Heavy oil hydrorefining method

The sequential use of three hydrogenation catalysts with optimized pore structures and elemental compositions in the hydrorefining process enhances impurity removal and catalyst longevity, addressing the limitations of conventional methods by maintaining high activity and stability during hydrorefining of heavy oil.

WO2024228292A1PCT designated stage expired Publication Date: 2024-11-07ENEOS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/007816
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2024-03-01
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Conventional hydrorefining methods using hydrogenation catalysts fail to effectively remove impurities such as sulfur, metals, and asphaltenes from heavy oil due to inadequate consideration of reactivity and pore structure, leading to rapid catalyst deactivation and reduced catalyst life.

Method used

A method involving a sequential contact of heavy oil with three different hydrogenation catalysts in a downflow fixed bed reactor, where the first catalyst has macropores and mesopores with specific pore distributions, the second catalyst has a higher content of Group 6 elements, and the third catalyst has a bimodal pore structure, optimizing pore diameters and surface areas to enhance impurity removal and catalyst longevity.

Benefits of technology

This approach significantly improves the activity and longevity of the hydrogenation catalysts, allowing for stable operation at high temperatures for extended periods, increasing the production of light fractions from heavy oil and maintaining high demetalization and hydrodesulfurization performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024007816_07112024_PF_FP_ABST
    Figure JP2024007816_07112024_PF_FP_ABST
Patent Text Reader

Abstract

This heavy oil hydrorefining method involves a step for sequentially bringing heavy oil into contact with a first hydrogenation catalyst, a second hydrogenation catalyst, and a third hydrogenation catalyst, which are placed in a downflow-type fixed bed reactor, in the presence of hydrogen. Both the first hydrogenation catalyst and the second hydrogenation catalyst include macropores and mesopores. The pore distribution of the first hydrogenation catalyst has a peak at a pore diameter of 50 nm or more and a peak at a pore diameter of less than 50 nm. The pore distribution of the second hydrogenation catalyst also has a peak at a pore diameter of 50 nm or more and a peak at a pore diameter of less than 50 nm. The volume V1MACRO of the macropores in the first hydrogenation catalyst is larger than the volume V2MACRO of the macropores in the second hydrogenation catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Heavy oil hydrorefining method

[0001] The present disclosure relates to a method for hydrorefining heavy oil.

[0002] Heavy oils, such as petroleum residues (e.g., vacuum residues), are hydrotreated to reduce impurities (sulfur, metal, and asphaltene). Hydrotreatment involves contacting heavy oils with a hydrogenation catalyst at high temperature and pressure in the presence of hydrogen. Because heavy oils contain large amounts of metals and asphaltene, metals and coke deposit on the surface of the hydrogenation catalyst as hydrotreatment continues. As a result, the activity of the hydrogenation catalyst gradually declines, eventually leading to the end of its useful life due to limitations in the reactor and the properties of the resulting oil. Therefore, in heavy oil hydrotreatment, it is desirable to further improve the activity (impurity removal performance) of the hydrogenation catalyst and extend its useful life. To this end, while efforts are being made to improve the performance of the hydrogenation catalyst itself, methods are being adopted in which multiple hydrogenation catalysts with different roles tailored to the reactivity of each impurity in the heavy oil are combined. In particular, in order to protect the hydrodesulfurization catalyst, which serves as the main catalyst, it is important to remove metal components and asphaltene components from heavy oil using a demetalization catalyst placed in the stage preceding the hydrodesulfurization catalyst.

[0003] Patent Document 1 below discloses a hydrorefining method using multiple catalysts, in which heavy oil is sequentially contacted with an upstream catalyst, a middle catalyst, and a downstream catalyst in the presence of hydrogen. In the hydrorefining method described in Patent Document 1 below, the volume ratios of the upstream catalyst, the middle catalyst, and the downstream catalyst, which have different pore sizes, are adjusted within a specific numerical range. Then, reactive metal compounds among the metal components are removed by the upstream catalyst, less reactive metal compounds among the metal components are removed by the middle catalyst, and sulfur components are mainly removed by the downstream catalyst. Patent Document 2 below also discloses a hydrorefining method for heavy oil using an upstream catalyst, a middle catalyst, and a downstream catalyst. In the hydrorefining method described in Patent Document 2 below, the desulfurization activity of the downstream catalyst is enhanced by adding silicon and phosphorus to the downstream catalyst in particular.

[0004] The following Patent Documents 3 and 4 disclose hydrogenation catalysts that contain not only mesopores but also macropores that promote the diffusion of macromolecules as catalysts for reducing metal content and asphaltene content.

[0005] Japanese Patent Publication No. 2003-171671 Japanese Patent No. 6773384 Japanese Patent No. 4538014 Japanese Patent No. 4818163

[0006] However, the above-mentioned conventional hydrogenation catalysts do not perform satisfactorily because they are not designed with a focus on the reactivity of refractory metal compounds or asphaltene components. For example, the design of conventional hydrogenation catalysts does not take into account the molecular size and reactivity of the metal and asphaltene components, respectively. Therefore, conventional hydrogenation catalysts do not have optimal pore structures, i.e., the pore size and pore volume distribution (pore distribution). Therefore, conventional hydrotreating methods have difficulty sufficiently removing impurities (e.g., metal components and asphaltene components) from heavy oil that reduce the activity of hydrodesulfurization catalysts and achieving a long catalyst life. For example, increasing the reaction temperature of hydrotreating improves the activity of the hydrogenation catalyst for impurity removal. However, increasing the reaction temperature promotes the deposition of coke and other impurities, rapidly reducing the activity of the hydrogenation catalyst. Therefore, it is difficult to stably operate a hydrotreating unit using conventional hydrogenation catalysts at high reaction temperatures for extended periods of time. Furthermore, although the performance of each of the first-stage catalysts (demetalization catalysts), middle-stage catalysts, and second-stage catalysts (hydrodesulfurization catalysts) has improved, there are cases in which the performance of each catalyst is not fully demonstrated when multiple catalysts are combined. Also, since there is a greater demand for light fractions (kerosene, diesel, etc.) than for heavy oil, it is desirable to produce more light fractions from heavy oil through cracking reactions that occur simultaneously during hydrorefining of heavy oil and through reactions in a fluid catalytic cracking unit located downstream of the hydrorefining unit.

[0007] An object of one aspect of the present invention is to provide a method for hydrotreating heavy oil, in which a hydrogenation catalyst has excellent activity for removing impurities from heavy oil, and the activity of the hydrogenation catalyst is maintained for a long period of time.

[0008] One aspect of the present invention relates to a method for hydrotreating heavy oil according to any one of the following [1] to

[10] .

[0009] [1] A method for producing a heavy oil product, comprising a step of sequentially contacting a first hydrogenation catalyst, a second hydrogenation catalyst, and a third hydrogenation catalyst in the presence of hydrogen, wherein the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are installed in a downflow fixed bed reactor, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are different catalysts, both the first hydrogenation catalyst and the second hydrogenation catalyst contain macropores and mesopores, the pore diameter of the macropores is 50 nm or more, and the pore diameter of the mesopores is less than 50 nm, and the pore distribution of the first hydrogenation catalyst (a distribution obtained by plotting the pore volume against the logarithm of the pore diameter) has a peak where the pore volume is maximized at pore diameters of 50 nm or more, and a peak where the pore volume is maximized at pore diameters of less than 50 nm, The pore distribution of the second hydrogenation catalyst (a distribution obtained by plotting the pore volume against the logarithm of the pore diameter) has a peak where the pore volume is maximized for pore diameters of 50 nm or more and a peak where the pore volume is maximized for pore diameters of less than 50 nm, and the volume V1 of the macropores in the first hydrogenation catalyst MACRO is the volume V2 of the macropores in the second hydrogenation catalyst MACRO The specific surface area of ​​the first hydrogenation catalyst is 185 m 2 / g or more, and the specific surface area of ​​the second hydrogenation catalyst is 160 m 2 / g or more, and the content of Group 6 elements in the second hydrogenation catalyst is 5% by mass or more and 7% by mass or less.

[0010] [2] A method comprising a step of sequentially contacting heavy oil with a first hydrogenation catalyst, a second hydrogenation catalyst, and a third hydrogenation catalyst in the presence of hydrogen, wherein the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are installed in a downflow fixed bed reactor, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are different catalysts, both the first hydrogenation catalyst and the second hydrogenation catalyst contain macropores and mesopores, the pore diameter of the macropores is 50 nm or more, and the pore diameter of the mesopores is less than 50 nm, and the pore distribution of the first hydrogenation catalyst (a distribution obtained by plotting the pore volume against the logarithm of the pore diameter) has a peak where the pore volume is maximized for pore diameters of 50 nm or more, and a peak where the pore volume is maximized for pore diameters of less than 50 nm, The pore distribution of the second hydrogenation catalyst (a distribution obtained by plotting the pore volume against the logarithm of the pore diameter) has a peak where the pore volume is maximized for pore diameters of 50 nm or more and a peak where the pore volume is maximized for pore diameters of less than 50 nm, and the median pore diameter PD1 of the macropores in the first hydrogenation catalyst MACRO is the pore diameter at which the cumulative volume of macropores in the pore distribution of the first hydrogenation catalyst is 50% of the total volume of macropores, and PD2 is the median pore diameter of macropores in the second hydrogenation catalyst. MACRO is the pore diameter at which the cumulative volume of macropores in the pore distribution of the second hydrogenation catalyst is 50% of the total volume of macropores, and the median pore diameter PD1 MACRO is the median pore diameter PD2 MACRO The specific surface area of ​​the first hydrogenation catalyst is 185 m 2 / g or more, and the specific surface area of ​​the second hydrogenation catalyst is 160 m 2 / g or more, and the content of Group 6 elements in the second hydrogenation catalyst is 5% by mass or more and 7% by mass or less.

[0011] [3] Volume V1 of macropores in the first hydrogenation catalyst MACRO is the volume V2 of the macropores in the second hydrogenation catalyst MACRO The method for hydrotreating heavy oil according to [2], wherein the ρ is greater than or equal to 1.

[0012] [4] Median pore diameter PD1 MACROis 300 nm or more and 1500 nm or less, and the median pore diameter PD2 MACRO The method for hydrotreating heavy oil according to [2] or [3], wherein the average particle size is 100 nm or more and 500 nm or less.

[0013] [5] Volume V1 MACRO is 0.20 ml / g or more and 0.50 ml / g or less, and volume V2 MACRO The method for hydrotreating heavy oil according to [1] or [3], wherein the solubility of HCl is 0.10 ml / g or more and 0.35 ml / g or less.

[0014] [6] Volume V2 of mesopores in the second hydrogenation catalyst MESO is 0.50 ml / g or more and 0.90 ml / g or less, and the median pore diameter PD2 of the mesopores in the second hydrogenation catalyst is MESO is the pore diameter at which the cumulative volume of mesopores in the pore distribution of the second hydrogenation catalyst is 50% of the total volume of mesopores, and the median pore diameter PD2 MESO The method for hydrotreating heavy oil according to any one of [1] to [5], wherein the average particle size is 6 nm or more and 20 nm or less.

