Vapor-deposited substrate, laminate for packaging material, packaging container, and packaging article

The integration of chemical recycled resin in packaging materials addresses the challenges of contaminants and thermal issues, ensuring high-quality vapor deposition layers and maintaining gas barrier properties, thus improving the performance and durability of packaging materials.

WO2024228273A1PCT designated stage expired Publication Date: 2024-11-07TOPPAN HOLDINGS INC

Patent Information

Application Number
PCT/JP2023/042976
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2023-11-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Packaging materials with recycled resin content face issues of uneven vapor deposition layers and decreased gas barrier properties due to contaminants and thermal deterioration, leading to potential cracks and reduced performance.

Method used

A vapor deposition substrate and laminate using a chemical recycled resin in a polyolefin resin film, which reduces impurities and thermal susceptibility, ensuring a high-quality vapor deposition layer and maintaining gas barrier properties.

Benefits of technology

The use of chemical recycled resin in packaging materials suppresses deterioration in gas barrier properties, even with high recycled resin content, enhancing the quality and strength of packaging containers and articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023042976_07112024_PF_FP_ABST
    Figure JP2023042976_07112024_PF_FP_ABST
Patent Text Reader

Abstract

This vapor-deposited substrate is obtained by forming a vapor-deposited layer on a substrate. The substrate is a polyolefin resin film containing a recycled resin, and the recycled resin is a chemically recycled resin. A laminate for a packaging material comprises the vapor-deposited substrate and a seal layer.
Need to check novelty before this filing date? Find Prior Art

Description

Vapor deposition substrate, laminate for packaging material, packaging container and packaged article

[0001] The present disclosure relates to a vapor deposition substrate, a laminate for packaging materials, a packaging container, and a packaging article.

[0002] Packaging materials used in packaging containers such as packaging bags are required to have various properties depending on their intended use. Therefore, in order to simultaneously satisfy these various performance requirements, packaging materials are generally composed of a laminate including a substrate and a sealant layer. A known example of such a packaging laminate is a laminate including a first layer including an inner liner and a second layer including an outer sheath, where the outer sheath is composed of a post-consumer resin (hereinafter also referred to as "PCR") that may contain contaminants such as paper, ink, and food residue (see Patent Document 1 below). Another known packaging laminate is a laminate film that includes at least a recycled polyethylene layer and a linear low-density polyethylene layer, where the recycled polyethylene layer contains 20% by mass or more of recycled polyethylene based on the total amount of the recycled polyethylene layer (see Patent Document 2).

[0003] JP 2022-552096 A JP 2023-040660 A

[0004] However, the laminate described in Patent Document 1 has the following problems when the PCR content is increased when the PCR is a recycled resin containing contaminants, i.e., a so-called material recycled resin. In the laminate described in Patent Document 1, foreign matter such as impurities, gels, and aggregates may appear on the surface of the outer sheath. When a vapor-deposited layer is formed on the surface of the outer sheath, the thickness of the vapor-deposited layer may become uneven, resulting in a decrease in barrier properties and cracks. Furthermore, in the laminate film described in Patent Document 2, foreign matter may be present on the surface of the recycled polyethylene layer containing material recycled polyethylene. When a vapor-deposited layer is formed on the surface of the recycled polyethylene layer as a barrier layer against oxygen, water vapor, etc., the thickness of the vapor-deposited layer may become uneven, resulting in a decrease in barrier properties and cracks.

[0005] An object of the present disclosure is to provide a vapor deposition substrate, a laminate for packaging materials, a packaging container, and a packaging article that can suppress a decrease in gas barrier properties even when a substrate containing recycled resin is used.

[0006] One aspect of the present disclosure provides a vapor deposition substrate comprising a substrate and a vapor deposition layer formed thereon, the substrate being a polyolefin resin film containing a recycled resin, and the recycled resin being a chemically recycled resin. According to the vapor deposition substrate, the recycled resin used in the substrate is a chemically recycled resin. Chemically recycled resins are produced by first reducing the molecular weight of discarded resin through a process, such as gasification, oilification, and monomerization via refined naphtha, or a process based on the material's characteristics, such as depolymerization, followed by polymerization. Therefore, chemically recycled resins are less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than material recycled resins, which are resins made by cleaning, crushing, and then melting resin products such as recovered used packaging materials. Furthermore, unlike material recycled resins, chemically recycled resins are not subject to heat treatments such as melting after the recycling process, making them less susceptible to thermal degradation and less likely to have foreign matter such as gels and aggregates on their surfaces. Therefore, even when a vapor deposition layer is formed on such a substrate, unevenness in the thickness of the vapor deposition layer is unlikely to occur, resulting in the formation of a high-quality vapor deposition layer. Therefore, even when a substrate containing recycled resin is used for the vapor deposition substrate, deterioration in gas barrier properties can be suppressed. One aspect of the present disclosure provides a packaging laminate comprising a vapor deposition substrate formed on a substrate with a vapor deposition layer, and a seal layer, wherein the substrate is a polyolefin resin film containing recycled resin, and the recycled resin is a chemically recycled resin. The packaging laminate can suppress deterioration in gas barrier properties even when a vapor deposition substrate formed on a substrate containing recycled resin with a vapor deposition layer is used.

[0007] The recycled resin content in the packaging laminate may be 10% by volume or more or 10% by mass or more. The higher the recycled resin content (use ratio) in the packaging laminate, the more environmental impact can be reduced. The recycled resin content in the packaging laminate is generally 10% by volume or more or 10% by mass or more, preferably 20% by volume or more or 20% by mass or more, more preferably 25% by volume or more or 25% by mass or more, even more preferably 30% by volume or more or 30% by mass or more, and particularly preferably 40% by volume or more or 40% by mass or more. Here, if it is not easy to calculate the mass ratio (mass%) after the packaging laminate is used as a packaging material, the unit of recycled resin content may be "volume %" so that it can be calculated using the film thickness ratio. In other words, the ratio of the film thickness of the layer using the recycled resin to the film thickness of the entire laminate can be used as the recycled resin content (volume %). The density of polyethylene and polypropylene, which constitute the majority of the packaging material, is 0.86 to 0.97 g / cm. 3 The range of the recycled resin content specified in volume percent generally also satisfies the value specified in mass percent.

[0008] The packaging laminate may further include a second substrate on one or both sides of the substrate, in which case the vapor deposition substrate is reinforced by the second substrate, thereby further improving the strength of the laminate.

[0009] In the laminate for packaging material, the recycled resin may be a post-consumer recycled resin (PCR). PCR can be secured in large quantities on the market, which can reduce the cost of the laminate. The recycled resin may be a combination of PCR and post-industrial recycled resin (PIR).

[0010] In the above laminate for packaging materials, the sealing layer may be a sealant film or a heat seal varnish layer.

[0011] In the above-mentioned laminate for packaging material, the vapor deposition substrate and the second substrate may be bonded together with a solventless adhesive.

[0012] The packaging laminate may further include an overcoat layer on the vapor deposition layer. In this case, the gas barrier properties of the laminate are further improved. Therefore, when the laminate is used to prepare a packaging container and contents are placed in the packaging container, deterioration of the contents due to gases such as oxygen can be effectively suppressed.

[0013] Another aspect of the present disclosure provides a packaging container obtained using the above-described packaging laminate. According to the packaging container, as already described, the chemically recycled resin contained in the substrate of the laminate is less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than materially recycled resin. Furthermore, unlike materially recycled resin, chemically recycled resin is not affected by heat treatments such as heat melting after the recycling process, making it less susceptible to thermal degradation and less likely to have foreign matter such as gels and aggregates on its surface. Therefore, even when a vapor deposition layer is formed on such a substrate, unevenness in the thickness of the vapor deposition layer is unlikely to occur, resulting in a high-quality vapor deposition layer. Therefore, a packaging container obtained using the above-described packaging laminate can suppress deterioration of gas barrier properties.

[0014] Yet another aspect of the present disclosure provides a packaging article comprising the above-described packaging container and contents to be accommodated in the packaging container. According to the packaging article, as already described, the chemically recycled resin contained in the substrate of the laminate is less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than materially recycled resin. Furthermore, unlike materially recycled resin, chemically recycled resin is not affected by heat treatments such as heat melting after the recycling process, making it less susceptible to thermal degradation and less likely to have foreign matter such as gels and aggregates on its surface. Therefore, even when a vapor deposition layer is formed on such a substrate, unevenness in the thickness of the vapor deposition layer is unlikely to occur, resulting in a high-quality vapor deposition layer. Therefore, a packaging article having a packaging container obtained using the above-described packaging laminate can suppress deterioration of gas barrier properties.

