Cool fabric

By using nano-grade cool-sensing microcapsules and inorganic particles in textiles, the problem of easy shedding and insufficient adsorption in existing textiles is solved, and an efficient and long-lasting cool-sensing effect is achieved.

CN119020988APending Publication Date: 2024-11-26TORAY FIBER RES INST(CHINA) CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310601336.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-25
Publication Date
2024-11-26

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a cool fabric. Inorganic particles are contained in fibers forming the fabric, and the inorganic particles and cool nano microcapsules are attached to the surfaces of the fibers. The processing method of the fabric is simple and easy to implement, and the fabric has excellent cool feeling performance and high washing durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of textiles, and in particular relates to a cool fabric. Background Art

[0002] With the improvement of living standards, people's pursuit of quality of life is becoming more and more obvious, especially the comfort and functionality of textiles. With the warming of the earth, hot summer days are often accompanied by humidity, sweating and other conditions. People have a great demand for cool and comfortable functional clothing, especially outdoors. People hope that their body temperature can always be kept in a cool and comfortable range. More and more clothing on the market is endowed with cooling functions. Among them, post-finishing has become one of the important ways to increase the added value of product cooling and improve its function.

[0003] For example, Chinese patent document CN115074996A discloses a fiber fabric with a cool feeling, which specifically discloses that the fiber fabric includes a base fiber material, a phase change material and a cool feeling promoter, the phase change material and / or the cool feeling promoter are combined with the base fiber material by padding and modified along with the base fiber material, the phase change material is a microcapsule, and the skin in contact with the fabric and the fiber surface is made cool and refreshing by an endothermic reaction, thereby obtaining a fiber fabric with a cool feeling. However, the microcapsules obtained by this method have a large particle size, are easy to fall off during washing, and have poor durability; and in a unit area, due to the small number of adsorbed particles, the area of ​​particle exposure is also small, and the cool feeling needs to be further improved.

[0004] For another example, Chinese patent document CN113152108A discloses a cool aramid fabric, which specifically discloses that the cool aramid fabric includes the following raw materials in parts by weight: 50-100 parts of aramid fiber, 3-8 parts of xylitol cool finishing agent, 5-8 parts of cool microcapsules, 0.6-1 part of cross-linking agent and 0.4-0.8 part of functional additive. The xylitol cool finishing agent and the cool microcapsules are compounded and acted on the fabric to obtain the cool aramid fabric. However, the cool microcapsules used are PCM-COOL produced by Changzhou Hans Chemical Co., Ltd., with an average particle size of 1-50 microns, which also has the problem of easy falling off after washing and poor durability.

[0005] For another example, Chinese patent document CN102720054A discloses an anti-ultraviolet cold feeling finished fabric, which specifically discloses that a polyurethane adhesive and silica-coated dodecanol microcapsules are finished on the fabric together using a padding process, and the particle size of the silica-coated dodecanol microcapsules is 0.2 to 6 μm. However, the polyurethane adhesive used in this method will have a certain impact on the hand feel and the comfort is not good. Summary of the invention

[0006] The purpose of the present invention is to provide a cool feeling fabric with good hand feeling, extremely superior cool feeling and long-lasting cool feeling.

[0007] The technical solution of the present invention is: The cooling fabric of the present invention comprises inorganic particles inside the fibers forming the cooling fabric, and inorganic particles and cooling nano-microcapsules are attached to the surface.

[0008] The present invention increases the adsorption amount of the cool microcapsules per unit area by using nano-scale cool microcapsules, effectively improves the cool effect, and has strong adsorption force, is not easy to fall off even after multiple washings, and has a long-lasting cool effect; in addition, the inorganic particles present inside and on the surface of the fiber can reflect infrared rays, reduce the heat absorption of the fabric, play a role in reflecting heat energy, and further improve the cool feeling. The cool fabric of the present invention can be used to make clothes, bedding, socks, etc. DETAILED DESCRIPTION

[0009] The cooling fabric of the present invention comprises fibers which contain inorganic particles inside and inorganic particles and cooling nano-microcapsules attached to the surface of the fibers.