[0015] [7] The method for hydrotreating heavy oil according to any one of [1] to [6], wherein the macropore distribution among the pore distributions of each of the first hydrogenation catalyst and the second hydrogenation catalyst is measured by mercury intrusion porosimetry, and the mesopore distribution among the pore distributions of each of the first hydrogenation catalyst and the second hydrogenation catalyst is measured by nitrogen adsorption.

[0016] [8] The method for hydrotreating heavy oil according to any one of [1] to [7], wherein the content of Group 8 to 10 elements in the second hydrogenation catalyst is 1.0% by mass or more and 3.0% by mass or less, and the content of phosphorus in the second hydrogenation catalyst is 0.1% by mass or more and 2.0% by mass or less.

[0017] [9] The method for hydrotreating heavy oil according to any one of [1] to [8], wherein the contents of the Group 6 elements and Groups 8 to 10 elements in the second hydrogenation catalyst are greater than the contents of the Group 6 elements and Groups 8 to 10 elements in the first hydrogenation catalyst, and the units of the contents are % by mass.

[0018]

[10] The method for hydrotreating heavy oil according to any one of [1] to [9], wherein the volume of the first hydrogenation catalyst is represented as Vc1, the volume of the second hydrogenation catalyst is represented as Vc2, the volume of the third hydrogenation catalyst is represented as Vc3, (Vc1 + Vc2) / (Vc1 + Vc2 + Vc3) is 40 vol% or more and 70 vol% or less, and (Vc2 + Vc3) / (Vc1 + Vc2 + Vc3) is 60 vol% or more and 95 vol% or less.

[0019] According to one aspect of the present invention, there is provided a method for hydrotreating heavy oil, in which a hydrogenation catalyst has excellent activity for removing impurities from heavy oil, and the activity of the hydrogenation catalyst is maintained for a long period of time.

[0020] FIG. 1(a) shows a schematic example of the pore distribution of the first hydrogenation catalyst, and FIG. 1(b) shows a schematic example of the pore distribution of the second hydrogenation catalyst.

[0021] [Method for Hydrotreating Heavy Oil] The inventors discovered that the balance between pore size and pore volume in the macropore region (pore diameter region of 50 nm or more) of the pore distribution of a hydrogenation catalyst is extremely important for the removal of metals and asphaltene from heavy oil. Macropores essentially provide a reaction path for recalcitrant macromolecules contained in heavy oil. Examples of recalcitrant macromolecules include molecules (supermolecules) that diffuse in an associated state, such as asphaltene, and bulky metal porphyrin molecules (porphyrin compounds containing vanadium or nickel). However, in conventional hydrogenation catalysts (such as desulfurization catalysts) that do not contain macropores, these macromolecules have difficulty diffusing from the surface to the interior of the catalyst particles. Therefore, the vicinity of the catalyst particle surface contributes significantly to the hydrogenation reaction of the macromolecules. As a result, the deposition of carbonaceous matter (coke) and metals near the surface of the catalyst particles is promoted, which easily causes pore blockage (mouthplugging) near the outer surface of the catalyst particles and significantly impairs catalytic performance.

[0022] In contrast, macropore-containing hydrodesulfurization catalysts allow macromolecules to easily diffuse from the surface to the interior of the catalyst particles. This suppresses the deposition of carbonaceous and metallic components near the surface of the catalyst particles, and also suppresses mouthplugging near the outer surface of the catalyst particles. As a result, the effective surface area of ​​the catalyst utilized for removing impurities from heavy oil increases, and the effective volume of mesopores utilized as reaction sites for macromolecules that have diffused into the catalyst particles also increases. Furthermore, suppressing mouthplugging on the surface of the catalyst particles alleviates the activity decline (rapid decline in activity at the later stage of the reaction) that is characteristic of hydrodesulfurization catalysts for heavy oil, significantly extending the life of the hydrodesulfurization catalyst.

[0023] On the other hand, the introduction of macropores into the hydrogenation catalyst reduces the bulk density of the hydrogenation catalyst, resulting in a decrease in the mass of the hydrogenation catalyst that can be packed into a reactor (hydrorefining apparatus). This means a decrease in the initial activity of the entire reactor. Even if the introduction of macropores increases the catalyst surface and reaction field that can be effectively utilized, and even if deterioration of the hydrogenation catalyst is significantly reduced, the decrease in the initial activity of the entire reactor creates a constraint that requires the reactor temperature to be high from the start of reactor operation.

[0024] The decrease in the initial activity of the entire reactor naturally depends greatly on the volume of macropores introduced into the hydrogenation catalyst. That is, if the volume of the macropores is too large, the deterioration of each catalyst particle is suppressed, but the bulk density of the hydrogenation catalyst decreases, reducing the mass of hydrogenation catalyst that can be packed into the reactor and decreasing the initial activity of the entire reactor. On the other hand, if the volume of the macropores is too small, the above-mentioned effects due to the macropores become smaller, and the difference in performance between a hydrogenation catalyst containing macropores and a conventional hydrogenation catalyst that does not contain macropores becomes smaller. From the above perspectives, there is an optimal value for the volume of macropores in the hydrogenation catalyst.

[0025] Among the impurities in heavy oil, relatively reactive metal compounds are easily removed from the heavy oil by the demetalization reaction in a hydrogenation catalyst (demetalization catalyst) installed near the inlet of the reactor, regardless of the pore structure of the hydrogenation catalyst. On the other hand, among the impurities in heavy oil, relatively unreactive metal compounds are difficult to remove by the demetalization catalyst and tend to remain in the heavy oil. When unreactive metal compounds are directly introduced into a hydrodesulfurization catalyst installed downstream of the demetalization catalyst, the high hydrogenation activity of the hydrodesulfurization catalyst and the small pore diameter of the hydrodesulfurization catalyst tend to lead to the generation and deposition of metals derived from carbonaceous and metal components, as well as pore blockage, on the surface of the hydrodesulfurization catalyst. As a result, the activity of the hydrodesulfurization catalyst rapidly decreases. Therefore, the middle-stage catalyst, which is installed between the upstream catalyst (demetalization catalyst) and the downstream catalyst (hydrodesulfurization catalyst), is required to have a pore structure that can introduce and diffuse various impurities in heavy oil into the catalyst, and hydrogenation activity (desulfurization activity) that the upstream catalyst does not have. In this embodiment, the upstream catalyst corresponds to the first hydrogenation catalyst, the middle catalyst corresponds to the second hydrogenation catalyst, and the downstream catalyst corresponds to the third hydrogenation catalyst.

[0026] As a result of research based on the above considerations, the inventors have found that the volume V1 of the macropores in the first hydrogenation catalyst MACRO The optimum value of is 0.20 ml / g or more and 0.50 ml / g or less, and the volume V2 of the macropores in the second hydrogenation catalyst MACRO It was found that the optimum value of the volume V1 of the macropores in the first hydrogenation catalyst is 0.10 ml / g or more and 0.35 ml / g or less. MACRO is the volume V2 of the macropores in the second hydrogenation catalyst MACR By combining the first hydrogenation catalyst and the second hydrogenation catalyst that satisfy the above conditions, the initial activity of the entire reactor is unlikely to be impaired in the hydrorefining of various heavy oils under various reaction conditions, the pores (e.g., mesopores) inside each catalyst are likely to be utilized to remove impurities introduced via macropores, deterioration of each of the first to third hydrogenation catalysts is alleviated, and the demetalization reaction is likely to be maintained for a long period of time.

[0027] Furthermore, when considering the function of macropores as reaction paths, there is naturally an optimal pore size for macropores. The larger the molecular weight, the larger the molecular size. When the molecules in heavy oil have a developed polycyclic structure or contain a large amount of polar molecules, the size of the associated molecules composed of these molecules becomes larger. The poorer the compatibility between heavy oil and impurities, the larger the size of the particles (apparent molecules) formed by the aggregation of impurities. The larger the apparent molecular size during diffusion, the larger the pore size required as a reaction path. For macropores to function as reaction paths, it is desirable for the pore diameter of the macropore to be approximately 5 to 10 times or more the size of the diffusing molecules. As a result of the inventors' research on the actual reactivity of heavy oil obtained from various crude oils, it was found that the reactivity and diffusibility of impurities in heavy oil vary significantly depending on the type (origin) of crude oil or the blending state of the crude oil. (The diffusibility of impurities is estimated from the deposition profile of metal components in the cross section of a hydrogenation catalyst particle.) In other words, it was found that various impurities with different molecular sizes at the time of diffusion exist in heavy oil depending on the type of crude oil or the blending state of the crude oil.

[0028] As a result of research based on the above considerations regarding the apparent molecular size during diffusion, the inventors have determined that the median pore diameter PD1 of the macropores in the first hydrogenation catalyst MACRO is 300 nm or more and 1500 nm or less (preferably 300 nm or more and 1000 nm or less, and more preferably 500 nm or more and 1000 nm or less). When the median pore diameter of the macropores in the first hydrogenation catalyst is within the above range, in the hydrorefining of various heavy oils under various reaction conditions, the initial activity of the entire reactor (hydrorefining apparatus) is unlikely to be impaired, the pores (e.g., mesopores) in the first hydrogenation catalyst are likely to be utilized for removing impurities introduced via the macropores, deterioration of each of the first to third hydrogenation catalysts is mitigated, and the demetalization reaction is likely to be maintained for a long period of time.

[0029] After heavy oil comes into contact with the first hydrogenation catalyst installed near the inlet of the reactor, the molecular size of impurities in the heavy oil decreases during diffusion due to various hydrogenation reactions in the first hydrogenation catalyst. Therefore, in the second hydrogenation catalyst installed downstream (later stage) of the first hydrogenation catalyst, the pore diameter of the macropores required for molecular diffusion into the catalyst can be made smaller than the macropore diameter in the first hydrogenation catalyst. In other words, by combining a first hydrogenation catalyst with a large macropore diameter and a second hydrogenation catalyst with a small macropore diameter, the total volume of the macropores occupying the space in the reactor as reaction paths is significantly reduced, and the catalytic activity per unit volume of the first hydrogenation catalyst and the second hydrogenation catalyst as a whole is significantly improved. As a result of research into the pore diameter of the macropores in the second hydrogenation catalyst, the inventors have found that the median pore diameter PD2 of the macropores in the second hydrogenation catalyst is 0.05 mm. MACRO It has been found that the optimum value of is 100 nm or more and 500 nm or less (preferably 150 nm or more and 350 nm or less, and more preferably 200 nm or more and 250 nm or less).

[0030] As a result of the above-mentioned considerations and research, the inventors have completed the present invention. Preferred embodiments of the present invention will be described below with reference to the drawings. The present invention is not limited to the following embodiments.

[0031] The method for hydrotreating heavy oil according to this embodiment includes a step of sequentially contacting heavy oil with a first hydrogenation catalyst (first-stage catalyst), a second hydrogenation catalyst (middle-stage catalyst), and a third hydrogenation catalyst (last-stage catalyst) in the presence of hydrogen. That is, the heavy oil contacts the first hydrogenation catalyst, the heavy oil after contacting the first hydrogenation catalyst contacts the second hydrogenation catalyst, and the heavy oil after contacting the second hydrogenation catalyst contacts the third hydrogenation catalyst. The first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are installed (packed) in a downflow fixed-bed reactor. For example, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst may all be packed as three catalyst layers in a single downflow fixed-bed reactor. For example, the first hydrogenation catalyst may be packed in a first downflow fixed bed reactor, the second hydrogenation catalyst may be packed in a second downflow fixed bed reactor, the third hydrogenation catalyst may be packed in a third downflow fixed bed reactor, the first downflow fixed bed reactor may be disposed upstream of the second downflow fixed bed reactor, and the second downflow fixed bed reactor may be disposed upstream of the third downflow fixed bed reactor.

