Method to form composite particles and articles made therefrom
The method of embedding inorganic powders within thermoplastic polymer powders addresses the challenges of residual stresses and additive incorporation in additive manufacturing, enabling the production of 3D printable articles with improved electrostatic dissipation and thermal conductivity for diverse applications.
Patent Information
- Application Number
- PCT/US2024/026155
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-04-26
- Filing Date
- 2024-04-25
- Publication Date
- 2024-10-31
AI Technical Summary
Current powder-based additive manufacturing methods face challenges with residual stresses, limited polymer options, and difficulties in incorporating electrostatic dissipative additives without compromising printability and properties, especially in forming complex or large parts.
A method to form composite thermoplastic polymer powders by embedding inorganic powders within thermoplastic polymer powders, allowing for improved flowability and electrostatic dissipation characteristics without melting, enabling the production of 3D printable articles with induced crystallinity that reverts to amorphous state upon heating and cooling.
This method allows for the creation of 3D printable articles with enhanced electrostatic dissipation and thermal conductivity, using lower solid loading of electrostatic dissipative additives, and maintaining desired particle morphology and size distribution, suitable for various applications including medical, electrical, and aerospace industries.
Smart Images

Figure IMGF000008_0001 
Figure IMGF000011_0001 
Figure IMGF000011_0002
Abstract
Description
METHOD TO FORM COMPOSITE PARTICLES AND ARTICLES MADE THEREFROMFIELD
[0001] The invention is directed to thermoplastic polymer particles useful for forming articles by additive manufacturing and in particular polymeric articles that are antistatic, static dissipative or conductive.BACKGROUND
[0002] Powder-based methods of additive manufacturing include the following. Selective laser sintering (SLS) is a 3D-printing technique that uses a laser to fuse powder material in successive layers (see, for example, U.S. Pat. No. 5,597,589). High-speed sintering (HSS) and multi-jet fusion (MJF) 3D-printing employ multiple jets that similarly deposit successive layers of infrared-absorbing (IR-absorbing) ink onto powder material, followed by exposure to IR energy for selective melting of the powder layer. Electrophotographic 3D-printing employs a rotating photoconductor that builds the object layer-by-layer from the base.
[0003] Selective laser sintering (SLS), multi-jet fusion (MJF), and high-speed sintering (HSS) 3D-printing methods use the same type of free-floating, non-fixed powder bed. They generally have the same material requirements for compatibility with the printing process since the additively built object will experience similar stresses, only with different heating mechanisms to obtain the melt phase. Typically, a free-body diagram of a 3D printed object can be used to determine the residual stresses expected in the printed object. This is necessary for successfully building the object. If the residual stress is too high, the object will deform or be deformed beyond acceptable tolerances.
[0004] The residual stresses have typically been minimized for these powder bed-based 3D printers by using crystalline or semicrystalline thermoplastic polymers having sufficiently large window between its melting temperature and its recrystallization temperature. Unfortunately, this has limited the polymers that have successfully used to print large or complex parts using SLS and MJF methods (e.g., polyamides), thus limiting the use of these additive manufacturing methods. Likewise, the use of semi-crystallinepolymers upon recrystallization after heating to make the additive manufactured article may limit the article's properties.
[0005] The thermoplastic powder needs to be deposited in successive layers requiring a good flowability to minimize defects in and between layers due to gaps arising from uneven spread of particles within a layer. Commonly, the powder has been made by melt compounding desired additives with a semicrystalline thermoplastic polymer such a polyamides that are subsequently cryogenically ground to a desired size. Unfortunately, these powders tend to angular with inadequate dry powder flow further requiring flow additives.
[0006] Production of particles that are more spherical without such angularities have been described for applications such as toner particles using emulsification methods but these have required the melting of the thermoplastic polymer, see for example U.S. Pat. No. 4,863,646 and WO 94 / 06059. Precipitation of thermoplastic polymers to form more spherical particles has also been described and to induce crystallinity in amorphous thermoplastic polymer such as polycarbonate, for example, U.S. Pat. No. 3,214,407 and 4,853,462; U.S. Pat. Publ. No. 2021 / 0277180, and PCT Pub. No. WO 2017 / 033146. These methods, however, do not lend themselves to the incorporation of particulate additives that may be useful to realize desirable characteristics such as electrostatic dissipation and melting to compound such additives inevitably results in distributions throughout the particle requiring excessive loading that may be deleterious to printing and the melting to compound such particles in amorphous thermoplastic polymers having induced crystallinity will cause them to revert to amorphous particles rendering them 3D unprintable.
[0007] Accordingly, it would be desirable to provide a method to produce a thermoplastic polymer powder that is 3D printable that avoids one or more of the problems of the prior art. Likewise, it would be desirable to provide a thermoplastic polymer powder having low solids loading of electrostatic dissipative additives, desired particle size and morphology, for producing articles employing powder bed additive manufacturing methods, including, for example, SLS methods employing a fiber laser requiring a minimalamount of absorption of the laser energy to be operative. It would also be desirable to provide electrostatic dissipative amorphous thermoplastic polymer additive manufactured articles.SUMMARY
[0008] Applicants have discovered a method to incorporate desirable particulate additives to thermoplastic polymer powders useful for additive manufacturing without further attriting the particles. The method may also improve the flowability (impart further desired morphology or size distribution) of the thermoplastic polymer powder as well as impart desirable characteristics such as electrostatic dissipation using less additives to impart such characteristics by conventional methods and other desirable characteristics such as electromagnetic shielding and increased thermal conductivity. The method enables the incorporation of solid particulates in the absence of melting (e.g. compounding) allowing the formation of thermoplastic polymer powders with induced crystallinity that then can revert to amorphous thermoplastic polymers upon heating and cooling in methods such as floating powder bed additive manufacturing methods. Such behavior may be determined by differential scanning calorimetry as described below.
[0009] The crystallinity may be determined by any suitable methods such as those known in the art. Illustratively, the percent crystallinity may be determined by x-ray diffraction including, for example, wide angle x-ray diffraction (WAXD), such as by using a Rigaku SmartLab x-ray diffractometer, or by differential scanning calorimetry (DSC), such as by using a TA Instruments DSC250 differential scanning calorimeter (ASTM D3418 - 15). The onset of the Tg, Tm and Tc peaks likewise are determined as per ASTM D3418 (i.e., deviation of the scan from linear) and unless otherwise stated herein any of these temperatures are to be understood to mean the onset temperatures. It is understood that amorphous means that the polymer essentially fails to display crystallinity in X-ray diffraction pattern or fails to display a melt peak in DSC. Herein, DSC is run at a heating and cooling rate of 20°C / min unless otherwise specified.
[0010] Illustratively a method to form a composite powder comprises contacting a thermoplastic polymer powder and an inorganic powder having an average primary particle size of less than 10 micrometers and the thermoplastic polymer powder having an average particle size of 10 micrometers to 100 micrometers, the thermoplastic polymer powder / inorganic powder having a weight ratio 8 to 100, to form a mixture and shearing the mixture in a vessel for a shear time and shear rate sufficient to form the composite powder having the inorganic powder embedded in the thermoplastic polymer powder, wherein the composite powder, generally, has an average particle size that is within 25% percent of the thermoplastic polymer powder average size.
