Photochromic materials

The production of photochromic yttrium oxyhydride powders through mechanochemical processing addresses the durability and scalability issues of existing photochromic materials, enabling versatile applications with enhanced performance and longevity.

WO2024227936A1PCT designated stage expired Publication Date: 2024-11-07INSTITUTT FOR ENERGITEKNIKK

Patent Information

Application Number
PCT/EP2024/062318
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-03
Filing Date
2024-05-03
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Current photochromic materials, particularly organic ones, suffer from fatigue and degradation issues when repeatedly cycled between clear and dark states, limiting their durability and suitability for applications like smart windows and paints, while inorganic materials lack coloration related to opacity and scalable production methods are not available for rare-earth oxyhydrides in particulate form.

Method used

A method involving mechanochemical processing of metallic yttrium to produce yttrium hydride followed by oxidation to create photochromic yttrium oxyhydride powders, allowing for scalable production and tailoring of photochromic properties, enabling applications in smart windows, contact lenses, and other uses.

Benefits of technology

The method produces highly photochromic yttrium oxyhydride powders with adjustable properties, enhancing durability and scalability, suitable for a range of applications including energy-saving smart windows and ophthalmic uses, with improved resistance to UV light and prolonged material lifetime.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 000026
    Figure 000026
  • Figure 000027
    Figure 000027
  • Figure 000028
    Figure 000028
Patent Text Reader

Abstract

The invention provides a method for the preparation of a particulate photochromic material containing yttrium oxyhydride (YHO). The method comprises the following steps: (a) subjecting metallic yttrium to mechanochemical processing in the presence of hydrogen gas whereby to produce particulate yttrium hydride; and (b) subjecting the particulate yttrium hydride to oxidation.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Photochromic materials

[0002] Technical field

[0003] The present invention relates to photochromic materials, to methods for their production and their use. Such materials have the property of being able to alter their optical properties reversibly on exposure to light.

[0004] More particularly, the invention relates to photochromic materials which comprise particles of yttrium oxyhydride and to methods for their production. The ability to produce these materials in finely divided (i.e. particulate) form, for example as powders, enables their use in a wide range of applications. For example, these find use in the production of energy-saving smart windows, optical sensors, sunglasses, and in paints and dyes. The method for production of the materials is readily scalable for mass production and the processing parameters can be controlled to tailor their photochromic properties.

[0005] Background of the invention

[0006] Photochromism describes the transformation of a chemical species between two states by the absorption of electromagnetic radiation. Photochromic materials which respond to visible or ultraviolet light by reversibly changing their colour are well known. Such materials have two states with an absorption band in the visible or ultraviolet part of the electromagnetic spectrum which changes dramatically in strength or wavelength.

[0007] To date, photochromism has been most thoroughly investigated in organic materials. Such materials include triarylmethanes, fulgides, nitrones, stilbenes, spiropyrans and spiro-oxazines. The nature of the chemical change varies depending on the material but includes cis-trans isomerisation, for example, but common to all photochemical reactions is that they result in an increased absorption of light in the visible light spectrum. Organic photochromic materials are used commercially, for example in switchable sunglasses and in photochromic glass which is used in smart windows to change their transparency based on outdoor illumination. Although highly functional, all organic photochromic materials suffer fatigue to some extent, i.e. the loss of reversibility and contrast, kinetics of coloration and bleaching, due to processes such as photodegradation that may be caused by repeated cycling between their clear and photo-darkened states on exposure to illumination or due to their age. This lack of durability makes organic photochromic materials less suitable for any application in which a long lifetime is desirable, such as in paints and in smart windows. Their complex fabrication methods and high cost are also drawbacks where they are required for use in large quantities, for example in the production of smart windows.

[0008] Inorganic photochromic materials are also available. Unlike the organic materials, they do not suffer from degradation and can be deposited by scalable methods, but their coloration is related to opacity to visible light. Inorganic materials known to exhibit photochromism include, for example, the oxides of molybdenum, tungsten, vanadium, titanium, and zinc.

[0009] Photochromic materials based on yttrium have been investigated and include yttrium oxyhydride, i.e. yttrium hydride which is doped with oxygen. However, to date, the methods used to produce such materials have been limited to the production of thin films. For example, the fabrication of photochromic yttrium oxyhydride films using reactive sputter deposition in which metallic yttrium is sputtered in a hydrogen atmosphere and the thus obtained yttrium hydride is oxidized in atmosphere is described in Mongstad et al., Solar Energy Materials & Solar Cells 95 (2011) 3596-3599.

[0010] In WO 2018 / 024394, an initial reactive sputter deposition of an yttrium hydride thin film is followed by subsequent treatment with oxygen to produce an yttrium oxyhydride-based photochromic thin film. Reaction of the metal hydride with oxygen-containing substances such as H2O, O2 and CO2 forms a multiphase material consisting of a mixture of metals, oxides, and oxyhydrides of yttrium and results in a thin film possessing photochromic properties. Photochromism of rare earth metal oxyhydride thin films has also been demonstrated by Cornelius et al., J. Phys. Chem, Lett. 2019, 10, 1342-1348, for example. Several powder forms of photochromic materials based on metal oxides have been produced. However, producing photochromic powder from the emerging new materials of rare-earth metal oxyhydrides has so far been unsuccessful. A method of producing a rare-earth oxyhydride powder from neodymium has been reported in Wideroe et al., Journal of Solid State Chemistry 184 (2011) 1890-1894. However, the resulting material did not exhibit any photochromic property. Zapp et al., Inorg. Chem. 2019, 58, 21 , 14635-14641 describe four different methods for the synthesis of yttrium hydride oxide (YHO) powders using: (a) yttria (Y2O3) and yttrium hydride (YH3); (b) yttria and calcium hydride (CaH2); (c) yttrium hydride and calcium oxide (CaO); and (d) yttrium oxide fluoride (YOF) and alkaline hydride AH (A = Li or Na). However, as evidenced herein, the YHO materials produced by these methods are not photochromic.

