Separator, secondary battery comprising same, and electric device

By filling the lithium-ion battery separator with high melting point inorganic particles and combining polydopamine modification and composite layer technology, the problem of polyolefin separator shrinkage at high temperature is solved, significantly improving the safety performance and cycle stability of the battery.

WO2024227351A1PCT designated stage expired Publication Date: 2024-11-07ZHEJIANG LIWINON ENERGY TECHNOLOGY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/139350
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-04
Filing Date
2023-12-18
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The polyolefin separators used in existing lithium-ion batteries are prone to shrink at high temperatures, which poses safety risks, and the modification solution may cause explosions in short circuits or local overheating.

Method used

The base film is filled with inorganic particles with melting points greater than or equal to 200°C, and the separator structure is reconstructed to improve heat shrinkage resistance by combining polydopamine modification and composite layer.

Benefits of technology

It effectively reduces the heat shrinkability of the diaphragm at high temperatures, and improves the safety performance and cycle stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023139350_07112024_PF_FP_ABST
    Figure CN2023139350_07112024_PF_FP_ABST
Patent Text Reader

Abstract

A separator, comprising a base membrane containing a plurality of holes, wherein part of the holes are filled with supporting particles, and the supporting particles comprise first inorganic particles having a melting point greater than or equal to 200ºC. Part of the holes in the base membrane of the separator are filled with the supporting particles, and the inorganic particles having a melting point greater than or equal to 200ºC are used for filling, such that the inorganic particles are dispersed in each region of the base membrane. Therefore, by reconstructing a base membrane system, the supporting effect of the inorganic particles can effectively ameliorate the problem of the base membrane being prone to shrinkage at a high temperature, the heat shrinkage resistance of the separator at a high temperature is effectively improved, and the safety performance of a battery is thus improved. In addition, further provided are a secondary battery comprising the separator, and an electric device.
Need to check novelty before this filing date? Find Prior Art

Description

Diaphragm and secondary battery and electrical device containing the same Technical Field

[0001] The present invention relates to the field of secondary batteries, and in particular to a diaphragm and a secondary battery and an electrical device containing the diaphragm. Background Art

[0002] With the continuous advancement of technology, people are increasingly demanding safer and more environmentally friendly lithium-ion batteries. A common lithium-ion battery mainly consists of a positive electrode, a negative electrode, a separator, and an electrolyte. The separator is located between the positive and negative electrodes, providing a path for the smooth movement of ions and also plays a vital role in preventing battery short circuits.

[0003] Currently, the mainstream separators used in lithium-ion batteries are all made of polyolefins. However, polyolefins will shrink severely at high temperatures and are prone to heat accumulation in the event of a short circuit or local overheating, which can even cause an explosion. Based on this, there are also related proposals to modify polyolefin separators to improve battery safety. However, the current modification schemes mainly modify the surface of polyolefins, such as coating the surface with a mixed layer of polymethyl methacrylate, aluminum oxide, or polyvinylidene fluoride and aluminum oxide. Although these modifications improve the safety of the battery to a certain extent compared to pure polyolefin separators, they still shrink to a large extent at high temperatures, and there are still major safety risks.

[0004] In view of this, it is indeed necessary to provide a technical solution to the above problems.

[0005] Summary of the Invention

[0006] One of the purposes of the present invention is to provide a separator to address the deficiencies of the prior art, so as to improve the problem that the current polyolefin separators are prone to shrinkage at high temperatures, resulting in poor battery safety performance.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A separator includes a base film having a plurality of pores, wherein a portion of the pores are filled with supporting particles, wherein the supporting particles include first inorganic particles having a melting point greater than or equal to 200°C.

[0009] Preferably, the base film is a polyolefin base film modified with polydopamine.

[0010] Preferably, the method for modifying the polyolefin base membrane with polydopamine is: immersing the polyolefin base membrane in a polydopamine solution, taking it out after standing, and drying it to obtain the modified polyolefin base membrane; the method for filling the support particles is: immersing the polyolefin base membrane modified with polydopamine in a solution containing support particles, taking it out and drying it to obtain a base membrane with support particles filled in some pores.

[0011] Preferably, the supporting particles further include a linking agent, and the mass ratio of the linking agent to the first inorganic particles is (1-5):(5-9).

[0012] Preferably, the linking agent is at least one of polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, and polyvinyl acetate acetal; and the first inorganic particles are at least one of aluminum oxide, titanium dioxide, and silicon dioxide.

[0013] Preferably, it further comprises a composite layer coated on at least one surface of the base film.

[0014] Preferably, the composite layer comprises second inorganic particles, polyethylene oxide and cellulose, and the weight ratio of the second inorganic particles, polyethylene oxide and cellulose is (4-8): (1-5): (1-5).

[0015] Preferably, the second inorganic particles are at least one of aluminum oxide, titanium dioxide, and silicon dioxide; the molecular weight of the polyethylene oxide is 500,000 to 600,000; the cellulose includes at least one of coniferous wood cellulose, broadleaf wood cellulose, and herbaceous wood cellulose; preferably, the preparation method of the composite layer is: first, the second inorganic particles and polyethylene oxide are mixed to form a solution, and the cellulose is dissolved to form a solution b; then, the solution a and the solution b are stirred and mixed to obtain a composite layer slurry; the composite layer slurry is coated on at least one surface of the base film and dried.

