Polishing composition for semiconductor process, and method for polishing substrate by using same
The polishing composition with specifically designed abrasive particles and additives addresses the challenges of high polishing rate and defect reduction in semiconductor processing, enhancing CMP efficiency and stability for complex semiconductor surfaces.
Patent Information
- Application Number
- PCT/KR2024/005675
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-28
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-31
AI Technical Summary
In semiconductor processing, existing chemical mechanical polishing (CMP) technologies face challenges in achieving a high polishing rate while minimizing defects and dishing or erosion, especially as semiconductor devices become more complex and denser.
A polishing composition with abrasive particles having a specific Rps value ratio of micropore to external specific surface area, controlled particle size distribution, and micropore characteristics is used, along with additives like nonionic polymers and chelating agents, to enhance polishing efficiency and reduce defect frequency.
The solution provides an excellent polishing rate with reduced defects and stable durability, effectively addressing the challenges of complex semiconductor surface structures and maintaining polishing efficiency.
Smart Images

Figure KR2024005675_31102024_PF_FP_ABST
Abstract
Description
Polishing composition for semiconductor process and method for polishing substrate using the same
[0001] [Cross-reference to related applications]
[0002] This application claims priority from Korean Patent Application No. 10-2023-0056015, filed April 28, 2023, the contents of which are incorporated herein by reference.
[0003] The implementation example relates to a polishing composition for a semiconductor process and a method for polishing a substrate using the same.
[0004]
[0005] As semiconductor devices become increasingly miniaturized and denser, increasingly finer patterning techniques are being employed. Consequently, their surface structures are becoming more complex, and the gaps between layers are becoming larger. Chemical Mechanical Polishing (CMP) is a planarization technique used to remove gaps in specific layers formed on substrates during semiconductor device manufacturing.
[0006] The CMP process involves applying slurry to a polishing pad, pressurizing and rotating the substrate, and polishing its surface. The target surface to be planarized varies depending on the process step, and the properties of the slurry applied also vary.
[0007] Polishing after metal wiring is formed requires maintaining sufficient polishing rate and polishing speed while minimizing dishing or erosion.
[0008] [Prior Art Literature]
[0009] [Patent Document]
[0010] (Patent Document 1) Domestic Publication Patent No. 10-2017-0021320
[0011] (Patent Document 2) Japanese Patent Publication No. H11-060232
[0012]
[0013] The purpose of the embodiment is to provide a polishing composition for semiconductor processes, which can exhibit an excellent polishing rate and implement a polished surface with reduced defects when applied to a CMP process.
[0014]
[0015] A polishing composition for a semiconductor process according to one embodiment of the present disclosure includes abrasive particles.
[0016] The Rps value, which is the ratio of the micropore surface area to the external surface area according to Equation 1 below of the above abrasive particles, is 0.5 to 2.
[0017] [Formula 1]
[0018]
[0019] In the above formula 1, Ap is the specific surface area of the micropores of the abrasive particles, and As is the external specific surface area of the abrasive particles.
[0020] The above Ap value is 25m 2 / g to 50m 2 / g may be.
[0021] The above As value is 10m 2 / g to 30m 2 / g may be.
[0022] The BET surface area of the above abrasive particles is 30 m 2 / g to 80m 2 / g may be.
[0023] The specific volume of the micropores of the above abrasive particles is 0.011 cm 3 / g to 0.2cm 3 / g may be.
[0024] The average diameter of the micropores of the above abrasive particles may be 15 nm to 40 nm.
[0025] The above abrasive particles may contain 10 wt% or less of secondary particles having a diameter of 120 nm or more.
[0026] The above abrasive particles may contain 10 wt% or less of secondary particles having a diameter of less than 50 nm.
[0027] The above polishing composition for semiconductor processing may contain 4 wt% to 12 wt% of the above polishing particles.
[0028] The above polishing composition for semiconductor processes may have a pH of 8 to 12.
[0029] A method for manufacturing a substrate according to another embodiment of the present specification includes a process of polishing a substrate by applying the above-described polishing composition for semiconductor processing as a slurry.
[0030] According to another embodiment of the present specification, the abrasive particles have an Rps value, which is a ratio of the micropore surface area to the external surface area according to Equation 1 below, of 0.5 to 2.
[0031] [Formula 1]
[0032]
[0033] In the above formula 1, Ap is the specific surface area of the micropores of the abrasive particles, and As is the external specific surface area of the abrasive particles.
[0034] The above Ap value is 25m 2 / g to 50m 2 / g may be.
[0035] The above As value is 10m 2 / g to 30m 2 / g may be.
[0036] The BET surface area of the above abrasive particles is 30 m 2 / g to 80m 2 / g may be.
[0037] The specific volume of the micropores of the above abrasive particles is 0.011 cm 3 / g to 0.2cm 3 / g can be less.
[0038] The average diameter of the micropores of the above abrasive particles may be 15 nm to 40 nm.
[0039] When the above-mentioned abrasive particles are added to ultrapure water, the above-mentioned abrasive particles may contain 10 wt% or less of secondary particles having a diameter of 120 nm or more.
[0040] When the above-mentioned abrasive particles are added to ultrapure water, the above-mentioned abrasive particles may contain 10 wt% or less of secondary particles having a diameter of less than 50 nm.
[0041]
[0042] The polishing composition for a semiconductor process of the embodiment can exhibit an excellent polishing rate when applied to a CMP process and can provide a polished surface with reduced defects.
[0043]
[0044] Figure 1 is a graph showing the diameter distribution of secondary particles of abrasive particles by manufacturing example.
[0045]
[0046] Hereinafter, embodiments will be described in detail so that those skilled in the art can easily implement the embodiments. However, the embodiments may be implemented in various different forms and are not limited to the embodiments described herein.
[0047] The terms "about," "substantially," and the like used in this specification are used in a sense of or near to the numerical value when manufacturing and material tolerances inherent to the meaning referred to are presented, and are used to prevent unscrupulous infringers from unfairly exploiting disclosures in which exact or absolute numerical values are mentioned to aid understanding of implementation examples.
[0048] Throughout this specification, the term "combination thereof" included in the expressions in the Makushi format means one or more mixtures or combinations selected from the group consisting of the components described in the expressions in the Makushi format, and means including one or more selected from the group consisting of said components.
[0049] Throughout this specification, references to “A and / or B” mean “A, B, or A and B.”
[0050] Throughout this specification, terms such as “first”, “second” or “A”, “B” are used to distinguish the same terms from each other unless otherwise specified.
[0051] In this specification, the meaning of B being positioned on A means that B may be positioned on A or that another layer may be positioned in between while B is positioned on A, and is not limited to being interpreted as B being positioned in contact with the surface of A.
[0052] In this specification, singular expressions are interpreted to include the singular or plural as interpreted in the context, unless otherwise specified.
[0053]
[0054] The inventors of the embodiment experimentally confirmed that when a semiconductor process polishing composition having controlled values such as the Rps value, which is the ratio of the specific surface area of micropores to the external specific surface area of polishing particles, is applied to CMP polishing, the polishing composition can effectively reduce the frequency of occurrence of defects on the polished surface while exhibiting an excellent polishing rate for the substrate to be polished, and completed the embodiment.
[0055]
[0056] Below, an implementation example is described in detail.