[0011] The composite particles may be used to make articles by heating the composite particle to a temperature sufficient to melt and bond the polymer particles. The method is particularly useful for forming an article by additive manufacturing methods such as floating powder bed methods (e.g., SLS, HSS and MJF methods). The additive manufactured articles may have electrostatic dissipative properties at inorganic solids loading substantially less than conventionally possible by compounding such additives into the thermoplastic polymers and cryogrinding to form particles that are then ground to form powders.
[0012] In an embodiment, a composite powder is comprised of a thermoplastic polymer powder having an average particle size of 20 to 100 micrometers equivalent spherical diameter and a D90 of at most 300 micrometers and a Dio of at least 1 micrometer and from 0.05% to 5% by weight of an inorganic particulate having an average primary particle size of at most 2 micrometers that is embedded in the thermoplastic powder at its surface. Embedded in the thermoplastic powder's surface means that the particles essentially (at least 95%, 98% or 99% to all of the particles by volume) reside within the outer volume of the composite particles. Outer volume means the volume that is defined by the % (midpoint) of the radius to the full length of the radius (surface) of the composite powder particles having a particle size ranging from 40 micrometers to 60 micrometers equivalent spherical diameter.
[0013] The composite thermoplastic polymer particles may be made into additive manufactured articles that take advantage of the properties of the wide range of engineering plastics. Examples of the applications the articles may be useful for include: biocompatible (medical), electrical, transportation (e.g., automotive, rail, trucking), plumbing, aerospace, food contact, industrial (e.g., machinery) and consumer (e.g., appliances) applications.DETAILED DESCRIPTION
[0014] The explanations and illustrations presented herein are intended to acquaint others skilled in the art with the invention, its principles, and its practical application. The specific embodiments of the present disclosure as set forth are not intended to be exhaustive or limit the scope of the disclosure.
[0015] One or more as used herein means that at least one, or more than one, of the recited components may be used as disclosed. It is understood that the functionality of any ingredient or component may be an average functionality due to imperfections in raw materials, incomplete conversion of the reactants and formation of by-products.
[0016] The method to make the composite particles starting with a thermoplastic powder having a particle size and size distribution that is suitable for powder bed 3D printing method. The thermoplastic polymer powder may be formed by any suitable method such as those known in the art. Exemplary methods may include emulsion methods, precipitation methods and grinding methods such as those known in the art and previously described.
[0017] The method is particularly useful to make composite thermoplastic polymer powders where the thermoplastic polymer is one that displays essentially no crystallinity when heated and cooled under conventional plastic heating rates (e.g., 1 to 200 °C / min, with 20 °C / min being a common rate when assessing the melt behavior of thermoplastic polymers by differential scanning calorimetry "DSC") when forming articles above the melt temperature of the polymer melt temperature when such polymer has induced crystallinity. Inorganic powders, surprisingly, may be incorporated, by the method intosuch amorphous polymers having induced crystallinity without causing the polymer to revert to being amorphous allowing them to be 3D printed. The thermoplastic polymer may be a homopolymer or a copolymer. Desirably, the thermoplastic polymer is comprised of a thermoplastic polymer having induced crystallinity.
[0018] The thermoplastic polymer of the thermoplastic polymer powder may be any that is useful for making additive manufactured articles. Desirably, the thermoplastic polymer is one that forms desirable properties such as those commonly referred to as an engineering plastic. Exemplary thermoplastic polymer may include those that have a repeating unit comprised of one or more of a carbonyl, sulfur dioxide, and sulfone group. The carbonyl group may be a part of a carbonate, ester, amide, or imide in the thermoplastic polymer. The thermoplastic polymer may have one or more other repeating units such as an ether. Examples of useful thermoplastic polymers include polyamides, polycarbonates, thermoplastic polyurethane, polyketones, polysulfones, polyarylates, polyolefin (e.g., polyethylene, polypropylene and combinations thereof) and polyimides and combinations thereof. The thermoplastic polymer may be linear or branched. The thermoplastic polymer may be aliphatic or aromatic with it desirable for the polymer to have at least a portion of said polymer comprised of repeating aromatic units within the polymer backbone, where it generally is desirable for at least about 50% by mole of the polymer to be aromatic (i.e., aromatic groups make up 50% or more of the molar mass of the polymer).
[0019] Examples of useful polycarbonates such as a polymer or copolymer having repeating structural carbonate units of formula (1):(1)O- R1— O - C - O wherein at least 60 percent of the total number of R1groups are aromatic, or each R1contains at least one Ce-30 aromatic group. Specifically, each R1can be derived from adihydroxy compound such as an aromatic dihydroxy compound of formula (2) or a bisphenol of formula (3), as follows:In formula (2), each Rhis independently a halogen atom, for example bromine, a Ci-io hydrocarbyl group such as a Ci-io alkyl, a halogen-substituted Cuo alkyl, a Ce-io aryl, or a halogen-substituted Ce-io aryl, and n is 0 to 4.
[0020] In formula (3), Raand Rbare each independently a halogen, C1-12 alkoxy, or Ci- 12 alkyl, and p and q are each independently integers of 0 to 4, such that when p or q is less than 4, the valence of each carbon of the ring is filled by hydrogen. In certain embodiments, p and q are each 0, or p and q are each 1, and Raand Rbare each a C1-3 alkyl group, specifically methyl, disposed meta to the hydroxy group on each arylene group. Xais a bridging group connecting the two hydroxy-substituted aromatic groups, where the bridging group and the hydroxy substituent of each Ce arylene group are disposed ortho, meta, or para (specifically para) to each other on the C& arylene group, for example, a single bond, — O— , — S— , — S(=O)— ,— S(=O)2— (e.g., bisphenol-S polycarbonate, polysulfone), — C(=O)— (e.g., polyketone),or a C1-18 organic group, which can be cyclic or acyclic, aromatic or non-aromatic, and can further comprise heteroatoms such as halogens, oxygen, nitrogen, sulfur, silicon, or phosphorous. For example, Xacan be a substituted or unsubstituted C3-18 cycloalkylidene; a C1-25 alkylidene of the formula — C(Rc)(Rd)— wherein Rcand Rdare each independently hydrogen, C1-12 alkyl, C1-12 cycloalkyl, C7-12 arylalkyl, C1-12 heteroalkyl, or cyclic C7-12 heteroarylalkyl; or a group of the formula— C(=Re)— wherein Reis a divalent C1-12 hydrocarbon group. Certain illustrative examples of dihydroxy compounds that can be used are described, for example, in WO 2013 / 175448 Al, US 2014 / 0295363, and WO 2014 / 072923.
[0021] Specific dihydroxy compounds include resorcinol, 2,2-bis(4-hydroxyphenyl) propane ("bisphenol A" or "BPA"), 3,3-bis(4-hydroxyphenyl) phthalimidine, 2-phenyl- 3,3'-bis(4-hydroxyphenyl) phthalimidine (also known as N-phenyl phenolphthalein bisphenol, "PPPBP", or 3,3-bis(4-hydroxyphenyl)-2-phenylisoindolin-l-one), l,l-bis(4- hydroxy-3-methylphenyl)cyclohexane, and l,l-bis(4-hydroxy-3-methylphenyl)-3,3,5- trimethylcyclohexane (isophorone bisphenol).
