Photocurable resin composition, hard coat film for molding, film for molding, insert molded article, out-molded article, method for producing insert molded article, and method for producing out-molded article

The photocurable resin composition, featuring urethane acrylate and alumina fine particles, addresses the limitations of hard coat films by enhancing moldability and scratch resistance, ensuring flexible and durable cured layers for improved processing and performance.

WO2024228370A1PCT designated stage expired Publication Date: 2024-11-07AICA KOGYO CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016463
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-10
Filing Date
2024-04-26
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing hard coat films for molding face limitations in moldability and scratch resistance, particularly in three-dimensional shaping due to the rigidity of the resin cured layer, which can lead to microcracks in curved portions, restricting processing shapes and requiring additional properties like car wash scratch resistance.

Method used

A photocurable resin composition comprising urethane acrylate obtained by reacting pentaerythritol triacrylate with a diisocyanate derived from ethylene glycol and isophorone diisocyanate, combined with alumina fine particles and a photopolymerization initiator, offering a weight average molecular weight of 2,000 to 12,000 and a primary average particle diameter of 40 to 150 nm, enhancing both moldability and scratch resistance.

Benefits of technology

The composition achieves excellent moldability, scratch resistance, and car wash scratch resistance, with the alumina fine particles improving hardness and abrasion resistance, allowing for flexible and durable cured layers that maintain optical properties and resist damage during processing and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016463_07112024_PF_FP_ABST
    Figure JP2024016463_07112024_PF_FP_ABST
Patent Text Reader

Abstract

This photocurable resin composition contains: a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate to obtain diisocyanate and by further reacting pentaerythritol triacrylate with the diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D). The weight-average molecular weight of the component (A) is 2,000-12,000. The primary average particle diameter of the component (B) is 40-150 nm.
Need to check novelty before this filing date? Find Prior Art

Description

Photocurable resin composition, molding hard coat film, molding film, insert molded article, out-mold molded article, method for manufacturing insert molded article, and method for manufacturing out-mold molded article CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This international application claims priority based on Japanese Patent Application No. 2023-076071 filed with the Japan Patent Office on May 2, 2023, priority based on Japanese Patent Application No. 2023-096973 filed with the Japan Patent Office on June 13, 2023, priority based on Japanese Patent Application No. 2023-185167 filed with the Japan Patent Office on October 30, 2023, and priority based on Japanese Patent Application No. 2023-185167 filed with the Japan Patent Office on May 2, 2023. This application claims priority based on Japanese Patent Application No. 2023-191904 filed with the Japan Patent Office on November 10, 2011, and the entire contents of Japanese Patent Application Nos. 2023-076071, 2023-096973, 2023-185167, and 2023-191904 are incorporated by reference into this international application.

[0002] The present disclosure relates to a photocurable resin composition, a hard coat film for molding, a molding film, an insert molded article, an out-mold molded article, a method for manufacturing an insert molded article, and a method for manufacturing an out-mold molded article.

[0003] Acrylic photocurable resin compositions are used in many fields to impart special properties to the surfaces of plastic films and plastic molded products. For example, a hard coat film can be obtained by applying a photocurable resin composition to a polyethylene terephthalate (PET) film to form a highly hard cured resin layer. Hard coat films are widely used as hard coat films for touch panels and molding applications.

[0004] After printing a pattern on the surface of a hard-coated film for molding, the film may be softened by heating and then molded into a three-dimensional shape. If the resin cured layer of the hard-coated film for molding is hard, microcracks are likely to occur in the curved surface when the hard-coated film for molding is processed into a three-dimensional shape. Therefore, the shape of the hard-coated film for molding has been restricted.

[0005] The applicant has invented a hard coating agent for insert molding that achieves both surface hardness and moldability (Patent Document 1). This hard coating agent contains a triazine ring-containing (meth)acrylate prepolymer and organic fine particles with an average primary particle diameter of 80 to 500 nm. A cured resin layer formed using this hard coating agent has excellent flexibility and surface properties when its film thickness is 1 to 10 μm.

[0006] Patent No. 4848200

[0007] As the applications of insert-molded products expand, various properties are being required of hard-coated molding films, such as moldability and scratch resistance.

[0008] In one aspect of the present disclosure, it is preferable to provide a photocurable resin composition, a molding hard coat film, a molding film, an insert molded article, an out-mold molded article, a method for manufacturing an insert molded article, and a method for manufacturing an out-mold molded article, which are excellent in moldability and scratch resistance.

[0009] One aspect of the present disclosure is a photocurable resin composition comprising: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the weight-average molecular weight of (A) is 2,000 to 12,000, and the average primary particle size of (B) is 40 to 150 nm.

[0010] The photocurable resin composition according to one aspect of the present disclosure is excellent in moldability and scratch resistance.

[0011] Another aspect of the present disclosure is a photocurable resin composition comprising: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the average primary particle diameter of (B) is 40 to 150 nm; and a film having a substrate and a cured layer of the photocurable resin composition formed on the substrate has a breaking elongation of 50% or more at an ambient temperature of 130°C and a tensile speed of 300 mm / min.

[0012] The photocurable resin composition according to another aspect of the present disclosure is excellent in moldability and scratch resistance.

[0013] Another aspect of the present disclosure is a photocurable resin composition comprising: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the weight-average molecular weight of (A) is 2,000 to 12,000; and when an abrasion test in accordance with DIN EN ISO 20566 is performed on a film having a substrate and a cured layer of the photocurable resin composition formed on the substrate using a car wash abrasion tester, the gloss of the cured layer after the abrasion test is 50% or more of the gloss of the cured layer before the abrasion test.

[0014] The photocurable resin composition according to another aspect of the present disclosure is excellent in moldability and scratch resistance.

[0015] Another aspect of the present disclosure is a method for producing an insert-molded product, which includes using a mold to form a molding film having a plastic substrate, a cured layer of a photocurable resin composition formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer, and then injecting a molten resin into the molding film from the side opposite the cured layer to form a resin molded product. The photocurable resin composition includes a urethane acrylate (A) obtained by reacting ethylene glycol and isophorone diisocyanate with a diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate, alumina fine particles (B), a leveling agent (C), and a photopolymerization initiator (D), wherein the weight-average molecular weight of (A) is 2,000 to 12,000, and the average primary particle size of (B) is 40 to 150 nm.

[0016] A method for producing an insert-molded article that is another aspect of the present disclosure can produce an insert-molded article that is excellent in moldability and scratch resistance.

[0017] Another aspect of the present disclosure is a method for producing an out-molded product, which comprises vacuum-forming or pressure-forming a molding film having a plastic substrate, a cured layer of a photocurable resin composition formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer, onto a pre-formed substrate. The photocurable resin composition includes a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate to form a diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate, alumina fine particles (B), a leveling agent (C), and a photopolymerization initiator (D), wherein the weight-average molecular weight of (A) is 2,000 to 12,000, and the average primary particle size of (B) is 40 to 150 nm.

[0018] The method for producing an out-molded article according to another aspect of the present disclosure can produce an out-molded article that is excellent in formability and scratch resistance.

[0019] 2A is a cross-sectional view showing the structure of a hard coat film for molding. Fig. 2A is a cross-sectional view showing the layer structure of molding films F11 to F12 and F15. Fig. 2B is a cross-sectional view showing the layer structure of molding films F13 to F14 and F16.

[0020] Exemplary embodiments of the present disclosure will now be described with reference to the drawings.

[0021] 1. Photocurable Resin Composition The photocurable resin composition contains a urethane acrylate (A) having a structure obtained by further reacting pentaerythritol triacrylate (hereinafter referred to as PETA) with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate (hereinafter referred to as IPDI), alumina fine particles (B), a leveling agent (C), and a photopolymerization initiator (D).

[0022] In this specification, (meth)acrylate refers to both acrylate and methacrylate. The above components (A) to (D) are referred to as components (A) to (D).

[0023] The IPDI used in the synthesis of component (A) is an alicyclic diisocyanate. IPDI is resistant to yellowing, has excellent weather stability, and is highly rigid. Therefore, by using IPDI in the synthesis of component (A), the hardness of the cured layer of the photocurable resin composition (hereinafter referred to as the cured resin layer) can be increased.