[0057]
[0058] Surface characteristics of abrasive particles
[0059] A polishing composition for a semiconductor process according to an embodiment comprises abrasive particles.
[0060] The Rps value, which is the ratio of the micropore surface area to the external surface area of the abrasive particle according to Equation 1 below, is 0.5 to 2.
[0061] [Formula 1]
[0062]
[0063] In the above formula 1, Ap is the specific surface area of the micropores of the abrasive particles, and As is the external specific surface area of the abrasive particles.
[0064] Micropore refers to a pore with a diameter of less than 2 nm.
[0065] The embodiment can control the degree of irregularity of the shape of the abrasive particles by controlling the Rps value of the abrasive particles, and can provide a certain level of roughness or higher to the surface of the abrasive particles. Abrasive particles having such characteristics can have a wider contact area with the surface to be polished when polishing pressure is applied in the CMP process compared to spherical particles having a smooth surface, and thus can exhibit a superior polishing rate for the surface to be polished. In addition, the degree of micropores formed on the surface of the abrasive particles can be controlled, thereby stably controlling the durability of the abrasive particles. This can effectively reduce the frequency of defects on the surface to be polished resulting from abrasive particles damaged during polishing.
[0066] The method for measuring the Rps value of abrasive particles is as follows.
[0067] Abrasive particles are degassed at 250°C for 3 hours. The degassed abrasive particles are fed into a surface area measuring device, and the amount of nitrogen adsorbed on the abrasive particles is measured while increasing the relative pressure (p / p°) from 0 to 1.0 at 77.3K, and the amount of nitrogen desorbed from the abrasive particles is measured while decreasing the relative pressure from 1.0 to 0, thereby obtaining a nitrogen adsorption / desorption isotherm of the abrasive particles. The specific surface area of the abrasive particles is calculated from the nitrogen adsorption / desorption isotherm by the BET (Brunauer-Emmett-Teller) method, and that value is used as the BET specific surface area of the abrasive particles.
[0068] The above p is the equilibrium pressure of nitrogen gas, and the above p° is the saturation pressure of nitrogen gas.
[0069] A t-plot is generated from the nitrogen adsorption / desorption isotherm according to the Harkins-Jura equation, and the external specific surface area As value of the abrasive particle is calculated. Then, the value obtained by subtracting the As value from the BET specific surface area value of the abrasive particle is used as the Ap value.
[0070] The Rps value is calculated by dividing the Ap value by the As value.
[0071] As an example of a surface area measuring device, the TriStar II 3020 model from Micromeritics can be applied.
[0072] The Rps value of the abrasive particles may be 0.5 to 2. The Rps value may be 0.7 or more. The Rps value may be 0.9 or more. The Rps value may be 1.8 or less. The Rps value may be 1.5 or less. In such cases, the polishing rate of the polishing composition for the substrate to be polished can be improved, while effectively suppressing the occurrence of defects derived from the abrasive particles.
[0073] The above Ap value is 25m 2 / g to 50m 2 / g may be. The above Ap value is 26m 2 / g or more. The above Ap value is 27m 2 / g or more. The above Ap value is 40m 2 / g or less. The above Ap value is 35m 2 / g or less. The above Ap value is 32m 2 / g or less. In this case, the polishing efficiency of the polishing composition can be increased by providing an appropriate roughness to the surface of the polishing particles.
[0074] The above As value is 10m 2 / g to 30m 2 / g may be. The above As value is 15m 2 / g or more. The above As value is 20m 2 / g or more. The above As value is 22m2 / g or more. The above As value is 28m 2 / g or less. The above As value is 26m 2 / g or less. In this case, the polishing composition can help to have both improved polishing rate and stable durability.
[0075] The specific surface area of an abrasive particle can influence not only its shape but also its size. Specifically, the specific surface area of an abrasive particle tends to increase as the particle size decreases. The embodiment can simultaneously control the particle size distribution and shape of an abrasive particle within an appropriate range by adjusting the values of parameters related to the specific surface area of the abrasive particle.
[0076] The BET surface area of the above abrasive particles is 30 m 2 / g to 80m 2 / g can be. The BET specific surface area is 40 m 2 / g or more. The BET specific surface area is 45 m 2 / g or more. The BET specific surface area is 48 m 2 / g or more. The BET specific surface area is 70 m 2 / g or less. The BET specific surface area is 65 m 2 / g or less. The BET specific surface area is 60 m 2 / g can be less.
[0077] In this case, the polishing properties of the polishing composition can be effectively improved while reducing the frequency of defect occurrence caused by small-diameter abrasive particles adsorbing on the polishing surface.
[0078] The embodiment can control the structural characteristics of micropores within abrasive particles. Abrasive particles with these characteristics can have stable durability despite having an irregular shape.
[0079] The specific volume of the micropores of the abrasive particles is 0.011 cm 3 / g to 0.2cm3 / g may be. The above specific volume is 0.012cm 3 / g or more. The above specific volume is 0.15cm 3 / g or less. The above specific volume is 0.1cm 3 / g or less. The above specific volume is 0.05cm 3 / g or less. The above specific volume is 0.03cm 3 / g or less. The above specific volume is 0.02cm 3 / g or less. In this case, damage to the abrasive particles due to polishing pressure can be suppressed, and defects caused by particles derived from the abrasive particles being adsorbed on the polished surface can be suppressed.
[0080] The average diameter of the micropores of the abrasive particles may be 15 nm to 40 nm. The average diameter may be 18 nm or more. The average diameter may be 20 nm or more. The average diameter may be 35 nm or less. The average diameter may be 30 nm or less. The average diameter may be 28 nm or less. In this case, the abrasive particles are less likely to be broken by external force and may have a more stable structure.
[0081] The specific volume and average diameter of micropores are measured using a surface area measuring device. The specific measurement conditions applied to the measurement of the specific volume and average diameter of micropores are identical to those applied to the BET surface area measurement.
[0082]
[0083] Particle size distribution of abrasive particles
[0084] The abrasive particles may contain up to 10 wt% of secondary particles having a diameter of 120 nm or more. The abrasive particles may contain up to 8 wt% of secondary particles having a diameter of 120 nm or more. The abrasive particles may contain up to 0.1 wt% of secondary particles having a diameter of 120 nm or more. In this case, the formation of scratches on the polishing surface by secondary particles having a large diameter during the polishing process can be effectively suppressed.
[0085] The abrasive particles may contain up to 10 wt% of secondary particles having a diameter of less than 50 nm. The abrasive particles may contain up to 8 wt% of secondary particles having a diameter of less than 50 nm. The abrasive particles may contain at least 0.1 wt% of secondary particles having a diameter of less than 50 nm. In such cases, the frequency of relatively small-sized particles among the abrasive particles being adsorbed on the surface to be polished due to interaction with the surface to be polished can be effectively reduced.
[0086] D of secondary particles of abrasive particles 50 can be 40 nm or more. The above D 50 can be 45 nm or more. The above D 50 can be 50 nm or more. The above D 50 can be 55 nm or more. The above D 50 may be less than 100 nm. The above D 50 may be less than 95 nm. The above D 50 may be less than 90 nm. The above D 50 may be less than 85 nm. The above D 50 The size may be 80 nm or less. In this case, it is possible to impart excellent polishing properties to the polishing composition while stably controlling the occurrence of defects on the polished surface.