[0015] According to the present disclosure, there are provided a vapor deposition substrate, a laminate for packaging material, a packaging container, and a packaging article that can suppress a decrease in gas barrier properties even when a substrate containing recycled resin is used.

[0016] Fig. 1 is a cross-sectional view showing one embodiment of a packaging laminate according to the present disclosure. Fig. 2 is a cross-sectional view showing another embodiment of a packaging laminate according to the present disclosure. Fig. 3 is a cross-sectional view showing another embodiment of a packaging laminate according to the present disclosure. Fig. 4 is a cross-sectional view showing yet another embodiment of a packaging laminate according to the present disclosure. Fig. 5 is a cross-sectional view showing one embodiment of a packaging article according to the present disclosure.

[0017] Preferred embodiments of the present disclosure will be described in detail below. In the drawings, the same or corresponding parts are designated by the same reference numerals, and redundant explanations will be omitted.

[0018] <<Packaging laminate>> First, embodiments of a packaging laminate according to the present disclosure will be described with reference to Figures 1 to 4. Figures 1 to 4 are cross-sectional views showing various embodiments of packaging laminates according to the present disclosure.

[0019] As shown in FIG. 1 , a packaging laminate (hereinafter also referred to as "laminate") 100 includes a vapor deposition substrate 10 and a seal layer 30. As shown in FIG. 2 , the vapor deposition substrate 10 includes a vapor deposition layer 61 formed on a substrate 11. Here, the substrate 11 is a polyolefin resin film containing recycled resin, and the recycled resin is a chemically recycled resin. As shown in FIGS. 2 to 4 , the laminate 100 may further include an overcoat layer 62 on the vapor deposition layer 61 of the vapor deposition substrate 10. A layer constituted by at least one of the vapor deposition layer 61 and the overcoat layer 62 functions as a "gas barrier layer." The laminate 100 may further include a second substrate 20 between the vapor deposition substrate 10 and the seal layer 30. As shown in FIG. 2 , the laminate 100 may further include a printed layer 50. When the laminate 100 is used for a tube container, as shown in FIG. 3, the laminate 100 may further include an outer sealant layer (also referred to as a "second sealant layer") 40 on the side of the deposition substrate 10 opposite to the seal layer 30.

[0020] According to the laminate 100, even when a vapor deposition base material is used in which a vapor deposition layer is formed on a substrate 11 containing recycled resin, a deterioration in gas barrier properties can be suppressed. In addition, the content of recycled resin in the packaging laminate 100 is preferably 10% by volume or more or 10% by mass or more.

[0021] <Vapor Deposition Substrate> The vapor deposition substrate 10 is a member formed by forming a vapor deposition layer 61 on a base material 11 .

[0022] (Substrate) The substrate 11 is made of a polyolefin resin film containing recycled resin, and the recycled resin is a chemically recycled resin.

[0023] The polyolefin resin film includes polyolefin resin films, such as polyethylene and polypropylene.

[0024] Polyethylene is a resin containing ethylene as a structural unit. Examples of polyethylene include ethylene homopolymers and copolymers of ethylene with other monomers. The proportion of ethylene in polyethylene is, for example, 80 mol % or more. Examples of other monomers include α-olefins, vinyl acetate, and acrylic acid esters. The α-olefin may be an olefin having a carbon number in the range of 3 to 20. Examples of α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Examples of polyethylene include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, etc. These may be used alone or in combination of two or more.

[0025] Polypropylene is a resin containing propylene as a structural unit, but may not contain ethylene as a structural unit, and may be a copolymer of propylene alone or with ethylene or various α-olefins. Examples of polypropylene include homopolypropylene, block polypropylene, and random polypropylene.

[0026] The polyolefin resin may be a non-recycled polyolefin resin, a chemically recycled polyolefin resin, or a mixture thereof. The non-recycled polyolefin resin may be a petroleum-derived polyolefin resin obtained using a petroleum-derived raw material monomer, a biomass-derived polyolefin resin obtained using a biomass-derived raw material monomer, or a mixture thereof, but from the viewpoint of reducing the environmental load, a biomass-derived polyolefin resin is preferable. The chemically recycled polyolefin resin may be composed of a single chemically recycled polyolefin resin, or may be composed of a mixture of multiple types of chemically recycled polyolefin resins.

[0027] The substrate 11 may have either a single layer or a multilayer structure. In the case of a multilayer structure, the substrate 11 is formed from two or more layers, at least one of which contains a chemically recycled resin. The substrate 11 may also be formed by co-extrusion of a layer made of an ethylene-vinyl alcohol copolymer or a layer made of a polyamide, optionally with an adhesive resin, and stretching the resulting film. Examples include a three-type, five-layer substrate consisting of chemically recycled resin / adhesive resin / ethylene-vinyl alcohol copolymer / adhesive resin / chemically recycled resin, a three-type, three-layer substrate consisting of chemically recycled resin / adhesive resin / ethylene-vinyl alcohol copolymer, a petroleum-derived (natural) resin / chemically recycled resin / petroleum-derived (natural) resin, or a petroleum-derived (natural) resin / other polyolefin / chemically recycled resin / other resin / petroleum-derived (natural) resin. In the multilayer substrate 10, materials of the same type may have different specific gravities depending on their functions.

[0028] The substrate 11 may further contain additives such as a filler, an antistatic agent, a plasticizer, a lubricant, a light-shielding pigment, and an antioxidant, as necessary. When the substrate 11 contains a light-shielding pigment, the substrate 11 can function as a light-shielding layer.

[0029] The substrate 11 may be an unstretched film or a stretched film. The stretched film may be a uniaxially stretched film or a biaxially stretched film. The deposition substrate 10 may be composed of either a stretched film or an unstretched film. When the substrate 11 is uniaxially stretched, the tear resistance and heat resistance of the laminate 100 can be improved. When the substrate 11 is a biaxially stretched film, the mechanical strength and dimensional stability of the laminate 100 can be improved.

[0030] When an adhesive layer is provided on the surface of the substrate 11, various pretreatments such as corona treatment, plasma treatment, ozone treatment, and flame treatment may be performed on the surface on the adhesive layer side in order to enhance adhesion to the adhesive layer, or a coating layer such as an easy-adhesion layer may be provided.

[0031] The thickness of the substrate 11 is not particularly limited and is, for example, 10 μm or more and 100 μm or less. From the viewpoint of reducing materials to reduce environmental impact and from the viewpoint of obtaining excellent heat resistance, impact resistance, and gas barrier properties, the thickness of the substrate 11 may be 15 μm or more, 20 μm or more, 25 μm or more, 30 μm or more, or 40 μm or more. The thickness of the substrate 11 may also be 60 μm or less, or 50 μm or less.

[0032] (Vapor deposition layer) The vapor deposition layer 61 may be formed on the sealing layer 30 side of the substrate 11 as shown in Fig. 2, or may be formed on the side of the substrate 11 opposite the sealing layer 30. The vapor deposition layer 61 may also be formed on both sides of the substrate 11. The vapor deposition layer 61 is a layer that improves the gas barrier properties of the laminate 100 and functions as a gas barrier layer. The vapor deposition layer 61 has barrier properties against gases such as water vapor or oxygen.

[0033] The vapor-deposited layer 61 may be, for example, a vapor-deposited layer of a metal or a vapor-deposited layer of an inorganic compound. Examples of metals include aluminum and silicon. Examples of inorganic oxides include aluminum oxide and silicon oxide (silica). When the vapor-deposited layer 61 is a vapor-deposited layer of a metal such as aluminum, the vapor-deposited layer 61 can function as a light-shielding layer.

[0034] (Overcoat Layer) The laminate 100 may have an overcoat layer 62 on the vapor deposition layer 61. In this case, the gas barrier properties of the laminate 100 are further improved. Therefore, when a packaging container is produced using the laminate 100 and contents are placed in the packaging container, deterioration of the contents due to gases such as oxygen can be effectively suppressed. As the overcoat layer 62, a coating layer obtained using a composition containing a water-soluble polymer and a silicon alkoxide, or a coating layer made of a resin such as polyurethane can be used.