[0022] Poly carbonates may also include copolymers comprising carbonate units and ester units ("poly(ester-carbonate)s", also known as polyester-polycarbonates).Poly(ester-carbonate)s further contain, in addition to recurring carbonate chain units of formula (1), repeating ester units of formula (4):(4) O O- C - T — C — O - J - O - wherein J is a divalent group derived from a dihydroxy compound (which includes a reactive derivative thereof), and can be, for example, a C2-10 alkylene, a C6-20 cycloalkylene a C6-20 arylene, or a polyoxyalkylene group in which the alkylene groups contain 2 to 6 carbon atoms, specifically, 2, 3, or 4 carbon atoms; and T is a divalent group derived from a dicarboxylic acid (which includes a reactive derivative thereof), and can be, for example, a C2-20 alkylene, a C6-20 cycloalkylene, or a C6-20 arylene.Copolyesters containing a combination of different T or J groups can be used. The polyester units can be branched or linear.
[0023] Specific dihydroxy compounds include aromatic dihydroxy compounds of formula (2) (e.g., resorcinol), bisphenols of formula (3) (e.g., bisphenol A), a Ci-8 aliphatic diol such as ethane diol, n-propane diol, i-propane diol, 1,4-butane diol, 1,6-cyclohexane diol, 1,6-hydroxymethylcyclohexane, or a combination comprising at least one of the foregoing dihydroxy compounds. Aliphatic dicarboxylic acids that can be used include Ce-2o aliphatic dicarboxylic acids (which includes the terminal carboxyl groups), specifically linear Cs-i2 aliphatic dicarboxylic acid such as decanedioic acid (sebacic acid); and alpha, omega-Cudicarboxylic acids such as dodecanedioic acid (DDDA). Aromatic dicarboxylic acids that can be used include terephthalic acid, isophthalic acid, naphthalene dicarboxylic acid, 1,6-cyclohexane dicarboxylic acid, or a combination comprising at least one of the foregoing acids. A combination of isophthalic acid and terephthalic acid wherein the weight ratio of isophthalic acid to terephthalic acid is 91:9 to 2:98 can be used.
[0024] Specific ester units include ethylene terephthalate units, n-propylene terephthalate units, n-butylene terephthalate units, ester units derived from isophthalic acid, terephthalic acid, and resorcinol (ITR ester units), and ester units derived from sebacic acid and bisphenol A. The molar ratio of ester units to carbonate units in the poly(ester-carbonate)s can vary broadly, for example 1:99 to 99:1, specifically, 10:90 to 90:10, more specifically, 25:75 to 75:25, or from 2:98 to 15:85.
[0025] The polycarbonates may have an intrinsic viscosity, as determined in chloroform at 25° C, of 0.3 to 1.5 deciliters per gram (dl / gm), specifically 0.45 to 1.0 dl / gm. The polycarbonates can have a weight average molecular weight of 5,000 to 200,000 Daltons, specifically 15,000 to 100,000 Daltons, as measured by gel permeation chromatography (GPC), using a crosslinked styrene-divinylbenzene column and calibrated to polycarbonate references. GPC samples are prepared at a concentration of 1 mg per mL (mg / mL) and are eluted at a flow rate of 1.5 mL per minute.
[0026] Examples of useful polysulfones may include polyarylethersulfones (PAES) which may be represented by:(1 ) wherein n is any integer value that gives rise to the PAES having an weight average molecular weight (Mw) anywhere from 1, 10, or 20 to 1000, 500 or 200 kDa, m typically varies from 0 to 10, each occurrence of R1represents an aromatic ring or fused rings of about 5-10 carbon atoms, such as but not limited to: 1,2-, 1,3-, or 1,4-phenylene, or a diphenylene such as but not limited to 4, 4' -diphenylene, and each occurrence of R2is independently C1-C20 alkyl, C5-C18 or C5-C12 aromatic ring or fused rings consisting of 5-10 carbon atoms, or a combination thereof. The fragment structure -R1-S(=O)2-R1- may also represent either of the fused heterocyclic ring structures shown in formulas 2 and 3; and wherein at least 60% of the total number of R1groups are aromatic, or each R2contains at least one C6-30 aromatic group. The fragment structure -R1-S(=O)2-R1- may also represent either of the fused heterocyclic ring structures shown in formulas 2 and 3:
[0027] In an embodiment R1and R2may be the residue of an aryl or diaryl compound:
[0028] In another embodiment, the PAES of formula (1), m has an integer value greater than or equal to zero (typically from 1 to 10, 6, 5, 4, 3, or 2), and each R2is a residue of a dihydroxy compound such as an aromatic dihydroxy compound:
[0029] In formulas (3), (4), and (5), each R3, R4, and R5is independently, for example, but not limited to: a halogen atom (e.g., chlorine or bromine), a C3-20 alkoxy, a C1-20 hydrocarbyl group (e.g., a C1-20 alkyl, a halogen-substituted C1-10 alkyl, a Ce-io aryl, or a halogen-substituted Ce-io aryl); and p, q, and r are each independently integers of 0 to 4, such that when p, q, or r is less than 4, the valence of each unsubstituted carbon of the ring is filled by hydrogen; and X represents a bridging group connecting the two phenolic groups, where the bridging group and the hydroxy substituent of each Ce arylene group are disposed ortho, meta, or para (preferably para) to each other on the Ce arylene group,and the X group consists of, for example: a single bond; -O-; -S-; -S(-O)-; -S(-O)2- (e.g., bisphenol-S); -C(=O)-; or a C1-20 organic group, which can be cyclic or acyclic, aromatic or non-aromatic, and can further comprise heteroatoms such as: halogens; oxygen; nitrogen; sulfur; silicon; or phosphorous.
[0030] Specific dihydroxy compounds include but are not limited to: resorcinol; 2,2- bis(4-hydroxyphenyl)propane ("bisphenol A" or"BPA", in which in which each of aryl rings is para-substituted and X is isopropylidene in formula (3)); 3,3-bis(4-hydroxyphenyl)- phthalimidine; 2-phenyl-3,3-bis(4-hydroxyphenyl)phthalimidine (also known as “N- phenyl phenolphthalein bisphenol", "PPPBP", or 3,3-bis(4-hydroxyphenyl)-2- phenylisoindolin-l-one); l,l-bis(4-hydroxy-3-methylphenyl)cyclohexane; l,l-bis(4- hydroxy-3-methylphenyl)-3,3,5-trimethylcyclohexane (also known as "isophorone bisphenol").
[0031] Examples of polyarylethersulfones that are suitable may any one or more of:nExamples of useful PAES polymers are: polyethersulfone (PSU, CAS # 25667-42, formula 7), poly(l,4-phenylene-ether-ether-sulfone (PES or PEES, CAS # 28212-68-2, formula 8), polyphenylenesulfone (PPSU, CAS # 25839-81-0, formula 9) and poly(bisphenol-A sulfone) (PSF, CAS # 25135-51-7, formula 10), such as are available under the tradenames RADEL from Curbel Plastics Inc., Arlington TX, PARYLS from UJU New Materials, Ltd., and UDEL from Solvay Specialty Polymers USA, LLC, Alpharetta, GA.
