Catalyst for ammonia synthesis which exhibits high activity under low-pressure and low-temperature conditions, and ammonia synthesis method using same

The catalyst system with a support and metal cocatalyst enhances ammonia synthesis efficiency at lower pressures and temperatures, addressing the energy and emissions issues of the Haber-Bosch process and improving hydrogen storage and transportation by increasing the ammonia synthesis rate and reducing energy consumption.

WO2024228414A1PCT designated stage expired Publication Date: 2024-11-07KOREA INST OF ENERGY RES
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/KR2023/006166
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-04
Publication Date
2024-11-07

AI Technical Summary

Technical Problem

The Haber-Bosch process for ammonia synthesis requires high pressure and temperature, leading to high energy consumption and greenhouse gas emissions, with catalytic activity inhibited by competitive adsorption of nitrogen and hydrogen, resulting in a low ammonia synthesis rate of around 20%. Additionally, the energy density of green hydrogen is low when pressurized and liquefied for transportation, making it difficult to achieve price competitiveness.

Method used

A catalyst system comprising a support coated with a first metal catalyst and a second metal cocatalyst, where the support can be Al2O3, SiO2, or other oxides, and the metals include iron, ruthenium, cobalt, nickel, or osmium, with lithium, sodium, or barium, allowing ammonia synthesis at lower pressures (below 100 atm) and temperatures (300-400°C), enhancing ammonia synthesis efficiency and reducing energy consumption.

Benefits of technology

The catalyst system achieves a higher ammonia synthesis rate than existing commercial catalysts under low pressure and temperature conditions, significantly reducing energy consumption and carbon dioxide emissions, while promoting nitrogen dissociation and hydrogenation reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure KR2023006166_07112024_PF_FP_ABST
    Figure KR2023006166_07112024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention relates to a catalyst for ammonia synthesis including a cocatalyst, and an ammonia synthesis method using same. According to the catalyst material of the present invention and the method for preparing same, ammonia can be synthesized with high efficiency at a lower temperature and pressure compared to those of conventional commercial Haber-Bosch processes, and thus the present invention has the effects of significantly reducing process energy consumption and carbon dioxide emissions.
Need to check novelty before this filing date? Find Prior Art

Description

Catalyst for ammonia synthesis showing high activity under low pressure and low temperature conditions and method for synthesizing ammonia using the same

[0001] The present invention relates to a catalyst for ammonia synthesis that exhibits high activity under low pressure and low temperature conditions and a method for synthesizing ammonia using the same.

[0002] Ammonia is a compound composed of nitrogen and oxygen. Its molecular formula is NH3. It exists as a gas at room temperature with a pungent odor. Small amounts are present in the atmosphere, trace amounts in natural waters, and even in soil, where it is produced by bacteria decomposing nitrogenous organic compounds. Ammonia is used as a raw material in various chemical industries, in the production of ammonia water, and as a solvent for ionic substances.

[0003] The most common method for producing ammonia is the Haber-Bosch process, which synthesizes it from hydrogen and nitrogen. This process is performed at high pressure (over 200 atm) and high temperature (400-500°C) in the presence of an iron or ruthenium catalyst. This reaction consumes a huge amount of energy, approximately 30 GJ / ton NH3, and the fossil fuels used to supply this energy emit a large amount of greenhouse gases equivalent to 1.8 tons CO2 / ton NH3. In addition, catalytic activity can be inhibited due to the competitive nature of nitrogen and hydrogen molecules to adsorb onto the catalyst surface. In addition, nitrogen among the reactants has a very stable triple bond structure, so the ammonia synthesis rate through catalytic reaction is generally only 20%.

[0004] In addition, to achieve the government's target hydrogen supply volume (5.26 million tons / year) by 2040, the government is planning to procure at least 10-50% of the target green hydrogen supply from overseas at low cost from 2030 onwards. However, green hydrogen still has low energy density when pressurized and liquefied for long-distance transport, and hydrogen loss and energy consumption are high during transport, making it difficult to secure price competitiveness. On the other hand, ammonia is evaluated as the most suitable hydrogen storage and transportation medium due to its high hydrogen storage density and easy liquefaction, so technology is needed to convert overseas green hydrogen into ammonia and store and transport it.