[0035] <Sealing layer> The sealing layer 30 is used to bond the sealing layers 30 together by applying heat and pressure when manufacturing a packaging container such as a packaging bag using the laminate 100, and a sealant film (also referred to as a "sealant layer") or a heat seal varnish layer can be used.

[0036] The sealing layer 30 preferably has a melting point lower than that of the substrate 11 disposed on the outside. In this case, when the laminate 100 is heat-sealed, it is possible to heat-seal the sealant film while suppressing melting of the substrate 11. Furthermore, by heating the laminate 100, the substrate 11 and the sealing layer 30 can be easily separated, and material recycling of each of the substrate 11 and the sealing layer 30 can be easily performed.

[0037] The sealing layer 30 may further contain additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, an antistatic agent, a light-shielding pigment, etc. When the sealing layer 30 contains a light-shielding pigment, the sealing layer 30 can function as a light-shielding layer.

[0038] The sealing layer 30 may be composed of a single layer or multiple layers. When the sealing layer 30 is composed of a single layer, it may be a recycled polyolefin resin film containing recycled resin, or a non-recycled polyolefin resin film. Chemically recycled polyolefin resin is preferred as a recycled polyolefin resin film due to its superior hygiene and quality. When the sealing layer 30 has three layers, the multiple layers may be composed of a first outer layer, an intermediate layer, and a second outer layer. Here, the first outer layer and the second outer layer may be composed of a non-recycled polyolefin resin film, and the intermediate layer may be composed of a recycled polyolefin resin film. The sealing layer 30 may also be colored white or other colors. For example, a white sealant containing a titanium oxide-based white pigment can be used. The sealing layer 30 is not limited to a white sealant, and may be composed of a sealing layer of a different color by containing a pigment other than the white pigment.

[0039] (Sealant Film) The sealant film may be a polyolefin resin film, a polyester resin film, or the like. The polyolefin resin film is preferably used in terms of sealing suitability, etc., and contains a resin made of a polyolefin resin. The polyolefin resin may be the same as the resin used in the substrate 11. The polyester resin film may be a copolymer polyester obtained by copolymerizing two or more copolymers, and such a polyester resin film is preferred in terms of low adsorption of components in the contents and flavor barrier properties.

[0040] The thickness of the sealant film is not particularly limited and may be adjusted appropriately depending on the application of the laminate 100. The thickness of the sealant film may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the sealant film may also be 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0041] (Heat Seal Varnish Layer) The heat seal varnish layer can be used primarily for light packaging applications containing lightweight snacks. The heat seal varnish layer is obtained by applying and drying an acrylic, elastomer, or olefin-based heat seal varnish. Examples of heat seal varnishes that can be used include heat seal varnishes in which heat seal varnish components are dispersed in an aqueous solvent (e.g., water). Examples of heat seal varnishes that can be used include acrylic resin emulsions in which acrylic resins are dispersed as heat seal varnish components in an aqueous solvent, styrene-acrylic emulsions in which styrene-acrylic copolymer resins are dispersed as heat seal varnish components in an aqueous solvent, ionomer-based emulsions in which ionomers are dispersed as heat seal varnish components in an aqueous solvent, and polyolefin-based emulsions in which polyolefin resins are dispersed as heat seal varnish components in an aqueous solvent. In particular, it is preferable to use an aqueous heat seal varnish prepared by dispersing an aqueous polyolefin resin containing at least one selected from the group consisting of a carboxyl group, a carboxyl group salt, a carboxylic anhydride group, and a carboxylic acid ester in an aqueous solvent as a heat seal varnish component among polyolefin emulsions. Specific examples of heat seal varnishes that can be used include A450NS (acrylic) manufactured by DIC Corporation and Chemipearl S (polyolefin) manufactured by Mitsui Chemicals, Inc. The thickness of the heat seal varnish layer may be, for example, 0.05 μm or more, 0.5 μm or more, or 1 μm or more, and may be 20 μm or less, 10 μm or less, or 5 μm or less. The thickness of the heat seal varnish layer is preferably 1 to 5 μm. In this case, sufficient heat seal strength can be obtained while also providing resistance to bending.

[0042] <Outer sealant layer> The outer sealant layer 40 may be the same as the sealing layer 30. The thickness of the outer sealant layer 40 may be the same as or different from the thickness of the sealing layer 30. The material constituting the outer sealant layer 40 may also be the same as or different from the material constituting the sealing layer 30.

[0043] <Second Substrate> The second substrate 20 is a substrate that reinforces the deposition substrate 10 and can further improve the strength of the laminate 100. The second substrate 20 may be provided on the inside of the deposition substrate 10 (the side of the sealing layer 30) as shown in FIG. 2, or on the outside of the deposition substrate 10 (the side of the deposition substrate 10 opposite the sealing layer 30) as shown in FIG. 4. The second substrate 20 may be provided on both the inside and outside of the deposition substrate 10. The second substrate 20 can be a film substrate made of a resin material. Examples of such resin materials include polyester films such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene, polypropylene, and cyclic olefin copolymers COC and COP, polystyrene, polyamides such as nylon 66, polycarbonate, polyacrylonitrile, and engineering plastics such as polyimide. The resin material is preferably a resin material that has mechanical strength and dimensional stability. The resin material is processed into a film and used as the film substrate. The film substrate may be an unstretched film or a stretched film.

[0044] The second substrate 20 may be a single layer or a laminate of multiple layers. When the second substrate 20 is composed of a single layer, the second substrate 20 may be a recycled resin film or a non-recycled resin film such as a petroleum-derived resin or a biomass-derived resin. When the second substrate 20 is composed of multiple layers, all layers may be recycled resin films, non-recycled resin films, or some layers may be non-recycled resin films and the remaining layers may be recycled resin films. When the multiple layers are three layers, the multiple layers may be composed of a first outer layer, an intermediate layer, and a second outer layer. Here, the first outer layer and the second outer layer may be non-recycled resin films, and the intermediate layer may be recycled resin film. In this case, the possibility of impurities, gels, aggregates, and other foreign matter migrating from the second substrate 20 through the sealing layer 30 to the contents due to heating during retort or boiling treatment of the packaging bag can be further reduced. Therefore, the laminate 100 can be safely used to package contents such as food.

[0045] The thickness of the second substrate 20 is not particularly limited and is adjusted appropriately depending on the application of the laminate 100. The thickness of the second substrate 20 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the second substrate 20 may also be 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0046] <Adhesive Layer> Examples of the adhesive layer include an adhesive layer formed using an adhesive agent and an adhesive layer containing an adhesive resin (hereinafter also referred to as an "adhesive resin layer").

[0047] Examples of adhesives include known adhesives such as urethane adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, and isocyanate adhesives.

[0048] The adhesive may or may not contain a biomass-derived component, but preferably contains a biomass-derived component from the viewpoint of reducing the environmental impact. Specific examples of biomass-derived components include the "DIC Dry BM Series" manufactured by DIC Corporation and the "ECOAD Series" manufactured by Toyo Ink Co., Ltd.

[0049] The adhesive may be an adhesive containing an organic solvent or an adhesive containing no organic solvent, but from the viewpoint of reducing the environmental load, an adhesive containing no organic solvent (solvent-free adhesive) is preferred.

[0050] The adhesive resin layer may be an extruded or non-extruded resin layer. The adhesive resin is a heat-sealable adhesive thermoplastic resin that can be melted and fused to each other by heat, and examples thereof include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, methylpentene polymer, and acid-modified polyolefin resins obtained by modifying polyolefin resins such as polyethylene or polypropylene with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, and the like.

[0051] The thickness of the adhesive layer is not particularly limited and may be, for example, 1 μm or more. By making the thickness of the adhesive layer 1 μm or more, sufficient adhesive strength can be obtained. The thickness of the adhesive layer may be 2 μm or more. The thickness of the adhesive layer may be 50 μm or less, 5 μm or less, or 3 μm or less.

[0052] <Printed Layer> The printed layer 50 can be provided on one or both surfaces of the deposition substrate 10, the second substrate 20, or the outer sealant layer 40. When the printed layer 50 is provided between layers of the laminate 100, the deposition substrate 10, the second substrate 20, or the outer sealant layer 40 protects the printed layer 50, thereby preventing deterioration of the printed layer 50. When the printed layer 50 is the outermost layer of the laminate 100 on the side opposite the seal layer 30, the printed layer 50 can be easily removed when recycling a package containing the laminate 100 after disposal. The printed layer 50 is a layer that displays characters, pictures, etc., and can be formed using ink. Examples of ink that can be used include inks obtained by adding various pigments, plasticizers, desiccants, stabilizers, etc. to a binder resin such as a urethane-based, acrylic-based, nitrocellulose-based, or rubber-based resin.