[0016] A second object of the present invention is to provide a secondary battery comprising a positive electrode sheet, a negative electrode sheet and a separator separated between the positive electrode sheet and the negative electrode sheet, wherein the separator is any one of the separators described above.

[0017] A third object of the present invention is to provide an electrical device comprising the secondary battery described above.

[0018] Compared to existing technologies, the present invention offers the following advantages: the separator provided by the present invention fills a portion of the pores in the base membrane with supporting particles, using inorganic particles with a melting point greater than or equal to 200°C, dispersing the inorganic particles throughout the base membrane. This restructured base membrane system effectively reduces the base membrane's tendency to shrink at high temperatures, effectively improving the separator's resistance to thermal shrinkage at high temperatures and, consequently, enhancing battery safety. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] FIG1 is a schematic diagram of a diaphragm structure according to the present invention.

[0020] FIG2 is a second schematic diagram of the diaphragm structure of the present invention.

[0021] FIG3 is a comparative test diagram of thermal shrinkage rates of Example 7 of the present invention and Comparative Example 2.

[0022] FIG4 is a graph showing the cycle performance of the batteries prepared in Example 7 of the present invention and Comparative Example 2.

[0023] In the figure: 1-base film; 2-composite layer. DETAILED DESCRIPTION

[0024] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below with reference to specific implementation methods and accompanying drawings, but the implementation methods of the present invention are not limited thereto.

[0025] The terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of the technical features being referred to. Thus, a feature specified as "first" or "second" may explicitly or implicitly include one or more of such features. In the description of the present invention, "plurality" means two or more, unless otherwise specifically defined.

[0026] The standard parts used in the present invention can all be purchased from the market, and special-shaped parts can be customized according to the description in the specification and the drawings. The specific connection methods of each part adopt conventional means such as mature bolts, rivets, welding, etc. in the existing technology. The machinery, parts and equipment all adopt conventional models in the existing technology, and the circuit connection adopts the conventional connection method in the existing technology, which will not be described in detail here.

[0027] In batteries, temperatures above 100°C are considered high. High temperatures pose significant challenges to all aspects of battery performance, especially safety. The polyolefin separators currently in mainstream use shrink significantly at temperatures as low as 130°C, posing a significant safety risk.

[0028] Based on this, the first aspect of the present invention is to provide a diaphragm, as shown in Figure 1, comprising a base membrane 1 containing a plurality of pores, wherein a portion of the pores are filled with supporting particles, and the supporting particles include first inorganic particles with a melting point greater than or equal to 200°C.

[0029] The base film 1 described in the present invention preferably refers to a base film based on polyolefin material, and the polyolefin material includes but is not limited to polyethylene and / or polypropylene base films. By reconstructing the structure of the material and filling a part of the pores with inorganic particles having a melting point ≥ 200°C, and using inorganic particles as auxiliary support, the thermal shrinkage performance of the polyolefin base film can be better improved, thereby ensuring the safety performance of the battery.

[0030] Preferably, the melting point of the first inorganic particle is greater than or equal to 500°C. More preferably, the melting point of the first inorganic particle is greater than or equal to 1000°C. Relatively speaking, the higher the melting point of the inorganic particles used as the support, the more significant the improvement in the thermal shrinkage performance of the diaphragm. Preferably, the first inorganic particles are at least one of aluminum oxide, titanium dioxide, and silicon dioxide. Further preferably, the first inorganic particle is aluminum oxide. Aluminum oxide is generally a white crystalline powder that absorbs moisture easily but does not deliquesce. It has a melting point of 2050°C, a boiling point of 2980°C, a relative density of 3.965, a Mohs hardness of 8.8, is an electrical insulator, and has a volume resistivity of 1.2×10 at 300°C. 13 Q·cm. Furthermore, alumina is practically insoluble in water and non-polar organic solvents such as ethanol and ether, and has very low solubility in weak acids or bases. This allows for good stability in batteries, and its inclusion as a component of supporting particles can effectively support the structure of the diaphragm and ensure its thermal stability at high temperatures.

[0031] More preferably, the present invention uses α-phase nano-alumina, which has a spherical crystal structure, a low specific surface area, and is more inert and resistant to high temperatures.

[0032] Furthermore, since only a portion of the pores are filled with support particles, a relatively large number of pores remain for ion passage, substantially unaffecting the battery's cycling performance. Preferably, the present invention utilizes a base membrane 1 having a relatively high porosity as its basis. This ensures that while supporting particles are filled, the base membrane still has a porosity similar to that of currently used separators, thereby better ensuring the battery's cycling performance.

[0033] In some embodiments, the base film 1 is a polyolefin base film modified with polydopamine.

