Negative electrode active material, negative electrode, secondary battery, and method for producing negative electrode active material
Incorporating silicon carbide into silicon-based particles addresses the mechanical strength and volume expansion issues in silicon-based negative electrodes, improving the lifespan and discharge capacity of lithium secondary batteries by preventing particle breakage and reducing irreversible capacity losses.
Patent Information
- Application Number
- PCT/KR2024/001647
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-02-02
- Filing Date
- 2024-02-05
- Publication Date
- 2024-11-07
AI Technical Summary
Silicon-based negative electrode active materials for lithium secondary batteries face challenges due to high volume expansion and low mechanical strength, leading to reduced cycle life and capacity due to cracking and irreversible capacity issues.
Incorporating silicon carbide into silicon-based particles within the negative electrode active material, with a controlled amount of 0.1 to 1 part by weight, to enhance mechanical stability and prevent particle breakage during charge/discharge cycles, thereby improving electrode lifespan and discharge capacity.
The integration of silicon carbide in silicon-based particles effectively suppresses particle breakage and enhances the lifespan and discharge capacity of lithium secondary batteries, maintaining capacity retention and reducing irreversible capacity losses.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
Negative active material, negative electrode, secondary battery and method for manufacturing negative active material
[0001] This invention claims the benefit of Korean Patent Application No. 10-2023-0058454, filed with the Korean Intellectual Property Office on May 4, 2023, and Korean Patent Application No. 10-2024-0016464, filed with the Korean Intellectual Property Office on February 2, 2024, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a negative electrode active material, a negative electrode, a secondary battery, and a method for manufacturing the negative electrode active material.
[0003] The rapid proliferation of battery-powered electronic devices such as mobile phones, laptops, and electric vehicles has led to a rapid increase in demand for compact, lightweight, and relatively high-capacity secondary batteries. Lithium secondary batteries, with their light weight and high energy density, are attracting attention as power sources for portable devices. Accordingly, active research and development efforts are underway to improve the performance of lithium secondary batteries.
[0004] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrolyte, an organic solvent, etc. In addition, an active material layer including a positive electrode active material and a negative electrode active material, respectively, may be formed on a current collector in the positive electrode and the negative electrode. A lithium-containing metal oxide such as LiCoO2 or LiMn2O4 is used as a positive electrode active material in the positive electrode, and a carbon-based or silicon-based negative electrode active material that does not contain lithium is used as an negative electrode active material in the negative electrode.
[0005] Generally, carbon materials such as graphite are used as the active material for the negative electrode of lithium secondary batteries, but the theoretical capacity density of carbon is 372 mAh / g (833 mAh / cm 3) is. Therefore, to improve the energy density of the negative electrode, silicon (Si), tin (Sn), their oxides and alloys that alloy with lithium are being considered as negative electrode active materials. Among them, silicon-based materials are attracting attention due to their low price and high capacity (4200 mAh / g) compared to carbon-based active materials, and their excellent fast-charging characteristics (see Korean Patent Publication No. 10-2020-0065514).
[0006] The present invention relates to a negative electrode active material, a negative electrode including the same, a secondary battery including the same, and a method for manufacturing the negative electrode active material.
[0007] One embodiment of the present invention provides a negative electrode active material comprising silicon particles and silicon carbide distributed within the silicon particles, wherein the silicon carbide is contained in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material.
[0008] One embodiment of the present invention provides a negative electrode including the negative electrode active material.
[0009] One embodiment of the present invention provides a secondary battery including the negative electrode.
[0010] One embodiment of the present invention provides a method for producing the negative electrode active material.
[0011] According to one embodiment of the present invention, a negative electrode active material includes a small amount of silicon carbide distributed in silicon particles. Silicon carbide has a very strong bonding force and is a mechanically stable material. When it is distributed inside Si, it suppresses particle breakage of the active material due to charge and discharge, thereby improving the electrode life characteristics. Therefore, for example, when a small amount of silicon carbide is distributed inside silicon particles in the above range, the life characteristics of the electrode can be effectively improved. In addition, such a negative electrode active material is advantageous in terms of cost and process because silicon carbide is formed during the reduction process of raw materials without adding a separate material during synthesis.
[0012] Therefore, the negative electrode including the negative electrode active material according to one embodiment of the present invention and the secondary battery including the negative electrode have the effect of improving the discharge capacity, initial efficiency, resistance performance and / or life characteristics of the battery.
[0013] Hereinafter, the present specification will be described in more detail.
[0014] In this specification, when a part is said to "include" a certain component, this does not mean that it excludes other components, but rather that it may include other components, unless otherwise specifically stated.
[0015] In this specification, when it is said that a member is located “on” another member, this includes not only cases where the member is in contact with the other member, but also cases where another member exists between the two members.
[0016] The terms and words used in this specification should not be interpreted as limited to their usual or dictionary meanings, but should be interpreted as meanings and concepts that conform to the technical idea of the present invention based on the principle that the inventor can appropriately define the concept of the term to explain his or her own invention in the best way.
[0017] The terms used in this specification are used solely to describe exemplary embodiments and are not intended to limit the present invention. The singular expressions of terms used herein include plural expressions, unless the context clearly dictates otherwise.
[0018] In this specification, the crystallinity of the structure included in the negative electrode active material can be confirmed through X-ray diffraction analysis, and the X-ray diffraction analysis can be performed using an X-ray diffraction (XRD) analysis device (product name: D4-endavor, manufacturer: bruker), and in addition to the above device, a device used in the art can be appropriately employed.
[0019] In this specification, the presence or absence of elements and the content of elements in the negative active material can be confirmed through inductively coupled plasma (ICP) analysis, and the ICP analysis can be performed using an inductively coupled plasma optical emission spectrometer (ICPAES, Perkin-Elmer 7300).
[0020] In this specification, the average particle diameter (D 50 ) can be defined as the particle size corresponding to 50% of the volume accumulation amount in the particle size distribution curve (graph curve of particle size distribution). The average particle size (D 50 ) can be measured, for example, using a laser diffraction method. The laser diffraction method can generally measure particle diameters from the submicron range to several mm, and can obtain results with high reproducibility and high resolution.