[0053] The ink may be either an aqueous ink or an oil-based ink, but is preferably an aqueous ink. Because an aqueous ink uses water or alcohol as a solvent, it can further reduce the environmental impact. In particular, when the adhesive is a solventless adhesive, using an aqueous ink as the ink can significantly reduce the environmental impact. The ink may be a biomass ink or not, but from the perspective of reducing the environmental impact, a biomass ink is preferred. Here, biomass ink refers to an ink containing components obtained from biological resources (biomass), such as cotton, pulp, rice bran, vegetable oil, and angiosperm seeds. The ink may be a recycled ink obtained by recovering and recycling used ink, or a non-recycled ink, but from the perspective of reducing the environmental impact, a recycled ink is preferred. Furthermore, easily recyclable inks can also be used. The use of easily recyclable inks allows for easy recycling after discarding packaging. Specific examples include "SunSpectro Solvawash" manufactured by DIC Corporation.

[0054] <Gas Barrier Layer> The laminate 100 may further include a gas barrier layer on the substrate 11 of the deposition substrate 10 or on the second substrate 20. The gas barrier layer is a layer that improves the gas barrier properties of the laminate 100. The gas barrier layer includes at least one of the deposition layer 61 and the overcoat layer 62 described above.

[0055] <Other Layers> The laminate 100 may further include a layer containing a non-polyolefin resin. Examples of the non-polyolefin resin include polyamide resins such as nylon, and polyester resins such as polyethylene terephthalate (PET).

[0056] <Laminate> (A) Recycled Resin Content In the laminate 100, the recycled resin content in the laminate 100 is preferably 10% by volume or more or 10% by mass or more. When the recycled resin content in a polyolefin resin film containing recycled resin is 100% by volume (100% by mass), the recycled resin content in the laminate 100 can be determined as the ratio of the total thickness of the film to the total thickness of the laminate 100. However, when the recycled resin content in a polyolefin resin film containing recycled resin is X% by mass (less than 100% by mass) and the thickness of the film is Y1 (μm), the recycled resin content is calculated as X / 100×Y1 (μm) for the film thickness Y2 (μm). The content of recycled resin in the laminate 100 is preferably 20% by volume or more or 20% by mass or more, more preferably 25% by volume or more or 25% by mass or more, even more preferably 30% by volume or more or 30% by mass or more, and particularly preferably 40% by volume or more or 40% by mass or more.

[0057] In the present disclosure, the recycled resin is a chemically recycled resin and does not include materially recycled resin. The chemically recycled resin may be a post-consumer recycled resin (PCR), a post-industrial recycled resin (PIR), or a mixture thereof, but is preferably PCR. Since PCR is available in large quantities on the market, if the chemically recycled resin is PCR, the cost of the laminate 100 can be reduced.

[0058] (B) Odor Components In a total ion chromatogram obtained by performing mass analysis of the laminate 100 using purge-and-trap gas chromatography-mass spectrometry, the ratio of the peak area of ​​nonanal as an indicator of odor components to the sum of the peak areas of all aliphatic hydrocarbon components is R1 (%), and the ratio of the peak area of ​​decanal to the sum of the peak areas of all aliphatic hydrocarbon components is R2 (%). R1 ​​is preferably less than 1.5%, more preferably 1.0% or less, and particularly preferably 0.5% or less. Furthermore, R2 is preferably less than 3.5%, more preferably 2.5% or less, and particularly preferably 1.5% or less. It is preferable that R1 is less than 1.5% and R2 is less than 3.5%. In this case, thermal degradation is suppressed overall in the laminate 100, and the quality of the laminate 100 can be further improved. Specifically, the mass analysis is carried out by cutting out a 1.0 gram sample from the laminate 100, placing this sample in a 20 mL vial together with a collector of odor components, heating it at 60°C for 1 hour to adsorb the volatile components from the sample onto the collector, and then analyzing the volatile components in the collector using a purge-and-trap gas chromatograph mass analyzer.

[0059] (C) Fisheyes Fisheyes refer to foreign matter such as gelled or charred particles that can be found on film. If a fisheye has a diameter of 1 mm or more, the product will be deemed defective. If the number of fisheyes is 0.5 mm or more but less than 1 mm, the product will be deemed defective. 2 Less than or equal to 50 particles / m 2 Particularly preferably 10 pieces / m or less 2 It would be better if it was below.

[0060] (D) Variation in Dynamic Friction Force On the surface of the deposition substrate 10 of the laminate 100, the variation in dynamic friction force (in-plane variation) σ refers to the standard deviation of the dynamic friction force. σ is preferably less than 0.45, more preferably less than 0.35, and particularly preferably less than 0.2. When σ is less than 0.45, the transportability of the laminate 100 can be improved when the layer with σ less than 0.45 is on the transport roller side. Furthermore, on the surface of the layer, regions where the dynamic friction force received from the transport roller is large and regions where it is small appear, and the difference in stress between these regions is reduced. This reduces residual strain within the layer, and can also suppress a decrease in the strength of the laminate 100 due to the residual strain. Furthermore, from the viewpoint of the strength of the laminate, σ is preferably 0.1 or more, more preferably 0.2 or more, and particularly preferably 0.3 or more. The dynamic friction coefficient is measured for the laminate 100 using a multi-function static and dynamic friction tester TL201Tt (manufactured by Trinity Lab Co., Ltd.) and a tactile probe. The standard deviation σ of the dynamic friction force is a value obtained based on JIS K 7125-ISO8295, and specifically, is determined by placing the laminate 100 on a test table with the deposition substrate 10 facing downwards and moving the tactile probe at a sliding speed of 10 mm / sec while contacting the laminate 100 with a load of 50 grams.

[0061] (F) Impurities The laminate 100 is analyzed using a Fourier transform infrared spectrophotometer (FT-IR: Fourier transform infrared spectroscopy) using attenuated total reflection (ATR) to obtain an ATR spectrum. In the ATR spectrum, -1 The absorption coefficient of the methylene group C-H inverse symmetric stretching near 1720 cm -1The ratio R3 of the absorption coefficients of C=O stretching near the polyolefin is preferably less than 0.1, more preferably less than 0.05, and particularly preferably 0.01 or less, as an indicator of the small amount of resin components other than polyolefin. In the above analysis, a diamond prism is used as the prism to be closely attached to the laminate 100, and the angle of incidence with respect to the surface of the laminate 100 is 45°.

[0062] When the laminate 100 includes a deposition substrate 10 and a sealing layer 30, both the deposition substrate 10 and the sealing layer 30 may be recycled resin films.

[0063] <<Packaging Article>> Next, an embodiment of a packaging article according to another aspect of the present disclosure will be described with reference to Fig. 5. Fig. 5 is a cross-sectional view showing one embodiment of a packaging article according to another aspect of the present disclosure.

[0064] As shown in Fig. 5, a packaged item 500 includes a packaging bag 400 as a packaging container and contents C contained in the packaging bag 400. The packaging bag 400 is obtained using a pair of laminates 100. The packaging bag 400 is obtained, for example, by bringing the seal layers 30 of the pair of laminates 100 face to face and bonding their peripheral edges together. The packaging bag 400 is composed of a storage section that stores the contents C and an adhesive section that is provided around the storage section. The adhesive section is a section formed by bonding the seal layers 30 of opposing laminates 100 together, and the storage section is a section where the seal layers 30 of opposing laminates 100 are not bonded together.

[0065] According to the packaging product 500, the chemically recycled resin contained in the substrate 11 of the laminate 100 is a recycled resin produced by first depolymerizing discarded resin through a process that involves gasifying, liquefying, and monomerizing it via refined naphtha, or by depolymerizing it to monomerize it, depending on the material's characteristics. Therefore, chemically recycled resin is less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than material recycled resin, which is a resin made by cleaning, crushing, and then melting resin products such as recovered used packaging materials to recycle them into raw materials. Furthermore, unlike material recycled resin, chemically recycled resin is not affected by heat treatments such as melting after the recycling process, making it less susceptible to thermal degradation and less likely to have foreign matter such as gels and aggregates on its surface. Therefore, even when a vapor deposition layer 61 is formed on such a substrate 11, the thickness of the vapor deposition layer 61 is less likely to be uneven, resulting in a high-quality vapor deposition layer 61. Therefore, the packaging bag 400 obtained using the packaging laminate 100 can suppress a decrease in gas barrier property even when using a vapor deposition substrate 10 formed by forming a vapor deposition layer 61 on a substrate 11 containing recycled resin. Therefore, a packaging article 500 having a packaging container 400 can suppress a decrease in gas barrier property. Furthermore, because the packaging article 500 can suppress a decrease in gas barrier property, the packaging article 500 can suppress deterioration of the quality of the contents C, such as food, due to gas, and can safely store the contents C. Furthermore, because the laminate 100 can improve quality, the packaging article 500 including the packaging bag 400 obtained using the packaging laminate 100 can improve properties such as strength.

