Organic coated steel sheet

The organic coated steel sheet with a nitrite-containing coating layer addresses hydrogen embrittlement in high-strength steel by reducing nitrite ions over hydrogen, enhancing durability and corrosion resistance for applications like automotive structural parts.

WO2024228381A1PCT designated stage expired Publication Date: 2024-11-07NIPPON STEEL CORPORATION
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/016687
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-01
Filing Date
2024-04-30
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

High-strength steel sheets are prone to hydrogen embrittlement cracking due to hydrogen penetration during electrodeposition coating, which can lead to cracks and reduced durability, especially in applications like automobiles where high strength is required.

Method used

An organic coated steel sheet with a tensile strength of 980 MPa or more, featuring an organic coating layer containing 1 to 30% by mass of nitrite, which preferentially reduces nitrite ions over hydrogen, thereby suppressing hydrogen embrittlement cracking. The coating layer can be applied directly or indirectly via a plating layer and chemical conversion coating.

Benefits of technology

The organic coated steel sheet effectively reduces hydrogen embrittlement cracking, ensuring high strength and durability, making it suitable for structural parts in fields like automobiles and building materials, while maintaining excellent corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024016687_07112024_PF_FP_ABST
    Figure JP2024016687_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides a high-strength steel sheet in which hydrogen embrittlement cracking is less likely to occur. An organic coated steel sheet (1) according to the present invention has: a steel sheet (2) which has a tensile strength of 980 MPa or more; and an organic coating layer (3) which is disposed on at least a part of the surface of the steel sheet. This organic coated steel sheet (1) is characterized in that the organic coating layer (3) contains a nitrite salt as a nitrite radical in an amount of 1-30% by mass and 0.05 g / m2 or more.
Need to check novelty before this filing date? Find Prior Art

Description

organic coated steel sheet

[0001] The present invention relates to an organic coated steel sheet.

[0002] In recent years, efforts have been made to increase the strength of steel sheets used in various fields such as automobiles, home appliances, building materials, etc. For example, in the automobile field, the use of high-strength steel sheets has been increasing with the aim of reducing the weight of vehicle bodies to improve fuel efficiency.

[0003] Such high-strength steel sheets, particularly those used for automotive components, are subjected to electrodeposition coating to impart desired properties such as corrosion resistance. It is known that during this electrodeposition coating process, water is electrolyzed by the application of a voltage, generating hydrogen. The hydrogen generated during the electrodeposition coating penetrates into the steel sheet, reaching positions deeper than the surface layer of the steel sheet. As a result, the hydrogen segregates at martensite grain boundaries in the steel structure, embrittling the grain boundaries and potentially causing cracks in the steel sheet. Cracking caused by such hydrogen penetration is called hydrogen embrittlement cracking or delayed fracture. It is known that hydrogen embrittlement cracking is more likely to occur as the strength of the steel sheet increases.

[0004] Various countermeasures have been investigated to prevent hydrogen embrittlement cracking (delayed fracture) of high-strength steel sheets. For example, Patent Document 1 discloses an Fe-based electroplated high-strength steel sheet with a low content of diffusible hydrogen in the steel, which is obtained by annealing the steel sheet after electroplating, thereby releasing diffusible hydrogen that has entered the steel sheet during electroplating into the furnace. The Fe-based electroplated high-strength steel sheet disclosed in Patent Document 1 is said to have excellent chemical conversion treatability, corrosion resistance after painting, and also excellent delayed fracture resistance.

[0005] Japanese Patent Application Laid-Open No. 2022-180344

[0006] In a high-strength plated steel sheet as disclosed in Patent Document 1, the formation of a plating layer on the surface of the base steel sheet is believed to be effective in suppressing the penetration of hydrogen, which can cause hydrogen embrittlement cracking. However, corrosion is likely to occur on the edge (cut surface) of the steel sheet where no plating layer is formed. Such corrosion on the edge can cause not only red rust but also hydrogen generation. Furthermore, if hydrogen generated as corrosion progresses penetrates into the steel sheet from the edge, there is a risk of the aforementioned hydrogen embrittlement cracking occurring in the high-strength steel sheet.

[0007] Therefore, an object of the present invention is to provide a high-strength steel sheet that can suppress hydrogen embrittlement cracking.

[0008] The present invention includes the following aspects.

[0009] (Aspect 1) A steel sheet having a tensile strength of 980 MPa or more and an organic coating layer disposed on at least a part of the surface of the steel sheet, wherein the organic coating layer contains nitrite in an amount of 1 to 30 mass % and 0.05 g / m as nitrite ions. 2 An organic coated steel sheet characterized by containing the above content.

[0010] (Aspect 2) The organic coated steel sheet according to Aspect 1, wherein the nitrite is at least one selected from the group consisting of lithium salts, sodium salts, potassium salts, magnesium salts, calcium salts, strontium salts, barium salts, and ammonium salts.

[0011] (Embodiment 3) The organic coated steel sheet according to embodiment 1 or 2, further comprising a plating layer disposed between the steel sheet and the organic coating layer.

[0012] (Embodiment 4) The organic coated steel sheet according to any one of the above embodiments 1 to 3, characterized in that the steel sheet has a tensile strength of 1.2 to 3.0 GPa.

[0013] (Embodiment 5) A molded article made using the organic coated steel sheet according to any one of embodiments 1 to 4.

[0014] According to the organic coated steel sheet of the present invention, it is possible to provide a high strength steel sheet that can suppress hydrogen embrittlement cracking.

[0015] Fig. 1 is a schematic diagram of an organic coated steel sheet 1 according to one embodiment of the present invention. Fig. 2 is a schematic diagram showing an apparatus 6 for evaluating hydrogen embrittlement cracking of a steel sheet.