[0010] The cooling nano-microcapsules in the present invention refer to nano-scale microcapsules containing certain cooling substances. The particle size of conventional microcapsules is generally between 5 and 2000 microns, while the particle size of nano-microcapsules is small, which can reach 1 to 1000 nm. The smaller the particle size, the better the dispersibility, the stronger the ability to penetrate into the pores between fibers, and the larger the surface area, the stronger the sustained release, and the effective extension of the cooling effect time, which will not affect the physical and mechanical properties of the fabric. However, considering the preparation process and cost, the average particle size of the cooling nano-microcapsules in the present invention is preferably 250 to 400 nm.

[0011] The inorganic particles herein are not particularly limited in type, and examples thereof include titanium dioxide, calcium carbonate, barium sulfate, zinc oxide, silicon dioxide, boron nitride, etc. Among them, one or more of titanium dioxide, calcium carbonate, barium sulfate and zinc oxide are preferred, as these particles can effectively reflect direct sunlight and have stable performance, thereby achieving the purpose of sustained cooling.

[0012] When the infrared rays in the solar radiation energy are absorbed by the fabric, the surface temperature of the fabric will rise rapidly. The inorganic particles have a good reflection effect on infrared rays. When their infrared reflectivity is greater than 20%, a reflective cooling effect can be obtained. Therefore, in the present invention, the inorganic particles are preferably particles with an infrared reflectivity greater than 20%.

[0013] If the average particle size of the inorganic particles is too large, the filter screen in the spinning assembly may be blocked during the spinning process, causing the assembly pressure to rise rapidly, affecting productivity. Therefore, the average particle size of the inorganic particles in the present invention is preferably less than 1.5 μm, more preferably less than 1.0 μm.

[0014] In the present invention, if the content of inorganic particles is higher than 30.0wt%, floating and broken fibers may occur during the spinning process; if the content of inorganic particles is lower than 5.0wt%, although there is no problem in spinning, the reflective cooling effect tends to decrease. Therefore, in the present invention, the content of inorganic particles is preferably 5.0-30.0wt%.

[0015] The cooling nano-microcapsules of the present invention include a wall material and a core material. The core material is not particularly limited, and examples thereof include alcohol compounds, aromatic compounds, hydrolyzates of glycoside compounds, amide compounds, ester compounds, ketone compounds, terpene oxides (such as eucalyptol, etc.), silk protein with moisture absorption and heat dissipation function, and ultra-high molecular weight polyethylene.

[0016] Examples of alcohol compounds include 2-isopropyl-5-methylcyclohexanol, menthyloxy-1,2-propanediol, 3-(1-methoxy)-2-methyl-1,2-propanediol, 5-methyl-2-(1-methylvinyl)cyclohexanol, methoxypropanediol, 5-methyl-2-isopropylcyclohexanol, pentanol, (R,S)-1,2,3,4-butanetetrol, cis- and trans-p-menthyl-3,8-diol, p-menthyl-3,8-diol, (2S)-3-(1-menthyloxy)propane-1,2-diol, (2R)-3-(1-methoxy)propane-1,2-diol, and (2RS)-3-(1-methoxy)propane-1,2-diol.

[0017] Amide compounds include: N-ethyl-5-methyl-2-(1-methylethyl)cyclohexanecarboxamide, N-ethyl-2-isopropyl-5-methylcyclohexylcarboxamide, N-ethyl-p-menthyl-3-carboxamide, N-2,3-trimethyl-2-isopropylbutyramide, 2-isopropyl-N,2,3-trimethylbutyramide, N-tert-butyl-p-menthyl-3-carboxamide, N-(4-methoxyphenyl)-p-menthyl-3-carboxamide, N-ethyl-p-menthyl-3-carboxamide, etc.

