Laminate for packaging material, packaging container, and packaging article

The packaging laminate with a chemically recycled resin sealant layer addresses hygiene and quality concerns in conventional laminates by minimizing contamination and thermal deterioration, enabling safe storage of contents with high recycled resin content, thus improving both hygiene and quality.

WO2024228275A1PCT designated stage expired Publication Date: 2024-11-07TOPPAN HOLDINGS INC

Patent Information

Application Number
PCT/JP2023/042986
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2023-11-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Conventional packaging laminates using recycled resin often suffer from hygiene issues due to contaminants and thermal deterioration, especially when the recycled resin content is high, leading to potential contamination and quality concerns.

Method used

A packaging laminate with a polyolefin resin film sealant layer made from chemically recycled resin, which is less prone to contamination and thermal deterioration, allowing for a higher recycled resin content of 10% or more by volume or mass, improving hygiene and quality.

Benefits of technology

The use of chemically recycled resin in the packaging laminate enhances hygiene and quality by reducing the risk of contamination and thermal issues, enabling safe storage of contents like food even with high recycled resin content, while also reducing environmental load and costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2023042986_07112024_PF_FP_ABST
    Figure JP2023042986_07112024_PF_FP_ABST
Patent Text Reader

Abstract

This laminate for a packaging material comprises an outer layer substrate and a sealant layer. The sealant layer is a polyolefin resin film containing a recycled resin. The content of the recycled resin in the laminate for a packaging material is 10% by volume or more or 10% by mass or more. The recycled resin is a chemically recycled resin.
Need to check novelty before this filing date? Find Prior Art

Description

Packaging laminate, packaging container, and packaging article

[0001] The present disclosure relates to a laminate for packaging, a packaging container, and a packaging article.

[0002] Packaging materials used in packaging bags and the like are required to have various properties depending on their applications. Therefore, in order to simultaneously satisfy these various performance requirements, packaging materials are generally composed of a laminate including an outer layer substrate and a sealant layer. A known example of such a packaging laminate is a laminate including a first layer including an inner liner and a second layer including an outer sheath, where the outer sheath is composed of a post-consumer resin (hereinafter also referred to as "PCR") that may contain contaminants such as paper, ink, and food residues (see, for example, Patent Document 1 listed below).

[0003] Special Publication No. 2022-552096

[0004] However, the laminate described in Patent Document 1 has the following problems when the PCR content is increased when the PCR is a recycled resin containing contaminants, i.e., a so-called material recycled resin. That is, in the laminate described in Patent Document 1, foreign matter such as impurities, gels, and aggregates may appear on the surface, leaving room for improvement in terms of hygiene. Furthermore, in the laminate described in Patent Document 1, odorous components generated due to thermal degradation of the polyolefin resin are detected, leaving room for improvement in terms of quality as well.

[0005] An object of the present disclosure is to provide a laminate for packaging materials, a packaging container, and a packaging article that can improve hygiene and quality even when the recycled resin content is sufficiently high.

[0006] One aspect of the present disclosure provides a packaging laminate including an outer layer substrate and a sealant layer, wherein the sealant layer is a polyolefin resin film containing a recycled resin, the content of the recycled resin in the packaging laminate is 10% by volume or more or 10% by mass or more, and the recycled resin is a chemically recycled resin. According to the packaging laminate, the sealant layer is required to have particularly high hygiene and quality because it comes into contact with the contents contained in a packaging container obtained using the packaging laminate. In contrast, in the packaging laminate of the present disclosure, the recycled resin in the polyolefin resin film used as the sealant layer is a chemically recycled resin. The chemically recycled resin is a recycled resin produced by first reducing the molecular weight of discarded resin through a process performed depending on the material properties, such as a process of monomerization via gasification, oilification, and refined naphtha, or a process of monomerization by depolymerization, and then polymerizing it. For this reason, chemically recycled resins are less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than material recycled resins, which are resins made by cleaning and crushing collected resin products such as used packaging materials, and then heating and melting them to recycle them into raw materials. Furthermore, unlike material recycled resins, chemically recycled resins are not affected by heat treatments such as heating and melting after the recycling process, and are therefore less susceptible to thermal degradation. Therefore, by increasing the recycled resin content in the packaging laminate to 10% by volume or 10% by mass or more, it is possible to achieve both improved hygiene and quality. In other words, the packaging laminate of the present disclosure can achieve improved hygiene and quality even when the recycled resin content is sufficiently high.

[0007] The higher the content (usage ratio) of recycled resin in the packaging laminate, the more the environmental impact can be reduced, and the recycled resin content is preferably 20% by mass or more, more preferably 25% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more. Here, if it is not easy to calculate the mass ratio (mass%) after the packaging laminate is made into a packaging material, the unit of recycled resin content may be "volume %" so that it can be calculated from the film thickness ratio. In other words, the ratio of the film thickness of the layer using recycled resin to the film thickness of the entire laminate can be used as the recycled resin content (volume %). The density of polyethylene and polypropylene, which make up the majority of the packaging material, is 0.86 to 0.97 g / cm 3 The range of the recycled resin content specified in volume % generally satisfies the range specified in mass %. That is, the recycled resin content in the packaging laminate is preferably 20% by volume or more, more preferably 25% by volume or more, even more preferably 30% by volume or more, and particularly preferably 40% by volume or more.

[0008] In the packaging laminate, the thickness of the sealant layer may be greater than the thickness of the outer layer base material, and the content of the recycled resin in the sealant layer may be 20% by volume or more or 20% by mass or more. In the packaging laminate, the sealant layer accounts for a large proportion of the packaging laminate, and the content of recycled resin can be easily increased by using a polyolefin resin film containing recycled resin as the sealant layer.

[0009] The packaging laminate may further include an intermediate substrate between the outer layer substrate and the sealant layer. In this case, the outer layer substrate is reinforced by the intermediate substrate, thereby further improving the strength of the laminate.

[0010] In the laminate for packaging material, the recycled resin may be a post-consumer recycled resin (PCR). PCR can be secured in large quantities on the market, which can reduce the cost of the laminate. The recycled resin may be a combination of PCR and post-industrial recycled resin (PIR).

[0011] The packaging laminate may further include a gas barrier layer between the outer layer base material and the sealant layer. In this case, the gas barrier properties of the laminate are further improved. Therefore, when a packaging container is produced using the laminate and contents are placed in the packaging container, deterioration of the contents due to gases such as oxygen can be effectively suppressed.

[0012] The laminate for packaging may further include a second sealant layer on the surface of the outer layer base material opposite to the sealant layer. This laminate for packaging is suitable as a packaging material for producing tube containers.

[0013] Another aspect of the present disclosure provides a packaging container obtained using the packaging laminate. According to the packaging container, as described above, a polyolefin resin film containing recycled resin is used as a sealant layer in the packaging laminate, and the recycled resin is a chemically recycled resin. Chemically recycled resin is less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than materially recycled resin. Furthermore, unlike materially recycled resin, chemically recycled resin is not affected by heat treatments such as heat melting after the recycling process, and is therefore less susceptible to thermal degradation. Therefore, a packaging container obtained using the packaging laminate can safely contain contents such as food even if the recycled resin content in the packaging laminate is sufficiently high, at 10% by volume or 10% by mass or more. Furthermore, because the packaging laminate can improve quality, the packaging container obtained using the packaging laminate can improve properties such as strength.