[0087] The diameter of the secondary particles of abrasive particles is measured using Dynamic Light Scattering (DLS). For example, the diameter of the secondary particles of abrasive particles was measured using a particle size analyzer, the Zetasizer nano-ZS model from Malvern Panalytical.
[0088] D of the primary particles of abrasive particles 50 can be 15 nm or more. The above D 50 can be 20 nm or more. The above D 50 can be 25 nm or more. The above D 50 may be less than 55 nm. The above D 50 may be less than 50 nm. The above D 50 The size may be 45 nm or less. In this case, the polishing composition can exhibit excellent polishing properties while stably reducing the frequency of defects caused by the adsorption of the polishing particles onto the surface to be polished.
[0089] The diameter of the primary particles of the abrasive is measured using a transmission electron microscope (TEM).
[0090] The degree of aggregation of the abrasive particles may be 3 or less. The degree of aggregation may be 2.8 or less. The degree of aggregation may be 2.5 or less. The degree of aggregation may be 2.3 or less. The degree of aggregation may be 1.1 or more. The degree of aggregation may be 1.5 or more. In such cases, the polishing composition may exhibit stable reproducibility of polishing properties and polishing rate.
[0091] The agglomeration of abrasive particles is measured using a method commonly applied in the field of CMP slurries.
[0092]
[0093] Composition of abrasive particles
[0094] The abrasive particles may include metal oxide particles. The abrasive particles may include silica. The abrasive particles may include colloidal silica.
[0095] The abrasive particles may contain at least 70 wt% colloidal silica. The abrasive particles may contain at least 80 wt% colloidal silica. The abrasive particles may contain at least 90 wt% colloidal silica. The abrasive particles may be colloidal silica.
[0096] The abrasive particles may contain up to 1000 ppb (by weight) of an alkali metal. The abrasive particles may contain up to 800 ppb (by weight) of an alkali metal. The abrasive particles may contain up to 600 ppb (by weight) of an alkali metal. The abrasive particles may contain up to 400 ppb (by weight) of an alkali metal. The abrasive particles may contain more than 50 ppb (by weight) of an alkali metal.
[0097] The abrasive particles may contain no more than 500 parts per billion (ppb) of a heavy metal (by weight). The abrasive particles may contain no more than 400 ppb (ppb) of a heavy metal (by weight). The abrasive particles may contain no more than 300 ppb (ppb) of a heavy metal (by weight). The abrasive particles may contain no more than 200 ppb (ppb) of a heavy metal (by weight). The abrasive particles may contain more than 10 ppb (ppb) of a heavy metal (by weight).
[0098] In this case, when polishing a substrate to be polished with exposed wiring, it is possible to effectively prevent metallic impurities from being absorbed or remaining on the polishing surface, thereby causing electrical defects such as poor circuit insulation or wiring short-circuits.
[0099]
[0100] Composition and properties of polishing compositions for semiconductor processes
[0101] A polishing composition for semiconductor processing may contain 4 to 12 wt% of abrasive particles. The polishing composition for semiconductor processing may contain 6 wt% or more of abrasive particles. The polishing composition for semiconductor processing may contain 10 wt% or less of abrasive particles. Such a polishing composition may help reduce the frequency of defect occurrence during the polishing process while ensuring that the abrasive particles are stably dispersed within the composition.
[0102] Polishing compositions for semiconductor processes may further include additives. The additives are not limited to those commonly used in the CMP field. For example, the additives may include at least one of a nonionic polymer, a chelating agent, an oxidizing agent, an acid component, a pH regulator, a dispersant, a polishing rate enhancer, a polishing regulator, a polishing pad protector, and a preservative.
[0103] A polishing composition for semiconductor processing can further improve the dispersibility of abrasive particles within the polishing composition by further including a nonionic polymer. Specifically, the nonionic polymer contained in the polishing composition can be adsorbed onto the abrasive particles, thereby increasing the dispersibility of the abrasive particles. Furthermore, the nonionic polymer not adsorbed onto the abrasive particles can further enhance the dispersion stability of the abrasive particles by exhibiting steric hindrance effects, etc. In particular, the nonionic polymer allows the polishing composition for semiconductor processing to have more stable dispersion stability even in an acidic environment. This nonionic polymer can reduce the occurrence of polishing-induced defects on the substrate during the polishing process.
[0104] The above nonionic polymer may be at least one selected from the group consisting of polyethylene glycol, polypropylene glycol, polyvinylpyrrolidone, polyethylene oxide, polypropylene oxide, polyalkyl oxide, polyoxyethylene oxide, polyethylene oxide-propylene oxide copolymer, cellulose, methylcellulose, methylhydroxyethylcellulose, methylhydroxypropylcellulose, hydroxyethylcellulose, carboxymethylcellulose, carboxymethylhydroxyethylcellulose, sulfoethylcellulose, and carboxymethylsulfoethylcellulose.
[0105] The nonionic polymer may have a weight average molecular weight of less than 25,000 g / mol. The weight average molecular weight may be greater than or equal to 1,000 g / mol and less than 25,000 g / mol. In this case, the nonionic polymer may exhibit excellent solubility and further improve the dispersion stability of the abrasive particles.
[0106] The polishing composition for semiconductor processing may contain 0.01 wt% to 5 wt% of a nonionic polymer. The polishing composition for semiconductor processing may contain 0.1 wt% or more of a nonionic polymer. The polishing composition for semiconductor processing may contain 2 wt% or less of a nonionic polymer. In such cases, it may help reduce the frequency of occurrence of defects on the surface of a polishing target substrate after polishing, and may suppress contamination such as re-attachment of particles to the surface.
[0107] A polishing composition for semiconductor processing may further include a chelating agent. Metals or metal ions removed from the substrate surface during the polishing process are highly likely to reattach to the substrate surface or remain there, forming defects. In particular, metals such as tungsten can readily dissolve in the polishing composition under certain conditions, but may also readily adhere to the surface to be polished. The chelating agent adsorbs to these metals or metal ions, facilitating their removal. This can further enhance the polishing rate of the polishing composition and effectively suppress the formation of defects on the substrate surface due to particle reattachment.
[0108] By way of example, the chelating agent may be at least one selected from the group consisting of butyric acid, citric acid, tartaric acid, succinic acid, oxalic acid, acetic acid, adipic acid, capric acid, caproic acid, caprylic acid, carboxylic acid, glutaric acid, glutamic acid, glycolic acid, thioglycolic acid, formic acid, mandelic acid, fumaric acid, lactic acid, lauric acid, malic acid, maleic acid, malonic acid, myristic acid, flammic acid, phthalic acid, isophthalic acid, terephthalic acid, citraconic acid, propionic acid, pyruvic acid, stearic acid, valeric acid, benzoic acid, phenylacetic acid, naphthoic acid, aspartic acid, amino acids, and ethylenediaminetetraacetic acid.
[0109] The amino acids that can be used include glycine, α-alanine, β-alanine, L-aspartic acid, N-methylglycine (methylglycine), and combinations thereof.
