Method for producing ethylene-vinyl alcohol copolymer

The described method addresses efficiency issues in EVOH production by optimizing the saponification process of EVAc in a column reactor with solvent vapor and alkali catalyst, achieving high productivity and quality EVOH with reduced solidification and coloring.

WO2024228377A1PCT designated stage expired Publication Date: 2024-11-07KURARAY CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016633
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2024-04-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

Existing methods for producing ethylene-vinyl alcohol copolymer (EVOH) face efficiency issues due to saponification process limitations, including solvent discharge and solidification of partially saponified ethylene-vinyl acetate copolymer (EVAc) in reactors, leading to decreased productivity during continuous production.

Method used

A method involving saponification of EVAc in a solution using an alkali catalyst to achieve a partially saponified product with a degree of 10-60 mol%, followed by further saponification in a column reactor with solvent vapor and alkali catalyst supply, allowing for efficient production of EVOH with a high saponification degree of 99-100 mol%, using methanol as a solvent and optimizing reaction conditions to prevent solidification and blockages.

Benefits of technology

This method enhances the productivity of EVOH production by preventing solidification and maintaining high efficiency during continuous operation, ensuring high-quality EVOH with improved melt moldability and reduced coloring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure 00000022_0000
    Figure 00000022_0000
Patent Text Reader

Abstract

The method for producing an ethylene-vinyl alcohol copolymer has a step (I) in which an ethylene-vinyl acetate copolymer in a solution of an ethylene-vinyl acetate copolymer is saponified using an alkali catalyst to obtain a solution of a saponified ethylene-vinyl acetate copolymer having a degree of saponification of from 10 mol% to less than 60 mol% and a step (II) in which the solution of the saponified ethylene-vinyl acetate copolymer is supplied to top of a tower reactor (A), solvent vapor is supplied to the lower part and discharged from the top, and an alkali catalyst is supplied below the location at which the solution of the saponified ethylene-vinyl acetate copolymer is supplied to further saponify the saponified ethylene-vinyl acetate copolymer, and a solution of an ethylene-vinyl alcohol copolymer having a degree of saponification of from 99 mol% to 100 mol% obtained is removed from the tower bottom. According to this production method, even when an ethylene-vinyl alcohol copolymer is produced continuously for a long period of time, the ethylene-vinyl acetate copolymer can be saponified efficiently, so that the ethylene-vinyl alcohol copolymer can be produced at good productivity.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing ethylene-vinyl alcohol copolymer

[0001] The present invention relates to a method for producing an ethylene-vinyl alcohol copolymer.

[0002] Ethylene-vinyl alcohol copolymer (hereinafter, sometimes abbreviated as "EVOH") is a useful polymer material that has excellent oxygen barrier properties, oil resistance, antistatic properties, mechanical strength, etc., and is widely used as various packaging materials such as films, sheets, and containers.

[0003] EVOH has conventionally been produced by saponifying ethylene-vinyl acetate copolymer (hereinafter sometimes abbreviated as EVAc) using an alkali catalyst or the like, and methods for improving the saponification process have been proposed in order to improve the productivity and quality of EVOH.

[0004] For example, Patent Document 1 describes a method for producing a saponified EVAc, which includes: (1) a step of saponifying EVAc having an ethylene content of 15 to 60 mol% in an alcohol solvent with an alkali catalyst in a column reactor until the degree of saponification reaches 70 to 98 mol%, thereby obtaining a partially saponified EVAc solution; (2) a step of adding water or a water / alcohol mixture to the partially saponified EVAc solution in a column reactor to form a mixed solution, which is then resaponified in the presence of an alkali catalyst, thereby obtaining a highly saponified EVAc solution having a degree of saponification of 99.4 mol% or more of vinyl acetate; and (3) a step of extruding the highly saponified EVAc solution into a coagulation bath, followed by acid treatment. It is claimed that this method produces pellets of a uniform saponified EVAc that are excellent in melt moldability.

[0005] Patent Document 2 describes a method for producing a saponified EVAc product, which comprises adding an alkali catalyst to an EVAc solution and mixing it, then supplying the resulting EVAc solution having a degree of saponification of 5 mol% or less to the top of a tower reactor, supplying solvent vapor from the bottom of the tower, discharging the solvent vapor from the top of the tower, and supplying an alkali catalyst below the position where the EVAc solution is supplied to saponify the EVAc. It also describes that this production method allows for the prevention of coloration of the saponified EVAc product by previously removing impurities such as vinyl esters and their by-product acetaldehyde before subjecting the EVAc to the saponification reaction.