[0014] Yet another aspect of the present disclosure provides a packaging article comprising the above-described packaging container and contents to be contained within the packaging container. According to the packaging article, as already described, the chemically recycled resin contained in the sealant layer of the laminate is less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than materially recycled resin. Furthermore, unlike materially recycled resin, chemically recycled resin is not affected by heat treatments such as heat melting after the recycling process, and is therefore less susceptible to thermal degradation. Therefore, the packaging article can be safely stored with contents such as food contained therein, even if the recycled resin content in the packaging laminate is sufficiently high, at 10% by volume or 10% by mass or more. Furthermore, because the packaging laminate can improve quality, packaging articles equipped with packaging containers obtained using the packaging laminate can have improved properties such as strength.

[0015] According to the present disclosure, there are provided a laminate for packaging materials, a packaging container, and a packaging article that can improve hygiene and quality even when the content of recycled resin is sufficiently high.

[0016] Fig. 1 is a cross-sectional view showing one embodiment of a packaging laminate according to the present disclosure. Fig. 2 is a cross-sectional view showing another embodiment of a packaging laminate according to the present disclosure. Fig. 3 is a cross-sectional view showing another embodiment of a packaging laminate according to the present disclosure. Fig. 4 is a cross-sectional view showing one embodiment of a packaging article according to the present disclosure.

[0017] Preferred embodiments of the present disclosure will be described in detail below. In the drawings, the same or corresponding parts are designated by the same reference numerals, and redundant explanations will be omitted.

[0018] <Packaging laminate> First, embodiments of the packaging laminate according to the present disclosure will be described with reference to Figures 1 to 3. Figures 1 to 3 are cross-sectional views showing various embodiments of the packaging laminate according to the present disclosure.

[0019] As shown in Figure 1, the packaging laminate (hereinafter also referred to as "laminate") 100 includes an outer layer base material 10 and a sealant layer 30. The laminate 100 may further include an intermediate base material 20 between the outer layer base material 10 and the sealant layer 30. The content of recycled resin in the packaging laminate 100 is 10% by volume or more or 10% by mass or more. Here, the sealant layer 30 is made of a polyolefin resin film containing recycled resin, and the recycled resin is a chemically recycled resin.

[0020] The laminate 100 may further include a printed layer 50, as shown in Fig. 2. The laminate 100 may further include a gas barrier layer 60 together with the printed layer 50, as shown in Fig. 2, or may further include the gas barrier layer 60 instead of the printed layer 50. When the laminate 100 is used for a tubular container, the laminate 100 may further include a second sealant layer 40 on the side of the outer layer base material 10 opposite the sealant layer 30, as shown in Fig. 3.

[0021] According to the laminate 100, even if the content of recycled resin is sufficiently high, hygiene and quality can be improved.

[0022] (Outer Layer Substrate) The outer layer substrate 10 can be a film substrate made of a resin material. Examples of such resin materials include polyester films such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene and polypropylene, polystyrene, polyamides such as nylon 66, polycarbonate, polyacrylonitrile, polyimide, and other engineering plastics. Resin materials having mechanical strength and dimensional stability are preferred. The resin materials are processed into a film and used as the film substrate.

[0023] The resin material may be a non-recycled resin, a recycled resin, or a mixture thereof. When using a recycled resin for the outer layer base material 10 because it does not come into contact with the contents, a material-recycled resin may be used, but from the viewpoints of hygiene and quality, it is preferable to use a chemically recycled resin. The non-recycled resin may be a petroleum-derived resin obtained using petroleum-derived raw material monomers, a biomass-derived resin obtained using biomass-derived raw material monomers, or a mixture thereof, but from the viewpoint of reducing the environmental load, a biomass-derived resin is preferable. The chemically recycled resin may be composed of a single chemically recycled resin, or a mixture of multiple types of chemically recycled resins.

[0024] The outer layer substrate 10 may have either a single layer or a multilayer structure. In the case of a multilayer structure, the outer layer substrate 10 is formed from two or more layers, at least one of which contains a chemically recycled resin. The outer layer substrate 10 may also be formed by co-extrusion of a layer made of an ethylene-vinyl alcohol copolymer or a layer made of a polyamide, optionally with an adhesive resin, and stretching the resulting film. Examples include a three-type, five-layer substrate consisting of chemically recycled resin / adhesive resin / ethylene-vinyl alcohol copolymer / adhesive resin / chemically recycled resin, a three-type, three-layer substrate consisting of chemically recycled resin / adhesive resin / ethylene-vinyl alcohol copolymer, a multilayer substrate consisting of petroleum-derived (natural) resin / chemically recycled resin / petroleum-derived (natural) resin, or a petroleum-derived (natural) resin / other polyolefin / chemically recycled resin / other resin / petroleum-derived (natural) resin, etc. In the multilayer substrate 10, the specific gravities of the same materials may differ depending on their functions.

[0025] The outer layer base material 10 may further contain additives such as a filler, an antistatic agent, a plasticizer, a lubricant, a light-shielding pigment, and an antioxidant, as necessary. When the outer layer base material 10 contains a light-shielding pigment, the outer layer base material 10 is able to function as a light-shielding layer.

[0026] The outer layer base material 10 may be an unstretched film or a stretched film. The stretched film may be a uniaxially stretched film or a biaxially stretched film. The outer layer base material 10 may be composed of either a stretched film or an unstretched film. When the outer layer base material 10 is uniaxially stretched, the tearability and heat resistance of the laminate 100 can be improved. When the outer layer base material 10 is a biaxially stretched film, the mechanical strength and dimensional stability of the laminate 100 can be improved.

[0027] When an adhesive layer is provided on the surface of the outer layer base material 10, various pretreatments such as corona treatment, plasma treatment, ozone treatment, and flame treatment may be performed on the surface on the adhesive layer side, or a coating layer such as an easy-adhesion layer may be provided, in order to enhance adhesion to the adhesive layer.

[0028] The thickness of the outer layer base material 10 is not particularly limited and is, for example, 10 μm or more and 100 μm or less. From the perspective of reducing material usage to reduce environmental impact and from the perspective of obtaining excellent heat resistance, impact resistance, and gas barrier properties, the thickness of the outer layer base material 10 may be 15 μm or more, 20 μm or more, 25 μm or more, 30 μm or more, or 40 μm or more. The thickness of the outer layer base material 10 may also be 60 μm or less, or 50 μm or less.

[0029] (Sealant Layer) The sealant layer 30 is made of a polyolefin resin film containing polyolefin resins such as polyethylene and polypropylene, and the polyolefin resins include chemically recycled resins. Polyethylene is a resin containing ethylene as a structural unit. Examples of polyethylene include ethylene homopolymers and copolymers of ethylene with other monomers. The proportion of ethylene in the polyethylene is, for example, 80 mol% or more. Examples of other monomers include α-olefins, vinyl acetate, and acrylic esters. The α-olefin may be an olefin having a carbon number in the range of 3 to 20. Examples of α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, 3-methyl-1-butene, 4-methyl-1-pentene, and 6-methyl-1-heptene. Examples of polyethylene include high density polyethylene (HDPE), medium density polyethylene (MDPE), low density polyethylene (LDPE), linear low density polyethylene (LLDPE), very low density polyethylene (VLDPE), ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-methyl acrylate copolymer, ethylene-methacrylic acid copolymer, ethylene-propylene copolymer, etc. These may be used alone or in combination of two or more.