[0005] Accordingly, through numerous technological developments and optimization of the Haber-Bosch process, the energy consumption has been reduced to 28 GJ / ton NH3, which is close to the theoretical value. However, in order to reduce the production cost, the energy required for ammonia synthesis must be further reduced, and since existing commercial catalysts are designed to operate under high temperature and high pressure conditions, their ammonia synthesis performance is very low under the low pressure and low temperature conditions we desire, so it is necessary to develop and use a groundbreaking catalyst that can sufficiently synthesize ammonia at much lower pressure (less than 100 atm) and temperature (less than 400°C) than the existing process conditions (400-500°C, more than 200 atm).

[0006] The purpose of the present invention is to provide a novel catalyst material and a method for producing the same, which exhibits a much higher ammonia synthesis rate than existing commercial ammonia synthesis catalysts at lower pressure (less than 100 atm) and lower temperature (400°C) than the existing Haber-Bosch process for producing ammonia.

[0007] The present invention provides a catalyst for ammonia synthesis, comprising: a support on which a first metal catalyst is supported; and a second metal cocatalyst additionally supported on the support on which the first metal catalyst is supported.

[0008] In the ammonia synthesis catalyst of the present invention, the support may be selected from the group consisting of Al2O3, SiO2, Fe2O3, MgO, CeO2, TiO2, ZrO2, V2O5, Cr2O3, Sm2O3 and La2O3, and a carbon component may be coated on the surface of the support.

[0009] In the ammonia synthesis catalyst of the present invention, the first metal may be selected from the group consisting of iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), and osmium (Os), and the first metal catalyst may be included in an amount of 1 to 20 mass% relative to the mass of the support.

[0010] In the ammonia synthesis catalyst of the present invention, the second metal may be selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba), and the second metal cocatalyst may be included in an amount of 0.1 to 3 mmol relative to the mass of the support.

[0011] The present invention provides a method for synthesizing ammonia using the above ammonia synthesis catalyst, and can provide a method for synthesizing ammonia at a temperature of 300 to 400°C and a pressure of 10 to 100 atm in the above ammonia synthesis method.

[0012] The present invention may include a step of (a) supporting a first metal catalyst on a support; and a step of (b) supporting a second metal promoter on the support on which the first metal catalyst is supported, and may include a step of (a) supporting a second metal promoter on a support; and a step of (b) supporting a first metal catalyst on the support on which the second metal promoter is supported.

[0013] In the method for producing a catalyst for ammonia synthesis of the present invention, the support may be selected from the group consisting of Al2O3, SiO2, Fe2O3, MgO, CeO2, TiO2, ZrO2, V2O5, Cr2O3, Sm2O3 and La2O3.

[0014] In the method for producing an ammonia synthesis catalyst of the present invention, the first metal may be selected from the group consisting of iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), and osmium (Os), and the first metal catalyst may be included in an amount of 1 to 20 mass% relative to the mass of the support.

[0015] In the method for producing an ammonia synthesis catalyst of the present invention, the second metal may be selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba), and the second metal cocatalyst may be included in an amount of 0.1 to 3 mmol relative to the mass of the support.

[0016] According to the catalyst material of the present invention and the method for manufacturing the same, ammonia can be synthesized with high efficiency at lower temperature and pressure than the existing commercial Haber-Bosch process, thereby significantly reducing process energy consumption and carbon dioxide emissions.

[0017] Figure 1 is an XRD graph of a catalyst for ammonia synthesis according to the present invention.

[0018] Figure 2 is a SEM image of a catalyst for ammonia synthesis according to the present invention.

[0019] The catalyst for producing ammonia of the present invention will be described in detail with reference to the attached drawings below.

[0020] The drawings presented below are provided as examples to ensure that those skilled in the art can fully understand the spirit of the present invention. Therefore, the present invention is not limited to the drawings presented below and may be embodied in other forms. The drawings presented below may be exaggerated to clarify the spirit of the present invention.

[0021] At this time, if there is no other definition in the technical and scientific terms used, they have the meaning commonly understood by a person of ordinary skill in the technical field to which this invention belongs, and the description of known functions and configurations that may unnecessarily obscure the gist of the present invention is omitted in the following description and attached drawings.

[0022] Additionally, the singular forms used in the specification and the appended claims are intended to include the plural forms as well, unless the context clearly dictates otherwise.