[0024] By reacting ethylene glycol, which has a very short carbon chain, with IPDI, the concentration of urethane bonds in the molecules of the photocurable resin composition can be increased. Increasing the concentration of urethane bonds allows the formation of a main skeleton with a linear structure that is highly rigid and has excellent chemical resistance. Using polyethylene glycol instead of ethylene glycol tends to decrease the concentration of urethane bonds, resulting in reduced chemical resistance.

[0025] The synthesis method of component (A) is not particularly limited. Known methods can be used to synthesize component (A). The reaction to synthesize component (A) may be a solvent-free reaction or a reaction using a solvent. When the molecular weight of component (A) is high, a reaction using a solvent is preferred. When a reaction using a solvent is used, stirring is easy even if the molecular weight of component (A) is high. Examples of solvents include ketones such as methyl ethyl ketone (hereinafter referred to as MEK), and aromatic inert solvents such as xylene.

[0026] Furthermore, it is preferable to use a catalyst for the reaction between the hydroxyl groups of ethylene glycol and PETA and the isocyanate groups. Examples of catalysts include tin-based catalysts such as dibutyltin dilaurate and metal alkoxide-based catalysts such as cobalt naphthenate. The reaction temperature for synthesizing component (A) can be set appropriately, but is preferably 40 to 120°C, and more preferably 60 to 100°C.

[0027] The weight average molecular weight (hereinafter referred to as Mw) of component (A) is, for example, 2,000 to 12,000, preferably 3,000 to 11,000, and more preferably 3,500 to 10,000.

[0028] When the Mw of component (A) is 2,000 or more, the breaking elongation of the cured resin layer is high, thereby improving the moldability of the photocurable resin composition.When the Mw of component (A) is 12,000 or less, the abrasion resistance and scratch resistance of the cured resin layer are improved.

[0029] The Mw of component (A) can be adjusted by the molar ratio of ethylene glycol to IPDI in the reaction. When the ratio of the number of moles of IPDI to the number of moles of ethylene glycol approaches 1, the Mw tends to increase.

[0030] The Mw is a value measured by gel permeation chromatography. When performing gel permeation chromatography, a column packed with a styrene-divinylbenzene-based packing material was used. Furthermore, when performing gel permeation chromatography, tetrahydrofuran was used as an eluent. The Mw was calculated by a conversion method based on the molecular weight of standard polystyrene.

[0031] The amount of component (A) is preferably 70 to 95 wt %, more preferably 75 to 93 wt %, and particularly preferably 80 to 90 wt %, based on the total solid content of the photocurable resin composition. When the amount of component (A) is 70 wt % or more, the photocurable resin composition has even higher moldability and chemical resistance. When the amount of component (A) is 95 wt % or less, the photocurable resin composition has even higher abrasion resistance and car wash scratch resistance.

[0032] Component (B) increases the hardness of the cured resin layer and improves its abrasion resistance, scratch resistance, and car wash scratch resistance. Car wash scratch resistance refers to the property of making the cured resin layer less susceptible to scratches even when using a car wash machine, etc. Scratch resistance and car wash scratch resistance correspond to scratch resistance.

[0033] Generally, the scratch resistance of a cured resin layer is evaluated by using steel wool (hereinafter referred to as SW) in a dry state to which a load of about 200 to 500 g / 25 mmφ is applied, and evaluating the degree of scratching of the cured resin layer.

[0034] On the other hand, when an automatic car wash is used, a material with a relatively low elastic modulus (e.g., a polymeric rubber-based material) hits the surface of the cured resin layer with a strong force for a short period of time in the presence of moisture. As such, the way in which force is applied to the surface of the cured resin layer differs between a general method for evaluating the abrasion resistance of a cured resin layer and when an automatic car wash is used. Therefore, even if the evaluation result of the general method for evaluating the abrasion resistance of a cured resin layer is good, the cured resin layer may be scratched when used in a car wash.

[0035] After repeated trial and error, the applicant discovered that adding component (B) to a photocurable resin composition improves the car wash scratch resistance of the cured resin layer. The applicant further discovered that adding component (B) with a specific particle size significantly improves the car wash scratch resistance of the cured resin layer.

[0036] The average primary particle size of component (B) is preferably 10 to 200 nm, more preferably 40 to 150 nm, particularly preferably 50 to 100 nm, and particularly preferably 60 to 80 nm. Component (B) is, for example, nanoalumina.

[0037] When the primary average particle diameter of component (B) is 10 nm or more, car wash scratch resistance is further improved. When the primary average particle diameter of component (B) is 200 nm or less, the molding hard coat film having a resin cured layer has good optical properties. When the primary average particle diameter of component (B) is 40 to 150 nm, car wash scratch resistance is significantly improved. The primary average particle diameter is the median diameter (d = 50) measured by dynamic light scattering (DLS).

[0038] The blending amount of component (B) is preferably 0.1 to 20 wt %, more preferably 0.5 to 15 wt %, particularly preferably 1 to 10 wt %, and particularly preferably 1.5 to 8 wt %, based on the total solid content of the photocurable resin composition. When the blending amount of component (B) is 0.1 wt % or more, car wash scratch resistance is further improved. When the blending amount of component (B) is 20 wt % or less, the moldability of the resin cured layer is further improved.

[0039] The component (C) improves the leveling properties when the photocurable resin composition is applied. The component (C) also improves the SW resistance of the cured resin layer. The SW resistance refers to the resistance of the cured resin layer to scratches when subjected to an evaluation method for scratch resistance using SW.

[0040] The component (C) preferably has a reactive functional group capable of polymerizing with the binder resin to form a cured resin layer. In this case, the component (C) can be prevented from being lost over time from the cured resin layer due to bleeding or the like. Furthermore, the SW resistance of the cured resin layer can be improved over the long term.

[0041] Examples of the component (C) include fluorine-based compounds, silicone-based compounds, fluorine-based silicone compounds, etc. As the component (C), these can be used alone or in combination of two or more types.

[0042] Of the silicone compounds, polysiloxane compounds are preferred as component (C). When a polysiloxane compound is used as component (C), the surface tension of the cured resin layer can be made uniform.

[0043] Examples of polysiloxane compounds include polyalkyl siloxanes, polyaryl siloxanes, polyalkylaryl siloxanes, polyester-modified siloxanes, polyether-modified siloxanes, etc. These can be used alone or in combination of two or more as component (C).

[0044] The blending amount of component (C) is preferably 0.1 to 3 wt %, more preferably 0.3 to 2 wt %, based on the total solid content of the photocurable resin composition. When the blending amount of component (C) is within this range, the leveling properties when the photocurable resin composition is applied are good, and the appearance of the cured resin layer is stable. Commercially available products of component (C) include BYK-UV3570 (manufactured by BYK Chemie, an acryloyl group-containing polyester-modified polydimethylsiloxane compound).

[0045] Component (D) generates radicals when irradiated with ultraviolet light, electron beams, or the like. The generated radicals trigger the polymerization reaction of the photocurable resin composition. Examples of component (D) include general-purpose photopolymerization initiators such as benzyl ketal-based, acetophenone-based, and phosphine oxide-based photopolymerization initiators.

[0046] By arbitrarily selecting the light absorption wavelength of component (D), it is possible to impart curability to the photocurable resin composition over a wide wavelength range from the ultraviolet region to the visible light region.

[0047] Examples of the benzyl ketal (D) component include 2,2-dimethoxy-1,2-diphenylethan-1-one. Examples of the α-hydroxyacetophenone (D) component include 1-hydroxycyclohexylphenyl ketone and 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one.

[0048] Examples of the α-aminoacetophenone (D) component include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one. Examples of the acylphosphine oxide (D) component include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide and bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide. These can be used alone or in combination of two or more as the (D) component.

[0049] Component (D) preferably contains an α-hydroxyacetophenone-based compound that is resistant to yellowing. Commercially available products of component (D) include Omnirad 127D, Omnirad 184, and Omnirad 2959 (all manufactured by IGM Resins). The amount of component (D) per 100 parts by weight of the radically polymerizable component in the photocurable resin composition is preferably 2 to 15 parts by weight, and more preferably 5 to 12 parts by weight.

[0050] The photocurable resin composition preferably further contains a light stabilizer (E). The light stabilizer (E) is hereinafter referred to as component (E). When the photocurable resin composition contains component (E), deterioration of the cured resin layer due to exposure to ultraviolet light or radiant heat when the cured resin layer is used outdoors can be suppressed.