[0034] Polydopamine (PDA) is a highly cross-linked polymer formed by the oxidative polymerization of dopamine. It shares many similarities with naturally occurring biopolymers, melanin, and eumelanin. Using PDA to modify polyolefin-based membranes is beneficial because PDA is biocompatible, resistant to many reagents, and exhibits strong adhesion to various materials and surfaces. Therefore, it can grow well on the surface of the membrane, thereby improving the membrane's compatibility with other substances, such as its hydrophilic properties. Furthermore, the PDA structural fragment is a conjugated system rich in π electron clouds, which can generate π-π interactions with other molecules containing π systems, leading to adsorption. Furthermore, the PDA structure contains active double bonds that can chemically react with multiple groups, such as amino (-NH2) and sulfhydryl (-SH). Through these reactions, other substances can be composited with the polyolefin-based membrane.

[0035] Specifically, the method for modifying the polyolefin-based membrane with polydopamine is as follows: immersing the polyolefin-based membrane in a polydopamine solution, letting it stand, taking it out, and drying it to obtain the modified polyolefin-based membrane.

[0036] More specifically, the method for modifying the polyolefin-based film with polydopamine is:

[0037] 1) Dissolve ammonium persulfate to prepare an ammonium persulfate solution, stir evenly, and let stand for use, which is referred to as solution A;

[0038] 2) dissolving dopamine hydrochloride to prepare a dopamine hydrochloride solution, stirring evenly and allowing to stand for use, which is designated as solution B;

[0039] 3) Mix Solution A and Solution B in a 1:1 ratio by weight, stir well, and pour into a Petri dish. Add dilute hydrochloric acid to adjust the pH to 4, and stir well again for use. This is referred to as Solution C.

[0040] 4) The polyolefin-based membrane is completely immersed in solution C, and after standing at room temperature for 36 to 60 hours, it is taken out and the excess ions on the surface are washed with deionized water to prepare a polydopamine-modified polyolefin-based membrane with good hydrophilicity, which is then vacuum-dried and stored for future use.

[0041] The growth of polydopamine on the surface of the polyolefin-based film can be regulated by adjusting the standing time. Specifically, the standing time can be 36 hours to 40 hours, 40 hours to 44 hours, 44 hours to 48 hours, 48 ​​hours to 52 hours, 52 hours to 56 hours, or 56 hours to 60 hours. Preferably, the standing time is 44 hours to 52 hours.

[0042] The polyolefin-based membrane is first modified with polydopamine, and then a portion of its pores is filled with support particles. Thanks to the hydrophilicity of the polyolefin-based membrane and the effect of surface polydopamine, the support particles can better fill the pores.

[0043] Specifically, the method for filling the support particles is as follows: immersing the polyolefin base film modified with polydopamine in a solution containing the support particles, taking it out and drying it, thereby obtaining a base film 1 in which a portion of the pores are filled with the support particles.

[0044] The modified polyolefin-based membrane is immersed in the solution containing the support particles for 18 to 30 hours. Specifically, the immersion time is 18 to 20 hours, 20 to 22 hours, 22 to 24 hours, 24 to 26 hours, 26 to 28 hours, or 28 to 30 hours. Preferably, the immersion time is 22 to 26 hours. Within this preferred immersion time, a greater number of support particles can be dispersed and filled within the pores of the polyolefin-based membrane, thereby improving the subsequent thermal shrinkage performance of the separator.

[0045] Preferably, the supporting particles also include a coupling agent, and the coupling agent is at least one of polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, and polyvinyl acetate acetal. The use of the coupling agent is increased, and it is composite-filled with inorganic particles. On the one hand, the coupling agent has a certain viscosity, which can ensure that the inorganic particles are stably filled in the pores to a certain extent without falling off; on the other hand, the coupling agent also contains a π system, and the π bond adsorption with polydopamine further ensures the reconstruction of the base film 1. Preferably, the coupling agent is polyethylene oxide. Polyethylene oxide is thermoplastic with a melting point of 87 to 140°C. When the battery is in a high temperature state, polyethylene oxide will be converted into a molten state to adhere the inorganic particles to the pores. Inorganic particles are not easy to fall off under high temperature conditions, which better ensures the stability of the base film 1.

[0046] In some embodiments, the mass ratio of the linker to the first inorganic particles is (1-5): (5-9). Specifically, the mass ratio of the linker to the first inorganic particles may be 1:9, 2:8, 3:7, 4:6 or 5:5. Preferably, the mass ratio of the linker to the first inorganic particles is (1-4): (6-9). The combination of the above mass ratios can, on the one hand, avoid the situation where the content of the linker is too low and the inorganic particles cannot be stably filled. On the other hand, it can also avoid the situation where the content of the linker is too high and the heat shrinkage resistance of the base film 1 is weakened. It is preferred that the mass proportion of the linker is lower than that of the inorganic particles, and the inorganic particles are used as the main support. On the basis of ensuring the stability of the inorganic particles, the heat shrinkage performance of the base film 1 is improved better.

[0047] In some embodiments, the diaphragm further comprises a composite layer 2, which is applied to at least one surface of the base film 1. Specifically, the composite layer 2 can be applied to one surface of the base film 1, or to two opposing surfaces of the base film 1. Preferably, the composite layer 2 is applied to two opposing surfaces of the base film 1, i.e., the structure is composite layer 2 + base film 1 + composite layer 2.

