Procedure for producing a bearing element and bearing element
A two-step bainite creation process in specific temperature ranges, combined with salt bath treatment, addresses the challenge of achieving high surface hardness and low residual stresses in bearing elements, enhancing wear resistance and service life while reducing costs.
Patent Information
- Application Number
- PCT/EP2023/061608
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-03
- Publication Date
- 2024-11-07
AI Technical Summary
Existing methods for producing bearing elements do not efficiently achieve a high service life while maintaining cost-effectiveness, particularly in achieving high surface hardness with low residual stresses for rolling bearings.
A two-step process involving carburization followed by bainite creation in specific temperature ranges, utilizing salt baths to minimize distortions and reduce grinding time, thereby achieving high surface hardness and low residual stresses.
The process results in a bearing element with improved wear resistance and extended service life, reducing production costs by minimizing grinding time and distortion, with residual stresses lower than in prior art products.
Smart Images

Figure EP2023061608_07112024_PF_FP_ABST
Abstract
Description
[0001] Procedure for producing a bearing element and bearing element
[0002] The invention concerns a procedure for producing a bearing element and a bearing element.
[0003] Case carburizing is a surface hardening treatment that may be used to produce a hard, wearresistant layer (case) on the surface of a steel component.
[0004] Carburizing is a heat treatment process where a steel component is heated in a gas atmosphere, which decomposes and provides carbon to the component surface. After treatment the case has a higher carbon content than the original material. When the steel component is cooled rapidly (quenched), either directly after carburizing or in a second re-hardening step, the carbon rich surface becomes hard, while the core remains soft and tough.
[0005] The most common method for hardening is to use case carburizing followed by martensitic rehardening.
[0006] The article “CarboBain: Case Hardening by Carbo-Austempering - a short Introduction to Transformation Kinetics, Microstructure and Residual Stresses”, published in HTM J. Heat Treatm. Mat. 72 (2017) 5, discloses a procedure for dry austempering of samples which were firstly carburized. Afterwards the samples were quenched to RT. Then the samples were reheated to 840 °C using a vacuum furnace and held for 30 min. Adjacent the samples were transferred internally into a quenching chamber where they were quenched in hot nitrogen gas to 220 °C and held for at least 90 seconds. Then the hot samples were transferred into a convection air furnace at 240 °C with a high gas speed of approx. 15 m / s. The transformation to bainite was done at 240°C (cf. page 250 and table 3).
[0007] The patent DE69811055 T2, which is cited in the above-mentioned article, discloses another procedure, during which bainite is produced in one step.
[0008] The problem of the invention is in particular to provide a bearing element with a high service life in a cost-efficient way. The problem is solved according to the invention by the features of claim 1 and by the features of claim 9, while advantageous embodiments and further embodiments of the invention can be taken from the subclaims. Proposed is a procedure for producing a bearing element, during which at least a part of a steel component is carburized and at least the part is brought in a first temperature range above a martensite start temperature of a carburized surface of the part and at least the part is held in the first temperature range for at least a first amount of time, whereat during the holding in the first temperature range a creation of bainite at least in the part is achieved, wherein after the holding in the first temperature range at least the part is heated up such that at least the part is brought in a second temperature range, wherein at least the part is held in the second temperature range for at least a second amount of time, whereat during the holding in the second temperature range a further creation of bainite at least in the part is achieved. Thereby a bearing element with a high service life can be provided in a cost-efficient way. In particular, a high hardness on the surface together with low residual stresses beneath the surface can be achieved, which is both desirable for running surfaces of rolling elements and raceways of rings of rolling bearings.
[0009] In particular, the bearing element can be a rolling bearing element, wherein the rolling bearing element can especially be a ring or a rolling element. In particular, the ring can be an inner ring or an outer ring. In particular, the rolling bearing element can be an element of a self-aligning rolling bearing, as for example a spherical roller bearing.
[0010] In particular, at least the part can be carburized at approximately 970°C.