[0032] The thermoplastic polymer may be polyketone including polyketones having ether repeating units such as polyetherketone, polyetheretherketone, polyetherketoneketone. An exemplary polyketone without ether repeating units may be formed by the reaction of carbon monoxide, an alkene monomer in the presence of a group 8 to 10 transition metal catalyst. In particular, the method may be any one of those described in US Pat. Nos. 4,835,250; 4,894,435 and 5,138,032 and US Pat. Publ. No. 2008 / 0058494 each incorporated by reference in its entirety. In particular, the method, reaction conditions and monomers are those described in US Pat. No. 5,138,032 from col. 2 line 52 to col. 5, line 17 specifically incorporated herein by reference. Such polyketones are typically comprised of repeating units represented by
[0033] where A is the residue of an alkene monomer converted to a saturated hydrocarbon group, m is from about 1 to 6 and n is at least about 2 to any practicable amount to realize the desired number average molecular weight (Mn) useful in the invention. Desirably, the alkene monomer is comprised of an olefin having from 2 to 12,8 or 6 carbons. Illustratively, the alkene monomer is ethylene or the alkene monomer comprises ethylene and at least one other olefin monomer such as propylene. When the polyketone is a copolymer of ethylene and another olefin monomer (e.g., propylene), the amount of ethylene and other olefin is as described in US Pat. No. 5,138,032 from col. 2, line 17 to col. 3, line 14. The polyketone desirably is one that is a terpolymer of carbon monoxide, ethylene and another alkene monomer (e.g., olefin of 3 to 12, 8 or 6 carbons and in particular propylene). Such polyketone may be represented by random repeating units:Where G is the saturated residue of an olefin of 3 to 12, 8 or 6 carbons polymerized through the double bond and x / y is at least 2 to 100 or 50 or 20. Desirably, G is propylene. The polyketone may be terminated by any useful group such as alkyl group, hydroxyl, ester, carboxylic acid, ether or combination thereof. The particular terminating group may arise from using a solvent such as a low molecular alcohol such as methanol or water or combination thereof. Examples of commercially available polyketones include those available under the tradename POKETONE from Hyosung, Korea.
[0034] Generally, the polyketone may be a polyaryletherketone (PAES) such as those known in the art. Illustratively, the PAES may be polyetherketoneketone (PEKK) such as those known in the art and in particular amorphous PEKK as described from col. 2, line 13 to 55 of U.S. Pat. No. 10,364,349, incorporated herein by reference. PEKKs may be made by known methods such as those described in U.S. Pat. Nos 3,065,205; 3,441,538; 3,442,857; 3,516,966; 4,704,448; 4,816,556 and 6,177,518.
[0035] The polyamide may be any of those known in the art and commonly are semicrystalline as described from col. 4, line 7 to col. 5, line 22 of U.S. Pat. No. 5,391,640, incorporated herein by reference. In particular, the polyamide may be amorphous as described from col. 5, line 23 to col. 8, line 12 of U.S. Pat. No. 5,391,640, incorporatedherein by reference. Examples of conventional polyamides include polypyrrolidone (nylon 4), polycaprolactam (nylon 6), polyheptanolactam (nylon 7), polycaprylactam (nylon 8), polynonanolactam (nylon 9), polyundecaneolactam (nylon 11), polydodecanolactam (nylon 12), poly(tet-ramethylenediamine-co-oxalic acid) (nylon 4,2), poly(-tetramethylenediamine-co-adipic acid) (nylon 4,6), poly(tetramethylenediamine- co-isophthalic acid) (nylon 4,1), polyhexamethylene azelaiamide (nylon 6,9), polyhexamethylene sebacamide (nylon 6,10), polyhexa- 5 methylene isophthalamide (nylon 6, IP), polymetaxyly-lene adipamide (nylon MXD6), the polyamide of n-dodecanedioic acid and hexamethylenediamine (nylon 6,12), the polyamide of dodecamethylenediamine and n-dodecanedioic acid (nylon 12,12), as well as copoly- 10 mers thereof which include: hexamethylene adipamide-caprolactam (nylon 6,6 / 6), hexamethylene adipamide / -hexamethylene-isophthalamide (nylon 6,6 / 6IP), hexa-methylene adipamide / hexamethylene-terephthalamide (nylon 6,6 / 6T), trimethylene adipamide-hexamethy- 15 lene-azelaicamide (nylon trimethyl 6, 2 / 6, 2), and hexa-methylene adipamide-hexamethylene-azelaicamide caprolactam (nylon 6, 6 / 6, 9 / 6) as well as others which are not particularly delineated here.
[0036] The polyimide may be any of those known in the art and desirably are known aromatic polyimides. Illustratively, Aromatic polyimides that may be suitable are described in U.S. Pat. Nos. 3,179,631; 3,249,588 and 4,755,555, each incorporated herein by reference. More particularly, the polyimide is amorphous such as those described by A. Rosenberg, et. al., in Optical Materials Express Vol. 8, No. 8, 1 Aug. 2018, 2159.
[0037] The thermoplastic polymer powder has a particle size and characteristics that are maintained during the method to form the composite powder. The thermoplastic polymer powder has a size and size distribution that are useful for additive manufacturing. The thermoplastic polymer powder may be formed by any useful methods such as described previously to form a powder useful for powder bed additive manufacturing such as SLS. Illustratively, thermoplastic polymer powder has a particle size that is useful for making additive manufactured articles (e.g., forms the induced crystalized polymer particles), and typically has a median particle size (D50) or averageparticle size, by volume, from about 1 micrometer (pm), 5 pm, 10 pm, 20 pm or 30 pm to 150 pm, 125 pm, 100 pm or 90 pm. Likewise, to enable consistent heating and fusion of the powder, it desirably has a D90 of at most 300 pm, 200 pm or 150 pm and a Dio of at least 0.1 pm, 0.5 pm or 1 pm by volume. D90 means the particle size (equivalent spherical diameter) in the particle size distribution, where 90% by volume of the particles are less than or equal to that size; similarly, D50 means the particle size (equivalent spherical diameter) in the particle size distribution, where at least 50% by volume of the particles are less than that size, and Dio means the particle size (equivalent spherical diameter) in the particle size distribution, where at least 10% by volume of the particles are less than that size. The particle size may be determined by any suitable method such as those known in the art including, for example, laser diffraction or image analysis of micrographs of a sufficient number of particles (~100 to ~200 particles). A representative laser diffractometer is one produced by Microtrac such as the Microtrac S3500.
[0038] The inorganic powder may be any imparting a desirable characteristic for forming an article such as by additive manufacturing. The inorganic powder has an average primary particle size of at most 5 micrometer and desirably at most 3, 2, 1 or 0.5 micrometer or 0.3 micrometer in diameter. The powder may be comprised of primary particles that are chemically bound into secondary particles (e.g., carbon black) and referred to as structured inorganic powders or the primary particles may not be chemically bound otherthan by hydrogen or Van-der Waals forces. The particle size may be determined as previously described.
[0039] Exemplary inorganic powders may include calcium carbonate, talc, silica, wollastonite, clay, calcium sulfate, mica, inorganic glass (e.g., silica, alumino-silicate, borosilicate, alkali alumino silicate and the like), oxides (e.g., alumina, zirconia, magnesia, silica "quartz", fumed silica, and calcia), carbides (e.g., boron carbide and silicon carbide), nitrides (e.g., silicon nitride, aluminum nitride), combinations of oxynitride, oxycarbides, or combination thereof. In certain embodiments, the inorganic comprises an acicular filler such as talc, clay minerals, chopped inorganic glass, metal, or carbon fibers, mullite, mica, wollastanite or combination thereof. The secondary particle size may be any useful sizeand may typically be from about 1 micrometer to 100 micrometer average size and desirably deagglomerates during the method.