[0048] The addition of composite layer 2 further stabilizes the inorganic particles within the pores, and the multi-layer structure enhances the mechanical properties of the diaphragm, resulting in higher thermal stability. In particular, the sandwich structure of composite layer 2 + base film 1 + composite layer 2 exhibits even greater thermal stability.

[0049] In some embodiments, the composite layer 2 includes second inorganic particles, polyethylene oxide, and cellulose.

[0050] Polyethylene oxide is a crystalline, thermoplastic polymer with an ether bond as its main functional group. -1There is a clear characteristic peak at the end. In addition, the PEO end also contains a large number of hydroxyl groups, and the cellulose surface used in the present invention contains a large number of carboxyl groups, which can form hydrogen bonds with the hydroxyl groups of PEO. The two can be used in conjunction to form a tightly structured cross-linked structure. This cross-linked structure can not only lock the second inorganic particles on the surface of the base film 1, further reducing the thermal shrinkage performance of the base film 1; but also form a gel state in the electrolyte with good stability, which can hold Li + The liquid remains on both sides of the diaphragm. Experiments have also proved that the diaphragm with the composite layer 2 of the present invention has a very high liquid absorption rate and liquid retention rate.

[0051] Specifically, the polyethylene oxide is a high-molecular-weight polyethylene oxide with a molecular weight of 500,000 to 600,000. The cellulose is lignocellulose. Lignocellulose is an organic fiber material obtained from natural, renewable wood through chemical and mechanical processing. It is non-toxic, odorless, non-polluting, and non-radioactive. Lignocellulose includes at least one of coniferous lignocellulose, broadleaf lignocellulose, and herbaceous lignocellulose.

[0052] Preferably, the lignocellulose is made of coniferous lignocellulose, which has the characteristics of long fibers, tight tissue structure and low content of miscellaneous cells (miscellaneous cells in chemical pulp are mostly lost during washing), so the slurry quality is good and the mechanical properties of the finished product are strong. The coniferous lignocellulose used in the present invention is used after ball milling, and the fiber diameter after ball milling can reach 1nm and the length is 0.5~1μm. The surface of the coniferous lignocellulose after ball milling has rich hydroxyl functional groups, which is very easy to form hydrogen bonds and is easier to form a cross-linked structure with PEO. In addition, the present invention preferably uses coniferous lignocellulose in combination with PEO and inorganic particles, which can not only improve the liquid absorption rate, liquid retention rate and heat shrinkage resistance of the diaphragm, but also can use coniferous lignocellulose as a supporting layer of the diaphragm, which can better ensure the integrity of the diaphragm structure. Preferably, the mass proportion of cellulose in the composite layer 2 can be 10~50%, and the proportion within this range has a good effect on simultaneously improving the liquid absorption rate and liquid retention rate of the diaphragm, and serving as a supporting layer.

[0053] Preferably, the second inorganic particles are at least one of aluminum oxide, titanium dioxide, and silicon dioxide. The second inorganic particles can be made of the same material as the first inorganic particles, and preferably both are aluminum oxide.

[0054] In some embodiments, the weight ratio of the second inorganic particles, polyethylene oxide and cellulose is (4-8): (1-5): (1-5). By regulating the proportions of the three, the liquid absorption rate and liquid retention rate of the diaphragm can be effectively improved, and the stability of the cross-linked structure can be avoided by avoiding excessive or insufficient content of cellulose and polyethylene oxide. Experiments show that the diaphragm still has a high liquid retention rate after 48 hours. After being applied to the battery, the cycle performance of the battery is also greatly improved. Specifically, the weight ratio of the three includes but is not limited to 4:5:1, 5:4:1, 6:3:1, 7:2:1, 8:1:1, 4:4:2, 5:3:2, 6:2:2, 7:1:2, 4:3:3, 5:2:3, 6:1:3, 4:2:4, 5:1:4 or 5:5:5. Preferably, the weight ratio of the three is (4-7): (2-5): 1. More preferably, the weight ratio of the three is 4:5:1, 5:4:1, 6:3:1, 7:2:1.

[0055] The method for preparing the above-mentioned diaphragm comprises the following steps:

[0056] S1. Modifying a polyolefin-based film using polydopamine to obtain a modified polyolefin-based film;

[0057] S2. Immerse the modified polyolefin-based membrane in a solution containing supporting particles, take it out and dry it, and obtain a polyolefin-based membrane with supporting particles filled in a portion of the pores, wherein the supporting particles include first inorganic particles with a melting point greater than or equal to 200° C., thereby completing the preparation of the diaphragm.

[0058] In some embodiments, the method further includes step S3: firstly, mixing the second inorganic particles with polyethylene oxide to form a solution a, and then dissolving the cellulose to form a solution b; then stirring and mixing the solution a and solution b to obtain a composite layer slurry; applying the composite layer slurry to at least one surface of the base film, and drying to complete the preparation of the separator. The polyethylene oxide and cellulose are prepared into separate solutions and then mixed. The cross-linked structure of the mixture is more uniform and stable, which is more conducive to the Li + Trapped on both sides of the diaphragm.