[0011] Advantageously at least the part is located in a salt bath during the first amount of time. Thereby a time needed for bringing the bearing element into a final shape through grinding can be reduced significantly, because in the salt bath distortions of the part are minimized, which entails a considerable reduction of costs. In particular, the whole component is located in the salt bath during the first amount of time. The salt bath can especially contain sodium nitrite, which has the chemical formula NaNO2, and / or potassium nitrate, which has the chemical formula KNO3. In particular, the salt bath can contain approximately the same amounts of substance of sodium nitrite and potassium nitrate. “Approximately” the same amounts of substance of sodium nitrite and potassium nitrate is especially suppose to mean that the amount of substance of sodium nitrite differs from the amount of substance of potassium nitrate by less than 20 percent, in particular less than 10 percent and preferably less than 3 percent. In particular, the salt bath can contain the same amounts of substance of sodium nitrite and potassium nitrate. The salt bath can especially consist of water, sodium nitrite dissolved in water and potassium nitrate dissolved in water. In particular, the part or the complete component can be located in the salt bath already in one or more than one cooling steps of the procedure, which precede the first amount of time.
[0012] With advantage at least the part is located in a further salt bath during the second amount of time. Thereby a time needed for bringing the bearing element into a final shape through grinding can be reduced significantly, because in the further salt bath distortions of the part are minimized, which entails a considerable reduction of costs. In particular, the whole component is located in the further salt bath during the second amount of time. The further salt bath can especially contain sodium nitrite and / or potassium nitrate. In particular, the further salt bath can contain approximately the same amounts of substance of sodium nitrite and potassium nitrate. “Approximately” the same amounts of substance of sodium nitrite and potassium nitrate is especially suppose to mean that the amounts of substance of sodium nitrite differs from the amount of substance of potassium nitrate by less than 20 percent, in particular less than 10 percent and preferably less than 3 percent. In particular, the further salt bath can contain the same amounts of substance of sodium nitrite and potassium nitrate. The further salt bath can especially consist of water, sodium nitrite dissolved in water and potassium nitrate dissolved in water.
[0013] In particular, the salt bath and the further salt bath can be the same.
[0014] Furthermore, it is suggested that the first temperature range is the temperature range between 200°C and 250°C. Thereby a high hardness of the surface of the part in a final state can be achieved. Advantageously the first temperature range is the temperature range between 210°C and 235°C, whereby an especially high hardness can be achieved and tensile stresses can be avoided safely.
[0015] Advantageously a lower bound of the first temperature range is at least 2 Kelvin above the martensite start temperature. Thereby the creation of martensite together with the production of tensile stresses can be avoided. In particular is the lower bound of the first temperature range at least 10 Kelvin and preferably at least 20 Kelvin above the martensite start temperature, whereby the creation of tensile stresses can be avoided especially safely.
[0016] In particular is the first amount of time at least one hour.
[0017] With advantage is the first amount of time at least three hours and preferably at least four hours.
[0018] Through this a high hardness of the part in the final state can be reached. Moreover, it is suggested that the second temperature range is the range from 235°C to 260°C. Thereby the surface of the part has in the final state very low residual stresses, which induces a high resistance against damages and a high service life. Preferably is the second temperature range the range from 240°C two 260°C, whereby additionally a short duration of the second amount of time can be reached.
[0019] Furthermore, it is suggested that the second amount of time is between 150 minutes and 16 hours. Through this very low residual stresses and an almost complete transformation of a surface layer of the part to bainite can be achieved. In particular is the second amount of time between 4 hours and 12 hours.
[0020] Advantageously during the holding in the first temperature range more bainite is produced in the component than during the holding in the second temperature range. Through this a high hardness of the part together with a relatively fast production of the bearing element can be achieved.
[0021] Moreover, it is suggested that the steel of the steel component contains 0.5 - 5.0 weight percent Chromium, 0.1 - 5.0 weight percent Molybdenum and 0.1 - 0.6 weight percent Carbon. Thereby a precondition for a cost-efficient high quality bearing element can be met.