[0023] Additionally, the numerical ranges used herein include lower and upper limits and all values ​​within that range, increments logically derived from the shape and width of the defined range, all doubly defined values, and all possible combinations of upper and lower limits of numerical ranges defined in different shapes. Unless otherwise specifically defined in the specification of the present invention, values ​​outside the numerical range that may arise due to experimental error or rounding of values ​​are also included in the defined numerical range.

[0024] In this specification and the appended claims, the terms first, second, etc. are not used in a limiting sense but are used for the purpose of distinguishing one component from another.

[0025] In this specification and the appended claims, terms such as “include” or “have” mean that a feature or component described in the specification is present, and unless specifically limited, do not preclude the possibility that one or more other features or components may be added.

[0026] In this specification and the appended claims, when a part such as a film (layer), region, component, etc. is said to be on or above another part, it includes not only the case where it is directly above and in contact with another part, but also the case where another film (layer), another region, another component, etc. is interposed therebetween.

[0027]

[0028] The ammonia synthesis catalyst of the present invention is characterized by comprising: a support on which a first metal catalyst is supported; and a second metal co-catalyst additionally supported on the support on which the first metal catalyst is supported.

[0029] In one specific example, the support may be selected from the group consisting of Al2O3, SiO2, Fe2O3, MgO, CeO2, TiO2, ZrO2, V2O5, Cr2O3, Sm2O3 and La2O3, and may be selected from the group consisting of a physical mixture thereof, an alloy obtained by chemical mixing thereof, a form in which another component is supported on a framework of one component, and a form in which another component is impregnated on a framework of one component, but it is most preferable to select MgO or hydrotalcite in which MgO and Al2O3 are mixed.

[0030] By using the support having a large surface area, the metal catalyst is dispersed into small and uniform particles, thereby reducing the unit cost of the catalyst, preventing sintering of the metal catalyst and co-catalyst during long-term use, and promoting the nitrogen dissociation step by supplying electrons to nitrogen molecules like the co-catalyst, and by bonding well with the dissociated nitrogen atoms, it has the advantage of promoting the hydrogenation reaction and the step of generating ammonia.

[0031] In one specific example, the surface of the support may be coated with a carbon component. The carbon component coating increases electrical conductivity, allowing electrons to be rapidly transferred to nitrogen molecules, thereby promoting the reaction. Simultaneously, the first metal catalyst or second metal cocatalyst can be highly dispersed.

[0032] In one specific example, a non-limiting example of the first metal may be a metal selected from the group consisting of iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), and osmium (Os), and preferably ruthenium.

[0033] The first metal catalyst may be included in an amount of 1 to 20 mass% relative to the support mass, preferably 1 to 15 mass%, and most preferably 1 to 10 mass%.

[0034] The average particle diameter of the first metal catalyst may be 0.1 to 50 nm, preferably 0.1 to 20 nm, and most preferably 0.1 to 5 nm. When the first metal catalyst has an average particle diameter within the above range, the reaction sites exposed to the surface area increase, thereby increasing the synthesis performance per unit mass of the first metal, and as the synthesis performance increases, the amount of the first metal used may be reduced, thereby reducing the unit cost of the catalyst.

[0035] In one specific example, the second metal may be an alkali metal or an alkaline earth metal, and non-limiting examples of the second metal include a metal selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba), and preferably barium.

[0036] The second metal cocatalyst may be included in an amount of 0.1 to 3 mmol relative to the mass of the support, preferably 0.3 to 2.5 mmol, and most preferably 0.5 to 2.0 mmol.

[0037] Due to the additional loading of the second metal cocatalyst, there is an advantage in that the nitrogen bonding force is weakened by supplying electrons to nitrogen, which is a reactant of the ammonia synthesis reaction (Lewis base), and the reaction rate of the nitrogen dissociation step (the rate-determining step of the overall reaction) is accelerated, thereby allowing the reaction to proceed in the forward direction.

[0038] In one specific example, the average particle diameter of the ammonia synthesis catalyst may be 1 to 1,000 μm, preferably 2 to 900 μm, and most preferably 3 to 800 μm, but is not limited thereto.

