Method for preparing modified zeolite filter material from electrolytic manganese residues and ardealite leachate and application of modified zeolite filter material

The method of preparing a modified zeolite filter material from electrolytic manganese slag and phosphogypsum leachate addresses environmental pollution by forming a multi-functionalized zeolite material that effectively absorbs COD, ammonia nitrogen, and heavy metals, enhancing resource utilization and pollution control.

CN119056147APending Publication Date: 2024-12-03CHANGSHU INSTITUTE OF TECHNOLOGY
0 Cites 1 Cited by

Patent Information

Application Number
CN202411323011.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

Electrolytic manganese slag and phosphogypsum leachate pose significant environmental pollution risks due to their hazardous components, and there is a need for effective resource utilization and treatment methods to mitigate these risks and promote sustainable development.

Method used

A method involving the preparation of a modified zeolite filter material through a hydrothermal process using electrolytic manganese slag and phosphogypsum leachate, involving specific ratios and reactions to form a multi-functionalized zeolite material capable of adsorbing pollutants.

Benefits of technology

The modified zeolite filter material effectively captures COD, ammonia nitrogen, and total phosphorus, and heavy metal pollutants, demonstrating a large adsorption capacity and wide range of application prospects. The modified zeolite filter material is capable of quickly absorbing COD, ammonia nitrogen, and heavy metal pollutants, and has a wide range of application prospects. The modified zeolite filter material is capable of absorbing COD, ammonia nitrogen, and mercury pollutants, and has a large adsorption capacity, and has a wide range of application prospects. The modified zeolite filter material is capable of absorbing heavy metal pollutants, has a large absorption capacity, and has a wide absorption capacity, and has a wide range of application prospects. The zeolite filter material is capable of absorbing COD, ammonia nitrogen, and ammonia nitrogen, and mercury pollutants, with a significant adsorption capacity for landfill leachate pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119056147A_ABST
    Figure CN119056147A_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a modified zeolite filter material from electrolytic manganese residues and ardealite leachate and application of the modified zeolite filter material, the method comprises the following steps: (1) mixing a gypsum material, fly ash and coal gangue, and uniformly stirring to obtain a hydrothermal pre-ingredient; (2) mixing a lime material and the ardealite leachate, uniformly stirring, and aging to obtain a hydrothermal pre-prepared solution; (3) mixing the electrolytic manganese residues and the hydrothermal pre-ingredient, uniformly stirring, granulating and aging to obtain granules to be subjected to hydrothermal treatment; and (4) sequentially adding the hydrothermal pre-prepared liquid and the to-be-hydrothermal granules into a hydrothermal reaction kettle, closing the kettle, and carrying out hydrothermal reaction to obtain the modified zeolite filter material. The preparation process is simple, and the high-activity modified zeolite filter material is prepared through reasonable burdening, hydrothermal solution modification and composite hydrothermal reaction and synergistic utilization of the electrolytic manganese residues and the ardealite leachate. The prepared modified zeolite filter material can be used for rapidly absorbing COD, ammonia nitrogen, total phosphorus and heavy metal pollutants, and is large in adsorption capacity and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of resource utilization of hazardous wastes, and in particular relates to a method for preparing a modified zeolite filter material by utilizing electrolytic manganese slag and phosphogypsum leachate and an application thereof. Background Art

[0002] Electrolytic manganese slag is an industrial waste generated in the production of electrolytic manganese metal, electrolytic manganese dioxide and high-purity manganese sulfate. For every ton of manganese metal produced, 8 to 10 tons of manganese slag will be produced, and the annual increase in manganese slag is even more astonishing, exceeding 10 million tons. These manganese slags have complex compositions, not only containing soluble salts such as manganese sulfate and ammonium sulfate, but also free heavy metal ions such as zinc, nickel and cobalt. If not handled properly, these harmful substances can easily spread into the environment, causing serious pollution to the soil, surface water and groundwater. The environmental pollution problem of manganese slag has become a key bottleneck restricting the high-quality development of the manganese industry. The environmental hazards of electrolytic manganese slag urgently need to receive more attention and effective solutions. We need to reduce the impact of manganese slag on the environment by implementing scientific pollution control technologies and active resource utilization methods, so as to promote the manganese industry to develop in a greener and healthier direction. This is not only a positive response to current environmental problems, but also a responsible attitude towards future sustainable development.

[0003] Phosphogypsum leachate contains a variety of high-concentration pollutants, including but not limited to heavy metals (such as As, Cr, Cd, Cu, Ni, Zn), fluorides, phosphates, sulfates, and radioactive uranium isotopes. If these pollutants are discharged directly into the environment without proper treatment, they will cause serious pollution to surface water, groundwater and soil, and may cause eutrophication of water bodies, deterioration of soil quality, and may even pose a threat to human health through the food chain. The harmfulness of phosphogypsum leachate to the environment is an issue that cannot be ignored. Improving the comprehensive utilization rate of phosphogypsum and developing effective treatment technologies are the key to achieving environmental protection and resource recycling.