[0032] The first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are different catalysts (compositions). The first hydrogenation catalyst is a catalyst (demetalization catalyst) with excellent demetalization activity. The second hydrogenation catalyst is a catalyst with not only demetalization activity but also excellent hydrodesulfurization activity. The third hydrogenation catalyst is a catalyst (hydrodesulfurization catalyst) with excellent hydrodesulfurization activity. Due to the hydrogenation activity (hydrocracking activity) of each hydrogenation catalyst, hydrocracking of heavy oil and asphaltene occurs, producing light fractions and carbonaceous components with low molecular weights. Due to the demetalization activity of each of the first hydrogenation catalyst and the second hydrogenation catalyst, metal components in the heavy oil (e.g., organometallic compounds containing vanadium, nickel, etc.) are decomposed and removed from the heavy oil. Metals produced by the decomposition of the metal components deposit on the surfaces of the first hydrogenation catalyst and the second hydrogenation catalyst, respectively, or accumulate in the pores of the first hydrogenation catalyst and the second hydrogenation catalyst, respectively. Due to the hydrodesulfurization activity of each of the second hydrogenation catalyst and the third hydrogenation catalyst, the sulfur content in the heavy oil is hydrogenated and removed from the heavy oil as hydrogen sulfide.

[0033] 1A is a schematic pore distribution of the first hydrogenation catalyst. 1B is a schematic pore distribution of the second hydrogenation catalyst. The vertical axis of the pore distribution represents the pore volume, and the horizontal axis of the actual pore distribution represents the logarithm of the pore diameter D (log 10 D). However, in Figure 1 (a) and Figure 1 (b), in order to make it easier to visually recognize the position and size of each peak in each pore distribution and the differences therebetween, the pore diameter D itself is displayed on the horizontal axis instead of the logarithm of the pore diameter D. That is, in Figure 1 (a) and Figure 1 (b), each pore distribution is simplified in order to emphasize the characteristics of each pore distribution. The mock pore distribution of the first hydrogenation catalyst is not limited to the pore distribution shown in Figure 1 (a). The mock pore distribution of the second hydrogenation catalyst is not limited to the pore distribution shown in Figure 1 (b).

[0034] As shown in (a) of Figure 1, the horizontal axis of the pore distribution of the first hydrogenation catalyst indicates the pore size (unit: nm) of the pores in the first hydrogenation catalyst. The vertical axis of the pore distribution of the first hydrogenation catalyst indicates the volume (unit: ml / g) of the pores in the first hydrogenation catalyst. The g in ml / g corresponds to the unit mass of the first hydrogenation catalyst. As shown in (b) of Figure 1, the horizontal axis of the pore distribution of the second hydrogenation catalyst indicates the pore size (unit: nm) of the pores in the second hydrogenation catalyst. The vertical axis of the pore distribution of the second hydrogenation catalyst indicates the volume (unit: ml / g) of the pores in the first hydrogenation catalyst. The g in ml / g corresponds to the unit mass of the second hydrogenation catalyst.

[0035] Both the first hydrogenation catalyst and the second hydrogenation catalyst contain macropores and mesopores. Macropores are pores with a pore diameter of 50 nm or more. For example, the pore diameter of macropores may be 50 nm or more and 3000 nm or less. Mesopores are pores with a pore diameter of less than 50 nm. For example, the pore diameter of mesopores may be 2 nm or more and less than 50 nm. Mercury porosimetry is superior to nitrogen adsorption porosimetry in terms of resolution for measuring pore diameters around 50 nm. In other words, measuring pore diameters around 50 nm using nitrogen adsorption is not appropriate in terms of measurement accuracy. Therefore, the macropore distribution in the pore distributions of each of the first hydrogenation catalyst and the second hydrogenation catalyst may be measured by mercury porosimetry. Nitrogen adsorption is superior to mercury porosimetry in terms of resolution for measuring pore diameters less than 50 nm. Therefore, the mesopore distribution in the pore distribution of each of the first hydrogenation catalyst and the second hydrogenation catalyst may be measured by a nitrogen adsorption method.

[0036] As shown in (a) of Figure 1, the pore distribution of the first hydrogenation catalyst (actually, a distribution obtained by plotting pore volume against the logarithm of pore diameter) has a peak where the pore volume is maximized for pore diameters of 50 nm or more, and a peak where the pore volume is maximized for pore diameters of less than 50 nm. As shown in (b) of Figure 1, the pore distribution of the second hydrogenation catalyst (actually, a distribution obtained by plotting pore volume against the logarithm of pore diameter) also has a peak where the pore volume is maximized for pore diameters of 50 nm or more, and a peak where the pore volume is maximized for pore diameters of less than 50 nm. In other words, both the first hydrogenation catalyst and the second hydrogenation catalyst are bimodal catalysts. A bimodal catalyst is a catalyst whose pore distribution has at least two peaks (peaks where the pore volume is maximized).

[0037] In one aspect of this embodiment, the hydrorefining method for heavy oil is characterized in that the volume V1 of the macropores in the first hydrogenation catalyst is MACRO (unit: ml / g) is the volume V2 of the macropores in the second hydrogenation catalyst MACRO (unit: ml / g) is larger than the volume V1 MACRO may be 0.20 ml / g or more and 0.50 ml / g or less, and the volume V2 MACRO The volume V1 may be 0.10 ml / g or more and 0.35 ml / g or less. MACRO can be expressed as the sum of the volumes of all macropores in the first hydrogenation catalyst. MACRO can be translated into the sum of the volumes of all macropores in the second hydrogenation catalyst.

[0038] In another aspect of this embodiment, the method for hydrotreating heavy oil further comprises: MACRO (unit: nm) is the median pore diameter PD2 of the macropores in the second hydrogenation catalyst MACRO (unit: nm) is larger than the median pore diameter PD1 MACRO may be 300 nm or more and 1500 nm or less, and the median pore diameter PD2 MACRO The median pore diameter PD1 of the macropores in the first hydrogenation catalyst may be 100 nm or more and 500 nm or less. MACROis the pore size at which the cumulative volume of macropores in the pore distribution of the first hydrogenation catalyst is 50% of the total volume of macropores. MACRO The pore size is a pore size at which the cumulative volume of macropores in the pore distribution of the second hydrogenation catalyst is 50% of the total volume of macropores.

[0039] The heavy oil hydrotreating method according to this embodiment may have both of the above-mentioned Technical Features 1 and 2. The heavy oil hydrotreating method according to this embodiment may have only Technical Feature 1 of the above-mentioned Technical Features 1 and 2. The heavy oil hydrotreating method according to this embodiment may have only Technical Feature 2 of the above-mentioned Technical Features 1 and 2. The above-mentioned Technical Features 1 and 2 can be summarized as a combination of a bimodal second hydrogenation catalyst (middle-stage catalyst) containing small macropores and mesopores and a bimodal first hydrogenation catalyst (front-stage catalyst) containing large macropores and mesopores. Due to the combination of the first and second hydrogenation catalysts, even if a hydrotreating unit (reactor) equipped with the first, second, and third hydrogenation catalysts is operated at a higher temperature than conventional systems, the overall hydrocracking performance, demetalization performance, and hydrodesulfurization performance of the hydrotreating unit are unlikely to deteriorate, and the hydrotreating unit can be operated stably at high temperatures for a long period of time. For example, according to this embodiment, the operation of the hydrotreating unit can be continued for 250 days or more, particularly 300 days or more. That is, according to this embodiment, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst each have excellent activity for removing impurities from heavy oil, and the activity of each hydrogenation catalyst is maintained for a long period of time. As a result, the performance of the hydrotreating unit as a whole in removing impurities (especially metal components) is improved, the cracking rate of heavy oil is increased, and a larger amount of light fraction can be produced from heavy oil than before.

[0040] The volume of the first hydrogenation catalyst is expressed as Vc1 (unit: e.g., liters). For example, Vc1 may be the volume of the first catalytic layer made of the first hydrogenation catalyst. The volume of the second hydrogenation catalyst is expressed as Vc2 (unit: e.g., liters). For example, Vc2 may be the volume of the second catalytic layer made of the second hydrogenation catalyst. The volume of the third hydrogenation catalyst is expressed as Vc3 (unit: e.g., liters). For example, Vc3 may be the volume of the third catalytic layer made of the third hydrogenation catalyst. (Vc1 + Vc2) / (Vc1 + Vc2 + Vc3) may be 40 vol% or more and 70 vol% or less, preferably 50 vol% or more and 70 vol% or less, and more preferably 60 vol% or more and 70 vol% or less. (Vc2 + Vc3) / (Vc1 + Vc2 + Vc3) may be 60 vol% or more and 95 vol% or less, preferably 70 vol% or more and 90 vol% or less. When (Vc1 + Vc2) / (Vc1 + Vc2 + Vc3) and (Vc2 + Vc3) / (Vc1 + Vc2 + Vc3) are each within the above ranges, the performance of the hydrotreating apparatus as a whole to remove impurities (particularly metal components) is likely to improve, and the performance of the hydrotreating apparatus as a whole to remove impurities is likely to be maintained over a long period of time.

[0041] For example, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst may be housed as three catalyst layers in the same reactor (e.g., a reaction tower). The first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst may be housed in different reactors. Hydrogen (hydrogen gas) may be injected into each hydrogenation catalyst (each catalyst layer). Before the heavy oil contacts the first hydrogenation catalyst, hydrorefining of the heavy oil may be performed using another catalyst. After the heavy oil contacts the third hydrogenation catalyst, hydrorefining or fluid catalytic cracking of the heavy oil may be performed using another catalyst. The first catalyst layer containing the first hydrogenation catalyst may further contain one or more other catalysts other than the second hydrogenation catalyst and the third hydrogenation catalyst. For example, the other catalysts are catalysts that do not function sufficiently as catalysts for hydrorefining, such as so-called guard catalysts and support catalysts. Similarly, the second catalyst layer containing the second hydrogenation catalyst may further contain one or more other catalysts other than the first hydrogenation catalyst and the third hydrogenation catalyst. The third catalyst layer containing the third hydrogenation catalyst may further contain one or more other catalysts other than the first hydrogenation catalyst and the second hydrogenation catalyst. When each of the catalyst layers containing the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst further contains the other catalyst, Vc1, Vc2, and Vc3 are volumes excluding the other catalysts.

[0042] [First Hydrogenation Catalyst] The first hydrogenation catalyst (pre-stage catalyst), which the heavy oil first comes into contact with, needs to remove a large amount of relatively reactive macromolecules from the metal components and asphaltene components. Therefore, the pore structure of the first hydrogenation catalyst is extremely important for promoting the diffusion of macromolecules into the first hydrogenation catalyst. In addition, if the activity of the first hydrogenation catalyst is too high, the generation and deposition of metals due to hydrocracking of the metal components is likely to be promoted at the entrances of the pores opening on the surface of the first hydrogenation catalyst, which makes the first hydrogenation catalyst prone to deactivation. To prevent such deactivation, it is desirable that the content of active metals in the first hydrogenation catalyst is low.