[0110] The chelating agent may contain two or more carboxyl groups or alcohol groups in the molecule. Two or more chelating agents containing two or more carboxyl groups or alcohol groups in the molecule may be used. Specifically, the chelating agent may include any one selected from the group consisting of EDTA (ethylenediaminetetraacetic acid), glycine, carboxylic acids, and combinations thereof. The carboxylic acids refer to compounds containing at least one or two carboxyl groups in the molecule.
[0111] The polishing composition for semiconductor processing may contain 0.003 wt% to 0.5 wt% of a chelating agent. The polishing composition for semiconductor processing may contain 0.005 wt% or more of a chelating agent. The polishing composition for semiconductor processing may contain 0.3 wt% or less of a chelating agent. In such cases, the polishing rate of the polishing composition can be controlled to an appropriate level, and the frequency of occurrence of surface defects on the substrate can be reduced.
[0112] Polishing compositions for semiconductor processing may further include an oxidizing agent. The oxidizing agent oxidizes metals such as tungsten, creating an environment that facilitates planarization of the substrate surface, and enhances polishing and etching rates.
[0113] The oxidizing agent may be at least one selected from the group consisting of hydrogen peroxide, urea peroxide, urea, percarbonate, periodic acid, periodate, perchloric acid, perchlorate, perbromic acid, perbromate, perboric acid, perborate, permanganic acid, permanganate, persulfate, bromate, chlorate, chlorite, chromate, iodate, iodic acid, ammonium peroxysulfate, benzoyl peroxide, calcium peroxide, barium peroxide, sodium peroxide, and urea peroxide.
[0114] A polishing composition for semiconductor processing may contain 0.01 wt% to 5 wt% of an oxidizing agent. In this case, the composition may exhibit excellent polishing properties for metals and may suppress the formation of an oxide film on the metal to be polished during the polishing process.
[0115] The polishing composition for semiconductor processes may further include a copper corrosion inhibitor. The copper corrosion inhibitor may include an azole compound.
[0116] The azole compound may include, for example, one selected from the group consisting of benzotriazole (BTA), 5-methyl-1H-benzotriazole (5-MBTA), 3-amino-1,2,4-triazole, 5-phenyl-1H-tetrazole, 3-amino-5-methyl-4H-1,2,4-triazole, 5-aminotetrazole (ATZ), 1,2,4-triazole, tolytriazole, and combinations thereof.
[0117] The azole compound may include one selected from the group consisting of 5-aminotetrazole (ATZ), 5-methyl-1H-benzotriazole (5-MBTA), and combinations thereof.
[0118] Azole compounds can act on the copper surface during the polishing process to prevent copper corrosion.
[0119] The above azole compound may be included in an amount of 0.02 to 2.00 parts by weight, 0.03 to 1.5 parts by weight, or 0.5 to 1.5 parts by weight based on 100 parts by weight of the abrasive particles.
[0120] When the azole compound is included in this range, a corrosion prevention effect on the copper surface of the composition for semiconductor processes can be obtained, and in particular, a strong corrosion prevention effect can be provided on a relatively wide surface such as a via hole surface.
[0121] The polishing composition for semiconductor processes may further include an acid component. The acid component may be, for example, at least one selected from the group consisting of hydrochloric acid, phosphoric acid, sulfuric acid, hydrofluoric acid, hydrobromic acid, iodic acid, formic acid, malonic acid, maleic acid, oxalic acid, acetic acid, adipic acid, citric acid, adipic acid, acetic acid, propionic acid, fumaric acid, lactic acid, salicylic acid, pimeline, benzoic acid, succinic acid, phthalic acid, butyric acid, glutaric acid, glutamic acid, glycolic acid, lactic acid, aspartic acid, tartaric acid, and salts thereof.
[0122] The polishing composition for semiconductor processes may further include a pH adjuster along with the acid component. The pH adjuster may be, for example, any one selected from the group consisting of ammonia, aminomethylpropanol, tetramethylammonium hydroxide, potassium hydroxide, sodium hydroxide, magnesium hydroxide, rubidium hydroxide, cesium hydroxide, sodium bicarbonate, sodium carbonate, imidazole, and combinations thereof.
[0123] The polishing composition for semiconductor processing may further include a dispersant.
[0124] Dispersants can prevent agglomeration of abrasive particles within a polishing composition and uniformly disperse them. Cationic dispersants can positively increase the zeta potential of the polishing composition, and anionic dispersants can negatively decrease the zeta potential of the polishing composition.
[0125] The dispersant may include anionic low-molecular weight polymers, cationic high-molecular weight polymers, organic acids, etc.
[0126] The anionic low molecular weight dispersant may be at least one selected from oxalic acid, citric acid, polysulfonic acid, polyacrylic acid, polymethacrylic acid, and combinations thereof.
[0127] The cationic polymer of the dispersant may be at least one selected from polylysine, polyethyleneimine, benzethonium chloride, bronidox, cetrimonium bromide, cetrimonium chloride, dimethyldioctadecyl ammonium chloride, tetramethylammonium hydroxide, distearyldimethyl ammonium chloride, polyaryl amine, and combinations thereof.
[0128] The organic acid of the dispersant may be at least one selected from hydroxylbenzoic acid, ascorbic acid, picolinic acid, glutamic acid, tryptophan, aminobutyric acid, and combinations thereof.
[0129] The polishing rate improver is an additive for increasing the polishing rate of a substrate or wiring to be polished, and may be at least one selected from potassium nitrate, iron nitrate, ammonium hydroxide, citric acid, acetic acid, and combinations thereof.
[0130] The polishing conditioner is intended to minimize the adsorption of the polishing composition onto the metal surface, and may include ammonium compounds, potassium nitrate, amino acids, salts thereof, etc.
[0131] The polishing composition for semiconductor processing may include a solvent. The solvent may be water, and specifically, ultrapure water.
[0132] The pH of the polishing composition for semiconductor processing may be 8 to 12. The pH may be 9 or higher. The pH may be 11 or lower. In such cases, the dispersibility of the abrasive particles and polymers contained in the polishing composition can be stably controlled. In addition, it can contribute to effectively suppressing the occurrence of defects on the polished surface due to the adsorption of the abrasive particles.
[0133] The zeta potential of the polishing composition for semiconductor processes may be -80 mV to -20 mV. The zeta potential value may be -75 mV or higher. The zeta potential value may be -70 mV or higher. The zeta potential value may be -65 mV or higher. The zeta potential value may be -60 mV or higher. The zeta potential value may be -25 mV or lower. The zeta potential value may be -30 mV or lower. The zeta potential value may be -35 mV or lower. The zeta potential value may be -40 mV or lower. In such cases, the abrasive particles can be stably dispersed within the polishing composition. In addition, the frequency of occurrence of defects such as scratches on the surface to be polished due to the abrasive particles can be effectively reduced.
[0134] The zeta potential value of the above polishing composition is measured using a zeta potential measuring device.
[0135]
[0136] Polishing properties of polishing compositions for semiconductor processes
[0137] The polishing rate of the polishing composition for a semiconductor process for a silicon oxide film may be 1350 Å / min or more. The polishing rate may be 1450 Å / min or more. The polishing rate may be 1550 Å / min or more. The polishing rate may be 1650 Å / min or more. The polishing rate may be 3500 Å / min or less. The polishing rate may be 3000 Å / min or less. The polishing rate may be 2500 Å / min or less.