[0051] Examples of the component (E) include a radical scavenger (e1) and an ultraviolet absorber (e2). Hereinafter, (e1) and (e2) will be referred to as the component (e1) and the component (e2), respectively.

[0052] Component (e1) efficiently traps alkyl radicals and peroxy radicals generated from polymers photodegraded by ultraviolet light, while component (e2) converts the energy of absorbed ultraviolet light into thermal energy, thereby inhibiting polymer decomposition.

[0053] Examples of the (e1) component include hindered amine-based (hereinafter referred to as HALS-based), hindered phenol-based, and aromatic amine-based compounds. These can be used alone or in combination of two or more types as the (e1) component. Among these, HALS-based compounds are preferred. HALS-based compounds have high radical scavenging efficiency even at low concentrations.

[0054] The blending amount of component (e1) is preferably 1 to 10 wt %, more preferably 2 to 8 wt %, and particularly preferably 3 to 6 wt %, based on the total solid content of the photocurable resin composition. When the blending amount of component (e1) is within this range, the light stability of the cured resin layer is further improved. Commercially available HALS-based products of component (e1) include Tinuvin 123 and Tinuvin 249 (both manufactured by BASF Japan Ltd.).

[0055] The component (e2) is a radical chain initiation inhibitor having an absorption band in the region of harmful high-energy ultraviolet light. When the photocurable resin composition contains the component (e2) and the component (e1), the weather resistance of the cured resin layer is further improved, and the cured resin layer is further stabilized.

[0056] Examples of the component (e2) include benzotriazoles, triazines, benzophenones, etc. These may be used alone or in combination of two or more as the component (e2).

[0057] Hydroxyphenyltriazines are preferred as component (e2). Hydroxyphenyltriazines can strongly absorb the long wavelength portion of ultraviolet light. The amount of component (e2) is preferably 0.3 to 5 wt %, more preferably 0.5 to 3 wt %, and particularly preferably 0.6 to 1.5 wt %, based on the total solid content of the photocurable resin composition. When the amount of component (e2) is within this range, the ultraviolet absorption properties of the cured resin layer are further improved.

[0058] The total amount of the component (e1) and the component (e2) is preferably 1 to 12 wt %, more preferably 1.5 to 10 wt %, and particularly preferably 4 to 8 wt %, based on the total solid content of the photocurable resin composition.

[0059] When the total amount is 1% by weight or more, the weather resistance of the cured resin layer is further improved. When the total amount is 12% by weight or less, the amounts of the (e1) and (e2) components are not excessive, and the adhesion between the plastic substrate and the cured resin layer is further improved. The total amount of the (e1) and (e2) components is, for example, the amount of the (E) component. Commercially available products of the (e2) component include Tinuvin 460 and Tinuvin 477 (both manufactured by BASF Japan).

[0060] The photocurable resin composition may contain, as necessary, a reactive diluent, an adhesion promoter, a bluing agent, a pigment, an antifoaming agent, a thickener, an anti-suspending agent, an antistatic agent, an antifogging agent, an antibacterial agent, a wax, a matting agent, a hydrophilic agent, a water-repellent agent, an inorganic filler, organic fine particles, and the like, within a range that does not excessively impair the performance of the photocurable resin composition.

[0061] The reactive diluent is preferably a polyfunctional (meth)acrylate. Polyfunctional (meth)acrylates have low viscosity and excellent compatibility with component (A). Among polyfunctional (meth)acrylates, bifunctional ones include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, and dicyclopentanyl diacrylate.

[0062] Among the polyfunctional (meth)acrylates, trifunctional ones include trimethylolpropane tri(meth)acrylate and pentaerythritol tri(meth)acrylate.

[0063] Among the polyfunctional (meth)acrylates, examples of tetrafunctional ones include ditrimethylolpropane tetra(meth)acrylate, pentaerythritol tetra(meth)acrylate, diglycerin tetra(meth)acrylate, etc. Among the polyfunctional (meth)acrylates, examples of pentafunctional ones include dipentaerythritol penta(meth)acrylate, etc.

[0064] Among the polyfunctional (meth)acrylates, examples of hexafunctional ones include dipentaerythritol hexa(meth)acrylate, etc. These can be used alone or in combination of two or more as the reactive diluent.

[0065] The amount of reactive diluent blended is preferably 20 parts by weight or less, more preferably 15 parts by weight or less, per 100 parts by weight of component (A). When the amount of reactive diluent blended is 20 parts by weight or less, the reactivity of the photocurable resin composition can be improved while ensuring the moldability of the resin cured layer. The amount of reactive diluent blended is preferably 15% by weight or less, more preferably 10% by weight or less, based on the total solid content of the photocurable resin composition.

[0066] When the photocurable resin composition is applied to a plastic substrate, the photocurable resin composition can be diluted with a solvent. When the photocurable resin composition is diluted with a solvent, the coating properties of the photocurable resin composition are improved.

[0067] Examples of the solvent include alcohol solvents, ketone solvents, ester solvents, ether solvents, hydrocarbon solvents, etc. Examples of the alcohol solvent include ethanol, n-propyl alcohol, isopropyl alcohol, n-butyl alcohol, isobutyl alcohol, diacetone alcohol, etc.

[0068] Examples of ketone solvents include acetone, MEK, methyl isobutyl ketone, cyclohexanone, etc. Examples of ester solvents include ethyl acetate, butyl acetate, etc.

[0069] Examples of the ether solvent include propylene glycol monomethyl ether (hereinafter referred to as PGM), diethyl ether, diisopropyl ether, etc. Examples of the hydrocarbon solvent include cyclohexane, methylcyclohexane, etc.

[0070] These solvents can be used alone or in combination of two or more. The weight ratio of the solids in the photocurable resin composition after dilution with a solvent is not particularly limited and is, for example, 10 to 70 wt %. The weight ratio of the solids in the photocurable resin composition after dilution with a solvent can be appropriately set so that the photocurable resin composition has a viscosity that makes it easy to apply.

[0071] Examples of plastic substrates onto which the photocurable resin composition is applied include polyester substrates, triacetyl cellulose substrates, polycarbonate (hereinafter referred to as PC) substrates, polysulfone substrates, nylon substrates, cycloolefin substrates, acrylic (hereinafter referred to as PMMA) substrates, polyimide substrates, acrylonitrile butadiene styrene (hereinafter referred to as ABS) substrates, polyolefin substrates, PVC substrates, PVA substrates, etc. The form of the plastic substrate is, for example, a film.

[0072] As the plastic substrate, a composite substrate of a PC substrate and an acrylic substrate (hereinafter referred to as a PC-acrylic composite substrate) is preferred. The PC substrate has excellent impact resistance and high heat resistance, while the acrylic substrate has high transparency and high hardness.

[0073] The PC acrylic composite substrate is a resin laminate in which an acrylic substrate is laminated on at least one surface of a PC substrate. The PC substrate and the acrylic substrate are preferably laminated by co-extrusion molding.

[0074] The plastic substrate can be subjected to a surface treatment. Examples of the surface treatment include a surface roughening treatment and a surface oxidation treatment. Examples of the surface roughening treatment include a primer treatment, a sandblasting method, and a solvent treatment. Examples of the surface oxidation treatment include a corona discharge treatment, a chromic acid treatment, and an ozone / ultraviolet irradiation treatment. By subjecting the plastic substrate to a surface treatment, the adhesion between the plastic substrate and the cured resin layer is improved.

[0075] The method for applying the photocurable resin composition to the plastic substrate is not particularly limited, and examples of the method for applying the photocurable resin composition to the plastic substrate include known coating methods and printing methods.

[0076] Examples of the coating method include spray coating, roll coating, die coating, air knife coating, blade coating, spin coating, reverse coating, gravure coating, and wire bar coating. Examples of the printing method include gravure printing, screen printing, offset printing, and inkjet printing. The film thickness of the photocurable resin composition is not particularly limited, and is, for example, 1 to 10 μm when dry.

[0077] After applying the photocurable resin composition to a plastic substrate, the photocurable resin composition can be cured by irradiating it with ultraviolet light. Examples of light sources for ultraviolet irradiation include low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, carbon arc lamps, xenon lamps, metal halide lamps, LED lamps, and electrodeless ultraviolet lamps.