[0016] Hereinafter, preferred embodiments of the organic coated steel sheet of the present invention will be described in detail. In this specification, various numerical ranges mean ranges including the upper and lower limit values ​​unless otherwise specified.

[0017] In order to achieve the above object, the present inventors have conducted extensive research focusing on the prevention of hydrogen penetration into steel sheets, which causes hydrogen embrittlement cracking. As a result, the present inventors have discovered a technology that can reduce hydrogen penetration into steel sheets during corrosion by formulating a paint with a specific composition. Specifically, the present inventors have discovered that by adding a specific amount of nitrite to a paint composition, the nitrite ions (NO 2 - It was found that the generation of hydrogen, which causes hydrogen embrittlement cracking, can be suppressed by reducing Cr(O) preferentially over hydrogen.

[0018] The present invention was completed based on these findings, and includes each embodiment of the organic coated steel sheet described above.

[0019] First, a preferred embodiment of the organic coated steel sheet of the present invention will be described in detail.

[0020] [Organic-coated steel sheet] As shown in Figure 1, an organic-coated steel sheet 1 according to one embodiment of the present invention basically comprises a steel sheet 2 having a pair of surfaces opposing each other in the thickness direction and a tensile strength of 980 MPa or more, and an organic coating layer 3 disposed on each of both surfaces of the steel sheet 2.

[0021] In this embodiment, as shown in FIG. 1 , the organic coated steel sheet 1 further includes a plating layer 4 disposed between the steel sheet 2 and the organic coating layer 3, and a chemical conversion coating 5 disposed between the plating layer 4 and the organic coating layer 3.

[0022] In this specification, the term "disposed on at least a part of the surface of the steel sheet" is used to mean not only an embodiment in which the material is directly disposed on at least a part of the surface of the steel sheet, but also an embodiment in which the material is indirectly disposed on at least a part of the surface of the steel sheet via another layer (e.g., a plating layer) or coating (e.g., a chemical conversion coating). When the steel sheet has such another layer or coating on its surface, the surface of the steel sheet refers to the interface between the steel sheet and the other layer or coating.

[0023] In the organic-coated steel sheet 1 shown in FIG. 1 , the organic coating layer 3 is disposed on each of both surfaces of the steel sheet 2 via a plating layer 4 and a chemical conversion coating 5, but this is not a limitation. That is, the organic coating layer 3 may be disposed on each of both surfaces of the steel sheet 2 with or without a plating layer 4 and a chemical conversion coating 5 therebetween, or may be disposed on only one surface of the steel sheet 2 with or without a plating layer 4 and a chemical conversion coating 5 therebetween. In the organic-coated steel sheet 1 shown in FIG. 1 , the organic coating layer 3 is disposed over the entire surface of the steel sheet 2, but this is not a limitation. That is, the organic coating layer 3 may be disposed over the entire surface of the steel sheet 2 as shown in FIG. 1 , or may be disposed over only a portion of the surface of the steel sheet 2.

[0024] In the organic coating steel sheet 1 of this embodiment, the organic coating layer 3 contains nitrite in an amount of 1 to 30 mass % and 0.05 g / m 2 Since the organic coating layer 3 contains a specific amount of nitrite in this way, the nitrite ions (NO 2 - ) is reduced preferentially over hydrogen, which makes it difficult for hydrogen to be generated, which causes hydrogen embrittlement cracking. As a result, the organic coated steel sheet 1 of this embodiment is a high-strength steel sheet that can suppress hydrogen embrittlement cracking.

[0025] It is not an essential constituent element of the organically coated steel sheet 1 to have layers or coatings (i.e., the plating layer 4 and the chemical conversion coating 5) other than the steel sheet 2 and the organic coating layer 3. Therefore, the organically coated steel sheet 1 may or may not have any layers or coatings other than the steel sheet 2 and the organic coating layer 3, depending on the required properties of the final product to which it is applied.

[0026] The various components of the organic coated steel sheet 1 will be described in more detail below.

[0027] (Steel Plate) In the organic coated steel plate 1, the steel plate 2 serving as the base material is a steel plate having a tensile strength (TS) of 980 MPa or more. It is generally known that the susceptibility of steel plates to hydrogen embrittlement increases as the strength increases. However, in the organic coated steel plate 1 of this embodiment, even if the steel plate 2 is a high-strength steel plate having a tensile strength of 980 MPa or more, the specific amount of nitrite contained in the organic coating layer 3 as described above can make it difficult to generate hydrogen, which causes hydrogen embrittlement cracking. Therefore, the organic coated steel plate 1 can be suitably used as a material for various structural parts in fields where such high strength is required.

[0028] The tensile strength of the steel plate 2 is not particularly limited as long as it is 980 MPa or more, but is preferably 1200 MPa (i.e., 1.2 GPa) or more, more preferably 1300 MPa (i.e., 1.3 GPa) or more, and even more preferably 1400 MPa (i.e., 1.4 GPa) or more. The upper limit of the tensile strength of the steel plate 2 is not particularly limited, but from the viewpoint of toughness and formability, it is, for example, 4000 MPa (i.e., 4.0 GPa) or less, preferably 3000 MPa (i.e., 3.0 GPa) or less.

[0029] In particular, the tensile strength of the steel plate 2 is preferably 1.2 to 3.0 GPa. It is known that a steel plate with a tensile strength of 1.2 GPa or more may fracture even with a trace amount of hydrogen on the order of a few ppm by mass. Particularly in the automotive field, there is a demand for high-strength steel plates while also sufficiently reducing the risk of hydrogen embrittlement cracking. Even if the tensile strength of the steel plate 2 is 1.2 GPa or more, the organic-coated steel plate 1 of this embodiment can be made less susceptible to the generation of hydrogen, which causes hydrogen embrittlement cracking, and is therefore suitable for use as a material for various structural components in the automotive field. Furthermore, if the tensile strength of the steel plate 2 is 3.0 GPa or less, the organic-coated steel plate 1 can be made to have excellent toughness and formability.