[0021] As used herein, the terms "about," "approximately," and "substantially" are used to mean a range or approximation of a numerical value or degree, taking into account inherent manufacturing and material tolerances, and are used to prevent infringers from unfairly exploiting the disclosure, which includes precise or absolute numerical values provided to aid understanding of the present invention.
[0022] Silicon-based anode active materials, commonly used in lithium secondary batteries, exhibit relatively large volumetric expansion / contraction during charge / discharge and a relatively high irreversible capacity, leading to low initial efficiency. During the charge / discharge reaction of lithium secondary batteries, lithium ions released from the anode are inserted into the anode during charging, and during discharge, lithium ions inserted into the anode are deintercalated from the anode and returned to the anode. However, silicon-based anode active materials exhibit significant volumetric changes and surface side reactions, preventing a significant portion of the lithium inserted into the anode during initial charging from returning to the anode. This increases the initial irreversible capacity. This high initial irreversible capacity leads to a rapid decline in battery capacity and cycle life. Furthermore, silicon-based anode active materials tend to break as charge / discharge cycles progress, resulting in continuous degradation of the battery life. Conventional silicon-based anode active materials are composed solely of pure silicon, which presents a disadvantage in suppressing electrode volumetric expansion due to their low mechanical strength.
[0023] The present invention provides a silicon-based negative electrode active material with improved breakage phenomenon and a method for manufacturing the same, and a lithium secondary battery with improved discharge capacity, initial efficiency, resistance performance, and / or lifespan characteristics by employing the improved negative electrode active material.
[0024] Hereinafter, embodiments of the present invention will be described in detail. However, the embodiments of the present invention may be modified in various ways, and the scope of the present invention is not limited to the embodiments described below.
[0025] <Cathode active material>
[0026] One embodiment of the present invention provides a negative electrode active material comprising silicon particles and silicon carbide distributed within the silicon particles, wherein the silicon carbide is contained in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material.
[0027] Compared to the graphite-based active materials used in the past, silicon-based particles have a significantly higher capacity, so there are many attempts to apply silicon-based particles as negative electrode active materials. However, due to the increased volume expansion rate of silicon-based particles during the charge / discharge process and the various side effects caused by this, they are limited to cases where they are mixed in small amounts with graphite-based active materials.
[0028] According to one embodiment of the present invention, a negative electrode active material is a silicon-based particle containing silicon carbide, which is distributed in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material, thereby effectively improving electrode life characteristics and suppressing particle breakage of the negative electrode active material during the charge / discharge process of a battery. In addition, the negative electrode active material as described above forms silicon carbide during the reduction process of raw materials without adding a separate material during synthesis, which is advantageous in terms of cost and process compared to a method of adding a separate material.
[0029] According to one embodiment, silicon oxide (SiO2) powder is heated to about 1,800°C in a carbon atmosphere (2C) to be reduced to molten silicon. Thereafter, the molten silicon is cooled at a preset cooling rate, for example, about 20 to 70°C / min, to additionally form silicon carbide (SiC) particles in addition to silicon (Si) particles. Through this cooling process, silicon oxide (SiO2) that remained unreacted in the previous reduction process reacts with carbon (C), thereby additionally forming silicon carbide (SiC) particles. Meanwhile, when the cooling process is performed at a preset rate of about 20 to 70°C / min, silicon carbide (SiC) is distributed in the silicon (Si) particles in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material.
[0030] According to one embodiment of the present invention, a negative active material includes silicon particles.
[0031] In one embodiment of the present invention, the silicon-based particles are SiO x (x=0), SiO x (0 <x<2), SiC, 및 Si 합금으로 이루어진 군에서 선택되는 1 이상을 포함할 수 있다.
[0032] The above silicon particles are SiO x (x=0) and SiO x (0 <x<2)로 이루어진 군에서 선택되는 1 이상을 포함할 수 있다.
[0033] The above silicon particles are SiO x (x=0) may be included. The silicon-based particles are SiO based on 100 parts by weight of the negative active material. x (x=0) may contain about 70 parts by weight or more. For example, the silicon-based particles may be SiO based on 100 parts by weight of the negative electrode active material. x(x=0) may contain about 80 parts by weight or more, or 90 parts by weight or more, and may contain 100 parts by weight or less, for example, 99.5 parts by weight or less, or 99 parts by weight or less.
[0034] In one embodiment of the present invention, the silicon-based particles are SiO x When (x=0) is included in the above content range, SiO as the silicon-based particles x (x=0) instead of SiO x (0 <x<2)를 상기 함량 범위로 포함하는 경우와 비교하여 높은 무게당 방전 용량을 발현할 수 있다는 장점이 있다.
[0035] For example, SiO as the silicon-based particles x When (x=0) is included in the above content range, the discharge capacity per weight of the secondary battery including it is about 3400 mAh / g or more, and SiO x (0 <x<2)를 상기 함량 범위로 포함하는 경우, 이를 포함하는 이차전지의 무게당 방전 용량은 약 1400mAh / g이다. 따라서, 본 발명의 일 예에 따른 음극 활물질을 적용한 이차전지는, 상기 실리콘계 입자가 SiO x Since (x=0) is included in the above content range, the silicon particles are SiO x (0 <x<2)를 상기 함량 범위로 포함하는 경우에 비하여 약 2배 이상의 용량을 발휘할 수 있다.
[0036] However, SiO as the silicon particles x In the case of a negative electrode active material including (x=0) in the above content range, particle breakage may occur due to excessive volume expansion during charge and discharge in a secondary battery to which it is applied, which may lower the capacity retention rate, and thus may cause problems in application in actual products. Accordingly, the negative electrode active material according to an example of the present invention is a silicon-based particle having SiO xThe above problem can be improved by including silicon carbide in the silicon-based particles in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material, while including (x=0) in the above content range.