[0078] The atmosphere during ultraviolet irradiation may be air or an inert gas such as nitrogen or argon. When ultraviolet irradiation is performed, the curing property of the coating film can be improved by heating the coating film of the photocurable resin composition using a back roll or an IR heater. The conditions for ultraviolet irradiation are not particularly limited. For example, the irradiation intensity of ultraviolet light is 500 to 3000 mW / cm. 2 and the exposure dose is 50 to 400 mJ / cm 2 is.

[0079] 2. Hard-coated film for molding The hard-coated film for molding has a plastic substrate and a cured resin layer. The cured resin layer is formed on the plastic substrate. The cured resin layer is a layer formed by applying a photocurable resin composition to the plastic substrate and curing it.

[0080] The breaking elongation of the hard-coated film for molding is preferably 50% or more, more preferably 100% or more, and particularly preferably 200% or more in an atmosphere of 130° C. When the breaking elongation is 50% or more, the formability of the hard-coated film for molding is further improved.

[0081] The moldable hard coat film can be used, for example, for vehicle exterior applications. Examples of vehicle exterior applications include automobile exterior applications. When used for vehicle exterior applications, the moldable hard coat film preferably has a ΔE measured thereon of 1.0 or less, more preferably 0.8 or less, and particularly preferably 0.5 or less.

[0082] The method for measuring ΔE will be described later. ΔE is an index of weather resistance. When the ΔE of the hard coat film for molding is 1.0 or less, damage to the decorative layer caused by ultraviolet light transmitted through the hard coat film for molding can be suppressed. In particular, even when red or blue, which has poor UV resistance, is used in the decorative layer, discoloration of the decorative layer over time can be suppressed when the hard coat film for molding has a ΔE of 1.0 or less.

[0083] A protective film may be laminated to the surface of the hard coat film for molding on which the cured resin layer is formed. The protective film protects the cured resin layer. When the protective film is laminated, scratches on the cured resin layer during the insert molding or out-molding process can be suppressed. As a result, the yield of insert-molded or out-molded products is improved.

[0084] 3. Molding Film The molding film includes a plastic substrate, a cured resin layer, and one or more of a decorative layer, an adhesive layer, and a backing sheet layer. The cured resin layer is formed, for example, on the plastic substrate. The molding film has a configuration in which one or more of a decorative layer, an adhesive layer, and a backing sheet layer are added to a molding hard coat film. The backing sheet layer is a reinforcing layer.

[0085] Examples of the layer structure of the molding film include resin cured layer / substrate / decorative layer / adhesive layer, resin cured layer / decorative layer / substrate / adhesive layer, resin cured layer / substrate / decorative layer / backing sheet layer, resin cured layer / decorative layer / substrate / backing sheet layer, resin cured layer / substrate / adhesive layer / backing sheet layer, resin cured layer / decorative layer / substrate / adhesive layer / backing sheet layer, resin cured layer / substrate / decorative layer / adhesive layer / backing sheet layer, resin cured layer / substrate / decorative layer / adhesive layer / backing sheet layer, etc. The layer structure represented by a layer / b layer / c layer / d layer is a layer structure in which the a layer, b layer, c layer, and d layer are arranged in this order in the thickness direction. The substrate is a plastic substrate.

[0086] The layer structure of the molding film may be different from the layer structure described above. For example, in any of the layer structures described above, at least one of a primer layer and an adhesive layer may be provided between any two layers. When at least one of a primer layer and an adhesive layer is provided between two layers, the adhesion between the layers is improved.

[0087] The decorative layer can be formed by, for example, a known printing method, such as gravure printing using printing ink, offset printing, silk screen printing, transfer printing, or ink jet printing.

[0088] Examples of binders for printing inks include acrylic, polyester, urethane, and vinyl chloride-vinyl acetate copolymer binders. These binders can be used alone or in combination of two or more. Printing inks are prepared by appropriately mixing, in addition to a binder, colorants such as pigments and dyes, stabilizers, plasticizers, curing agents, catalysts, and the like.

[0089] Examples of colorants include inorganic pigments, organic pigments, metallic pigments, pearl pigments, and fluorescent pigments. Examples of inorganic pigments include titanium white, red iron oxide, and ultramarine. Examples of organic pigments include Hansa Yellow A and phthalocyanine blue. Examples of metallic pigments include aluminum and brass. These colorants can be used alone or in combination of two or more.

[0090] The decorative layer may also be formed by vacuum deposition, sputtering, electroless plating, etc. In this case, metals such as aluminum, indium, chromium, nickel, gold, and silver can be used.

[0091] When printing ink is used, the thickness of the decorative layer is preferably 3 to 50 μm, more preferably 5 to 30 μm. When the thickness of the decorative layer is within this range, the decorative layer has high concealing properties. Furthermore, when the thickness of the decorative layer is within this range, complex designs such as gradations can be fully expressed.

[0092] The adhesive layer is, for example, a pressure-sensitive adhesive layer. The adhesive layer contains, for example, an adhesive polymer such as an acrylic, polyolefin, rubber, polyester, silicone, or polyurethane. The adhesive polymer may be crosslinked with, for example, an isocyanate, epoxy, or metal chelate crosslinking agent.

[0093] The adhesive layer may be thermosetting, thermoplastic, or photocurable. The adhesive layer is preferably acrylic. Acrylic adhesive layers have high transparency and weather resistance. The adhesive layer is more preferably crosslinked acrylic. The adhesive layer may contain a tackifier.

[0094] The adhesive layer can be formed using a known method, for example, using a gravure coater, a flexo coater, a roll coater, a knife coater, a comma coater, etc. Alternatively, a pressure-sensitive adhesive layer previously formed into a sheet shape may be laminated.

[0095] The thickness of the adhesive layer is preferably 10 to 100 μm, more preferably 20 to 80 μm, and particularly preferably 25 to 60 μm. When the thickness of the adhesive layer is 10 μm or more, the adhesion between the molding film and the adherend is improved. When the thickness of the adhesive layer is 100 μm or less, the adhesive layer can be prevented from protruding from the edge of the molding film in a high-temperature environment. Furthermore, when the thickness of the adhesive layer is 100 μm or less, a decrease in the pencil hardness of the molding film can be prevented.

[0096] The backing sheet layer imparts stiffness to the molding film during insert molding. By imparting stiffness to the molding film, the molding film becomes easier to handle during preforming. The backing sheet layer also improves adhesion between the injection molding resin and the molding film. The backing sheet layer also suppresses thermal damage during injection. The backing sheet layer also improves the effect of concealing the underlying surface.

[0097] Examples of materials for the backing sheet layer include polyethylene-based, polypropylene-based, polyester-based, polyurethane-based, polyvinyl chloride-based, ABS-based, etc. The backing sheet layer may be colored.

[0098] The heat distortion temperature of the backing sheet layer is preferably 85 to 120°C. The heat distortion temperature is the deflection temperature under load. When the heat distortion temperature is 85°C or higher, deformation and distortion of the molding film due to heat when drying the printing ink of the decorative layer can be suppressed.

[0099] When the heat distortion temperature is 120°C or less, the temperature of the molding film does not need to be high when preforming the molding film. Therefore, variations in the elongation and distortion of the molding film during preforming can be suppressed. Polypropylene, ABS-based materials, etc. are preferred as materials for the backing sheet layer. The deflection temperature under load of polypropylene is 100°C. The deflection temperature under load of ABS-based materials is 95°C.

[0100] 4. Insert molding Insert molding can be performed using a molding film. For example, the molding film is placed so that the surface on which the cured resin layer is formed faces the inner wall surface of the mold.

[0101] At this time, if necessary, the molding film may be preformed so that it conforms to the shape of the mold. Next, the mold is closed and a molten injection molding resin is injected into the cavity. The molten injection molding resin corresponds to the molten resin.

[0102] At this time, the injection molding resin is injected into the molding film from the side opposite the resin cured layer. The side of the molding film opposite the resin cured layer comes into contact with the injection molding resin. The resin is then cooled and solidified to form an insert molded product. The insert molded product is a resin molded product.

[0103] One method of preforming is to preheat a molding film to a temperature above its softening point, place it in a mold, and vacuum-suck the molding film through suction holes in the mold. Alternatively, preforming can be performed using a molding mold separate from the injection molding mold by a known molding method such as vacuum forming, pressure forming, or press molding.