[0043] Volume V1 of mesopores in the first hydrogenation catalyst MESO The volume V1 may be 0.4 ml / g or more and 1.1 ml / g or less, preferably 0.6 ml / g or more and 1.1 ml / g or less. MESOcan be expressed as the sum of the volumes of all mesopores in the first hydrogenation catalyst. MESO When the median pore diameter PD1 of the mesopores in the first hydrogenation catalyst is 0.4 ml / g or more, it is easy to suppress a decrease in the demetalization activity due to metal deposition on the surface of the first hydrogenation catalyst. MESO The median pore diameter PD1 may be 6 nm or more and 20 nm or less, preferably 8 nm or more and 15 nm or less. MESO is the pore size at which the cumulative volume of mesopores in the pore distribution of the first hydrogenation catalyst is 50% of the total volume of mesopores. 2 / g or more 350m 2 / g or less, preferably 190m 2 / g or more 350m 2 / g or less. Demetalization catalysts that can be industrially used as the first hydrogenation catalyst have limitations on their specific surface area and pore volume due to their target performance. This is because the specific surface area of ​​a catalyst is positively correlated with the catalytic reaction active sites, and the pore diameter and pore volume affect the mass transfer of reactants (heavy oil molecules). On the other hand, a trade-off exists in the characteristics of catalysts, whereby the specific surface area decreases when the pore diameter and pore volume are enlarged in an attempt to promote the mass transfer of reactants (heavy oil molecules). In order to ensure the desired performance of a demetalization catalyst, it is necessary to employ a catalyst with a high specific surface area. On the other hand, in order to maintain the minimum pore diameter and pore volume, limitations also arise on the specific surface area, resulting in the existence of an upper limit. As a result of research and investigation by the inventors, the specific surface area of ​​a first hydrogenation catalyst (demetalization catalyst) exhibiting high performance is 185 m 2 / g or more 350m 2 / g or less, preferably 190m 2 / g or more 300m 2 / g or less. 2 If the saturation rate is less than 1 / g, the first hydrogenation catalyst cannot exhibit sufficient performance, and the performance of the entire catalyst system consisting of the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst is impaired, which is undesirable.

[0044] Volume V1 of macropores in the first hydrogenation catalyst MACROThe volume V1 may be 0.20 ml / g or more and 0.50 ml / g or less, preferably 0.25 ml / g or more and 0.45 ml / g or less. MACRO When the volume V1 is 0.20 ml / g or more, the demetalization activity of the first hydrogenation catalyst is improved. MACRO When the median pore diameter PD1 of the macropores in the first hydrogenation catalyst is 0.50 ml / g or less, the mechanical strength of the first hydrogenation catalyst is improved. The total volume of pores having a pore diameter of 2000 nm or more in the first hydrogenation catalyst may be 0.1 ml / g or less, preferably 0.05 ml / g or less. When the total volume of pores having a pore diameter of 2000 nm or more is 0.1 ml / g or less, the mechanical strength of the first hydrogenation catalyst is improved. MACRO may be 300 nm or more and 1500 nm or less, preferably 300 nm or more and 1000 nm or less, and more preferably 500 nm or more and 1000 nm or less.

[0045] The first hydrogenation catalyst includes a porous support made of an inorganic oxide. All of the pore-related characteristics in the first hydrogenation catalyst described above originate from the porous support. In other words, the pores in the first hydrogenation catalyst described above reflect the characteristics of the pores in the porous support constituting the first hydrogenation catalyst. The "first support" described below refers to the porous support constituting the first hydrogenation catalyst. The first support may be an oxide of one or more elements selected from the group consisting of Group 2 elements, Group 4 elements, Group 13 elements, and Group 14 elements. For example, the first support preferably includes one or more oxides selected from the group consisting of silica, alumina, magnesia, zirconia, boria, and calcia. More preferably, the first support includes one or more oxides selected from the group consisting of γ-alumina, δ-alumina, η-alumina, χ-alumina, silica-alumina, silica, alumina-magnesia, silica-magnesia, and alumina-silica-magnesia. It is particularly preferred that the first support be γ-alumina. Alumina (Al 2 O 3 The content of ) may be 50% by mass or more, preferably 70% by mass or more.

[0046] The first hydrogenation catalyst may contain one or more metals selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements as a metal component (metal component having hydrogenation activity) supported on the first support. For example, the first hydrogenation catalyst may preferably contain at least one of molybdenum and tungsten. The first hydrogenation catalyst may further contain at least one of nickel and cobalt in addition to at least one of molybdenum and tungsten. The metal component supported on the first support may be a metal, oxide, or sulfide. The total content of the Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements in the first hydrogenation catalyst may be 0.1% by mass or more and 10% by mass or less, preferably 0.5% by mass or less and 6% by mass or less, more preferably 1% by mass or more and 5% by mass or less. The first hydrogenation catalyst may further contain a compound (e.g., an oxide) containing at least one of phosphorus and boron. The total content of phosphorus and boron in the first hydrogenation catalyst may be 0% by mass or more and 3% by mass or less, preferably 0.1% by mass or more and 1% by mass or less. When the contents of each element in the first hydrogenation catalyst are within the above ranges, the demetalization activity of the first hydrogenation catalyst is improved, and excessive hydrocracking reaction on the surface of the first hydrogenation catalyst is likely to be suppressed, thereby making it possible to suppress deactivation of the first hydrogenation catalyst.

[0047] An example of a method for producing the first hydrogenation catalyst will be described below.

[0048] The raw material for the first support is a raw material powder containing alumina such as γ-alumina (including hydrous alumina) or pseudo-boehmite as a main component. The raw material powder may further contain the oxides described above in addition to γ-alumina or pseudo-boehmite. The raw material powder is mixed and kneaded with a liquid, a molding aid, etc. to obtain a kneaded material (dough) having the desired moisture content, hardness, and viscosity. The kneaded material is extrusion-molded to form a molded body. The molded body is dried with hot air or the like to reduce the moisture content to an appropriate level, and then fired to obtain the first support. The content of γ-alumina (excluding adsorbed water) or pseudo-boehmite (excluding water of crystallization and adsorbed water) in the raw material powder may be 60% by mass or more and 100% by mass or less, preferably 75% by mass or more and 100% by mass or less.

[0049] The total volume of mesopores in the raw material powder may be 0.6 ml / g or more, preferably 0.8 ml / g or more. The pore size distribution of mesopores in the raw material powder may be measured by a nitrogen adsorption method. When the total volume of mesopores in the raw material powder is less than 0.6 ml / g, the volume V1 of mesopores in the first hydrogenation catalyst may be 0.6 ml / g or more. MESO Therefore, the effective amount of metal deposition in the first hydrogenation catalyst is reduced. The average particle size (median diameter) of the raw material powder may be preferably 10 μm or more and 300 μm or less, and more preferably 10 μm or more and 100 μm or less. The average particle size of the raw material powder may be measured by a general wet laser light scattering method. When the average particle size of the raw material powder is less than 10 μm, the volume V1 of the macropores in the first hydrogenation catalyst is MACRO If the average particle size of the raw material powder exceeds 300 μm, the volume of pores having a pore size of 2000 nm or more in the first hydrogenation catalyst increases, resulting in a decrease in the mechanical strength of the first hydrogenation catalyst.

[0050] The γ-alumina is preferably γ-alumina obtained by calcining pseudo-boehmite at 450°C or higher and 850°C or lower. A used catalyst (e.g., a hydrogenation catalyst in which a metal component is supported on γ-alumina) may be used as a raw material for γ-alumina. The average particle size of the raw material powder may be adjusted to a desired value by pulverizing the raw material powder using a ball mill, roller mill, jet mill, pulverizer, or the like. The pore distribution of the first support can be controlled by the average particle size of the raw material powder.

[0051] The method for forming the raw material powder is not particularly limited. For example, a paste or clay containing the raw material powder and a liquid (water or an organic solvent) may be formed. For example, the forming means may be extrusion molding, pressure molding, or application to a processing sheet. A carrier having a desired shape and dimensions can be obtained by drying or firing the formed raw material powder. The raw material powder may be formed into a spherical shape by dispersing a gel-like or slurry-like raw material powder in a gas using a spray dryer or the like and drying it. The raw material powder in a sol-like or slurry-like state may be formed into a spherical shape in a liquid. If necessary, a forming aid may be added to the raw material powder. A tablet made of the raw material powder may be formed by pressure molding using a tablet machine. The raw material powder may be granulated by rolling granulation.

[0052] When the raw material powder and the liquid are mixed, the raw material powder and the liquid may be mixed and kneaded using a general mixer or kneader used in catalyst preparation. Preferably, the raw material powder and water may be mixed using a stirring blade. Instead of water, an organic solvent such as an alcohol or a ketone may be used as the liquid to be mixed with the raw material powder. The raw material powder may be mixed with one or more additives such as an acid such as nitric acid, acetic acid, or formic acid, a base such as ammonia, an organic compound (molding aid) such as water-soluble cellulose ether, a surfactant, and an active ingredient. Preferably, a molding aid such as water-soluble cellulose ether may be mixed with the raw material powder. The pore distribution of the first support can be controlled by the concentration of these additives, the mixing and kneading conditions, the firing temperature, etc.

[0053] To achieve the above-described characteristics regarding the macropores in the first carrier, it is important to balance the appropriate moisture content and the amount of molding aid added in the process of mixing and kneading the raw material powder, water, and molding aid. The moisture content of the raw material mixture (referred to as "dough") containing the raw material powder, water, and molding aid may be preferably 53.0 mass% or more and 60.0 mass% or less, more preferably 54.0 mass% or more and 58.0 mass% or less. The mass ratio of the molding aid added to the raw material powder may be preferably 0.5 mass% or more and 5 mass% or less, more preferably 1.0 mass% or more and 3.0 mass% or less, per 100 mass parts of raw material powder.

[0054] A pellet-shaped or honeycomb-shaped compact may be formed from the raw material mixture using a molding device such as a plunger extruder or a screw extruder. The compact may be dried at room temperature or higher and 150°C or lower, preferably 100°C or higher and 140°C or lower. The dried compact may be calcined at 350°C or higher and 900°C or lower, preferably 450°C or higher and 850°C or lower, for 0.5 hours or higher and 5 hours or lower. A first support may be obtained.

[0055] For example, the shape of the first carrier may be a sphere, a cylinder, a cylindrical column, a prism, or a columnar body having a trefoil or tetrafoil cross section. For example, the maximum diameter of the cross section of the first carrier (a cross section perpendicular to the length direction in the case of a columnar or cylindrical body) may be 0.5 mm or more and 6 mm or less. For example, the length of the first carrier may be adjusted as desired, taking into account ease of handling.