[0037] SiO as the above silicon particles x When (x=0) is included in the above content range and silicon carbide is included in the above content range within the silicon-based particles, when silicon-based particles are used as a negative electrode active material, particle breakage due to volume expansion during charge and discharge is minimized, thereby improving the capacity retention rate of the negative electrode active material, thereby complementing the application problem, and providing a negative electrode, negative electrode, and / or secondary battery that exhibits a relatively high discharge capacity per weight compared to the conventional case.
[0038] In one embodiment of the present invention, pure silicon (Si) particles may be used as the silicon-based particles. Using pure silicon (Si) particles as the silicon-based particles means that, based on 100 parts by weight of the total silicon-based particles, pure Si particles (SiO) that are not combined with other particles or elements x (x=0)) may mean including it in the above range. That is, in one embodiment of the present invention, the silicon-based particles are SiO based on 100 parts by weight of the total silicon-based particles. x It can be made of silicon particles having 100 parts by weight of (x=0).
[0039] In one embodiment of the present invention, the silicon-based particles are SiO based on 100 parts by weight of the negative electrode active material. x (0 <x<2)를 약 10 중량부 이하, 예컨대 5 중량부 이하, 또는 3 중량부 내지 5 중량부로 포함할 수 있다. 즉, 상기 실리콘계 입자는 그 외 미량의 불순물을 더 포함할 수 있다.
[0040] In one embodiment of the present invention, the silicon-based particles may include metal impurities, and at this time, the metal impurities may be metals that may generally be included in silicon-based particles, and may be included in an amount of, for example, about 0.1 part by weight or less based on 100 parts by weight of silicon-based particles.
[0041] In one embodiment of the present invention, the silicon-based particles may exist in, for example, a crystalline or amorphous form, and may or may not be porous. In one example, the silicon-based particles may not be porous. The silicon-based particles may be, for example, spherical or fragment-shaped particles. Alternatively, the silicon-based particles may have a fibrous structure, or may exist in the form of a silicon-containing film or coating.
[0042] The negative active material according to one embodiment of the present invention includes silicon carbide distributed in the silicon particles.
[0043] In this specification, the silicon carbide has a bond of Si and C. Silicon carbide is a material with very strong bonding strength and mechanical stability. When distributed within Si, it suppresses particle breakage of the active material due to charge and discharge, thereby improving electrode life characteristics. Therefore, by distributing silicon carbide within the silicon-based particles as described above, particle breakage of the active material can be prevented, effectively improving electrode life characteristics.
[0044] In one embodiment of the present invention, the silicon carbide may be included in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material. For example, the silicon carbide may be included in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material, the silicon carbide may be included in an amount of about 0.2 part by weight or more and 0.8 part by weight or less based on 100 parts by weight of the total negative electrode active material, and the silicon carbide may be included in an amount of about 0.4 part by weight or more and 0.8 part by weight or less based on 100 parts by weight of the total negative electrode active material.
[0045] Therefore, when a small amount of silicon carbide is distributed inside or on the surface of the silicon-based particles in the above range, the capacity reduction of the electrode can be minimized and the particle breakage of the active material can be effectively prevented, thereby effectively improving the life characteristics of the electrode. In addition, since the negative electrode active material as described above can be formed during the reduction process of the raw material without adding a separate material during synthesis, it is advantageous in terms of cost and process compared to the case where a separate material is added. In one embodiment of the present invention, carbon may be included in an amount of about 0.03 to 0.3 parts by weight based on a total of 100 parts by weight of the negative electrode active material.
[0046] The content of the above silicon carbide can be analyzed using the rietveld refinement method of XRD measuring equipment.
[0047] In one embodiment of the present invention, the average particle diameter (D) of the negative electrode active material 50) may be about 0.01㎛ to 100㎛, for example, 0.5㎛ to 20㎛, or 1㎛ to 10㎛. When the average particle diameter is within the above range, the specific surface area of the particles becomes an appropriate range, so that the viscosity of the negative electrode slurry is formed within an appropriate range. Accordingly, the particles constituting the negative electrode slurry are smoothly dispersed. In addition, since the size of the negative electrode active material has a value equal to or greater than the lower limit, the contact area between the negative electrode active material particles and the conductive material is excellent due to the composite composed of the conductive material and the binder in the negative electrode slurry, so that the possibility of the conductive network continuing increases, thereby increasing the capacity retention rate. On the other hand, when the average particle diameter satisfies a value equal to or less than the upper limit, excessively large particles are excluded, so that the surface of the negative electrode is formed smoothly, thereby preventing the phenomenon of uneven current density during charge and discharge.
[0048] In one embodiment of the present invention, the negative electrode active material generally has a characteristic BET specific surface area. The BET specific surface area of the negative electrode active material is, for example, about 0.01 m 2 / g to 100.0 m 2 / g, or 0.1 m 2 / g to 50.0 m 2 / g, or 0.1 m 2 / g to 10.0 m 2 / g, or 0.5 m 2 / g to 5 m 2 / g. The BET surface area is measured according to DIN 66131 (using nitrogen).
[0049] <Method for manufacturing negative active material>
[0050] One embodiment of the present invention provides a method for producing the aforementioned negative electrode active material. For example, the method includes the steps of reducing silicon dioxide with carbon to silicon; and forming silicon carbide using the carbon remaining after the reduction. The present invention also provides a method for producing the negative electrode active material, including the steps of reducing silicon dioxide with carbon to obtain silicon; and forming silicon carbide by controlling cooling conditions after silicon synthesis.
[0051] The method for manufacturing the above-described negative active material is advantageous in terms of cost and process because it forms silicon carbide during the reduction process of raw materials without adding separate materials during synthesis.
[0052] The step of reducing silicon dioxide to silicon by reacting it with carbon can be carried out at a high temperature of about 1800°C or higher. In addition, if the cooling rate is controlled after the reduction reaction, the silicon dioxide that has not reacted in the reduction process or the remaining carbon reacts to form silicon carbide within the Si. At this time, the cooling rate is in the range of about 20 to 70°C / min, and the content of silicon carbide within the Si can be controlled by controlling the cooling rate. According to one embodiment, the cooling rate is, for example, more than about 20°C / min and less than or equal to 55°C / min, for example, more than or equal to about 23°C / min and less than or equal to 50°C / min. When silicon carbide is formed, a Si-C peak is confirmed when measuring XRD of the Si particles, and the distribution ratio of silicon carbide can be confirmed using the Rietveld refinement method.