[0011] The present inventors have now developed a fabrication method for the production of photochromic yttrium oxyhydride powders. The method is readily scalable to enable the production of a large volume of highly photochromic material in which the processing parameters can be adjusted to tailor the properties of the material. The ability to fabricate a photochromic yttrium oxyhydride in particulate form, for example as a powder, opens up the possibility of new applications for such materials such as photochromic contact lenses, goggles, spectacles, etc.

[0012] Summary of the invention

[0013] The present invention provides a method for the production of a particulate photochromic material containing yttrium oxyhydride. More specifically, it provides a method to produce photochromic yttrium oxyhydride-based powders. The method involves an initial hydrogenation process to produce yttrium hydride in the form of particles (e.g. as a powder), for example by reactive ball-milling, followed by treatment with an oxidising agent which allows for a reaction between the yttrium hydride and oxygen to produce the particulate photochromic material.

[0014] As used herein the term “yttrium oxyhydride” refers to yttrium hydride that contains oxygen, i.e. to oxygen-containing yttrium hydride. Yttrium oxyhydride may also be referred to as “yttrium hydride oxide” or “YHO”. In one aspect the invention provides a method for the preparation of a particulate photochromic material containing yttrium oxyhydride, said method comprising the following steps:

[0015] (a) subjecting metallic yttrium to mechanochemical processing in the presence of hydrogen gas whereby to produce particulate yttrium hydride; and

[0016] (b) subjecting the particulate yttrium hydride to oxidation.

[0017] In another aspect, the invention provides a particulate photochromic material comprising, consisting essentially of, or consisting of yttrium oxyhydride, wherein said material is obtainable, obtained or directly obtained by a method as herein described.

[0018] In another aspect, the invention provides a particulate photochromic material comprising, consisting essentially of, or consisting of yttrium oxyhydride.

[0019] In another aspect, the invention provides the use of a particulate photochromic material containing yttrium oxyhydride in the production of a paint, a dye, contact lenses, goggles, spectacles, or smart windows.

[0020] In another aspect, the invention provides a paint, a dye, contact lenses, goggles, spectacles, or smart windows comprising a particulate photochromic material containing yttrium oxyhydride.

[0021] Detailed description of the invention

[0022] The production method according to the invention involves an initial step of mechanochemical processing of metallic yttrium in a hydrogen atmosphere. The term “mechanochemical processing” as used herein refers to a method in which a chemical reaction is initiated by means of mechanical energy input. This step is performed in a hydrogen atmosphere such that the metallic yttrium is reduced in size to form particles or aggregates of particles and undergoes a mechanochemical reaction whereby it is converted to its hydride. In one embodiment, the yttrium is converted to yttrium dihydride (YH2). This step is followed by oxidation of the particulate yttrium hydride to generate yttrium oxyhydride having photochromic properties.

[0023] For use in the method of the invention, the metallic yttrium should have a high degree of purity. Generally, the elemental yttrium will have a purity of at least 95%, at least 96%, at least 97%, at least 98% or at least 99%. In one embodiment, the yttrium has a purity of at least 99.5%. In another embodiment, the yttrium has a purity of at least 99.9%. Elemental yttrium having a purity of 99.99% is available from various commercial suppliers, for example Stanford Advanced Materials (California, USA) or Plasmaterials, Inc. (California, USA).

[0024] In one embodiment, the metallic yttrium is employed in the form of beads or lumps. Where yttrium is used in the form of beads, these may range in size (diameter) from about 1 mm to about 10 mm.

[0025] Any mechanochemical method in which sufficient energy is transferred to the reactants, i.e. elemental yttrium and gaseous hydrogen, to “activate” their chemical reaction may be used in the method of the invention. Since one of the reactants (i.e. hydrogen) is in a gaseous state, the reaction is most conveniently performed in a closed environment.

[0026] In one embodiment, mechanochemical processing is performed by ball-milling of metallic yttrium in the presence of hydrogen gas. This method is also referred to herein as “reactive ball-milling”. Ball-milling is a technique well known in the art in which balls are used in a ball-mill to grind a solid material. Size reduction of the solid material is achieved as it is trapped between colliding balls (also known as “milling balls”) contained in a hollow cylinder (known as a “milling vial”) which is agitated at high speed I frequency. The balls may be made of steel, hardened steel, stainless steel, or ceramic materials (e.g. titanium carbide or silicon carbide). In one embodiment, the balls are made of stainless steel or hardened steel. In one embodiment, the milling vials are made of stainless steel or hardened steel.

[0027] In one embodiment, the metallic yttrium is ball-milled in a planetary ball-milling machine. Examples of suitable types of ball-milling machines include those supplied by FRITSCH (for example, the Pulverisette 6 model) and by RETSCH GmbH, Germany (for example, the PM 100 model).