[0006] Japanese Patent Laid-Open No. 9-67411

[0007] However, in the method described in Patent Document 1, during resaponification, the saponified EVAc is discharged from the tower reactor together with the solvent, which causes a decrease in production efficiency.In addition, in the method described in Patent Document 2, when EVOH is produced continuously over a long period of time, the partially saponified EVAc may solidify in the tower reactor used for saponification, which causes a decrease in production efficiency.

[0008] The present invention has been made to solve the above problems, and an object of the present invention is to provide a highly productive method for producing EVOH, which can efficiently saponify EVAc.

[0009] The above-mentioned problems are solved by providing a method for producing EVOH, which comprises: a step (I) of saponifying EVAc in an EVAc solution with an alkali catalyst to obtain a solution of partially saponified EVAc having a degree of saponification of 10 mol % or more and less than 60 mol %; and a step (II) of supplying the solution of partially saponified EVAc to an upper part of a tower reactor (A), supplying solvent vapor to a lower part of the tower and discharging it from the upper part of the tower, and supplying an alkali catalyst to a part of the tower reactor (A) below the position where the solution of partially saponified EVAc is supplied, thereby further saponifying the partially saponified EVAc, and then withdrawing the resulting solution of EVOH having a degree of saponification of 99 mol % or more and 100 mol % or less from the bottom of the tower.

[0010] In this case, the degree of saponification of the partially saponified EVAc obtained in step (I) is preferably 10 mol% or more and less than 50 mol%. It is also preferable that the ethylene unit content of the EVAc used in step (I) is 10 mol% or more and less than 60 mol%. The solvent for the EVAc solution used in step (I) and the solvent vapor used in step (II) are preferably alcohols, more preferably methanol. It is also preferable that the concentration of the EVAc solution used in step (I) is 60 mass% or less. It is also preferable that the amount of solvent vapor supplied to the column reactor (A) in step (II) is 50 parts by mass or more and less than 500 parts by mass per 100 parts by mass of the partially saponified EVAc supplied to the column reactor (A). It is also preferable that in step (I), the EVAc solution and the alkali catalyst are mixed in a non-column mixer to obtain a solution of partially saponified EVAc having a degree of saponification of 10 mol% or more and less than 60 mol%.

[0011] According to the production method of the present invention, even when EVOH is produced continuously over a long period of time, EVAc can be efficiently saponified, and therefore EVOH can be produced with high productivity.

[0012] FIG. 1 is a schematic diagram of a column reactor used in Examples 1 to 13 and Comparative Examples 1 to 4.

[0013] The present invention provides a method for producing EVOH, comprising: a step (I) of saponifying EVAc in an EVAc solution with an alkali catalyst to obtain a solution of partially saponified EVAc having a saponification degree of 10 mol % or more and less than 60 mol %, and a step (II) of supplying the solution of partially saponified EVAc to an upper part of a tower reactor (A), supplying solvent vapor to a lower part of the tower and discharging it from the upper part of the tower, and supplying an alkali catalyst to a part of the tower reactor (A) below the position where the solution of partially saponified EVAc is supplied, thereby further saponifying the partially saponified EVAc, and then withdrawing the resulting solution of EVOH having a saponification degree of 99 mol % or more and 100 mol % or less from the bottom of the tower. This production method allows efficient saponification of EVAc even when EVOH is produced continuously over a long period of time, thereby enabling EVOH to be produced with high productivity.

[0014] In step (I), the EVAc in a solution (a solution in which EVAc is dissolved) is saponified using an alkali catalyst to obtain a solution of a partially saponified EVAc product.

[0015] The EVAc used in step (I) may be produced by copolymerizing ethylene and vinyl acetate according to a conventional method. While there are no limitations on the polymerization method or solvent, solution polymerization using methanol as the solvent is preferred. Radical initiators, such as various azonitrile initiators and organic peroxide initiators, can be used as the polymerization catalyst. Furthermore, the EVAc may contain other monomers copolymerizable with ethylene and vinyl acetate (e.g., α-olefins such as propylene, unsaturated acids such as acrylic acid, various nitriles, and various amides) in addition to ethylene and vinyl acetate, as long as the effects of the present invention are not impaired. The content of units derived from the other monomers in the EVAc is typically 10 mol % or less.