[0053] Meanwhile, in this embodiment, a method for manufacturing a negative electrode active material containing silicon carbide was described as described above through silicon reduction and cooling, but it is not limited thereto, and a negative electrode active material containing silicon carbide can also be manufactured by other methods. For example, by injecting nano carbon particles into silicon particles, a negative electrode active material containing silicon carbide in an amount of about 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material can be manufactured.
[0054] <Cathode>
[0055] The negative electrode according to one embodiment of the present invention may include the negative electrode active material described above.
[0056] For example, the negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on at least one surface of the negative electrode current collector. The negative electrode active material layer may include a negative electrode active material formed within Si by silicon carbide manufactured in the process. Furthermore, the negative electrode active material layer may further include a binder, a thickener, and / or a conductive material.
[0057] In one embodiment of the present invention, the negative electrode current collector may generally have a thickness of about 1 μm to 100 μm. The negative electrode current collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and for example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc., aluminum-cadmium alloy, etc. may be used. In addition, the bonding strength of the negative electrode active material may be strengthened by forming fine unevenness on the surface, and the negative electrode current collector may be used in various forms such as a film, sheet, foil, net, porous body, foam, non-woven fabric, etc.
[0058] In one embodiment of the present invention, the thickness of the negative electrode current collector may be about 1 µm or more and 100 µm or less, and the thickness of the negative electrode active material layer may be about 20 µm or more and 500 µm or less. However, the thickness may be modified in various ways depending on the type and purpose of the negative electrode used and is not limited thereto.
[0059] The above negative electrode active material layer can be formed by applying a negative electrode slurry including a negative electrode active material, a binder, a thickener, and / or a conductive agent to at least one surface of a current collector, and drying and rolling.
[0060] In one embodiment of the present invention, the negative electrode slurry may include a negative electrode active material layer composition; and a slurry solvent.
[0061] In one embodiment of the present invention, the solid content of the cathode slurry can satisfy a range of about 5% or more and 40% or less.
[0062] In another embodiment, the solid content of the cathode slurry can satisfy a range of about 5% to 40%, for example, 7% to 35%, or 10% to 30%.
[0063] The solid content of the above negative electrode slurry may refer to the content of the negative electrode active material layer composition included in the negative electrode slurry, and may refer to the content of the negative electrode active material composition based on 100 parts by weight of the negative electrode slurry.
[0064] When the solid content of the above negative electrode slurry satisfies the above range, the viscosity is appropriate when forming the negative electrode active material layer, thereby minimizing particle agglomeration of the negative electrode active material layer composition, thereby enabling efficient formation of the negative electrode active material layer.
[0065] In one embodiment of the present invention, the slurry solvent is not limited to any solvent capable of dissolving the negative electrode active material layer composition, but for example, distilled water may be used.
[0066] According to one embodiment of the present invention, a negative electrode can be formed by coating and drying the negative electrode slurry on a negative electrode current collector layer.
[0067] Through the above drying step, the slurry solvent in the cathode slurry can be dried.
[0068] In one embodiment of the present invention, the negative electrode active material layer composition may include at least one selected from the group consisting of a negative electrode active material; a negative electrode conductive material; and a negative electrode binder.
[0069] In one embodiment of the present invention, the negative electrode active material of the present invention may be used as the negative electrode active material, or the negative electrode active material of the present invention and an additional negative electrode active material may be used together. In this case, a lithium secondary battery with improved overall performance, such as cycle life characteristics, can be manufactured.
[0070] As the above-mentioned additional negative electrode active material, a compound capable of reversible intercalation and deintercalation of lithium may be used. For example, it may be a carbon-based negative electrode active material. In addition, the above-mentioned additional negative electrode active material may be a carbonaceous material such as artificial graphite, natural graphite, graphitized carbon fiber, amorphous carbon, etc.; a metallic compound capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO β(0 < β < 2), SnO2, vanadium oxide, lithium titanium oxide, lithium vanadium oxide, and the like, which can dope and dedope lithium; or a composite including the metallic compound and a carbonaceous material, such as a Si-C composite or a Sn-C composite, and any one or a mixture of two or more of these may be used. In addition, a metallic lithium thin film may be used as the negative electrode active material. In addition, both low-crystalline carbon and high-crystalline carbon may be used as the carbonaceous material. Representative examples of low-crystalline carbon include soft carbon and hard carbon, and representative examples of high-crystalline carbon include natural graphite or artificial graphite in the form of amorphous, plate-like, flaky, spherical, or fiber-like forms, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch derived cokes.
[0071] In one embodiment of the present invention, the negative electrode includes a negative current collector; and a negative electrode active material layer, and the negative electrode active material layer includes a negative electrode active material according to the present invention, and the negative electrode active material may be included in an amount of about 60 parts by weight or more based on 100 parts by weight of the negative electrode active material layer.
[0072] In another embodiment, the negative electrode active material may be included in an amount of about 60 parts by weight or more, for example, about 65 parts by weight or more, or about 70 parts by weight or more, and may be included in an amount of about 95 parts by weight or less, or about 90 parts by weight or less, or about 80 parts by weight or less, based on 100 parts by weight of the negative electrode active material layer composition.
[0073] The negative electrode active material layer composition according to the present invention includes a negative electrode conductive material and a negative electrode binder that can control the volume expansion rate during the charge and discharge process even when the negative electrode active material having a significantly high capacity is used within the above range, so that the performance of the negative electrode is not deteriorated and the negative electrode has excellent output characteristics during charge and discharge.
[0074] In one embodiment of the present invention, the negative active material may have a non-spherical shape and its circularity is, for example, about 0.9 or less, for example, about 0.7 to 0.9, for example, about 0.8 to 0.9, for example, about 0.85 to 0.9.