[0030] The tensile strength (TS) of a steel plate can be measured by cutting a No. 5 tensile test piece according to JIS Z2241:2011 from the steel plate and conducting a tensile test in accordance with JIS Z2241:2011. It is preferable to cut the test piece from the steel plate so that the longitudinal direction of the test piece is perpendicular to the rolling direction of the steel plate. For example, if it is difficult to obtain a No. 5 tensile test piece due to dimensional constraints, other test pieces according to JIS Z2241:2011 can be used. However, to perform an appropriate evaluation, the plate thickness of the steel plate must be set to a lower limit of 0.5 mm. Furthermore, if it is difficult to obtain a No. 5 tensile test piece due to dimensional constraints and it is also difficult to use other test pieces according to JIS Z2241:2011, a micro-Vickers test can be conducted in accordance with JIS Z2244-1:2020, and the hardness (HV) converted into tensile strength can be used. Samples for the micro-Vickers test can be prepared as follows. First, a sample is cut from any position 50 mm or more away from the end face of the steel plate, other than the processed portion, so that the thickness cross section perpendicular to the plate surface can be observed. If a sample cannot be obtained from the above position, a sample is cut from a position avoiding the end. The thickness cross section is preferably parallel to the rolling direction. The size of the sample depends on the measuring device, but it should be large enough to observe approximately 10 mm in a direction perpendicular to the thickness direction. The cross section of the sample cut out as described above is polished using #600 to #1500 silicon carbide paper. Furthermore, after polishing, the cross section is mirror-finished using a diluted solution such as alcohol or a liquid in which diamond powder with a particle size of 1 to 6 μm is dispersed in pure water. Next, the cross section is electropolished to obtain an observation surface. The micro-Vickers test is performed at 30 points at 1 / 4 of the plate thickness with a load of 500 gf, and the average value is used. The Vickers hardness obtained by the micro-Vickers test can be converted to tensile strength using the following formula: Tensile strength [MPa] = 3.12 × Vickers hardness [HV] + 16

[0031] The steel plate 2 is not particularly limited in any respect other than the tensile strength, and any steel plate can be used according to the desired mechanical strength, etc. For example, the thickness of the steel plate 2 is not particularly limited, but can be about 0.2 mm to 10.0 mm.

[0032] (Organic Coating Layer) In the organic coated steel sheet 1, the organic coating layer 3 contains nitrite in an amount of 1 to 30 mass % and 0.05 g / m 2 The organic coating layer 3 contains the nitrite in such a specific amount. 2 - ) is reduced preferentially over hydrogen, making it possible to make it difficult for hydrogen to be generated, which causes hydrogen embrittlement cracking.

[0033] The nitrite salt that can be used in the organic-coated steel sheet 1 of this embodiment is not particularly limited, and examples thereof include alkali metal salts, alkaline earth metal salts, and ammonium salts of nitrite. Specific examples include lithium salts, sodium salts, potassium salts, magnesium salts, calcium salts, strontium salts, barium salts, and ammonium salts of nitrite. Among these, in order to obtain the effects of the nitrite more effectively, it is preferable that the nitrite salt is at least one selected from the group consisting of lithium salts, sodium salts, potassium salts, magnesium salts, calcium salts, strontium salts, barium salts, and ammonium salts of nitrite.

[0034] Nitrite in the organic coating layer can be identified by known methods. For example, this can be done using an element distribution image obtained by SEM-EDS. Specifically, first, the cross section of the organic-coated steel sheet along the sheet thickness direction is flattened by mechanical polishing. Next, the surface of the organic-coated steel sheet is chemically polished by colloidal polishing until it is polished to a mirror finish. The cross section of the polished organic-coated steel sheet is observed using an SEM. Specifically, an element distribution image is taken using SEM-EDS at a magnification of 5000x (area 200 μm long and 200 μm wide). If an element corresponding to the nitrite cation is detected in this element distribution image at a gram equivalent of 90% or more of the separately measured gram equivalent of the nitrite ion (100%), it is determined that nitrite is present in the organic coating layer. Note that if multiple elements corresponding to the nitrite cation are detected, the total gram equivalent is used for determination. For the analysis and quantification of elements, EPMA (electron probe microanalysis) and GDS (glow discharge optical emission spectroscopy) can be used. The gram equivalent (eq) of nitrite radicals in the organic coating layer can be determined from the content measured by a colorimetric method utilizing color development by diazotization, which will be described later.

[0035] The content of nitrite in the organic coating layer 3 is 1 to 30 mass % and 0.05 g / m as nitrite ion. 2 The content is not particularly limited as long as it is equal to or greater than this. The content of the nitrite salt as nitrite radical is preferably as high as possible in that a higher effect is more likely to be obtained. Specifically, the content is preferably 5 mass% or more relative to the total mass of the organic coating layer (i.e., the mass of the total solid content of the organic coating layer). The content of the nitrite salt may be 10 mass% or more, 15 mass% or more, 20 mass% or more, or 25 mass% or more. However, the upper limit of the content of the nitrite salt is set to 30 mass% because, in terms of the solubility product, a range exceeding 30 mass% makes it impossible to stably produce organic-coated steel sheets.