[0138] PI according to the following formula 2-1 of the polishing composition for semiconductor processes S The value can be greater than 200Å / (min·wt%).
[0139] [Formula 2-1]
[0140]
[0141] In the above equation 2-1, the P Sis the polishing rate [unit: Å / min] of the polishing composition for semiconductor processes on the silicon oxide film.
[0142] The above C is the content of abrasive particles in the polishing composition for semiconductor processes [unit: wt%].
[0143] The above PI S The value may be 200Å / (min·wt%) or more. The above PI S The value may be 210Å / (min·wt%) or more. The above PI S The value may be 220Å / (min·wt%) or more. The above PI S The value may be less than 300Å / (min·wt%).
[0144] The polishing rate for a barrier film containing tantalum and tantalum nitride of a polishing composition for semiconductor processing may be 780 Å / min or more. The polishing rate may be 800 Å / min or more. The polishing rate may be 830 Å / min or more. The polishing rate may be 1200 Å / min or less.
[0145] PI according to the following formula 2-2 of the polishing composition for semiconductor processes T The value can be greater than 200Å / (min·wt%).
[0146] [Formula 2-2]
[0147]
[0148] In the above equation 2-2, the P T is the polishing rate [unit: Å / min] for a barrier film containing tantalum and tantalum nitride of a polishing composition for semiconductor processes.
[0149] The above C is the content of abrasive particles in the polishing composition for semiconductor processes [unit: wt%].
[0150] The above PI T The value may be 80Å / (min ·wt%) or more. The above PI S The value may be 85Å / (min·wt%) or more. The above PI SThe value may be 90Å / (min·wt%) or more. The above PI S The value may be 95Å / (min·wt%) or more. The above PI S The value may be 100Å / (min·wt%) or more. The above PI S The value may be less than 200Å / (min·wt%).
[0151] The polishing rate of the polishing composition for a semiconductor process for a copper film may be 850 Å / min or more. The polishing rate may be 900 Å / min or more. The polishing rate may be 950 Å / min or more. The polishing rate may be 1000 Å / min or more. The polishing rate may be 1050 Å / min or more. The polishing rate may be 1100 Å / min or more. The polishing rate may be 2500 Å / min or less.
[0152] PI according to the following formula 2-3 of the polishing composition for semiconductor processes C The value can be greater than 100Å / (min·wt%).
[0153] [Formula 2-3]
[0154]
[0155] In the above equation 2-3, the P C is the polishing rate of a copper film of a polishing composition for semiconductor processes [unit: Å / min].
[0156] The above C is the abrasive particle content [unit: wt%] in the polishing composition for semiconductor processes.
[0157] The above PI C The value may be 110Å / (min·wt%) or more. The above PI C The value may be 120Å / (min·wt%) or more. The above PI C The value may be 130Å / (min·wt%) or more. The above PI C The value may be 140Å / (min·wt%) or more. The above PI C The value may be less than or equal to 250Å / (min·wt%). The above PIC The value may be less than 200Å / (min·wt%).
[0158] In such cases, the polishing composition can exhibit excellent polishing rates on a polishing target substrate in which wiring, an oxide film, and a barrier film are exposed together.
[0159] The polishing rate for each film is measured under the conditions of a pressure of 2.2 psi, a carrier speed of 87 rpm, a platen speed of 93 rpm, and a slurry flow rate of 250 ml / min.
[0160] When measuring the polishing rate for each thin film, the polishing machine can be applied, for example, the AP-300 model from CTS.
[0161]
[0162] Method for manufacturing polishing composition for semiconductor process
[0163] A method for manufacturing a polishing composition for a semiconductor process according to an embodiment includes a polishing particle forming step of preparing polishing particles and a manufacturing step of preparing a polishing composition for a semiconductor process including the polishing particles.
[0164] The abrasive particle formation step may include a preparatory process of preparing a first abrasive particle preparation composition and a second abrasive particle preparation composition, and a reaction process of obtaining abrasive particles from a reaction solution in which the first abrasive particle preparation composition and the second abrasive particle preparation composition are mixed.
[0165] In the preparation process, the first polishing particle composition may include an organic silicon compound and a first organic solvent.
[0166] The organic silicon compound may be an alkoxy silane compound. Examples of the organic silicon compound that can be used include tetraethoxysilane (TEOS) and tetramethoxysilane (TMOS).
[0167] Examples of the first organic solvent that can be used include ethanol, methanol, and isopropyl alcohol.
[0168] The first abrasive particle composition may contain 20 to 50 parts by weight of the organic silicon compound relative to 100 parts by weight of the first organic solvent. The first abrasive particle composition may contain 25 parts by weight or more of the organic silicon compound relative to 100 parts by weight of the first organic solvent. The first abrasive particle composition may contain 45 parts by weight or less of the organic silicon compound relative to 100 parts by weight of the first organic solvent.
[0169] The first polishing particle composition can be prepared by mixing an organic silicon compound with a first organic solvent in a double-jacket reactor. However, the method for preparing the first polishing particle composition is not limited thereto.
[0170] The second polishing particle composition may include water, a catalyst, and a second organic solvent.
[0171] The second polishing particle composition may contain 1 to 15 parts by weight of water relative to 100 parts by weight of the second organic solvent. The second polishing particle composition may contain 3 parts by weight or more of water relative to 100 parts by weight of the second organic solvent. The second polishing particle composition may contain 10 parts by weight or less of water relative to 100 parts by weight of the second organic solvent.
[0172] The catalyst can participate in the hydrolysis and polymerization reactions of organic silicon compounds during the reaction process, thereby contributing to controlling the shape and particle size distribution of the abrasive particles.
[0173] The catalyst may be at least one of potassium hydroxide, sodium hydroxide, ammonia, TMAH (Tetramethylammonium Hydroxide), and TEA (triethanolamine).
[0174] The second polishing particle composition may contain 0.5 parts by weight or more of the catalyst relative to 100 parts by weight of the second organic solvent. The second polishing particle composition may contain 1 part by weight or more of the catalyst relative to 100 parts by weight of the second organic solvent. The second polishing particle composition may contain 10 parts by weight or less of the catalyst relative to 100 parts by weight of the second organic solvent. The second polishing particle composition may contain 7 parts by weight or less of the catalyst relative to 100 parts by weight of the second organic solvent.
[0175] Examples of the second organic solvent that can be used include ethanol, methanol, isopropyl alcohol, etc. The second organic solvent may be the same compound as the first organic solvent.
[0176] During the reaction process, a reaction solution can be prepared by mixing the first abrasive particle-preparing composition and the second abrasive particle-preparing composition. To prepare the reaction solution, the second abrasive particle-preparing composition can be added to the first abrasive particle-preparing composition, and the first abrasive particle-preparing composition can be added to the second abrasive particle-preparing composition. Specifically, the first abrasive particle-preparing composition can be added to the second abrasive particle-preparing composition.
[0177] During the reaction process, abrasive particles can be obtained through hydrolysis and polymerization of an organic silicon compound. In an embodiment, the shape characteristics and particle size distribution, including the micropore distribution, of the obtained abrasive particles can be controlled within a predetermined range by controlling the content of each component in the reaction solution, the reaction temperature, etc.