[0104] On the other hand, preforming may not be necessary, in which case the molding film and the injection resin can be molded together at the same time by the injection pressure of the injection molding resin.

[0105] As the injection molding resin, known resins that can be injection molded can be used. Examples of injection molding resins include polyethylene resin, polypropylene resin, polystyrene resin, ABS resin, AS resin, acrylic resin, urethane resin, polyester resin, polycarbonate resin, polyphenylene ether resin, polyacetal resin, and polysulfone resin. As the injection molding resin, these can be used alone or in combination of two or more.

[0106] When the insert-molded article is an automobile body or the like, the size of the insert-molded article is large. When the size of the insert-molded article is large, or when the size of the insert-molded article is small but the thickness is thin, it is preferable to make the shrinkage rate of the insert-molded article after insert molding similar to the shrinkage rate of the molding film. In this case, defects such as warping in the insert-molded article can be suppressed.

[0107] When insert molding is performed, the surface of the molding film that comes into close contact with the injection molding resin is preferably a backing sheet layer or an adhesive layer.

[0108] The injection-molded resin can be colored. In this case, the molding film does not need to have a decorative layer. Also, by coloring the injection-molded resin and blending the color of the decorative layer with the color of the injection-molded resin, the appearance of the insert-molded product can be made more sophisticated.

[0109] Insert-molded products can be used, for example, as a replacement for products whose outer surfaces are painted. Examples of products whose outer surfaces are painted include automobile bodies. By coloring the injection-molded resin, the process of coloring the outer surface of the insert-molded product with paint can be omitted. In this case, it is possible to suppress appearance defects such as orange peel and pits that occur during the process of coloring the outer surface with paint.

[0110] 5. Out-mold molding Out-mold molding can be performed using a molding film. For example, TOM (Three-Dimensional Overlay Method) molding can be performed using a molding film. TOM molding is a film molding method in which a pre-formed substrate is subjected to three-dimensional surface decoration by vacuum forming or pressure forming inside an airtight box. When TOM molding is performed using a molding film, large three-dimensional products can be produced regardless of the material of the substrate.

[0111] When TOM molding is performed using a molding film, the surface of the molding film that comes into close contact with the molded article is preferably an adhesive layer.

[0112] 6. Examples The present disclosure will be described in detail below with examples and comparative examples, but these are intended to be specific examples and are not intended to be limiting. Unless otherwise specified, measurements were performed under conditions of a temperature of 25°C and a relative humidity of 65%. The blend amounts are values ​​calculated as solid content. The blend amounts are expressed in parts by weight.

[0113] (6-1) Preparation of Urethane Acrylate (i) Preparation of Urethane Acrylate 1 Into a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer, 200 parts by weight of ethylene glycol, 825 parts by weight of IPDI (NCO group 37.5%), a catalyst, and MEK were added so that the weight ratio of solids was 50% by weight. Next, the mixture was stirred at 80°C for 6 hours to react. The reaction was terminated when the peak of the isocyanate group in infrared absorption analysis reached a predetermined amount.

[0114] Next, 438 parts by weight of PETA (hydroxyl value 120 mg KOH / g) was added, and the mixture was stirred at 70 ° C for 6 hours. After the reaction, it was confirmed by infrared absorption analysis that the isocyanate groups had disappeared. Next, MEK was added to adjust the weight ratio of the solids to 50%. Through the above process, a hexafunctional urethane acrylate 1 with Mw of 6,200 was obtained.

[0115] (ii) Preparation of Urethane Acrylate 2: 200 parts by weight of ethylene glycol, 930 parts by weight of IPDI (NCO group 37.5%), a catalyst, and MEK were added to a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer so that the weight ratio of the solid content was 50%. The mixture was then stirred at 80°C for 6 hours to react. The reaction was terminated when the peak of the isocyanate group reached a predetermined level in infrared absorption analysis.

[0116] Next, 886 parts by weight of PETA (hydroxyl value 120 mg KOH / g) was added, and the mixture was stirred at 70 ° C for 6 hours. After the reaction, it was confirmed by infrared absorption analysis that the isocyanate groups had disappeared. Next, MEK was added to adjust the weight ratio of the solids to 50%. Through the above process, a hexafunctional urethane acrylate 2 with Mw of 3,200 was obtained.

[0117] (iii) Preparation of Urethane Acrylate 3: 200 parts by weight of ethylene glycol, 895 parts by weight of IPDI (NCO group 37.5%), a catalyst, and MEK were added to a four-neck flask equipped with a stirrer, reflux condenser, dropping funnel, and thermometer so that the weight ratio of the solid content was 50%. The mixture was then stirred at 80°C for 6 hours to react. The reaction was terminated when the peak of the isocyanate group reached a predetermined level in infrared absorption analysis.

[0118] Next, 743 parts by weight of PETA (hydroxyl value 120 mg KOH / g) was added, and the mixture was stirred at 70 ° C for 6 hours. After the reaction, it was confirmed by infrared absorption analysis that the isocyanate groups had disappeared. Next, MEK was added to adjust the weight ratio of the solids to 50%. Through the above process, a hexafunctional urethane acrylate 3 with Mw of 3,800 was obtained.

[0119] (iv) Preparation of Urethane Acrylate 4: 200 parts by weight of ethylene glycol, 790 parts by weight of IPDI (NCO group 37.5%), a catalyst, and MEK were added to a four-neck flask equipped with a stirrer, a reflux condenser, a dropping funnel, and a thermometer so that the weight ratio of the solid content was 50%. The mixture was then stirred at 80°C for 6 hours to react. The reaction was terminated when the peak of the isocyanate group reached a predetermined level in infrared absorption analysis.

[0120] Next, 295 parts by weight of PETA (hydroxyl value 120 mg KOH / g) was added, and the mixture was stirred at 70 ° C for 6 hours. After the reaction, the disappearance of the isocyanate groups was confirmed by infrared absorption analysis. Next, MEK was added to adjust the solid content to 50%. Through the above process, a hexafunctional urethane acrylate 4 with Mw of 9,800 was obtained.

[0121] (v) Preparation of Urethane Acrylates A and B Urethane acrylates A and B were prepared by a method basically similar to the preparation method of Urethane Acrylates 1 to 3. The skeletons of Urethane Acrylates A and B were the same as those of Urethane Acrylates 1 to 3. The skeletons of Urethane Acrylates A and B were PETA-IPDI-(ethylene glycol-IPDI)n-PETA skeletons.

[0122] Urethane acrylate A was hexafunctional. The weight ratio of the solid content in urethane acrylate A was 50% by weight. The Mw of urethane acrylate A was 1,800. Urethane acrylate B was hexafunctional. The weight ratio of the solid content in urethane acrylate B was 50% by weight. The Mw of urethane acrylate A was 13,000.

[0123] (6-2) Production of Photocurable Resin Compositions The photocurable resin compositions of Examples 1 to 11 and Comparative Examples 1 to 5 were produced by the following method: First, the components shown in Tables 1 to 3 were mixed in the formulations shown in Tables 1 to 3.

[0124]

[0125]

[0126] The unit of blending amount in Tables 1 to 3 is parts by weight. In Tables 1 to 3, "ureac" means urethane acrylate. "A" in Tables 1 to 3 means component (A). Urethane acrylates 1 to 4 correspond to component (A). "B" in Tables 1 to 3 means component (B). In Tables 1 to 3, among the "B" rows, the components listed in the rows "average particle size 70 nm," "average particle size 100 nm," "average particle size 50 nm," and "average particle size 25 nm" are alumina fine particles with an average particle size of 70 nm, alumina fine particles with an average particle size of 100 nm, alumina fine particles with an average particle size of 50 nm, and alumina fine particles with an average particle size of 25 nm, respectively.

[0127] "C" in Tables 1 to 3 refers to component (C). BYK-UV3570 corresponds to component (C). BYK-UV3570 is the trade name of an acryloyl group-containing polyester-modified polydimethylsiloxane compound manufactured by BYK Chemie.

[0128] "D" in Tables 1 to 3 refers to component (D). Omnirad 2959 and Omnirad 127D each correspond to component (D). Omnirad 2959 and Omnirad 127D are trade names of products manufactured by IGM Resins.