[0036] In addition, the content of nitrite as nitrite ions per surface area of ​​the steel sheet is set to 0.50 g / m, as this is likely to provide a higher effect. 2 It is preferable that the content is 1.00 g / m or more. 2More preferably, it is 5.00 g / m or more. 2 The upper limit of the content of nitrite per surface area of ​​the steel sheet is not particularly limited, but is, for example, 10.00 g / m 2 is.

[0037] The organic coating layer 3 contains a resin as a base coating. It may also contain components other than nitrites, as long as the effects of the present invention are not impaired. Examples of such components include additives such as color pigments, anti-rust pigments, dispersants, leveling agents, and lubricants, as well as dilution solvents.

[0038] The resin that can be contained in the organic coating layer is not particularly limited, but is preferably one that functions as a binder that binds each component contained in the organic coating layer, and examples thereof include solvent-based resins that dissolve or disperse in organic solvents, and water-soluble or water-dispersible aqueous resins.

[0039] The solvent-based resin is not particularly limited, but examples thereof include polyester resin, urethane resin, epoxy resin, acrylic resin, and a mixed resin of two or more of these resins. The resin may be a crosslinked resin having a crosslinked structure, or a non-crosslinked resin having no crosslinked structure. When a crosslinked structure is imparted to the resin, a water-soluble crosslinking agent (curing agent) is preferably used for crosslinking. Specific examples of the crosslinking agent include melamine and isocyanate.

[0040] On the other hand, the aqueous resin is not particularly limited, but examples thereof include water-soluble or water-dispersible polyester resins, urethane resins, acrylic resins, epoxy resins, phenolic resins, and mixed resins of two or more of these resins.

[0041] The content of the resin that can be contained in the organic coating layer is not particularly limited, but is, for example, 10 to 90 mass% relative to the total mass of the organic coating layer (i.e., the mass of the total solid content of the organic coating layer). The content of the resin is preferably 20 to 80 mass%, more preferably 25 to 75 mass%, relative to the total mass of the organic coating layer, from the viewpoint of exhibiting the function as a binder and achieving both adhesion to adjacent layers, coatings, or steel sheets and corrosion resistance.

[0042] The color pigment that can be contained in the organic coating layer is not particularly limited, and any color pigment can be used depending on the desired appearance, design, etc. Examples of such color pigments include aluminum pigments, carbon black, silica, titania, zirconia, etc. The content of the color pigment is not particularly limited, but may be, for example, about 1 to 60 mass % relative to the total mass of the organic coating layer.

[0043] The rust-preventive pigment that can be contained in the organic coating layer is not particularly limited, but examples thereof include aluminum tripolyphosphate; Zn salt, Mg salt, Al salt, Ti salt, Zr salt, or Ce salt of phosphoric acid or phosphorous acid; hydrocalumite-treated phosphate compounds; Ca ion-exchanged silica; amorphous silica, etc. The content of the rust-preventive pigment is not particularly limited, but examples thereof include a content of about 1 to 40 mass% relative to the total mass of the organic coating layer.

[0044] The lubricant that can be contained in the organic coating layer is not particularly limited, but examples thereof include polyolefin wax, paraffin wax, fluororesin wax, etc. The content of the lubricant is not particularly limited, but examples thereof include a content of about 0.1 to 10 mass % relative to the total mass of the organic coating layer.

[0045] The amount of the organic coating layer (i.e., the mass of the total solid content of the organic coating layer per unit area) is not particularly limited, but may be, for example, 2 to 20 g / m 2When the coating weight of the organic coating layer is within this range, the adhesion between the organic coating layer and the adjacent layer, film, or steel sheet is improved, and the above-mentioned effects of the nitrite can be more reliably obtained. The coating weight of the organic coating layer is preferably 2 to 15 g / m 2 is.

[0046] The thickness of the organic coating layer is not particularly limited, but may be, for example, about 1 to 50 μm. From the viewpoints of adhesion, corrosion resistance, and the effects of the nitrite, the thickness of the organic coating layer is preferably 3 μm or more, more preferably 5 μm or more, and even more preferably 10 μm or more. The thickness of the organic coating layer is preferably 30 μm or less.

[0047] As described above, the organic coating layer may be disposed on each of both surfaces of the steel sheet with or without a plating layer and a chemical conversion coating therebetween, or may be disposed on only one surface of the steel sheet with or without a plating layer and a chemical conversion coating therebetween. Furthermore, as described above, the organic coating layer may be disposed over the entire surface of the steel sheet, or may be disposed on only a portion of the surface of the steel sheet.

[0048] The method for forming the organic coating layer is not particularly limited, but after preparing a coating composition containing at least the specific amount of nitrite as described above, the organic coating layer can be formed by applying this coating composition to the surface of the steel sheet or the plating layer or chemical conversion coating formed on the surface of the steel sheet, and then heating and drying. The means for applying the coating composition is not particularly limited, but any coating process such as electrodeposition coating, powder coating, solvent coating, etc. can be used.

[0049] The organic coating layer may have a single-layer structure consisting of a single layer, or may have a multi-layer structure consisting of multiple layers. When the organic coating layer has a multi-layer structure, an example of the multi-layer structure includes a multi-layer structure consisting of an undercoat layer, an intermediate coat layer, and a top coat layer.

[0050] 1 , plating layers 4 are formed on both sides of a steel sheet 2 and are disposed between the steel sheet 2 and an organic coating layer 3. More specifically, in the organic coated steel sheet 1, a chemical conversion coating 5 is disposed between the steel sheet 2 and the organic coating layer 3, and the plating layer 4 is disposed between the chemical conversion coating 5 and the steel sheet 2. It should be noted that the presence of the chemical conversion coating 5 is not an essential constituent feature of the organic coated steel sheet 1, and therefore the organic coating layer 3 may be disposed directly on the surface of the plating layer 4.