[0016] The ethylene unit content of the EVAc used in step (I) is preferably 5 mol% or more and less than 70 mol%. If the ethylene unit content is less than 5 mol%, in step (II), the partially saponified EVAc in the column reactor (A) may precipitate and clog the holes in the trays, thereby increasing the pressure and shortening the continuous operation period. The ethylene unit content is more preferably 10 mol% or more, even more preferably 15 mol% or more, and particularly preferably 20 mol% or more. On the other hand, if the ethylene unit content is 70 mol% or more, the gas barrier properties of the resulting EVOH may be reduced. The ethylene unit content is more preferably 65 mol% or less, even more preferably 60 mol% or less, and particularly preferably 55 mol% or less.

[0017] The solvent for the EVAc solution is not particularly limited as long as it can dissolve EVAc, but alcohol is preferred. When alcohol is used as the solvent, the saponification reaction of EVAc proceeds through a transesterification reaction between the acetate ester group of EVAc and an alcohol-based compound, so the amount of alkaline catalyst used can be reduced, allowing the saponification reaction to proceed efficiently. Examples of the alcohol include methanol, ethanol, 1-propanol, and 2-propanol, with methanol being preferred.

[0018] The concentration of EVAc in the EVAc solution is not particularly limited, but is preferably 70% by mass or less. If the concentration exceeds 70% by mass, it may be difficult to uniformly mix the EVAc solution with the alkali catalyst, or in step (II), the partially saponified EVAc in the column reactor (A) may precipitate and clog the holes in the trays, thereby increasing the pressure and shortening the continuous operation period. The EVAc concentration is more preferably 60% by mass or less. On the other hand, from the viewpoint of productivity, the EVAc concentration is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more.

[0019] Examples of the alkali catalyst include compounds such as alkali metal hydroxides, such as sodium hydroxide, potassium hydroxide, and lithium hydroxide; and alkali metal alkoxides, such as sodium methoxide, sodium ethoxide, and potassium t-butoxide. Among these, sodium hydroxide, potassium hydroxide, sodium methoxide, and sodium ethoxide are preferred, and sodium hydroxide is more preferred. The alkali catalyst may be used as is or in the form of a solution. When used as a solution, the solvent may be the same as that used for the EVAc solution.

[0020] The EVAc solution is mixed with the alkali catalyst to saponify the EVAc in the mixed solution. The mixing method is not particularly limited, but examples include a method using a mixer such as a static mixer, a mechanical stirrer, a dynamic mixer, or a non-tower reactor, or a tower reactor. From the viewpoint of excellent mixing efficiency, a non-tower reactor is preferred as the mixer, and a static mixer is more preferred.

[0021] The concentration of the alkali catalyst in the mixed solution containing the EVAc and the alkali catalyst is preferably 0.005 to 1 mol / L. If the concentration is less than 0.005 mol / L, the EVAc may not be sufficiently saponified. The concentration is more preferably 0.01 mol / L or more, even more preferably 0.05 mol / L or more, and particularly preferably 0.1 mol / L or more. On the other hand, if the concentration exceeds 1 mol / L, the degree of saponification of the resulting partially saponified EVAc may be too high. The concentration is more preferably 0.5 mol / L or less, even more preferably 0.3 mol / L or less.

[0022] The mixing time for mixing the EVAc solution and the alkali catalyst is not particularly limited, but is preferably 1 to 100 minutes. If the mixing time is less than 1 minute, the EVAc may not be sufficiently saponified. The mixing time is more preferably 3 minutes or more, and even more preferably 5 minutes or more. On the other hand, if the mixing time exceeds 100 minutes, the production efficiency may decrease, or the degree of saponification of the partially saponified EVAc may become too high. The mixing time is more preferably 50 minutes or less, and even more preferably 30 minutes or less.

[0023] The temperature of the mixture during mixing of the EVAc solution and the alkali catalyst is preferably 10 to 80° C. The temperature is more preferably 20° C. or higher, even more preferably 30° C. or higher, even more preferably 40° C. or higher, and particularly preferably 50° C. or higher. On the other hand, the temperature is more preferably 70° C. or lower.