[0004] The research on preparing modified zeolite filter material from electrolytic manganese slag and phosphogypsum leachate has significant environmental significance and research value. It not only provides a new technical approach for the harmless treatment and resource utilization of these two industrial wastes, but also brings innovative solutions to the fields of water treatment and environmental protection. In this way, waste reduction, resource utilization and harmlessness can be achieved, which has important environmental and economic dual value. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a method for preparing modified zeolite filter material using electrolytic manganese slag and phosphogypsum leachate and its application.

[0006] Technical solution: The present invention provides a method for preparing a modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate, comprising the following steps:

[0007] (1) mixing gypsum material, fly ash and coal gangue, stirring evenly to obtain hydrothermal pre-batch;

[0008] (2) mixing the lime material and the phosphogypsum leachate, stirring evenly, and aging to obtain a hydrothermal pre-mixed solution;

[0009] (3) mixing the electrolytic manganese slag and the hydrothermal pre-mixed ingredients, stirring evenly, granulating, aging, and obtaining hydrothermal pellets;

[0010] (4) Adding the pre-prepared hydrothermal solution and the pellets to be hydrothermally heated into the hydrothermal reaction kettle in sequence, closing the kettle to carry out the hydrothermal reaction, and obtaining a modified zeolite filter material.

[0011] Furthermore, in step (1), the mass ratio of gypsum material, fly ash and coal gangue is 15-45:20-60:100.

[0012] Furthermore, the gypsum material in step (1) is any one or more combinations of ordinary gypsum, phosphogypsum, desulfurized gypsum, and citric acid gypsum.

[0013] Furthermore, the solid-liquid ratio of the lime material and the phosphogypsum leachate in step (2) is 0.25-5.75:100 g / mL; and the aging time is 2-12 hours.

[0014] Furthermore, the lime material described in step (2) is any one or more combinations of quicklime or slaked lime.

[0015] Furthermore, the mass ratio of the electrolytic manganese slag to the hydrothermal pre-batch in step (3) is 40 to 120:100.

[0016] Furthermore, the aging time in step (3) is 0.5 to 4.5 days.

[0017] Furthermore, the liquid-to-solid ratio of the hydrothermal pre-prepared liquid and the pellets to be hydrothermally heated in step (4) is 2 to 40:1 mL / g.

[0018] Furthermore, the hydrothermal reaction time in step (4) is 0.5 to 7.5 hours, and the hydrothermal temperature is 120 to 360°C.

[0019] The present invention also provides the use of the modified zeolite filter material prepared by the method in treating garbage leachate.

[0020] Reaction mechanism: Gypsum materials, fly ash and coal gangue are mixed, and the mineral components of the three materials are mixed with each other. When lime materials and phosphogypsum leachate are mixed, lime milk reacts with phosphates, fluorides, ammonia nitrogen and other cations in the phosphogypsum leachate to form a phosphate precipitation mixture of calcium phosphate, hydroxyapatite, struvite and the like that is insoluble in water. The formed precipitation mixture adsorbs organic pollutants and other inorganic impurities in the phosphogypsum leachate. At the same time, the lime material adjusts the pH value of the leachate through an acid-base neutralization reaction, making the acidic leachate more neutral, which is helpful for the subsequent hydrothermal excitation process and the loading and functionalization of organic matter. During the hydrothermal reaction, the hydrothermal pellets are dissolved under high temperature and high pressure, releasing ions such as manganese, calcium, iron, aluminum, magnesium, fluorine and sulfate. These ions can react with the phosphate precipitation mixture in the hydrothermal pre-mixed solution to form a mixed precipitate of multi-element mixing and substitution. At the same time, under high temperature and high pressure environment, the hydroxide and metal cations released in the hydrothermal pellets promote the hydration and geopolymerization of silicates, aluminates, and aluminosilicates to form aluminosilicate-based gels, and promote the hydrolysis and polymerization of phosphate and aluminate precipitates to form polyphosphate aluminate gels. The polyphosphate aluminate gel further reacts with the aluminosilicate-based gel and the mixed precipitate of multi-element blending substitution to form a multi-component blended and cross-linked zeolite material. At the same time, under the hydrothermal environment, the iron and manganese in the hydrothermal pellets undergo oxidation reactions to form multivalent iron-manganese blended oxides. The iron-manganese blended oxides are mixed in the formed cross-linked zeolite-based material. Under high temperature environment, organic pollutants, fluorine, and phosphorus pollutants in the hydrothermal pre-mixed liquid react with the iron-manganese blended oxides, and the intermediate products formed strengthen the functionalization of the cross-linked zeolite-based material. The multi-functionalization between particles and on the surface of zeolite-based materials is not only conducive to strengthening the capture of heavy metal pollutants, but also conducive to strengthening ion exchange, electrostatic adsorption, surface complexation and redox processes.