[0051] Generally, the formation of a plating layer such as zinc plating is prone to hydrogen generation, resulting in a higher risk of hydrogen embrittlement cracking. However, even though the organic coated steel sheet 1 of the present embodiment has the plating layer 4, the specific amount of nitrite contained in the organic coating layer 3 as described above makes it difficult to generate hydrogen, which causes hydrogen embrittlement cracking. Therefore, the organic coated steel sheet 1 can suppress hydrogen embrittlement cracking while enjoying the advantages of having the plating layer 4 (e.g., improved corrosion resistance, etc.).

[0052] The plating layer 4 may be either a hot-dip plating layer or an electroplated layer. Examples of the hot-dip plating layer include a hot-dip galvanized layer (GI), a galvannealed layer (GA), a hot-dip aluminum plating layer, a hot-dip Zn—Al alloy plating layer, a hot-dip Zn—Al—Mg alloy plating layer, and a hot-dip Zn—Al—Mg—Si alloy plating layer. Examples of the electroplated layer include an electrogalvanized layer (EG) and an electrolytic Zn—Ni alloy plating layer. Of these, the plating layer is preferably a hot-dip galvanized layer, a galvannealed layer, or an electrogalvanized layer.

[0053] The coating weight of the plating layer is not particularly limited, but for example, it is 10 to 180 g / m per side. 2 The coating weight of the plating layer is determined by dissolving the plating layer in an acid solution to which an inhibitor that suppresses corrosion of the base steel has been added, and then measuring the change in weight before and after pickling.

[0054] The thickness of the plating layer is not particularly limited, but may be, for example, about 3 to 50 μm.

[0055] In the organic coated steel sheet 1 shown in Fig. 1 , the plating layer 4 is disposed on each of both surfaces of the steel sheet 2, but this is not a limitation. That is, the plating layer 4 may be disposed on each of both surfaces of the steel sheet 2 as shown in Fig. 1 , or may be disposed on only one surface of the steel sheet 2. In the organic coated steel sheet 1 shown in Fig. 1 , the plating layer 4 is disposed over the entire surface of the steel sheet 2, but this is not a limitation. That is, the plating layer 4 may be disposed over the entire surface of the steel sheet 2 as shown in Fig. 1 , or may be disposed on only a portion of the surface of the steel sheet 2.

[0056] It should be noted that the presence of a plating layer is not an essential constituent requirement for the organic coated steel sheet of the present invention, and therefore the organic coated steel sheet of the present invention may or may not have a plating layer depending on the required properties of the final product to which it is applied.

[0057] 1 , the chemical conversion coating 5 is formed on the surface of the above-mentioned plating layer 4 and is disposed between the plating layer 4 and the organic coating layer 3. It is not essential that the organic coated steel sheet 1 has the plating layer 4, and therefore the above-mentioned chemical conversion coating 5 may be disposed directly on the surface of the steel sheet 2.

[0058] The chemical conversion coating 5 functions to improve the barrier properties and adhesion against corrosion factors such as moisture and corrosive ions, and as a result, the corrosion resistance of the organic coated steel sheet 1 can be improved.

[0059] The components forming the chemical conversion coating 5 are not particularly limited, but examples include phosphoric acid, phosphates, silica, fluorides, vanadium compounds, silane coupling agents, zirconium compounds, resins, tannin, and tannic acid. Among these components, at least one component selected from the group consisting of phosphoric acid, phosphates, silica, fluorides, and vanadium compounds is preferred. When the chemical conversion coating is formed from such components, the chemical conversion coating functions as an inhibitor, forming a precipitated film or a passive film on the plating layer or the surface of the steel sheet, thereby further improving corrosion resistance.

[0060] Examples of phosphates that can be used to form the chemical conversion coating include crystalline and amorphous phosphates. More specifically, examples of crystalline phosphates include zinc phosphate, zinc iron phosphate, manganese phosphate, manganese iron phosphate, and zinc calcium phosphate. Examples of amorphous phosphates include iron phosphate, tin phosphate, zirconium phosphate, titanium phosphate, and hafnium phosphate.

[0061] Examples of fluorides that can be used to form the chemical conversion coating include zirconium fluoride, titanium fluoride, hafnium fluoride, indium fluoride, etc. Examples of vanadium compounds that can be used to form the chemical conversion coating include vanadium oxide, etc.

[0062] The chemical conversion coating may contain a nitrite similar to that contained in the organic coating layer. In this case, the amount of nitrite contained in the chemical conversion coating is not particularly limited, but may be, for example, about 1 to 30 mass % relative to the total mass of the chemical conversion coating (i.e., the mass of all solids in the chemical conversion coating). If the chemical conversion coating also contains such a nitrite, it can further reduce the generation of hydrogen, which causes hydrogen embrittlement cracking.

[0063] The amount of the chemical conversion coating (i.e., the mass per unit area of ​​the total solid content of the chemical conversion coating) depends on the components that form it, and is not particularly limited, but for example, it is 10 to 2000 mg / m per side. 2 The deposition amount of the chemical conversion coating is preferably 100 to 1500 mg / m 2 is.

[0064] The deposition weight of the chemical conversion coating can be measured by known analytical methods such as fluorescent X-ray analysis. For example, a calibration curve showing the relationship between fluorescent X-ray intensity and deposition weight can be prepared in advance using a sample whose phosphorus deposition amount is known by chemical analysis, and the deposition weight of the chemical conversion coating can be determined from the measurement results of the fluorescent X-ray intensity using this calibration curve.

[0065] The thickness of the chemical conversion coating also depends on the components that form it, and is not particularly limited, but examples thereof include a thickness of about 0.01 to 5.00 μm, and the thickness of the chemical conversion coating is preferably 0.03 to 3.00 μm.

