Ether / ester composite polyurethane foam cosmetic
The ester/ether composite polyurethane foam with a specific ratio addresses the hydrolysis and hardness issues of existing foams by offering improved hydrolysis resistance and hardness, resulting in a stable and effective cosmetic distribution with enhanced application feel.
Patent Information
- Application Number
- PCT/KR2024/002126
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-25
- Filing Date
- 2024-02-15
- Publication Date
- 2024-10-31
AI Technical Summary
Ester-based polyurethane foam used in cushion cosmetics offers better application feel but has low hydrolysis resistance, making it difficult to commercialize, while ether-based foam has excellent hydrolysis resistance but weaker hardness, necessitating a balance between the two.
Development of an ester/ether composite polyurethane foam with a specific ether/ester ratio of 1:9 to 3:7, combined with a cosmetic composition having a low water content and specific emulsifier ratios, to enhance usability and maintain stability and hardness.
The ester/ether composite polyurethane foam provides improved hydrolysis resistance and hardness, ensuring a stable and uniform cosmetic distribution with a reduced hardness reduction after impregnation, enhancing the overall application feel and usability.
Smart Images

Figure KR2024002126_31102024_PF_FP_ABST
Abstract
Description
Ether / ester complex polyurethane foam cosmetics
[0001] The present invention relates to cosmetics, and more particularly, to cosmetics comprising a polyurethane foam impregnated with a liquid cosmetic.
[0002] Cosmetics exist in various forms, such as solid and liquid, and in the case of liquid cosmetics, it is common to store them in flexible containers, such as tubes, to prevent leakage and facilitate discharge.
[0003] Recently, cushion cosmetics have been used in which a liquid cosmetic having low or high viscosity is impregnated into an impregnating agent such as polyurethane foam, and then the polyurethane foam is pressurized using a tool such as a puff so that the cosmetic is applied to the puff and discharged.
[0004] Polyurethane foam is mainly used as an impregnating material for such cosmetics. This polyurethane foam can be classified into ether polyurethane foam and ester polyurethane foam depending on the type of polyol used in the polymerization reaction. In general, ether polyurethane foam is known to have excellent hydrolysis resistance, so ether polyurethane foam is preferred as a polyurethane foam for impregnating cosmetics.
[0005] However, ether-based polyurethane foams are less hard than ester-based polyurethane foams, making them less comfortable for consumers to apply, especially in cushion cosmetics that require application with a puff. Therefore, ester-based polyurethane foams are increasingly being used. However, foams containing only ester-based polyols exhibit poor hydrolysis resistance, hindering their commercialization. Therefore, there is a pressing need to develop foams that maximize the advantages of ester-based polyurethane foams while minimizing their disadvantages.
[0006] In order to solve the problems of the above prior art, the present invention aims to provide a cosmetic comprising an ester / ether composite polyurethane foam having a specific ether / ester ratio.
[0007] Additionally, we aim to provide cosmetics with improved usability and convenience.
[0008] In order to achieve the above technical task, the present invention provides a cosmetic comprising a polyurethane foam impregnated with a cosmetic composition, wherein the polyurethane of the polyurethane foam contains an ether group and an ester group in a molar ratio of 1:9 to 3:7, and the cosmetic composition has a water content of 35 wt% or less.
[0009] In the present invention, the water content of the cosmetic composition may be 30 wt% or less. In addition, the water content of the cosmetic composition may be 20 wt% or less. In addition, the water content of the cosmetic composition may be 5 wt% or less.
[0010] The cosmetic composition of the present invention preferably includes an oil phase component and an aqueous phase component, and the weight ratio of the aqueous phase component: oil phase component is 1:1.85 or more.
[0011] In addition, the cosmetic composition includes a main emulsifier and an auxiliary emulsifier, and it is preferable that the main emulsifier and the auxiliary emulsifier are in a weight ratio of 3:1 to 4:1.
[0012] At this time, it is preferable that the main emulsifier includes at least one substance selected from the group consisting of lauryl PEG-10 tris(trimethylsiloxy)silylethyl dimethicone, lauryl PEG-9 polydimethylsiloxyethyl dimethicone, and cetyl PEG / PPG-10 / 1 dimethicone, and the auxiliary emulsifier includes at least one substance selected from PEG-10 dimethicone and sorbitan isostearate.