[0030] Polypropylene is a resin containing propylene as a structural unit, but may not contain ethylene as a structural unit, and may be a copolymer of propylene alone or with ethylene or various α-olefins. Examples of polypropylene include homopolypropylene, block polypropylene, and random polypropylene.

[0031] The sealant layer 30 preferably has a melting point lower than the melting point of the outer layer base material 10. In this case, when the laminate 100 is heat-sealed, it is possible to heat-seal the sealant layer 30 while suppressing melting of the outer layer base material 10. Furthermore, by heating the laminate 100, the outer layer base material 10 and the sealant layer 30 can be easily separated, and material recycling of each of the outer layer base material 10 and the sealant layer 30 can be easily carried out.

[0032] The sealant layer 30 may further contain additives such as a flame retardant, a slip agent, an antiblocking agent, an antioxidant, a light stabilizer, a tackifier, an antistatic agent, a light-shielding pigment, etc. When the sealant layer 30 contains a light-shielding pigment, the sealant layer 30 can function as a light-shielding layer.

[0033] The sealant layer 30 may be composed of a single layer or multiple layers. When the sealant layer 30 is composed of a single layer, a polyolefin resin film containing a chemically recycled resin (chemically recycled polyolefin resin) as the recycled resin is used. In this case, the sealant layer 30 may also contain a petroleum-derived polyolefin resin or a biomass-derived polyolefin resin. The sealant layer 30 is the layer that comes into contact with the contents when the contents are placed in a packaging container obtained using the laminate 100. When the sealant layer 30 is a polyolefin resin film containing a chemically recycled polyolefin resin, the sealant layer 30 contains less foreign matter such as impurities, gels, and aggregates, which further reduces the possibility of impurities, gels, aggregates, and other foreign matter migrating to the contents upon heating during retort or boiling treatment of the packaging container. Therefore, the laminate 100 can be safely used to package contents such as food. When the sealant layer 30 is composed of multiple layers, all of the layers may be polyolefin resin films containing chemically recycled polyolefin resin, or the sealant layer 30 may have a multilayer structure consisting of a non-recycled polyolefin resin film and a polyolefin resin film containing chemically recycled polyolefin resin. When the sealant layer 30 has three layers, the multiple layers may be composed of a first outer layer, an intermediate layer, and a second outer layer. For example, the first outer layer and the second outer layer may be composed of non-recycled polyolefin resin films, and the intermediate layer may be composed of a recycled polyolefin resin film. The sealant layer 30 may also be colored white or other colors. For example, a white sealant containing a titanium oxide-based white pigment can be used. The sealant layer 30 is not limited to a white sealant, and may be composed of a sealant of a different color by containing a pigment other than the white pigment.

[0034] The thickness of the sealant layer 30 is not particularly limited and may be adjusted appropriately depending on the application of the laminate 100. The thickness of the sealant layer 30 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the sealant layer 30 may also be 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0035] (Second sealant layer) The second sealant layer 40 may be the same as the sealant layer 30. The thickness of the second sealant layer 40 may be the same as or different from the thickness of the sealant layer 30. The material constituting the second sealant layer 40 may also be the same as or different from the material constituting the sealant layer 30.

[0036] (Intermediate Substrate) The intermediate substrate 20 is a substrate that reinforces the outer layer substrate 10 and can further improve the strength of the laminate 100. The intermediate substrate 20 can be a film substrate made of the same resin material as the resin material used in the outer layer substrate 10. That is, examples of resin materials include polyester films such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyolefin resins such as polyethylene and polypropylene, polystyrene, polyamides such as nylon 66, polycarbonate, polyacrylonitrile, polyimide, and other engineering plastics. As the resin material, a resin material having mechanical strength and dimensional stability is preferred. The resin material is processed into a film and used as the film substrate. The film substrate may be an unstretched film or a stretched film.

[0037] The intermediate substrate 20 may be a single layer or a laminate of multiple layers. When the intermediate substrate 20 is composed of a single layer, it may be a recycled polyolefin resin film or a non-recycled polyolefin resin film. When the intermediate substrate 20 is composed of multiple layers, all layers may be recycled polyolefin resin films, non-recycled polyolefin resin films, or some layers may be non-recycled polyolefin resin films and the remaining layers may be recycled polyolefin resin films. Materials other than those listed above can be used for the intermediate substrate 20 as long as the recycled resin content in the laminate 100 is 10% by volume or more or 10% by mass or more. For example, polyethylene terephthalate resin can be used as the material for the intermediate substrate 20, although this reduces the polyolefin resin content in the packaging material. Furthermore, using polyethylene terephthalate resin produced by chemical recycling as the material for the intermediate substrate 20 can increase the recycled resin content. Nylon resin film or the like can also be used for the intermediate substrate 20. Furthermore, nylon resin film produced by chemical recycling may also be used as the nylon resin film. When the plurality of layers is three, the plurality of layers may be composed of a first outer layer, an intermediate layer, and a second outer layer. Here, the first outer layer and the second outer layer may be composed of non-recycled polyolefin resin films, and the intermediate layer may be composed of a recycled polyolefin resin film. In this case, the possibility that foreign matter such as impurities, gels, and aggregates will migrate from the intermediate substrate 20 through the sealant layer 30 to the contents due to heating during retort or boiling treatment of the packaging container can be further reduced. Therefore, the laminate 100 can be safely used to package contents such as food.

[0038] The thickness of the intermediate substrate 20 is not particularly limited and is adjusted appropriately depending on the application of the laminate 100. The thickness of the intermediate substrate 20 may be, for example, 10 μm or more, 25 μm or more, 30 μm or more, 40 μm or more, or 50 μm or more. The thickness of the intermediate substrate 20 may also be 100 μm or less, 80 μm or less, 60 μm or less, or 50 μm or less.

[0039] (Adhesive Layer) Examples of the adhesive layer include an adhesive layer formed using an adhesive agent and an adhesive layer containing an adhesive resin (hereinafter also referred to as an "adhesive resin layer").

[0040] Examples of adhesives include known adhesives such as urethane adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, and isocyanate adhesives.

[0041] The adhesive may or may not contain a biomass-derived component, but preferably contains a biomass-derived component from the viewpoint of reducing the environmental impact. Specific examples of biomass-derived components include the "DIC Dry BM Series" manufactured by DIC Corporation and the "ECOAD Series" manufactured by Toyo Ink Co., Ltd.

[0042] The adhesive may be an adhesive containing an organic solvent or an adhesive containing no organic solvent, but from the viewpoint of reducing the environmental load, an adhesive containing no organic solvent (solvent-free adhesive) is preferred.

[0043] The adhesive resin layer may be an extruded resin layer or a non-extruded resin layer. The adhesive resin is a heat-sealable adhesive thermoplastic resin that can be melted and mutually fused by heat. For example, low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear (linear) low-density polyethylene, polypropylene, ethylene-propylene copolymer, methylpentene polymer, acid-modified polyolefin resins obtained by modifying polyolefin resins such as polyethylene or polypropylene with unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, and the like can be used. The thickness of the adhesive layer is not particularly limited and may be, for example, 1 μm or more. By making the thickness of the adhesive layer 1 μm or more, sufficient adhesive strength can be obtained. The thickness of the adhesive layer may be 2 μm or more. The thickness of the adhesive layer may be 50 μm or less, 5 μm or less, or 3 μm or less.