[0066] In the organic-coated steel sheet 1 shown in FIG. 1 , the chemical conversion coating 5 is disposed on each of both surfaces of the steel sheet 2 via a plating layer 4, but this is not a limitation. That is, the chemical conversion coating 5 may be disposed on each of both surfaces of the steel sheet 2 with or without a plating layer 4 therebetween, as in FIG. 1 , or may be disposed on only one surface of the steel sheet 2 with or without a plating layer 4 therebetween. Also, in FIG. 1 , the chemical conversion coating 5 is disposed over the entire surface of the steel sheet 2, but this is not a limitation. That is, the chemical conversion coating 5 may be disposed over the entire surface of the steel sheet 2 as in FIG. 1 , or may be disposed on only a portion of the surface of the steel sheet 2.

[0067] The method for forming the chemical conversion coating is not particularly limited, but for example, the chemical conversion coating can be formed as follows. First, the surface of the steel sheet or the surface of the plating layer on which the chemical conversion coating is to be formed is subjected to known degreasing and cleaning processes to remove impurities such as oil and surface oxides that have adhered. Next, a composition for forming a chemical conversion coating containing the various components described above is applied to this surface by coating or immersion. The composition adhered to the surface is then dried under any drying conditions to form the chemical conversion coating.

[0068] It should be noted that the presence of a chemical conversion coating is not an essential constituent requirement for the organic coated steel sheet of the present invention, and therefore the organic coated steel sheet of the present invention may or may not have a chemical conversion coating depending on the required properties of the final product to which it is applied.

[0069] (Other Coatings) Various components of the organically coated steel sheet 1 of this embodiment have been described above with reference to Fig. 1, but the organically coated steel sheet of the present invention is not limited to the configuration shown in Fig. 1. For example, the organically coated steel sheet may have a functional coating, such as a primer coating, interposed between the steel sheet and the organic coating layer to further improve adhesion and corrosion resistance.

[0070] Examples of the primer coating include a chromate coating and a primer coating that is substantially free of chromium (i.e., a chromate-free coating). The chromate-free coating can be formed using a treatment liquid such as a silica-based treatment liquid containing a silicon compound such as liquid-phase silica, vapor-phase silica, or silicate as the main coating component, or a zircon-based treatment liquid containing a zircon-based compound as the main coating component. These treatment liquids may contain an organic resin together with the main coating component.

[0071] The deposition amount of the base treatment coating (i.e., the mass per unit area of ​​the total solid content of the base treatment coating) can be any amount depending on the treatment liquid used. For example, in the case of a base treatment coating made from a silica-based treatment liquid, the deposition amount is 1 to 20 mg / m2 in terms of Si. 2 The amount of adhesion can be adjusted to about 100%.

[0072] (Application examples of organic coated steel sheet) As described above, the organic coated steel sheet of the present invention is a high-strength steel sheet that can suppress hydrogen embrittlement cracking, and therefore can be processed into formed bodies or the like and applied to structural members in various fields such as various structural parts for transportation machinery including automobiles, industrial machinery, home appliances, etc., and various architectural structures.

[0073] In particular, the organic-coated steel sheet of the present invention is preferably used as a structural member in the automotive field. Steel sheets used in structural members in the automotive field are often used in atmospheric corrosive environments, and hydrogen embrittlement cracking caused by the penetration of hydrogen generated in such environments can be a major problem. Therefore, when the organic-coated steel sheet of the present invention is applied to structural members in the automotive field, the effect of the present invention, that is, the ability to suppress hydrogen embrittlement cracking, can be particularly suitably exerted.

[0074] Furthermore, when the organic coated steel sheet of the present invention is applied to structural members in the various fields as described above, the forming method is not particularly limited, and any forming method can be adopted depending on the structure, properties, etc. of the structural member to be applied. Examples of such forming methods include, but are not limited to, cold pressing.

[0075] The present invention includes a formed body obtained by forming the above-mentioned organic-coated steel sheet into a predetermined shape by any such forming method. That is, the present invention includes, as an embodiment different from the above-mentioned embodiment, a formed body obtained by using the organic-coated steel sheet 1 of the above-mentioned embodiment.

[0076] [Formed Article] Hereinafter, a formed article formed using the organic coated steel sheet 1 of the above-described embodiment, which is another embodiment of the present invention, will be described.

[0077] The formed body of this embodiment can be obtained by forming, by any forming method and under any forming conditions, the organically coated steel sheet 1 of the above-described embodiment, i.e., the organically coated steel sheet 1 including a steel sheet 2 having a tensile strength of 980 MPa or more and a plating layer 4, a chemical conversion coating 5, and an organic coating layer 3 disposed on each of both surfaces of the steel sheet 2. Alternatively, the formed body of this embodiment can be obtained by forming an organic coating layer similar to the organic coating layer 3 of the organically coated steel sheet 1 of the above-described embodiment on a formed body that has been formed in advance by any forming method and under any forming conditions.

[0078] In the latter case, the specific manufacturing method of the molded body before forming the organic coating layer is not particularly limited, and for example, a commonly used molding method such as hot stamping and normal molding conditions corresponding to the molding method can be adopted. For example, when manufacturing the molded body by hot stamping, the molded body can be manufactured by heating the steel sheet in a predetermined temperature range and for a holding time, and then hot stamping in the predetermined temperature range.

[0079] The molded body of this embodiment is also a high-strength molded body that can suppress hydrogen embrittlement cracking, and can therefore be suitably used as structural members in a variety of fields, such as various structural parts for transportation machinery including automobiles, industrial machinery, home appliances, etc., and various architectural structures.