[0178] In the reaction process, the reaction solution may contain 60 to 120 parts by weight of the composition for producing second polishing particles relative to 100 parts by weight of the composition for producing first polishing particles. The reaction solution may contain 65 parts by weight or more of the composition for producing second polishing particles relative to 100 parts by weight of the composition for producing first polishing particles. The reaction solution may contain 70 parts by weight or more of the composition for producing second polishing particles relative to 100 parts by weight of the composition for producing first polishing particles. The reaction solution may contain 100 parts by weight or less of the composition for producing second polishing particles relative to 100 parts by weight of the composition for producing first polishing particles.
[0179] The reaction solution may contain 3 parts by weight or more of water per 100 parts by weight of the organic silicon compound. The reaction solution may contain 5 parts by weight or more of water per 100 parts by weight of the organic silicon compound. The reaction solution may contain 10 parts by weight or more of water per 100 parts by weight of the organic silicon compound. The reaction solution may contain 50 parts by weight or less of water per 100 parts by weight of the organic silicon compound. The reaction solution may contain 30 parts by weight or less of water per 100 parts by weight of the organic silicon compound. The reaction solution may contain 20 parts by weight or less of water per 100 parts by weight of the organic silicon compound.
[0180] The reaction solution may contain 1 part by weight or more of the catalyst per 100 parts by weight of the organosilicon compound. The reaction solution may contain 3 parts by weight or more of the catalyst per 100 parts by weight of the organosilicon compound. The reaction solution may contain 4 parts by weight or more of the catalyst per 100 parts by weight of the organosilicon compound. The reaction solution may contain 20 parts by weight or less of the catalyst per 100 parts by weight of the organosilicon compound. The reaction solution may contain 15 parts by weight or less of the catalyst per 100 parts by weight of the organosilicon compound. The reaction solution may contain 13 parts by weight or less of the catalyst per 100 parts by weight of the organosilicon compound.
[0181] In this case, abrasive particles having the desired shape characteristics and particle size distribution can be obtained in the embodiment.
[0182] During the reaction process, the reaction temperature can be set to 20°C to 60°C. The reaction temperature can be 30°C or higher. The reaction temperature can be 40°C or higher. The reaction temperature can be 55°C or lower. In these cases, it can help the synthesis of the abrasive particles proceed smoothly.
[0183] During the reaction process, the reaction time may be between 2 and 10 hours. The reaction time may be 3 hours or more. The reaction time may be 4 hours or more. The reaction time may be 8 hours or less. The reaction time may be 7 hours or less. In such cases, the abrasive particles may contribute to having the desired size and shape in the embodiment.
[0184] Abrasive particles can be prepared by reacting a silicate precursor with an alkoxysilane precursor.
[0185] Descriptions of the surface properties, diameter distribution, composition, etc. of the abrasive particles are omitted as they overlap with the previous content.
[0186] In the manufacturing stage, a polishing composition for semiconductor processing can be prepared by mixing abrasive particles and a solvent. The polishing composition for semiconductor processing can further include additives along with the abrasive particles and solvent after purification.
[0187] Description of the composition and properties of the polishing composition for semiconductor processes is omitted as it overlaps with the previous content.
[0188]
[0189] Method for manufacturing substrate
[0190] The method for manufacturing a substrate of the embodiment includes a process of polishing a substrate by applying a polishing composition for semiconductor processing as a slurry.
[0191] The substrate may include at least one of an insulating film, a metal wiring, and a barrier layer on its upper surface. The metal wiring may include copper or tungsten. When the metal wiring includes copper, the barrier layer may include tantalum and its nitride. When the metal wiring includes tungsten, the barrier layer may include titanium and its nitride.
[0192] Specifically, the process of polishing a substrate can be performed by bringing the substrate, which is a target of polishing, into contact with a polishing composition for semiconductor processes supplied from a spray nozzle, onto a polishing pad, while a polishing head that fixes the substrate rotates and a platen to which the polishing pad is attached also rotates.
[0193] The process of polishing the substrate may further include a process of conditioning the polishing pad surface prior to polishing, if necessary.
[0194] The polishing composition for semiconductor processing can polish a wafer that comes into contact with a polishing pad while penetrating toward the substrate.
[0195] During the process of polishing the substrate, a pressure of 6.89 kPa to 48.26 kPa may be applied. The pressure may be 13.79 kPa to 34.47 kPa.
[0196] The process of polishing the substrate can be carried out for 50 seconds to 10 minutes, but this can be varied depending on the desired degree of polishing.
[0197] Description of the above polishing composition for semiconductor processes is omitted as it overlaps with the previous content.
[0198] The method for manufacturing a substrate may further include a cleaning process for cleaning the polished substrate.
[0199] The above cleaning process can be performed by cleaning the polished substrate using purified water and an inert gas.
[0200]
[0201] abrasive particles
[0202] The abrasive particles according to the embodiment have an Rps value, which is the ratio of the micropore surface area to the external surface area according to Equation 1 below, of 0.5 to 2.
[0203] [Formula 1]
[0204]
[0205] In the above formula 1, Ap is the specific surface area of the micropores of the abrasive particles, and As is the external specific surface area of the abrasive particles.
[0206] The above Ap value is 25m 2 / g to 50m 2 / g may be.
[0207] The above As value is 10m 2 / g to 30m 2 / g may be.
[0208] The BET surface area of the above abrasive particles is 30 m 2 / g to 80m 2 / g may be.
[0209] The specific volume of the micropores of the above abrasive particles is 0.011 cm 3 / g to 0.2cm 3 / g can be less.
[0210]
[0211] The average diameter of the micropores of the above abrasive particles may be 15 nm to 40 nm.
[0212] When the above-mentioned abrasive particles are added to ultrapure water, the above-mentioned abrasive particles may contain 10 wt% or less of secondary particles having a diameter of 120 nm or more.
[0213] When the above-mentioned abrasive particles are added to ultrapure water, the above-mentioned abrasive particles may contain 10 wt% or less of secondary particles having a diameter of less than 50 nm.
[0214] The above abrasive particles are identical to the abrasive particles described above. Descriptions of the surface properties, particle size distribution, composition, and manufacturing method of the above abrasive particles overlap with the above content and are therefore omitted.
[0215]
[0216] Hereinafter, specific examples will be described in more detail. The following examples are merely illustrative to aid understanding of the present invention and are not intended to limit the scope of the present invention.
[0217]
[0218] Manufacturing example: Manufacturing of abrasive particles
[0219] Manufacturing Example 1: In a first double jacket reactor, 41 parts by weight of a first organic solvent and 15 parts by weight of an organic silicon compound were mixed to prepare a first composition for preparing abrasive particles, totaling 56 parts by weight. In a second double jacket reactor, 1 part by weight of a catalyst and 2 parts by weight of water were added to 41 parts by weight of a second organic solvent, totaling 44 parts by weight of a second composition for preparing abrasive particles. The temperature of the second double jacket reactor was set to 45°C, and the first composition for preparing abrasive particles was added to the second composition for preparing abrasive particles, and hydrolysis and polymerization reactions were performed for 5 hours to obtain abrasive particles.
[0220] Tetraethoxysilane (TEOS) was used as the organic silicon compound, ethanol and isopropyl alcohol were used as the first and second organic solvents, respectively, and ammonia was used as the catalyst.