[0021] Beneficial effects: Compared with the prior art, the present invention has the following outstanding and significant advantages: The present invention has a simple preparation process, and through reasonable ingredients, hydrothermal modification and composite hydrothermal reaction, the electrolytic manganese slag and phosphogypsum leachate are used to prepare a highly active modified zeolite filter material. The modified zeolite filter material prepared by the present invention can be used to quickly absorb COD, ammonia nitrogen, total phosphorus, and heavy metal pollutants, has a large adsorption capacity, and has a wide range of application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The figure is a flow chart of the processing method of the present invention. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0024] Landfill leachate: The original landfill leachate was obtained from Zhuji Sanfeng Environmental Protection Energy Co., Ltd. The COD mass concentration of this batch of concentrated landfill leachate was 3639 mg / L, the total phosphorus concentration was 294 mg / L, and the ammonia nitrogen concentration was 1062 mg / L. 500 mg of mercury pollutant was dissolved in 1 L of the original landfill leachate to obtain the landfill leachate for the test.

[0025] Phosphogypsum leachate: The phosphogypsum leachate was sampled from the on-site collection pool at the phosphogypsum dump in Xifeng County, Guizhou Province. The pH was 2.23, the total phosphorus was 816 mg / L, the sulfate concentration was 2146 mg / L, the calcium ion concentration was 439.51 mg / L, the magnesium ion concentration was 564.89 mg / g, and the fluoride concentration was 91.37 mg / g.

[0026] Electrolytic manganese slag: The electrolytic manganese slag is taken from Guizhou Energy Mining Manganese Industry Group Co., Ltd., mainly including 23.52% SO3, 13.17% SiO2, 15.21% CaO, 13.09% Fe2O3, 6.82% Al2O3, 10.21% MnO, 2.96% K2O, 1.55% MgO, 0.86% TiO2 and other components (inevitable impurities and ignition loss).

[0027] Fly ash: from Taicang Power Plant of Huaneng Power International Co., Ltd., mainly including 43.21% SiO2, 27.08% Al2O3, 15.62% Fe2O3, 6.58% CaO, 3.42% TiO2, 1.43% SO3, 1.04% K2O, 0.63% Na2O and other components (unavoidable impurities and loss on ignition).

[0028] Coal gangue: from Shanxi Xishan Coal and Electricity Co., Ltd., mainly including 46.87% SiO2, 33.51% Al2O3, 12.04% Fe2O3, 2.72% CaO, 2.36K2O, 1.37% TiO2 and other components (unavoidable impurities and loss on ignition).

[0029] Phosphogypsum: Phosphogypsum is taken from Guizhou Xifeng Phosphate Mine Co., Ltd. The phosphogypsum sample mainly contains 52.70% SO3, 37.01% CaO, 4.37% SiO2, 2.07% Al2O3, 1.63% P2O5 and other components (inevitable impurities and loss on ignition).

[0030] Citric acid gypsum: Citric acid gypsum is obtained from Shandong Citric Acid Biochemical Co., Ltd., the main component is CaSO4·2H2O, and the purity is 99.5%.

[0031] Desulfurized gypsum: Desulfurized gypsum is taken from Changshu No. 2 Waste Incineration Power Plant, mainly including 40.13% SO3, 32.04% CaO, 1.35% SiO2, 0.73% MgO, 0.64% Al2O3, 0.51% Fe2O3 and other components (inevitable impurities and ignition loss).

[0032] Example 1 Effect of the mass ratio of gypsum material, fly ash and coal gangue on the performance of the prepared modified zeolite filter material

[0033] According to the mass ratio of 7.5:20:100, 10:20:100, 12.5:20:100, 15:5:100, 15:10:100, 15:15:100, 15:20:100, 30:20:100, 45:20:100, 15:40:100, 30:40:100, 45:40:100, 15 :60:100, 30:60:100, 45:60:100, 45:65:100, 45:70:100, 45:75:100, 50:60:100, 55:60:100, 60:60:100 Weigh and mix gypsum material, fly ash, and coal gangue, stir evenly, and obtain hydrothermal pre-batch, wherein the gypsum material is ordinary gypsum. Weigh and mix lime material and phosphogypsum leachate according to a solid-liquid ratio of 0.25:100 g / mL, stir evenly, and age for 2 hours to obtain a hydrothermal pre-batch, wherein the lime material is quicklime. Weigh and mix electrolytic manganese slag and hydrothermal pre-batch according to a mass ratio of 40:100, stir evenly, granulate, and age for 0.5 days to obtain hydrothermal pellets. The hydrothermal pre-prepared liquid and the pellets to be hydroheated were sequentially added into the hydrothermal reactor, the liquid-to-solid ratio of the hydrothermal pre-prepared liquid and the pellets to be hydroheated was 2:1 mL / g, the reactor was closed for hydrothermal reaction to obtain a modified zeolite filter material, wherein the hydrothermal time was 0.5 hours and the hydrothermal temperature was 120°C.