[0039] In addition, the specific surface area of ​​the above ammonia synthesis catalyst through BET measurement is 10 to 200 m 2 / g may be, preferably 20 to 180 m 2 / g can be, most preferably 30 to 150 m 2 / g. The ammonia synthesis catalyst having the above average particle size and specific surface area has the advantage that nitrogen molecules can be easily adsorbed on the surface of the catalyst.

[0040] A method for synthesizing ammonia using the ammonia synthesis catalyst of the present invention is characterized by synthesizing ammonia at a temperature of 300 to 400°C and a pressure of 10 to 100 atm.

[0041] The most common method for producing ammonia is the Haber-Bosch process, which synthesizes ammonia from hydrogen and nitrogen. It is performed at high pressure (over 200 atm) and high temperature (400-500°C) in the presence of a catalyst. This reaction consumes a huge amount of energy, emits a large amount of greenhouse gases, and the catalytic activity can be inhibited due to the competitive nature of nitrogen and hydrogen molecules to adsorb on the catalyst surface. In addition, nitrogen among the reactants has a very stable triple bond structure, so the ammonia synthesis rate through the catalytic reaction is generally only 20%.

[0042] However, the method of synthesizing ammonia using the ammonia synthesis catalyst of the present invention has the effect of significantly reducing process energy consumption and carbon dioxide emissions because it shows a higher ammonia synthesis rate than existing commercial ammonia synthesis catalysts at lower pressure and lower temperature compared to the Haber-Bosch process.

[0043]

[0044] The method for producing an ammonia synthesis catalyst of the present invention is characterized by comprising the steps of: (a) supporting a first metal catalyst on a support; and (b) supporting a second metal promoter on the support on which the first metal catalyst is supported. In addition, the method may comprise the steps of: (a) supporting a second metal promoter on the support; and (b) supporting a first metal catalyst on the support on which the second metal promoter is supported.

[0045] In one specific example, the support may be selected from the group consisting of Al2O3, SiO2, Fe2O3, MgO, CeO2, TiO2, ZrO2, V2O5, Cr2O3, Sm2O3 and La2O3, and may be selected from the group consisting of a physical mixture thereof, an alloy obtained by chemical mixing thereof, a form in which another component is supported on a framework of one component, and a form in which another component is impregnated on a framework of one component, but it is most preferable to select MgO or hydrotalcite in which MgO and Al2O3 are mixed.

[0046] In one specific example, the method for supporting the first metal catalyst may include dissolving the first metal catalyst precursor in a suitable solvent (water, alcohol, acetone, THF, DMF), impregnating the support through a simple wetness impregnation method or a wetness impregnation method, and then drying the solvent and performing a reduction treatment. A vapor deposition method may be used, but there is no particular limitation as long as it is a general supporting method.

[0047] In one specific example, in the method for supporting the first metal catalyst, the first metal may be selected from the group consisting of iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni) and osmium (Os), and preferably may be ruthenium, and at this time, the precursor of the ruthenium catalyst may be ruthenium metal, ruthenium oxide (RuO2; ruthenium oxide), ruthenium red, ruthenium acetylacetonate (Ru(acac)3; ruthenium acetylacetonate), ruthenium chloride (RuCl3; ruthenium chloride), ruthenocene (Bis(cyclopentadienyl) ruthenium), ruthenium nitrosyl nitrate, ruthenium iodide (RuI3; ruthenium iodide), triruthenium dodecacarbonyl (Ru3(CO) 12 ; triruthenium dodecacarbonyl), ruthenium nitrate (Ru(NO3)3; ruthenium nitrate), etc. can be used, but are not limited thereto. At this time, the first metal catalyst may be included in an amount of 1 to 20 mass% relative to the support mass, preferably 1 to 15 mass%, and most preferably 1 to 10 mass%.

[0048] In one specific example, before the step of supporting the first metal catalyst, the first metal catalyst may be additionally pretreated. The pretreatment step is a step of heating and calcining while flowing an inert gas such as nitrogen, argon, helium, or a reducing gas such as ammonia reaction synthesis gas (H2+N2), hydrogen, diluted hydrogen (balance gas: an inert gas such as nitrogen, argon, or hydrogen), carbon monoxide, or diluted carbon monoxide (balance gas: an inert gas such as nitrogen, argon, or hydrogen). The heating temperature varies depending on the component of the first metal, but is preferably heated to 250 to 700°C.