[0059] Furthermore, when both the first and second inorganic particles are made of the same material and the linker is polyethylene oxide, Liquid A can also serve as a solution containing the support particles. Specifically, the modified polyolefin-based membrane can be immersed in Liquid A, removed, and dried to yield a polyolefin-based membrane with support particles filling some of its pores. Preferably, both the first and second inorganic particles are aluminum oxide, and the linker is polyethylene oxide. This provides improved compatibility between the base membrane and the composite layer, further stabilizing the overall structure of the diaphragm.

[0060] A second aspect of the present invention is to provide a secondary battery comprising a positive electrode sheet, a negative electrode sheet and a separator separated between the positive electrode sheet and the negative electrode sheet, wherein the separator is any one of the separators described above.

[0061] In some embodiments, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer coated on at least one surface of the positive electrode current collector. The positive electrode active material may be, but is not limited to, a chemical formula such as Li x Ni h Co y M z O 2-d N d (wherein 0.95≤x≤1.2, h>0, y≥0, z≥0, and h+y+z=1, 0≤d≤1, M is selected from a combination of one or more of Mn and Al, and N is selected from a combination of one or more of F, P, and S), the positive electrode active material may also be, but is not limited to, LiCoO2, LiNiO2, LiVO2, LiCrO2, LiMn2O4, LiCoMnO4, Li2NiMn3O8, LiNi 0.5 Mn 1.5 The positive electrode active material may be a combination of one or more of O4, LiCoPO4, LiMnPO4, LiFePO4, LiNiPO4, LiCoFSO4, CuS2, FeS2, MoS2, NiS, TiS2, etc. The positive electrode active material may also be subjected to a modification treatment. Methods for modifying the positive electrode active material should be known to those skilled in the art. For example, the positive electrode active material may be modified by coating, doping, etc. The materials used for the modification treatment may include, but are not limited to, a combination of one or more of Al, B, P, Zr, Si, Ti, Ge, Sn, Mg, Ce, W, etc. The positive electrode current collector may be any material suitable for use as a positive electrode current collector for lithium-ion batteries in the art. For example, the positive electrode current collector may include, but is not limited to, metal foil, and more specifically, may include, but is not limited to, aluminum foil.

[0062] The negative electrode plate includes a negative electrode current collector and a negative electrode active material layer coated on at least one surface of the negative electrode current collector. The negative electrode active material layer can be one or more of, but not limited to, graphite, soft carbon, hard carbon, carbon fiber, mesophase carbon microbeads, silicon-based materials, tin-based materials, lithium titanate, or other metals capable of forming alloys with lithium. The graphite can be selected from one or more of artificial graphite, natural graphite, and modified graphite; the silicon-based material can be selected from one or more of elemental silicon, silicon oxide compounds, silicon-carbon composites, and silicon alloys; and the tin-based material can be selected from one or more of elemental tin, tin oxide compounds, and tin alloys. The negative electrode current collector is typically a structure or component that collects current. The negative electrode current collector can be any material suitable for use as a negative electrode current collector in lithium-ion batteries. For example, the negative electrode current collector can be, but not limited to, metal foil, and more specifically, can be, but not limited to, copper foil.

[0063] The secondary battery also includes an electrolyte, which includes an organic solvent, an electrolyte lithium salt, and additives. The electrolyte lithium salt can be LiPF6 and / or LiBOB, as used in high-temperature electrolytes; can also be at least one of LiBF4, LiBOB, and LiPF6, as used in low-temperature electrolytes; can also be at least one of LiBF4, LiBOB, LiPF6, and LiTFSI, as used in overcharge-preventing electrolytes; or can be at least one of LiClO4, LiAsF6, LiCF3SO3, and LiN(CF3SO2)2. The organic solvent can be a cyclic carbonate, including PC and EC; a chain carbonate, including DFC, DMC, or EMC; or a carboxylic acid ester, including MF, MA, EA, and MP. Additives include, but are not limited to, at least one of a film-forming additive, a conductive additive, a flame retardant additive, an overcharge prevention additive, an additive for controlling the H2O and HF content in the electrolyte, an additive for improving low-temperature performance, and a multifunctional additive.

[0064] 3. Electrical devices

[0065] A third aspect of the present invention is to provide an electrical device comprising the secondary battery described above.

[0066] The electrical device may be a vehicle, mobile phone, portable device, laptop computer, ship, spacecraft, electric toy, electric tool, etc. Vehicles may be fuel-powered vehicles, gas-powered vehicles, or new energy vehicles. New energy vehicles may be pure electric vehicles, hybrid vehicles, or extended-range vehicles. Spacecraft include aircraft, rockets, space shuttles, and spacecraft. Electric toys include fixed or mobile electric toys, such as game consoles, electric car toys, electric ship toys, and electric airplane toys. Electric tools include metal cutting power tools, grinding power tools, assembly power tools, and railway power tools, such as electric drills, electric grinders, electric wrenches, electric screwdrivers, electric hammers, impact drills, concrete vibrators, and electric planers.

[0067] To make the technical solutions and advantages of the present invention more clear, the present invention and its beneficial effects will be described in further detail below with reference to specific implementation methods and accompanying drawings, but the implementation methods of the present invention are not limited thereto.