[0028] The milling vial may have a volume of 10 to 500 mL, preferably 100 to 400 mL, more preferably 200 to 250 mL. The balls for use in the ball-milling process are spherical and may have a diameter in the range of from 2 to 20 mm, preferably from 5 to 15 mm, e.g. from 8 to 12 mm. In performing the step of reactive ball-milling, the ball mill may be rotated with a rotational velocity of 250 to 550 rpm, for example 300 to 500 rpm, or 350 to 450 rpm.

[0029] In principle, reactive ball-milling can be carried out using any number of balls. However, the number of collision events in which the mechanical energy is transferred to the reactants is decreased when using a lower number of balls. As a result, a longer milling time may be required. The number of balls used during the milling process may readily be selected by those skilled in the art depending on the desired extent of comminution (i.e. size reduction), the amount of yttrium material and the desired milling time. For example, it may be chosen so that the ball to starting material mass ratio is within the range 1 :10 to 1000:1 , preferably 1:1 to 100:1, more preferably 10:1 to 50:1. The ball to starting material mass ratio is calculated by dividing the total weight of the balls by the total weight of the starting material.

[0030] The milling time will vary depending on factors such as the ball-to-powder weight ratio, the rotational speed of the ball mill, and the desired extent of size reduction of the yttrium material. Suitable milling times may readily be determined by those skilled in the art. In one embodiment, the method involves ball milling for at least 5 hours, preferably at least 10 hours, at least 15 hours or at least 20 hours to form a particulate yttrium hydride material. In one set of embodiments, ball milling may be performed for 5 to 20 hours, e.g. for 5 to 10 hours.

[0031] As will be understood, the temperature of the ball-milling process will be governed by the mechanical energy transferred (i.e. dissipated) to the powder. The temperature therefore depends on the ball-to-powder mass ratio and milling intensity, i.e. rotational velocity. Ball mills should be operated at the manufacturer’s recommended operating temperatures. Typically, the material may be ball-milled at a temperature in the range of from 30 to 70°C, preferably 40 to 60°C, more preferably 45 to 55°C. If appropriate, the temperature of the milling vial can be reduced by cryogenic cooling.

[0032] Mechanomechanical processing of the metallic yttrium is carried out under a hydrogen atmosphere in order to produce yttrium hydride. When using a ball-mill, for example, the milling chamber may be provided with a gas inlet to allow the introduction of hydrogen gas. Prior to the introduction of hydrogen gas, the chamber may be evacuated to remove any air, for example using a vacuum pump. After reaching a vacuum of approximately 3 to 10 mbar, the milling vial may be filled with hydrogen gas via the gas inlet. Suitable hydrogen pressures may readily be determined by those skilled in the art, but may suitably be in the range from 5-100 bar, for example 10-100 bar, 20-60 bar, or 40-50 bar.

[0033] The lid of the vial may be provided with a pressure transducer and thermometer to monitor the pressure and temperature inside the milling vial. Initially, the hydrogen pressure within the vial can be expected to increase due to the temperature increase generated by the milling process. It will then start to decrease as hydrogen is absorbed by the ball-milled material. When a constant hydrogen pressure is reached, it may be assumed that the ball-milled material is saturated with hydrogen.

[0034] Mechanochemical processing should be carried out substantially in the absence of any liquid, in particular in the absence of water. Any ball-milling method will thus be considered “dry” ball-milling. The presence of oxygen, e.g. air, should also generally be avoided during the mechanochemical processing step.

[0035] Optionally, the mechanochemical processing step may be repeated one or more times. For example, at least one additional ball-milling step may be performed in the presence of hydrogen gas. In this way, the homogeneity of the powder in terms of the hydrogen content may be improved. Alternatively, one or more additional mechanochemical processing steps, such as ball-milling, may be performed in order to further reduce the particle size of the material once yttrium hydride has been obtained. In this case, the additional mechanochemical processing steps (e.g. ball-milling) need not necessarily be performed in the presence of hydrogen gas. Where any additional ball-milling steps are carried out, the milling balls used may be the same or different in the different steps. For example, an initial (i.e. “rough”) ball-milling process may be carried out using stainless steel balls to obtain particles or aggregates of particles of yttrium hydride having a first diameter, followed by a second ball-milling process using different milling balls, for example milling balls made of a different material (e.g. zirconium balls) and / or having different dimensions (e.g. a smaller diameter), to produce particles or aggregates of particles having a second diameter which is smaller than the first diameter.

[0036] During ball-milling the material is continuously fractured and cold welded together. Ball-milling will typically be performed until no more hydrogen is absorbed, i.e. until all yttrium has reacted with hydrogen. This point can be determined by monitoring the hydrogen pressure in the milling vial. Following ball-milling, the resulting material is thus expected to be mainly yttrium hydride, for example yttrium dihydride (YH2). In one embodiment, the resulting material consists essentially of or consists of yttrium hydride. In another embodiment, the material consists essentially of or consists of yttrium dihydride (YH2).

[0037] Following completion of the mechanochemical processing step (e.g. reactive ballmilling), the obtained yttrium hydride particles may have a maximum particle size (diameter) of between 5 nm and 1 pm, preferably 10 nm to 700 nm, more preferably 70 nm to 400 nm.