[0018] Examples of the ester compounds include 1-isopropyl-4-methylcyclohexyl-2-ol acetate, 2-hydroxypropionic acid 5-methyl-2-isopropylcyclohexyl ester, 5-methyl-2-(1-methylethyl)-cyclohexyl monosuccinate, (N-ethyl-p-menthyl-3-carboxamide) ethyl acetate, (1R,3R,4S)-3-menthyl 3,6-oxaheptanoate, (1R,2S,5R)-menthyl methoxyacetate, (1R,2S,5R)-3-menthyl 3,6,9-trioxadecanoate, (1R,2S,5R)-3-menthyl (2-hydroxyethoxy)acetate, p-menthyl-3-hydroxy acid-1-glyceride, p-menthyl-3-hydroxy acid-1-vinylglyceride, and 11-hydroxy-3,6,9-trioxaundecanoic acid-(1R,2S,5R)-menthyl ester.

[0019] Examples of ketone compounds include 1,7,7-trimethylbicyclo[2.2.1]heptane-2-one, menthone glycerol ketal, 4-methyl-3-(1-pyrrolidinyl)-2[5H]-furanone, 5-methyl-4-(1-pyrrolidinyl)-3-[2H]-furanone, 4,5-dimethyl-3-(1-pyrrolidinyl)-2[5H]-furanone, 4-methyl-3-(1-pyrrolidinyl)-2[5H]-furanone, and 3,3,5-trimethylcyclohexanone glycerol ketal.

[0020] Among them, the core material is preferably one or more of 5-methyl-2-isopropylcyclohexanol, pentaerythritol, (R,S)-1,2,3,4-butanetetrol and eucalyptol. These substances can effectively stimulate TRPM8 receptors distributed in the skin, reduce the temperature of the human body surface, and make the human body feel obviously cool.

[0021] The wall material of the cooling nano-microcapsules in the present invention contains a component that can be chemically cross-linked and grafted. The chemically cross-linked and grafted component is not particularly limited, and is preferably a polymer with a high degree of cross-linking, such as acrylic acid, acrylonitrile, methyl methacrylate, acrylamide, styrene, vinyl acetate, isoprene, etc. In the present invention, the cooling nano-microcapsules are firmly attached to the fibers through a chemical bond connection formed by a cross-linking reaction between the chemically cross-linked and grafted component in the wall material and the fibers.

[0022] The cooling nano-microcapsules in the present invention can be a core-wall single-layer structure or a multilayer structure of two or more layers with (core-wall) n cycles. In order to maintain the stability of the long-lasting cooling performance, a multilayer structure of two or more layers is preferred, for example, a three-layer cycle structure of core-wall-core-wall-core-wall.

[0023] The fabric of the present invention, its fiber raw material can be natural fibers such as cotton, wool, silk, hemp, etc., can also be regenerated fibers such as viscose, cuprammonium, acetate, etc., can also be synthetic fibers such as polyester, nylon, acrylic, spandex, vinylon, aramid, etc. Wherein, fibers such as cotton and viscose have a large amount of hydroxyl groups, which can directly react with groups such as carboxyl, epoxy, carbonyl, acid amine in the nano cooling microcapsule wall material. If there is no reactive group on the molecular main chain or side chain of the fiber, it is considered to first perform surface modification treatment, and then treat with nano cooling microcapsules. For example, aramid fiber needs to be modified first, and then react with nano cooling microcapsules to improve wash resistance, so that the fabric has long-term and efficient cooling performance. Aramid fiber modification can be carried out by known physical methods or chemical methods. Among them, the physical modification method is to clean the fiber surface through physical techniques such as plasma and electron beam, and introduce polar or active groups such as hydroxyl and carbonyl groups on the fiber surface; it can also form some active centers on the fiber surface, thereby initiating a grafting reaction, improving the physical and chemical state of the fiber surface, and thus strengthening the interaction between the fiber and the matrix. Chemical modification is to introduce active or polar groups such as amino, hydroxyl, and carboxyl groups on the fiber surface through chemical reactions such as nitration reduction reaction and chlorosulfonation.