[0075] In the present invention, the spherical shape is determined by the following formula A, where A is an area and P is a boundary line.
[0076] [Formula A]
[0077] 4πA / P 2
[0078] Previously, graphite compounds were typically used solely as anode active materials. However, with the increasing demand for high-capacity batteries, attempts to mix silicon-based compounds to increase capacity have been increasing. However, silicon-based compounds have limitations in that their volume rapidly expands during the charge / discharge process, damaging the conductive path formed within the anode active material layer and lowering battery performance. Therefore, the type of anode conductive material used together with the anode active material is crucial.
[0079] In one embodiment of the present invention, the negative electrode conductive material may include at least one selected from the group consisting of a dot-shaped conductive material; a planar conductive material; and a linear conductive material.
[0080] In one embodiment of the present invention, the dot-shaped conductive material can be used to improve conductivity of the negative electrode, and refers to a conductive material having conductivity without causing chemical change. For example, the dot-shaped conductive material may be at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black, channel black, paneth black, lamp black, thermal black, conductive fiber, fluorocarbon, aluminum powder, nickel powder, zinc oxide, potassium titanate, titanium oxide, and polyphenylene derivatives, and according to one embodiment, may include carbon black in terms of implementing high conductivity and excellent dispersibility.
[0081] In one embodiment of the present invention, the dot-shaped conductive material has a BET specific surface area of about 40 m 2 / g or more than 70m 2 / g can be less than 45m, for example 2 / g or more than 65m 2 / g or less, or 50m 2 / g or more than 60m 2 / g can be less.
[0082] In one embodiment of the present invention, the particle size of the dot-shaped conductive material may be about 10 nm to 100 nm, for example, about 20 nm to 90 nm, or about 40 nm to 60 nm.
[0083] In one embodiment of the present invention, the negative conductive material may include a planar conductive material.
[0084] The above-mentioned planar conductive material can improve conductivity by increasing planar contact between silicon particles within the cathode, and at the same time, suppress the disconnection of the conductive path due to volume expansion, and is used as a concept including a bulk conductive material or a plate-shaped conductive material.
[0085] In one embodiment of the present invention, the planar conductive material may include at least one selected from the group consisting of plate-shaped graphite, graphene, graphene oxide, and graphite flakes, and may be plate-shaped graphite according to one embodiment.
[0086] In one embodiment of the present invention, the average particle diameter (D) of the surface-shaped conductive material 50 ) may be about 2 ㎛ to 7 ㎛, for example, about 3 ㎛ to 6 ㎛, or about 4 ㎛ to 5 ㎛. When the above range is satisfied, dispersion is easy without causing excessive viscosity increase of the negative electrode slurry due to sufficient particle size. Therefore, the dispersion effect is excellent when dispersion is performed using the same equipment and time.
[0087] In one embodiment of the present invention, the surface-shaped conductive material is D 10 This is about 0.5μm or more and 1.5μm or less, and D 50 This is approximately 2.5 μm or more and 3.5 μm or less, and D 90 This may be approximately 7.0 μm or more and 15.0 μm or less.
[0088] In one embodiment of the present invention, the planar conductive material may be a high-specific surface area planar conductive material having a high BET specific surface area; or a low-specific surface area planar conductive material.
[0089] In one embodiment of the present invention, a high surface area surface conductive material or a low surface area surface conductive material may be used without limitation as the planar conductive material, but according to one embodiment, the planar conductive material according to the present invention may be affected to some extent by dispersion influence on electrode performance, and thus a low surface area surface conductive material that does not cause dispersion problems may be used.
[0090] In one embodiment of the present invention, the surface-shaped conductive material has a BET specific surface area of about 5 m 2 / g can be more than that.
[0091] In another embodiment, the surface-shaped conductive material has a BET surface area of about 5 m 2 / g or more than 500m 2 / g can be less than or equal to 5m, for example 2 / g or more than 300m 2 / g or less, or 5m 2 / g or more than 250m 2 / g can be less.
[0092] In another embodiment, the surface-shaped conductive material is a high surface area surface-shaped conductive material, and has a BET surface area of about 50 m 2 / g or more than 500m 2 / g or less, for example, about 80m 2 / g or more than 300m 2 / g or less, or 100m 2 / g or more than 300m 2 / g can satisfy the range below.
[0093] In another embodiment, the surface-shaped conductive material is a low surface area surface-shaped conductive material, and has a BET surface area of about 5 m 2 / g or more than 40m 2 / g or less, for example 5m 2 / g or more than 30m 2 / g or less, or 5m 2 / g or more than 25m 2 / g can satisfy the range below.
[0094] Other cathode conductive materials may include linear conductive materials such as carbon nanotubes. The carbon nanotubes may be bundle-type carbon nanotubes. The bundle-type carbon nanotubes may include a plurality of carbon nanotube units. For example, the term "bundle type" herein refers to a secondary shape in the form of a bundle or rope in which a plurality of carbon nanotube units are arranged in a substantially identical orientation with their longitudinal axes aligned in parallel or entangled with each other, unless otherwise stated. The carbon nanotube units have a cylindrical shape with a nano-sized diameter of a graphite sheet, and are sp 2 It has a bonding structure. At this time, depending on the angle and structure at which the graphite plane is rolled, it can exhibit the characteristics of a conductor or semiconductor. Compared to entangled type carbon nanotubes, the bundled carbon nanotubes can be uniformly dispersed during the manufacture of the cathode, and can smoothly form a conductive network within the cathode, thereby improving the conductivity of the cathode.
[0095] In one embodiment of the present invention, the negative electrode conductive material may be included in an amount of about 10 parts by weight or more and 40 parts by weight or less based on 100 parts by weight of the negative electrode active material layer composition.
[0096] In another embodiment, the negative electrode conductive material may be included in an amount of about 10 parts by weight or more and 40 parts by weight or less, for example, 10 parts by weight or more and 30 parts by weight or less, or 15 parts by weight or more and 25 parts by weight or less, based on 100 parts by weight of the negative electrode active material layer composition.