[0038] The yttrium hydride particles are then subjected to oxidation in order to convert the yttrium hydride to yttrium oxyhydride (YHO). Oxidation may be performed by exposure to dry air. The water content in dry air is equivalent to a relative humidity (RH) of up to 10% at 25°C. As referred to herein, “humidity” refers to water vapour or liquid water in air. Alternatively, oxidation may be carried out by exposure to any of the following oxidation agents: hydrogen peroxide, hydrogen peroxide solution, oxygen or an oxygen-containing gas, and ozone. Any combination of these treatments may also be employed.

[0039] Oxidation may be performed in the same ball-milling chamber used for mechanochemical processing. In this case, any unreacted hydrogen is first removed from the chamber (e.g. by creating a vacuum), followed by the introduction of the oxidation agent, such as dry air.

[0040] Alternatively, the yttrium hydride may be transferred to a separate environment in order to perform the step of oxidation. Prior to oxidation, the yttrium hydride material is highly reactive and should be handled with care. During transfer to another environment for oxidation, the material should ideally be maintained in an inert atmosphere. For example, it may be kept under argon or nitrogen, preferably under argon.

[0041] The environment in which oxidation is performed should be substantially free from water. In this context, water includes both liquid water and water vapour. An environment having a water content of less than 10 ppm, preferably less than 1 ppm, e.g. less than 0.1 ppm, is appropriate. The temperature of the environment for oxidation should preferably be maintained at below 125°C. Typically, oxidation will be performed at ambient temperature, i.e. at a temperature in the range of from 18 to 25°C.

[0042] The incorporation of oxygen during the oxidation step will be directly related to the amount of hydrogen introduced during the first step of the process. In treating the yttrium hydride particles with oxygen, the oxygen will react with the material, initially causing an oxide layer to form on the exposed outer surface of the particle. On prolonged exposure, oxygen will penetrate into the interior of the particles. An equilibrium in the oxidation process will be reached once the oxidation reaction has caused the formation of oxygen-rich phases of sufficient depth to impose an impenetrable barrier to the further diffusion of oxygen. The speed and extent of the oxidation process will be dependent on the porosity and size of the particles. The final oxygen content of the material can be adjusted by controlling the temperature and duration of the oxidation reaction, and the concentration of oxygen (e.g. the pressure of any oxygen-containing gas).

[0043] Whilst not wishing to be bound by theory, the inventors postulate that the final photochromic particles may have a “core-shell” structure in which the amount of oxygen may vary from the exterior surface (i.e. shell) to the interior of the particle. For example, the core may comprise a reduced amount of oxygen (or no oxygen), for example due to the diffusion barrier as described above. The thickness of the shell and thus the composition of the final photochromic particles, specifically the oxygen to yttrium atomic ratio may thus vary throughout the particles.

[0044] In some embodiments, the thickness of the active photochromic shell (outer layer) may be adjusted as required, for example in order to provide the desired balance between optical transparency and optical modulation (the difference in transmittance of visible light between the clear and photo-darkened states of the material). For example, a thicker layer may increase the photochromic modulation caused by incident light but will present a lower optical transmissivity. On the other hand, a layer that is too thin will exhibit high transmittance but lower photochromic modulation. Thus, the photochromic effect and contrast between maximum transmission and maximum absorption may be adjusted as a function of the particle size and the thickness of the shell.

[0045] The reaction between the yttrium hydride and the oxygen during the treatment with oxygen can be controlled by adjusting the temperature and moisture level during this treatment step. A higher temperature will result in a higher diffusivity of oxygen resulting in a higher degree of oxidation. Increasing the moisture content will have the same effect due to the increased availability of oxygen and the different activation energy for the oxidation process in the presence of water.

[0046] The concentration of oxygen used to treat the yttrium hydride may vary but should be sufficient to obtain the desired oxygen-yttrium atomic ratio. The oxygen treatment results in a material having increased photochromic properties compared to the initial yttrium hydride.

[0047] The oxidation process should be carefully controlled. In particular, the temperature should be controlled such that the yttrium hydride does not burn. Burning can be avoided by maintaining the temperature of the material below about 150°C. In one set of embodiments, the temperature of the material may be maintained in the range from 100 to 125°C. In one set of embodiments, oxidation may be carried out with active cooling. The duration of the oxidation step may be varied and suitable times may readily be selected by those skilled in the art taking account of factors such as the concentration of oxygen employed and the pressure under which oxidation is performed. Oxidation may, for example, be carried out for a period of from 12 hours to one week. In one set of embodiments, the duration may be about 24 hours.

[0048] In the case where oxidation is carried out under pressure, suitable pressures may range from 1 bar to 20 bar. At higher pressures, active cooling may be desirable in order to keep the temperature of the material below about 125°C. Active cooling may be achieved by carrying out oxidation during cryogenic ball milling in which the milling vial is cooled using liquid nitrogen.

[0049] The resulting yttrium oxyhydride is produced in the form of a particulate material, i.e. it comprises a plurality of particles. As used herein, the term “particle” refers to a volume of the material in which the crystal lattice is continuous. A particle may be approximately spherical or have other geometries. An aggregate of particles is defined as a cluster of densely packed particles.

[0050] In one set of embodiments, the particulate material is provided in the form of microparticles or aggregates of microparticles. As used herein the term “microparticle” refers to a particle having at least one dimension (e.g. a diameter) which is less than about 1 mm.