[0034] Landfill leachate purification test: Weigh 1g of modified zeolite filter material and add it to 1L of landfill leachate, stir continuously for 30min, centrifuge, and the supernatant obtained is the purified liquid after treatment.

[0035] Detection of pollutant concentrations of COD, ammonia nitrogen, total phosphorus, and mercury: The concentration of chemical oxygen demand (COD) in the solution is determined in accordance with the national standard "Determination of Chemical Oxygen Demand in Water Quality - Dichromate Method" (GB 11914-1989); the concentration of ammonia nitrogen in the solution is determined in accordance with the "Determination of Ammonia Nitrogen in Water Quality - Salicylic Acid Spectrophotometric Method" (HJ536-2009); the concentration of total phosphorus in the solution is determined in accordance with the standard "Determination of Phosphate and Total Phosphorus in Water Quality - Continuous Flow - Ammonium Molybdate Spectrophotometric Method" (HJ 670-2013). The concentration of dissolved mercury in the solution is determined in accordance with the standard "Determination of Mercury, Arsenic, Selenium, Bismuth and Antimony in Water Quality - Atomic Fluorescence Method" (HJ 695-2014). The adsorption performance of adsorbents for COD, ammonia nitrogen, total phosphorus, and mercury pollutants is calculated according to formula (1), where q e is the pollutant adsorption capacity of modified zeolite filter media mg / g, c0 and c t are the pollutant concentrations in the solution before and after the adsorption experiment in mg / L, V is the volume of the experimental leachate in L (1L), and m is the dosage of modified zeolite filter material (1g).

[0036]

[0037] The test results of the modified zeolite filter material adsorption capacity of COD, total phosphorus, ammonia nitrogen and mercury pollutants in this embodiment are shown in Table 1.

[0038] Table 1 Effect of mass ratio of gypsum material, fly ash and coal gangue on the performance of prepared modified zeolite filter material

[0039]

[0040] It can be seen from Table 1 that when the mass ratio of gypsum material, fly ash and coal gangue is less than 15:20:100 (as in Table 1, the mass ratio of gypsum material, fly ash and coal gangue = 15:15:100, 15:10:100, 15:5:100, 12.5:20:100, 10:20:100, 7.5:20:100 and lower ratios not listed in Table 1), less gypsum material and fly ash are added, and the reaction between materials during granulation, aging and hydrothermal processes is insufficient, resulting in the prepared modified zeolite filter material. The adsorption capacity of COD, ammonia nitrogen, total phosphorus and mercury pollutants is significantly reduced as the mass ratio of gypsum material, fly ash and coal gangue decreases. When the mass ratio of gypsum material, fly ash and coal gangue is equal to 15-45:20-60:100 (as in Table 1, the mass ratio of gypsum material, fly ash and coal gangue = 15:20:100, 30:20:100, 45:20:100, 15:40:100, 30:40:100, 45:40:100, 15:60:100, 30:60:100, 45:60:100), the gypsum material, fly ash and coal gangue are mixed, and the mineral components of the three materials are mixed with each other. During the hydrothermal reaction, the hydrothermal pellets are dissolved under high temperature and high pressure environment, releasing ions such as manganese, calcium, iron, aluminum, magnesium, fluorine and sulfate, which can react with the phosphate precipitation mixture in the hydrothermal pre-mixed solution to form a mixed precipitate of multi-element mixing substitution. At the same time, under high temperature and high pressure environment, the hydroxide and metal cations released in the hydrothermal pellets promote the hydration and geopolymerization of silicates, aluminates, and aluminosilicates to form aluminosilicate-based gels, and promote the hydrolysis and polymerization of phosphate and aluminate precipitates to form polyphosphate aluminate gels. The polyphosphate aluminate gel further reacts with the aluminosilicate-based gel and the mixed precipitate of multi-element blending substitution to form a multi-component blended and cross-linked zeolite material. At the same time, under the hydrothermal environment, the iron and manganese in the hydrothermal pellets undergo oxidation reactions to form multivalent iron-manganese blended oxides. The iron-manganese blended oxides are mixed in the formed cross-linked zeolite-based material. Under high temperature environment, organic pollutants, fluorine, and phosphorus pollutants in the hydrothermal pre-mixed liquid react with the iron-manganese blended oxides, and the intermediate products formed strengthen the functionalization of the cross-linked zeolite-based material. The multi-functionalization between particles and on the surface of zeolite-based materials is not only conducive to strengthening the capture of heavy metal pollutants, but also conducive to strengthening ion exchange, electrostatic adsorption, surface complexation and redox processes. Finally, the prepared modified zeolite filter materials had COD adsorption capacity greater than 1452 mg / g, ammonia nitrogen adsorption capacity greater than 378 mg / g, total phosphorus adsorption capacity greater than 128 mg / g, and heavy metal mercury adsorption capacity greater than 265 mg / g for leachate.When the mass ratio of gypsum material, fly ash and coal gangue is greater than 45:60:100 (as in Table 1, the mass ratio of gypsum material, fly ash and coal gangue = 45:65:100, 45:70:100, 45:75:100, 50:60:100, 55:60:100, 60:60:100 and higher ratios not listed in Table 1), the gypsum material and fly ash are added in excess, and the material reaction is unbalanced during the hydrothermal reaction, resulting in the prepared modified zeolite filter material. The adsorption capacity of COD, ammonia nitrogen, total phosphorus and mercury pollutants is significantly reduced as the mass ratio of gypsum material, fly ash and coal gangue further increases.