[0040] Desirably, the inorganic powder imparts electrostatic dissipation, improved powder flow or both. Exemplary inorganic powders include those that are structured powders. Exemplary, inorganic powders include carbon blacks that may be standard, conductive or non-conductive. The carbon black may have any useful oil absorption number (ASTM D-2414-09). For example, the carbon black typically should have an oil absorption number (OAN) of about 40, 50, or 60 to 200, 180 or 150 ccs per 100 grams. The specific surface area (ISO 9277:2010) may be any useful, and generally is at least 10 m2 / g, 20 m2 / g or 50 m2 / g to any practical surface area, 1000 m2 / g, 500 m2 / g, 300 m2 / g or 200 m2 / g.
[0041] The carbon black may be a standard carbon black which is not specially treated to render it nonconductive. Standard carbon black is carbon black which is not specifically surface treated or oxidized. Alternatively, one or more conductive carbon blacks may be used exclusively or in conjunction with the standard carbon black. Conductive carbon blacks are generally recognized as having at a purity of at least 97% carbon, OAN of 100 or greater and specific surface area of 120 m2 / g or greater. Examples of standard carbon blacks include RAVEN 790, RAVEN 450, RAVEN 500, RAVEN 430, RAVEN 420 and RAVEN 410 carbon blacks available from Colombian and carbon blacks available from Cabot Corporation under the tradenames VULCAN, PROPEL, REGAL, STERLING, and SPHERON.
[0042] The amount of the inorganic powder may be any amount useful to impart a desired characteristic, but, surprisingly, it has been found the composite particles formed by the method may realize desired electrostatic dissipative properties at a lower weight percent compared to melt compounding and then forming the particles. This may be due to the inorganic powder being embedded at the surface of the composite particles and upon localized sequential melting without shear when forming a 3D printed article, the inorganic particles are believed, without being limiting, to form an electrically conductive lattice within the article (display non-uniformity in distribution on the 10 to 100 micrometer scale with 3 dimensional connectivity). Such characteristic, surprisingly, maybe realized even when using standard carbon blacks having an OAN of 20 to 100 (cc / 100 grams) and surface area of ~20 m2 / g to 120 m2 / g.
[0043] The amount of inorganic powder may be any useful to realize the composite powder. To realize the desired characteristics, particularly when using a structured inorganic powder, and to have sufficient thermoplastic polymer to readily 3D print, the amount of inorganic powder is, generally, at most about ~10%, 6%, 5%, 4%, 3% to 0.01% 0.1% by weight of the thermoplastic polymer and inorganic powder. In other words, the weight ratio of the thermoplastic polymer powder / inorganic powder is from 8 to 10,000. Desirably the ratio is 16 or 20 to 500, 250 or 100.
[0044] The composite powder may be further comprised of constituents that impart a desired characteristic that may be added prior to, during or after the forming of the composite powder. These constituents may be any suitable for use with or in a polymer such as UV stabilizers, colorants or pigments (e.g., organic dyes), plasticizers, flame retardants, antioxidants, anticorrosive agents, toughening agents, rheology modifiers (e.g., plasticizers), opacifiers, inhibitors, fluorescence markers, thermal degradation reducers, thermal resistance conferring agents, biocides, scratch and abrasion resistance additives, slip and release aids, surface texture and appearance enhancing agents, matting agents, anti-graffiti agents, antifouling additives, adhesion promoting additives, thermal conductive agents, electromagnetic shielding agents, and stabilizers.
[0045] To make the mixture of the thermoplastic polymer powder and inorganic powder, they may be combined in any suitable manner. Illustratively, they may be mixed dry in the same vessel where shear is applied to form the composite powder. They may be combined prior to being placed in the vessel and then added to the vessel where sufficient shear is applied to realize the composite powder.
[0046] The shearing of the mixture, generally, is imparted by an axial impeller rotor where no stator, baffle or the like in the vessel is a distance that is within 100 times, 500 times or 1000 times, the average size of the thermoplastic polymer powder. For example, no part of the impeller passes a stationary component in the vessel closer than 1 mm, 2 mm, 5 mm or 10 mm including the closest inner wall of the vessel (e.g., bottom). Anillustration of a suitable apparatus includes those shown in U.S. Pat. No. 2,945,634, and, in particular, as depicted in Figures 1 and 4, incorporated herein by reference. Other illustrations of apparatus that may be useful include those described in U.S. Pat. Nos. 2,706,622; 2,752,097 and 3,250,519. The vessel may be comprised of one or more baffles to redirect the flow of the mixture, but such baffle is not in proximity to the impeller (no closer than as previously described). An illustration of such a baffle is depicted in Fig 1, of U.S. Pat. No. 2,945,634.
[0047] Sufficient shear rate and shear time is any that is useful to make the composite powder (embeds the inorganic powder) wherein the powder has a useful powder size and size distribution as described for the thermoplastic polymer powder. That is the method embeds the inorganic particles without substantial changes (e.g., attrition or agglomeration due to fusing of the thermoplastic polymer powder particles) to underlying thermoplastic polymer powder particle size and size distribution (i.e., the composite powder has an average particle size that is within 25% of the thermoplastic polymer powder average particle size). Desirably, the composite powder average size is within 20%, 15% or 10%. Likewise, the Dgo and Dio particle size of the composite powder is within the same percentages as the average size. The method may also preferentially remove smaller particles shifting the DM to a larger size such as the DM increasing by 5%, 10%, or 25% larger.
[0048] Illustratively, the shear rate may be any useful that raises the bulk temperature of the mixture sufficiently to facilitate the embedding of the inorganic powder and typically raises the bulk temperature at least 5 °C, 10 °C or 20 °C during the shearing time in the absence of externally applied heat. Typical shear rates may be at least 1 s’1, 5 s’1, or 10 s-1to 1000 s1500 s’1, 250 s1or 100 s’1. Bulk temperature of the mixture is the temperature of the mixture as measured by a thermocouple probe at from 1 cm to 5 cm distant from the impeller.
[0049] The time may be any useful time to form the composite, but surprisingly it has been discovered that short times may be sufficient. For example, the shear time may be from 1 minute, 2 minutes, 5 minutes to 60 minutes, 30 minutes or 25 minutes. It has alsobeen discovered that the maximum bulk temperature reached during the method desirably is below and within 40 °C, 30 °C, 20 °C, or 10 °C of the glass transition temperature of the thermoplastic polymer.
[0050] The mixture may be further externally heated or cooled while shearing to facilitate the embedding of the inorganic powder and may be desirable when depending on glass transition temperature (Tg) of the thermoplastic polymer (e.g., Tg is greater than 100 °C). The externally provided heating may be by any suitable method such as those known in the art (e.g., heated vessel jacket or introduction of a heated gas into the vessel during the shearing).
[0051] The vessel in which the shearing is performed may be filled with the thermoplastic polymer powder and inorganic powder to any useful fill volume, but generally the amount of mixture occupies from 20% or 50% to 90% of the vessel's volume. The fill volume is the volume occupied by the thermoplastic polymer powder, inorganic powder and any void volume between the particles.