[0051] In one set of embodiments, the particulate material is provided in the form of nanoparticles or aggregates of nanoparticles. As used herein, the term “nanoparticle” refers to a particle having at least one dimension (e.g. a diameter) which is less than about 1 pm.

[0052] It will be understood that the terms “particle”, “microparticle” and “nanoparticle” as used herein do not imply any particular shape, but include all known shapes including, but not limited to, a sphere, a rod, and any other substantially spherical shape such as an ovoid. A core-shell particle will comprise a core having a composition which is distinct from its surrounding shell.

[0053] In one set of embodiments, the particulate material may be provided in the form of a free-flowing powder.

[0054] As shown in the accompanying examples, the inventors have used X-ray diffraction to show that the main peaks of the produced material are shifted compared to that of the starting material YH2 prior to oxidation. These X-ray results fit well with earlier literature for photochromic rare earth oxyhydrides in the form of thin films (see Montero 2017 and Cornelius 2019). The results confirm the particulate material has at least one photochromic YHO phase.

[0055] The photochromic yttrium oxyhydride material which is produced by the method herein described is novel and also forms part of the invention.

[0056] In a further aspect the invention thus provides photochromic yttrium oxyhydride in particulate form obtained, directly obtained, or obtainable by any method as herein described. In particular, the invention provides a photochromic yttrium oxyhydride- based powder obtained, directly obtained, or obtainable by any method as herein described.

[0057] In a yet further aspect, the invention provides photochromic yttrium oxyhydride in particulate form. In particular, the invention provides a photochromic yttrium oxyhydride-based powder.

[0058] As used herein, the term “photochromic” means that the yttrium oxyhydride reversibly transitions between first and second states when exposed to electromagnetic radiation in the visible or ultraviolet part of the spectrum, the first and second states having absorption bands in the visible or ultraviolet part of the electromagnetic spectrum that change in strength or wavelength. Specifically, the second photochromic state is a photo-darkened state with respect to the first photochromic state, i.e. the second photochromic state has an increased absorption of wavelengths across the visible or ultraviolet spectrum with respect to the first photochromic state. In one embodiment, the yttrium oxyhydride material according to the invention is photochromic with a dynamic contrast between about 20 to about 60%. In another embodiment, the yttrium oxyhydride material according to the invention is photochromic with a dynamic contrast between about 50 and 60%. Dynamic contrast is defined as the difference in transmittance between the photo-darkened and non-photodarkened states of the photochromic material.

[0059] By controlling the hydrogen and oxygen incorporated into the material, the transparency and degree of photodarkening of the material can be controlled. The production process is thus capable of the large-scale production of photochromic materials with tailored properties for a range of applications.

[0060] In some embodiments, the yttrium oxyhydride powder has a particle size of from 0.1 nm to 100 pm, preferably from 1 nm to 10 pm, more preferably from 5 nm to 1 pm. Particle size may be measured by SEM, for example using a Zetasizer.

[0061] The particulate nature of the photochromic materials according to the invention enables their use in a broad range of applications as herein described. Their particulate nature permits their dispersion in a range of solid or liquid carriers. Any liquid or solid carrier containing particles of the photochromic material forms a further aspect of the invention. The magnitude of the photochromic effects may further be adjusted by varying the properties of the carrier material and / or by varying the concentration of the photochromic particles. Suitable carrier materials may include, but are not limited to, polymers, glasses, paints, dyes and inks.

[0062] A particular application for the materials is in the production of energy-saving smart windows. Photochromic windows offer a solution to the problem of glare and unwanted heating due to direct illumination and require only light to function. Upon illumination with sunlight, the photochromic material alters its transmission properties to control the passage of visible light. This state is reversed when the illumination is removed. For use in buildings, a photochromic window which is transparent in the non-illuminated state but dim under illumination is ideal. Such dynamic optical transmissivity allows the material to adapt to climatic demands thus reducing CO2 emissions associated with buildings. When used in the production of smart windows the photochromic material may be dispersed in the glass during manufacture. Alternatively, it may be embedded in a substantially transparent coating material which is applied as a coating on the glass or on a polymer substrate for use in the window industry. For example, the photochromic particles may be dispersed in a polymer solution which can be applied to the surface of the glass or the polymer substrate by conventional techniques such as painting, spray coating, dip coating, spray pyrolysis, atmospheric plasma deposition, etc. The thickness of the coating may be varied as desired. The photochromic coating may be adapted to decrease the visible light transmission when exposed to ultraviolet light. In one embodiment, the photochromic coating is adapted to absorb at least 10%, preferably at least 40%, e.g. at least 60% visible light in response to exposure to UV light.

[0063] Transparent substrates can include organic and inorganic materials. In one embodiment, the substrate may include a transparent polymer. The transparent polymer may be selected from a polyacrylate, a polyester, a polycarbonate, a polysiloxane, a polysilazane, a polyether, a polyvinyl compound, or any combination thereof.

[0064] In one embodiment, the transparent polymer includes a polyacrylate. The polyacrylate can be a poly(methylacrylate), a poly(ethylacrylate), a poly(propylacrylate), a poly(vinylacrylate), a poly (methyl methacrylate), a poly (ethyl methacrylate), a poly(propyl methacrylate), a poly(vinyl methacrylate), a poly(vinyl pyrrolidone) or a mixture thereof. In another embodiment, the polyacrylate can be a copolymer of two, three, or more acrylic precursors. The acrylic precursors can include methyl acrylate, ethyl acrylate, propyl acrylate, vinyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, vinyl methacrylate. For example, a copolymeric polyacrylate can include poly (methyl methacrylate vinyl methacrylate).