[0013] In the present invention, it is preferable that the hardness of the polyurethane foam after impregnation is 50 to 65. At this time, it is more preferable that the hardness reduction rate before and after impregnation based on the hardness before impregnation of the polyurethane foam is 30% or less.
[0014] According to the present invention, a cosmetic product comprising an ester / ether composite polyurethane foam having a specific ether / ester ratio can be provided.
[0015] In addition, according to the present invention, it is possible to provide a cosmetic product having a composite polyurethane foam in which the cosmetic composition exists in a stable state in a supported state and can be uniformly redistributed within the foam when pressurized.
[0016] FIG. 1 is a schematic drawing of a cosmetic product according to one embodiment of the present invention.
[0017] Figure 2 is a two-dimensional drawing conceptually illustrating the structure of the impregnating material of the present invention.
[0018] Figure 3 is a schematic diagram for explaining the behavior of the impregnating agent and cosmetic composition in the present invention.
[0019] The present invention will be described in detail by explaining a preferred embodiment of the present invention with reference to the drawings below.
[0020] In the present invention, ether polyurethane foam includes a polyurethane foam processed into a foamed foam formed by reacting polyether polyol with a compound having an isocyanate (-NCO) group. In addition, ester polyurethane foam includes a polyurethane foam processed into a foamed foam formed by reacting polyester polyol with a compound having an isocyanate (-NCO) group. In addition, ether / ester polyurethane foam in the present invention includes a polyurethane foam processed into a foamed foam formed by reacting a mixture of polyether polyol and polyester polyol with a compound having an isocyanate (-NCO) group, or a polyurethane foam processed into a foamed foam formed by reacting a hybrid copolymer of polyether polyol and polyester polyol with a compound having an isocyanate (-NCO) group. In addition, the ether:ester ratio in the present invention means the molar ratio of ester groups and ether groups in the ether / ester polyurethane foam. For example, ether:ester = 1:9 means that the molar ratio of ether groups and ester groups in polyurethane is 1:9.
[0021] FIG. 1 is a schematic drawing of a cosmetic product according to one embodiment of the present invention.
[0022] As illustrated, the cosmetic (10) comprises a container body (11) for containing a liquid cosmetic. The container body (11) contains an impregnating agent (100) containing the liquid cosmetic. The cosmetic may include an inner lid (13) and / or an outer lid (15) for preventing leakage of the liquid cosmetic from the foam (100). In addition, although not illustrated, a fixing member for fixing the impregnating agent may be further provided to prevent the three-dimensional fabric impregnating agent from detaching. This will be described separately later.
[0023] In the present invention, the impregnating material (100) is preferably an ether-ester polyurethane foam. More preferably, the ether-ester polyurethane foam is an ether-ester polyurethane foam having a high ester ratio. Here, a high ester ratio means that the ratio of ester groups within the polyurethane is higher than half, and for example, the ether:ester ratio is preferably 1:9 to 3:7.
[0024] For example, the ether:ester ratio may be 1:9 to 1.5:8.5, 1:9 to 2:8, 1:9 to 2.5:7.5, 2:8 to 3:7, or 2.5:7.5 to 3:7. Although there are some literatures that disclose mixing polyether polyol and polyester polyol in polyurethane foam, there is no literature published that studies the properties or confirms the effects of polyurethane foam in which polyester polyol, which is known to be vulnerable to hydrolysis resistance in the past, is used in a higher ratio than polyether polyol among the raw materials, as in the present invention.
[0025] In the present invention, the discharge behavior of the cosmetic composition of the impregnated material impregnated with the liquid cosmetic can be explained as follows.
[0026] The impregnating material is a porous foam composed of cells or lattices as units. A single cell can be defined by a skeleton and pores within the skeleton. In the present invention, the skeleton of the cell is such that at least a portion or all of the cell walls constituting the unit lattice are perforated, and the pores of the skeleton are interconnected. This can be referred to as an open pore structure or a network structure.
[0027] Figure 2 is a two-dimensional conceptual diagram illustrating the structure of the impregnating material (20) of the present invention. The cells are composed of a skeleton (12) and internal pores (14) defined by the skeleton. In the drawing, the skeleton (12) is depicted as separating each cell, but when viewed three-dimensionally, the skeleton (12) of the cells has an open wall surface, and adjacent cells are connected to each other.