[0024] In the present invention, when the content of the cooling nano microcapsules is less than 5.0wt%, the cooling feeling of the fabric tends to decrease; as the content of the cooling nano microcapsules increases, the cooling feeling of the fabric also increases, but when the content of the cooling nano microcapsules is greater than 15.0wt%, the cooling effect reaches saturation, and excessive microcapsules are prone to agglomeration, which may affect other properties of the fabric. Therefore, preferably, the content of the cooling nano microcapsules in the present invention is 5.0-15.0wt%, and more preferably 6.0-12.0wt%.

[0025] As a preferred embodiment, the contact cooling Q-Max value of the fabric of the present invention is measured according to the GB / T 35263-2017 textile instantaneous cooling test standard, and the initial and after washing 50 times are both within 0.15 J / (cm 2 •s) and above.

[0026] The fabric of the present invention can be a woven fabric or a knitted fabric, without particular limitation, and can be used to make clothes, bedding, socks, etc., wherein the clothes can be underwear, shirts, mountaineering clothes, casual clothes, golf clothes, etc.

[0027] The manufacturing method of the fabric of the present invention is not particularly limited, and can be obtained by the following method: selecting a grey cloth containing inorganic particles in the fiber, and subjecting the grey cloth to scouring and post-finishing processing to obtain a product. In the post-finishing processing, a cooling nano-microcapsule dispersion and a solution containing inorganic particles are used for processing, and the amount of the cooling nano-microcapsule dispersion is preferably 40 to 80% by weight; the amount of the solution containing inorganic particles is preferably 30 to 60% by weight.

[0028] The post-finishing process can be a bath treatment or a padding process, preferably a padding process. The padding process can be one dip and one padding, or two dips and two paddings, preferably one dip and one padding. The specific conditions of the bath treatment are as follows: heat treatment at a temperature of 40 to 60°C for 30 to 60 minutes, followed by drying at a temperature of 110 to 130°C.

[0029] As long as the purpose of the present invention is not affected, the fibers may contain dyes and various dyeing auxiliaries as required for coloring.

[0030] The present invention will be further described below with reference to the embodiments and comparative examples.

[0031] The physical parameters of the present invention are measured according to the following method: (1) Inorganic particle content and infrared reflectivity ① First, boil the crucible with hydrochloric acid (1:4) for 1 to 2 hours, wash and dry it; place it in a high-temperature furnace at 500-550℃ and burn it for 1 hour, move it to the furnace mouth and cool it to about 200℃, then move it into a dryer, cool it to room temperature, and weigh it accurately; then place the cooled crucible in a high-temperature furnace and burn it for 30 minutes, take it out and cool it and weigh it until the constant weight is recorded as m1 (the difference between the two weighings does not exceed 0.5mg. If it exceeds 0.5mg, continue to place it in the high-temperature furnace and burn it). Among them, the division value of the analytical balance is 0.0001g / division; ② Weigh 10g of fabric (cut it into small pieces as much as possible), then put it into a crucible and weigh it accurately and record it as m2; ③ First, heat the crucible with a low fire in an electric furnace to fully carbonize the sample until it is smokeless, then place it in a high-temperature furnace for 4 hours, take out the crucible and wait for it to cool to below 200°C, then place it in a dryer for 40 minutes to cool to room temperature, weigh and record. Place it in the high-temperature furnace again and continue to burn for 30 minutes, take it out, cool it and weigh it as m3 (the difference between the two weighings should not exceed 0.5 mg. If it exceeds 0.5 mg, continue to place it in the high-temperature furnace to burn). Then calculate the proportion of residual ash as the content of inorganic particles in the fabric according to the following formula. The calculation formula is as follows: Ash content (%) = [(m3-m1) / (m2-m1)] × 100% Where: m1 is the mass of the empty crucible (g) m2 is the mass of the sample plus the empty crucible (g) m3 is the mass of residual ash plus empty crucible (g) ④ Repeat the above steps ① to ③, measure 3 groups of samples in total, and take the average value of the 3 groups of data as the content of the inorganic particles in the present invention; ⑤ Use Lambda-950 UV-Vis-NIR spectrophotometer to test the near-infrared reflectivity of inorganic particles in the residual ash, with a scanning range of 760-2500nm. Calculate the infrared reflectivity of inorganic particles (the reflectivity ratio of near-infrared solar radiation of inorganic particles) according to the following formula:

[0032] In the formula, R s is the infrared reflectivity of the inorganic particles (%), λ is the spectral wavelength (nm), R(λ) is the reflectance of the sample when the wavelength is λ (%), E λ It is the solar spectrum irradiance, with a wavelength range of 760 to 2500nm.