[0044] (Printed Layer) As shown in FIG. 2 or FIG. 3, the printed layer 50 may be provided between layers in the laminate 100, or on the outside. When the printed layer 50 is provided between layers, the printed layer 50 is provided on the surface opposite the sealant layer 30 side (outer surface), for example, as shown in FIG. 2 or FIG. 3. The printed layer 50 may also be provided on the surface of the outer layer base material 10 facing the sealant layer 30 (inner surface). When the printed layer 50 is provided on the inner surface of the outer layer base material 10, the printed layer 50 is protected by the outer layer base material 10, and deterioration of the printed layer 50 can be prevented. When the printed layer 50 is provided on the outer surface of the outer layer base material 10 and the printed layer 50 is the outermost layer of the laminate 100, the printed layer 50 can be easily removed when recycling a package including the laminate 100 after disposal. 2 or 3, when the laminate 100 includes an intermediate substrate 20, the printed layer 50 may be provided on the intermediate substrate 20. Here, the printed layer 50 may be provided between the outer layer substrate 10 and the intermediate substrate 20 as shown in FIG. 2 or 3, or may be provided between the intermediate substrate 20 and the sealant layer 30.

[0045] Furthermore, when the laminate 100 includes a second sealant layer 40, the printed layer 50 may be provided on the second sealant layer 40. When the printed layer 50 is provided on the second sealant layer 40, providing the printed layer 50 on the surface (outer surface) of the second sealant layer 40 opposite the outer layer base material 10 makes it possible to easily remove the printed layer 50 when recycling the package including the laminate 100 after disposal. The printed layer 50 is a layer that displays letters, pictures, etc., and can be formed using ink.

[0046] As the ink, for example, inks obtained by adding various pigments, plasticizers, drying agents, stabilizers, etc. to a binder resin such as a urethane-based, acrylic-based, nitrocellulose-based, or rubber-based ink can be used.

[0047] The ink may be either an aqueous ink or an oil-based ink, but is preferably an aqueous ink. Because an aqueous ink uses water or alcohol as a solvent, it can further reduce the environmental impact. In particular, when the adhesive is a solventless adhesive, using an aqueous ink as the ink can significantly reduce the environmental impact. The ink may be a biomass ink or not, but from the perspective of reducing the environmental impact, a biomass ink is preferred. Here, biomass ink refers to an ink containing components obtained from biological resources (biomass), such as cotton, pulp, rice bran, vegetable oil, and angiosperm seeds. The ink may be a recycled ink obtained by recovering and recycling used ink, or a non-recycled ink, but from the perspective of reducing the environmental impact, a recycled ink is preferred. Furthermore, an easily recyclable ink can also be used as the ink. The use of an easily recyclable ink makes it possible to easily recycle the packaging after disposal. Specifically, an example of an easily recyclable ink is "SunSpectro Solvawash" manufactured by DIC Corporation.

[0048] (Gas barrier layer) As shown in Fig. 2 or 3, the laminate 100 may include a gas barrier layer 60 together with the printed layer 50, or may include the gas barrier layer 60 instead of the printed layer 50. The gas barrier layer 60 may be provided on at least one surface of the outer layer substrate 10. Furthermore, when the laminate 100 includes an intermediate substrate 20, the gas barrier layer 60 may be provided on at least one surface of the intermediate substrate 20, as shown in Fig. 2 or 3. The gas barrier layer 60 is a layer that improves the gas barrier properties of the laminate 100. The gas barrier layer 60 has barrier properties against gases such as water vapor or oxygen, for example.

[0049] The gas barrier layer 60 may be, for example, a vapor deposition layer such as a metal vapor deposition layer or an inorganic compound vapor deposition layer. Examples of metals include aluminum and silicon. Examples of inorganic oxides include aluminum oxide and silicon oxide (silica). When the gas barrier layer 60 is a vapor deposition layer of a metal such as aluminum, the gas barrier layer 60 can function as a light-blocking layer. The gas barrier layer 60 may further include an overcoat layer on the vapor deposition layer. Examples of the overcoat layer include a coating layer obtained using a composition containing a water-soluble polymer and silicon alkoxide, or a coating layer made of a resin such as urethane.

[0050] (Other Layers) The laminate 100 may further include a layer containing a resin other than polyolefin resin (non-polyolefin resin) as long as the recycled resin content is 10% by volume or more or 10% by mass or more. Examples of non-polyolefin resins include polyamide resins such as nylon and polyester resins such as polyethylene terephthalate (PET).

[0051] (Laminate) (A) Recycled Resin Content In the laminate 100, the recycled resin content in the laminate 100 is 10% by volume or more or 10% by mass or more. When the recycled resin content in a polyolefin resin film containing recycled resin is 100% by volume (100% by mass), the recycled resin content in the laminate 100 can be determined as the ratio of the total thickness of the film to the total thickness of the laminate 100. However, when the recycled resin content in a polyolefin resin film containing recycled resin is X% by mass (less than 100% by mass) and the thickness of the film is Y1 (μm), the recycled resin content is calculated as X / 100×Y1 (μm) for the film thickness Y2 (μm). The content of recycled resin in the laminate 100 is preferably 20% by volume or more or 20% by mass or more, more preferably 25% by volume or more or 25% by mass or more, even more preferably 30% by volume or more or 30% by mass or more, and particularly preferably 40% by volume or more or 40% by mass or more.

[0052] In the present disclosure, the recycled resin is a chemically recycled resin and does not include materially recycled resin. The chemically recycled resin may be a post-consumer recycled resin (PCR), a post-industrial recycled resin (PIR), or a mixture thereof, but is preferably PCR. Since PCR is available in large quantities on the market, if the chemically recycled resin is PCR, the cost of the laminate 100 can be reduced.

[0053] (B) Odor Components In a total ion chromatogram obtained by performing mass analysis of the laminate 100 using purge-and-trap gas chromatography-mass spectrometry, the ratio of the peak area of ​​nonanal as an indicator of odor components to the sum of the peak areas of all aliphatic hydrocarbon components is R1 (%), and the ratio of the peak area of ​​decanal to the sum of the peak areas of all aliphatic hydrocarbon components is R2 (%). R1 ​​is preferably less than 1.5%, more preferably 1.0% or less, and particularly preferably 0.5% or less. Furthermore, R2 is preferably less than 3.5%, more preferably 2.5% or less, and particularly preferably 1.5% or less. It is preferable that R1 is less than 1.5% and R2 is less than 3.5%. In this case, thermal degradation is suppressed overall in the laminate 100, and the quality of the laminate 100 can be further improved. Specifically, the mass analysis is carried out by cutting out a 1.0 gram sample from the laminate 100, placing this sample in a 20 mL vial together with a collector of odor components, heating it at 60°C for 1 hour to adsorb the volatile components from the sample onto the collector, and then analyzing the volatile components in the collector using a purge-and-trap gas chromatograph mass analyzer.

[0054] (C) Fisheyes Fisheyes refer to foreign matter such as gelled or charred particles that can be found on film. If a fisheye has a diameter of 1 mm or more, the product will be deemed defective. If the number of fisheyes is 0.5 mm or more but less than 1 mm, the product will be deemed defective. 2 Less than or equal to 50 particles / m 2 Particularly preferably 10 pieces / m or less 2 It would be better if it was below.