[0028] The discharge characteristics of the foam cosmetic of the present invention based on the cell structure of FIG. 2 are conceptually explained with reference to FIG. 3. However, the following description is merely supplementary to the understanding of the present invention and does not limit the technical idea of the present invention.
[0029] As illustrated in (a) of Fig. 3, the impregnating material (10) is impregnated with a liquid cosmetic composition (20). When the surface of the impregnating material (10) is pressed with a puff or a finger, stress is applied to the impregnating material (10) and the cosmetic composition (20). As illustrated in (b) of Fig. 3, the unit cells within the impregnating material are deformed by the pressurization, and the liquid cosmetic therebetween flows within the cells and between adjacent cells. At this time, the skeleton of the cells acts as resistance to the flow of the liquid cosmetic, and thus, part or all of the vertically downward pressing force acts as shear stress on the liquid cosmetic within the impregnating material.
[0030] Among polyurethane foams that constitute impregnating materials, foams using polyether polyol as a raw material have the advantages of excellent hydrolysis resistance, high elasticity, and low cost, but have the disadvantage of poor oil resistance. On the other hand, foams using polyester polyol have the advantages of easy bubble control and excellent wear and chemical resistance, but are known to have the disadvantages of being prone to hydrolysis and breaking when stored at high temperatures for long periods of time. The ether-ester polyurethane foam of the present invention can complement the disadvantages of single-composition polyether foam or polyester foam. Additionally, polyester polyurethane foam has the advantage of easy cell size control compared to polyether polyurethane, and can be advantageous in the production of polyurethane foams with smaller cell sizes.
[0031] In the foam of the present invention, the content (molar ratio) of ester groups in the polyurethane is higher than the content (molar ratio) of ether groups, and the molar ratio of ether:ester may preferably be in the range of 1:9 to 3:7. For example, the molar ratio of ether:ester in the present invention may be determined by the mixing ratio of polyether polyol and polyester polyol. That is, a polyurethane having an ether:ester ratio of 1.5:8.5 may be produced by mixing polyether polyol and polyester polyol at a ratio of 1.5:8.5.
[0032] In the present invention, the cell size within the polyurethane foam can be expressed by the number of pores. In the present invention, the number of pores may be from about 70 ppi to about 250 ppi, from about 80 ppi to about 250 ppi, from about 90 ppi to about 250 ppi, from about 100 ppi to about 250 ppi, from about 110 ppi to about 250 ppi, from about 120 ppi to about 250 ppi, or from about 150 ppi to about 250 ppi, but is not limited thereto. Preferably, the number of pores may be 110 ppi or less, 150 ppi or less, or 200 ppi or less.
[0033] The above pore count is defined as the number of pores present within a 1-inch long sample of foam. Specifically, the pore count can be measured according to a standard such as JIS K6400-1, as follows:
[0034] A specimen measuring 10 mm in thickness, 100 mm in width and length is collected, and the specimen is placed on a stand with a magnifying glass equipped with a scale of 5 to 10 times. The number of cells within a 10 mm straight line is counted while moving the magnifying glass or specimen. At this time, the measurement positions are set to 3 places, and the average value of the measurement values at the 3 places is used as the number of cells, which can be calculated according to the following mathematical formula 1.
[0035] (Equation 1)
[0036] N = n × 2.54 (where N is the number of cells (number / 25.4 mm) and n is the number of cells (average) between 10 mm)
[0037] The cell size can also be expressed as the pore size. In the present invention, the pore size may be, but is not limited to, about 0.1 mm to about 0.6 mm, about 0.15 mm to about 0.6 mm, about 0.20 mm to about 0.6 mm, about 0.25 mm to about 0.60 mm, or about 0.30 mm to about 0.60 mm. Preferably, the pore size in the present invention is 0.5 mm or less. For example, the pore size may be 0.1 mm to 0.5 mm, 0.2 mm to 0.5 mm, or 0.3 mm to 0.5 mm.
[0038] Furthermore, the present invention can utilize a foam in which the degree of deformation caused by pressurization is appropriately controlled. For example, in the present invention, the elastic modulus or hardness of the polyurethane foam can be appropriately controlled. For example, the hardness of the foam can be adjusted by controlling the molecular weight of the polyol participating in the urethane reaction.