[0097] The negative electrode conductive material according to the present invention has a substantially separate composition from the conductive material applied to the positive electrode. That is, the negative electrode conductive material according to the present invention serves to secure the contact between the negative electrode active materials, which undergo a significant volume expansion of the electrode due to charging and discharging, and the positive electrode conductive material serves to provide some conductivity while acting as a buffer during rolling, and thus has a different composition and role from the negative electrode conductive material of the present invention.
[0098] In addition, the negative electrode conductive material according to the present invention is applied to a silicon-based negative electrode active material and has a substantially different composition from the conductive material applied to a graphite-based active material. That is, the conductive material used in an electrode having a graphite-based active material simply has smaller particles than the active material, and thus has the characteristics of improving output characteristics and imparting some conductivity, and is different in composition and role from the negative electrode conductive material applied together with a silicon-based negative electrode active material as in the present invention.
[0099] In one embodiment of the present invention, the planar conductive material used as the aforementioned negative electrode conductive material has a structure and function different from those of carbon-based active materials typically used as negative electrode active materials. For example, the carbon-based active material used as the negative electrode active material may be artificial graphite or natural graphite, and refers to a material processed into a spherical or dot-shaped form to facilitate the storage and release of lithium ions.
[0100] On the other hand, the planar conductive material used as the negative electrode conductive material is a material having a planar or plate-like shape, and can be expressed as plate-like graphite. In other words, it refers to a material included to maintain a conductive path within the negative electrode active material layer, and is a material that secures a planar conductive path within the negative electrode active material layer, rather than a material that plays a role in storing and releasing lithium.
[0101] That is, in the present invention, the use of plate-shaped graphite as a conductive material means that it is processed into a planar or plate-shaped form and used as a material that secures a conductive path rather than a role for storing or releasing lithium. In this case, the included negative electrode active material has high capacity characteristics for lithium storage and release, and serves to store and release all lithium ions delivered from the positive electrode.
[0102] On the other hand, in the present invention, the use of a carbon-based active material as an active material means that it is processed into a dot or spherical shape and used as a material that plays a role in storing or releasing lithium.
[0103] In one embodiment of the present invention, the carbon-based active material, artificial graphite or natural graphite, has a BET specific surface area of about 0.1 m 2 / g or more than 4.5 m 2 / g or less can be satisfied. In addition, the plate-shaped graphite, which is a planar conductive material, has a BET surface area of about 5 m in the form of a planar surface. 2 / g can be more than that.
[0104] In one embodiment of the present invention, the negative electrode binder may include at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluoroelastomer, polyacrylic acid, and materials in which hydrogens thereof are substituted with Li, Na, Ca, etc., and may also include various copolymers thereof.
[0105] The binder according to one embodiment of the present invention serves to hold the negative electrode active material and the negative electrode conductive material in order to prevent distortion and structural deformation of the negative electrode structure during volume expansion and relaxation of the silicon-based negative electrode active material, and any general negative electrode binder satisfying the above-mentioned role can be applied, for example, an aqueous binder can be used, or a PAM-based binder can be used.
[0106] In one embodiment of the present invention, the negative electrode binder may be included in an amount of about 30 parts by weight or less, for example, 25 parts by weight or less, or 20 parts by weight or less, based on 100 parts by weight of the negative electrode active material layer composition, and may be included in an amount of 1 part by weight or more, or 3 parts by weight or more.
[0107] Secondary battery
[0108] A secondary battery according to one embodiment of the present invention may include the negative electrode according to the above-described embodiment. For example, the secondary battery may include a negative electrode, a positive electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte, wherein the negative electrode is the same as the negative electrode described above. Since the negative electrode has been described above, a detailed description thereof will be omitted.
[0109] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on at least one surface of the positive electrode current collector, and including the positive electrode active material.
[0110] In the above positive electrode, the positive electrode current collector is not particularly limited as long as it is conductive and does not cause a chemical change in the battery, and for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the positive electrode current collector may typically have a thickness of about 3 µm to 500 µm, and fine unevenness may be formed on the surface of the current collector to increase the adhesive strength of the positive electrode active material. For example, it may be used in various forms such as a film, sheet, foil, net, porous body, foam, or non-woven fabric.
[0111] The above positive electrode active material may be a commonly used positive electrode active material. For example, the positive electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound having the chemical formula Li 1+c1 Mn 2-c1 Lithium manganese oxides such as O4(0≤c1≤0.33), LiMnO3, LiMn2O3, LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, Cu2V2O7; chemical formula LiNi 1-c2 M c2Ni-site type lithium nickel oxide represented by O2 (wherein, M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B, and Ga, and satisfies 0.01≤c2≤0.5); chemical formula LiMn 2-c3 M c3 Lithium manganese composite oxide represented by O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn, and Ta, and satisfies 0.01≤c3≤0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu, and Zn); or LiMn2O4 in which a portion of Li in the chemical formula is replaced with an alkaline earth metal ion; but is not limited thereto. For example, the positive electrode may be Li-metal.
[0112] The above-described positive electrode active material layer may include a positive electrode conductive material and a positive electrode binder together with the positive electrode active material described above.
[0113] The above-mentioned positive electrode conductive material is used to provide conductivity to the electrode, and in the battery to be formed, as long as it does not cause a chemical change and has electronic conductivity, it can be used without any special restrictions. Examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, summer black, and carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, and the like. One of these may be used alone or a mixture of two or more may be used.
[0114] In addition, the positive electrode binder plays a role of improving the adhesion between positive electrode active material particles and the adhesiveness between the positive electrode active material and the positive electrode current collector. Examples thereof include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated-EPDM, styrene butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these may be used alone or a mixture of two or more thereof may be used.
[0115] The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. Any separator commonly used in secondary batteries can be used without special restrictions, and may have low resistance to ion movement of the electrolyte and excellent electrolyte moisture retention capacity. According to one embodiment, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof, may be used. In addition, a conventional porous non-woven fabric, for example, a non-woven fabric made of high-melting-point glass fiber, polyethylene terephthalate fiber, etc. may be used. In addition, a coated separator containing a ceramic component or a polymer material to secure heat resistance or mechanical strength may be used, and may optionally be used in a single-layer or multi-layer structure.