[0049] In one specific example, the method for supporting the second metal promoter may include dissolving the second metal promoter precursor in a suitable solvent (water, alcohol, acetone, THF, DMF), impregnating the support with a simple wetness impregnation method (incipient wetness impregnation), and then drying the solvent and performing a reduction treatment. A vapor deposition method may also be used, but there is no particular limitation as long as it is a general supporting method.

[0050] In one specific example, in the method for supporting the second metal promoter, the second metal may be selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr) and barium (Ba), and preferably barium, and at this time, the barium promoter precursor may be barium nitrate (Ba(NO3)2; barium nitrate), barium hydroxide (Ba(OH)2; barium hydroxide), barium perchlorate (Ba(ClO4)2; barium perchlorate), barium isopropoxide (Ba(OCH(CH3)2)2; barium isopropoxide), barium fluoride (BaF2; barium fluoride), barium oxide (BaO; barium oxide), barium bromide (BaBr2; barium bromide), Barium chloride (BaCl2; barium chloride), barium iodide (BaI2; barium iodide), barium acetate (Ba(CH3COO)2; barium acetate), barium carbonate (BaCO3; barium carbonate), barium sulfate (BaSO4; barium sulfate), etc. can be used, but are not limited thereto. At this time, the second metal promoter can be included in an amount of 0.1 to 3 mmol relative to the mass of the support, preferably 0.3 to 2.5 mmol, and most preferably 0.5 to 2.0 mmol.

[0051] In one specific example, before the step of supporting the second metal promoter, the second metal promoter may be additionally pretreated. The pretreatment step is a step of heating and calcining while flowing a reducing gas such as an inert gas such as nitrogen, argon, or helium, or an ammonia reaction synthesis gas (H2+N2), hydrogen, diluted hydrogen (balance gas: an inert gas such as nitrogen, argon, or hydrogen), carbon monoxide, or diluted carbon monoxide (balance gas: an inert gas such as nitrogen, argon, or hydrogen). The heating temperature varies depending on the component of the first metal, but is preferably heated to 250 to 700°C.

[0052] The present invention is described in detail below through examples. However, these examples are provided for the purpose of explaining the present invention in more detail, and the scope of the present invention is not limited by the following examples.

[0053]

[0054] <Example 1> Preparation of a catalyst for ammonia synthesis

[0055] 1 mmol barium nitrate (Ba(NO3)2) is completely dissolved in distilled water, mixed evenly with 1 g of MgO-based support, and the solvent is completely evaporated through a drying process. The powder is recovered and heat-treated at 500 degrees under nitrogen. Triruthenium dodecacarbonyl (C) is added to the heat-treated powder. 12 O 12 Ru3) Add a solution of 0.05 g dissolved in an organic solvent, stir, and then dry to evaporate the organic solvent.

[0056]

[0057] <Example 2> Preparation of a catalyst with a ruthenium content of 9 wt%

[0058] C 12 O 12 It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that 0.09 g was used instead of 30.05 g of Ru.

[0059]

[0060] <Example 3> Preparation of a catalyst having a barium content of 0.5 mmol / g

[0061] It was prepared using the same manufacturing method as the ammonia synthesis catalyst prepared in Example 1, except that 0.5 mmol was used instead of 21 mmol of Ba(NO3).

[0062]

[0063] <Example 4> Preparation of a catalyst having a barium content of 2.0 mmol / g

[0064] It was prepared using the same manufacturing method as the ammonia synthesis catalyst prepared in Example 1, except that 2.0 mmol was used instead of 21 mmol of Ba(NO3).

[0065]

[0066] <Example 5> Preparation of a catalyst using hydrotalcite as a support

[0067] It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that hydrotalcite was used instead of the MgO series support.

[0068]

[0069] <Comparative Example 1> Preparation of a catalyst not containing ruthenium

[0070] C 12 O 12 It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that Ru3 was not used.

[0071]

[0072] <Comparative Example 2> Preparation of a catalyst not containing barium

[0073] It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that Ba(NO3)2 was not used.

[0074]

[0075] <Comparative Example 3> Preparation of a catalyst with a ruthenium content of 2 wt%

[0076] C 12 O 12 It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that 0.02 g was used instead of 30.05 g of Ru.

[0077]

[0078] <Comparative Example 4> Preparation of a catalyst containing cesium as a cocatalyst

[0079] It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that cesium nitrate (CsNO3) was used instead of barium nitrate (Ba(NO3)2).