[0052] The method may further induce desired morphology and flowability of the composite powder compared to the thermoplastic polymer powder. Illustratively the the composite powder may have a flowability of at least about 0.5 g / s, 1 g / s or 2 g / s to any practically achievable rate (e.g., 50 g / s) using a 15-mm nozzle as determined by Method A of ASTM D 1895 with or without addition of a flow aid (e.g., AEROSIL 200). The flowability of the composite powder may be 5%, 10%, 20, 30% or 50% to or more compared to the flowability of the thermoplastic polymer powder.
[0053] Desirably, the composite powder has a sphericity in terms of particle shape, and in particular particle roundness, which aids in flowability, and as derived from micrograph images of individual particles, may be expressed in terms of circular character, or circularity, where individual particle circularity is defined as the 4nA / P2, where A is the area of the particle and P is the perimeter length of the particle, both as viewed from a random perspective. Sphericity, a related parameter, is derived as the square root of circularity. Circularity is a numerical value greater than zero and less than or equal to one. A perfectly circular particle is referred to as having a circularity of 1.00.Tables of population circularity data are represented in such a way that various levels of circularity (e.g., 0.65, 0.75, 0.85, 0.90, and 0.95) are accompanied by percentages of the particle sample population with a circularity greater than the tabulated value. Particle size and shape can be measured by any suitable methods known in the art to measure particle size by diameter. In some embodiments, the particle size and shape are determined by laser diffraction as is known in the art. For example, particle size can be determined using a laser diffractometer such as the Microtrac S3500 with image analysis accessory using PartAnSI software to analyze the captured images of the particles. Desirably, at least about 65%, 75% or 80% of the particles (by number) have a circularity that is at least about 0.6, 0.75, 0.8 or 0.85. Likewise, the composite powder sphericity is at within 5%, 10, or 20% of the thermoplastic polymer powder.
[0054] The composite powder is useful to make powder bed additive manufactured articles. The composite powder may be made into a body by an additive manufacturing method such as SLS, MJF, HSS or electrophotography. Illustratively, in SLS, a layer of the composite powder may be deposited on a bed at a fixed temperature below the melting temperature of the composite powder and a predetermined (selected) area of the bed is sintered (fused) together using a heating source such as a laser controlled and directed as described above. Layers are then in succession deposited and sintered to the preceding layer and within the layer to build up an additive manufactured part.
[0055] The method, surprisingly, allows for the manufacture of antistatic polymeric (electrically insulating polymers such as the polymers described herein) articles having reduced amounts of electrically conductive inorganic particles such as carbon black. For example, the additive manufactured article is comprised of a fused thermoplastic polymer powder and inorganic powder, wherein the sheet (surface) resistance is at most 1 x 1012Q / n and the inorganic powder is present in an amount of at most 5% by weight of the additive manufactured article. The sheet or surface resistance may be determined by ANSI / ESD STM11.11 surface resistance and ANSI / ESD STM11.12 volume resistivity utilizing a Prostat PRF-911 concentric ring fixture (Prostat Corp. Bensenville, IL). The thermoplastic polymer of the additive manufactured article may be amorphous (e.g.,fused induced crystalline thermoplastic polymer powder reverted to amorphous during the additive manufacturing process). Desirably, the sheet resistance is at most about 1 x IO10Q / zi, 1 x 109Q / n, 1 x 107Q / n 1 x 105Q / n or 1 x 103Q / n. The amount of inorganic powder may be at most 4%, 3%, 2%, or 1% to 0.1% by weight of the thermoplastic polymer powder and inorganic powder.
[0056] The composite powder may be comprised of an amorphous thermoplastic polymer powder having induced crystallinity and having an average particle size of 20 to 100 micrometers equivalent spherical diameter and a D90 of at most 300 micrometers and a D10 of at 10 micrometers and from 0.05% to 5% by weight of an inorganic particulate have an average primary particle size of at most 5, 3, 2 or 1 micrometer that is embedded in the thermoplastic powder at its surface. The amount of inorganic powder may be as described above for the additive manufactured article.
[0057] The term "powder bed fusing" or "powder bed fusion" is used herein to mean processes wherein the composite thermoplastic polymer particles are selectively sintered or melted and fused, layer-by-layer to provide a 3-D object. Sintering can result in objects having a density of less than about 90% of the density of the solid powder composition, whereas melting can provide objects having a density of 90%-100% of the solid powder composition. Use of induced crystalized polymer particles can facilitate melting such that resulting densities can approach densities achieved by injection molding methods.
[0058] Powder bed fusing or powder bed fusion further includes all laser sintering and all selective laser sintering processes as well as other powder bed fusing technologies as defined by ASTM F2792-12a. For example, sintering of the powder composition can be accomplished via application of electromagnetic radiation other than that produced by a laser, with the selectivity of the sintering achieved, for example, through selective application of inhibitors, absorbers, susceptors, or the electromagnetic radiation (e.g., through use of masks or directed laser beams). Any other suitable source of electromagnetic radiation can be used, including, for example, infrared radiation sources, microwave generators, lasers, radiative heaters, lamps, or a combination thereof. In certain embodiments, selective mask sintering ("SMS") techniques can be used toproduce three-dimensional objects. For further discussion of SMS processes, see for example U.S. Pat. No. 6,531,086, which describes an SMS machine in which a shielding mask is used to selectively block infrared radiation, resulting in the selective irradiation of a portion of a powder layer.
[0059] The composite thermoplastic particles may be particularly useful for SMS with due to the surface embedded inorganic particulates enhancing the infrared absorption properties of the composite thermoplastic polymer powder such as carbon particulates described herein.
[0060] Powder bed fused (e.g., laser sintered) objects can be produced from the thermoplastic polymer composite powder using any suitable powder bed fusing processes including laser sintering processes. These articles include a plurality of overlying and adherent sintered layers that include a continuous polymeric matrix and an continuous matrix of the comprised of the thermoplastic polymer and interconnected inorganic powder, which is believed, without being limited due to the inorganic powder location on the surface of the thermoplastic polymer of the composite powder.
