Electroplating method of cyanide-free zinc plating electroplate liquid
By preparing the electroplating solution in the cyanide-free galvanizing process and controlling the electroplating conditions, the problem of insufficient brightness and uniformity of the plating layer is solved, and efficient and uniform deposition of zinc coating is achieved, avoiding slow plating and burning.
Patent Information
- Application Number
- CN202411028252.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-12-03
AI Technical Summary
The existing cyanide-free galvanizing process has shortcomings in brightness and uniformity of the plating, and the narrow current density during electroplating causes the plating to be slow and easy to burn, resulting in defective products.
By preparing cyanide-free galvanized electroplating solution, including mechanical polishing, cleaning and pickling, pretreatment workpieces, select the appropriate current density (low, medium, and high current density) for electroplating, and add auxiliary additives and complexing agents to the electroplating solution. , brighteners, wetting agents and antioxidants, control the plating temperature and time, and ensure uniformity and adhesion of the plating layer.
A bright, uniform and strong adhesion zinc coating is achieved, which avoids the problems of slow plating and burning. It is suitable for electroplating conditions of different workpieces, and improves the plating quality and electroplating efficiency.
Abstract
Description
Technical Field
[0001] The present application relates to an electroplating method of a cyanide-free zinc plating solution, belonging to the technical field of electroplating processes. Background Art
[0002] Traditional zinc plating processes often use cyanide as a key component of the electroplating solution, but cyanide has extremely high toxicity and environmental hazards, which limits its application. Therefore, the cyanide-free zinc plating process has gradually become the focus of research and application. However, due to the serious hydrogen evolution during the cyanide zinc plating process, the zinc coating has a high brittleness, and the cyanide zinc plating solution has a high toxicity, the wastewater treatment is difficult, and the air and groundwater are seriously polluted. Now alkaline zinc plating and weak acid zinc plating processes are gradually developed and used in industrial electroplating to replace cyanide zinc plating. However, the current cyanide-free zinc plating process still has some shortcomings in terms of brightness and coating uniformity, which needs further improvement and optimization.
[0003] The existing cyanide-free zinc plating process still has the problems of narrow current density during electroplating and slow plating and easy burning during electroplating. Summary of the invention
[0004] The purpose of the present application is to provide an electroplating method of a cyanide-free zinc plating solution to solve the current problems of slow and easy burning of the cyanide-free zinc plating layer, narrow current density, and defective products.
[0005] According to one aspect of the present application, a method for electroplating a cyanide-free zinc plating solution is provided, the electroplating method comprising the following steps:
[0006] S1: preparing a cyanide-free zinc plating solution;
[0007] S2: After mechanical polishing, cleaning and pickling of the workpiece to be processed, a pre-processed workpiece is obtained;
[0008] S3: immersing the pretreated workpiece in a cyanide-free zinc plating solution, connecting a power supply, and electroplating to obtain a workpiece with a coating;
[0009] S4: passivating and drying the workpiece containing the coating to obtain a workpiece containing a cyanide-free zinc coating.
[0010] Optionally, in step S3, the electroplating density includes low current density, medium current density and high current density.
[0011] Optionally, the low current density is 1-2A / dm 2 .
[0012] Optionally, the low current density is independently selected from 1A / dm 2 , 1.2A / dm 2 , 1.5A / dm 2, 1.8A / dm 2 , 2A / dm 2 Any value in or a range between any two of the above.
[0013] Optionally, the low current density is suitable for workpieces with more complex shapes or requiring higher coating uniformity; at this current density, the coating thickness uniformity is better, but the deposition rate is slower, which is suitable for electroplating processes that require careful control.
[0014] Optionally, the medium current density is 2 to 4 A / dm 2 .
[0015] Optionally, the medium current density is independently selected from 2A / dm 2 , 2.2A / dm 2 , 2.5A / dm 2 , 2.8A / dm 2 、3A / dm 2 , 3.2A / dm 2 , 3.4A / dm 2 、3.5A / dm 2 、3.8A / dm 2 , 4A / dm 2 Any value in or a range between any two of the above.