[0055] (D) Variation in Dynamic Friction Force On the surface of the sealant layer 30 of the laminate 100, the variation in dynamic friction force (in-plane variation) σ refers to the standard deviation of the dynamic friction force. σ is preferably less than 0.45, more preferably less than 0.35, and particularly preferably less than 0.2. When σ is less than 0.45, the transportability of the laminate 100 can be improved when the layer with σ less than 0.45 is on the transport roller side. Furthermore, on the surface of the layer, regions where the dynamic friction force received from the transport roller is high and regions where it is low appear, and the difference in stress between these regions is reduced. This reduces residual strain within the layer, and can also suppress a decrease in the strength of the laminate 100 due to this residual strain. Furthermore, from the viewpoint of the strength of the laminate, σ is preferably 0.1 or more, more preferably 0.2 or more, and particularly preferably 0.3 or more. The dynamic friction coefficient is measured for the laminate 100 using a multi-function static and dynamic friction tester TL201Tt (manufactured by Trinity Lab Co., Ltd.) and a tactile probe. The standard deviation σ of the dynamic friction force is a value obtained based on JIS K 7125-ISO8295, and specifically, is determined by placing the laminate 100 on a test table with the sealant layer 30 facing downward, and moving the tactile probe at a sliding speed of 10 mm / sec while contacting the laminate 100 with a load of 50 grams.

[0056] (E) Impurities The laminate 100 is analyzed using a Fourier transform infrared spectrophotometer (FT-IR: Fourier transform infrared spectroscopy) by attenuated total reflection (ATR) to obtain an ATR spectrum. In the ATR spectrum, -1 The absorption coefficient of the methylene group C-H inverse symmetric stretching near 1720 cm -1The ratio R3 of the absorption coefficients of C=O stretching near the polyolefin is preferably less than 0.1, more preferably less than 0.05, and particularly preferably 0.01 or less, as an indicator of the small amount of resin components other than polyolefin. In the above analysis, a diamond prism is used as the prism to be closely attached to the laminate 100, and the angle of incidence with respect to the surface of the laminate 100 is 45°.

[0057] Furthermore, when the laminate 100 includes an outer layer base material 10 and a sealant layer 30, both the outer layer base material 10 and the sealant layer 30 may be recycled polyolefin resin films.

[0058] <Packaging Item> Next, an embodiment of a packaging item according to another aspect of the present disclosure will be described with reference to FIG. 4. FIG. 4 is a cross-sectional view showing one embodiment of a packaging item according to another aspect of the present disclosure. As shown in FIG. 4, a packaging item 500 includes a packaging bag 400 as a packaging container and a content C accommodated in the packaging bag 400. The packaging bag 400 is obtained using a pair of laminates 100. The packaging bag 400 is obtained, for example, by bringing the sealant layers 30 of the pair of laminates 100 face each other and adhering their peripheral edges. The packaging bag 400 is composed of a storage section that accommodates the content C and an adhesive section provided around the storage section. The adhesive section is a section formed by adhering the sealant layers 30 of opposing laminates 100 to each other, and the storage section is a section where the sealant layers 30 of opposing laminates 100 are not adhered to each other.

[0059] According to the packaging item 500, the chemically recycled resin contained in the laminate 100 is less likely to be contaminated with foreign matter such as impurities, gels, and aggregates than material recycled resin, which is a resin made by cleaning and crushing used resin products such as recovered packaging materials, then melting them with heat to recycle them into raw materials. Furthermore, unlike material recycled resin, chemically recycled resin is not affected by heat treatments such as melting after the recycling process, and is therefore less susceptible to thermal degradation. Therefore, the packaging item 500 can safely contain contents C, such as food, even if the recycled resin content in the laminate 100 is sufficiently high, at 10% by volume or more or 10% by mass or more. Furthermore, because the laminate 100 can improve quality, the packaging item 500 equipped with a packaging bag 400 obtained using the packaging laminate 100 can improve properties such as strength.

[0060] (Contents) The contents C are not particularly limited and may be appropriately selected depending on the intended use of the packaging bag 400. The contents C are not particularly limited, and examples of the contents C include food, shampoo, conditioner, body soap, and detergent.

[0061] (Packaging Bag) The pair of laminates 100 constituting the packaging bag 400 may have the same configuration as each other, or may have different configurations from each other.

[0062] The packaging bag 400 may have a half-cut line, and may further have an easy-open processed part at both ends or one end of the half-cut line. Examples of the easy-open processed part include a group of scars, and a V-shaped, U-shaped, or I-shaped notch.

[0063] In the adhesive portion of the packaging bag 400, the sealant layers 30 of the pair of laminates 100 may be directly bonded to each other by heat sealing (see FIG. 4), or may be bonded to each other by an adhesive.

[0064] (Method for Manufacturing Packaged Article) Next, an example of a method for manufacturing the packaged article 500 using the laminate 100 will be described.

[0065] First, a pair of laminates 100 is prepared. Then, the sealant layers 30 of the pair of laminates 100 are placed opposite each other and bonded together. At this time, parts of the peripheral edges of the laminates are bonded together in a U-shape to form bonded sections, and unbonded sections (unbonded sections) are also formed. In this way, a packaging bag having an opening formed by the unbonded sections is obtained.

[0066] Next, the contents C are filled into the packaging bag through the opening. Thereafter, the sealant layers 30 of the laminate 100 are bonded together at the unbonded portions, thereby making the unbonded portions also bonded. In this manner, a packaged article 500 including the packaging bag 400 and the contents C contained therein can be manufactured.

[0067] Although preferred embodiments of the present disclosure have been described above, the present disclosure is not limited to the above embodiments. For example, in the packaged article 500 shown in Fig. 4, the packaging bag 400 is formed using a pair of laminates 100, but the laminates 100 may be replaced with a laminate 200. The packaging bag may also be manufactured by folding one laminate 100, 200 with the sealant layer 30 facing inward and bonding the overlapping peripheral edges together.

[0068] 4, the packaging bag 400 may be a standing pouch-shaped packaging bag, a two-sided bag, a three-sided bag, a four-sided bag, a palm-shaped bag, or a gusset bag. The packaging bag 400 may be provided with a stopper or a synthetic resin zipper that can be repeatedly sealed by fitting a strip-shaped protrusion and a strip-shaped groove.

[0069] In the above embodiment, the packaging container is configured as a packaging bag, but the packaging container may be a tube container. When the packaging container is a tube container, the laminate 100 includes a second sealant layer 40 that is adhered to the outer layer base material 10.

[0070] The above describes embodiments of the present disclosure, but the outline of the present disclosure is as follows. [1] A packaging laminate comprising an outer layer substrate and a sealant layer, wherein the sealant layer is a polyolefin resin film containing a recycled resin, the content of the recycled resin in the packaging laminate is 10% by volume or more or 10% by mass or more, and the recycled resin is a chemically recycled resin. [2] The packaging laminate according to [1], wherein the content of the recycled resin in the packaging laminate is 20% by volume or more or 20% by mass or more. [3] The packaging laminate according to [1] or [2], wherein the thickness of the sealant layer is greater than the thickness of the outer layer substrate, and the content of the recycled resin contained in the sealant layer is 20% by volume or more or 20% by mass or more. [4] The packaging laminate according to any of [1] to [3], further comprising an intermediate substrate between the outer layer substrate and the sealant layer. [5] The laminate for packaging according to any one of [1] to [4], further comprising a gas barrier layer between the outer layer base material and the sealant layer. [6] The laminate for packaging according to any one of [1] to [5], further comprising a second sealant layer on the surface of the outer layer base material opposite to the sealant layer side. [7] A packaging container obtained using the laminate for packaging according to any one of [1] to [6]. [8] A packaging article comprising the packaging container according to [7] and contents to be placed in the packaging container.