[0041] Therefore, in summary, considering the benefits and costs, when the mass ratio of gypsum material, fly ash and coal gangue is equal to 15-45:20-60:100, it is most conducive to improving the adsorption performance of the prepared modified zeolite filter material.

[0042] Example 2 Effect of the mass ratio of electrolytic manganese slag and hydrothermal pre-batch on the performance of the prepared modified zeolite filter material

[0043] Weigh and mix gypsum material, fly ash and coal gangue according to a mass ratio of 45:60:100, stir evenly, and obtain a hydrothermal pre-batch, wherein the gypsum material is phosphogypsum. Weigh and mix lime material and phosphogypsum leachate according to a solid-liquid ratio of 3:100 g / mL, stir evenly, and age for 7 hours to obtain a hydrothermal pre-batch, wherein the lime material is slaked lime. Weigh and mix electrolytic manganese slag and hydrothermal pre-batch according to a mass ratio of 25:100, 30:100, 35:100, 40:100, 80:100, 120:100, 130:100, 140:100, 150:100, stir evenly, granulate, and age for 2.5 days to obtain hydrothermal pellets. The hydrothermal pre-prepared liquid and the pellets to be hydroheated were sequentially added into the hydrothermal reactor, the liquid-to-solid ratio of the hydrothermal pre-prepared liquid and the pellets to be hydroheated was 21:1 mL / g, the reactor was closed for hydrothermal reaction to obtain a modified zeolite filter material, wherein the hydrothermal time was 4 hours and the hydrothermal temperature was 240°C.

[0044] The landfill leachate purification test, COD, ammonia nitrogen, total phosphorus, mercury pollutant concentration detection and adsorption capacity calculation are all the same as in Example 1. The modified zeolite filter material adsorption capacity detection results of COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 2.

[0045] Table 2 Effect of mass ratio of electrolytic manganese slag and hydrothermal pre-batch on the performance of prepared modified zeolite filter material

[0046]

[0047] It can be seen from Table 2 that when the mass ratio of electrolytic manganese slag to hydrothermal pre-batch is less than 40:100 (as in Table 2, the mass ratio of electrolytic manganese slag to hydrothermal pre-batch = 35:100, 30:100, 25:100 and lower ratios not listed in Table 2), less electrolytic manganese slag is added, and the reaction between materials during the hydrothermal process is insufficient, resulting in the prepared modified zeolite filter material. The adsorption capacity of COD, ammonia nitrogen, total phosphorus and mercury pollutants is significantly reduced as the mass ratio of electrolytic manganese slag to hydrothermal pre-batch decreases. When the mass ratio of electrolytic manganese slag to hydrothermal premix is ​​equal to 40-120:100 (as in Table 2, the mass ratio of electrolytic manganese slag to hydrothermal premix is ​​40:100, 80:100, 120:100), during the hydrothermal reaction, the hydrothermal pellets are dissolved under high temperature and high pressure, releasing ions such as manganese, calcium, iron, aluminum, magnesium, fluorine, and sulfate, which can react with the phosphate precipitation mixture in the hydrothermal premix to form a mixed precipitate of multi-element mixing and substitution. At the same time, under high temperature and high pressure, the hydroxyl and metal cations released in the hydrothermal pellets promote the hydration and geopolymerization of silicates, aluminates, and aluminosilicates to form a silicate-based gel, and promote the hydrolysis and polymerization of phosphate and aluminate precipitates to form a polyphosphate aluminate gel. The polyphosphate aluminate gel further reacts with the silicate-based gel and the multi-element mixed precipitate to form a multi-component mixed and cross-linked zeolite material. At the same time, under the hydrothermal environment, the iron and manganese in the hydrothermal pellets undergo oxidation reaction to form multivalent iron-manganese mixed oxides. The iron-manganese mixed oxides are mixed in the formed cross-linked zeolite-based material. Under high temperature environment, organic pollutants, fluorine, and phosphorus pollutants in the hydrothermal pre-mixed liquid react with the iron-manganese mixed oxides, and the intermediate products formed strengthen the functionalization of the cross-linked zeolite-based material. The multi-functionalization between particles and on the surface of zeolite-based materials is not only conducive to strengthening the capture of heavy metal pollutants, but also conducive to strengthening ion exchange, electrostatic adsorption, surface complexation and redox processes. Finally, the prepared modified zeolite filter material has an adsorption capacity of more than 1514 mg / g for COD of landfill leachate, more than 415 mg / g for ammonia nitrogen, more than 142 mg / g for total phosphorus, and more than 281 mg / g for heavy metal mercury. When the mass ratio of electrolytic manganese slag to hydrothermal pre-batch is greater than 120:100 (as in Table 2, the mass ratio of electrolytic manganese slag to hydrothermal pre-batch = 130:100, 140:100, 150:100 and higher ratios not listed in Table 2), excessive addition of electrolytic manganese slag causes an imbalance in the material reaction during the hydrothermal reaction, resulting in a significant decrease in the adsorption capacity of the prepared modified zeolite filter material for COD, ammonia nitrogen, total phosphorus and mercury pollutants as the mass ratio of electrolytic manganese slag to hydrothermal pre-batch further increases.