[0116] Examples of the above electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries.
[0117] For example, the electrolyte may include a non-aqueous organic solvent and a metal salt.
[0118] As the above non-aqueous organic solvent, for example, an aprotic organic solvent such as N-methyl-2-pyrrolidinone, propylene carbonate, ethylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, gamma-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyl tetrahydrofuran, dimethylsulfoxide, 1,3-dioxolan, formamide, dimethylformamide, dioxolan, acetonitrile, nitromethane, methyl formate, methyl acetate, triester phosphate, trimethoxy methane, dioxolan derivatives, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate can be used.
[0119] Among the above carbonate-based organic solvents, ethylene carbonate and propylene carbonate, which are cyclic carbonates, are high-viscosity organic solvents with high dielectric constants and thus can be used as non-aqueous organic solvents because they easily dissociate lithium salts. By mixing and using low-viscosity, low-dielectric constant linear carbonates such as dimethyl carbonate and diethyl carbonate in an appropriate ratio with these cyclic carbonates, an electrolyte having high electrical conductivity can be prepared.
[0120] The metal salt may be a lithium salt, and the lithium salt is a substance that is easily dissolved in the non-aqueous electrolyte, for example, the anion of the lithium salt is F - , Cl - , I - , NO3 - , N(CN)2 -, BF4 - , ClO4 - , PF6 - , (CF3)2PF4 - , (CF3)3PF3 - , (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , (SF5)3C - , (CF3SO2)3C - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - and (CF3CF2SO2)2N - One or more selected from the group consisting of may be used.
[0121] In addition to the electrolyte components, the electrolyte may further include one or more additives, such as, for example, haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethylphosphite, triethanolamine, cyclic ethers, ethylene diamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, or aluminum trichloride, for the purpose of improving the life characteristics of the battery, suppressing battery capacity decrease, and improving the discharge capacity of the battery.
[0122] According to another embodiment of the present invention, a battery module including the secondary battery as a unit cell and a battery pack including the same are provided. The battery module and the battery pack include the secondary battery having a high capacity, high rate characteristics, and cycle characteristics, and thus can be used as a power source for medium- to large-sized devices selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.
[0123] <Examples and Comparative Examples>
[0124] Example 1
[0125] After a reduction reaction using carbon at a high temperature of 1800°C or higher, silicon carbide was formed within Si by controlling the cooling rate as shown in Table 1 below, so that Si and / or unreacted silicon dioxide and residual carbon reacted. Based on 100 parts by weight of the negative active material, a negative active material was obtained that included 0.6 parts by weight of silicon carbide and the remaining 99.4 parts by weight of Si.
[0126] Example 2
[0127] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 0.1 parts by weight of silicon carbide and the remaining 99.9 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0128] Example 3
[0129] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 0.2 parts by weight of silicon carbide and the remaining 99.8 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0130] Example 4
[0131] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 0.4 parts by weight of silicon carbide and the remaining 99.6 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0132] Example 5
[0133] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 0.8 parts by weight of silicon carbide and the remaining 99.2 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0134] Example 6
[0135] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 1.0 part by weight of silicon carbide and the remaining 99.0 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0136] Comparative Example 1
[0137] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material composed only of Si and not containing silicon carbide based on 100 parts by weight of the negative electrode active material.
[0138] Comparative Example 2
[0139] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 0.05 parts by weight of silicon carbide and the remaining 99.95 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0140] Comparative Example 3
[0141] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 1.5 parts by weight of silicon carbide and the remaining approximately 98.5 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0142] Comparative Example 4
[0143] Except that the cooling rate after the reduction reaction was tested differently as shown in Table 1 below, the same procedure as in Example 1 was performed to obtain a negative electrode active material comprising 2.0 parts by weight of silicon carbide and the remaining 98.0 parts by weight of Si based on 100 parts by weight of the negative electrode active material.
[0144] The composition of the negative active material manufactured in the above examples and comparative examples is as shown in Table 1 below.
[0145] Cooling rate (℃ / min) based on 100 parts by weight of negative electrode active material Silicon carbide content (parts by weight based on 100 parts by weight of negative electrode active material) C content (parts by weight) Example 10.6 0.18 35 Example 20.10 0.03 23 Example 30.20 0.06 26 Example 40.4 0.12 31 Example 50.8 0.24 42 Example 6 10.348 Comparative Example 10.0 15 Comparative Example 20.0 5 0.01 20 Comparative Example 31.5 0.45 57 Comparative Example 420.60 69
[0146] The above silicon carbide and C contents were measured using the rietveld refinement method of XRD analysis equipment.
[0147] Discharge capacity, initial efficiency, life (capacity retention rate), and capacity characteristic evaluation
[0148] A positive electrode / negative electrode and a battery were manufactured using positive / negative electrode active materials, respectively, using the following method.
[0149] <Manufacturing of the cathode>
[0150] A negative electrode slurry was prepared by adding a negative electrode active material including the silicon-based active material of Table 1, a first conductive material, a second conductive material, and polyacrylamide as a binder in a weight ratio of 80:9.6:0.4:10 to distilled water as a solvent for forming a negative electrode slurry (solid content concentration 28 wt%).
[0151] For example, the first challenge material is a plate-shaped graphite (specific surface area: 17 m 2 / g, average particle size (D 50 ): 3.5 μm), and the second conductive material was SWCNT.
[0152] As a mixing method, the first conductive agent, binder, and water were dispersed using a homogenous mixer at 2500 rpm for 30 min, the second conductive agent was added and dispersed for 10 min, and then the silicon-based active material was added and dispersed for 30 min at 2500 rpm to produce a negative electrode slurry.
[0153] As a negative electrode collector layer, the negative electrode slurry is applied at 227 mg / 50 cm on the cross section of a copper collector (thickness: 15 μm). 2 The coating was carried out with a loading amount of , rolled (roll pressed), and dried in a vacuum oven at 130°C for 10 hours to form a negative electrode active material layer (thickness: 23 μm), which was used as a negative electrode (thickness of negative electrode: 38 μm, porosity of negative electrode: 40.0%).