[0080]

[0081] <Comparative Example 5> Preparation of a catalyst containing potassium as a cocatalyst

[0082] It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that potassium nitrate (KNO3) was used instead of barium nitrate (Ba(NO3)2).

[0083]

[0084] <Comparative Example 6> Preparation of a catalyst using SiO2 as a support

[0085] It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that a SiO2 series support (silica) was used instead of the MgO series support.

[0086]

[0087] <Comparative Example 7> Preparation of a catalyst using CeO2 as a support

[0088] It was manufactured using the same manufacturing method as the ammonia synthesis catalyst manufactured in Example 1, except that a CeO2 series support (ceria) was used instead of the MgO series support.

[0089]

[0090] <Experimental Example 1> Structural Analysis of a Catalyst for Ammonia Synthesis

[0091] First, the structure of the ammonia synthesis catalyst manufactured through the manufacturing method of Example 1 was observed through X-ray diffraction analysis.

[0092]

[0093] Referring to Figure 1, the presence of crystals of the MgO support is visible, and it can be seen that the barium component used as a cocatalyst exists in the form of an oxide. Barium is easily oxidized in the air and therefore exists in the form of an oxide, but it can be easily oxidized by hydrogen under the ammonia synthesis reaction conditions and act as a cocatalyst. Since the pick of barium nitrate used as a barium precursor is not visible, it can be seen that the barium nitrate precursor is converted into the form of barium or barium oxide during the manufacturing process. In addition, it is difficult to observe the pick of ruthenium or its oxide, which can be seen that the ruthenium is very finely dispersed in the support.

[0094] Next, the specific surface area was measured using the nitrogen physical adsorption method, and it was confirmed that the ammonia synthesis catalyst of Example 1 had a specific surface area of ​​approximately 80 m2 / g.

[0095] Finally, the catalyst for ammonia synthesis was analyzed using SEM, and as shown in Fig. 2, it was confirmed that it had an average particle size of approximately 1 to 300 μm.

[0096]

[0097] <Experimental Example 2> Analysis of ammonia synthesis rate using ammonia synthesis catalyst

[0098] After synthesizing ammonia using the catalysts synthesized through the manufacturing methods of Examples 1 to 5 and Comparative Examples 1 to 7, the ammonia synthesis rate was evaluated. A mixed gas of H2 / N2=3 (molar ratio) was injected top-down into a high-pressure gas phase fixed bed reactor. The reaction was carried out at 50 atm and 400°C, and 5,000 h -1 The reaction was carried out at a reaction flow rate (GHSV), and the results are shown in Table 1.

[0099] Catalyst componentCatalyst content (wt%)Promoter componentPromoter content (mmol / g)Support typeAmmonia synthesis rate (g-NH3 / g-cat·hr)Example 1Ru5Ba1MgO0.8Example 2Ru9Ba1MgO0.79Example 3Ru5Ba0.5MgO0.5Example 4Ru5Ba2MgO0.5Example 5Ru5Ba1Hydrotalcite0.78Comparative Example 1Ru0Ba1MgO~0Comparative Example 2Ru5Ba0MgO0.1Comparative Example 3Ru2Ba1MgO0.2Comparative Example 4Ru5Cs1MgO0.3Comparative Example 5Ru5K1MgO0.2Comparative Example 6Ru5Ba1SiO20.06Comparative Example 7Ru5Ba1CeO20.25

[0100] Referring to Table 1 above, when ammonia was synthesized using the catalysts (support type: MgO or hydrotalcite, first metal catalyst component: Ru, second metal promoter component: Ba) manufactured through the manufacturing methods of Examples 1 to 5, it was found that the ammonia synthesis rate was very excellent compared to the catalysts manufactured through the manufacturing methods of Comparative Examples 1 to 7. In particular, in the case of catalysts containing 3 to 10 wt% of the first metal catalyst and 1 mmol / g of the second metal promoter (Examples 1, 2, and 5), an ammonia synthesis rate of about 0.8 g-NH3 / g-cathr was shown. In general, when an ammonia synthesis rate of 0.3 g-NH3 / g-cathr or more is shown, it can be seen as a higher level than the performance of existing commercial catalysts under the same low pressure conditions, and therefore, it was found that the ammonia synthesis rate was very excellent.