[0016] Optionally, the medium current density is suitable for most industrial electroplating applications, such as automotive parts, fasteners, etc., and can provide good coating brightness and thickness control; and can balance deposition speed and coating quality.
[0017] Optionally, the high current density is 4 to 8 A / dm 2 .
[0018] Optionally, the high current density is independently selected from 4A / dm 2 , 4.2A / dm 2 , 4.5A / dm 2 , 4.8A / dm 2 , 5A / dm 2 , 5.2A / dm 2 , 5.5A / dm 2 , 5.8A / dm 2 、6A / dm 2 、6.5A / dm 2 , 7A / dm 2 , 7.5A / dm 2 , 8A / dm 2 Any value in or a range between any two of the above.
[0019] Optionally, the high current density is suitable for depositing thicker and faster coatings, but may result in a rough coating or burning, requiring better process control.
[0020] Optionally, the electroplating temperature is 15 to 50° C., and the electroplating time is 10 to 30 minutes.
[0021] Optionally, the electroplating temperature is independently selected from any value of 15°C, 20°C, 25°C, 30°C, 35°C, 40°C, 45°C, 50°C or a range between any two of the above values.
[0022] Optionally, the electroplating time is independently selected from any value among 10 min, 15 min, 20 min, 25 min, 30 min or a range between any two of the above.
[0023] Optionally, the electroplating anode is a zinc electrode.
[0024] Optionally, in step S1, the method for preparing the cyanide-free zinc plating solution comprises:
[0025] (1) stirring a mixture containing an auxiliary additive, a complexing agent, a leveling agent and water for 1 hour to obtain a first mixed solution;
[0026] (2) adding a brightener, a wetting agent and an antioxidant to the first mixed solution, stirring, and adjusting the pH to obtain the cyanide-free zinc plating solution.
[0027] Optionally, in step (1), the dosage of the auxiliary additive, complexing agent and leveling agent is: (25-400): (2-2.5): (0.1-0.5).
[0028] Optionally, the dosage of the brightener, wetting agent and antioxidant is: (0.5-3.0): (2-5): (0.3-5).
[0029] Optionally, the brightener is selected from at least one of benzyl acetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and its derivatives, and p-methoxybenzaldehyde.
[0030] Optionally, the brightener is p-methoxybenzaldehyde.
[0031] Optionally, in step (1), the auxiliary additive is selected from at least one of aluminum salt, zinc salt, potassium salt and ammonium salt.
[0032] Optionally, the aluminum salt is selected from at least one of aluminum sulfate, aluminum chloride and aluminum nitrate.
[0033] Optionally, the zinc salt is selected from at least one of zinc chloride, zinc sulfate and zinc nitrate.
[0034] Optionally, the potassium salt is selected from at least one of potassium chloride, potassium nitrate and potassium nitrate.
[0035] Optionally, the ammonium salt is selected from at least one of ammonium nitrate, ammonium sulfate and ammonium chloride.
[0036] Optionally, in step (1), the complexing agent is selected from at least one of ethylenediaminetetraacetic acid, triethanolamine, sodium citrate and glycine.
[0037] Optionally, the leveling agent is selected from at least one of polyethylene glycol, polyacrylamide, and sodium N,N-dimethyldithiocarbamate.
[0038] Optionally, in step (2), the wetting agent is selected from sodium alkyl sulfonate and / or sodium alkylbenzene sulfonate.
[0039] Optionally, in step (2), the antioxidant is selected from ascorbic acid and / or sodium metabisulfite.
[0040] Optionally, in step (1), the temperature of stirring I is 20 to 50° C., the speed of stirring I is 150 to 500 r / min, and the time of stirring I is 2 to 6 h.
[0041] Optionally, in step (2), the temperature of stirring II is 30 to 80° C., the rotation speed of stirring II is 100 to 600 r / min, and the time of stirring II is 2 to 8 h.
[0042] Optionally, in step S1, the pH value of the cyanide-free zinc plating solution is 5-6.
[0043] Optionally, in step S2, the pickling solution is dilute hydrochloric acid.
[0044] Optionally, in step S4, the passivation method is chromic acid passivation.