[0129] "E" in Tables 1 to 3 refers to component (E). Tinuvin 249 and Tinuvin 477 each correspond to component (E). Tinuvin 249 corresponds to component (e1). Tinuvin 477 corresponds to component (e2). Tinuvin 249 and Tinuvin 477 are each the trade names of products manufactured by BASF Japan Ltd.

[0130] PGM-AC-4130Y in Tables 1 to 3 is a filler made of nanosilica. The average particle size of PGM-AC-4130Y is 40 to 50 nm. PGM-AC-4130Y is the trade name of a product manufactured by Nissan Chemical Industries, Ltd.

[0131] Next, the mixture was stirred until it was uniformly dissolved and dispersed. Next, PGM was added to dilute the mixture so that the weight ratio of the solid content was 30% by weight, and the mixture was further stirred. By the above steps, the photocurable resin compositions of Examples 1 to 11 and Comparative Examples 1 to 5 were obtained.

[0132] (6-3) Production of Hard Coat Film for Molding Hard coat films for molding were produced from the photocurable resin compositions of each of the Examples and Comparative Examples by the following method.

[0133] A plastic substrate was prepared. The plastic substrate was Iupilon Film DF02PUL (trade name, manufactured by Mitsubishi Gas Chemical Company, Inc.). The thickness of the plastic substrate was 125 μm. The plastic substrate was a laminated film in which a PMMA layer and a PC layer were laminated.

[0134] A photocurable resin composition was applied to the PMMA layer side of the plastic substrate. The dry film thickness of the photocurable resin composition was 3 μm. Next, it was dried in a thermostatic chamber at 80°C for 1 minute. Next, the coating film of the photocurable resin composition was irradiated with ultraviolet light using a high-pressure mercury lamp. The output of the high-pressure mercury lamp was 1300 mW / cm. 2 The integrated light intensity of the ultraviolet rays was 200 mJ. The coating film of the photocurable resin composition became a cured resin layer. Through the above steps, a hard coat film for molding was obtained.

[0135] Hereinafter, the moldable hard-coated film produced using the photocurable resin composition of Example 1 will be referred to as the moldable hard-coated film of Example 1. The same applies to the moldable hard-coated films produced using the photocurable resin compositions of Examples 2 to 11 and Comparative Examples 1 to 5.

[0136] The structure of the hard-coated molding film 1 of each example and comparative example is shown in Figure 1. The hard-coated molding film 1 includes a plastic substrate 3 and a cured resin layer 5. The cured resin layer 5 is formed on the plastic substrate 3.

[0137] (6-4) Evaluation Method of Hard Coat Film for Forming The hard coat films for forming of each Example and Comparative Example were evaluated as follows.

[0138] (i) Chemical Resistance Hand cream was applied to the resin-cured layer of the moldable hard coat film. The hand cream was Neutrogena SPF 45 (trade name, manufactured by Johnson & Johnson). Next, the moldable hard coat film was left at 80°C for 24 hours. Then, the temperature was returned to room temperature. Next, the hand cream was wiped off. Next, the surface of the portion of the resin-cured layer from which the hand cream had been wiped off was observed. Based on the observation results, the chemical resistance of the resin-cured layer was evaluated according to the following criteria. ○ indicates a better evaluation result than ×.

[0139] ◯: No trace of coating on the cured resin layer.

[0140] ×: Traces of coating found on the cured resin layer.

[0141] (ii) Abrasion Resistance Evaluation was carried out using a friction tester FR-IBS manufactured by Suga Test Instruments. During the evaluation, a friction element with a test white cotton cloth attached was brought into contact with the resin cured layer of the hard coat film for molding under a load of 9 N, and the friction element was reciprocated 100 times. The test white cotton cloth was Kanakin No. 3. The diameter of the friction element was 16 mm. The reciprocation speed was 1 reciprocation per second.

[0142] After 100 reciprocations, the surface of the cured resin layer was observed and the abrasion resistance of the cured resin layer was evaluated according to the following criteria: ◯ indicates a better evaluation result than ×.

[0143] ◯: No scratches on the cured resin layer.

[0144] ×: Scratches on the resin cured layer.

[0145] (iii) Adhesion Evaluation was performed in accordance with the cross-cut method of JIS K 5600-5-6. A 10 x 10 grid was created at 1 mm intervals on the resin cured layer of the molding hard coat film. Next, cellophane tape CT-24 (trade name, manufactured by Nichiban Co., Ltd.) was attached to the resin cured layer with the grid, and the cellophane tape CT-24 was pulled upward. Next, the peeling state of the resin cured layer was observed, and the adhesion was evaluated according to the following criteria. ○ is an evaluation result better than ×.

[0146] ◯: The cured resin layer was not peeled off in any of the 100 squares.

[0147] x: The cured resin layer peeled off in one or more of the 100 squares.

[0148] (iv) Moldability A rectangular test piece was cut out from the moldable hard coat film. The length of the short side of the rectangle was 25 mm, and the length of the long side was 110 mm. A tensile test was performed on this test piece using a TechnoGraph TGI-1KN manufactured by Minebea Co., Ltd. In the tensile test, the distance between chucks was 50 mm. The ambient temperature was 130°C. The tensile speed was 300 mm / min.

[0149] After the tensile test, the test pieces were visually inspected for cracks. Based on the fracture elongation G (%) calculated by the following formula (1), the formability was evaluated according to the following criteria: ◎ is the best evaluation result; ○ is the second best evaluation result; △ is the third best evaluation result; × is the worst evaluation result.

[0150] G=(Δ / 50)×100 Formula (1) Δ in formula (1) is the length (mm) of extension of the test piece when the test piece breaks in the tensile test.

[0151] ⊚: Breaking elongation G exceeds 200%.

[0152] Good: The breaking elongation G is greater than 100% and not more than 200%.

[0153] Δ: The breaking elongation G is 50% or more and 100% or less.

[0154] ×: The breaking elongation G is less than 50%.

[0155] (v) Scratch Resistance An abrasion test was performed using an abrasion tester manufactured by Toyo Seiki Seisakusho. In the abrasion test, steel wool #0000 was brought into contact with the cured resin layer of the hard coat film from above. A load of 500 g was then placed on the steel wool. The contact area between the cured resin layer and the steel wool was 4 cm. 2 In this state, the steel wool was moved back and forth 10 times at a speed of 30 times per minute.

[0156] The haze of the cured resin layer before the abrasion test and the haze of the cured resin layer after the abrasion test were measured. The haze measurement method was a method conforming to JIS K7136. Haze-GARD2 manufactured by Toyo Seiki Seisakusho was used for measuring the haze. The increase rate of the haze of the cured resin layer after the abrasion test relative to the haze of the cured resin layer before the abrasion test was defined as the increase rate of the haze. Based on the increase rate of the haze, the scratch resistance of the cured resin layer was evaluated according to the following criteria. ○ indicates a better evaluation result than ×.

[0157] Good: The increase in haze is less than 5%.

[0158] ×: The rate of increase in haze is 5% or more.

[0159] (vi) Car Wash Scratch Resistance An abrasion test was conducted in accordance with DIN EN ISO 20566 using a car wash abrasion resistance tester (manufactured by Amtec Kistler GmbH). The gloss g1 of the cured resin layer before the abrasion test and the gloss g2 of the cured resin layer after the abrasion test were measured using a micro-tri-gloss (manufactured by BYK). The gloss measurement angle was 20°. The gloss retention rate Y (%) was calculated using the following formula (2):

[0160] (Formula 2) Y = (g2 / g1) x 100 Based on the gloss retention rate Y, the car wash scratch resistance of the cured resin layer was evaluated according to the following criteria: ⊚ is the best evaluation result; ◯ is an evaluation result inferior to ⊚ but better than ×.

[0161] ⊚: Gloss retention Y exceeds 75%.

[0162] Good: The gloss retention rate Y is 50% or more and 75% or less.

[0163] ×: Gloss retention Y is less than 50%.

[0164] (6-5) Evaluation Results of Hard Coat Films for Forming The evaluation results of the hard coat films for forming of each Example and each Comparative Example are shown in Tables 4 to 6. In Tables 4 to 6, the numerical value listed in the row for formability is the breaking elongation G. In Tables 4 to 6, the numerical value listed in the row for scratch resistance is the rate of increase in haze. In Tables 4 to 6, the numerical value listed in the row for car wash scratch resistance is the gloss retention rate Y.