[0071] The present disclosure will be explained in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0072] Example 1 A petroleum-derived biaxially oriented PET film (thickness: 35 μm) was prepared as the outer layer substrate, and a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness: 50 μm) was prepared as the sealant layer. Note that "PCR Chemi R 100%-LDPE" means that the content of post-consumer chemical recycled resin (PCR Chemi R) in the sealant layer was 100% by volume (100% by mass). A printed layer was then formed on one surface of the outer layer substrate using aqueous flexographic ink, and a dry lamination adhesive (urethane adhesive) was applied to the surface of the printed layer to form an adhesive layer with a thickness of 3 μm (dry film thickness). A sealant layer was then bonded to the adhesive layer to produce a packaging laminate (outer layer substrate / printed layer / adhesive layer / sealant layer).

[0073] Example 2: A petroleum-derived biaxially oriented PET film (35 μm thick) was prepared as the outer layer substrate, a biaxially oriented PET film (35 μm thick) was prepared as the intermediate substrate, and a chemically recycled low-density polyethylene (PCR ChemiR 100%-LDPE) film (50 μm thick) was prepared as the sealant layer. Note that "PCR ChemiR 100%-LDPE" indicates that the post-consumer chemical recycled resin (PCR ChemiR) content in the sealant layer was 100% by volume (100% by mass). A 10-nm-thick layer of aluminum oxide was vapor-deposited on one side of the intermediate substrate, and a 300-nm-thick organic-inorganic hybrid layer was formed as an overcoat layer on the resulting vapor-deposited layer. The organic-inorganic hybrid layer was formed using a composition containing polyvinyl alcohol resin and tetraethoxysilane. Next, a printing layer was formed on one surface of the outer layer substrate using an aqueous flexographic ink, and then a dry laminating adhesive (urethane adhesive) was applied to the surface of the printing layer to form a first adhesive layer with a thickness of 3 μm (dry film thickness), and the overcoat layer of the intermediate substrate was bonded to the first adhesive layer. Subsequently, a dry laminating adhesive (urethane adhesive) was applied to the surface of the intermediate substrate opposite the overcoat layer to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and a sealant layer was bonded to the second adhesive layer to produce a packaging laminate (outer layer substrate / printing layer / first adhesive layer / overcoat layer / vapor-deposited layer / intermediate substrate / second adhesive layer / sealant layer).

[0074] (Example 3) The outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a biomass-derived biaxially oriented PET film (thickness 35 μm), the sealant layer was changed from a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 50 μm) to a chemically recycled low-density polyethylene (PCR Chemi R 40%-LDPE) film (thickness 50 μm), and the adhesive was changed from a dry lamination adhesive (urethane-based adhesive) to a solventless adhesive (polyester-based) to form an adhesive layer with a thickness of 1.5 μm (after drying). A packaging laminate (outer layer substrate / printed layer / adhesive layer / sealant layer) was produced in the same manner as in Example 1. Note that "PCR Chemi R 40%-LDPE" means that the content of post-consumer chemical recycled resin (PCR Chemi R) in the sealant layer is 40% by mass.

[0075] (Example 4) The intermediate substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived polyamide film (nylon 6: thickness 35 μm), and the sealant layer was changed from a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 50 μm) to a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm), a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 20 μm), and a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm). Except for this, a laminate for packaging (outer layer substrate / printed layer / first adhesive layer / overcoat layer / deposited layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 2.

[0076] (Example 5) The outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived polyamide film (nylon 6: thickness 35 μm), and the sealant layer was changed from a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 50 μm) to a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm), a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 20 μm), and a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm). Except for this, a laminate for packaging (outer layer substrate / printed layer / first adhesive layer / overcoat layer / deposited layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 2.

[0077] Example 6 A packaging laminate (outer layer substrate / printed layer / first adhesive layer / overcoat layer / vapor-deposited layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 2, except that the outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived oriented polypropylene film (OPP: thickness 35 μm), the intermediate substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived oriented polypropylene film (OPP: thickness 35 μm), and the sealant layer was changed from a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 50 μm) to an unstretched polypropylene (PCR Chemi R 40%-CPP) film (thickness 50 μm) containing 40% by mass of chemically recycled polypropylene. The vapor deposition layer on the OPP film of the intermediate substrate was formed by vapor deposition of silicon oxide to a thickness of 10 nm, and the overcoat layer was an organic-inorganic hybrid layer formed using a composition containing polyvinyl alcohol resin, tetraethoxysilane, and a silane coupling agent.

[0078] Example 7 A packaging laminate (outer layer substrate / printed layer / first adhesive layer / overcoat / vapor deposition layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 2, except that the outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived oriented polypropylene film (OPP: thickness 25 μm) and the intermediate substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived oriented polypropylene film (OPP: thickness 25 μm). The vapor deposition layer on the OPP film of the intermediate substrate was formed by vapor deposition of silicon oxide with a thickness of 10 nm, and the overcoat layer was an organic-inorganic hybrid layer formed using a composition containing a polyvinyl alcohol resin, tetraethoxysilane, and a silane coupling agent.

[0079] (Example 8) The outer layer substrate was changed from a petroleum-derived oriented polypropylene film (OPP: thickness 25 μm) to a biomass-derived oriented polypropylene film (OPP: thickness 25 μm), and the sealant layer was changed from a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 50 μm) to a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm), a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 20 μm), and a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm). A laminate for packaging (outer layer substrate / printed layer / first adhesive layer / overcoat layer / deposited layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 7, except that the outer layer substrate was changed from a petroleum-derived oriented polypropylene film (OPP: thickness 25 μm) to a biomass-derived oriented polypropylene film (OPP: thickness 25 μm), and the sealant layer was changed from a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 50 μm) to a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm). A laminate for packaging (outer layer substrate / printed layer / first adhesive layer / overcoat layer / deposited layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 7, except that the outer layer substrate was changed from a petroleum-derived oriented polypropylene film (OPP: thickness 25 μm) to a petroleum-derived low-density polyethylene (LDPE) film (thickness 50 μm).

[0080] (Example 9) A petroleum-derived biaxially oriented PET film (thickness 30 μm) was prepared as the outer layer substrate, and a three-layer co-extruded film of a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm), a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 40 μm), and a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm) was prepared as the sealant layer. A petroleum-derived low-density polyethylene (LDPE) film (thickness 80 μm) was prepared as the second sealant layer (outer sealant layer). Note that "PCR Chemi R 100%-LDPE" means that the content of post-consumer chemical recycled resin (PCR Chemi R) in the PCR Chemi R 100%-LDPE film of the sealant layer was 100% by volume (100% by mass). Then, a printed layer was formed on one surface of the second sealant layer (outer sealant layer) using an aqueous flexographic ink, and then a dry laminating adhesive (urethane-based adhesive) was applied to one surface of the outer layer substrate to form a first adhesive layer with a thickness of 3 μm (dry film thickness), and the outer layer substrate and the surface of the second sealant layer (outer sealant layer) opposite the printed layer were bonded together using the first adhesive layer. Subsequently, a dry laminating adhesive (urethane-based adhesive) was applied to the other surface of the outer layer substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the sealant layer was bonded to the second adhesive layer to produce a packaging laminate (printed layer / second sealant layer (outer sealant layer) / first adhesive layer / outer layer substrate / second adhesive layer / sealant layer).