[0045] Optionally, the drying temperature is 20 to 200° C., and the drying time is 0.2 to 2 hours.
[0046] As an optional implementation method, the present application is implemented through the following technical solutions:
[0047] Operation steps of cyanide-free zinc plating:
[0048] (1) Prepare the electroplating solution: dissolve zinc chloride in deionized water, add potassium chloride and boric acid, fully dissolve and mix evenly, add brightener, wetting agent, complexing agent, antioxidant, leveling agent, and stir evenly;
[0049] (2) Pretreatment of workpieces: Mechanical polishing, cleaning, pickling (such as dilute hydrochloric acid) of the workpieces to remove oxides and oil stains; use electrolytic degreasing (such as cathodic electrolytic degreasing) to ensure that the workpiece surface is clean;
[0050] (3) Electroplating process: immerse the workpiece in the electroplating solution and connect the power supply; control the current density and temperature to maintain a stable electroplating environment; the electroplating time is adjusted according to the required coating thickness, generally 10-30 minutes;
[0051] (4) Post-treatment: After electroplating, the workpiece is removed and cleaned with deionized water; passivation treatment (such as chromic acid passivation) is performed to improve the corrosion resistance of the coating; and finally, drying treatment is performed to ensure that the workpiece surface is clean and free of water stains.
[0052] During electroplating, regularly analyze and adjust the composition of the plating solution to maintain the stability of the formula; ensure that the operating environment is well ventilated to prevent acid mist from harming operators, and use appropriate protective equipment such as gloves, goggles and protective clothing.
[0053] In cyanide zinc electroplating, the choice of current density is also affected by the following factors: Bath composition: cyanide concentration, zinc ion concentration, type and concentration of additives. Temperature: The temperature of the plating solution needs to be kept within a certain range (usually 20-30°C) to ensure the stability of the electroplating process. Stirring: Stirring can improve the uniformity and brightness of the coating. Workpiece shape and size: Complex-shaped workpieces require lower current density, while simple-shaped workpieces can use higher current density. Adjust according to the different workpieces during actual electroplating.
[0054] The beneficial effects of this application include:
[0055] The electroplating method of the cyanide-free zinc plating solution provided by the present application has relatively simple operating conditions, and can obtain a bright, uniform and highly adhesive zinc coating. In addition, the electroplating density of the cyanide-free zinc plating solution disclosed in the present application is wide during electroplating, which can meet the conditions of electroplating different workpieces, thereby avoiding the problems of slow coating and burning.
[0056] The electroplating method of the cyanide-free zinc plating solution provided in the present application can select a suitable current density according to specific process requirements and workpiece characteristics, thereby ensuring the best coating quality and electroplating efficiency. DETAILED DESCRIPTION
[0057] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0058] Unless otherwise specified, the raw materials in the examples of this application were purchased through commercial channels.
[0059] Unless otherwise specified, the instruments and equipment used in this application are all conventional instruments and equipment.
[0060] Example 1
[0061] S1: preparing electroplating solution: weighing 50g zinc sulfate, 30g sodium chloride, 2g ethylenediaminetetraacetic acid complexing agent, 0.1g polyethylene glycol leveling agent, and 400g water, adding them into a container, stirring at 150r / min and 20°C for 2h on a magnetic stirrer to obtain a uniformly mixed first mixed solution; adding 0.5g p-methoxybenzaldehyde brightener, 2g sodium alkyl sulfonate wetting agent, 0.3g ascorbic acid antioxidant into the first mixed solution, and adding 485.1g water again, stirring at 100r / min and 30°C on a magnetic stirrer for 2h, adjusting the pH value to 5 with boric acid, and obtaining a cyanide-free zinc plating solution;
[0062] S2: Pretreatment of workpiece: Mechanical polishing, ultrasonic water washing, and pickling activation are performed on the metal tools to be electroplated in sequence to remove oxides and oil stains;
[0063] S3: Electroplating: With the zinc electrode as the anode and the metal tool to be electroplated as the cathode, electroplating is performed using the electroplating solution prepared in step S1. The electroplating temperature is 15-30°C and the current density is 1-2A·dm 2 , the electroplating time is 20 to 30 minutes;
[0064] S4: post-processing, cleaning the metal tool after electroplating in step S3 and drying it at 50° C. for 30 min to obtain a bright and uniform zinc-plated layer with a coating thickness of 0.3 to 0.6 μm.