[0066] (Contents) The contents C are not particularly limited and may be appropriately selected depending on the intended use of the packaging bag 400. The contents C are not particularly limited, and examples of the contents C include food, shampoo, conditioner, body soap, and detergent.

[0067] (Packaging Bag) The pair of laminates 100 constituting the packaging bag 400 may have the same configuration as each other, or may have different configurations from each other.

[0068] The packaging bag 400 may have a half-cut line, and may further have an easy-open processed part at both ends or one end of the half-cut line. Examples of the easy-open processed part include a group of scars, and a V-shaped, U-shaped, or I-shaped notch.

[0069] In the adhesive portion of the packaging bag 400, the seal layers 30 of the pair of laminates 100 may be directly bonded to each other by heat sealing (see FIG. 5), or may be bonded to each other by an adhesive.

[0070] (Method for Manufacturing Packaged Article) Next, an example of a method for manufacturing the packaged article 500 using the laminate 100 will be described.

[0071] First, a pair of laminates 100 is prepared. Then, the sealing layers 30 of the pair of laminates 100 are placed opposite each other and bonded together. At this time, parts of the peripheral edges of the laminates are bonded together in a U-shape to form bonded sections, and also to form unbonded sections (unbonded sections). In this way, a packaging bag having an opening formed by the unbonded sections is obtained.

[0072] Next, the contents C are filled into the packaging bag through the opening. Thereafter, the seal layers 30 of the laminate 100 are bonded together at the unbonded portions, thereby forming the unbonded portions into bonded portions. In this manner, a packaged article 500 including the packaging bag 400 and the contents C contained therein can be manufactured.

[0073] While the preferred embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments. For example, in the packaged article 500 shown in Fig. 5, the packaging bag 400 is formed using a pair of laminates 100. However, the packaging bag may be manufactured by folding one laminate 100 with the sealing layer 30 facing inward and bonding the overlapping peripheral edges together.

[0074] 5, the packaging bag 400 may be a standing pouch-shaped packaging bag, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag, or a gusset bag. The packaging bag 400 may be provided with a stopper or a synthetic resin zipper that can be repeatedly sealed by fitting a strip-shaped protrusion and a strip-shaped groove.

[0075] Furthermore, although the packaging container is configured as a packaging bag in the above embodiment, the packaging container may also be a tube container. When the packaging container is a tube container, the laminate 100 has an outer sealant layer 40 that is adhered to the vapor deposition substrate 10. When the packaging bag is used for packaging sweets or the like (light packaging), a bag made using a heat seal varnish layer as the seal layer of the laminate 100 can be used as the packaging bag. Specifically, a vapor deposition layer made of a metal or inorganic oxide is provided on a substrate, and a heat seal varnish layer is provided directly on the vapor deposition layer, and the bag made using this laminate can be used as the packaging bag.

[0076] The embodiments of the present disclosure have been described above, but the outline of the present disclosure is as follows. [1] A vapor deposition substrate comprising a vapor deposition layer formed on a substrate, wherein the substrate is a polyolefin resin film containing a recycled resin, and the recycled resin is a chemically recycled resin. [2] A packaging laminate comprising the vapor deposition substrate according to [1] and a seal layer. [3] The packaging laminate according to [2], wherein the content of the recycled resin in the packaging laminate is 10% by volume or more or 10% by mass or more. [4] The packaging laminate according to [2] or [3], further comprising a second substrate on one or both sides of the substrate. [5] The packaging laminate according to any one of [2] to [4], wherein the recycled resin is a post-consumer recycled resin. [6] The packaging laminate according to [2] to [5], wherein the seal layer is a sealant film or a heat seal varnish layer. [7] The laminate according to [4], wherein the vapor deposition substrate and the second substrate are bonded together with a solventless adhesive. [8] The laminate for packaging material according to any one of [1] to [7], further comprising an overcoat layer on the vapor deposition layer. [9] A packaging container obtained by using the laminate for packaging material according to any one of [1] to [8].

[10] A packaging article comprising the packaging container according to [9] and contents to be contained in the packaging container.

[0077] The present disclosure will be explained in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0078] Example 1 A chemically recycled low-density polyethylene (PCR ChemiR 100%-LDPE) film (thickness: 35 μm) was prepared as the substrate, and a petroleum-derived LDPE film (thickness: 60 μm) was prepared as the sealing layer. Note that "PCR ChemiR 100%-LDPE" means that the content of post-consumer chemical recycled resin (PCR ChemiR) in the substrate is 100% by volume (100% by mass). Then, a SiOx vapor deposition layer (thickness: 10 nm) was formed on the substrate to obtain a vapor deposition substrate, and then an overcoat layer (thickness: 0.3 μm) was formed on the vapor deposition layer. The overcoat layer was formed using tetraethoxysilane [Si(OC 2 H 5 ) 4 89.6 g of hydrochloric acid (0.1 N) was added to 10.4 g of TEOS (hereinafter referred to as "TEOS") and stirred for 30 minutes to obtain a hydrolyzed solid content of 3 wt% (SiO 2 The coating was formed by mixing liquids A and B in a 60 / 40 weight ratio using a hydrolysis solution (liquid A) of 1.0 wt % polyvinyl alcohol (based on the weight ratio of 1.0 wt %) and a 3.0 wt % water / isopropyl alcohol solution (water:isopropyl alcohol weight ratio of 90:10) (liquid B). The coating was then applied with a bar coater and dried in a dryer at 120°C for 1 minute. Next, a printing layer was formed on the overcoat layer of the vapor-deposited substrate using aqueous flexographic ink. A dry lamination adhesive (urethane adhesive) was then applied to the surface of the printing layer to form an adhesive layer with a thickness of 3 μm (dry film thickness). A seal layer was then bonded to the adhesive layer to produce a packaging laminate (vapor-deposited substrate (substrate / vapor-deposited layer) / overcoat layer / printing layer / adhesive layer / seal layer).

[0079] Example 2 A laminate for a packaging material (deposited substrate (substrate / deposited layer) / overcoat layer / printed layer / adhesive layer / sealing layer) was produced in the same manner as in Example 1, except that the substrate was changed from a PCR Chemi R 100%-LDPE film (thickness 35 μm) to a PCR Chemi R 100%-LDPE film (thickness 25 μm), the seal layer was changed from a petroleum-derived LDPE film (thickness 60 μm) to a biomass-derived LDPE film (thickness 60 μm), the dry lamination adhesive (urethane-based adhesive) was changed to a 1.5 μm-thick solventless adhesive (polyester-based), and the SiOx vapor-deposited layer (thickness 10 nm) was changed to an aluminum oxide vapor-deposited layer (thickness 10 nm).

[0080] Example 3: A chemically recycled low-density polyethylene (PCR ChemiR 100%-LDPE) film (35 μm thick) was prepared as the substrate. "PCR ChemiR 100%-LDPE" refers to a substrate containing 100% by volume (100% by mass) of post-consumer chemically recycled resin (PCR ChemiR). A SiOx vapor-deposited layer (10 nm thick) was then formed on the substrate to form a vapor-deposited substrate. An overcoat layer (0.3 μm thick) was then formed on the vapor-deposited layer in the same manner as in Example 1. A printed layer was then formed on the overcoat layer using aqueous flexographic ink. A polyolefin-based heat seal varnish was then applied to the surface of the printed layer and dried to form a seal layer (1 μm thick), producing a packaging laminate (substrate / printed layer / seal layer). An aqueous polyolefin dispersion (Chemipearl S, manufactured by Mitsui Chemicals, Inc.) was used as the polyolefin-based heat seal varnish.