[0024] The degree of saponification of the partially saponified EVAc obtained by mixing the EVAc solution with the alkali catalyst must be 10 mol% or more and less than 60 mol%. By saponifying EVAc to a predetermined degree of saponification in this way, impurities such as aldehydes, which are by-produced during the process, are discharged together with the solvent from the top of the column in step (II) before condensation, resulting in EVOH with little coloration. When the degree of saponification of the partially saponified EVAc is less than 10 mol%, the solution viscosity increases as the degree of saponification of the partially saponified EVAc increases in step (II), resulting in poor flowability due to the high viscosity. On the other hand, when the degree of saponification of the partially saponified EVAc is 10 mol% or more, the solution viscosity becomes similar to that of the EVAc solution, and surprisingly, as the degree of saponification increases further in step (II), the viscosity decreases. Therefore, the partially saponified EVAc in the column reactor (A) is less likely to solidify, even during long-term continuous EVOH production. This suppresses pressure increases due to blockage of the holes in the shelves, enabling efficient production of EVOH. The saponification degree is more preferably 11 mol% or more, even more preferably 12 mol% or more, and particularly preferably 13 mol% or more. On the other hand, by having the saponification degree of less than 60 mol%, the partially saponified EVAc is prevented from being discharged from the column reactor (A) together with solvent vapor in step (II). The saponification degree is more preferably 55 mol% or less, even more preferably 50 mol% or less.

[0025] In step (II), the solution of the partially saponified EVAc is supplied to the top of the tower reactor (A), solvent vapor is supplied to the bottom of the tower and discharged from the top, and an alkali catalyst is supplied to the tower reactor (A) below the position where the solution of the partially saponified EVAc is supplied to further saponify the partially saponified EVAc, and the resulting solution of EVOH having a saponification degree of 99 mol % or more and 100 mol % or less is withdrawn from the bottom of the tower. In this way, in step (II), the partially saponified EVAc is resaponified to obtain EVOH with a high saponification degree.

[0026] FIG. 1 is a schematic diagram of a tower reactor (A) used in the Examples described later. Step (II) will be described with reference to FIG. 1. The solution of partially saponified EVAc obtained in step (I) is supplied to the top of the tower reactor (A). In FIG. 1, the solution of partially saponified EVAc is supplied to the tower reactor (A) through a partially saponified EVAc solution supply port 2 at the top of the tower. An alkali catalyst is supplied to a position below the position at the top of the tower where the solution of partially saponified EVAc is supplied. In FIG. 1, an alkali catalyst is supplied to the tower reactor (A) through an alkali catalyst supply port 3 located below the partially saponified EVAc solution supply port 2. Solvent vapor is supplied to the bottom of the tower and discharged from the top of the tower. The solvent vapor is preferably supplied to a position above the position at which the EVOH solution described later is removed. The position from which the solvent vapor is discharged is preferably above the position from which the partially saponified EVAc solution is supplied, from the viewpoint of more efficiently removing impurities such as aldehyde remaining in the solution. From the same viewpoint, it is also preferable that the solvent vapor be discharged from the top of the column. In Figure 1, solvent vapor is blown in through a solvent vapor inlet 4 at the bottom of the column and discharged from a solvent vapor outlet 1 at the top of the column.

[0027] The partially saponified EVAc solution supplied to the top of the column is transported from the top to the bottom of the column reactor (A). The partially saponified EVAc solution supplied to the top of the column comes into contact with the solvent vapor, and by-products such as aldehydes and acetate esters are discharged together with the solvent vapor from the top of the column (solvent vapor outlet 1). The partially saponified EVAc solution transported to the position where the alkaline catalyst is supplied (alkaline catalyst supply port 3) comes into contact with the alkaline catalyst to re-saponify the partially saponified EVAc, and the EVOH solution is then discharged from the bottom of the column (EVOH solution outlet 5). By supplying the alkaline catalyst below the position where the partially saponified EVAc solution is supplied to the top of the column, impurities such as aldehydes remaining in the partially saponified EVAc solution can be removed in advance by the solvent vapor at the top of the column before re-saponification. This suppresses coloration of the partially saponified EVAc during re-saponification.