[0081] (Example 10) The outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 30 μm) to a petroleum-derived oriented polypropylene film (OPP: thickness 30 μm), and the second sealant layer (outer sealant layer) was changed from a petroleum-derived low-density polyethylene (LDPE) film (thickness 80 μm) to a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm) and a chemically recycled low-density polyethylene (PCR Chemi R 100%-LDPE) film (thickness 40 μm) and a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm). Except for this, a packaging laminate (printed layer / second sealant layer (outer sealant layer) / first adhesive layer / outer layer substrate / second adhesive layer / sealant layer) was produced in the same manner as in Example 9. The vapor deposition layer on the OPP film of the outer layer substrate was formed by vapor deposition of silicon oxide to a thickness of 10 nm, and the overcoat layer was an organic-inorganic hybrid layer formed using a composition containing polyvinyl alcohol resin, tetraethoxysilane, and a silane coupling agent.

[0082] Comparative Example 1 A petroleum-derived biaxially oriented PET film (35 μm thick) was prepared as the outer layer substrate, and a low-density polyethylene (PCRMR100%-LDPE) film (60 μm thick) made by material recycling using used polyethylene bags was prepared as the sealant layer. Note that "PCRMR100%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the outer layer substrate is 100% by volume (100% by mass). A printed layer was then formed on one surface of the outer layer substrate using aqueous flexographic ink, a dry laminating adhesive (urethane adhesive) was applied to the surface of the printed layer to form an adhesive layer with a thickness of 3 μm (dry film thickness), and a sealant layer was bonded to the adhesive layer to produce a packaging laminate (outer layer substrate / printed layer / adhesive layer / sealant layer).

[0083] (Comparative Example 2) The outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived biaxially oriented PET film (thickness 50 μm), and the sealant layer was changed from a PCRMR 100%-LDPE film (thickness 60 μm) to a low-density polyethylene (PCRMR 40%-LDPE) film (thickness 60 μm) obtained by cleaning used polyethylene bags and mechanically recycling low-density polyethylene (PCRMR-LDPE) pellets and petroleum-derived LDPE pellets in a 40:60 (mass ratio). Except for this, a packaging laminate (outer layer substrate / printing layer / adhesive layer / sealant layer) was produced in the same manner as in Comparative Example 1. Note that "PCRMR 40%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the sealant layer is 40% by mass. In this case, the volume of the layer made of recycled materials can be calculated by taking into account the density of the mixed resin, and the film thickness ratio can be calculated using this. Note that the densities of the mixed resins are the same, and mass % is volume %. The density of the PCRMR40%-LDPE film used in the sealant layer is low density (0.920 g / cm 3 )

[0084] (Comparative Example 3) A petroleum-derived biaxially oriented PET film (35 μm thick) was prepared as the outer layer substrate, a petroleum-derived biaxially oriented PET film (35 μm thick) was prepared as the intermediate substrate, and a three-layer co-extruded film was prepared as the sealant layer: a petroleum-derived low-density polyethylene (LDPE) film (20 μm thick), a low-density polyethylene (PCRMR100%-LDPE) film (20 μm thick) material recycled from used polyethylene bags, and a petroleum-derived low-density polyethylene (LDPE) film (20 μm thick). A printed layer was then formed on one side of the outer layer substrate using aqueous flexographic ink, a laminating adhesive (urethane adhesive) was applied to the surface of the printed layer, a first adhesive layer with a thickness of 3 μm (dry film thickness), and the intermediate substrate was bonded to the first adhesive layer. Next, a dry lamination adhesive (urethane adhesive) was applied to the surface of the intermediate substrate opposite the first adhesive layer to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and a sealant layer was bonded to the second adhesive layer to produce a packaging laminate (outer layer substrate / printed layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer).

[0085] (Comparative Example 4) The outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived biaxially oriented polypropylene film (OPP: thickness 35 μm), the intermediate layer was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived biaxially oriented polypropylene film (OPP: thickness 35 μm), and the sealant layer was changed from a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm) and a low-density polyethylene (PCRMR100%-LDPE) film (thickness 20 μm) obtained by material recycling using used polyethylene bags to a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm) and a petroleum-derived low-density polyethylene (LDPE) film (thickness 20 μm) three-layer co-extruded film of a low-density polyethylene (PCRMR100%-LDPE) film (thickness 50 μm) obtained by material recycling using used polyethylene bags. A packaging laminate (outer layer substrate / printed layer / first adhesive layer / intermediate substrate / second adhesive layer / sealant layer) was produced in the same manner as in Comparative Example 3, except that the outer layer substrate was changed from a petroleum-derived biaxially oriented PET film (thickness 35 μm) to a petroleum-derived low-density polyethylene (PCRMR100%-LDPE) film (thickness 50 μm) obtained by material recycling using used polyethylene bags.

[0086] Comparative Example 5 A petroleum-derived biaxially oriented PET film (thickness 50 μm) was prepared as the outer layer substrate. A low-density polyethylene (PCRMR40%-LDPE) film (thickness 80 μm) was prepared as the sealant layer by washing used polyethylene bags and mixing low-density polyethylene (PCRMR-LDPE) pellets obtained by mechanical recycling with petroleum-derived LDPE pellets in a ratio of 40:60 (mass ratio). A low-density polyethylene (PCRMR40%-LDPE) film (thickness 80 μm) was prepared as the second sealant layer (outer sealant layer) by washing used polyethylene bags and mixing low-density polyethylene (PCRMR-LDPE) pellets obtained by mechanical recycling with petroleum-derived LDPE pellets in a ratio of 40:60 (mass ratio). Incidentally, "PCRMR40%-LDPE" means that the content of post-consumer mechanically recycled resin (PCRMR) in the sealant layer or the second sealant layer is 40% by mass. In this case, the volume of the sealant layer or the second sealant layer can be calculated taking into account the density of the mixed resins, and this can be used to calculate the film thickness ratio. Note that the densities of the mixed resins are the same, and mass% is volume%. The density of the PCRMR-LDPE40% film used for the outer layer substrate is low density (0.920 g / cm 3 ). Then, a printed layer was formed on one surface of the second sealant layer (outer sealant layer) using aqueous flexographic ink, and then a dry laminating adhesive (urethane-based adhesive) was applied to one surface of the outer layer substrate to form a first adhesive layer with a thickness of 3 μm (dry film thickness), and the outer layer substrate and the surface of the second sealant layer (outer sealant layer) opposite the printed layer were bonded together using the first adhesive layer. Subsequently, a dry laminating adhesive (urethane-based adhesive) was applied to the other surface of the outer layer substrate to form a second adhesive layer with a thickness of 3 μm (dry film thickness), and the sealant layer was bonded to the second adhesive layer to produce a packaging laminate (printed layer / second sealant layer (outer sealant layer) / first adhesive layer / outer layer substrate / second adhesive layer / sealant layer).

[0087] Reference Example 1 A petroleum-derived biaxially stretched PET film (thickness 25 μm) was prepared as the outer layer substrate, and a petroleum-derived LDPE film (thickness 60 μm) was prepared as the sealant layer. A printed layer was then formed on one surface of the outer layer substrate using an aqueous flexographic ink, a laminating adhesive (urethane adhesive) was applied to the surface of the printed surface to form an adhesive layer with a thickness of 3 μm (dry film thickness), and the sealant layer was attached to the adhesive layer to produce a packaging laminate (outer layer substrate / printed layer / adhesive layer / sealant layer).