[0056] The first hydrogenation catalyst can be obtained by supporting the above-described metal component (metal component having hydrogenation activity) on the first support. For example, methods for supporting the metal component on the first support include impregnation, pore-filling, thermal impregnation, vacuum impregnation, and immersion. For example, the first support impregnated with the metal component may be dried at 80°C to 200°C for 10 minutes to 24 hours. The dried first support may be calcined at 400°C to 600°C, preferably 450°C to 550°C, for 15 minutes to 10 hours, thereby supporting the metal component on the first support. The metal component may be added to the above-described raw material powder during the production process of the first support. For example, the metal component may be added to γ-alumina or pseudo-boehmite in advance. The metal component may be added to the raw material powder or raw material mixture during the process of mixing and kneading the raw material powder. That is, the metal component may be kneaded into the raw material powder in advance. The metal component may be added to the raw material powder or the raw material mixture at the time of molding the raw material powder or the raw material mixture. The metal component may be supported on the molded body during drying of the molded body or before firing. For example, when a used hydrogenation catalyst is used as part of the raw material powder, the raw material powder may already contain at least a part of the metal component.

[0057] [Second Hydrogenation Catalyst] Except for the matters described below, the second hydrogenation catalyst and the method for producing the same may be the same as the first hydrogenation catalyst and the method for producing the same described above.

[0058] The second hydrogenation catalyst (middle stage catalyst) installed downstream of the first hydrogenation catalyst removes impurities (comparatively less reactive components of metal components and asphaltene components) that are difficult to remove with the first hydrogenation catalyst. For this purpose, it is desirable that the content of metal components (metal components having hydrogenation activity) in the second hydrogenation catalyst be greater than the content of metal components (metal components having hydrogenation activity) in the first hydrogenation catalyst. As described above, macromolecules among impurities are easily removed by the macropores in the first hydrogenation catalyst, so the volume V2 of the macropores (pores for the diffusion of impurity molecules) in the second hydrogenation catalyst is MACRO and median pore diameter PD2 MACRO is the volume V1 of the macropores in the first hydrogenation catalyst MACRO and median pore diameter PD1 MACRO It may be slightly smaller than

[0059] Volume V2 of mesopores in the second hydrogenation catalyst MESO The volume V2 may be 0.50 ml / g or more and 0.90 ml / g or less, preferably 0.55 ml / g or more and 0.85 ml / g or less, and more preferably 0.60 ml / g or more and 0.80 ml / g or less. MESO can be expressed as the total volume of all mesopores in the second hydrogenation catalyst. MESO The median pore diameter PD2 may be 6 nm or more and 20 nm or less, preferably 8 nm or more and 15 nm or less. MESO The specific surface area of ​​the second hydrogenation catalyst is 160 m, and the specific surface area of ​​the second hydrogenation catalyst is 160 m. The ... 2 / g or more 300m 2 / g or less, preferably 170m 2 / g or more 250m 2 / g or less. Transition catalysts that can be industrially used as second hydrogenation catalysts have constraints on their specific surface area and pore volume due to their target performance. The reason for this is that, like the first hydrogenation catalyst, the specific surface area of ​​the catalyst is positively correlated with the catalytic reaction active sites, and the pore diameter and pore volume affect the mass transfer of reactants (heavy oil molecules). On the other hand, there is a trade-off relationship between catalyst characteristics, in that increasing the pore diameter and pore volume to promote the mass transfer of reactants (heavy oil molecules) reduces the specific surface area. As a result, in order to ensure the desired performance as the second hydrogenation catalyst, it is naturally necessary to employ a catalyst having a high specific surface area while maintaining a minimum pore diameter and pore volume. As a result of research and investigation by the inventors, the specific surface area of ​​a second hydrogenation catalyst (transition catalyst) that exhibits high performance is 160 m 2 / g or more 300m 2 / g or less, preferably 170m 2 / g or more 250m 2 It was found that the specific surface area of ​​the second hydrogenation catalyst was 160 m / g or less. 2 If the saturation rate is less than 1 / g, the second hydrogenation catalyst will not be able to exhibit sufficient performance, and the performance of the entire catalyst system consisting of the first hydrogenation catalyst, the second hydrogenation catalyst and the third hydrogenation catalyst will be impaired, which is undesirable.

[0060] Volume V2 of macropores in the second hydrogenation catalyst MACRO The volume V2 may be 0.10 ml / g or more and 0.35 ml / g or less, preferably 0.15 ml / g or more and 0.30 ml / g or less. MACRO When the median pore diameter PD2 of the macropores in the second hydrogenation catalyst is 0.35 ml / g or less, the demetallization activity and hydrodesulfurization activity of the second hydrogenation catalyst are likely to be improved, and the mechanical strength of the second hydrogenation catalyst is improved. The total volume of pores having a pore diameter of 2000 nm or more in the second hydrogenation catalyst may be 0.1 ml / g or less, preferably 0.05 ml / g or less. When the total volume of pores having a pore diameter of 2000 nm or more is 0.1 ml / g or less, the mechanical strength of the second hydrogenation catalyst is improved. MACROmay be 100 nm or more and 500 nm or less, preferably 150 nm or more and 350 nm or less, and more preferably 200 nm or more and 250 nm or less.

[0061] The second hydrogenation catalyst includes a porous support made of an inorganic oxide. All of the pore characteristics in the second hydrogenation catalyst described above originate from the porous support. In other words, the pores in the second hydrogenation catalyst described above reflect the characteristics of the pores in the porous support constituting the second hydrogenation catalyst. The "second support" described below refers to the porous support constituting the second hydrogenation catalyst. Except for the pore distribution in the second support, the second support may be the same as the first support described above. The second support may be an oxide of one or more elements selected from the group consisting of Group 2 elements, Group 4 elements, Group 13 elements, and Group 14 elements. For example, the second support preferably includes one or more oxides selected from the group consisting of silica, alumina, magnesia, zirconia, boria, and calcia. The second support more preferably contains one or more oxides selected from the group consisting of γ-alumina, δ-alumina, η-alumina, χ-alumina, silica-alumina, silica, alumina-magnesia, silica-magnesia, and alumina-silica-magnesia. The second support is particularly preferably γ-alumina. The alumina (Al 2 O 3 The content of the hydroxybenzoates may be 50% by mass or more, preferably 70% by mass or more. Methods for controlling the second carrier to have a desired pore distribution include reducing the amount of water mixed with the raw material powder in the second carrier preparation process, optimizing the amount of molding aid, increasing the kneading intensity (shear force during kneading, kneading time, etc.), or optimizing the molding conditions (type of molding machine, molding pressure, etc.), while keeping the particle size of the raw material powder within an appropriate range (described below). In particular, in the production of the second carrier, the amount of water mixed with the mixed powder is adjusted to be less than that of the first carrier, and therefore the volume of macropores formed in the second carrier is reduced due to evaporation of moisture from the raw material mixture (dough). In addition, the low moisture content of the dough results in a harder dough, which is easier to handle and has the advantage of excellent productivity in extrusion molding.

[0062] The second hydrogenation catalyst may contain one or more metals selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements as the metal component (metal component having hydrogenation activity) supported on the second support. For example, the second hydrogenation catalyst may preferably contain at least one of molybdenum and tungsten. The second hydrogenation catalyst may further contain at least one of nickel and cobalt in addition to at least one of molybdenum and tungsten. The metal component supported on the second support may be a metal, oxide, or sulfide. The content of the Group 6 element in the second hydrogenation catalyst may be 5.0% by mass or more and 7.0% by mass or less, preferably 5.2% by mass or more and 6.8% by mass or less, and more preferably 5.4% by mass or more and 6.6% by mass or less. The total content of the Group 8 to 10 elements in the second hydrogenation catalyst may be 1.0% by mass or more and 3.0% by mass or less, preferably 1.2% by mass or more and 2.8% by mass or less. The second hydrogenation catalyst may further contain a compound (e.g., an oxide) containing at least one of phosphorus and boron. The total content of phosphorus and boron in the second hydrogenation catalyst may be 0.1 mass% or more and 2.0 mass% or less, preferably 0.2 mass% or more and 1.5 mass% or less, and more preferably 0.3 mass% or more and 1.3 mass% or less. When the contents of each element in the second hydrogenation catalyst are within the above ranges, the demetalization activity and hydrodesulfurization activity of the second hydrogenation catalyst are likely to be improved. In particular, when the content of the Group 6 element in the second hydrogenation catalyst is less than 5.0 mass%, it is difficult for the second hydrogenation catalyst to exhibit the desulfurization and demetalization performance expected of the second hydrogenation catalyst, and this is not preferred. Furthermore, if the content of the Group 6 element in the second hydrogenation catalyst exceeds 7.0 mass%, the desulfurization and demetalization performance expected of the second hydrogenation catalyst will be exceeded, thereby accelerating the poisoning of the catalyst and impairing the performance of the entire catalyst system consisting of the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst, which is therefore undesirable. Basically, the order and combination of the catalyst systems packed into the reactor are determined so that, in the order of the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst, the pore diameter and pore volume decrease, the specific surface area increases, and the content of the active metal (particularly the Group 6 element) increases.This is in response to changes in the properties and molecular structure of the heavy oil (reactant) being processed from the inlet to the outlet of the catalyst tower, and in response to changes in the required level of catalytic activity and poisoning resistance. From this perspective, there is an optimal value for the content of active metals (particularly Group 6 elements) in the second hydrogenation catalyst, taking into account the balance with the preceding and following catalysts. The content (unit: mass%) of Group 6 elements and Groups 8 to 10 elements in the second hydrogenation catalyst may be greater than the content (unit: mass%) of Group 6 elements and Groups 8 to 10 elements in the first hydrogenation catalyst. When the content (unit: mass%) of Group 6 elements and Groups 8 to 10 elements in the second hydrogenation catalyst is greater than the content (unit: mass%) of Group 6 elements and Groups 8 to 10 elements in the first hydrogenation catalyst, the demetalization activity and hydrodesulfurization activity of the second hydrogenation catalyst are improved, and as a result, excessive hydrocracking reactions on the surface of the subsequent third hydrogenation catalyst are more likely to be suppressed, and deactivation of the third hydrogenation catalyst is more likely to be suppressed.

[0063] An example of a method for preparing the second hydrogenation catalyst is described below. Except for the matters described below, the method for preparing the second hydrogenation catalyst may be the same as the method for preparing the first hydrogenation catalyst described above, although consideration and changes to conditions are required to control the macropore distribution.

[0064] The raw material for the second support is a raw material powder containing alumina such as γ-alumina (including hydrous alumina) or pseudo-boehmite as a main component. The raw material powder may further contain the oxides described above in addition to γ-alumina or pseudo-boehmite. The raw material powder is mixed and kneaded with a liquid, a molding aid, etc. to obtain a kneaded product (dough) with the desired moisture content, hardness, and viscosity. The kneaded product is extrusion-molded to form a molded body. The molded body is dried with hot air or the like to reduce the moisture content to an appropriate level, and then fired to obtain the second support. The content of γ-alumina (excluding adsorbed water) or pseudo-boehmite (excluding water of crystallization and adsorbed water) in the raw material powder may be 60% by mass or more and 100% by mass or less, preferably 75% by mass or more and 100% by mass or less.