[0048] Therefore, in summary, considering the benefits and costs, when the mass ratio of electrolytic manganese slag to hydrothermal premix is ​​equal to 40-120:100, it is most conducive to improving the adsorption performance of the prepared modified zeolite filter material.

[0049] Example 3 Effect of hydrothermal time on the performance of prepared modified zeolite filter material

[0050] Weigh and mix gypsum material, fly ash and coal gangue according to a mass ratio of 45:60:100, stir evenly, and obtain a hydrothermal pre-mixed material, wherein the gypsum material is desulfurized gypsum. Weigh and mix lime material and phosphogypsum leachate according to a solid-liquid ratio of 5.75:100 g / mL, stir evenly, and age for 12 hours to obtain a hydrothermal pre-mixed liquid, wherein the lime material is slaked lime. Weigh and mix electrolytic manganese slag and hydrothermal pre-mixed materials according to a mass ratio of 120:100, stir evenly, granulate, and age for 4.5 days to obtain hydrothermal pellets. To the hydrothermal reactor, hydrothermal pre-prepared liquid and pellets to be hydroheated were added in sequence, the liquid-to-solid ratio of the hydrothermal pre-prepared liquid and the pellets to be hydroheated was 40:1 mL / g, the reactor was closed for hydrothermal reaction to obtain modified zeolite filter material, wherein the hydrothermal time was 0.25 hour, 0.3 hour, 0.4 hour, 0.5 hour, 4 hours, 7.5 hours, 7.75 hours, 8 hours, and 8.25 hours, and the hydrothermal temperature was 360°C.

[0051] The landfill leachate purification test, COD, ammonia nitrogen, total phosphorus, mercury pollutant concentration detection and adsorption capacity calculation are all the same as in Example 1. The modified zeolite filter material adsorption capacity detection results of COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 3.

[0052] Table 3 Effect of hydrothermal time on the performance of prepared modified zeolite filter material

[0053] Water heating time COD(mg / g) Ammonia nitrogen (mg / g) Total phosphorus (mg / g) Mercury (mg / g) 0.25 hours 1426.51 385.42 132.74 249.65 0.3 hours 1485.78 404.14 139.82 255.91 0.4 hours 1539.43 437.75 145.93 276.14 0.5 hours 1613.05 492.63 160.37 298.21 4 hours 1645.74 513.82 172.41 306.64 7.5 hours 1703.27 528.49 179.25 322.72 7.75 hours 1610.04 489.31 158.67 295.36 8 hours 1567.41 458.98 147.09 287.63 8.25 hours 1513.09 426.54 139.16 264.92

[0054] It can be seen from Table 3 that when the hydrothermal time is less than 0.5 hours (such as in Table 3, when the hydrothermal time = 0.4 hours, 0.3 hours, 0.25 hours and lower values ​​not listed in Table 3), the hydrothermal time is short, and the reaction between materials during the hydrothermal process is insufficient, resulting in the prepared modified zeolite filter material for COD, ammonia nitrogen, total phosphorus and mercury pollutant adsorption capacity being significantly reduced as the hydrothermal time decreases. When the hydrothermal time is equal to 0.5 to 7.5 hours (such as in Table 3, when the hydrothermal time = 0.5 hours, 4 hours, 7.5 hours), during the hydrothermal reaction process, the hydrothermal pellets are dissolved under high temperature and high pressure environment, releasing ions such as manganese, calcium, iron, aluminum, magnesium, fluorine, and sulfate, which can react with the phosphate precipitation mixture in the hydrothermal pre-mixed solution to form a mixed precipitate of multi-element mixing substitution. At the same time, under high temperature and high pressure environment, the hydroxide and metal cations released in the hydrothermal pellets promote the hydration and geopolymerization of silicates, aluminates, and aluminosilicates to form aluminosilicate-based gels, and promote the hydrolysis and polymerization of phosphate and aluminate precipitates to form polyphosphate aluminate gels. The polyphosphate aluminate gel further reacts with the aluminosilicate-based gel and the mixed precipitate of multi-element blending substitution to form a multi-component blended and cross-linked zeolite material. At the same time, under the hydrothermal environment, the iron and manganese in the hydrothermal pellets undergo oxidation reactions to form multivalent iron-manganese blended oxides. The iron-manganese blended oxides are mixed in the formed cross-linked zeolite-based material. Under high temperature environment, organic pollutants, fluorine, and phosphorus pollutants in the hydrothermal pre-mixed liquid react with the iron-manganese blended oxides, and the intermediate products formed strengthen the functionalization of the cross-linked zeolite-based material. The multi-functionalization between particles and on the surface of zeolite-based materials is not only conducive to strengthening the capture of heavy metal pollutants, but also conducive to strengthening ion exchange, electrostatic adsorption, surface complexation and redox processes. Finally, the prepared modified zeolite filter material has an adsorption capacity of COD greater than 1613 mg / g, an adsorption capacity of ammonia nitrogen greater than 492 mg / g, an adsorption capacity of total phosphorus greater than 160 mg / g, and an adsorption capacity of heavy metal mercury greater than 298 mg / g. When the hydrothermal time is greater than 7.5 hours (as in Table 3, when the hydrothermal time = 7.75 hours, 8 hours, 8.25 hours, and higher values ​​not listed in Table 3), the hydrothermal time is too long, and the material reaction is unbalanced during the hydrothermal reaction, resulting in the prepared modified zeolite filter material having a significant decrease in the adsorption capacity of COD, ammonia nitrogen, total phosphorus and mercury pollutants as the hydrothermal time further increases.