[0088] <Recycled Resin Content> For the packaging laminates of the Examples, Comparative Examples, and Reference Examples produced as described above, the recycled resin content in the packaging laminate was calculated based on the following formula: Recycled Resin Content = 100 × Total Thickness of Layers Containing Recycled Resin / Overall Thickness of Packaging Laminate However, when the layer containing recycled resin is a layer containing recycled resin and a resin derived from petroleum or biomass, the value obtained by multiplying the thickness of this layer by the recycled resin content (% by mass) in that layer was used as the thickness of the layer containing recycled resin.

[0089] <Evaluation> The laminates for packaging materials of Examples, Comparative Examples, and Reference Examples prepared as described above were evaluated as follows: Evaluation 1 (generation of odorous components), Evaluation 2 (fisheyes), Evaluation 3 (impurities), and Evaluation 4 (variation in dynamic friction force). Here, Evaluation 1 is an evaluation regarding quality, and Evaluations 2 and 3 are evaluations regarding hygiene.

[0090] (1) Evaluation 1 (Odor Component Generation) First, the packaging laminate was analyzed using purge-and-trap gas chromatography mass spectrometry. Specifically, a 1.0 gram sample was cut from the packaging laminate, placed in a 20 mL vial with an odor component collector, and heated at 60°C for 1 hour to adsorb volatile components from the sample onto the collector. The volatile components in the collector were analyzed using a purge-and-trap gas chromatography mass spectrometer to obtain a total ion chromatogram. Next, in the total ion chromatogram obtained as above, the ratio R1 of the peak area of ​​nonanal to the sum of the peak areas of all aliphatic hydrocarbon components, and the ratio R2 of the peak area of ​​decanal to the sum of the peak areas of all aliphatic hydrocarbon components, both of which serve as indicators of odor components, were calculated. Evaluation was then performed based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation criteria) ⊚: R1 is less than 1.5% and R2 is less than 0.35% ◯: R1 is less than 1.5% and R2 is 0.35% or more, or R1 is 1.5% or more and R2 is less than 0.35% ×: R1 is 1.5% or more and R2 is 0.35% or more

[0091] (2) Evaluation 2 (Fisheyes) A ​​sample measuring 1 m x 1 m was cut out from the packaging laminate, and the sample was placed on a black table with the sealant layer facing up. Protrusions (protruding foreign matter) with a diameter of 0.5 mm or more but less than 1 mm were designated as fisheye 1 and the number N1 of these was counted visually, and protrusions (protruding foreign matter) with a diameter of 1 mm or more were designated as fisheye 2 and the number N2 of these was counted visually, and evaluation was performed based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation criteria) ⊚: N1 is 10 or less and N2 is 0 ○: N1 is 11 to 99 and N2 is 0 ×: N1 is 100 or more or N2 is 1 or more

[0092] (3) Evaluation 3 (Impurities) The packaging laminate was analyzed using a Fourier transform infrared spectrophotometer (FT-IR: Fourier Transform Infrared Spectroscopy) using attenuated total reflection (ATR) to obtain an ATR spectrum. At this time, a diamond prism was used as the prism to be brought into close contact with the packaging laminate, and the angle of incidence with respect to the surface of the packaging laminate was 45°. Then, in the ATR spectrum, a peak at 2915 cm originating from polyethylene was observed. -1 The absorption coefficient of the methylene group C-H inverse symmetric stretching near 1720 cm -1 The ratio R3 of the absorption coefficients of C=O stretching near the nucleus was calculated and evaluated based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation criteria) ⊚: R3 is less than 0.05 ◯: R3 is 0.05 or more but less than 0.1 ×: R3 is 0.1 or more

[0093] (4) Evaluation 4 (Variation in Dynamic Friction Force) The dynamic friction force of the packaging laminate was measured using a multi-function static and dynamic friction tester TL201Tt (manufactured by Trinity Lab Co., Ltd.) and a tactile probe. Specifically, the packaging laminate was placed on a test table with the sealant layer facing up, and the tactile probe was moved at a sliding speed of 10 mm / sec while being brought into contact with the packaging laminate (outer layer substrate side) with a load of 50 grams, and the standard deviation of the dynamic friction force was determined, and this standard deviation σ of the dynamic friction force was taken as the variation in the dynamic friction force. Evaluation was then performed based on the following evaluation criteria. The results are shown in Tables 1 to 3. (Evaluation Criteria) A...σ is less than 0.35 B...σ is 0.35 or more but less than 0.45 C...σ is 0.45 or more

[0094]

[0095] The results shown in Tables 1 to 3 show that in the packaging laminates of Examples 1 to 10, which used chemical recycled resin, almost no odorous components were generated and the amount of foreign matter and impurities was small, even when the recycled resin content was increased to 10% by volume or more or 10% by mass or more. In contrast, in the packaging laminates of Comparative Examples 1 to 5, which used material recycled resin, when the recycled resin content was increased to 10% by volume or more or 10% by mass or more, at least one of the following occurred: an increase in the amount of odorous components generated, an increase in the number of fisheyes, and an increase in the amount of impurities.

[0096] In the above examples and comparative examples, examples were shown in which the polyolefin resin was polyethylene, but even if polypropylene was used as the polyolefin resin, similar results would be obtained in terms of odor components, fish eyes, impurities, and dynamic friction coefficient due to the similarity in resin structure.

[0097] From the above, it was confirmed that the laminate for packaging materials of the present disclosure can improve hygiene and quality even when the content of recycled resin is sufficiently high.

[0098] 10...outer layer substrate, 20...intermediate substrate, 30...sealant layer, 60...gas barrier layer, 100...laminated body, 400...packaging bag (packaging container), 500...packaged article, C...contents

Claims

1. A laminate for packaging material comprising an outer layer base material and a sealant layer, wherein the sealant layer is a polyolefin resin film containing a recycled resin, the content of the recycled resin in the laminate for packaging material is 10% by volume or more or 10% by mass or more, and the recycled resin is a chemically recycled resin.

2. The packaging laminate according to claim 1, wherein the content of the recycled resin in the packaging laminate is 20% by volume or more or 20% by mass or more.

3. The packaging laminate according to claim 1, wherein the thickness of the sealant layer is greater than the thickness of the outer layer base material, and the content of the recycled resin in the sealant layer is 20% by volume or more or 20% by mass or more.

4. The packaging laminate according to claim 1, further comprising an intermediate substrate between the outer layer substrate and the sealant layer.

5. The packaging laminate according to claim 1, further comprising a gas barrier layer between the outer layer substrate and the sealant layer.

6. The packaging laminate according to claim 1, further comprising a second sealant layer on the surface of the outer layer substrate opposite to the sealant layer side.

7. A packaging container obtained by using the packaging laminate according to any one of claims 1 to 6.

8. A packaging article comprising the packaging container according to claim 7 and a content contained in the packaging container.

Citation Information

Patent Citations

  • Flexible pouches using post-consumer resins

    JP2022552096A

  • Vapor-deposited resin film, laminate including said vapor-deposited resin film, and packaging container including said laminate

    JP2022031795A

  • Polyolefin resin-based cross-linked foam and adhesive tape

    JP2023001768A

  • Laminate film, packaging bag and package

    JP2023031593A

  • Laminate, packaging material, and packaging container

    JP2023048882A

Cited By

  • Sealant film and packaging bags

    JP7885420B1