[0033] (2) Average particle size of inorganic particles A 5cm*5cm fabric was cut as a sample, and the cross section of the sample was observed at 3000 times using a scanning electron microscope (SEM). Ten inorganic particles were randomly selected on the cross section and the particle size of each particle was obtained using the measurement software provided by the SEM. Using the same method, a total of 5 cross sections were measured for each inorganic particle to obtain 50 sets of data, and the average value was taken as the average particle size of the inorganic particles of the present invention.

[0034] (3) Content of Cooling Nanocapsules Weigh 5 g of fabric, dissolve the fibers with 100 mL of solvent (such as formic acid for polyamide fibers and hexafluoroisopropanol for polyester fibers), filter and dry, weigh the dried material, and calculate the content, which is the total content of inorganic particles and microcapsules. Then, subtract the content of inorganic particles in (1) from the total content to obtain the content of cool nano-microcapsules.

[0035] (4) Average particle size of cooling nanocapsules A piece of smooth, color-free and defect-free sample cloth was cut from the fabric, and then a 0.5 cm*0.5 cm sample was prepared. After gold spraying, it was placed on a JSM-6360LA electron microscope scanner test platform produced by JEOL of Japan for scanning and observation. Ten different cooling nano-microcapsules were selected within the field of view, and the particle size of each nano-microcapsule was measured 5 times to obtain 50 sets of data, and the average value was taken as the average particle size of the cooling nano-microcapsules of the present invention.

[0036] (5) Q-Max value Place the fabric in a humidified environment at 20±2℃ and 65±4%RH for more than 24 hours. Cut 5 samples of 10cm*10cm in size according to the trapezoidal sampling method, avoid wrinkles and defects, use KES-F7 thermal energy meter, set △T to 15℃, measure its Q-max value, and measure 5 sets of data to take the average value.

[0037] (6) Washing method According to GB 8629-2001 washing standard.

[0038] Embodiment 01: A plain knitted fabric formed by a core-sheath structure PET composite fiber of 75D / 36f (the content of titanium dioxide particles is 7% by weight, the infrared reflectivity is 25%, and the average particle size is 1.0 μm) is selected. The fabric is refined and then subjected to post-finishing processing to obtain the cool fabric of the present invention. The test results of various properties are shown in Table 1.

[0039] Among them, in the post-finishing process, 10% by weight of a cool nano-microcapsule dispersion (core material: 5-methyl-2-isopropylcyclohexanol, wall material: chitosan, number of core and wall material circulation layers: 3, average particle size 280nm) and 6% by weight of a solution containing titanium dioxide particles (infrared reflectivity 25%, average particle size 1.0μm) were used for a dip-rolling process, and then heat treated at a temperature of 130°C for 3 minutes.

[0040] Embodiment 02: A plain knitted fabric formed by a core-sheath structure PET composite fiber of 75D / 36f (the content of titanium dioxide particles is 25% by weight, the infrared reflectivity is 25%, and the average particle size is 1.0 μm) is selected, and in the post-finishing process, 12% by weight of a dispersion of cool nano-microcapsules (core material: 5-methyl-2-isopropyl cyclohexanol, wall material: chitosan, number of core and wall material circulation layers: 3, average particle size 280 nm) and 10% by weight of a solution containing titanium dioxide particles (infrared reflectivity is 25%, average particle size is 1.0 μm) are added, and the rest is the same as in Example 01 to obtain a cool fabric of the present invention, and the test results of various properties thereof are shown in Table 1.