[0101] In comparison, it was found that in the case of a catalyst that did not include a first metal catalyst, such as Comparative Example 1, or did not include a second metal co-catalyst, such as Comparative Example 2, hardly any ammonia was synthesized under the conditions of 50 atm and 400°C.

[0102] In addition, in the case of a catalyst having a different content of the first metal catalyst, such as Comparative Example 3, it was confirmed that the ammonia synthesis rate was significantly lower compared to the catalysts of Examples 1 and 2.

[0103] In addition, it was confirmed that the ammonia synthesis rate was significantly reduced even when the components of the cocatalyst were different, such as in Comparative Examples 4 and 5, or when the types of the support were different, such as in Comparative Examples 6 and 7.

[0104] As described above, the ammonia synthesis catalyst according to the present invention exhibits an excellent ammonia synthesis rate even under low temperature and low pressure conditions, unlike the ammonia synthesis according to the general Haber-Bosch method, by using a specific support, catalyst, and cocatalyst.

Claims

1. A support on which a first metal catalyst is supported; and A catalyst for ammonia synthesis, wherein a second metal cocatalyst is additionally supported on a support on which the first metal catalyst is supported.

2. In paragraph 1, A catalyst for ammonia synthesis, wherein the support is selected from the group consisting of Al2O3, SiO2, Fe2O3, MgO, CeO2, TiO2, ZrO2, V2O5, Cr2O3, Sm2O3 and La2O3.

3. In paragraph 2, A catalyst for ammonia synthesis, wherein a carbon component is coated on the surface of the support.

4. In paragraph 1, A catalyst for ammonia synthesis, wherein the first metal is selected from the group consisting of iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), and osmium (Os).

5. In paragraph 1, A catalyst for ammonia synthesis, wherein the first metal catalyst is included in an amount of 1 to 20 mass% relative to the mass of the support.

6. In paragraph 1, A catalyst for ammonia synthesis, wherein the second metal is selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba).

7. In paragraph 1, A catalyst for ammonia synthesis, wherein the second metal cocatalyst is contained in an amount of 0.1 to 3 mmol relative to the mass of the support.

8. A method for synthesizing ammonia at a temperature of 300 to 400°C and a pressure of 10 to 100 atm using an ammonia synthesis catalyst according to any one of claims 1 to 7. 9.(a) a step of supporting a first metal catalyst on a support; and (b) A method for producing a catalyst for ammonia synthesis, comprising the step of supporting a second metal co-catalyst on a support supporting the first metal catalyst. 10.(a) a step of supporting a second metal catalyst on a support; and (b) A method for producing a catalyst for ammonia synthesis, comprising the step of supporting a first metal catalyst on a support supporting a second metal cocatalyst.

11. In paragraph 9 or 10, A method for producing a catalyst for ammonia synthesis, wherein the support is selected from the group consisting of Al2O3, SiO2, Fe2O3, MgO, CeO2, TiO2, ZrO2, V2O5, Cr2O3, Sm2O3 and La2O3.

12. In paragraph 9 or 10, A method for producing a catalyst for ammonia synthesis, wherein the first metal is selected from the group consisting of iron (Fe), ruthenium (Ru), cobalt (Co), nickel (Ni), and osmium (Os).

13. In paragraph 9 or 10, A method for producing a catalyst for ammonia synthesis, wherein the first metal catalyst is included in an amount of 1 to 20 mass% relative to the mass of the support.

14. In paragraph 9 or 10, A method for producing a catalyst for ammonia synthesis, wherein the second metal is selected from the group consisting of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), and barium (Ba).

15. In paragraph 9 or 10, A method for producing a catalyst for ammonia synthesis, wherein the second metal cocatalyst is included in an amount of 0.1 to 3 mmol relative to the mass of the support.

Citation Information

Patent Citations

  • Ru-based ammonia synthesizing catalyst carried by nano carbon fiber and its prepn.

    CN1389295A

  • Catalyst for ammonia synthesis and method for ammonia synthesis using the same

    JP2019126776A

  • Ammonia synthesis catalyst

    JP6736073B2

  • Metal support, supported metal catalyst, and ammonia synthesis method using said catalyst

    JP6802544B2

  • Carrier for kids and operation system thereof

    KR1020210005422A