[0028] In step (II), the same alkali catalyst as in step (I) is used. The same solvent vapor as that used in the EVAc solution in step (I) is used. Regarding the solvent used in step (II), the saponification reaction must be carried out until the degree of saponification of the partially saponified EVAc reaches 99 mol% or more. However, in a reaction system containing a large amount of water in the solvent, the hydrolysis reaction of the acetate ester becomes dominant, making it difficult to efficiently proceed with the saponification reaction. This may require an increased amount of alkali catalyst to increase the degree of saponification. Therefore, it is preferable that the solvent used in step (II) does not contain water. However, if it does contain water, its water content is preferably 1.5% by mass or less, more preferably 1% by mass or less, and even more preferably 0.8% by mass or less, in order to reduce the amount of alkali catalyst used. It is preferable that the water content of the solvent used in step (II) be equal to or less than the above-mentioned upper limit, because the amount of catalyst residue contained in the resulting EVOH is reduced, thereby preventing a decrease in thermal stability, etc. The concentration of the partially saponified EVAc in the solution of the partially saponified EVAc used in step (II) is not particularly limited, but is preferably 70% by mass or less. If the concentration exceeds 70% by mass, the partially saponified EVAc may precipitate in the column reactor (A) and clog the holes in the trays, resulting in an increase in pressure and a shortened continuous operation period. The concentration of the partially saponified EVAc is more preferably 60% by mass or less. On the other hand, from the viewpoint of productivity, the concentration of the partially saponified EVAc is preferably 10% by mass or more, more preferably 20% by mass or more, even more preferably 30% by mass or more, and particularly preferably 40% by mass or more.

[0029] Generally, as the saponification reaction progresses, the solubility of the partially saponified EVAc in the solvent decreases, so it is preferable to pressurize the column reactor (A) in step (II) and carry out the reaction at a high temperature. The pressure in the column reactor (A) is preferably 0.1 to 1.0 MPa. The pressure is more preferably 0.8 MPa or less, even more preferably 0.6 MPa or less, and particularly preferably 0.55 MPa or less. The pressure may be 0.2 MPa or more.

[0030] The temperature of the tower reactor (A) is preferably 60 to 180° C. From the viewpoint of increasing the reaction efficiency, the temperature is more preferably 70° C. or higher, further preferably 80° C. or higher, and particularly preferably 90° C. or higher. On the other hand, the temperature of the tower reactor (A) is more preferably 150° C. or lower, further preferably 140° C. or lower, and particularly preferably 130° C. or lower.

[0031] In step (II), the amount of solvent vapor supplied to the tower reactor (A) is preferably 50 parts by mass or more but less than 500 parts by mass relative to 100 parts by mass of the partially saponified EVAc supplied to the tower reactor (A). If the amount of solvent vapor is less than 50 parts by mass, impurities such as aldehydes in the partially saponified EVAc may not be sufficiently removed, and the resulting EVOH may be discolored. The amount of solvent vapor is more preferably 60 parts by mass or more. On the other hand, if the amount of solvent vapor is 500 parts by mass or more, the partially saponified EVAc may be discharged together with the solvent vapor. The amount of solvent vapor is more preferably 300 parts by mass or less, even more preferably 200 parts by mass or less, even more preferably 150 parts by mass or less, and particularly preferably 100 parts by mass or less. The temperature of the solvent vapor may be, for example, approximately the boiling point of the solvent at the pressure inside the tower.

[0032] The amount of the alkali catalyst added in step (II) is preferably 0.01 to 10 parts by mass relative to 100 parts by mass of the partially saponified EVAc product. The amount is more preferably 0.05 parts by mass or more, even more preferably 0.1 parts by mass or more, and particularly preferably 0.3 parts by mass or more. On the other hand, the amount is more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less.

[0033] According to the above-described production method of the present invention, it is preferable to continuously operate the column reactor (A) in step (II) for 35 days or more to continuously produce EVOH. This allows EVOH to be produced more efficiently. The number of days for continuous production of EVOH is more preferably 40 days or more, even more preferably 45 days or more, even more preferably 50 days or more, and particularly preferably 55 days or more.

[0034] The EVOH solution obtained in step (II) is preferably pelletized by a known method. Examples of the pelletization method include a method in which the EVOH solution is cooled and solidified, followed by cutting, and a method in which the EVOH is melt-kneaded in an extruder, then discharged, and then cut. Specific examples of the method for cutting EVOH include a method in which EVOH is extruded into strands and then cut with a pelletizer, and a method in which EVOH discharged from a die is cut by a center hot cut method or an underwater cut method. When the EVOH solution is pelletized, hydrous EVOH pellets are obtained.