[0165]

[0166]

[0167] The moldable hard coat films of each Example were excellent in all of chemical resistance, abrasion resistance, adhesion, moldability, scratch resistance, and car wash scratch resistance. The reason why the moldable hard coat films of each Example were excellent in car wash scratch resistance is because the photocurable resin composition of each Example contained component (B).

[0168] The photocurable resin compositions of Examples 1 to 7 and 9 to 11 contained component (B) having an average particle size of 50 to 100 nm. The molding hard coat films of Examples 1 to 7 and 9 to 11 were particularly good in car wash scratch resistance.

[0169] The photocurable resin composition of Comparative Example 1 did not contain component (C). The hard coat film for molding of Comparative Example 1 was inferior in abrasion resistance, scratch resistance, and car wash scratch resistance. The photocurable resin composition of Comparative Example 2 did not contain component (B). The hard coat film for molding of Comparative Example 2 was inferior in scratch resistance and car wash scratch resistance.

[0170] The photocurable resin composition of Comparative Example 3 did not contain component (B) but contained nanosilica having an average particle size of 40 to 50 nm. The hard coat film for molding of Comparative Example 3 was poor in abrasion resistance, scratch resistance, and car wash scratch resistance.

[0171] In the photocurable resin composition of Comparative Example 4, the Mw of component (A) was less than 2,000. In addition, in the hard-coated molding film of Comparative Example 4, the breaking elongation G was less than 50%. The hard-coated molding film of Comparative Example 4 was poor in moldability.

[0172] In the photocurable resin composition of Comparative Example 5, the Mw of component (A) exceeded 12,000. In addition, in the hard coat film for molding of Comparative Example 5, the gloss retention rate Y was less than 50%. The hard coat film for molding of Comparative Example 5 was poor in abrasion resistance, scratch resistance, and car wash scratch resistance.

[0173] (6-6) Evaluation of Weather Resistance Basically in the same manner as in Example 2, hard-coated films F1 to F5 for molding shown in Table 7 were produced.

[0174] In Table 7, "molding HC film" means a molding hard coat film. Molding hard coat film F1 was the molding hard coat film of Example 2. Molding hard coat film F2 was basically the same as the molding hard coat film of Example 2, but the photocurable resin composition of Example 1 was used to form the resin cured layer.

[0175] The hard coat film for molding F3 was basically the same as the hard coat film for molding in Example 2, but a polycarbonate film (trade name: PC-1151, manufactured by Teijin Ltd.) was used as the plastic substrate. The thickness of the plastic substrate in the hard coat film for molding F3 was 200 μm.

[0176] The hard coat film for molding F4 was basically the same as the hard coat film for molding in Example 2, but an acrylic film (product name: HBA007P, manufactured by Mitsubishi Chemical Corporation) was used as the plastic substrate. The thickness of the plastic substrate in the hard coat film for molding F4 was 125 μm.

[0177] The hard-coated molding film F5 was basically the same as the hard-coated molding film of Example 2, but a PET film (product name: U403, manufactured by Toray Industries, Inc.) was used as the plastic substrate. The thickness of the plastic substrate in the hard-coated molding film F5 was 125 μm.

[0178] ΔE was measured for each of the hard coat films for molding F1 to F5. The method for measuring ΔE was as follows: Using a color difference meter SD-6000 manufactured by Nippon Denshoku Industries Co., Ltd., the color of the hard coat film for molding before irradiation with UVB was measured in accordance with JIS Z 8722.

[0179] Next, the hard coat film for molding was irradiated with UVB for 1000 hours at 60°C. The intensity of the UVB was 0.55 W / m 2 After UVB irradiation, the color of the hard coat film for molding was measured again in accordance with JIS Z 8722 using a color difference meter SD-6000 manufactured by Nippon Denshoku Industries Co., Ltd. The difference between the color before UVB irradiation and the color after UVB irradiation was taken as ΔE. The smaller the ΔE, the better the weather resistance of the hard coat films for molding F1 to F5. The ΔE of the hard coat films for molding F1 to F5 is shown in the row "ΔE of HC film for molding" in Table 7.

[0180] The ΔE of the plastic substrates used in the hard coat films F1 to F5 was also measured in the same manner. The smaller the ΔE, the better the weather resistance of the plastic substrate. The ΔE of the plastic substrates is shown in the "ΔE of the substrate alone" row in Table 7.

[0181] The ΔE of the hard coat films for molding F1 to F5 was significantly affected by the type of plastic substrate. By using a plastic substrate with a small ΔE, the ΔE of the hard coat films for molding F1 to F5 can be suppressed.

[0182] The photocurable resin composition of Example 2 contains component (E). In the hard coat films F1, and F3 to F5 for molding, the cured resin layer is formed using the photocurable resin composition of Example 2. The hard coat films F1, and F3 to F5 for molding had small ΔE and good weather resistance.

[0183] (6-7) Evaluation of Injection Molding Insert molding was performed using the hard-coated film for molding of Example 1. The injection molding resin used for insert molding was black ABS. An insert-molded product was obtained by insert molding.

[0184] Using a BYK painted surface texture measuring instrument Wave Scan 3 Dual, LW (long wave) and SW (short wave) were measured for the film surface of the insert molded article. Similar measurements were also performed on the painted surface of a painted steel plate as a comparative example. The measurement results for LW and SW are shown in the "Wave Scan" row in Table 8. The appearance of each of the insert molded article and the painted steel plate was also observed. The observation results for appearance are shown in the "Evaluation" row in Table 8.

[0185] The coated steel sheet had an appearance defect called "yellow peel," whereas the insert molded product did not have this appearance defect.

[0186] (6-8) Evaluation of molding films Molding films F11 to F16 were produced, each having the layer structure shown in Table 9. Molding films F11 to F16 have a layer structure in which the fourth layer, third layer, second layer, and top layer shown in Table 9 are arranged in that order in the thickness direction.

[0187] In Table 9, "substrate" refers to a plastic substrate. The layer structures of molding films F11 to F12 and F15 are shown in Figure 2A. Molding films F11 to F12 and F15 each include a plastic substrate 3, a resin cured layer 5, a decorative layer 7, and an adhesive layer 9. The resin cured layer 5 is formed on one main surface of the plastic substrate 3. The decorative layer 7 and adhesive layer 9 are formed on the other main surface of the plastic substrate 3. The decorative layer 7 is formed between the plastic substrate 3 and the adhesive layer 9.

[0188] The layer structure of molding films F13 to F14 and F16 is shown in Figure 2B. Molding films F13 to F14 and F16 each include a plastic substrate 3, a cured resin layer 5, a decorative layer 7, and an adhesive layer 9. The adhesive layer 9 is formed on one main surface of the plastic substrate 3. The cured resin layer 5 and the decorative layer 7 are formed on the other main surface of the plastic substrate 3. The decorative layer 7 is formed between the plastic substrate 3 and the cured resin layer 5.

[0189] In all of the molding films F11 to F16, the plastic substrate was Iupilon Film DF02PUL (trade name, manufactured by Mitsubishi Gas Chemical Company, Inc.).

[0190] In molding films F11 and F13, the resin cured layer was a layer formed using the photocurable resin composition of Example 1. In molding films F12 and F14, the resin cured layer was a layer formed using the photocurable resin composition of Example 2. In molding films F15 and F16, the resin cured layer was a layer formed using the photocurable resin composition of Comparative Example 4.

[0191] In all of the molding films F11 to F16, the curing conditions for curing the resin cured layer were the same as the curing conditions for producing the molding hard coat film in the above section (6-3).

[0192] For all of the molding films F11 to F16, the decorative layer was formed using IPX-HF (trade name, manufactured by Teikoku Ink Co., Ltd.). The dry thickness of the decorative layer was 20 μm. When forming the decorative layer, after applying IPX-HF, it was dried at 80°C for 10 minutes. It was then cured at 90°C for 60 minutes.

[0193] In all of the molding films F11 to F16, the adhesive layer was formed using Ultrasol OP-3511 (trade name, manufactured by Aica Kogyo Co., Ltd.). Ultrasol OP-3511 was a crosslinked acrylic. The dry thickness of the adhesive layer was 30 μm. When forming the adhesive layer, after application of Ultrasol OP-3511, the film was cured at 40°C for 2 days.