[0080] The organic coated steel sheet of the present invention and the molded body made using the same, as well as the molded body obtained by forming an organic coating layer on the molded body, are not limited to the above-mentioned embodiments or the examples described below, and can be appropriately combined, substituted, modified, etc. within the scope that does not deviate from the purpose and intent of the present invention.

[0081] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to these examples.

[0082] In order to verify the effects of the present invention, unplated steel sheets and galvanized steel sheets having tensile strengths of 1470 MPa to 3000 MPa and steel compositions shown in Tables 1 and 2 below were prepared as test materials, and organic coated steel sheet samples serving as examples of the present invention were produced according to the following procedure.

[0083] (Pretreatment step) The steel sheet of the test material was immersed in an aqueous solution containing 2.5 mass % of an aqueous alkaline degreasing agent (manufactured by Nippon Parkerizing Co., Ltd., "FC-301") at a temperature of 40°C for 2 minutes to degrease the surface of the steel sheet. Furthermore, the degreased steel sheet was washed with water and dried.

[0084] (Chemical conversion treatment step) Solid nitrite was dissolved in a zinc phosphate-based chemical conversion treatment solution (manufactured by Nippon Paint Industrial Coating Co., Ltd., "Surfdyne SD5350 series"), and a zinc phosphate coating was formed in an amount of 2.3 g / m 2 The immersion treatment time was adjusted so that the steel sheet after the above pretreatment step was then transferred to a hot air furnace and dried in a state where the surface temperature reached 70°C, thereby forming a zinc phosphate coating (i.e., chemical conversion coating) with a predetermined adhesion amount on the surface of the steel sheet.

[0085] (Painting step) The steel sheet after the chemical conversion treatment step was coated with a paint composition containing the following base paint and a nitrite-containing pigment to form an organic coating layer on the surface of the steel sheet. Note that the steel sheet of Sample No. 1 in Table 3 was not subjected to this painting step, and is a steel sheet on which no organic coating layer is formed. This steel sheet contains sodium nitrite, a nitrite, in the chemical conversion treatment coating.

[0086] The base paint used was a polyester-based clear paint obtained as follows: This polyester-based clear paint was prepared by dissolving a commercially available organic solvent-soluble amorphous polyester resin, "Vylon (registered trademark) GK140" manufactured by Toyobo Co., Ltd., in an organic solvent (an organic solvent obtained by mixing Solvesso (registered trademark) 150 and cyclohexanone in a mass ratio of 1:1), to which was added 15 parts by mass of "Cymel (registered trademark) 303" manufactured by Mitsui Cytec Co., Ltd., a commercially available hexamethoxymethylmelamine crosslinking agent, per 100 parts by mass of the polyester resin solids, and further adding 0.5 parts by mass of "Catalyst (registered trademark) 6003B" manufactured by Mitsui Cytec Co., Ltd., a commercially available acidic catalyst.

[0087] The nitrite-containing pigment was adjusted so that the nitrite content in the organic coating layer, in terms of nitrite radical, matched the ion-equivalent salt content (mass %) of the organic coating layer shown in Tables 3 to 8. Specifically, the pigment was prepared by adding a commercially available pigment to an aqueous solution containing solid nitrite, followed by stirring. The type of nitrite used is shown in Tables 3 to 8 below as "salt contained in organic coating layer." Note that the steel sheet of Sample No. 2 in Table 3 does not contain salts such as nitrite in the organic coating layer. This steel sheet contains sodium nitrite, a nitrite, in the chemical conversion coating. The steel sheets of Samples No. 49 and 50 in Table 4 contain sodium chloride and sodium nitrate in the organic coating layer instead of nitrite. These steel sheets also contain sodium chloride and sodium nitrate in the chemical conversion coating.

[0088] The coating composition was prepared by mixing the base coating with the nitrite-containing pigment in a mass ratio of 7:3, and thoroughly stirring with a mixer to disperse the mixture. The mass ratio is the mass ratio of the solids excluding the solvent.

[0089] The coating compositions prepared in this way were applied by bar coating to the surfaces of the steel sheets after the chemical conversion treatment process. The steel sheets were then transferred to a hot air oven and dried and air-dried in a state where the temperature of the steel sheet surface reached 230°C, forming organic coating layers on the surfaces of the steel sheets. In this coating process, the dilution conditions and bar size were adjusted so that the thicknesses of the formed organic coating layers were 1 μm, 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, and 30 μm, respectively.

[0090] For each sample of organically coated steel sheet obtained through the above pretreatment, chemical conversion coating, and painting processes, the organic coating layer was analyzed and hydrogen embrittlement cracking was evaluated as follows. The results are shown in Tables 3 to 8 below.

[0091] (Analysis of Nitrite Radicals in Organic Coating Layer) First, the organic coating layer was collected from a sample of organically coated steel sheet to be analyzed, homogenized using a Polytron homogenizer, and extracted under weakly alkaline conditions. Then, after removing the resin component from the extract by suction filtration, the content of nitrite radicals in the organic coating layer (ion-equivalent content of salts contained in the organic coating layer in g / m ) was determined by a colorimetric method utilizing color development due to diazotization. 2 ) was measured. When the organic coating layer was sampled from the sample of organic-coated steel sheet to be analyzed, the organic coating layer was sampled from the edge, welded part, processed part and part affected by these, and part other than the part where the organic coating layer was poorly formed. From the viewpoint of increasing the detection sensitivity, the larger the sampled amount, the better.