[0035] When water-containing EVOH pellets are obtained by cooling and solidifying an EVOH solution, the water-containing EVOH pellets are preferably washed and deliquored by a known method. Alternatively, the water-containing EVOH pellets are preferably immersed in a solution containing a boron compound, an alkali metal salt, an alkaline earth metal salt, or the like by a known method to incorporate the compound into the water-containing EVOH. The incorporation of these compounds can improve the mechanical properties, thermal stability, and the like of EVOH molded articles. When water-containing EVOH is obtained by melt-kneading and pelletizing EVOH, the washing, deliquoring, and chemical treatment of the EVOH may be carried out in an extruder.

[0036] The obtained water-containing EVOH pellets can be dried by a known method to obtain EVOH pellets. The moisture content of the dried EVOH pellets is preferably 0.5% by mass or less. The drying method is not particularly limited, and examples thereof include stationary drying combined with air drying or nitrogen drying, fluidized drying, and vacuum drying. However, multi-stage drying combining several drying methods is preferred, and multi-stage drying including preliminary drying and main drying is more preferred.

[0037] The saponification degree of the EVOH thus obtained must be in the range of 99 mol% or more and 100 mol% or less. According to the production method of the present invention, EVOH with such a high saponification degree can be efficiently produced. The saponification degree is preferably 99.3 mol% or more, more preferably 99.5 mol% or more, and even more preferably 99.7 mol% or more.

[0038] The yellow index (YI) of the EVOH is preferably not more than 20, more preferably not more than 15, even more preferably not more than 13, and particularly preferably not more than 9.5. According to the production method of the present invention, such EVOH with little coloration can be efficiently produced.

[0039] The EVOH obtained by the method of the present invention can be molded into various types of articles such as films, sheets, containers, pipes, fibers, etc.

[0040] The present invention will be explained in more detail below using examples.

[0041] [Evaluation Method] (1) Degree of Saponification of Partially Saponified EVAc Product After Step (I) The partially saponified EVAc product solutions after step (I) obtained in Examples and Comparative Examples were concentrated using a rotary evaporator and then dried under reduced pressure at 40°C for 10 hours to obtain a dried partially saponified EVAc product. 20 mg of the resulting dried partially saponified EVAc product was dissolved in CDCl 3 After dissolving in 6 mL, the measurement was carried out under the following conditions: 1 H-NMR measurement was performed, and the degree of saponification was calculated from the ratio of the integral value of the methine hydrogen (saponified site) of the vinyl alcohol unit observed at 3.1 to 4.1 ppm to the integral value of the methine hydrogen (unsaponified site) of the vinyl acetate unit observed at 4.5 to 5.2 ppm. (Measurement conditions) Apparatus name: JEOL Ltd. Superconducting Nuclear Magnetic Resonance Apparatus Lambda 500 Observation frequency: 500 MHz Measurement temperature: 25°C Number of accumulations: 1024

[0042] (2) Saponification Degree of EVOH In the Examples and Comparative Examples, dried EVOH pellets obtained 3 days after the start of production were pulverized, and 20 mg of the resulting powder was dissolved in 6 mL of a mixed solution of deuterated dimethyl sulfoxide and deuterated trifluoroacetic acid (mass ratio: deuterated dimethyl sulfoxide / deuterated trifluoroacetic acid = 95:5) and then measured under the following conditions: 1H-NMR measurement was performed, and the degree of saponification was calculated from the ratio of the integral value of the methine hydrogen of the vinyl alcohol unit observed at 3.1 to 4.1 ppm (saponified site) to the integral value of the methyl group hydrogen of the vinyl acetate unit observed at 1.9 to 2.0 ppm (unsaponified site). (Measurement conditions) Apparatus name: JEOL Ltd. Superconducting Nuclear Magnetic Resonance Apparatus Lambda 500 Observation frequency: 500 MHz Measurement temperature: 80°C Number of accumulations: 128

[0043] (3) Pressure at the bottom of the tower reactor (A) in step (II) The pressure at the bottom of the tower reactor (A) [plate tower (saponification tower, total number of plates: 21)] used in step (II) in the examples and comparative examples was measured using a pressure gauge installed at the bottom (below the first plate). The pressure at the bottom of the tower three days after the start of EVOH production is shown in Table 1.