[0065] In one embodiment, the transparent polymer includes a polyester. The polyester can be a polyethylene terephthalate (PET), a polyethylene naphthalate, a polybutylene terephthalate, a polyethylene isonaphthalate, or any combination thereof. In one embodiment, the transparent polymer includes a polyether. The polyether can be polyethylene ether, poly propylene ether, polybutylene ether, or any combination thereof. In another embodiment, the polyether can be a copolymer of two, three, or more polyols. For example, the polyether can be a copolymer of 1,2- ethanediol, 1,2-propanediol, 1,3- propanediol, 1 ,2-butanediol, 1,3-butanediol, 1,4- butanediol.

[0066] In one embodiment, the transparent polymer can be a polyvinyl compound. The polyvinyl compound can be a polyvinyl alcohol, a polyvinyl ester, a polyvinyl acetal, a poly(vinyl pyrrolidone) or any combination thereof. In another embodiment, the polyvinyl compound can be a copolymer of a vinyl alcohol derivative and an olefin. The vinyl alcohol derivative can be vinyl acetate. In one embodiment, the polyvinyl compound can be poly(ethylene vinyl acetate).

[0067] In one embodiment, the transparent polymer can be a polysilazane. Polysilazanes are polymers having a silicon-nitrogen backbone. They can be used as high performance binders due to their dense Si-O-Si and Si-N-Si network and are suitable precursors for ceramic materials.

[0068] Other applications for the photochromic powders herein described are in ophthalmology, such as photochromic contact lenses, or as coatings on goggles or spectacles (e.g. sunglasses). In one embodiment, the photochromic particles may thus be dispersed in contact lenses to provide photochromic contact lenses.

[0069] The particulate (e.g. powder) form of the photochromic materials aids their deposition on substrates that have uneven surfaces. For example, these can be deposited by dispersion in a liquid carrier which is readily painted, spray coated, dip coated or spin-coated onto a surface.

[0070] The photochromic materials may also be incorporated into paints, dyes or inks. Inks can be printed using an inkjet printing machine.

[0071] Due to the ability of yttrium oxyhydride to absorb UV light, a further advantage of the photochromic materials herein described is their capability to prolong the lifetime of host materials or substrates that are sensitive to UV light (e.g. organic materials).

[0072] The invention is illustrated further by way of the following non-limiting Examples and the accompanying figures, in which:

[0073] Figure 1 : Pressure and temperature in the vial as a function of milling time. Milling is stopped after 5 hours.

[0074] Figure 2: Photochromic YHO powder showing increased absorption and photodarkening after illumination with UV light (upper figure); and recovery to initial state after storage in the dark (lower figure).

[0075] Figure 3: Photochromic properties of YHO powder demonstrated through photodarkening and bleaching by UV illumination: (a) reflectance and (b) absorptance values demonstrate the optical modulation before illumination (“initial” - circles), after illumination (“90 minutes” - downward triangles) and after storage in the dark (“5 minutes bleaching” - upward triangles). Reference glass (squares) is shown in the reflectance graph.

[0076] Figure 4: X-ray diffraction pattern for photochromic YHO powder vs. YH2 which is the starting material prior to oxidation. Main peaks are shifted to lower angles due to oxidation.

[0077] Figure 5: Free-standing polymer layer formed from polystyrene and photochromic YHO powder before illumination (left hand figure) and after illumination (right hand figure). Images demonstrate photo-darkening of part of the film after UV illumination.

[0078] Figure 6: Photo-darkened YHO / polystyrene film demonstrates photochromism under UV illumination. Illumination performed using a mask such that letters and bars at the sides are formed by UV illumination.

[0079] Figure 7: SEM of YHO showing clusters of nanoparticles. The top two images show sub 300 nm clusters. Figure 8: Reflectance spectra of YHO powder synthesised according to the method of Zapp et al. (Inorg. Chem. 2019, 58, 21 , 14635-14641) before and after UV illumination.

[0080] Figure 9: Photochromic properties of YHO powder demonstrated by subjecting a pressed palette of YHO powder to UV light and measuring reflectance changes with UV “ON / OFF” cycles. Contrast (%) is determined based on normalised reflection values from the RED component of captured images (background adjusted).

[0081] Examples

[0082] Example 1 - Preparation of photochromic yttrium oxyhydride (YHO)

[0083] The yttrium starting material either as powder or as lumps was ball milled using a Fritsch Pulverisette 6 planetary ball mill operating at 400 rpm. The milling vial and milling balls were made of hardened steel. The lid of the milling vial was equipped with a gas inlet with a valve to evacuate the inner volume of the ball milling vial or to fill the volume with a gas. The lid of the vial was equipped with a pressure transducer and thermometer to monitor the pressure and temperature inside the milling vial. The number of balls used during the milling process was chosen so that the ball to starting material mass ratio was about 40:1.

[0084] After loading the starting material and the balls, the lid of the milling vial was tightened to make the milling vial air- and gas-tight. The milling vial was then connected to a vacuum pump via the gas inlet of the lid in order to evacuate any air in the milling vial. After reaching a vacuum of approximately 10-3 mbar, the milling vial was filled with H2 until a pressure of 44 bar was achieved.