[0022] In particular, the steel can contain Silicon and / or Manganese and / or Nickel and / or Vanadium, whereat the remainder can especially be Iron and normally occurring impurities.
[0023] In particular, the steel can be a low carbon steel for case hardening, such as 20NiCrMo7 , 20NiCrMo2-2, 18CrNiMo7-6, 16MnCr5, 20MnCr5 or 25CrMo4. In particular, the steel can be a medium carbon steel such as 42CrMo4 or 50CrMo4.
[0024] In particular, directly after the carburization the component can be cooled to 320°C and can be held at this temperature between 20 minutes and 30 minutes in nitrogen gas under overpressure and can be put directly afterwards from one furnace in a different furnace for air tempering at 320°C for a time between six hours and 24 hours and can be cooled to room temperature. In particular, directly after this cooling to room temperature the component can be heated up to 870°C and can be held for 15 minutes at 870°C.
[0025] Furthermore, a bearing element, which is produced according to at least one of the procedures described above is proposed. Thereby a bearing element with a high service life can be provided in a cost-efficient way. In particular, a high hardness on the surface together with low residual stresses beneath the surface can be achieved, which is both desirable for running surfaces of rolling elements and raceways of rings of rolling bearings. In particular, a time which is necessary for grinding the component in a desired end shape can be reduced significantly, which results in a significant reduction of costs.
[0026] In particular, the bearing element can be a rolling bearing element, wherein the rolling bearing element can especially be a ring or a rolling element. In particular, the ring can be an inner ring or an outer ring.
[0027] Advantageously the bearing element is a rolling bearing element with a running surface area, at which residual stresses are lower than -250 Megapascal, preferably lower than -300 Megapascal, in a complete depth range between 0 millimeter to 0.5 millimeter below the surface. Thereby a high service life can be reached.
[0028] In particular, the bearing element can be a rolling element and a case of the bearing element, a surface of which is a running surface area, has a depth up to 1.3*(1 Millimeter+Dw / 30), where Dw = diameter of the rolling element in Millimeters.
[0029] In particular, the bearing element can be a ring and a case of the bearing element, a surface of which is a running surface area, has a depth, which is the same as the depth of a case of a rolling element, which is supposed to roll on the running surface area.
[0030] Advantageously the bearing element is a rolling bearing element with a running surface area, which has a higher hardness than 58 HRC. Thereby an improved wear resistance can be achieved.
[0031] Further advantages can be seen in the following description of the drawings. Example of embodiments of the invention are shown in the drawings. The drawings, the description and the claims contain numerous features in combination. The skilled person will expediently also consider the features individually and combine them to form useful further combinations.
[0032] Fig. 1 shows a temperature-time diagram for a first procedure for producing a bearing element according to the invention,
[0033] Fig. 2 shows a temperature-time diagram for a further procedure for producing a bearing element according to the invention. Fig. 3 shows measurement values for the hardness HV1 for two different rings in different depths under a surface of a case,
[0034] Fig. 4 shows a microstructure of a first ring at a depth of 300 pm under a surface of a case,
[0035] Fig. 5 shows a microstructure of a core of the first ring,
[0036] Fig. 6 shows a microstructure of a second ring at a depth of 300 pm under a surface of a case,
[0037] Fig. 7 shows a microstructure of a core of the second ring.
[0038] Figure 1 shows a temperature-time diagram for a procedure for producing a rolling bearing element according to the invention. The rolling bearing element can be a rolling element or an inner ring or an outer ring. During the procedure a steel component is carburized at approximately 970°C in a time span between the point in time T 1 and the point in time T2. The steel of the steel component contains 0.5 - 5.0 weight percent Chromium, 0.1 - 5.0 weight percent Molybdenum and 0.1 - 0.6 weight percent Carbon. The steel can contain Silicon and / or Manganese and / or Nickel and / or Vanadium, whereat the remainder is Iron and normally occurring impurities. The carburization is done long enough to produce a layer starting at a surface of the component with enriched carbon content.