[0039] In the present invention, the hardness of the polyurethane foam may be in the range of about 40 to about 90, about 50 to about 90, about 60 to about 90, about 70 to about 90, about 80 to about 90, about 40 to about 80, about 50 to about 80, about 60 to about 80, about 70 to about 80, about 40 to about 70, about 50 to about 70, about 60 to about 70, about 40 to about 60, or about 50 to about 60, based on the ASKER hardness tester Type F before impregnation with the cosmetic composition, but is not limited thereto.
[0040] In addition, the hardness of the polyurethane foam in the present invention may be in the range of about 50 to about 65, about 50 to 63, about 50 to 60, about 50 to 58, about 50 to 55, about 53 to about 65, about 53 to about 60, about 55 to about 65, about 55 to about 63, about 55 to about 60, about 58 to about 65, about 58 to about 60, about 60 to about 65, or about 60 to about 63, based on the hardness after impregnation with the cosmetic composition, but is not limited thereto.
[0041] When impregnating a cosmetic composition into an impregnating agent, the hardness typically decreases after impregnation. However, if the difference in hardness before and after impregnation is too great, designing the cosmetic composition to be impregnated into the impregnating agent becomes difficult, and the impregnation may have a negative impact on the user experience of the cosmetic. The inventors of the present invention discovered that the rate of decrease in hardness before and after impregnation varies depending on the composition of the impregnating agent. They continued their research into a polyurethane foam that minimizes the difference in hardness before and after impregnation with a cosmetic composition while still maintaining excellent user experience and effectiveness, and completed the present invention.
[0042] The polyurethane foam of the present invention exhibits a less significant decrease in hardness before and after impregnation than conventional foams, which exhibit an Asker hardness of approximately 70 to 90 before impregnation and approximately 40 to 45 after impregnation based on Type F. Accordingly, the polyurethane foam of the present invention exhibits a higher hardness after impregnation than other polyurethane foams available on the market, thereby providing a high-hardness impregnating material that provides a dense and firm feel.
[0043] In the present invention, the reduction rate of the hardness of the polyurethane foam after impregnation compared to the hardness before impregnation with the cosmetic ((hardness before impregnation - hardness after impregnation) / hardness before impregnation) may be less than 50%, preferably 45% or less, and more preferably 30% or less. In addition, it may be 29% or less, 28% or less, 27% or less, or 26% or less, and may be 24% or more, 25% or more, 26% or more, or 27% or more. When the reduction rate is 50% or more, the swelling of the impregnating material after impregnation may be excessively large, which may affect the physical properties of the impregnating material and may not be good for the usability.
[0044] Furthermore, it was experimentally confirmed that the polyurethane foam of the present invention was evaluated as being significantly higher than cosmetics containing other polyol ratios in terms of the "feel of use" of the cosmetic, which is one of the important sensory characteristics when using cosmetics containing polyurethane foam as an impregnating agent, as can be confirmed in the experimental examples described below. This is because, after impregnation with a cosmetic composition, a polyurethane foam having a hardness of about 50 to about 65 was judged to be the softest when the impregnated cosmetic composition was taken using an applicator, and the amount of the cosmetic composition taken on the applicator was determined to be appropriate.
[0045] In the present invention, polyurethane foam can be manufactured by reacting a mixture of polyether polyol and polyester polyol with a compound having an isocyanate (-NCO) group.
[0046] The monomer of the polyether polyol comprises a monomer selected from the group consisting of an alkylene oxide, a diol, a triol, or combinations thereof; the monomer of the polyester polyol may comprise an organic acid having two or more carboxyl groups, but is not limited thereto. In one embodiment of the present invention, the monomer of the polyether polyol comprises an alkylene oxide selected from the group consisting of ethylene oxide and propylene oxide; a diol selected from the group consisting of dipropylene glycol (hereinafter also referred to as "DPG"), monoethylene glycol (hereinafter also referred to as "MEG"), and propylene glycol (hereinafter also referred to as "PG"); or a triol selected from the group consisting of glycerin and trimethylol propane (hereinafter also referred to as "TMP"). Or combinations thereof may be included, but are not limited thereto. In one embodiment of the present invention, the polyether polyol includes, but is not limited to, one obtained by addition polymerizing an alkylene oxide, such as propylene oxide or ethylene oxide, to an initiator having activated hydrogen.The above initiator is mainly used, but is not limited to, two-functional groups such as propylene glycol, dipropylene glycol, ethylene glycol, diethylene glycol, diethanol amine, bisphenol, water, etc., or three-functional groups such as glycerine, trimethylol propane, triethanol amine, haxanetriol, etc.