[0081] Example 4: A chemically recycled high-density polyethylene (PCR ChemiR 100%-HDPE) film (25 μm thick) was prepared as the substrate. A petroleum-derived LDPE film (50 μm thick) was prepared as the seal layer. A petroleum-derived stretched high-density polyethylene (HDPE) film (15 μm thick) was prepared as the second substrate. Note that "PCR ChemiR 100%-HDPE" means that the content of post-consumer chemical recycled resin (PCR ChemiR) in the substrate is 100% by volume (100% by mass). A SiOx vapor-deposited layer (10 nm thick) was then formed on the substrate to form a vapor-deposited substrate. An overcoat layer (0.3 μm thick) was then formed on the vapor-deposited layer in the same manner as in Example 1. A printing layer was then formed on the overcoat layer using aqueous flexographic ink. A dry lamination adhesive (urethane-based adhesive) was then applied to the surface of the printing layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness). The seal layer was then bonded to the first adhesive layer. Finally, a dry lamination adhesive (urethane adhesive) was applied to the surface of the substrate of the vapor deposition substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the second substrate was bonded to the second adhesive layer to produce a laminate for packaging (second substrate / first adhesive layer / vapor deposition substrate (substrate / vapor deposition layer) / overcoat layer / printing layer / second adhesive layer / sealing layer).

[0082] Example 5: A chemically recycled low-density polyethylene (PCR ChemiR 100%-LDPE) film (50 μm thick) was prepared as the substrate. A petroleum-derived LDPE film (80 μm thick) was prepared as the sealing layer. Another petroleum-derived LDPE film (80 μm thick) was prepared as the outer sealant layer. Note that "PCR ChemiR 100%-LDPE" means that the content of post-consumer chemical recycled resin (PCR ChemiR) in the substrate is 100% by volume (100% by mass). A SiOx vapor-deposited layer (10 nm thick) was then formed on the substrate to form a vapor-deposited substrate. An overcoat layer (0.3 μm thick) was then formed on the vapor-deposited layer in the same manner as in Example 1. A printing layer was then formed on the overcoat layer using aqueous flexographic ink. A dry lamination adhesive (urethane-based adhesive) was then applied to the surface of the printing layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness). The sealing layer was then bonded to the first adhesive layer. Finally, a dry lamination adhesive (urethane adhesive) was applied to the surface of the substrate of the vapor deposition substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and an outer sealant layer was attached to the second adhesive layer to produce a laminate for packaging (outer sealant layer / first adhesive layer / vapor deposition substrate (substrate / vapor deposition layer) / overcoat layer / printing layer / second adhesive layer / sealing layer).

[0083] Example 6: A PCR ChemiR 100%-OPP film (50 μm thick) was prepared as the substrate, a petroleum-derived LDPE film (80 μm thick) was prepared as the seal layer, and a petroleum-derived LDPE film (80 μm thick) was prepared as the outer sealant layer. Note that "PCR ChemiR 100%-OPP" indicates that the content of post-consumer chemical recycled resin (PCR ChemiR) in the substrate is 100% by volume (100% by mass). A SiOx vapor-deposited layer (10 nm thick) was then formed on the substrate to form a vapor-deposited substrate. An overcoat layer (0.3 μm thick) was then formed on the vapor-deposited layer in the same manner as in Example 1. A printing layer was then formed on the overcoat layer using aqueous flexographic ink. A dry lamination adhesive (urethane-based adhesive) was then applied to the surface of the printing layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness). The sealing layer was then bonded to the first adhesive layer. Finally, a dry lamination adhesive (urethane adhesive) was applied to the surface of the substrate of the vapor deposition substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and an outer sealant layer was attached to the second adhesive layer to produce a laminate for packaging (outer sealant layer / first adhesive layer / vapor deposition substrate (substrate / vapor deposition layer) / overcoat layer / printing layer / second adhesive layer / sealing layer).

[0084] Example 7: A PCR ChemiR 100%-OPP film (25 μm thick) was prepared as the substrate. A petroleum-derived unstretched polypropylene (CPP) film (50 μm thick) was prepared as the seal layer. A PCR ChemiR 100%-OPP film (25 μm thick) was prepared as the second substrate. Note that "PCR ChemiR 100%-OPP" means that the content of post-consumer chemical recycled resin (PCR ChemiR) in the substrate is 100% by volume (100% by mass). A SiOx vapor deposition layer (10 nm thick) was then formed on the substrate to form a vapor deposition substrate. An overcoat layer (0.3 μm thick) was then formed on the vapor deposition layer in the same manner as in Example 1. A printing layer was then formed on the overcoat layer using aqueous flexographic ink. A dry lamination adhesive (urethane adhesive) was then applied to the surface of the printing layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness). The seal layer was then bonded to the first adhesive layer. Finally, a dry lamination adhesive (urethane adhesive) was applied to the surface of the substrate of the vapor deposition substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the second substrate was bonded to the second adhesive layer to produce a laminate for packaging (second substrate / first adhesive layer / vapor deposition substrate (substrate / vapor deposition layer) / overcoat layer / printing layer / second adhesive layer / sealing layer).

[0085] Example 8: A PCR ChemiR 100%-OPP film (25 μm thick) was prepared as the substrate, a petroleum-derived LDPE film (60 μm thick) was prepared as the seal layer, and a PCR ChemiR 100%-OPP film (25 μm thick) was prepared as the second substrate. Note that "PCR ChemiR 100%-OPP" means that the content of post-consumer chemical recycled resin (PCR ChemiR) in the substrate is 100% by volume (100% by mass). A SiOx vapor deposition layer (10 nm thick) was then formed on the substrate to form a vapor deposition substrate. An overcoat layer (0.3 μm thick) was then formed on the vapor deposition layer in the same manner as in Example 1. A printing layer was then formed on the overcoat layer using aqueous flexographic ink. A dry lamination adhesive (urethane adhesive) was then applied to the surface of the printing layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness). The seal layer was then bonded to the first adhesive layer. Finally, a dry lamination adhesive (urethane adhesive) was applied to the surface of the substrate of the vapor deposition substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the second substrate was bonded to the second adhesive layer to produce a laminate for packaging (second substrate / first adhesive layer / vapor deposition substrate (substrate / vapor deposition layer) / overcoat layer / printing layer / second adhesive layer / sealing layer).

[0086] Comparative Example 1 A low-density polyethylene (PCRMR 100%-LDPE) film (thickness: 25 μm) made by material recycling using used polyethylene bags was prepared as the substrate, and a petroleum-derived LDPE film (thickness: 60 μm) was prepared as the sealing layer (sealant layer). Note that "PCR ChemiR 100%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the vapor-deposited substrate is 100% by volume (100% by mass). A vapor-deposited layer (thickness: 10 nm) made of aluminum oxide was formed on one surface of the substrate to obtain a vapor-deposited substrate, and then an overcoat layer (thickness: 0.3 μm) was formed on the vapor-deposited layer. The overcoat layer was formed using tetraethoxysilane [Si(OC 2 H 5 ) 4 89.6 g of hydrochloric acid (0.1 N) was added to 10.4 g of TEOS (hereinafter referred to as "TEOS") and stirred for 30 minutes to obtain a hydrolyzed solid content of 3 wt% (SiO 2The coating agent was prepared by mixing liquids A and B in a blending ratio (by weight) of 60 / 40 using a hydrolysis solution (liquid A) of 1.0 wt % polyvinyl alcohol (based on 100% conversion) and a 3.0 wt % water / isopropyl alcohol solution (water:isopropyl alcohol weight ratio of 90:10) (liquid B). The coating agent was applied using a bar coater and dried in a dryer at 120°C for 1 minute. Next, a printing layer was formed on the overcoat layer of the vapor-deposited substrate using aqueous flexo ink, a dry-laminating adhesive (urethane adhesive) was applied to the surface of the printing layer to form an adhesive layer with a thickness of 3 µm (dry film thickness), and a seal layer was attached to the adhesive layer to prepare a packaging laminate (vapor-deposited substrate (substrate / vapor-deposited layer) / overcoat layer / printed layer / adhesive layer / seal layer).