[0221] Manufacturing Example 2: Abrasive particles were manufactured under the same conditions as Manufacturing Example 1, except that 4.5 parts by weight of an organic silicon compound and 45.75 parts by weight of a first organic solvent were applied in the composition for manufacturing the first abrasive particle, and 3 parts by weight of water and 45.75 parts by weight of a second organic solvent were applied in the composition for manufacturing the second abrasive particle.
[0222] Manufacturing Example 3: Abrasive particles were manufactured under the same conditions as Manufacturing Example 1, except that 4.5 parts by weight of an organic silicon compound and 43.25 parts by weight of a first organic solvent were applied in the composition for manufacturing the first abrasive particle, and 8 parts by weight of water and 43.25 parts by weight of a second organic solvent were applied in the composition for manufacturing the second abrasive particle.
[0223]
[0224] The process conditions for each manufacturing example are listed in Table 1 below.
[0225]
[0226] Manufacturing example: Manufacturing of polishing composition
[0227] Example 1: 8 wt% of the polishing particles according to Manufacturing Example 1, 0.4 wt% of citric acid, 0.2 wt% of benzotriazole, 0.2 wt% of polyethylene glycol, and 0.2 wt% of hydrogen peroxide were added and mixed in ultrapure water as a solvent to prepare a polishing composition having a total weight of 100 wt%.
[0228] Comparative Example 1: A polishing composition was prepared under the same conditions as Example 1, except that 16 wt% of the polishing particles according to Manufacturing Example 2 were applied as polishing particles to prepare a polishing composition with a total content of 100 wt%.
[0229] Comparative Example 2: A polishing composition was prepared under the same conditions as Example 1, except that 8 wt% of the polishing particles according to Manufacturing Example 2 were applied as polishing particles to prepare a polishing composition with a total content of 100 wt%.
[0230] Comparative Example 3: A polishing composition was prepared under the same conditions as Example 1, except that 8 wt% of the polishing particles according to Manufacturing Example 3 were applied as polishing particles to prepare a polishing composition with a total content of 100 wt%.
[0231] Abrasive particle content in the abrasive composition of each example and comparative example, D of the secondary particles of the abrasive particles 50 , zeta potential, and pH were applied as described in Table 1 below.
[0232]
[0233] Evaluation example: Measurement of surface properties of abrasive particles
[0234] The Ap value, As value, BET specific surface area value, specific volume of micropores, and average diameter of micropores of each abrasive particle were measured using a surface area layer measuring device, TriStar II 3020 from Micromeritics.
[0235] During measurement, the abrasive particles were degassed at 250°C for 3 hours, and then the degassed abrasive particles were placed in a surface area measuring device, and the amount of nitrogen adsorbed on the abrasive particles was measured while increasing the relative pressure (p / p°) from 0 to 1.0 at 77.3 K, and the amount of nitrogen desorbed from the abrasive particles was measured while decreasing the relative pressure from 1.0 to 0, thereby obtaining a nitrogen adsorption isotherm and a nitrogen desorption isotherm of the abrasive particles. From the nitrogen adsorption / desorption isotherm, the Ap value, the As value, the BET specific surface area value, the specific volume of micropores, and the average diameter of micropores were calculated, and the Rps value was calculated from the Ap value and the As value.
[0236]
[0237] The measurement and calculation results for each manufacturing example are listed in Table 2 below.
[0238]
[0239] Evaluation example: Measurement of secondary particle size distribution of abrasive particles
[0240] The secondary particle size distribution of the abrasive particles for each manufacturing example was measured using a particle size analyzer, the Zetasizer nano-ZS model from Malvern Panalytical.
[0241]
[0242] The measurement results for each manufacturing example are shown in Table 3 below and Figure 1.
[0243]
[0244] Evaluation example: Measurement of polishing rate
[0245] The polishing compositions for each example and comparative example were applied as slurry, and the polishing rates for each silicon oxide film, a barrier film including tantalum and tantalum nitride, and a copper film formed on a wafer with a diameter of 300 mm were measured. The polishing rates for each film were measured under the conditions of a polishing time of 60 seconds, a pressure of 2.2 psi, a carrier speed of 93 rpm, a platen speed of 87 rpm, and a slurry flow rate of 300 ml / min, and the polishing machine used was the AP-300 model from CTS.
[0246] Afterwards, PI according to the above formula 2-1 is calculated from the measured polishing rate value. S Value, PI according to the above formula 2-2 T Value, PI according to the above formula 2-3 C The value was calculated.
[0247]
[0248] The measured and calculated values for each example and comparative example are listed in Table 4 below.
[0249]
[0250] Evaluation example: Measurement of roughness of polished surface
[0251] The polishing compositions for each example and comparative example were applied as slurry and the polishing rate for copper films on wafers with a diameter of 300 mm was measured. The polishing rate for each film was measured under the conditions of a polishing time of 60 seconds, a pressure of 2.2 psi, a carrier speed of 93 rpm, a platen speed of 87 rpm, and a slurry flow rate of 300 ml / min, and the polishing machine used was the AP-300 model from CTS.
[0252]
[0253] Afterwards, the arithmetic mean roughness (Ra) according to ISO 4287 of the copper film surface polished using the polishing composition for each example and comparative example was measured using an atomic force microscope, Park XE-100 model from Park systems.
[0254]
[0255] The measurement values for each example and comparative example are listed in Table 5 below.
[0256]
[0257] Evaluation example: Measurement of the frequency of defect occurrence on the polished surface
[0258] The polishing compositions for each example and comparative example were applied as slurry to polish the surface of a SiO2 wafer. The polishing conditions were the same as those applied in the previous polishing rate measurement evaluation.
[0259] The number of defects formed on the polished SiO2 wafer surface was measured using a wafer defect detector, the AIT-XP+ model from KLA Tencor.
[0260] Thereafter, the polishing compositions for each example and comparative example were applied as slurry to polish the surface of the SiO2 wafer on which the copper pattern was formed. The measurement conditions were the same as those applied to the previous polishing rate measurement evaluation.
[0261] The number of defects formed on the surface of the polished pattern wafer was measured using a wafer defect detector, the AIT-XP+ model from KLA Tencor.
[0262]
[0263] The measurement results for each example and comparative example are listed in Table 5 below.
[0264]
[0265] Evaluation Example: Dissing Evaluation of Copper Wiring
[0266] The polishing compositions for each example and comparative example were applied as slurry to polish a first pattern wafer having a diameter of 300 mm. The first pattern wafer has a barrier film including tantalum and tantalum nitride having a thickness of 160 nm formed on a SiO2 film having a copper pattern having a width of 1 μm. The polishing conditions were the same as those applied to the previous polishing rate measurement evaluation. The dishing value of the copper wiring was measured using AFM at the center portion located at the center of the polished substrate surface, the edge portion located at the edge of the substrate surface, and the middle portion located at the center of the straight line connecting the center of the center portion and the center of the edge portion.
[0267] Thereafter, the polishing compositions for each example and comparative example were applied as slurry to polish a second pattern wafer. The second pattern wafer was formed by forming a barrier film containing tantalum and tantalum nitride with a thickness of 400 nm on a SiO2 film on which a copper pattern with a width of 10 μm was formed. The polishing conditions were the same as those applied to the previous polishing rate measurement evaluation. The dishing value of the copper wiring from the polished substrate surface was measured using AFM.