[0068] Example 1

[0069] A separator includes a base film having a plurality of pores, wherein a portion of the pores are filled with supporting particles, wherein the supporting particles include first inorganic particles having a melting point greater than or equal to 200°C.

[0070] Specifically, the base film in this embodiment is a polyolefin base film modified with polydopamine; and the supporting particles are polyethylene oxide and aluminum oxide.

[0071] The method for modifying polyolefin-based membrane with polydopamine is as follows:

[0072] 1) Weigh 57 g of ammonium persulfate into a 500 mL beaker to prepare a 0.5 mol / L ammonium persulfate solution. Stir well and let stand for use. This is referred to as Solution A.

[0073] 2) Weigh 47.4 g of dopamine hydrochloride into a 500 mL beaker to prepare a 0.5 mol / L dopamine solution. Stir thoroughly and let stand until ready to use. This is referred to as Solution B.

[0074] 3) Use a syringe to draw 200 mL each of Solution A and Solution B, stir well, and pour into a Petri dish. Add dilute hydrochloric acid to adjust the pH to 4, stir well again, and set aside. This is called Solution C.

[0075] 4) Cut a polyethylene film of a certain size of 20*20 cm, clamp it with a dovetail clip and completely immerse it in solution C. After standing at room temperature for 48 hours, take it out and wash the excess ions on the surface with deionized water to prepare a polydopamine-modified polyolefin film with good hydrophilicity. Dry it in a vacuum at 45°C and store it for later use.

[0076] The preparation method of the diaphragm is as follows:

[0077] S1. Preparation of a solution containing supported particles: First, weigh 0.6 g of polyethylene oxide (PEO) and pour it into a beaker. Then weigh 1.4 g of Al2O3 powder and add 100 mL of deionized water to prepare a 20 mg / mL PEO / Al2O3 slurry, which is referred to as solution a.

[0078] S2. Take a culture dish with a diameter of 20 cm, use a syringe to draw 20 mL of liquid a and pour it into it, immerse the polyolefin-based membrane modified with polydopamine in liquid a. The modified polyolefin-based membrane has good hydrophilicity and good compatibility with PEO / Al2O3 slurry. After immersion for 24 hours, PEO / Al2O3 can fill part of the pores of the polyolefin-based membrane. Take it out, wipe off the surface floating liquid, and dry it in a vacuum drying oven at 45°C for use, completing the preparation of the diaphragm.

[0079] Example 2

[0080] The difference from Example 1 is the composition of the supporting particles, where the mass ratio of PEO to Al2O3 is 1:9.

[0081] The rest is the same as in Example 1 and will not be described again here.

[0082] Example 3

[0083] The difference from Example 1 is the composition of the supporting particles, where the mass ratio of PEO to Al2O3 is 5:5.

[0084] The rest is the same as in Example 1 and will not be described again here.

[0085] Example 4

[0086] The difference from Example 1 is the composition of the supporting particles. The supporting particles in this embodiment are PEO and SiO2.

[0087] The rest is the same as in Example 1 and will not be described again here.

[0088] Example 5

[0089] The difference from Example 1 is the composition of the supporting particles. The supporting particles in this embodiment are PEO and TiO2.

[0090] The rest is the same as in Example 1 and will not be described again here.

[0091] Example 6

[0092] Different from Example 1, the separator of this embodiment further comprises a composite layer coated on one surface of the base membrane, and the composite layer comprises aluminum oxide, polyethylene oxide and coniferous wood cellulose.

[0093] The preparation method of the diaphragm is as follows:

[0094] S1. Preparation of a solution containing supported particles: First, weigh 0.6 g of polyethylene oxide (PEO) and pour it into a beaker. Then weigh 1.4 g of Al2O3 powder and add 100 mL of deionized water to prepare a 20 mg / mL PEO / Al2O3 slurry, which is referred to as solution a.

[0095] S2. Take a culture dish with a diameter of 20 cm, draw 20 mL of liquid a into it with a syringe, immerse the polyolefin-based membrane modified with polydopamine in liquid a. The modified polyolefin-based membrane has good hydrophilicity and good compatibility with the PEO / Al2O3 slurry. After immersion for 24 hours, PEO / Al2O3 can be filled in part of the pores of the polyolefin-based membrane. Take it out, wipe off the surface floating liquid, and dry it in a vacuum drying oven at 45°C for later use.

[0096] S3. Preparation of cellulose slurry: First, weigh 2 g of cellulose and place it in a ball mill. Add 100 mL of deionized water and ball mill at a ball-to-material ratio of 50:1 at a speed of 1032 r / min for 1 h. Collect the slurry and set aside. This is referred to as liquid b.

[0097] S4. Preparation of composite layer slurry: Use a syringe to draw 2 mL of liquid b and 18 mL of liquid a into a 100 mL beaker and stir evenly to obtain composite layer slurry;

[0098] S5. Take the composite layer slurry and apply it on one surface of the base film prepared in step S2 to a coating thickness of 1 to 2 μm. Dry it at 60° C. to prepare the diaphragm of this embodiment.

[0099] The rest is the same as in Example 1 and will not be described again here.

[0100] Example 7

[0101] Different from Example 6, the composite layer of this embodiment is coated on two opposite surfaces of the base film, that is, the structure is composite layer + base film + composite layer.