[0041] Embodiment 03: In the cooling nano-microcapsule dispersion in the post-finishing process, the 5-methyl-2-isopropylcyclohexanol core material with an average particle size of 280 nm is replaced by a 5-methyl-2-isopropylcyclohexanol core material with an average particle size of 150 nm, and the rest is the same as in Example 2 to obtain the cooling fabric of the present invention. The test results of various properties are shown in Table 1.

[0042] Embodiment 04: In the cooling nano-microcapsule dispersion in the post-finishing process, the 5-methyl-2-isopropylcyclohexanol core material with an average particle size of 280 nm is replaced by a 5-methyl-2-isopropylcyclohexanol core material with an average particle size of 400 nm, and the rest is the same as in Example 2 to obtain the cooling fabric of the present invention. The test results of various properties are shown in Table 1.

[0043] Embodiment 05: In the cooling nano-microcapsule dispersion in the post-finishing process, the 5-methyl-2-isopropylcyclohexanol core material with an average particle size of 280 nm is replaced by a 5-methyl-2-isopropylcyclohexanol core material with an average particle size of 500 nm, and the rest is the same as in Example 2 to obtain the cooling fabric of the present invention. The test results of various properties are shown in Table 1.

[0044] Embodiment 06: In the post-finishing process, the cooling nano-microcapsules whose core material is 5-methyl-2-isopropylcyclohexanol are replaced by cooling nano-microcapsules whose core material is (R, S)-1,2,3,4-butanetetrol, and the rest are the same as in Example 02, to obtain the cooling fabric of the present invention, and the test results of various properties thereof are shown in Table 1.

[0045] Embodiment 07: In the post-finishing process, the cooling nano-microcapsules whose core material is 5-methyl-2-isopropylcyclohexanol are replaced by cooling nano-microcapsules whose core material is pentapentanol, and the rest are the same as in Example 02, to obtain the cooling fabric of the present invention, and the test results of various properties thereof are shown in Table 1.

[0046] Embodiment 08: In the post-finishing process, the cooling nano-microcapsules whose core material is 5-methyl-2-isopropylcyclohexanol are replaced by cooling nano-microcapsules whose core material is eucalyptol, and the rest are the same as in Example 02, to obtain the cooling fabric of the present invention, and the test results of various properties thereof are shown in Table 1.

[0047] Embodiment 09: The 75D / 36f core-sheath structure PET composite fiber and the titanium dioxide particles in the post-finishing process are replaced with zinc oxide particles, and the rest is the same as in Example 02 to obtain the cool feeling fabric of the present invention. The test results of various properties are shown in Table 1.

[0048] Embodiment 10: The 75D / 36f core-sheath structure PET composite fiber and the titanium dioxide particles with a reflectivity of 25% in the post-finishing process are replaced with titanium dioxide particles with a reflectivity of 15%, and the rest is the same as in Example 02 to obtain the cool fabric of the present invention. The test results of various properties are shown in Table 1.

[0049] Embodiment 11: The 75D / 36f core-sheath structure PET composite fiber and the titanium dioxide particles with a reflectivity of 25% in the post-finishing process are replaced with titanium dioxide particles with a reflectivity of 35%, and the rest is the same as in Example 02 to obtain the cool fabric of the present invention. The test results of various properties are shown in Table 1.

[0050] Embodiment 12: In the post-finishing process, the solution of titanium dioxide particles with an average particle size of 1.00 μm is replaced by a solution of titanium dioxide particles with an average particle size of 1.8 μm, and the rest is the same as in Example 02 to obtain the cool fabric of the present invention. The test results of various properties are shown in Table 1.

[0051] Embodiment 13: The cooling nano-microcapsules with 3 core-wall material circulation layers were replaced with cooling nano-microcapsules with 1 core-wall material circulation layer, and the rest was the same as in Example 02 to obtain the cooling fabric of the present invention. The test results of various properties are shown in Table 1.

[0052] Clothes, bedding, socks, etc. made from the cool fabrics of Examples 01 to 13.

[0053] Comparative Example 01: No cool nano-microcapsule dispersion was used in the post-finishing process, and the rest was the same as in Example 02 to obtain a fabric. The test results of various properties are shown in Table 1.