[0085] Once filled with H2 gas, the milling vial was mounted in the planetary ball mill and the milling process was started. The milling process was carried out for 5 hours.

[0086] The milling vial was equipped with pressure and temperature sensors placed in the lid together with a radio transmitter to send pressure and temperature data to a PC. Figure 1 shows how the H2 pressure and temperature inside the milling vial changed during the 5-hour milling run and for 1 hour after the end of the milling process. In the initial stages of the milling process (up to 1 hour), the temperature of the vial increased steeply from room temperature up to about 50°C. In the intermediate stages of milling, the temperature moderately increased. This increase in temperature is typical for planetary ball mills and is mostly due to the impact and attrition of the balls on the internal walls of the vial. A constant temperature was reached after about 3 hours of milling at which point an equilibrium between the heat generated by the balls and the heat dissipated by the vial was attained. The temperature of the vial at the point of equilibrium was 52.5°C. As soon as the milling ended, the mill and its cooling fans switched off automatically. This results in a slight increase of the temperature of the vial, which then cools down to room temperature.

[0087] As can be seen from Figure 1 , the H2 pressure increased during the first minutes of milling due to the temperature increase but started to decrease as H2 was absorbed by the ball milled material. Hydrogen absorption (and the pressure decrease) proceeded for about 1 .5 hours of milling. After that, the H2 pressure remained constant, indicating that the ball milled material was saturated with hydrogen. As soon as the milling ended, some changes in the value of the pressure were observed, reflecting the automatic stop of the mill and changes of the vial temperature. The overall change in H2 pressure measured at room temperature inside the vial before and after the milling run was AP = 10 bar. Taking account of the internal volume of the vial not occupied by the milling balls and by the ball- milled material, this change in pressure corresponds to about 7.8 x102mol of H2 absorbed by the yttrium material.

[0088] Following the reactive ball milling process, the obtained yttrium hydride particles were absorptive black in appearance and highly volatile under air. The particles were then oxidised by exposure to dry air having the following composition: 5-15% O2; remainder N2 (H2O content < 10ppm). The obtained yttrium oxyhydride particles had a particle size (diameter) of between 200 nm and 1 pm as measured usng a Zetasizer (Particle Size Analyzer). Example 2 - Properties of photochromic yttrium oxyhydride (YHO)

[0089] The following tests were carried out in respect of the yttrium oxyhydride (YHO) powder sample prepared in Example 1.

[0090] The YHO powder was placed in a circular vial for steady observation and illuminated by a 405nm peak Thorlabs purple laser with 4.5mW / cm2intensity for 60 minutes. The resulting image is shown in Figure 2. The upper figure shows the area after illumination with UV light and the lower figure shows the same area after 60 minutes storage under dark. These results demonstrate reversible photochromism.

[0091] Optical reflectance (R) of the YHO powder in the clear state (“Initial”), after illumination (“After 90 minutes UV illumination”), and after partial recovery under dark (“5 Minutes bleaching”) were obtained with an integrated sphere using an Ocean Optics QE6500 spectrophotometer (Dunedin, FL, USA) between 350nm and 900nm and compared to a reference glass sample (“Reference Empty Glass”). Absorption was calculated by: T+R+A=1 where transmittance of the powder was 0. Measurements were performed by placing the powder samples between two borosilicate laboratory slides. The results are shown in Figure 3 and confirm photochromic properties of the YHO powder by photodarkening and bleaching by UV illumination.

[0092] The crystallographic structures of the YHO powders were characterized by grazingincidence X-ray diffraction (GIXRD) in a Bruker Siemens D5000 (CuKa radiation, parallel beam geometry and 2° angle of incidence) (Billerica, MA, USA). The diffraction peaks show good correlation with standard diffraction peaks of YH2 obtained from the Joint Committee of Powder Diffraction Standards (JCPDS), card number 04-006-6935. The diffractions peaks of the YHO powders were shifted to lower angles due to oxidation.

[0093] Free standing YHO layers were prepared by a cast deposition method. YHO powders were dispersed via an ultrasonic probe homogenizer (Bandelin, Sonoplus) for 120 seconds in a polystyrene (PS) solution (30-60 mg / ml in toluene). After casting the YHO dispersed solution, it was left to dry for at least 6 to 12 hours. Figure 5 shows the resulting free-standing polymer layers. The left image shows the sample before illumination and, in the right image, the sample is shown after illumination with the same 405nm peak Thorlabs purple laser mentioned above. The dashed lines highlight the same area for the images.

[0094] A casting method was deployed on glass substrates using the YHO dispersed PS solution. After drying for more than 6 hours, a Si wafer mask with “IFE” engraved on it was placed and illuminated with an AM 1.5G solar simulator for excitation. The image in Figure 6 shows the letters “IFE” as a result of photodarkening. The rest of the surface remained in its initial state.

[0095] Images of the YHO powder were obtained by Hitachi S-4800 field emission SEM under 5.0kV acceleration and are shown in Figure 7. The images have the following magnification (from top to bottom): 180kx; 100kx; 35kx; and 10kx. The top image shows smaller than 300nm clusters. The apparent agglomeration indicates that even smaller sizes of particles were obtained during production.