[0065] The total volume of mesopores in the raw material powder may be 0.6 ml / g or more, preferably 0.8 ml / g or more. The pore size distribution of mesopores in the raw material powder may be measured by nitrogen adsorption. When the total volume of mesopores in the raw material powder is less than 0.6 ml / g, the volume V2 of mesopores in the first hydrogenation catalyst may be MESO Therefore, the effective metal deposition amount in the second hydrogenation catalyst is reduced. The average particle size (median diameter) of the raw material powder may be preferably 10 μm or more and 300 μm or less. The average particle size of the raw material powder may be measured by a general wet laser light scattering method. When the average particle size of the raw material powder is less than 10 μm, the volume V2 of the macropores in the second hydrogenation catalyst is MACRO If the average particle size of the raw material powder exceeds 300 μm, the volume of pores having a pore size of 2000 nm or more in the second hydrogenation catalyst increases, resulting in a decrease in the mechanical strength of the second hydrogenation catalyst.

[0066] The raw material powder for the second support is most preferably composed of pseudo-boehmite. However, the raw material powder for the second support may further contain γ-alumina in addition to pseudo-boehmite. A used catalyst (e.g., a hydrogenation catalyst in which a metal component is supported on γ-alumina) may be used as a raw material for γ-alumina. The average particle size of the raw material powder may be adjusted to a desired value by pulverizing the raw material powder using a ball mill, roller mill, jet mill, pulverizer, or the like. The pore size distribution of the second support can be controlled by the average particle size of the raw material powder. The average particle size of the raw material powder for the second support may be equal to or slightly smaller than the average particle size of the raw material powder for the first support.

[0067] It is preferable that the raw material powder and a liquid are mixed and kneaded before molding the raw material powder. The raw material powder and a liquid may be mixed using a general mixer or kneader used in catalyst preparation. Preferably, the raw material powder and water may be mixed using a stirring blade. Instead of water, an organic solvent such as an alcohol or a ketone may be used as the liquid to be mixed with the raw material powder. The raw material powder may be mixed with one or more additives such as an acid such as nitric acid, acetic acid, or formic acid, a base such as ammonia, an organic compound (molding aid) such as water-soluble cellulose ether, a surfactant, and an active ingredient. Preferably, a molding aid such as water-soluble cellulose ether may be mixed with the raw material powder. The pore distribution of the second support can be controlled by the concentration of these additives, the mixing and kneading conditions, the firing temperature, etc.

[0068] To achieve the above-described characteristics regarding the macropores in the second carrier, it is important to balance the appropriate moisture content and the amount of molding aid added in the process of mixing and kneading the raw material powder, water, and molding aid. The moisture content of the raw material mixture (dough) containing the raw material powder, water, and molding aid may be preferably 51.0 mass% or more and 56.0 mass% or less, more preferably 53.0 mass% or more and 55.0 mass% or less. The mass ratio of the molding aid added to the raw material powder may be preferably 0.1 mass% or more and 5 mass% or less, more preferably 0.3 mass% or more and 3.0 mass% or less, per 100 mass parts of the raw material powder.

[0069] For example, the shape of the second carrier may be a sphere, a cylinder, a cylindrical column, a prism, or a columnar body having a trefoil or quatrefoil cross section. For example, the maximum diameter of the cross section of the second carrier (a cross section perpendicular to the length direction in the case of a columnar or cylindrical body) may be 0.5 mm or more and 6 mm or less. For example, the length of the second carrier may be adjusted as desired, taking into account ease of handling.

[0070] [Third hydrogenation catalyst] Volume V3 of mesopores in the third hydrogenation catalyst MESO The median pore diameter PD3 of the mesopores in the third hydrogenation catalyst may be 0.5 ml / g or more and 1.0 ml / g or less, preferably 0.6 ml / g or more and 1.0 ml / g or less. MESO The median pore diameter PD3 may be 5 nm or more and 15 nm or less, preferably 7 nm or more and 13 nm or less.MESO is the pore size at which the cumulative volume of mesopores in the pore distribution of the third hydrogenation catalyst is 50% of the total volume of mesopores. 2 / g or more 350m 2 / g or less. The volume V3 of the macropores in the third hydrogenation catalyst MACRO The volume V3 may be 0.2 ml / g or less, preferably 0.1 ml / g or less. MACRO When the solubility is 0.2 ml / g or less, the hydrodesulfurization activity and mechanical strength of the third hydrogenation catalyst are likely to be improved.

[0071] The third hydrogenation catalyst includes a porous support made of an inorganic oxide. All of the pore characteristics in the third hydrogenation catalyst described above originate from the porous support. In other words, the pores in the third hydrogenation catalyst described above reflect the characteristics of the pores in the porous support constituting the third hydrogenation catalyst. The "third support" described below refers to the porous support constituting the third hydrogenation catalyst. Except for the pore distribution in the third support, the third support may be the same as the first support described above. The third support may be an oxide of one or more elements selected from the group consisting of Group 2 elements, Group 4 elements, Group 13 elements, and Group 14 elements. For example, the third support preferably includes one or more oxides selected from the group consisting of silica, alumina, magnesia, zirconia, boria, and calcia. More preferably, the third support comprises one or more oxides selected from the group consisting of γ-alumina, δ-alumina, η-alumina, χ-alumina, silica-alumina, silica, alumina-magnesia, silica-magnesia, and alumina-silica-magnesia.

[0072] The third hydrogenation catalyst may contain one or more metals selected from the group consisting of Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements as a metal component (metal component having hydrogenation activity) supported on a third support. For example, the third hydrogenation catalyst may preferably contain at least one of molybdenum and tungsten. The third hydrogenation catalyst may further contain at least one of nickel and cobalt in addition to at least one of molybdenum and tungsten. The metal component supported on the third support may be a metal, oxide, or sulfide. The total content of the Group 6 elements, Group 8 elements, Group 9 elements, and Group 10 elements in the third hydrogenation catalyst may be 3% by mass or more and 25% by mass or less, preferably 5% by mass or more and 20% by mass or less, and more preferably 7% by mass or more and 17% by mass or less. The third hydrogenation catalyst may further contain a compound (e.g., an oxide) containing at least one of phosphorus and boron. The total content of phosphorus and boron in the third hydrogenation catalyst may be 0% by mass or more and 5% by mass or less, preferably 0.5% by mass or more and 3% by mass or less. When the contents of each element in the third hydrogenation catalyst are within the above ranges, the hydrodesulfurization activity of the third hydrogenation catalyst is likely to be improved.

[0073] An example of a method for preparing the third hydrogenation catalyst will be described below. Except for the matters described below, the method for preparing the third hydrogenation catalyst may be similar to the methods for preparing the first hydrogenation catalyst and the second hydrogenation catalyst described above, although consideration must be given to the selection of raw materials and changes to preparation conditions in order to adjust the supported metal composition.

[0074] A raw material powder containing pseudoboehmite as a main component may be used as the raw material for the third support. The raw material powder is mixed with a liquid, and a molded body is formed through processes such as kneading and molding. The molded body is dried or fired to obtain the third support. The raw material powder and liquid are preferably mixed before molding. The raw material powder and liquid may be mixed and kneaded using a mixer or kneader commonly used in catalyst preparation. Preferably, the raw material powder and water may be mixed using a stirring blade. Instead of water, an organic solvent such as alcohol or ketone may be used as the liquid to be mixed with the raw material powder. The raw material powder may be mixed with one or more additives, such as acids such as nitric acid, acetic acid, and formic acid, bases such as ammonia, organic compounds (molding aids) such as water-soluble cellulose ether, surfactants, and active ingredients. The pore size distribution of the third support can be controlled by the concentration of these additives, the mixing and kneading conditions, the firing temperature, and the like.

[0075] For example, the shape of the third support may be a sphere, a cylinder, a cylindrical column, a prism, or a columnar body having a trefoil or quatrefoil cross section. For example, the maximum diameter of the cross section of the third support (a cross section perpendicular to the length direction in the case of a columnar or cylindrical body) may be 0.5 mm or more and 6 mm or less. For example, the length of the third support may be adjusted as desired, taking into account ease of handling.

[0076] [Heavy Oil] Heavy oil contains a fraction having a boiling point of 360°C or higher as a main component. For example, the content of the fraction having a boiling point of 360°C or higher in the heavy oil may be 50% by volume or higher, more preferably 70% by volume or higher, and even more preferably 90% by volume or higher. For example, the heavy oil may be various heavy fractions or residual oils obtained by atmospheric or vacuum distillation of a feedstock. Fractions obtained by processes such as cracking, isomerization, reforming, or solvent extraction of heavy fractions or residual oils may also be used as heavy oils. For example, the feedstock may be crude oil, tar sands, shale oil, coal liquefaction oil, etc. For example, according to this embodiment, heavy oils containing metals such as vanadium and nickel in a mass equivalent of 10 ppm by mass or 50 ppm by mass or higher can be subjected to hydrorefining.

[0077] The present invention is not necessarily limited to the above-described embodiments. Various modifications of the present invention are possible without departing from the spirit of the present invention, and these modifications are also included in the present invention.

[0078] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to these examples.

[0079] [Second Hydrogenation Catalyst] The second hydrogenation catalyst was prepared by the following method. 1.5 kg of commercially available pseudo-boehmite powder (hydrated alumina Versal-250 manufactured by UOP), approximately 1,400 ml of ion-exchanged water, and 10 g of water-soluble cellulose ether were kneaded together to obtain a raw material mixture with a moisture content of 54% by mass, adjusted appropriately with ion-exchanged water. The content of water of crystallization in the pseudo-boehmite powder was 18% by mass. The content of adsorbed water in the pseudo-boehmite powder was 12% by mass. The raw material mixture was extrusion-molded to form numerous four-lobed cylinders, yielding compacts (pellets). The maximum outer diameter of the four-lobed cross section was 1.9 mm. The compact was dried at 130°C for 15 hours and then calcined at 800°C for 1 hour in an air stream to obtain a second support for the second hydrogenation catalyst. The second support consisted of porous γ-alumina. An acidic aqueous solution containing molybdenum, nickel, and phosphorus was impregnated into the second support by a spraying method. After impregnation with the acidic aqueous solution, the second support was dried at 130°C for 20 hours. After drying, the second support was calcined in an air stream at 450°C for 25 minutes to obtain a second hydrogenation catalyst. The molybdenum content in the second hydrogenation catalyst was 6.0% by mass. The nickel content in the second hydrogenation catalyst was 1.5% by mass. The phosphorus content in the second hydrogenation catalyst was 1.0% by mass.

[0080] The pore distribution of the second hydrogenation catalyst was measured. The mesopore distribution and specific surface area in the second hydrogenation catalyst were measured by nitrogen adsorption. The macropore distribution in the second hydrogenation catalyst was measured by mercury intrusion porosimetry. The pore distribution of the second hydrogenation catalyst (a distribution obtained by plotting pore volume against the logarithm of pore diameter) had a peak where the pore volume was maximized for pore diameters of 50 nm or more, and a peak where the pore volume was maximized for pore diameters of less than 50 nm. In other words, the second hydrogenation catalyst was a bimodal catalyst containing macropores and mesopores. The volume V2 of mesopores in the second hydrogenation catalyst MESO The median pore diameter PD2 of the mesopores in the second hydrogenation catalyst was 0.68 ml / g. MESO The specific surface area of ​​the second hydrogenation catalyst was 183 m 2 / g. The volume V2 of the macropores in the second hydrogenation catalyst MACRO The median pore diameter PD2 of the macropores in the second hydrogenation catalyst was 0.19 ml / g. MACRO The volume of pores having a pore diameter of 2000 nm or more in the second hydrogenation catalyst was less than 0.01 ml / g.