[0054] Table 1

[0055] According to Table 1, (1) It can be seen from Examples 2 and 3 that, under the same conditions, the Q-max of the fabric with an average particle size of 280 nm of cooling nano-microcapsules is higher before and after washing than that of the fabric with an average particle size of 150 nm of cooling nano-microcapsules, and the Q-max of the former is higher than that of the latter after washing.

[0056] (2) It can be seen from Examples 4 and 5 that, under the same conditions, the Q-max of the fabric with an average particle size of 400 nm of cooling nano-microcapsules is higher before and after washing than that of the fabric with an average particle size of 500 nm of cooling nano-microcapsules.

[0057] (3) It can be seen from Examples 2 and 6 that, under the same conditions, the Q-max of the fabric whose cooling nano-microcapsule component is 5-methyl-2-isopropylcyclohexanol before and after washing is higher than that of the fabric whose cooling nano-microcapsule component is (R,S)-1,2,3,4-butanetetrol.

[0058] (4) It can be seen from Examples 2 and 7 that, under the same conditions, the Q-max of the fabric whose cooling nano-microcapsule component is 5-methyl-2-isopropylcyclohexanol is higher than that of the fabric whose cooling nano-microcapsule component is pentaerythritol before washing, while the Q-max of the two fabrics are equivalent after washing.

[0059] (5) It can be seen from Examples 2 and 8 that, under the same conditions, the Q-max of the fabric containing 5-methyl-2-isopropylcyclohexanol as the cooling nano-microcapsule component before and after washing is higher than that of the fabric containing eucalyptol as the cooling nano-microcapsule component.

[0060] (6) It can be seen from Examples 2 and 9 that, under the same conditions, the Q-max of the fabric whose inorganic particles are titanium dioxide is higher before and after washing than that of the fabric whose inorganic particles are zinc oxide.

[0061] (7) It can be seen from Example 2 and Example 10 that, under the same conditions, the Q-max of the fabric with an inorganic particle infrared reflectivity of 25% before and after washing is higher than that of the fabric with an inorganic particle infrared reflectivity of 15%.

[0062] (8) It can be seen from Examples 2 and 12 that, under the same conditions, the Q-max of the fabric with an inorganic particle size of 1.0 μm before and after washing is higher than that of the fabric with an average particle size of cooling nano-microcapsules of 1.8 μm.

[0063] (9) It can be seen from Examples 2 and 13 that, under the same conditions, the Q-max of the fabric with multiple layers of cooling microcapsules attached is comparable to that of the fabric with single layer of cooling microcapsules attached before washing, but the Q-max of the former is higher than that of the latter after washing.

[0064] (10) It can be seen from Comparative Example 1 and Example 2 that, under the same conditions, the fabric without cooling nano-microcapsules attached has a much worse cooling feeling than the fabric with cooling nano-microcapsules attached.

Claims

1. A cool fabric, characterized by: The fiber forming the cool fabric contains inorganic particles inside, and the inorganic particles and cool nano-microcapsules are attached to the surface of the fiber.

2. The cool fabric according to claim 1, characterized in that: The average particle size of the cooling nano-microcapsules is 250-400 nm.

3. The cool fabric according to claim 2, characterized in that: The cooling nano-microcapsule comprises a wall material and a core material, wherein the core material is one or more of 5-methyl-2-isopropylcyclohexanol, pentapentanol, (R, S)-1,2,3,4-butanetetrol and eucalyptol.

4. The cool fabric according to claim 1, characterized in that: The inorganic particles are particles with an infrared reflectivity greater than 20%.

5. The cool fabric according to claim 4, characterized in that: The average particle size of the inorganic particles is less than 1.5 μm.

6. The cool fabric according to any one of claims 1 to 5, characterized in that: The contact coolness Q-Max value of the cool fabric is 0.15 J / (cm 2 •s) and above.

Citation Information

Cited By

  • Cool-sense chinlon yarn and preparation process and application thereof

    CN119615455A

  • Cool fabric and preparation method thereof

    CN120925148A