[0096] Comparative Example 3 - Properties of yttrium oxyhydride (YHO) powder synthesised according to Zapp et al., 2019

[0097] YHO powder synthesised according to method (a) disclosed in Zapp et al. (Inorg. Chem. 2019, 58, 21 , 14635-14641) was tested. Method (a) involves the reaction of yttria (Y2O3) and yttrium hydride (YH3).

[0098] Optical reflectance (R) of the resulting YHO powder before and after UV illumination was measured as described in Example 2. The results are shown in Figure 8. The reflectance spectra of the powder before and after illumination with UV light are the same. Thus, the powder is not photochromic.

[0099] Example 4 Properties of photochromic yttrium oxyhydride (YHO)

[0100] The following test was carried out in respect of the yttrium oxyhydride (YHO) powder sample prepared in Example 1. The powder was made into a palette using a press. The palette was subjected to UV light, 405nm Thorlabs in “On / Off” cycles for several hours. A camera was used to capture images through a long-pass filter which filtered blue light from the UV light. The images were processed to split into red, green and blue components. The red component was used to determine reflection changes during the UV “On / Off” cycles. Reflection values were normalised and adjusted to take account of any background light. Relative contrast was calculated using (Ro-R) / Ro where Ro is the initial reflection value and R is the reflection value at any given data point. The results are shown in Figure 9. This demonstrates that individual “On / Off” cycles have up to about 11% relative contrast. The contrast obtained at the end of the cycles, relative to the initial values, was about 31%.

Claims

Claims:

1. A method for the preparation of a particulate photochromic material containing yttrium oxyhydride, said method comprising the following steps:(a) subjecting metallic yttrium to mechanochemical processing in the presence of hydrogen gas whereby to produce particulate yttrium hydride; and(b) subjecting the particulate yttrium hydride to oxidation.

2. A method as claimed in claim 1 , wherein the yttrium hydride is yttrium dihydride.

3. A method as claimed in claim 1 or claim 2, wherein mechanochemical processing in step (a) comprises ball-milling.

4. A method as claimed in claim 3, wherein ball-milling is performed using a planetary ball mill.

5. A method as claimed in claim 3 or claim 4, wherein the planetary ball mill is rotated with a rotational velocity of 250 to 550 rpm, for example 300 to 500 rpm.

6. A method as claimed in any one of claims 3 to 5, wherein the ball to metallic yttrium mass ratio is in the range 1 : 10 to 1000: 1 , preferably 1 : 1 to 100: 1 , more preferably 10:1 to 50:1.

7. A method as claimed in any one of claims 3 to 6, wherein ball-milling is performed for 5 to 20 hours, e.g. for 5 to 10 hours.

8. A method as claimed in any one of claims 3 to 7, wherein ball-milling is performed at a temperature in the range of from 30 to 70°C, preferably 40 to 60°C, more preferably 45 to 55°C.

9. A method as claimed in any one of the preceding claims, wherein the metallic yttrium is exposed to hydrogen gas at a pressure in the range from 5-100 bar, for example 10-100 bar, 20-60 bar, or 40-50 bar.

10. A method as claimed in any one of the preceding claims, wherein the particulate yttrium hydride has an average particle size of between 5 nm and 1 pm, preferably 10 nm to 700 nm, more preferably 70 nm to 400 nm.

11. A method as claimed in any one of the preceding claims, wherein oxidation in step (b) is performed by exposure of the particulate yttrium hydride to any of the following oxidation agents: dry air, hydrogen peroxide, hydrogen peroxide solution, oxygen, an oxygen-containing gas, ozone, or any combination thereof.

12. A method as claimed in any one of the preceding claims, wherein oxidation is performed in an atmosphere which has a water content of less than 10 ppm, preferably less than 1 ppm, e.g. less than 0.1 ppm.

13. A method as claimed in any one of the preceding claims, wherein oxidation is performed at a temperature below about 150°C, preferably below about 125°C.

14. A method as claimed in any one of the preceding claims, wherein oxidation is carried out for a period of from 12 hours to one week.

15. A method as claimed in any one of the preceding claims, wherein oxidation is carried out at a pressure in the range from 1 bar to 20 bar.

16. A method as claimed in any one of the preceding claims, wherein the particulate photochromic material containing yttrium oxyhydride has an average particle size of from 0.1 nm to 100 pm, preferably from 1 nm to 10 pm, more preferably from 5 nm to 1 pm.

17. A particulate photochromic material comprising, consisting essentially of, or consisting of yttrium oxyhydride, wherein said material is obtainable, obtained or directly obtained by a method as claimed in any one of claims 1 to 16.

18. A particulate photochromic material comprising, consisting essentially of, or consisting of yttrium oxyhydride.

19. A particulate photochromic material as claimed in claim 17 or claim 18 having a dynamic contrast between about 20% to about 60%.

20. Use of a particulate photochromic material containing yttrium oxyhydride as claimed in any one of claims 17 to 19 in the production of a paint, a dye, contact lenses, goggles, spectacles, or smart windows.

21. A paint, a dye, contact lenses, goggles, spectacles, or smart windows comprising a particulate photochromic material containing yttrium oxyhydride as claimed in any one of claims 17 to 19.

Citation Information

Patent Citations

  • Fabrication of photochromic device

    WO2018024394A1

  • Method for producing an oxyhydride-based photochromic device

    US20220357491A1

Cited By

  • Self-recovery photochromic material and preparation method thereof

    CN122609221A