tert-BuO)Zn + and ClZn + Contains ingredients, Double metal cyanide (DMC) catalyst.

21. In paragraph 20, Above (NC)6Co 3- , (AcO)Zn + , Zn 2+ , (tert-BuO)Zn + and ClZn + A double metal cyanide (DMC) catalyst comprising a component having a composition represented by the following chemical formula 3: [Chemical Formula 3] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [ClZn + ] r [Zn 2+ ] a [(NC)6Co 3- ] (In the above chemical formula 3, p is 0.3 to 0.8; q is 0.2 to 0.5; r is 0.05 to 0.5; p + q + r is 0.9 to 1.2; (p + q + r + 2a is 3).

22. In paragraph 21, The above p is 0.4 to 0.8; The above q is 0.2 to 0.5; The above r is 0.1 to 0.3, Double metal cyanide (DMC) catalyst. 23.(NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound consisting of the components, lithium acetate (AcOLi) and acetic acid in a tert-butanol (tert-BuOH) solvent containing less than 30 wt% of water, is prepared by reacting the ClZn + A method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 2, comprising the steps of adding 1 equivalent and 1 to 0.4 equivalents of each component, reacting them, filtering them to obtain a solid compound, and removing the remaining solvent by vacuum depressurization: [Chemical Formula 2] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [Zn 2+ ] a [(NC)6Co 3- ] (In the above chemical formula 2, p is 0.1 to 1.2; q is 0.01 to 0.9; p + q is 0.9 to 1.2; (p + q + 2a is 3).

24. In paragraph 23, The above (NC)6Co as the starting material 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOCH2CH(Me)OH], a method for producing a DMC catalyst.

25. In paragraph 23, The above (NC)6Co as the starting material 3- , ClZn + , and Zn 2+ A method for producing a double metal cyanide (DMC) catalyst, wherein the DMC compound is produced by reacting H3Co(CN)6 and ZnCl2 in a molar ratio of 1:

2. 26.(NC)6Co 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound consisting of ClZn, lithium acetate (AcOLi) and acetic acid in a tert-butanol (tert-BuOH) solvent containing less than 30 wt% of water + A method for producing a double metal cyanide (DMC) catalyst having a composition represented by the following chemical formula 3, comprising the steps of adding 0.95 to 0.5 equivalents and 0.95 to 0.5 equivalents of each component, reacting them, filtering them to obtain a solid compound, and removing the remaining solvent by vacuum depressurization: [Chemical Formula 3] [(AcO)Zn + ] p [(tert-BuO)Zn + ] q [ClZn + ] r [Zn 2+ ] a [(NC)6Co 3- ] (In the above chemical formula 3, p is 0.3 to 0.8; q is 0.2 to 0.5; r is 0.05 to 0.5; p + q + r is 0.9 to 1.2; (p + q + r + 2a is 3).

27. In paragraph 26, The above (NC)6Co as the starting material 3- , ClZn + , and Zn 2+ A double metal cyanide (DMC) compound composed of [ClZn + ][Zn 2+ ][(NC)6Co 3- ][MeOCH2CH(Me)OH], a method for producing a DMC catalyst.

28. In paragraph 26, The above (NC)6Co as the starting material 3- , ClZn + , and Zn 2+ A method for producing a double metal cyanide (DMC) catalyst, wherein the DMC compound is produced by reacting H3Co(CN)6 and ZnCl2 in a molar ratio of 1:

2.

29. A step of preparing a double metal cyanide (DMC) catalyst according to any one of claims 23 to 28; and A step of polymerizing propylene oxide in the presence of a polyol starter using the above DMC catalyst; including, Method for producing polyether polyol.

30. In paragraph 29, The above polyol starter is polypropylene glycol having a molecular weight of 300 to 800. Method for producing polyether polyol.

31. A step of preparing a double metal cyanide (DMC) catalyst according to any one of claims 23 to 28; and A step of copolymerizing propylene oxide and CO2 in the presence of a polyol starter using the above DMC catalyst; including, A method for producing poly(ether-co-carbonate) polyol.

32. In paragraph 31, The above polyol starter is polypropylene glycol having a molecular weight of 300 to 800. A method for producing poly(ether-co-carbonate) polyol.

Citation Information

Patent Citations

  • High active double metal cyanide catalyst, manufacturing method thereof, and application thereof

    JP2019077850A

  • Double metal cyanide catalyst and epoxide / carbon dioxide copolymer manufactured using same

    KR1020150010602A

  • Display Device and Driving Method thereof

    KR1020240119986A

  • Eco-friendly cashmere and method for manufacturing thereof

    KR102380109B1