[0102] The rest is the same as in Example 6 and will not be described again here.

[0103] Example 8

[0104] The difference from Example 7 is the composition of the composite layer.

[0105] In the composite layer of this embodiment, the weight proportions of aluminum oxide, polyethylene oxide and coniferous wood cellulose are 8 parts, 1 part and 1 part respectively.

[0106] The rest is the same as in Example 7 and will not be described again here.

[0107] Example 9

[0108] The difference from Example 7 is the composition of the composite layer.

[0109] In the composite layer of this embodiment, the weight proportions of aluminum oxide, polyethylene oxide and coniferous wood cellulose are 7 parts, 2 parts and 1 part respectively.

[0110] The rest is the same as in Example 7 and will not be described again here.

[0111] Example 10

[0112] The difference from Example 7 is the composition of the composite layer.

[0113] The weight proportions of aluminum oxide, polyethylene oxide and coniferous wood cellulose in the composite layer of this embodiment are 5 parts, 4 parts and 1 part respectively.

[0114] The rest is the same as in Example 7 and will not be described again here.

[0115] Example 11

[0116] The difference from Example 7 is the composition of the composite layer.

[0117] In the composite layer of this embodiment, the weight proportions of aluminum oxide, polyethylene oxide and coniferous wood cellulose are 4 parts, 5 parts and 1 part respectively.

[0118] The rest is the same as in Example 7 and will not be described again here.

[0119] Example 12

[0120] The difference from Example 7 is the composition of the composite layer.

[0121] The composite layer of this embodiment is composed of silicon dioxide, polyethylene oxide and coniferous wood cellulose.

[0122] The rest is the same as in Example 7 and will not be described again here.

[0123] Example 13

[0124] The difference from Example 7 is the composition of the composite layer.

[0125] The composite layer of this embodiment is composed of titanium dioxide, polyethylene oxide and coniferous wood cellulose.

[0126] The rest is the same as in Example 7 and will not be described again here.

[0127] Example 14

[0128] The difference from Example 7 is the composition of the composite layer.

[0129] The composite layer of this embodiment is composed of aluminum oxide and polyethylene oxide, wherein the weight portion of aluminum oxide is 7 parts and the weight portion of polyethylene oxide is 3 parts.

[0130] The difference from Example 7 is the composition of the composite layer.

[0131] Example 15

[0132] The difference from Example 7 is the composition of the composite layer.

[0133] The composite layer of this embodiment is composed of aluminum oxide and coniferous wood cellulose, wherein the weight portion of aluminum oxide is 7 parts and the weight portion of coniferous wood cellulose is 1 part.

[0134] The difference from Example 7 is the composition of the composite layer.

[0135] Example 16

[0136] The difference from Example 7 is the composition of the composite layer.

[0137] The composite layer of this embodiment is composed of polyethylene oxide and coniferous wood cellulose, wherein the weight portion of polyethylene oxide is 3 parts and the weight portion of coniferous wood cellulose is 1 part.

[0138] The difference from Example 7 is the composition of the composite layer.

[0139] Comparative Example 1

[0140] This comparative example is a common untreated polyethylene film.

[0141] Comparative Example 2

[0142] A diaphragm comprises a base film and a composite layer coated on two opposite surfaces of the base film, wherein the base film is an untreated polyethylene film and the composite layer is a conventional PVDF / Al2O3 ceramic coating.

[0143] The separators obtained in Examples 1 to 16 and Comparative Examples 1 to 2 were tested for their heat shrinkage at 130° C. and liquid holdup.

[0144] Liquid retention test: Cut discs of the same size, weigh them once, soak them in electrolyte for 0.5 hours, wipe off any surface liquid, and weigh them again to obtain liquid absorption data. The discs were then left at room temperature for 1 hour, 2 hours, 4 hours, 8 hours, 24 hours, and 48 hours, and their liquid retention data were measured. While the liquid absorption data is not listed in Table 1, the 1-hour liquid retention data can be referenced, as they are similar.

[0145] The test results are shown in Table 1 and Figure 3 below.

[0146] Table 1

[0147] A comparison of the results of Examples 1-5 and Comparative Examples 1-2 shows that the present invention, by reconstructing the polyolefin separator and introducing inorganic particles into a portion of the pores of the polyolefin separator, effectively reduces the thermal shrinkage of the polyolefin separator at a high temperature of 130°C. The comparison of Examples 1-5 also shows that different mass ratios of the linking agent to the inorganic particles have different effects on the improvement of thermal shrinkage. This is mainly because, if the linking agent content is relatively low, the inorganic particles are relatively easy to fall off, and the stability of the separator at high temperatures cannot be better supported. Conversely, if the linking agent content is high, the proportion of inorganic particles is reduced, and of course, the stability of the separator at high temperatures cannot be better supported.

[0148] In addition, it can be seen from the comparison of the results of Examples 1 to 5 and Examples 6 to 14 that adding the composite layer of the present invention to the surface of the base film can effectively enhance the liquid absorption rate and liquid retention rate of the separator. This is mainly because the cross-linked structure formed in the composite layer can + It is retained on both sides of the diaphragm, which improves the liquid absorption rate and liquid retention rate of the diaphragm and ensures the cycle performance of the battery.