[0039] If the rolling bearing element is a rolling element, the layer has a depth up to 1 ,3*(1 Millimeter+Dw / 30), where Dw = diameter of the rolling element in Millimeters. If the rolling bearing element is a ring, the layer has a depth, which is the same as the depth of a layer of a rolling element, which is supposed to roll on the layer of the ring. For example the layer can have a depth between 2.5 millimeters to 3.5 millimeters. After the carburization the surface carbon content of the layer is between 0.5 weight percent and 1.5 weight percent.
[0040] The following second step of the procedure between the point in time T2 and the point in time T3 is shown in figure 1 in a simplified way. In the second step the component is cooled to 320°C and is held at this temperature between 20 minutes and 30 minutes in nitrogen gas under overpressure. After this still in the second step the component is put in a different furnace for air tempering at 320°C for a time between six hours and 24 hours. After this the component is cooled to room temperature. This ends the second step at the point in time T3. Afterwards the component is heated up to 870°C between the point in time T4 and the point in time T5. The component is held for 15 minutes at 870°C until the point in time T6. The 870°C are in the austenitic temperature range of the layer.
[0041] In the time span between the point in time T6 and the point in time T7 the component is cooled down to 220°C, which is 20 kelvin above a martensite start temperature of the carburized surface of the layer. The difference between the point in time T7 and the point in time T6 is between 15 seconds and 15 minutes. In the point in time T6 the component is put in a salt bath and is left in the salt bath until the point in time T10. The salt bath consists of water, sodium nitrite dissolved in water and potassium nitrate dissolved in water. The salt bath was created by putting the same amounts of substance of sodium nitrite and potassium nitrate in water. This mixture in the salt bath decreases the melting point. From the point in time T7 until the point in time T8 the component is held at 220°C. In the time span from the point in time T7 to the point in time T8 bainite is created in the layer. The difference between the point in time T8 and the point in time T7 is 11 hours. From the point in time T8 to the point in time T9 the component and the salt bath is heated up relatively quickly to 255°C. From the point in time T9 to the point in time T10 the component is held at 255°C. In the time span from T9 to T10 further bainite is created in the layer. The difference between the point in time T10 and the point in time T9 is 4 hours. At a point in time T10 98 weight percent of the layer consist of bainite. The remaining two weight percent of the layer consists in particular of retained austenite. After the point in time T10 the component is cooled down to room temperature. After this cooling down to room temperature the layer builds a hardened case and the surface of the layer constitutes a running surface area, at which residual stresses are lower than -300 Megapascal in a complete depth range between 0 millimeter to 0.5 millimeter below this surface. These residual stresses are lower than in prior art products, which leads to improved rolling contact fatigue resistance of the component.
[0042] As a comparison, martensitic re-hardening typically results in residual stresses above -200 MPa.
[0043] Because of the usage of the salt bath between the point in time T7 and the point in time T10 together with the described heat treatment between these points in time very little grinding is needed to bring the component into an end shape. In the prior art 12 minutes for grinding are needed, for the described component only three minutes are needed, which means that costs can be cut with the invention enormously. The described two-step bainitizing results in a high surface hardness, typically above 58 HRC.
[0044] This distinguishes it from a one-step bainitizing, which would achieve lower hardness. Increased hardness leads to improved wear resistance.
[0045] Using bainitic re-hardening improves generally the temperature stability of the component compared to martensitic re-hardening.
[0046] In the following measuring results for two inner rings produced according to the described procedure are presented. For the first ring the case depth was circa 1.8 millimeters. For the second ring the case depth was circa 2 millimeters. The content of retained austenite was for each ring in the surface and in the core less than one weight percent. Table six shows measuring results for the hardness HV10 for three different measurements R1 , R2 and R3 on the surface of the case, for the track and for the core of each ring. The track is a location which is the ring diameter divided by 20 under the surface of the case. In the next to last column of Table 6 the average for the different measurements is given and from this the hardness of the last column is calculated.