[0047] In the present invention, the monomer of the polyester polyol includes a polyvalent organic acid having 2 or more carboxyl groups and having about 2 to about 20 carbon atoms, and may include, for example, a higher fatty acid, a saturated fatty acid, or an unsaturated fatty acid, but is not limited thereto. For example, the carbon atoms of the polyvalent organic acid may be about 2 to about 20, about 2 to about 18, about 2 to about 16, about 2 to about 14, about 2 to about 12, about 2 to about 10, about 2 to about 8, about 2 to about 6, or about 2 to about 4. In one embodiment of the present invention, the polyvalent organic acid having 2 or more carboxyl groups may include, for example, one selected from the group consisting of adipic acid, oxalic acid, and succinic acid, but is not limited thereto. In one embodiment of the present invention, the monomer of the polyester polyol may include, but is not limited to, one selected from the group consisting of soybean oil, castor oil, citric acid, palmitic acid, myristic acid, oleic acid, stearic acid, linoleic acid, and linolenic acid.
[0048] In the present invention, the compound having the isocyanate (-NCO) group includes, but is not limited to, a group consisting of polyisocyanates having two or more isocyanate groups, such as aromatic, alicyclic, and aliphatic polyisocyanates, combinations of two or more of the above polyisocyanates, and modified polyisocyanates obtained by modifying them. In one embodiment of the present invention, the compound having the isocyanate (-NCO) group is selected from the group consisting of aromatic diisocyanates such as methylene diphenyl diisocyanate (hereinafter also referred to as "MDI"), toluene diisocyanate (hereinafter also referred to as "TDI"), 2,4- or 2,6-tolylene diisocyanate, xylylene diisocyanate (XDI), paraphenylene diisocyanate, 1,5-naphthalene diisocyanate, and tridine diisocyanate; Aliphatic diisocyanates having aromatic rings such as α,α,α',α'-tetramethylxylylene diisocyanate; Aliphatic diisocyanates such as methylene diisocyanate, propylene diisocyanate, lysine diisocyanate, 2,2,4- or 2,4,4-trimethylhexamethylene diisocyanate, and 1,6-hexamethylene diisocyanate (HMDI); It may also be composed of alicyclic diisocyanates such as 1,4-cyclohexanediisocyanate, methylcyclohexanediisocyanate (hydrogenated TDI), 1-isocyanate-3-isocyanatemethyl-3,5,5-trimethylcyclohexane (IPDI), 4,4'-dicyclohexylmethanediisocyanate, isopropylidenedicyclohexyl-4,4'-diisocyanate, or combinations thereof, but is not limited thereto.
[0049] Hereinafter, the characteristics of a cosmetic composition suitable for impregnation into the ether-ester polyurethane foam of the present invention described above will be described.
[0050] To complement the hydrolysis properties of the polyurethane foam having the aforementioned high ester content, the cosmetic composition of the present invention has a low water content. Preferably, the water content of the cosmetic composition is 35 wt% or less, more preferably 30 wt% or less. For example, the water content of the cosmetic composition may be about 20 wt% or less, 10 wt% or less, 5 wt% or less, or 1 wt% or less of the cosmetic composition. Furthermore, it goes without saying that the cosmetic composition of the present invention may include anhydrous cosmetics.
[0051] The cosmetic composition of the present invention comprises an oil component, an aqueous component, a thickener, and a powder. These components and their contents determine the flow properties of the cosmetic composition.
[0052] The composition of the present invention may include 10 to 60 wt% of an oily component, 0.1 to 20 wt% of a thickener, and 30 to 70 wt% of a pigment based on the total cosmetic composition.
[0053] The oily component of the present invention includes oil, a sunscreen, and a dispersant, and includes at least one selected from the group consisting of butylene glycol dicaprylate / dicaprate, dimethicone, ethylhexyl methoxycinnamate, and polybutene. Preferably, the oily component may be included in an amount of 30 to 45 wt% based on the total composition.