[0268]
[0269] The measurement results for each example and comparative example are listed in Table 6 below.
[0270]
[0271] Composition for manufacturing abrasive particles of the first type Composition for manufacturing abrasive particles of the second type Reaction temperature (℃ Reaction time (hour) TEOS (parts by weight) Ethanol (parts by weight) Water (parts by weight) Ammonia (parts by weight) Isopropyl alcohol (parts by weight) Manufacturing example 1 1 5 4 1 2 1 4 1 4 5 ...
[0272] Abrasive particle content (wt%)D 50 (nm)Zeta potential(mV)pHExample 1876-4810.4Comparative Example 11680-5510.4Comparative Example 2880-5510.5Comparative Example 3885-5410.4
[0273] RpsAp(m 2 / g)As(m 2 / g)BET specific surface area (m 2 / g) Micropore volume (cm) 3 / g) Average micropore diameter (nm) Manufacturing example 11.156628.260324.434952.69520.013624.8160 Manufacturing example 20.25619.345936.496245.84210.004413.7418 Manufacturing example 30.299724.255480.9398105.19520.010310.2189
[0274] Secondary particle diameter (nm) Intensity Manufacturing example 1 Manufacturing example 2 Manufacturing example 30.40000.4630000.5360000.6210000.7190000.8330000.9650001.120001.290001.50001.740002.010002.330002.70003.120003.620004.190004.850005.6100 06.50007.530008.7200010.100011.700013.500015.700018.20002100024.400028.200032.700037.81.630043.85.740050.711.11.921.8958.815.89.237.9368 .118.318.115.478.817.723.420.791.314.422.521.41069.51617.51224.67.510.71421.211.384.13164000.3241900002200002550002950003420003960004590 00531000615000712000825000955000111000012800001480000172000019900002300000267000030900003580000415000048000005560000644000074600008630000
[0275] Polishing rate (Å / min) for silicon oxide film PI S (Å / (min·wt%)) Polishing rate for barrier film (Å / min) PI T (Å / (min·wt%)) Polishing rate for copper film (Å / min)PI C (Å / (min·wt%))Example 11899237.38858107.251178147.25Comparative Example 11834114.62575847.375136485.25Comparative Example 21321165.12555269831103.875Comparative Example 31602200.25851106.3751624203
[0276] Ra value of copper film after polishing (Å) Number of defects on SiO2 wafer surface after polishing (number) Number of defects on pattern wafer surface after polishing (number) Example 13.73611473 Comparative example 15.9913431581 Comparative example 26.39877598 Comparative example 34.8212461105
[0277] Center sectionMiddle sectionEdge sectionDissing value of 1㎛ wide copper wire (Å)Dissing value of 10㎛ wide copper wire (Å)Dissing value of 1㎛ wide copper wire (Å)Dissing value of 10㎛ wide copper wire (Å)Dissing value of 1㎛ wide copper wire (Å)Dissing value of 10㎛ wide copper wire (Å)Example 13326371468Comparative example 17379441673Comparative example 25298321356Comparative example 393910512491
[0278] In Table 5 above, Example 1 has a higher PI than the comparative examples. S Values and PI T The values were shown. This is thought to be because the irregular shape of the abrasive particles of Example 1 contributes to improving the polishing rate of the polishing composition. In Table 6, Example 1 showed a lower Ra value than the comparative examples. This means that when polishing a copper film, Example 1 can form a smoother polished surface than the comparative examples.
[0279] In terms of the number of defects on the surface of the SiO2 wafer and the number of defects on the surface of the patterned wafer after polishing, Example 1 showed a lower number of defects than the comparative examples.
[0280] This is thought to be because Example 1 has a smaller content of abrasive particles with a large diameter than other comparative examples, and thus the frequency of scratches on the polished surface caused by the abrasive particles is lower.
[0281] In particular, it is thought that the reason Example 1 shows a significantly lower number of defects than Comparative Example 1 is because the polishing composition of Example 1 contains a lower content of abrasive particles than Comparative Example 1.
[0282] In the copper wiring dishing evaluation of Table 7, Example 1 showed a dishing value similar to or lower than that of the comparative examples.
[0283]
[0284] Although the preferred embodiments have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concepts of the implementation examples defined in the following claims also fall within the scope of the present invention.
Claims
1. Contains abrasive particles, A polishing composition for semiconductor processing, wherein the Rps value, which is the ratio of the external specific surface area of the above-mentioned polishing particles to the specific surface area of the micropores according to Equation 1 below, is 0.5 to 2; [Formula 1] In the above equation 1, The above Ap is the specific surface area of the micropores of the abrasive particles, The above As is the external specific surface area of the abrasive particles.
2. In paragraph 1, The above Ap value is 25m 2 / g to 50m 2 / g, polishing composition for semiconductor process.
3. In paragraph 1, The above As value is 10m 2 / g to 30m 2 / g, polishing composition for semiconductor process.
4. In paragraph 1, The BET surface area of the above abrasive particles is 30 m 2 / g to 80m 2 / g, polishing composition for semiconductor processes 5. In paragraph 1, The specific volume of the micropores of the above abrasive particles is 0.011 cm 3 / g to 0.2cm 3 / g, polishing composition for semiconductor process.
6. In paragraph 1, A polishing composition for semiconductor processing, wherein the average diameter of the micropores of the above-mentioned polishing particles is 15 nm to 40 nm.
7. In paragraph 1, A polishing composition for semiconductor processing, wherein the above-mentioned polishing particles contain 10 wt% or less of secondary particles having a diameter of 120 nm or more.
8. In paragraph 1, A polishing composition for semiconductor processing, wherein the above-mentioned polishing particles contain 10 wt% or less of secondary particles having a diameter of less than 50 nm.
9. In paragraph 1, A polishing composition for semiconductor processing, comprising 4 to 12 wt% of the above-mentioned abrasive particles.
10. In paragraph 1, A polishing composition for semiconductor processes having a pH of 8 to 12.
11. A method for manufacturing a substrate, comprising a process of polishing a substrate by applying a semiconductor process polishing composition according to Article 1 as a slurry.
12. Abrasive particles having an Rps value, which is the ratio of the micropore surface area to the external surface area according to Equation 1 below, of 0.5 to 2; [Formula 1] In the above formula 1, Ap is the specific surface area of the micropores of the abrasive particles, and As is the external specific surface area of the abrasive particles.
13. In paragraph 12, The above Ap value is 25m 2 / g to 50m 2 / g, abrasive particles.
14. In paragraph 12, The above As value is 10m 2 / g to 30m 2 / g, abrasive particles.
15. In paragraph 12, BET surface area is 30m 2 / g to 80m 2 / g, abrasive particles.
16. In paragraph 12, The specific volume of the above micropores is 0.011 cm 3 / g to 0.2cm 3 / g, abrasive particles.
17. In paragraph 12, Abrasive particles having an average diameter of the above micropores of 15 nm to 40 nm.
Citation Information
Patent Citations
JP1989060232U
Colloidal silica chemical-mechanical polishing composition
KR1020170021320A
Abrasive grain and method for producing the same, polishing tool and method for producing the same, grindstone for polishing and method for producing the same and polishing apparatus
JP2003105324A
Silica sol and manufacturing method therefor
JP2005060217A