[0087] Comparative Example 2 The substrate was changed from a PCRMR 100%-LDPE film (thickness 25 μm) to a low-density polyethylene (PCRMR 40%-LDPE) film (thickness 60 μm) obtained by mixing low-density polyethylene (PCRMR-LDPE) pellets obtained by cleaning and mechanically recycling used polyethylene bags with petroleum-derived LDPE pellets in a ratio of 40:60 (mass ratio), the seal layer (sealant layer) was changed from a petroleum-derived LDPE film (thickness 60 μm) to a petroleum-derived LDPE film (thickness 50 μm), and the aluminum oxide vapor-deposited layer (thickness 10 nm) was changed to a SiOx vapor-deposited layer (thickness 10 nm). Except for this, a laminate for packaging (vapor-deposited substrate (substrate / vapor-deposited layer) / overcoat layer / printed layer / adhesive layer / sealing layer) was produced in the same manner as in Comparative Example 1. Incidentally, "PCRMR40%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the substrate is 40% by mass. In this case, the volume of a layer made of recycled materials can be calculated taking into account the density of the mixed resins, and this can be used to calculate the film thickness ratio. Note that the densities of the mixed resins are the same, and the mass % is also the volume %. The density of the PCRMR-LDPE40% film used as the substrate is low density (0.920 g / cm 3 )

[0088] (Comparative Example 3) A PCRMR 100%-LDPE film (thickness 25 μm) was prepared as the substrate, a PCRMR 100%-LDPE film (thickness 25 μm) was prepared as the second substrate, and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the seal layer (sealant layer). Then, a vapor-deposited layer (thickness 10 nm) made of aluminum oxide was formed on one surface of the substrate to obtain a vapor-deposited substrate, and then an overcoat layer (thickness 0.3 μm) was formed on the vapor-deposited layer. The overcoat layer was formed using tetraethoxysilane [Si(OC 2 H 5 ) 4 89.6 g of hydrochloric acid (0.1 N) was added to 10.4 g of TEOS (hereinafter referred to as "TEOS") and stirred for 30 minutes to obtain a hydrolyzed solid content of 3 wt% (SiO 2 The coating agent was formed by mixing liquids A and B in a 60 / 40 weight ratio (by weight) using a hydrolysis solution (liquid A) of 100 wt % polyvinyl alcohol (based on the weight ratio of 100 wt %) and a 3.0 wt % water / isopropyl alcohol solution (liquid B) of 90:10 water:isopropyl alcohol (based on the weight ratio of 100 wt %). The coating agent was applied using a bar coater and dried in a dryer at 120°C for 1 minute. On the other hand, a printed layer was formed on one surface of the second substrate using aqueous flexographic ink, and a laminating adhesive (urethane adhesive) was applied to the surface of the printed layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness). The overcoat layer on the vapor-deposited substrate was then bonded to the first adhesive layer. Next, a dry lamination adhesive (urethane-based adhesive) was applied to the substrate of the vapor deposition substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the second adhesive layer was bonded to the seal layer to produce a laminate for packaging (second substrate / printed layer / first adhesive layer / overcoat layer / vapor deposition substrate (vapor deposition layer / substrate) / second adhesive layer / seal layer).

[0089] (Comparative Example 4) A low-density polyethylene (PCRMR-LLDPE 100%) film (thickness 35 μm) that had been material-cycled using used packaging material (nylon / printed layer / PET layer / aluminum vapor-deposited layer / linear low-density polyethylene (LLDPE) sealant layer) was prepared as the substrate, and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the seal layer (sealant layer). Then, a vapor-deposited layer (thickness 10 nm) made of aluminum oxide was formed on one surface of the substrate to obtain a vapor-deposited substrate, and then an overcoat layer (thickness 0.3 μm) was formed on the vapor-deposited layer. The overcoat layer was formed using tetraethoxysilane [Si(OC 2 H 5 ) 4 89.6 g of hydrochloric acid (0.1 N) was added to 10.4 g of TEOS (hereinafter referred to as "TEOS") and stirred for 30 minutes to obtain a hydrolyzed solid content of 3 wt% (SiO 2 A coating agent was formed by mixing liquids A and B in a blending ratio (by weight) of 60 / 40 using a hydrolysis solution (liquid A) of 1.0 wt % polyvinyl alcohol (based on the weight ratio of 1000 ppm or less) and a 3.0 wt % solution of polyvinyl alcohol in water / isopropyl alcohol (water:isopropyl alcohol weight ratio of 90:10) (liquid B). The coating agent was applied using a bar coater and dried in a dryer at 120°C for 1 minute. A printed layer was then formed on the overcoat layer on the vapor-deposited substrate using an aqueous flexographic ink, a laminating adhesive (urethane adhesive) was applied to the printed surface to form an adhesive layer with a thickness of 3 µm (dry film thickness), and a seal layer was attached to the adhesive layer to produce a packaging laminate (vapor-deposited substrate (substrate / vapor-deposited layer) / overcoat layer / printed layer / adhesive layer / seal layer).

[0090] Comparative Example 5: A low-density polyethylene (PCRMR-HDPE-LLDPE 100%) film (25 μm thick) that had been material-recycled using used packaging material (high-density polyethylene (HDPE) layer / printed layer / HDPE layer / LLDPE sealant layer) was prepared as the substrate, and a petroleum-derived LDPE film (60 μm thick) was prepared as the seal layer (sealant layer). Note that "PCRMR-HDPE-LLDPE 100%" means that the total content of mechanically recycled high-density polyethylene (HDPE) and linear low-density polyethylene (LLDPE) in the vapor-deposited substrate was 100% by volume (100% by mass). A vapor-deposited layer (10 nm thick) of aluminum oxide was formed on one surface of the substrate to obtain a vapor-deposited substrate, and then an overcoat layer (0.3 μm thick) was formed on the vapor-deposited layer. The overcoat layer was formed using tetraethoxysilane [Si(OC 2 H 5 ) 4 89.6 g of hydrochloric acid (0.1 N) was added to 10.4 g of TEOS (hereinafter referred to as "TEOS") and stirred for 30 minutes to obtain a hydrolyzed solid content of 3 wt% (SiO 2 A coating agent was formed by mixing liquids A and B in a blending ratio (by weight) of 60 / 40 using a hydrolysis solution (liquid A) of 1.0 wt % polyvinyl alcohol (based on the weight ratio of 1000 ppm or less) and a 3.0 wt % solution of polyvinyl alcohol in water / isopropyl alcohol (water:isopropyl alcohol weight ratio of 90:10) (liquid B). The coating agent was applied using a bar coater and dried in a dryer at 120°C for 1 minute. A printed layer was then formed on the overcoat layer on the vapor-deposited substrate using an aqueous flexographic ink, a laminating adhesive (urethane adhesive) was applied to the printed surface to form an adhesive layer with a thickness of 3 µm (dry film thickness), and a seal layer was attached to the adhesive layer to produce a packaging laminate (vapor-deposited substrate (substrate / vapor-deposited layer) / overcoat layer / printed layer / adhesive layer / seal layer).

[0091] (Comparative Example 6) A laminate for a packaging material (deposited substrate (substrate / deposited layer) / overcoat layer / printed layer / adhesive layer / sealing layer) was produced in the same manner as in Comparative Example 1, except that the seal layer (sealant layer) was changed from a petroleum-derived LDPE film (thickness 50 μm) to a petroleum-derived LDPE film (thickness 60 μm).

[0092] Reference Example 1 A petroleum-derived LDPE film (thickness 25 μm) was prepared as the substrate, and a petroleum-derived LLDPE film (thickness 60 μm) was prepared as the sealing layer (sealant layer). A vapor-deposited layer (thickness 10 nm) made of aluminum oxide was formed on one surface of the substrate to obtain a vapor-deposited substrate, and then an overcoat layer (thickness 0.3 μm) was formed on the vapor-deposited layer. The overcoat layer was formed using tetraethoxysilane [Si(OC 2 H 5 ) 4 89.6 g of hydrochloric acid (0.1 N) was added to 10.4 g of TEOS (hereinafter referred to as "TEOS") and stirred for 30 minutes to obtain a hydrolyzed solid content of 3 wt% (SiO 2 The coating agent was prepared by mixing liquids A and B in a blending ratio (by weight) of 60 / 40 using a hydrolysis solution (liquid A) of 1.0 wt % polyvinyl alcohol (based on 1000 ppm conversion) and a 3.0 wt % water / isopropyl alcohol solution (liquid B) of 90:10 water:isopropyl alcohol by weight ratio. The coating agent was applied with a bar coater and dried in a dryer at 120°C for 1 minute. Subsequently, a printing layer was formed on the overcoat layer on the vapor-deposited substrate using an aqueous flexographic ink, a laminating adhesive (urethane adhesive) was applied to the surface of the printed surface to form an adhesive layer with a thickness of 3 µm (dry film thickness), and a seal layer was attached to the adhesive layer to prepare a packaging laminate (vapor-deposited substrate (substrate / vapor-deposited layer) / overcoat layer / printed layer / adhesive layer / seal layer).