[0044] (4) Number of continuous production days In the examples and comparative examples, when EVOH was continuously produced, the production was stopped when the pressure at the bottom of the tower measured in accordance with the above evaluation method (3) exceeded 0.52 MPa, and the number of days from the start of production to the stop of production was recorded as the number of continuous production days.

[0045] (5) Distillate of Step (II) Three days after the start of production of EVOH in the Examples and Comparative Examples, the distillate condensed from the mixed vapor discharged (distilled) from the top of the column in Step (II) was visually inspected for cloudiness and the presence of resin, and evaluated according to the following criteria. A rating of D was determined to indicate poor production efficiency. Evaluation: Criteria A: Colorless and transparent B: Slightly cloudy C: Significantly cloudy D: Resin present (6) Evaluation of Yellowness of EVOH In the Examples and Comparative Examples, the YI (yellowness index) of dried EVOH pellets obtained three days after the start of production was measured in accordance with JIS-K-7103.

[0046] Example 1 (Step I) A 57% by mass EVAc methanol solution, prepared by dissolving EVAc having an ethylene unit content of 44 mol% and a vinyl acetate unit content of 56 mol%, in methanol, was mixed with a 120 g / L sodium hydroxide methanol solution in a volume ratio of 95:5 at 60°C for 10 minutes in a static mixer to obtain a partially saponified EVAc solution. The degree of saponification of the resulting partially saponified EVAc solution was measured according to the method described in the evaluation method (1) above. The results are shown in Table 1.

[0047] (Step II) Subsequently, the methanol solution of partially saponified EVAc obtained in step (I) was further saponified using a tower reactor (A) (a plate tower (saponification tower, total number of plates: 21), inner diameter: 140 mm, height: 4700 mm). FIG. 1 is a schematic diagram of the tower reactor (A). The methanol solution of partially saponified EVAc was continuously fed to the 20th plate of the tower reactor (A), whose temperature inside the tower was 118°C, from a feed port 2 for the partially saponified EVAc solution at a rate of 8 kg / h. Methanol vapor was continuously fed to the bottom of the first plate from a solvent vapor inlet 4 in an amount equivalent to 75 parts by mass per 100 parts by mass of the partially saponified EVAc fed to the tower reactor (A). A methanol solution containing sodium hydroxide in an amount equivalent to 1 part by mass per 100 parts by mass of the partially saponified EVAc supplied to the column reactor (A) was continuously supplied to the 14th tray from the alkali catalyst supply port 3. The by-products, methyl acetate and aldehyde, were distilled together with excess methanol as a mixed vapor from the top of the column (solvent vapor outlet 1), and an EVOH methanol solution was obtained from the bottom of the column (EVOH solution outlet 5). The column bottom pressure, the number of days of continuous production, and the distillate in step (II) were evaluated according to the methods described in the evaluation methods (3) to (5) above. The results are shown in Table 1.

[0048] (Production of EVOH Pellets) To the EVOH methanol solution obtained in step (II), acetic acid was added in an amount equimolar to the sodium hydroxide supplied to the column reactor (A) in step (II) to neutralize the remaining sodium hydroxide. The solution was then concentrated until the copolymer concentration reached 40% by mass. This solution was extruded through a 3.5 mm nozzle into a methanol-water mixed solvent (methanol / water = 10 / 90 by weight) maintained at 5°C to solidify into strands, which were then cut with a cutter to obtain hydrous EVOH pellets. The pellets were then washed in a large amount of 0.1 g / L aqueous acetic acid solution. After removing the remaining methanol and sodium acetate, the pellets were dried at 60°C for 5 hours and then at 110°C for 10 hours to obtain dried EVOH pellets. The resulting dried EVOH pellets were measured for saponification degree and yellowness index according to the methods described in the evaluation methods (2) and (6) above. The results are shown in Table 1.

[0049] (Examples 2 and 5, Comparative Examples 1 to 4) Dried EVOH pellets were prepared and evaluated in the same manner as in Example 1, except that the concentration of sodium hydroxide in step (I) was adjusted so that the degree of saponification of the resulting partially saponified EVAc product would be as shown in Table 1. The results are shown in Table 1.