[0065] Example 2
[0066] S1: 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water were weighed and added into a container, and stirred at 500 r / min and 50° C. for 6 h on a magnetic stirrer to obtain a uniformly mixed first mixed solution; 0.5 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant were added into the first mixed solution, and 485.1 g of water was added again to mix, and stirred at 600 r / min and 80° C. for 8 h on a magnetic stirrer, and the pH value was adjusted to 6 with boric acid to obtain a cyanide-free zinc plating solution;
[0067] S2: Pretreatment of workpiece: Mechanical polishing, ultrasonic water washing, and pickling activation are performed on the metal tools to be electroplated in sequence to remove oxides and oil stains;
[0068] S3: Electroplating: With the zinc electrode as the anode and the metal tool to be electroplated as the cathode, electroplating is performed using the electroplating solution prepared in step S1. The electroplating temperature is 20-35°C and the current density is 2-4A·dm 2 , the electroplating time is 15 to 20 minutes;
[0069] S4: post-processing, cleaning the metal tool after electroplating in step S3 and drying it at 60° C. for 1 hour to obtain a bright and uniform zinc-plated layer with a coating thickness of 0.25 to 0.4 μm.
[0070] Example 3
[0071] S1: 50 g of zinc sulfate, 30 g of sodium chloride, 2 g of ethylenediaminetetraacetic acid complexing agent, 0.1 g of polyethylene glycol leveling agent, and 400 g of water were weighed and added into a container, and stirred for 3 h at 40° C. with a magnetic stirrer at 300 r / min to obtain a uniformly mixed first mixed solution; 0.5 g of p-methoxybenzaldehyde brightener, 2 g of sodium alkyl sulfonate wetting agent, and 0.3 g of ascorbic acid antioxidant were added into the first mixed solution, and 485.1 g of water was added again to mix, and stirred for 5 h at 50° C. with a magnetic stirrer at 400 r / min, and the pH value was adjusted to 5 with boric acid to obtain a cyanide-free zinc plating solution;
[0072] S2: Pretreatment of workpiece: Mechanical polishing, ultrasonic water washing, and pickling activation are performed on the metal tools to be electroplated in sequence to remove oxides and oil stains;
[0073] S3: Electroplating: With the zinc electrode as the anode and the metal tool to be electroplated as the cathode, electroplating is performed using the electroplating solution prepared in step S1. The electroplating temperature is 25-50°C and the current density is 4-8A·dm 2 , the electroplating time is 10 to 15 minutes;
[0074] S4: post-processing, cleaning the metal tool after electroplating in step S3 and drying it at 70° C. for 40 min to obtain a bright and uniform zinc-plated layer with a coating thickness of 0.3 to 0.6 μm.
[0075] Comparative Example 1
[0076] In the process of preparing the electroplating solution in step S1 of Example 1, no methoxyformaldehyde brightener is added, and other conditions and configuration of the plating solution are the same as those in Example 1.
[0077] The metal tools obtained by processing in the above-mentioned Examples 1 to 3 and Comparative Example 1 were observed under a microscope, and it was found that the surfaces of the coatings in Examples 1 to 3 were uniform and dense, without peeling or bubbling. After corrosion resistance tests and hardness tests, it was found that the test time for the appearance of rust spots in the neutral salt spray test was 150 to 200 hours; the surface hardness reached 2000 to 2800 HV; it was found that the surface of the coating in Comparative Example 1 was uneven, with small concave and convex spots, and slight peeling and bubbling. After corrosion resistance tests and hardness tests, effective corrosion and hardness tests could not be carried out.
[0078] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for electroplating a cyanide-free zinc plating solution, characterized in that: The electroplating method comprises the following steps: S1: preparing a cyanide-free zinc plating solution; S2: After mechanical polishing, cleaning and pickling of the workpiece to be processed, a pre-processed workpiece is obtained; S3: immersing the pretreated workpiece in a cyanide-free zinc plating solution, connecting a power supply, and electroplating to obtain a workpiece with a coating; S4: passivating and drying the workpiece containing the coating to obtain a workpiece containing a cyanide-free zinc coating.