[0194] Each of the molding films F11 to F16 was subjected to vacuum and pressure molding using a TOM molding machine NGF-T-0203 manufactured by Fuse Vacuum Co., Ltd., as follows. First, the molding film was heated to 150°C. Next, vacuum and pressure molding was performed using a cylindrical mold with a diameter of 30 mm and height of 20 mm under pressure conditions of 300 kPa for 15 seconds.

[0195] Based on the results of vacuum and pressure molding, the moldability of the molding film was evaluated according to the following criteria. The evaluation results of moldability are shown in the "Moldability" row in Table 9. ○ indicates an evaluation result that is better than ×.

[0196] ◯: The molding film was completely shaped.

[0197] ×: Whitening or cracking occurred in the molding film, or the molding film was incompletely shaped.

[0198] For molding films F11 to F14, the resin cured layer was formed using the photocurable resin composition of Example 1 or 2. Molding films F11 to F14 had good moldability. For molding films F15 to F16, the resin cured layer was formed using the photocurable resin composition of Comparative Example 4. Molding films F15 to F16 had poor moldability.

[0199] 7. Effects of the Photocurable Resin Composition, Hard-Coated Molding Film, and Molding Film The photocurable resin composition, hard-coated molding film, and molding film of the present disclosure have high breaking elongation and good moldability. Furthermore, the photocurable resin composition, hard-coated molding film, and molding film of the present disclosure have excellent scratch resistance. The photocurable resin composition, hard-coated molding film, and molding film of the present disclosure are useful, for example, as materials for molded articles used in automotive exterior applications. Examples of molded articles used in automotive exterior applications include roofs, hoods, pillars, fenders, doors, headlamps, front grilles, bumpers, etc.

[0200] 8. Other Embodiments Although the embodiments of the present disclosure have been described above, the present disclosure is not limited to the above-described embodiments and can be implemented in various modifications.

[0201] (1) The function of one component in each of the above embodiments may be shared among multiple components, or the functions of multiple components may be performed by one component. Also, part of the configuration of each of the above embodiments may be omitted. Furthermore, at least part of the configuration of each of the above embodiments may be added to or substituted for the configuration of another of the above embodiments.

[0202] (2) In addition to the above-mentioned molding hard coat film and molding film, the present disclosure can also be realized in various forms, such as a system including any of these as a component, a method for producing a photocurable resin composition, a method for producing a molding hard coat film, a method for producing a molding film, etc. [Technical Concept Disclosed by the Present Specification] [Item 1] A photocurable resin composition comprising: a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate to form a diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the weight-average molecular weight of (A) is 2,000 to 12,000; and the average primary particle diameter of (B) is 40 to 150 nm.

[0203] [Item 2] A photocurable resin composition comprising: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the average primary particle diameter of (B) is 40 to 150 nm; and a film having a substrate and a cured layer of the photocurable resin composition formed on the substrate has a breaking elongation of 50% or more at an ambient temperature of 130°C and a tensile speed of 300 mm / min.

[0204] [Item 3] A photocurable resin composition comprising: a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate to form a diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the weight average molecular weight of (A) is 2,000 to 12,000; and when a film having a substrate and a cured layer of the photocurable resin composition formed on the substrate is subjected to an abrasion test in accordance with DIN EN ISO 20566 using a car wash abrasion tester, the gloss of the cured layer after the abrasion test is 50% or more of the gloss of the cured layer before the abrasion test. [Item 4] The photocurable resin composition according to any one of Items 1 to 3, wherein the leveling agent (C) is a silicone-based compound. [Item 5] The photocurable resin composition according to any one of items 1 to 4, further comprising a light stabilizer (E). [Item 6] A moldable hard coat film having a plastic substrate and a cured layer of the photocurable resin composition according to any one of items 1 to 5, formed on the plastic substrate. [Item 7] A moldable film having a plastic substrate and a cured layer of the photocurable resin composition according to any one of items 1 to 5, formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer. [Item 8] The moldable film according to item 7, which is for use in vehicle exterior applications.[Item 9] A method for producing an insert-molded product, comprising: using a mold to form a molding film having a plastic substrate, a cured layer of a photocurable resin composition formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer; and injecting a molten resin into the molding film from the side opposite the cured layer to form a resin molded product, wherein the photocurable resin composition comprises: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D); wherein the weight-average molecular weight of (A) is 2,000 to 12,000; and the average primary particle diameter of (B) is 40 to 150 nm. [Item 10] A method for producing an out-molded product, comprising vacuum-forming or pressure-forming a molding film having a plastic substrate, a cured layer of a photocurable resin composition formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer, onto a pre-formed substrate, wherein the photocurable resin composition comprises: a urethane acrylate (A) obtained by reacting ethylene glycol with isophorone diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D), wherein the weight-average molecular weight of (A) is 2,000 to 12,000; and the average primary particle diameter of (B) is 40 to 150 nm. [Item 11] A method for producing an out-molded product using the molding film according to Item 7 or 8. [Item 12] An out-molded product using the molding film according to Item 7 or 8.

[0205] 1...Molding hard coat film, 3...Plastic substrate, 5...Resin cured layer, 7...Decorative layer, 9...Adhesive layer, F11 to F16...Molding film

Claims

1. A photocurable resin composition comprising: urethane acrylate (A) obtained by reacting diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate, and further reacting pentaerythritol triacrylate with the diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D); wherein the weight average molecular weight of (A) is 2,000 to 12,000; and the average primary particle diameter of (B) is 40 to 150 nm.

2. A photocurable resin composition comprising: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D); wherein the primary average particle diameter of (B) is 40 to 150 nm; and the breaking elongation of a film having a substrate and a cured layer of the photocurable resin composition formed on the substrate is 50% or more at an ambient temperature of 130°C and a tensile speed of 300 mm / min.

3. A photocurable resin composition comprising: urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with a diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D); wherein the weight average molecular weight of (A) is 2,000 to 12,000; and when an abrasion test conforming to DIN EN ISO20566 is performed on a film having a substrate and a cured layer of the photocurable resin composition formed on the substrate using a car wash abrasion tester, the gloss of the cured layer after the abrasion test is 50% or more of the gloss of the cured layer before the abrasion test.

4. The photocurable resin composition according to any one of claims 1 to 3, wherein the leveling agent (C) is a silicone compound.

5. The photocurable resin composition according to any one of claims 1 to 3, further comprising a light stabilizer (E).

6. A molding hard coat film comprising: a plastic substrate; and a cured layer of the photocurable resin composition according to any one of claims 1 to 3 formed on the plastic substrate.

7. A molding film comprising: a plastic substrate; a cured layer of the photocurable resin composition according to any one of claims 1 to 3 formed on the plastic substrate; and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer.

8. The molding film according to claim 7, which is used for vehicle exterior applications.

9. A method for producing an insert molded product, comprising the steps of: shaping a molding film having a plastic substrate, a cured layer of a photocurable resin composition formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer using a mold; and injecting molten resin into the molding film from the opposite side to the cured layer to form a resin molded product, wherein the photocurable resin composition comprises urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate; alumina fine particles (B); a leveling agent (C); and a photopolymerization initiator (D); wherein the weight average molecular weight of (A) is 2,000 to 12,000; and the primary average particle diameter of (B) is 40 to 150 nm.

10. A method for producing an out-molded product, comprising vacuum forming or pressure-molding a molding film having a plastic substrate, a cured layer of a photocurable resin composition formed on the plastic substrate, and one or more of a decorative layer, a pressure-sensitive adhesive layer, and a backing sheet layer, onto a preformed substrate, wherein the photocurable resin composition comprises urethane acrylate (A) obtained by further reacting pentaerythritol triacrylate with diisocyanate obtained by reacting ethylene glycol with isophorone diisocyanate, alumina fine particles (B), a leveling agent (C), and a photopolymerization initiator (D), wherein the weight average molecular weight of (A) is 2,000 to 12,000, and the primary average particle diameter of (B) is 40 to 150 nm.

11. An insert molded product using the molding film according to claim 7.

12. An out-molded product using the molding film according to claim 7.

Citation Information

Patent Citations

  • Hard coating agent and hard coating film for insert molding

    JP4848200B2

  • Active energy ray-curable oligomer, active energy ray-curable resin composition, cured coating film, and plastic film

    JP2011042770A

  • Curable composition, cured article and laminate

    JP2016060839A

  • Hard coat coating composition and hard coat film for molding