[0054] The thickener controls the degree of thickening of the composition depending on the content range, and may include at least one selected from the group consisting of disteardimonium hectorite, hectorite, bentonite, vinyl dimethicone / methicone silsesquioxane crosspolymer, dextrin palmitate, dextrin palmitate / ethylhexanoate, dextrin myristate, stearoyl inulin, polyethylene, ceresin, ozokerite, microcrystalline wax, carnauba wax, and stearyl alcohol.
[0055] The present invention is characterized by including an organic thickener instead of a large amount of wax component, for example, the organic thickener is dextrin palmitate. Preferably, the organic thickener may be included in an amount of 2 to 3 wt% based on the total composition.
[0056] The thickener may contain a small amount of a wax component in addition to an organic thickener, for example, microcrystalline wax. The content range is preferably 1 to 2.5 wt% based on the total composition.
[0057] The pigment may be, but is not limited to, one or more selected from the group consisting of titanium dioxide, synthetic fluorphlogopite, yellow iron oxide, red iron oxide, and black iron oxide. Preferably, it includes titanium dioxide. Preferably, the pigment may be included in an amount of 46 to 52 wt% based on the total composition.
[0058] In addition, the cosmetic composition of the present invention includes a primary emulsifier and an auxiliary emulsifier, and the primary emulsifier and auxiliary emulsifier may be used in a weight ratio of 3:1 to 4:1. In the present invention, the total emulsifier may be used in an amount of 3 to 5 wt% based on the entire composition.
[0059] The above emulsifier comprises at least one substance selected from the group consisting of lauryl PEG-10 tris(trimethylsiloxy)silylethyl dimethicone, lauryl PEG-9 polydimethylsiloxyethyl dimethicone and cetyl PEG / PPG-10 / 1 dimethicone.
[0060] The above auxiliary emulsifier may be at least one of PEG-10 dimethicone and sorbitan isostearate.
[0061] In addition, in the present invention, the weight ratio of the aqueous component: oil component is preferably 1:1.85 or more, more preferably 1:5 or more, 1:20 or more, or 1:99 or more. If the ratio of the aqueous component increases beyond this, hydrolysis of the polyurethane foam may occur.
[0062] Hereinafter, preferred embodiments of the present invention will be described.
[0063] A. Polyurethane foam
[0064] Composite polyurethane foams were prepared by varying the ratio of polyester polyol to polyether polyol. For comparison, a 100% polyester polyol polyurethane foam was prepared. The prepared foams were cut into pieces measuring 5 cm in diameter and 10 mm in height, and their hardness (based on an ASKER hardness tester Type F) was measured.
[0065] The composition and hardness of each polyurethane foam are shown in Table 1 below.
[0066] Classification Ether:Ester Ratio Hardness PU11: 985 PU22: 881 PU33: 778 PU44: 674 PU50: 1089
[0067] B. Cosmetic Composition
[0068] A non-aqueous cosmetic composition was prepared. The cosmetic composition was prepared by mixing the ingredients in Table 2 below.
[0069] Ingredients by weight %, oily ingredients: Butylene glycol dicaprylate / dicaprate 20, dimethicone 10, ethylhexyl methoxycinnamate 6, polybutene 10, thickener: microcrystalline wax 1, dextrin palmitate 1, pigment: titanium dioxide (CI 77891) 30, iron oxide 12, methyl methacrylate crosspolymer 10
[0070] C. Sensory Evaluation
[0071] After impregnating 15 g of the cosmetic composition in Table 2 into each manufactured polyurethane foam, the hardness of the foam was measured and shown in the table below.
[0072] Hardness reduction rate before and after impregnation (%) PU16325.88PU25927.16PU35726.92PU44933.78PU56823.60
[0073] Next, after impregnating each manufactured polyurethane foam (PU1, PU2, PU3, PU4, and PU5) with the cosmetic composition, a sensory evaluation was conducted on 20 women in their 20s and 30s who were talented in evaluating cosmetics. In this experiment, the five types of polyurethane foams used were all visually identical, and the sensory evaluation was conducted without any background information about the polyurethane foam to the subjects.