[0092] (Evaluation of Hydrogen Embrittlement Cracking) The steel plate to be evaluated was cut to obtain a flat plate measuring 100 mm x 15 mm. Next, both longitudinal ends of this flat plate were ground by 2.5 mm each by mechanical grinding to obtain a flat test piece measuring 100 mm x 10 mm. A corrosion test was performed on this test piece according to the standard JASO M 609-91 (Corrosion Test Method for Automotive Materials) to corrode the test piece and promote hydrogen embrittlement cracking. A stress of 1250 MPa equivalent to YS was applied to this corroded test piece using an apparatus 6 for evaluating hydrogen embrittlement cracking of steel plate shown in Figure 2, and the plate thickness of the test piece at fracture was measured.

[0093] 2 includes a holder 7 for holding a test piece 10 and bolts 8, which are stress applying means for applying stress to the test piece 10. In the test piece 6 shown in FIG. 2, the holder 7 is configured as a structure having a loading jig 7a and a receiving jig 7b, and is configured to be able to perform a four-point bending test in which the test piece 10 is bent by two fulcrums of the loading jig 7a and two fulcrums of the receiving jig 7b.

[0094] Furthermore, prior to applying a stress of 1250 MPa to the above-mentioned test piece, the steel plate was bent by tightening the bolt 8 of the device 6 shown in Figure 2, and the tightening amount of the bolt 8 was determined so that the target stress would be applied to the convex portion of the bent steel plate. Specifically, a strain gauge was attached in the tensile direction at the apex of the convex portion of the bent steel plate, and the relationship between the strain at the apex of the convex portion of the steel plate due to bending of the steel plate by tightening the bolt 8 and the tightening amount of the bolt 8 was measured in advance. Then, the strain value of the steel plate at the stress desired to be applied to the test piece was read from the strain-stress curve, and the bolt 8 was tightened so as to obtain the desired strain value.

[0095] The evaluation of hydrogen embrittlement cracking for each steel plate was carried out by confirming the presence or absence of hydrogen embrittlement cracking in a corrosion test. Cracking of steel plates during corrosion can be classified into hydrogen embrittlement cracking and metal thinning cracking due to a reduction in plate thickness and strength caused by corrosion. The two types of cracking were distinguished by calculating the percent reduction in plate thickness (%) before and after corrosion using the plate thickness of the test specimen before corrosion and the plate thickness when the test specimen after corrosion was fractured using the apparatus 6 shown in Figure 2 , and evaluating the percent reduction in plate thickness according to the following evaluation criteria. The plate thickness when the test specimen after corrosion was fractured was measured at the portion exposed through the opening of the receiving jig 7b in the jig shown in Figure 2 , which is the portion exposed to saltwater during the corrosion test. Specifically, the plate thickness was measured within 1 cm on either side of the two supports of the loading jig 7a, which is the center of the test specimen. Excellent: The thickness reduction rate is 30% or more (thinning cracks have occurred, not hydrogen embrittlement cracks) Good: The thickness reduction rate is 20% or more but less than 30% (almost no hydrogen embrittlement cracks have occurred) Fair: The thickness reduction rate is 10% or more but less than 20% (little hydrogen embrittlement cracks have occurred) Poor: The thickness reduction rate is less than 10% (hydrogen embrittlement cracks have occurred)

[0096]

[0097]

[0098]

[0099]

[0100]

[0101]

[0102]

[0103]

[0104] As shown in Tables 3 to 8, the organically coated steel sheets of the examples of the present invention were able to sufficiently suppress hydrogen embrittlement cracking caused by hydrogen during corrosion because the organic coating layer contained a specific amount of nitrite. In contrast, the steel sheets of the comparative examples were unable to suppress hydrogen embrittlement cracking caused by hydrogen during corrosion because they did not have an organic coating layer or the organic coating layer did not contain a specific amount of nitrite.

[0105] The organic coated steel sheet of the present invention is a high-strength steel sheet that can suppress hydrogen embrittlement cracking, and therefore can be suitably used for structural members in various fields, such as various structural parts for transportation machinery including automobiles, industrial machinery, home appliances, and various architectural structures.

[0106] 1 Organic coated steel sheet 2 Steel sheet 3 Organic coating layer 4 Plating layer 5 Chemical conversion coating

Claims

1. A steel sheet having a tensile strength of 980 MPa or more and an organic coating layer disposed on at least a part of the surface of the steel sheet, wherein the organic coating layer contains 1 to 30 mass% of nitrite as nitrite ion and 0.05 g / m 2 An organic coated steel sheet, characterized in that it contains the above content.

2. The organic coated steel sheet according to claim 1, wherein the nitrite is at least one selected from the group consisting of lithium salts, sodium salts, potassium salts, magnesium salts, calcium salts, strontium salts, barium salts, and ammonium salts.

3. The organic coated steel sheet according to claim 1 or 2, characterized in that a plating layer is disposed between the steel sheet and the organic coating layer.

4. The organic coated steel sheet according to claim 1 or 2, characterized in that the tensile strength of the steel sheet is 1.2 to 3.0 GPa.

5. The organic coated steel sheet according to claim 3, characterized in that the tensile strength of the steel sheet is 1.2 to 3.0 GPa.

6. A molded article made using the organic coated steel sheet according to claim 1 or 2.

7. A molded article made using the organic coated steel sheet according to claim 3.

8. A molded article made using the organic coated steel sheet according to claim 4.

9. A molded article made using the organic coated steel sheet according to claim 5.

Citation Information

Patent Citations

  • Chromate-free chemically converted galvanized steel sheet having excellent corrosion resistance at cut edge face

    JP2010126764A

  • Chemical conversion steel sheet

    JP2021011612A

  • Hot stamping alloyed hot-dip galvanized steel sheet, hot stamping molding and method for manufacturing them

    JP2022131411A

  • Fe-BASED ELECTRIC PLATING HIGH-STRENGTH STEEL SHEET AND METHOD FOR PRODUCING THE SAME