[0149] Furthermore, a comparison of the results from Examples 7 to 14 also demonstrates that the different compositions and contents of the composite layer also have a certain impact on the thermal shrinkage, liquid absorption rate, and liquid holdup of the separator. In particular, in Example 7, when the aluminum oxide, polyethylene oxide, and cellulose are simultaneously adjusted to the optimal ratio, the thermal shrinkage, liquid absorption rate, and liquid holdup of the separator are significantly improved compared to the conventional PVDF / Al2O3 ceramic separator in Comparative Example 2.

[0150] The separators obtained in Example 7 and Comparative Example 2 were sliced ​​into 19 mm discs using a slicer and applied to button batteries. The conventional preparation method is referred to and will not be described in detail here.

[0151] Testing the cycle performance of the button battery: At 25°C, the button battery was charged at 1C and discharged at 1C rate, and a full charge and discharge cycle test was performed. The test results are shown in Figure 4.

[0152] As can be seen from Figure 4, compared with the conventional PVDF / Al2O3 ceramic diaphragm in Comparative Example 2, the button battery in Example 7 of the present invention still has a relatively high cycle capacity retention rate of up to 93% after 600 cycles. It can be seen that the present invention also effectively improves the battery cycle stability.

[0153] In summary, the present invention can effectively improve the thermal shrinkage, liquid absorption rate and liquid retention rate of the diaphragm by reconstructing the base membrane structure and then coordinating the setting of the composite layer, which not only ensures the safety of the battery but also improves the cycle stability of the battery.

[0154] Based on the disclosure and teachings of the above description, those skilled in the art will be able to make changes and modifications to the above embodiments. Therefore, the present invention is not limited to the above specific embodiments. Any obvious improvements, substitutions, or modifications made by those skilled in the art based on the present invention fall within the scope of protection of the present invention. In addition, although certain specific terms are used in this description, these terms are only for convenience of description and do not constitute any limitation to the present invention.

Claims

1. A diaphragm, It is characterized in that The invention comprises a base film having a plurality of pores, wherein a part of the pores are filled with supporting particles, and the supporting particles comprise first inorganic particles having a melting point greater than or equal to 200°C.

2. The diaphragm according to claim 1, It is characterized in that The base film is a polyolefin base film modified by polydopamine.

3. The diaphragm according to claim 2, It is characterized in that The method for modifying a polyolefin base membrane with polydopamine is as follows: immersing the polyolefin base membrane in a polydopamine solution, taking it out after standing, and drying it to obtain the modified polyolefin base membrane; the method for filling supporting particles is as follows: immersing the polyolefin base membrane modified with polydopamine in a solution containing supporting particles, taking it out and drying it to obtain a base membrane with supporting particles filled in some pores.

4. The diaphragm according to any one of claims 1 to 3, It is characterized in that The supporting particles further include a coupling agent, and the mass ratio of the coupling agent to the first inorganic particles is (1-5):(5-9).

5. The diaphragm according to claim 4, It is characterized in that The coupling agent is at least one of polyethylene oxide, polyvinyl alcohol, polyvinyl pyrrolidone, and polyvinyl acetate acetal; the first inorganic particles are at least one of aluminum oxide, titanium dioxide, and silicon dioxide.

6. The diaphragm according to claim 1, It is characterized in that It also includes a composite layer coated on at least one surface of the base film.

7. The diaphragm according to claim 6, It is characterized in that The composite layer comprises second inorganic particles, polyethylene oxide and cellulose, and the weight ratio of the second inorganic particles, polyethylene oxide and cellulose is (4-8): (1-5): (1-5).

8. The diaphragm according to claim 7, It is characterized in that The second inorganic particles are at least one of aluminum oxide, titanium dioxide, and silicon dioxide; the molecular weight of the polyethylene oxide is 500,000 to 600,000; the cellulose includes at least one of coniferous wood cellulose, broadleaf wood cellulose, and herbaceous wood cellulose; preferably, the preparation method of the composite layer is: first, the second inorganic particles and polyethylene oxide are mixed into a solution to prepare liquid a, and the cellulose is dissolved to prepare liquid b; then, liquid a and liquid b are stirred and mixed to obtain a composite layer slurry; the composite layer slurry is coated on at least one surface of the base film and dried.

9. A secondary battery, comprising a positive electrode sheet, a negative electrode sheet and a separator between the positive electrode sheet and the negative electrode sheet, It is characterized in that The separator is the separator according to any one of claims 1 to 8.

10. An electrical device, It is characterized in that A secondary battery comprising the secondary battery according to claim 9.

Citation Information

Patent Citations

  • Nonwoven material with particle filler

    CN101960646A

  • Heat shrinkage resistant organic / inorganic composite lithium battery diaphragm and preparation method thereof

    CN110690388A

  • Diaphragm, preparation method thereof and secondary battery

    CN114552122A

  • Oil-based composite diaphragm, preparation method thereof and secondary battery

    CN114865222A

  • Diaphragm, and secondary battery and electric device comprising same

    CN116613470A