[0050] (Examples 3, 6, and 7) Dried EVOH pellets were prepared and evaluated in the same manner as in Example 1, except that EVAc having an ethylene unit content shown in Table 1 was used and the concentration of sodium hydroxide in step (I) was adjusted so that the degree of saponification of the partially saponified EVAc obtained was as shown in Table 1. The results are shown in Table 1.

[0051] (Examples 4, 10, and 11) EVOH pellets were produced and evaluated in the same manner as in Example 1, except that the amount of methanol vapor supplied to the column reactor (A) in step (II) was changed as shown in Table 1. The results are shown in Table 1.

[0052] Example 8 EVOH pellets were prepared and evaluated in the same manner as in Example 1, except that ethanol was used as the solvent instead of methanol in steps (I) and (II). The results are shown in Table 1.

[0053] (Example 9) EVOH pellets were prepared and evaluated in the same manner as in Example 1, except that in step (I), the concentration of the EVAc methanol solution used was changed to be as shown in Table 1, and the concentration of sodium hydroxide was adjusted so that the degree of saponification of the resulting partially saponified EVAc product was as shown in Table 1. The results are shown in Table 1.

[0054] Examples 12 and 13 Dried EVOH pellets were prepared and evaluated in the same manner as in Example 1, except that the mixing method in step (I) was changed as shown in Table 1. The results are shown in Table 1.

[0055]

[0056] 1 Solvent vapor outlet 2 EVAc partially saponified product solution supply port 3 Alkaline catalyst supply port 4 Solvent vapor blowing port 5 EVOH solution outlet

Claims

1. A method for producing an ethylene-vinyl alcohol copolymer, comprising: a step (I) of saponifying an ethylene-vinyl acetate copolymer in a solution of ethylene-vinyl acetate copolymer with an alkali catalyst to obtain a solution of partially saponified ethylene-vinyl acetate copolymer having a degree of saponification of 10 mol % or more and less than 60 mol %; and a step (II) of supplying the solution of partially saponified ethylene-vinyl acetate copolymer to an upper part of a tower reactor (A), supplying solvent vapor to a lower part of the tower and discharging it from the upper part of the tower, and supplying an alkali catalyst to a part of the tower reactor (A) lower than the position where the solution of partially saponified ethylene-vinyl acetate copolymer is supplied, thereby further saponifying the partially saponified ethylene-vinyl acetate copolymer, and then withdrawing the obtained solution of ethylene-vinyl alcohol copolymer having a degree of saponification of 99 mol % or more and 100 mol % or less from the bottom of the tower.

2. The method according to claim 1, wherein the degree of saponification of the partially saponified ethylene-vinyl acetate copolymer obtained in step (I) is 10 mol % or more and less than 50 mol %.

3. The method according to claim 1 or 2, wherein the ethylene unit content of the ethylene-vinyl acetate copolymer used in step (I) is 10 mol % or more and less than 60 mol %.

4. The process according to claim 1 or 2, wherein the solvent for the ethylene-vinyl acetate copolymer solution used in step (I) and the solvent vapor used in step (II) are alcohols.

5. The process of claim 4, wherein the alcohol is methanol.

6. The method according to claim 1 or 2, wherein the concentration of the solution of ethylene-vinyl acetate copolymer used in step (I) is 60% by mass or less.

7. The production method according to claim 1 or 2, wherein the amount of the solvent vapor supplied to the tower reactor (A) in the step (II) is 50 parts by mass or more and less than 500 parts by mass per 100 parts by mass of the partially saponified ethylene-vinyl acetate copolymer supplied to the tower reactor (A).

8. The method according to claim 1 or 2, wherein in step (I), the ethylene-vinyl acetate copolymer solution and the alkali catalyst are mixed in a non-tower mixer to obtain a solution of partially saponified ethylene-vinyl acetate copolymer having a degree of saponification of 10 mol % or more and less than 60 mol %.

Citation Information

Patent Citations

  • Flexible device buffer layer, preparation method thereof and flexible device

    CN110316690A

  • JP1974027591A

  • Method for producing ethylene-vinyl acetate copolymer saponified product

    JP2009242645A

  • Method for producing saponified ethylene-vinyl acetate copolymer

    JP2010077352A

  • Process for production of ethylene-vinyl alcohol copolymer and production method for ethylene-vinyl alcohol copolymer

    WO2023068242A1