[0055] Therefore, in summary, considering the benefits and costs, when the hydrothermal time is equal to 0.5 to 7.5 hours, it is most conducive to improving the adsorption performance of the prepared modified zeolite filter material.

[0056] Example 4 Effect of gypsum material type on the performance of prepared modified zeolite filter material

[0057] Weigh and mix gypsum material, fly ash, and coal gangue according to a mass ratio of 45:60:100, stir evenly, and obtain a hydrothermal pre-batch, wherein the gypsum material is any one of ordinary gypsum, phosphogypsum, desulfurized gypsum, and citric acid gypsum. Weigh and mix lime material and phosphogypsum leachate according to a solid-liquid ratio of 5.75:100g / mL, stir evenly, and age for 12 hours to obtain a hydrothermal pre-batch, wherein the lime material is slaked lime. Weigh and mix electrolytic manganese slag and hydrothermal pre-batch according to a mass ratio of 120:100, stir evenly, granulate, and age for 4.5 days to obtain hydrothermal pellets. Add the hydrothermal pre-batch liquid and the pellets to be hydrothermally heated to the hydrothermal reactor in sequence, the liquid-solid ratio of the hydrothermal pre-batch liquid and the pellets to be hydrothermally heated is 40:1mL / g, close the reactor for hydrothermal reaction, and obtain a modified zeolite filter material, wherein the hydrothermal time is 7.5 hours and the hydrothermal temperature is 360°C.

[0058] The landfill leachate purification test, COD, ammonia nitrogen, total phosphorus, mercury pollutant concentration detection and adsorption capacity calculation are all the same as in Example 1. The modified zeolite filter material adsorption capacity detection results of COD, total phosphorus, ammonia nitrogen and mercury pollutants in this example are shown in Table 4.

[0059] Table 4 Effect of gypsum material type on the performance of prepared modified zeolite filter media

[0060] Water heating time COD(mg / g) Ammonia nitrogen (mg / g) Total phosphorus (mg / g) Mercury (mg / g) Ordinary gypsum 1710.87 521.56 187.13 320.95 Phosphogypsum 1698.51 526.14 183.42 325.97 Desulfurization gypsum 1703.27 528.49 179.25 322.72 Citric Acid Gypsum 1706.42 523.63 181.91 321.04

[0061] It can be seen from Table 4 that when the gypsum material is any one of ordinary gypsum, phosphogypsum, desulfurized gypsum and citric acid gypsum, there is no significant difference in the performance of the prepared modified zeolite filter material.

[0062] Comparative Example Effects of Different Processes on the Performance of Modified Zeolite Filter Media Prepared

[0063] The process of the present invention: weigh and mix gypsum material, fly ash and coal gangue according to a mass ratio of 45:60:100, stir evenly, and obtain a hydrothermal pre-batch, wherein the gypsum material is citric acid gypsum. Weigh and mix lime material and phosphogypsum leachate according to a solid-liquid ratio of 5.75:100g / mL, stir evenly, and age for 12 hours to obtain a hydrothermal pre-batch, wherein the lime material is slaked lime. Weigh and mix electrolytic manganese slag and hydrothermal pre-batch according to a mass ratio of 120:100, stir evenly, granulate, and age for 4.5 days to obtain hydrothermal pellets. Add the hydrothermal pre-batch liquid and the pellets to be hydrothermally heated to the hydrothermal reactor in sequence, the liquid-solid ratio of the hydrothermal pre-batch liquid and the pellets to be hydrothermally heated is 40:1mL / g, close the reactor for hydrothermal reaction, and obtain a modified zeolite filter material, wherein the hydrothermal time is 7.5 hours and the hydrothermal temperature is 360°C.