[0081] [Conventional Middle Stage Catalyst] A conventional middle stage catalyst (hydrogenation catalyst) was used as a comparison with the second hydrogenation catalyst. The conventional middle stage catalyst was prepared in the same manner as the second hydrogenation catalyst, except that 2 kg of pseudoboehmite powder (hydrated alumina Versal-250 manufactured by UOP), 1 L of 1 mass % ammonia water, and 0.9 L of water were used as raw materials, and the moisture content of the dough was 52 mass %. The pore distribution of the conventional middle stage catalyst was measured in the same manner as the second hydrogenation catalyst. The volume of mesopores in the conventional middle stage catalyst was 0.77 ml / g. The median pore diameter of mesopores in the conventional middle stage catalyst was 16.5 nm. The specific surface area of ​​the conventional middle stage catalyst was 165 m 2 / g. The volume of macropores in the conventional middle stage catalyst was less than 0.01 ml / g. The volume of pores with a pore diameter of 2000 nm or more in the conventional middle stage catalyst was less than 0.01 ml / g. As described above, the conventional middle stage catalyst did not contain macropores. Except for the above-mentioned matters regarding pores and specific surface area, the conventional middle stage catalyst was almost similar to the second hydrogenation catalyst.

[0082] [First Hydrogenation Catalyst] The first hydrogenation catalyst was prepared by the following method. 450 g of commercially available pseudo-boehmite powder (hydrated alumina Versal-250 manufactured by UOP), 12 g of water-soluble cellulose ether, and 539 g of an ammoniacal molybdenum aqueous solution (molybdenum content: 1.84% by mass) were kneaded together to obtain a raw material mixture (dough) with a moisture content of 56% by mass, adjusted appropriately with ion-exchanged water. The raw material mixture was extrusion-molded to form numerous cylinders with a four-lobed cross section, resulting in a molded product (pellets). The content of water of crystallization in the pseudo-boehmite powder was 18% by mass. The content of adsorbed water in the pseudo-boehmite powder was 12% by mass. The maximum outer diameter of the cross section (four-lobed) of the molded product was 1.9 mm. The molded product was dried at 130°C for 15 hours and then calcined at 800°C for 1 hour in an air stream to obtain the first hydrogenation catalyst. The molybdenum content of the first hydrogenation catalyst was 3.0% by mass. The pore size distribution of the first hydrogenation catalyst was measured in the same manner as for the second hydrogenation catalyst. The pore size distribution of the first hydrogenation catalyst (a distribution obtained by plotting pore volume against the logarithm of pore size) had a peak where the pore volume was maximized for pore sizes of 50 nm or more, and a peak where the pore volume was maximized for pore sizes of less than 50 nm. In other words, the first hydrogenation catalyst was a bimodal catalyst containing macropores and mesopores. The volume V1 of the mesopores in the first hydrogenation catalyst MESO The median pore diameter PD1 of the mesopores in the first hydrogenation catalyst was 0.77 ml / g. MESO The specific surface area of ​​the first hydrogenation catalyst was 248 m 2 / g. The volume V1 of the macropores in the first hydrogenation catalyst MACRO The median pore diameter PD1 of the macropores in the first hydrogenation catalyst was 0.31 ml / g.MACRO The volume of pores having a pore diameter of 2000 nm or more in the first hydrogenation catalyst was less than 0.01 ml / g. The volume V1 of macropores in the first hydrogenation catalyst MACRO is the volume V2 of the macropores in the second hydrogenation catalyst MACRO The median pore diameter PD1 of the macropores in the first hydrogenation catalyst was larger than MACRO is the median pore diameter PD2 of the macropores in the second hydrogenation catalyst MACRO It was bigger than that.

[0083] [Third Hydrogenation Catalyst] The third hydrogenation catalyst was prepared by the following method. 2 kg of commercially available pseudoboehmite powder (a 7:3 mixture of hydrated alumina Catapal-C1 manufactured by SASOL and hydrated alumina Versal-250 manufactured by UOP), approximately 2000 ml of ion-exchanged water, and 61.5 g of nitric acid were kneaded to obtain a raw material mixture (dough) with a moisture content of 52 mass%. The raw material mixture was extrusion-molded to form numerous cylindrical bodies, resulting in a molded body (pellet). The outer diameter of the cross-section (circular shape) of the molded body was 1.0 mm. The molded body was dried at 130°C for 15 hours and then calcined at 600°C for 1 hour in an air stream to obtain a third support. The third support was impregnated with an aqueous molybdic acid solution by a spray method, dried, and then further impregnated with an aqueous nickel nitrate solution by a spray method and dried. Thereafter, the catalyst was calcined at 500°C for 30 minutes under air flow to obtain a third hydrogenation catalyst. The third support (support for the third hydrogenation catalyst) was made of porous γ-alumina. The molybdenum content in the third hydrogenation catalyst was 8.0 mass%. The nickel content in the third hydrogenation catalyst was 2.2 mass%. The pore size distribution of the third hydrogenation catalyst was measured in the same manner as for the second hydrogenation catalyst. The volume V3 of mesopores in the third hydrogenation catalyst was MESO The median pore diameter PD3 of the mesopores in the third hydrogenation catalyst was 0.62 ml / g. MESO The specific surface area of ​​the third hydrogenation catalyst was 231 m 2 / g. The volume V3 of the macropores in the third hydrogenation catalyst MACROThe volume of pores having a diameter of 2000 nm or more in the third hydrogenation catalyst was less than 0.01 ml / g. As described above, the third hydrogenation catalyst did not contain macropores.

[0084] Before carrying out the hydrorefining of heavy oil described below, the first hydrogenation catalyst, the second hydrogenation catalyst, the conventional middle stage catalyst, and the third hydrogenation catalyst were each subjected to a sulfurization treatment. In the sulfurization treatment of each catalyst, each catalyst was contacted with a non-aromatic hydrocarbon oil in which 1 volume % of dimethyl disulfide was dissolved.

[0085] [Heavy Oil] Mixed oil A and mixed oil B were used as heavy oils. Mixed oil A was a mixed oil consisting of atmospheric residue (AR) and vacuum residue (VR). Mixed oil B was a mixed oil consisting of atmospheric residue and deasphalted oil. Deasphalted oil is a fraction obtained by removing asphaltene from vacuum residue by solvent extraction. The densities of mixed oil A and mixed oil B are shown in Table 1 below. The contents of each impurity in mixed oil A and mixed oil B are shown in Table 1 below.

[0086]

[0087] [Hydrotrefining of Heavy Oil] (Example 1) Hydrotreating of Example 1 was carried out by the following method.

[0088] The hydrotreating apparatus had three cylindrical reactors (first-stage reactor, middle reactor, and second-stage reactor). Each of the first-stage reactor, middle reactor, and second-stage reactor was a downflow-type fixed-bed reactor. The length of each reactor was 1000 mm, and the inner diameter of each reactor was 25 mm. The first-stage reactor was connected to the middle-stage reactor, and the middle reactor was connected to the second-stage reactor. The first hydrogenation catalyst was packed in the first-stage reactor, the second hydrogenation catalyst was packed in the middle reactor, and the third hydrogenation catalyst was packed in the second-stage reactor. The volume proportions (unit: vol%) of the catalyst layers of the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst are shown in Table 2 below. In the hydrotreating of Example 1, mixed oil A was used as the heavy oil. The heavy oil was supplied to a first-stage reactor, the heavy oil that had come into contact with the first hydrogenation catalyst in the first-stage reactor was supplied to a middle-stage reactor, and the heavy oil that had come into contact with the second hydrogenation catalyst in the middle-stage reactor was supplied to a second-stage reactor. The product oil was recovered from the outlet of the second-stage reactor.

[0089] During hydrotreating, hydrogen gas was continuously supplied to each reactor. The hydrogen partial pressure in each reactor was maintained at 14.4 MPa. During hydrotreating, the hydrogen / oil ratio was maintained at 800 L / L. During hydrotreating, the liquid hourly space velocity was 0.45 hr -1 The temperature of each reactor (each catalytic layer) during hydrotreating was continuously adjusted so that the sulfur content in the product oil (fraction with a boiling point of 360°C or higher) was maintained at 0.35% by mass. In order to maintain a constant impurity content in the product oil, it is necessary to compensate for the activity of each hydrogenation catalyst by increasing the reaction temperature (the temperature of each hydrogenation catalyst layer) as the hydrogenation catalyst is deactivated. Therefore, the smaller the increase in temperature of each reactor (each catalytic layer) over time during hydrotreating, the more suppressed the deactivation of each hydrogenation catalyst is, and the better the activity of each hydrogenation catalyst for removing impurities from the heavy oil is maintained.

[0090] The temperature at the inlet of the middle-stage reactor (second hydrogenation catalyst layer) was maintained at a temperature equal to the temperature at the outlet of the first-stage reactor (first hydrogenation catalyst layer). The temperature at the inlet of the second-stage reactor (third hydrogenation catalyst layer) was maintained at a temperature 5°C lower than the temperature at the outlet of the middle-stage reactor (second hydrogenation catalyst layer). The temperature at the inlet of the first-stage reactor (first hydrogenation catalyst layer) at the start of hydrotreating was adjusted to about 340°C to 360°C so as to adjust the sulfur content in the product oil to the target value.

[0091] By continuing the above-mentioned hydrotreating of heavy oil, the various items shown in Table 2 below were measured. In Table 2 below, "Reaction temperature at 300 days" refers to the average temperature (CAT; Catalyst Average Temperature) of all reactors (all catalyst layers) 300 days after the start of hydrotreating. The lower the "Reaction temperature at 300 days," the better the activity of each hydrogenation catalyst for removing impurities from heavy oil that is maintained. In Table 2 below, "[V] at 300 days" refers to the vanadium content in the product oil (fraction having a boiling point of 360°C or higher) 300 days after the start of hydrotreating. In Table 2 below, "[Ni] at 300 days" refers to the nickel content in the product oil (fraction having a boiling point of 360°C or higher) 300 days after the start of hydrotreating. In Table 2 below, "days to 388°C" refers to the time required for the average temperature (CAT) of all reactors (all catalyst layers) to reach 388°C. The longer the "days to 388°C," the more suppressed is the deactivation of each hydrogenation catalyst, and the more excellent activity of each hydrogenation catalyst for removing impurities from heavy oil is maintained. In Table 2 below, "[V] at 388°C" refers to the vanadium content in the product oil (fraction having a boiling point of 360°C or higher) at the time when the average temperature (CAT) of all reactors (all catalyst layers) reached 388°C. In Table 2 below, "[Ni] at 388°C" refers to the nickel content in the product oil (fraction having a boiling point of 360°C or higher) at the time when the average temperature (CAT) of all reactors (all catalyst layers) reached 388°C.