[0061] Laser sintering processes are known and are based on the selective sintering of polymer particles, where layers of polymer particles are briefly exposed to laser light and the polymer particles exposed to the laser light are thus bonded to one another. Successive sintering of layers of polymer particles produces three-dimensional objects. Details concerning the selective laser sintering process are found, by way of example, in the specifications of U.S. Pat. No. 6,136,948 and WO 96 / 06881. However, the induced crystalized polymer particles described herein can also be used in other rapid prototyping or rapid manufacturing processing (e.g., sheet lamination), in particular in those described above. For example, the induced crystalized polymer particles can in particular be used for producing moldings from powders via the SLS (selective laser sintering) process, as described in U.S. Pat. No. 6,136,948 or WO 96 / 06881, via the SIB process (selective inhibition of bonding of powder), as described in WO 01 / 38061, via 3D printing, as described in EP 0431 924.Illustrative EmbodimentsIllustration 1. A method to form a composite powder comprising: contacting a thermoplastic polymer powder and a inorganic powder having an average primary particle size of less than 1 micrometer and the thermoplastic polymer powder having an average particle size of at least 10 micrometers to 100 micrometers, the thermoplastic polymer powder / inorganic powder having a weight ratio 8 to 100, to form a mixture and shearing the mixture in a vessel for a shear time and shear rate sufficient to form the composite powder having the inorganic powder embedded in the thermoplastic polymer powder, wherein the composite powder has an average particle size that is within 25 percent of the thermoplastic polymer powder average size.Illustration 2. The method of either illustration 1, wherein the inorganic powder is comprised of one or more of a carbon black, graphite, fumed silica, carbon nanotubes, carbon fibers.Illustration 3. The method of either illustration 1 or 2, wherein the inorganic powder is comprised of a structured inorganic powder having a specific surface area of at least 10 m2 / g and oil absorption number of at least 50.Illustration 4. The method of illustration 3, wherein the structured inorganic powder is carbon black.Illustration 5. The method of illustration 4, wherein the carbon black has a specific surface area of at least 50m2 / g and oil absorption number of at least 75.Illustration 6. The method of illustration 5, wherein carbon black is a conductive carbon black.Illustration 7. The method of any one of the preceding illustrations, wherein the polymer composite powder average particle size is within 10 percent of the thermoplastic polymer powder average particle size.Illustration 8. The method of any one of the preceding illustrations wherein the inorganic powder is present in an amount of at most about 5% to 0.1% by weight of the inorganic powder and thermoplastic polymer.Illustration 9. The method of any one of the preceding illustrations, wherein the shearing is performed by an impeller in the vessel.Illustration 10. The method of illustration 9, wherein the impeller is an axial flow impeller.Illustration 11. The method of illustration 10 wherein the vessel having a baffle for redirecting the flow of the mixture not in proximity to the impeller.Illustration 12. The method of any one of the preceding illustrations, wherein the vessel has a fill loading of the thermoplastic polymer powder and inorganic powder of 20% to 90% by volume of the vessel.Illustration 13. The method of illustration 12, wherein the fill loading is 50% to 85%.Illustration 14. The method of any one of the preceding illustrations, wherein the thermoplastic polymer powder D90 particle size of at most 300 pm, an average particle diameter from about 10 pm to about 50 pm and Dio particle size of at least 0.5 pm and the composite powder has a D90 particle size of at most 300 pm, an average particle diameter from 10 pm to 50 pm and Dio particle size of at least 0.5 pmIllustration 15. The method of any one of the preceding illustrations, wherein the thermoplastic polymer powder and composite powder have a flowability of at least about 0.5 g / s as determined by Method A of ASTM D 1895 using a 15 mm nozzle.Illustration 16. The method of any one of the preceding illustrations, wherein the composite powder and thermoplastic polymer have a circularity of at at least 80% of the particles by number have a circularity of 0.65 or greater.Illustration 17. The method of any one of the preceding illustrations further comprising the heating of the thermoplastic polymer, inorganic powder.Illustration 18. The method of illustration 17, wherein the heating is applied prior to introduction into the vessel, incurred during the method.Illustration 19. The method of illustration 18, wherein the heating incurred during the method is provided by one or more of the shearing, heating of the vessel, and introducing a heated gas to the thermoplastic polymer powder in the vessel.Illustration 20. The method of any one of the preceding illustrations, wherein the heating causes a bulk mixture temperature that is below the thermoplastic polymer powder's glass transition temperature.Illustration 21. The method of illustration 20, wherein the maximum bulk mixture temperature is within 30 °C of the glass transition temperature of the thermoplastic polymer.Illustration 22. The method of any one of the preceding illustrations, wherein the shear time is 1 minute to 30 minutes.Illustration 23. The method of any one of illustrations 20 to 22, wherein the shear time is determined by the bulk temperature reaching a predetermined temperature below the glass transition temperature of the thermoplastic polymer powder.Illustration 24. The method of illustration 23, wherein a portion of the shear time is for a time at or above the predetermined temperature and below the glass transition temperature of the thermoplastic polymer.Illustration 25. A method of forming an article comprising heating the composite powder made by any one of the preceding illustrations above the thermoplastic polymer's melting temperature and shaping said composite powder into the article.Illustration 26. The method of illustration 25, wherein the shaping is by a powder additive manufacturing method.Illustration 27. The method of either illustrations 25 or 26, wherein the article has a sheet resistance of at most 1 x 109Q / n and the inorganic powder is present in an amount of at most 5% by weight of the article.Illustration 28. The method of illustration 27, wherein the sheet resistance is at most 1 x 107Q / n.Illustration 29. The method of either illustration 1 or 28, wherein the amount of inorganic powder is at least 0.1%.Illustration 30. An additive manufactured article comprising a fused thermoplastic polymer powder and inorganic powder, the additive manufactured articlehaving a sheet resistance is at most 1 x 109Q / n and the inorganic powder is present in an amount of at most 5% by weight of the additive manufactured article.Illustration 31. The additive manufactured article of illustration 30, wherein the thermoplastic polymer is amorphous.Illustration 32. The additive manufactured article of either illustration 30 or 31, wherein the inorganic powder has an average primary particle size of at most 1 micrometer.Illustration 33. The additive manufactured article of any one of illustrations 30 to 32, wherein the inorganic powder is a carbon black.Illustration 34. A composite powder comprising a thermoplastic polymer powder having induced crystallinity and an average particle size of 20 to 100 micrometers equivalent spherical diameter and a D90 of at most 300 micrometers and a D10 of at 10 micrometers and from 0.1% to 5% by weight of an inorganic powder having an average primary particle size of at most 1 micrometer that is embedded in the thermoplastic polymer powder at its surface.Illustration 35. The composite powder of illustration 34, wherein the thermoplastic polymer powder having induced crystallinity reverts to being amorphous upon heating above its melt temperature and cooling back below its melt temperature.Illustration 36. The composite powder of either illustration 34 or 35, wherein the inorganic powder is a carbon black.Examples
[0062] Materials used to make the composite powder is shown in Table 1.Comparative Example 1
[0063] A ground aliphatic polyketone as described in Example 1 of WO2022245720 after screening with a 125 micrometers screen is 3D printed using a Farsoon ST252P SLS printer into ASTM D638 Type IV tensile bars and disks for measuring the surface resistance. The glass transition temperature of the aliphatic ketone is about 70 °C. Thesurface resistivity and mechanical properties of exemplary samples are shown in Table 3.The as ground and screened aliphatic powder has a D90VOisize of 76.93 micrometers,D50VOisize 50.73 micrometers and D10VOisize of 35.43 micrometers and a D90num of 56.30 micrometers, D50num of 39.40 micrometers and D10num of 25.91 as measured in air using laser diffraction (Microtrac S3500). The same powder when subjected to the mixing of the Examples in the absence of any additives has a D90VOisize of 76.34 micrometers, D50VOisize 50.63 micrometers and D10VOisize of 35.48 micrometers and a D90num of 56.28 micrometers, D50num of 39.51 micrometers and D10num of 26.13. This shows that the method essentially maintains the particle size and size distribution of the powder subjected to the method. The bulk density of Comp. Ex. l's powder is 0.467 g / cc as determined by ASTM C29 / C29M.Examples 1-10 and Comparative Examples 2 and 3