[0064] Comparative process 1: Weigh and mix gypsum material, fly ash, and coal gangue in a mass ratio of 45:60:100, stir evenly, and obtain a hydrothermal pre-mixed material, wherein the gypsum material is citric acid gypsum. Weigh and mix lime material and phosphogypsum leachate in a solid-liquid ratio of 5.75:100 g / mL, stir evenly, and age for 12 hours to obtain a hydrothermal pre-mixed liquid, wherein the lime material is slaked lime. Add the hydrothermal pre-mixed liquid and the hydrothermal pre-mixed material to the hydrothermal reactor in sequence, the liquid-solid ratio of the hydrothermal pre-mixed liquid and the hydrothermal pre-mixed material is 40:1 mL / g, close the reactor for hydrothermal reaction, and obtain a modified zeolite filter material, wherein the hydrothermal time is 7.5 hours and the hydrothermal temperature is 360°C.

[0065] Comparative process 2: Weigh and mix gypsum material, fly ash, and coal gangue in a mass ratio of 45:60:100, stir evenly, and obtain a hydrothermal pre-batch, wherein the gypsum material is citric acid gypsum. Weigh and mix lime material and water in a solid-liquid ratio of 5.75:100g / mL, stir evenly, and age for 12 hours to obtain a hydrothermal pre-batch liquid, wherein the lime material is slaked lime. Weigh and mix electrolytic manganese slag and hydrothermal pre-batch in a mass ratio of 120:100, stir evenly, granulate, and age for 4.5 days to obtain hydrothermal pellets. Add the hydrothermal pre-batch liquid and the pellets to be hydrothermally heated to the hydrothermal reactor in sequence, the liquid-solid ratio of the hydrothermal pre-batch liquid and the pellets to be hydrothermally heated is 40:1mL / g, close the reactor for hydrothermal reaction, and obtain a modified zeolite filter material, wherein the hydrothermal time is 7.5 hours and the hydrothermal temperature is 360°C.

[0066] The landfill leachate purification test, COD, ammonia nitrogen, total phosphorus, mercury pollutant concentration detection and adsorption capacity calculation are all the same as in Example 1. The modified zeolite filter material adsorption capacity detection results of COD, total phosphorus, ammonia nitrogen and mercury pollutants in this comparative example are shown in Table 5.

[0067] Table 5 Effect of different processes on the performance of prepared modified zeolite filter media

[0068]

[0069]

[0070] It can be seen from Table 5 that the adsorption performance of the modified zeolite filter material prepared by the present invention is significantly better than that of the zeolite filter material prepared by comparative process 1 and comparative process 2.

Claims

1. A method for preparing modified zeolite filter material using electrolytic manganese slag and phosphogypsum leachate, characterized in that: The following steps are involved: (1) mixing gypsum material, fly ash and coal gangue, stirring evenly to obtain hydrothermal pre-batch; (2) mixing the lime material and the phosphogypsum leachate, stirring evenly, and aging to obtain a hydrothermal pre-mixed solution; (3) mixing the electrolytic manganese slag and the hydrothermal pre-mixed ingredients, stirring evenly, granulating, aging, and obtaining hydrothermal pellets; (4) Adding the pre-prepared hydrothermal solution and the pellets to be hydrothermally heated into the hydrothermal reaction kettle in sequence, closing the kettle to carry out the hydrothermal reaction, and obtaining a modified zeolite filter material.

2. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: In step (1), the mass ratio of gypsum material, fly ash and coal gangue is 15-45:20-60:

100.

3. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The gypsum material in step (1) is any one or more combinations of ordinary gypsum, phosphogypsum, desulfurized gypsum, and citric acid gypsum.

4. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The solid-liquid ratio of the lime material and the phosphogypsum leachate in step (2) is 0.25-5.75:100 g / mL; and the aging time is 2-12 hours.

5. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The lime material described in step (2) is any one or more combinations of quicklime or slaked lime.

6. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The mass ratio of the electrolytic manganese slag to the hydrothermal pre-batch in step (3) is 40 to 120:

100.

7. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The aging time described in step (3) is 0.5 to 4.5 days.

8. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The liquid-to-solid ratio of the hydrothermal pre-prepared liquid and the pellets to be hydrothermally prepared in step (4) is 2 to 40:1 mL / g.

9. The method for preparing modified zeolite filter material by using electrolytic manganese slag and phosphogypsum leachate according to claim 1, characterized in that: The hydrothermal reaction time in step (4) is 0.5 to 7.5 hours, and the hydrothermal temperature is 120 to 360°C.

10. Use of the modified zeolite filter material prepared by the method according to any one of claims 1 to 9 in treating landfill leachate.

Citation Information

Cited By

  • Method for reducing arsenic content of rice growing in alkaline arsenic polluted rice field

    CN120479925A