[0092] (Comparative Examples 1 to 3) In Comparative Example 1, a conventional middle-stage catalyst was used instead of the second hydrogenation catalyst. In Comparative Example 2, neither the second hydrogenation catalyst nor the conventional middle-stage catalyst was used. In Comparative Example 3, the first hydrogenation catalyst was not used. The volume ratio of each hydrogenation catalyst layer used in each of Comparative Examples 1 to 3 is shown in Table 2 below. Hydrotreating for each of Comparative Examples 1 to 3 was carried out in the same manner as in Example 1, except for the above-mentioned details. In hydrotreating for each of Comparative Examples 1 to 3, the same measurements as in Example 1 were carried out. The measurement results for each of Comparative Examples 1 to 3 are shown in Table 2 below.

[0093]

[0094] The second hydrogenation catalyst of Example 1 had superior performance in removing difficult-to-react metal components compared to the conventional middle-stage catalyst of Comparative Example 1. Therefore, the metal components were sufficiently removed by the second hydrogenation catalyst, and metal leakage to the third hydrogenation catalyst of Example 1 was suppressed. As a result, poisoning and deactivation of the third hydrogenation catalyst by metal components was suppressed, and the "number of days to reach 388°C" in Example 1 was extended by 39 days compared to Comparative Example 1. In Comparative Example 2, in which the second hydrogenation catalyst was not used, only the first hydrogenation catalyst specialized for demetalization function was installed in the upstream stage of the third hydrogenation catalyst. As a result, the demetalization reaction did not proceed sufficiently in the upstream stage of the third hydrogenation catalyst of Comparative Example 2, and the "number of days to reach 388°C" in Comparative Example 2 was 138 days shorter than that of Example 1. In Comparative Example 3, in which the first hydrogenation catalyst was not used, only the second hydrogenation catalyst specialized for removing difficult-to-react metal components was installed in the upstream stage of the third hydrogenation catalyst. As a result, the demetallization reaction did not proceed sufficiently in the upstream stage of the third hydrogenation catalyst in Comparative Example 3, and the "number of days to reach 388°C" in Comparative Example 3 was 20 days shorter than that in Example 1.

[0095] (Examples 2 to 5 and Comparative Example 4) In the hydrorefining of each of Examples 2 to 5 and Comparative Example 4, mixed oil B was used as the heavy oil instead of mixed oil A. In Comparative Example 4, a conventional middle-stage catalyst was used instead of the second hydrogenation catalyst. The volume ratios of the hydrogenation catalysts used in each of Examples 2 to 5 and Comparative Example 4 are shown in Table 3 below. Hydrorefining of each of Examples 2 to 5 and Comparative Example 4 was carried out in the same manner as in Example 1, except for the above-mentioned details. In the hydrorefining of each of Examples 2 to 5 and Comparative Example 4, the same measurements as in Example 1 were also carried out. The measurement results of each of Examples 2 to 5 and Comparative Example 4 are shown in Table 3 below.

[0096]

[0097] In all of Examples 2 to 5, the "reaction temperature at 300 days" was lower than that in Comparative Example 1. In other words, Examples 2 to 5 demonstrated that the use of the second hydrogenation catalyst extended the life of each hydrogenation catalyst, regardless of the change in the volume ratio of the first hydrogenation catalyst to the third hydrogenation catalyst.

[0098] (Examples 6 and 7) In the hydrorefining of Examples 6 and 7, mixed oil B was used as the heavy oil instead of mixed oil A. The volumetric ratios of the hydrogenation catalysts used in Examples 6 and 7 are shown in Table 4 below. Hydrorefining of Examples 6 and 7 was carried out in the same manner as in Example 1, except for the above-mentioned points. In the hydrorefining of Examples 6 and 7, the same measurements as in Example 1 were carried out. The measurement results of Examples 6 and 7 are shown in Table 4 below. Table 4 below compares Examples 4, 6, 7 and Comparative Example 4, which have the same volumetric ratio of the third hydrogenation catalyst.

[0099]

[0100] In all of Examples 4, 6, and 7, the "reaction temperature at 300 days" was lower than that in Comparative Example 4. That is, Examples 4, 6, and 7 demonstrated that the use of the second hydrogenation catalyst extended the life of each hydrogenation catalyst, even when the total volume ratio of the first hydrogenation catalyst and the second hydrogenation catalyst was fixed and the volume ratio of the second hydrogenation catalyst to the third hydrogenation catalyst was varied.

[0101] For example, the product oil obtained by the heavy oil hydrorefining method according to one aspect of the present invention may be used as a base material for heavy oil, kerosene, light oil, gasoline, naphtha, etc., either directly or after secondary refining such as catalytic cracking, hydrocracking, hydrorefining, etc.

[0102] PD1 MACRO ...median pore diameter of macropores in the first hydrogenation catalyst, PD1 MESO ...median pore diameter of mesopores in the first hydrogenation catalyst, PD2 MACRO ...median pore diameter of macropores in the second hydrogenation catalyst, PD2 MESO ...median pore diameter of mesopores in the second hydrogenation catalyst.

Claims

1. A process for producing a heavy oil mixture comprising a step of sequentially contacting a first hydrogenation catalyst, a second hydrogenation catalyst, and a third hydrogenation catalyst in the presence of hydrogen, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst being installed in a downflow type fixed bed reactor, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst being different catalysts from one another, the first hydrogenation catalyst and the second hydrogenation catalyst both containing macropores and mesopores, the pore diameter of the macropores being 50 nm or more, and the pore diameter of the mesopores being less than 50 nm, and the pore distribution of the first hydrogenation catalyst having a peak where the pore volume is maximized at a pore diameter of 50 nm or more and a peak where the pore volume is maximized at a pore diameter of less than 50 nm, The pore distribution of the second hydrogenation catalyst has a peak where the pore volume is maximized at a pore diameter of 50 nm or more and a peak where the pore volume is maximized at a pore diameter of less than 50 nm, and the volume V1 of the macropores in the first hydrogenation catalyst MACRO is the volume V2 of the macropores in the second hydrogenation catalyst MACRO The specific surface area of ​​the first hydrogenation catalyst is greater than 185 m 2 / g or more, and the specific surface area of ​​the second hydrogenation catalyst is 160 m 2 / g or more, and the content of Group 6 elements in the second hydrogenation catalyst is 5 mass % or more and 7 mass % or less.

2. A process for sequentially contacting heavy oil with a first hydrogenation catalyst, a second hydrogenation catalyst, and a third hydrogenation catalyst in the presence of hydrogen, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst being installed in a downflow type fixed bed reactor, the first hydrogenation catalyst, the second hydrogenation catalyst, and the third hydrogenation catalyst being different catalysts from one another, both the first hydrogenation catalyst and the second hydrogenation catalyst containing macropores and mesopores, the pore diameter of the macropores being 50 nm or more, and the pore diameter of the mesopores being less than 50 nm, and the pore distribution of the first hydrogenation catalyst having a peak where the pore volume is maximized at a pore diameter of 50 nm or more and a peak where the pore volume is maximized at a pore diameter of less than 50 nm, The pore distribution of the second hydrogenation catalyst has a peak where the pore volume is maximized at a pore diameter of 50 nm or more and a peak where the pore volume is maximized at a pore diameter of less than 50 nm, and the median pore diameter PD1 of the macropores in the first hydrogenation catalyst MACRO is a pore diameter in which the integrated volume of the macropores in the pore distribution of the first hydrogenation catalyst is 50% of the total volume of the macropores, and the median pore diameter PD2 of the macropores in the second hydrogenation catalyst MACRO is a pore size in which the cumulative volume of the macropores in the pore distribution of the second hydrogenation catalyst is 50% of the total volume of the macropores, and the median pore size PD1 MACRO is the median pore diameter PD2 MACRO The specific surface area of ​​the first hydrogenation catalyst is greater than 185 m 2 / g or more, and the specific surface area of ​​the second hydrogenation catalyst is 160 m 2 / g or more, and the content of Group 6 elements in the second hydrogenation catalyst is 5 mass % or more and 7 mass % or less.

3. The volume V1 of the macropores in the first hydrogenation catalyst MACRO is the volume V2 of the macropores in the second hydrogenation catalyst MACRO The method for hydrotreating heavy oil according to claim 2, wherein the ratio of the stoichiometric ratio of the heavy oil to the total stoichiometric ratio is greater than 1.

4. The median pore diameter PD1 MACROis 300 nm or more and 1500 nm or less, and the median pore diameter PD2 MACRO The method for hydrorefining heavy oil according to claim 2 or 3, wherein the average particle size is 100 nm or more and 500 nm or less.

5. The volume V1 MACRO is 0.20 ml / g or more and 0.50 ml / g or less, and the volume V2 MACRO The method for hydrorefining heavy oil according to claim 1 or 3, wherein the solubility in stoichiometric amounts is 0.10 ml / g or more and 0.35 ml / g or less.

6. The volume V2 of the mesopores in the second hydrogenation catalyst MESO is 0.50 ml / g or more and 0.90 ml / g or less, and the median pore diameter PD2 of the mesopores in the second hydrogenation catalyst is MESO is a pore diameter at which the integrated volume of the mesopores in the pore distribution of the second hydrogenation catalyst is 50% of the total volume of the mesopores, and the median pore diameter PD2 MESO The method for hydrotreating heavy oil according to any one of claims 1 to 3, wherein the average particle size is 6 nm or more and 20 nm or less.

7. A method for hydrorefining heavy oil according to any one of claims 1 to 3, wherein the macropore distribution among the pore distributions of the first hydrogenation catalyst and the second hydrogenation catalyst is measured by mercury intrusion porosimetry, and the mesopore distribution among the pore distributions of the first hydrogenation catalyst and the second hydrogenation catalyst is measured by nitrogen adsorption.

8. A method for hydrorefining heavy oil according to any one of claims 1 to 3, wherein the content of Group 8 to 10 elements in the second hydrogenation catalyst is 1.0 mass% or more and 3.0 mass% or less, and the content of phosphorus in the second hydrogenation catalyst is 0.1 mass% or more and 2.0 mass% or less.

9. The method for hydrorefining heavy oil according to any one of claims 1 to 3, wherein the second hydrogenation catalyst has a larger content of the Group 6 element and the Group 8 to 10 element than the first hydrogenation catalyst, and the content is expressed in units of mass%.

10. A method for hydrorefining heavy oil according to any one of claims 1 to 3, wherein a volume of the first hydrogenation catalyst is represented as Vc1, a volume of the second hydrogenation catalyst is represented as Vc2, a volume of the third hydrogenation catalyst is represented as Vc3, (Vc1+Vc2) / (Vc1+Vc2+Vc3) is 40 volume % or more and 70 volume % or less, and (Vc2+Vc3) / (Vc1+Vc2+Vc3) is 60 volume % or more and 95 volume % or less.

Citation Information

Patent Citations

  • Hydrogenation catalyst for heavy oil and method of manufacturing heavy fuel oil

    JP2002177796A

  • Method for demetallating petroleum heavy oil

    JP2004115581A

  • Hydrogenation purification method for heavy residual oil

    JP2013209529A

  • Hydroprocessing catalyst for heavy hydrocarbon oil, method for manufacturing hydroprocessing catalyst for heavy hydrocarbon oil, and hydroprocessing method for heavy hydrocarbon oil