[0074] The sensory evaluation items were evaluated on three dimensions: feel, touch, and usability. Based on the 5-point scale, they were evaluated as 5 points (very good), 4 points (good), 3 points (average), 2 points (bad), and 1 point (very bad), and the average value was derived. The description of each sensory evaluation item is as follows.
[0075] 1) Dispensing feeling: When taking the cosmetic composition from the impregnating material to the applicator (general NBR puff), evaluate whether the amount dispensed is appropriate. If the amount dispensed at one time is too small, multiple applications are required, which may affect the durability of the impregnating material.
[0076] 2) Touch: Evaluate the sensory characteristics felt when the applicator touches the impregnated material.
[0077] 3) Feel: Evaluate the overall feel of use when taking the cosmetic composition impregnated with the applicator.
[0078] Classification PU1 (Example 1) PU2 (Example 2) PU3 (Example 3) PU4 (Comparative Example 1) PU5 (Comparative Example 2) Discharge 4.034.214.113.783.63 Touch 3.924.074.383.813.32 Feeling of use 4.474.394.663.913.25 Average 4.144.224.383.833.40
[0079] As shown in Table 4 above, the sensory properties of polyurethane foams PU1 to PU3 (Examples 1 to 3) according to the present invention were evaluated as superior to those of PU4 and PU5 (Comparative Examples 1 and 2). A notable item is the touch sensation, in which the touch sensation was significantly improved as the ester ratio increased from 1:9 (Example 1) to 3:7 (Example 3), but when the ester ratio increased to 4:6 or more (Comparative Example 1), the touch sensation was evaluated as low. In addition, the excellent effects of the examples were confirmed in terms of the discharge sensation and overall usability. From this, it can be seen that the polyurethane foam according to the present invention has high hardness even after impregnation, thereby providing a dense and solid usability while having an appropriate discharge amount and durability.
[0080] While the present invention has been described in detail through exemplary embodiments thereof, the above description is merely illustrative and not intended to limit the invention. It should be understood that various modifications and variations are possible within the scope of the appended claims and the spirit of the invention, and are construed as falling within the scope of the present invention.
[0081] The present invention can be applied to cosmetics.
Claims
1. In a cosmetic product comprising a polyurethane foam impregnated with a cosmetic composition, The polyurethane of the above polyurethane foam contains ether and ester groups in a molar ratio of 1:9 to 3:7, A cosmetic composition characterized in that the water content is 35 wt% or less.
2. In paragraph 1, A cosmetic composition characterized in that the water content of the cosmetic composition is 30 wt% or less.
3. In paragraph 1, A cosmetic composition characterized in that the water content of the cosmetic composition is 20 wt% or less.
4. In paragraph 1, A cosmetic composition characterized in that the water content of the cosmetic composition is 5 wt% or less.
5. In paragraph 1, A cosmetic composition characterized in that the weight ratio of the aqueous component: oil component of the cosmetic composition is 1:1.85 or more.
6. In paragraph 1, A cosmetic composition comprising a main emulsifier and an auxiliary emulsifier, wherein the main emulsifier and the auxiliary emulsifier are in a weight ratio of 3:1 to 4:
1.
7. In paragraph 6, A cosmetic product characterized in that the emulsifier comprises at least one substance selected from the group consisting of lauryl PEG-10 tris(trimethylsiloxy)silylethyl dimethicone, lauryl PEG-9 polydimethylsiloxyethyl dimethicone, and cetyl PEG / PPG-10 / 1 dimethicone.
8. In paragraph 6, A cosmetic product characterized in that the auxiliary emulsifier comprises at least one of PEG-10 dimethicone and sorbitan isostearate.
9. In paragraph 1, A cosmetic product characterized in that the hardness of the polyurethane foam after impregnation is 50 to 65.
10. In paragraph 1, A cosmetic product characterized in that the hardness reduction rate before and after impregnation is 30% or less based on the hardness before impregnation of the polyurethane foam.
Citation Information
Patent Citations
UV blocking cosmetic composition prepared by being impregnated in urethane foam
KR1020090100643A
Container for cosmetic composition comprising sponge for application
KR1020140004575A
Foam impregnate cosmetics
KR1020160106000A
Foamed material comprising polyetherester elastomer and other polymer and cosmetics comprising the same
KR1020170034239A
Health care system for companion animal
KR1020210130374A