[0064] Each of the Examples 1-10 and Comparative Examples 2 and 3 use the ground aliphatic polyketone of Comparative Example 1. The composition of each Example and Comparative Examples 2 and 3 and process conditions are shown in Table 2. The characteristics of the samples of the Examples and Comparative Examples are shown in Table 3. The shearing is performed in an industrial mixer as described herein (e.g., U.S. Pat. No. 2,945,634, Figures 1 and 4). The rotor speed is 1200 rpm resulting a in maximum calculated shear of about 60 s T The maximum temperature reached is 60 °C.Example 11
[0065] 99 parts by weight (pbw) of a recycled ground sieved (106 micrometer sieve) polyamide (PA12 available under the tradename PA33OO available from Farsoon, China) is sheared with 1 pbw of Regal 660R carbon black in the same manner as described for Examples 1-10 for a time of 480 seconds. This composite powder is printed into 4x4 inches 3mm thick specimens using the same process as described for Comparative Example 1. The parts printed well and the surface resistance results measured as described herein is shown in Table 4. This example shows that the method may besuccessfully employed in rehabilitating polymer powders that have been subject to long periods of elevated temperatures during printing and then recycled to form powders that are printable, forming additive manufactured articles with desirable electrostatic dissipation even at low concentrations of added inorganic particles.Table 1.Table 2Table 3Table 4
Claims
What is claimed is:Claim 1. A method to form a composite powder comprising: contacting a thermoplastic polymer powder and a inorganic powder having an average primary particle size of less than 1 micrometer and the thermoplastic polymer powder having an average particle size of at least 10 micrometers to 100 micrometers, the thermoplastic polymer powder / inorganic powder having a weight ratio of 8 to 10,000, to form a mixture and shearing the mixture in a vessel for a shear time and shear rate sufficient to form the composite powder having the inorganic powder embedded in the thermoplastic polymer powder, wherein the composite powder has an average particle size that is within 25 percent of the thermoplastic polymer powder average size.Claim 2. The method of either claim 1, wherein the inorganic powder is comprised of one or more of a carbon black, graphite, fumed silica, carbon nanotubes, carbon fibers.Claim 3. The method of either claim 1 or 2, wherein the inorganic powder is comprised of a structured inorganic powder having a specific surface area of at least 10 m2 / g and oil absorption number of at least 50.Claim 4. The method of claim 3, wherein the structured inorganic powder is carbon black.Claim 5. The method of claim 4, wherein the carbon black has a specific surface area of at least 50m2 / g and oil absorption number of at least 75.Claim 6. The method of claim 5, wherein carbon black is a conductive carbon black.Claim 7. The method of any one of the preceding claims, wherein the polymer composite powder average particle size is within 10 percent of the thermoplastic polymer powder average particle size.Claim 8. The method of any one of the preceding claims wherein the inorganic powder is present in an amount of at most about 5% to 0.1% by weight of the inorganic powder and thermoplastic polymer.Claim 9. The method of any one of the preceding claims, wherein the shearing is performed by an impeller in the vessel.Claim 10. The method of claim 9, wherein the impeller is an axial flow impeller.Claim 11. The method of claim 10 wherein the vessel having a baffle for redirecting the flow of the mixture not in proximity to the impeller.Claim 12. The method of any one of the preceding claims, wherein the vessel has a fill loading of the thermoplastic polymer powder and inorganic powder of 20% to 90% by volume of the vessel.Claim 13. The method of claim 12, wherein the fill loading is 50% to 85%.Claim 14. The method of any one of the preceding claims, wherein the thermoplastic polymer powder D90 particle size of at most 300 pm, an average particle diameter from about 10 pm to about 50 pm and Dio particle size of at least 0.5 pm and the composite powder has a D90 particle size of at most 300 pm, an average particle diameter from 10 pm to 50 pm and Dw particle size of at least 0.5 pmClaim 15. The method of any one of the preceding claims, wherein the thermoplastic polymer powder and composite powder have a flowability of at least about 0.5 g / s as determined by Method A of ASTM D 1895 using a 15 mm nozzle.Claim 16. The method of any one of the preceding claims, wherein the composite powder and thermoplastic polymer have a circularity of at least 80% of the particles by number have a circularity of 0.65 or greater.Claim 17. The method of any one of the preceding claims further comprising the heating of the thermoplastic polymer, inorganic powder.Claim 18. The method of claim 17, wherein the heating is applied prior to introduction into the vessel, incurred during the method.Claim 19. The method of claim 18, wherein the heating incurred during the method is provided by one or more of the shearing, heating of the vessel, and introducing a heated gas to the thermoplastic polymer powder in the vessel.Claim 20. The method of any one of the preceding claims, wherein the heating causes a bulk mixture temperature that is below the thermoplastic polymer powder's glass transition temperature.Claim 21. The method of claim 20, wherein the maximum bulk mixture temperature is within 30 °C of the glass transition temperature of the thermoplastic polymer.Claim 22. The method of any one of the preceding claims, wherein the shear time is 1 minute to 30 minutes.Claim 23. The method of any one of claims 20 to 22, wherein the shear time is determined by the bulk temperature reaching a predetermined temperature below the glass transition temperature of the thermoplastic polymer powder.Claim 24. The method of claim 23, wherein a portion of the shear time is for a time at or above the predetermined temperature and below the glass transition temperature of the thermoplastic polymer.Claim 25. A method of forming an article comprising heating the composite powder made by any one of the preceding claims above the thermoplastic polymer's melting temperature and shaping said composite powder into the article.Claim 26. The method of claim 25, wherein the shaping is by a powder additive manufacturing method.Claim 27. The method of either claims 25 or 26, wherein the article has a sheet resistance of at most 1 x 109Q / n and the inorganic powder is present in an amount of at most 5% by weight of the article.Claim 28. The method of claim 27, wherein the sheet resistance is at most 1 x 107Q / n.Claim 29. The method of either claim 27 or 28, wherein the amount of inorganic powder is at least 0.1%.Claim 30. An additive manufactured article comprising a fused thermoplastic polymer powder and inorganic powder, wherein the additive manufactured article has a sheet resistance that is at most 1 x 109Q / n and the inorganic powder is present in an amount of at most 5% by weight of the additive manufactured article.Claim 31. The additive manufactured article of claim 30, wherein the thermoplastic polymer is amorphous.Claim 32. The additive manufactured article of either claim 30 or 31, wherein the inorganic powder has an average primary particle size of at most 1 micrometer.Claim 33. The additive manufactured article of any one of claims 30 to 32, wherein the inorganic powder is a carbon black.Claim 34. A composite powder comprising a thermoplastic polymer powder having induced crystallinity and an average particle size of 20 to 100 micrometers equivalent spherical diameter and a D90 of at most 300 micrometers and a D10 of at 10 micrometers and from 0.1% to 5% by weight of an inorganic powder having an average primary particle size of at most 1 micrometer that is embedded in the thermoplastic polymer powder at its surface.Claim 35. The composite powder of claim 34, wherein the thermoplastic polymer powder having induced crystallinity reverts to being amorphous upon heating above its melt temperature and cooling back below its melt temperature.Claim 36. The composite powder of either claim 34 or 35, wherein the inorganic powder is a carbon black.
Citation Information
Patent Citations
Three-dimensional printing techniques
EP0431924A2
Assemblies containing polyetherketoneketone tie layers
US10364349B1
Process for preparing polyketone
US20080058494A1
Plastic flame housing and method of making the same
US20140295363A1
Mixing or stirring apparatus
US2706622A