2. The electroplating method according to claim 1, characterized in that: In the step S3, the electroplating density includes low current density, medium current density and high current density; Preferably, the low current density is 1-2A / dm 2 ; Preferably, the medium current density is 2 to 4 A / dm 2 ; Preferably, the high current density is 4 to 8 A / dm 2 ; Preferably, the electroplating temperature is 15-50°C and the electroplating time is 10-30 minutes; Preferably, the electroplating anode is a zinc electrode.
3. The electroplating method according to claim 1, characterized in that: In the step S1, the method for preparing the cyanide-free zinc plating solution comprises: (1) stirring a mixture containing an auxiliary additive, a complexing agent, a leveling agent and water for 1 hour to obtain a first mixed solution; (2) adding a brightener, a wetting agent and an antioxidant into the first mixed solution, stirring II, and adjusting the pH to obtain the cyanide-free zinc plating solution.
4. The electroplating method according to claim 3, characterized in that: In the step (1), the dosage of the auxiliary additive, complexing agent and leveling agent is: (25-400): (2-2.5): (0.1-0.5); Preferably, the dosage of the brightener, wetting agent and antioxidant is: (0.5-3.0): (2-5): (0.3-5); Preferably, the brightener is selected from at least one of benzyl acetone, benzylamine, acetylene alcohol compounds, benzyl chloride, thiourea and its derivatives, and p-methoxybenzaldehyde.
5. The electroplating method according to claim 3, characterized in that: In the step (1), the auxiliary additive is selected from at least one of aluminum salt, zinc salt, potassium salt and ammonium salt; Preferably, the aluminum salt is selected from at least one of aluminum sulfate, aluminum chloride and aluminum nitrate; Preferably, the zinc salt is selected from at least one of zinc chloride, zinc sulfate and zinc nitrate; Preferably, the potassium salt is selected from at least one of potassium chloride, potassium nitrate and potassium nitrate; Preferably, the ammonium salt is selected from at least one of ammonium nitrate, ammonium sulfate and ammonium chloride.
6. The electroplating method according to claim 3, characterized in that: In the step (1), the complexing agent is selected from at least one of ethylenediaminetetraacetic acid, triethanolamine, sodium citrate, and glycine; Preferably, the leveling agent is selected from at least one of polyethylene glycol, polyacrylamide, and sodium N,N-dimethyldithiocarbamate; Preferably, in step (2), the wetting agent is selected from sodium alkyl sulfonate and / or sodium alkylbenzene sulfonate; Preferably, in step (2), the antioxidant is selected from ascorbic acid and / or sodium metabisulfite.
7. The electroplating method according to claim 3, characterized in that: In the step (1), the temperature of the stirring I is 20 to 50° C., the speed of the stirring I is 150 to 500 r / min, and the time of the stirring I is 2 to 6 h; Preferably, in step (2), the temperature of stirring II is 30 to 80° C., the speed of stirring II is 100 to 600 r / min, and the time of stirring II is 2 to 8 h.
8. The electroplating method according to claim 1, characterized in that: In the step S1, the pH value of the cyanide-free zinc plating solution is 5-6.
9. The electroplating method according to claim 1, characterized in that: In step S2, the pickling solution is dilute hydrochloric acid.
10. The electroplating method according to claim 1, characterized in that: In the step S4, the passivation method is chromic acid passivation; Preferably, the drying temperature is 20-200° C., and the drying time is 0.2-2 h.
Citation Information
Patent Citations
Zn plating liquid
CN102418122A
Chloride bath electrogalvanizing method
JP1996283982A
Additive for acid zinc alloy plating bath, acid zinc alloy plating bath, and method for producing zinc alloy plated article
US20160090659A1
Acid zinc plating baths and methods for electrodepositing bright zinc deposits
US4162947A
Cited By
Alkaline system multi-stage current-interface coordinated regulation zinc electrode preparation method
CN121204749A