[0047] Figure 3 shows measurement values for the hardness HV1 for the two different rings in different depths under a surface of each case of the respective ring.
[0048] The figures 4 to 7 show different microstructures of both rings.
[0049] Table 1 shows residual stresses of the case in Megapascal in certain depths in pm in a certain direction (“0 deg”) and in a direction perpendicular to the direction (“90 deg”) and deviations from the measured values. In the last column the average residual stresses for each depth is given.
[0050] Table 2 shows the same things for a different case: The only difference in the production of this case was that the time interval between T9 and T10 was 11 hours and the carburization depth was changed slightly.
[0051] Tables 3-5 show the same things for different bearing elements of the prior art.
[0052] Figure 2 illustrates a second procedure according to the invention. Essentially identical times are basically numbered with the same reference numerals. However, the letter "a" has been added to the reference numerals of the embodiments in Fig. 2 to distinguish them.
[0053] The second procedure according to the invention is identical to the first procedure according to the invention except for the following differences: the steps from the point in time T3 to the point in time T7 in the first procedure are omitted in the second procedure. Instead the last cooling operation, which is performed in the first procedure between the point in time T2 and the point in time T3 is only executed to 220°C. The results from the second procedure are the same as the results from the first procedure.
[0054] Table 1:
[0055] Table 2:
[0056] Table 3:
[0057]
[0058] Table 4:
[0059] Table 5: Table 6:
[0060] List of reference numerals:
Claims
Claims:1 . Procedure for producing a bearing element, during which at least a part of a steel component is carburized and at least the part is brought in a first temperature range above a martensite start temperature of a carburized surface of the part and at least the part is held in the first temperature range for at least a first amount of time (T8-T7), whereat during the holding in the first temperature range a creation of bainite at least in the part is achieved, wherein after the holding in the first temperature range at least the part is heated up such that at least the part is brought in a second temperature range, wherein at least the part is held in the second temperature range for at least a second amount of time (T 10-T9), whereat during the holding in the second temperature range a further creation of bainite at least in the part is achieved.
2. Procedure for producing a bearing element according to claim 1 , characterized in that at least the part is located in a salt bath during the first amount of time (T8-T7) and / or during the second amount of time (T 10-T9).
3. Procedure for producing a bearing element at least according to claim 1 or claim 2, characterized in that the first temperature range is the temperature range between 200°C and 250°C.
4. Procedure for producing a bearing element at least according to one of the claims 1 to 3, characterized in that the first amount of time is at least three hours.
5. Procedure for producing a bearing element at least according to one of the claims 1 to 4, characterized in that the second temperature range is the range from 235°C to 260°C.
6. Procedure for producing a bearing element at least according to one of the claims 1 to 5, characterized in that the second amount of time is between 150 minutes and 16 hours.
7. Procedure for producing a bearing element at least according to one of the claims 1 to 6, characterized in thatsteel of the steel component contains 0.5 - 5.0 weight percent Chromium, 0.1 - 5.0 weight percent Molybdenum and 0.1 - 0.6 weight percent Carbon.
8. Bearing element, which is produced according to at least one of the claims 1 to 7.
9. Bearing element according to claim 8, characterized in that the bearing element is a rolling bearing element with a running surface area, at which residual stresses are lower than -250 Megapascal in a complete depth range between 0 millimeter to 0.5 millimeter below the surface.
10. Bearing element according to at least one of the claims 8 or 9, characterized in that the bearing element is a rolling bearing element with a running surface area, which has a higher hardness than 58 HRC.
Citation Information
Patent Citations
OBJECT MADE OF STEEL WITH HIGH HARDNESS AND TIGHTNESS AND METHOD FOR ITS MANUFACTURE
DE69811055T2
Bainite hardening
EP0896068A1
Method for heat treating a steel component
EP2714944A1
Toroidal-type continuously variable transmission
JP2004150592A
Carburized parts and their manufacturing methods
JP4688727B2