[0093] <Recycled Resin Content> For the packaging laminates of the Examples, Comparative Examples, and Reference Examples prepared as described above, the recycled resin content in the packaging laminate was calculated according to the following formula: Recycled Resin Content = 100 × Total Thickness of Layers Containing Recycled Resin / Total Thickness of Packaging Laminate However, when the layer containing recycled resin is a layer containing recycled resin and a petroleum-derived resin, the value obtained by multiplying the thickness of this layer by the recycled resin content (mass%) in that layer was used as the thickness of the layer containing recycled resin. Note that the thicknesses of the printed layer, vapor-deposited layer, and overcoat layer were quite small, so they were not taken into consideration when calculating the recycled resin content in the laminate.

[0094] <Evaluation> The laminates for packaging materials of the Examples, Comparative Examples, and Reference Examples prepared as described above were evaluated as follows: Evaluation 1 (generation of odorous components), Evaluation 2 (fisheyes), Evaluation 3 (impurities), Evaluation 4 (variation in dynamic friction force), and Evaluation 5 (gas barrier properties). Here, Evaluation 1 is an evaluation regarding quality, and Evaluations 2 and 3 are evaluations regarding hygiene.

[0095] (1) Evaluation 1 (Odor Component Generation) First, the packaging laminate was analyzed using purge-and-trap gas chromatography mass spectrometry. Specifically, a 1.0 gram sample was cut from the packaging laminate, placed in a 20 mL vial with an odor component collector, and heated at 60°C for 1 hour to adsorb volatile components from the sample onto the collector. The volatile components in the collector were analyzed using a purge-and-trap gas chromatography mass spectrometer to obtain a total ion chromatogram. Next, in the total ion chromatogram obtained as above, the ratio R1 of the peak area of ​​nonanal to the sum of the peak areas of all aliphatic hydrocarbon components, and the ratio R2 of the peak area of ​​decanal to the sum of the peak areas of all aliphatic hydrocarbon components, both of which serve as indicators of odor components, were calculated. Evaluation was then performed based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation criteria) ⊚: R1 is less than 1.5% and R2 is less than 0.35% ◯: R1 is less than 1.5% and R2 is 0.35% or more, or R1 is 1.5% or more and R2 is less than 0.35% ×: R1 is 1.5% or more and R2 is 0.35% or more

[0096] (2) Evaluation 2 (Fisheyes) A ​​sample measuring 1 m x 1 m was cut out from the packaging laminate, and the sample was placed on a black table with the seal layer side facing down. Protrusions (protruding foreign matter) with a diameter of 0.5 mm or more but less than 1 mm were designated as fisheye 1 and the number N1 of these was counted visually, and protrusions (protruding foreign matter) with a diameter of 1 mm or more were designated as fisheye 2 and the number N2 of these was counted visually, and evaluation was performed based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation criteria) ⊚: N1 is 10 or less and N2 is 0 ○: N1 is 11 to 99 and N2 is 0 ×: N1 is 100 or more or N2 is 1 or more

[0097] (3) Evaluation 3 (impurities) The packaging laminate was analyzed using a Fourier transform infrared spectrophotometer (FT-IR: Fourier transform infrared spectroscopy) using attenuated total reflection (ATR) to obtain an ATR spectrum. At this time, a diamond prism was used as the prism to be brought into close contact with the packaging laminate, and the angle of incidence with respect to the surface of the packaging laminate was 45°. Then, in the ATR spectrum, a peak at 2915 cm originating from polyethylene was observed. -1 The absorption coefficient of the methylene group C-H inverse symmetric stretching near 1720 cm -1 The ratio R3 of the absorption coefficients of C=O stretching near the nucleus was calculated and evaluated based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation criteria) ⊚: R3 is less than 0.05 ◯: R3 is 0.05 or more but less than 0.1 ×: R3 is 0.1 or more

[0098] (4) Evaluation 4 (Variation in Dynamic Friction Force) The dynamic friction force of the packaging laminate was measured using a multi-function static and dynamic friction tester TL201Tt (manufactured by Trinity Lab Co., Ltd.) and a tactile probe. Specifically, the packaging laminate was placed on a test table with the sealant layer facing down, and the tactile probe was moved at a sliding speed of 10 mm / sec while being brought into contact with the packaging laminate (on the deposition substrate side) with a load of 50 grams, to determine the standard deviation of the dynamic friction force. This standard deviation σ of the dynamic friction force was taken as the variation in the dynamic friction force. Evaluation was then performed based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation Criteria) A...σ is less than 0.35 B...σ is 0.35 or more but less than 0.45 C...σ is 0.45 or more (5) Evaluation 5 (Gas Barrier Property) The gas barrier property of the packaging laminate was evaluated as follows. Specifically, the oxygen permeability (unit: cc / m 2 The oxygen permeability (per 1000 cc / (m·day·atm)) was measured according to JIS K7126, Method B (constant pressure method), and the oxygen permeability was used as an index of gas barrier properties. The measuring device used was an OXTRAN 2 / 20 manufactured by MOCON Corporation, and measurements were taken at a temperature of 30°C and a relative humidity of 70%. (Evaluation criteria) A: Oxygen permeability is 1 cc / (m 2 B: Oxygen permeability was less than 1 cc / (m 2 ・day・atm) or more, 10cc / (m 2 C: Oxygen permeability was less than 10 cc / (m 2 ・day・atm) or more.

[0099]

[0100] The results shown in Tables 1 to 3 show that all of the packaging laminates of Examples 1 to 8, even when using a vapor deposition substrate having a substrate containing recycled resin, generated almost no odorous components, contained little foreign matter such as gels and aggregates and impurities, and had good gas barrier properties, and had performance equivalent to that of the packaging laminate of Reference Example 1. In contrast, the packaging laminates of Comparative Examples 1 to 5, which used material recycled resin, when the recycled resin content was increased to 10% by volume or more, exhibited at least one of the following: an increased amount of odorous components, an increased number of fisheyes, and an increased amount of impurities; the gas barrier properties were not good, and the packaging laminate did not have performance equivalent to that of Reference Example 1.

[0101] From the above, it has been confirmed that the laminate for packaging materials of the present disclosure can suppress deterioration in gas barrier properties even when using a vapor deposition base material in which a vapor deposition layer is formed on a substrate containing recycled resin.

[0102] 10...deposition substrate, 11...substrate, 20...second substrate, 30...seal layer, 61...deposition layer, 62...overcoat layer, 100...laminated body, 400...packaging bag (packaging container), 500...packaged article, C...contents

Claims

1. A vapor-deposited substrate comprising a vapor-deposited layer formed on a substrate, the substrate being a polyolefin resin film containing a recycled resin, the recycled resin being a chemically recycled resin.

2. A laminate for packaging material comprising the deposition base material according to claim 1 and a seal layer.

3. The packaging laminate according to claim 2, wherein the content of the recycled resin in the packaging laminate is 10% by volume or more or 10% by mass or more.

4. The laminate for packaging material according to claim 2, further comprising a second substrate on one or both sides of the substrate.

5. The laminate for packaging materials according to claim 2, wherein the recycled resin is a post-consumer recycled resin.

6. The laminate for packaging materials according to claim 2, wherein the sealing layer comprises a sealant film or a heat seal varnish layer.

7. The laminate according to claim 4, wherein the deposition substrate and the second substrate are bonded together with a solventless adhesive.

8. The laminate for packaging materials according to claim 2, further comprising an overcoat layer on the vapor deposition layer.

9. A packaging container obtained by using the packaging laminate according to any one of claims 1 to 8.

10. A packaging article comprising the packaging container according to claim 9 and a content contained within the packaging container.

Citation Information

Patent Citations

  • Flexible pouches using post-consumer resins

    JP2022552096A

  • Material-recycled pe-containing film and package including the same

    JP2023040660A

  • Vapor-deposited resin film, laminate including said vapor-deposited resin film, and packaging container including said laminate

    JP2022031795A

  • Polyolefin resin-based cross-linked foam and adhesive tape

    JP2023001768A

  • Laminate film, packaging bag and package

    JP2023031593A