[0154] <Manufacturing of the positive electrode>
[0155] LiNi as a cathode active material 0.6 Co 0.2 Mn 0.2 O2 (average particle size (D50): 15㎛), carbon black (product name: Super C65, manufacturer: Timcal) as a conductive agent, and polyvinylidene fluoride (PVdF) as a binder were added to N-methyl-2-pyrrolidone (NMP) as a solvent for forming a cathode slurry at a weight ratio of 97:1.5:1.5 to prepare a cathode slurry (solid content concentration: 78 wt%).
[0156] The positive electrode slurry was applied to both sides of an aluminum current collector (thickness: 12㎛) as a positive electrode collector at a density of 537mg / 25cm. 2 A positive electrode was manufactured by coating with a loading amount, rolling, and drying in a vacuum oven at 130°C for 10 hours to form a positive electrode active material layer (thickness: 65 μm) (positive electrode thickness: 77 μm, porosity 26%).
[0157] A lithium secondary battery was manufactured by interposing a polyethylene separator between the positive electrode and the negative electrode of the above examples and comparative examples and injecting an electrolyte.
[0158] The above electrolyte was an organic solvent containing fluoroethylene carbonate (FEC) and diethyl carbonate (DMC) mixed in a volume ratio of 10:90, vinylene carbonate added at 3 wt% based on the total weight of the electrolyte, and LiPF6 added as a lithium salt at a concentration of 1 M.
[0159] <Experimental Example>
[0160] Experimental Example 1: Cycle Life and Capacity Data
[0161] The life cycle and capacity of the secondary battery containing the negative electrode manufactured as described above were evaluated using an electrochemical charge / discharge tester. The secondary battery was subjected to an in-situ cycle test at 4.2-3.0 V 1C / 0.5C, and the life cycle was measured by charging / discharging at 0.33C / 0.33C (4.2-3.0 V) every 50 cycles during the test.
[0162] Life maintenance rate (%) = {(discharge capacity at Nth cycle) / (discharge capacity at first cycle)} * 100
[0163] In addition, a Li metal / negative electrode cell was manufactured using the negative electrode manufactured as described above to measure capacity data. Then, the discharge capacity in the first cycle of the Li metal / negative electrode cell at 1.5 V-0.005 V, 0.1 C / 0.1 C was shown.
[0164] Silicon carbide content (weight parts based on 100 weight parts of negative active material) Lifespan retention rate after 200 cycles (%) Capacity (mAh / g) Example 10.6903462 Example 20.1873476 Example 30.2873471 Example 40.4883467 Example 50.8893456 Example 61.0873450 Comparative Example 10853488 Comparative Example 20.05843484 Comparative Example 31.5853436 Comparative Example 42853418
[0165] As can be seen in Table 2, Examples 1 to 6, in which electrodes were manufactured with silicon-based active materials satisfying the silicon carbide content range according to the present invention, both the life maintenance rate and capacity were excellent after 200 cycles. For example, since Examples 1 to 6 include silicon carbide within the scope of the present invention, it appears that the electrode life maintenance rate and capacity were excellent by reducing the stress applied to the silicon-based active material during charge and discharge while minimizing capacity degradation, thereby suppressing changes in the electrode structure. On the other hand, Comparative Examples 1 and 2 are electrodes in which the silicon carbide content is less than 0.1 parts by weight based on 100 parts by weight of the total negative active material, and thus the life maintenance rate was relatively low. This is understood to be a phenomenon that occurred due to a decrease in the particle breakage suppression effect by silicon carbide.
[0166] In Comparative Examples 3 and 4, the electrodes in which the silicon carbide content exceeded 1 part by weight based on 100 parts by weight of the total negative active material exhibited relatively low lifespan and capacity. This is understood to be a phenomenon that occurred because the silicon carbide content exceeded the scope of the present invention, resulting in a low energy density of silicon.
[0167] Experimental Example 2: Cycle Resistance Increase Rate
[0168] In the above experimental example 1, the life maintenance rate was measured by charging / discharging at 0.33C / 0.33C (4.2-3.0V) every 50 cycles during the test, and then the resistance was measured by discharging at 2.5C pulse at SOC50 to compare and analyze the resistance increase rate.
[0169] For the above resistance increase rate measurement evaluation, data for each of 200 cycles were calculated, and the results were as shown in Table 3 below.
[0170] Silicon carbide content (weight parts based on 100 weight parts of negative active material) Resistance increase rate (%) after 200 cycles (3.0~4.2 V range 1C / 0.5C) Example 10.66 Example 20.19 Example 30.28 Example 40.48 Example 50.87 Example 61.09 Comparative Example 10.10 Comparative Example 20.0512 Comparative Example 31.510 Comparative Example 42.11
[0171] As can be seen in Table 3, it was confirmed that the resistance increase rate of the comparative example was higher than that of the examples after 200 cycles. In other words, it was confirmed that when the ratio of silicon carbide did not satisfy the range of the present invention, the resistance also increased due to instability in the silicon electrode structure.
[0172] Although the present invention has been described above with reference to embodiments thereof, it will be understood by those skilled in the art or those with ordinary knowledge in the art that various modifications and changes may be made to the present invention without departing from the spirit and technical scope of the present invention as set forth in the claims below. Accordingly, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. Silicon particles; and As a negative active material comprising silicon carbide distributed within the above silicon particles, The negative electrode active material, wherein the silicon carbide is contained in an amount of 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material.
2. In claim 1, The above-mentioned silicon carbide is a negative electrode active material containing 0.2 parts by weight or more and 0.8 parts by weight or less based on 100 parts by weight of the total negative electrode active material.
3. In claim 1, The above silicon-based particles are a negative electrode active material containing 90 parts by weight or more of SiOx (x=0) based on 100 parts by weight of the above negative electrode active material.
4. In claim 1, The above silicon particles are SiOx (0) based on 100 parts by weight of the negative electrode active material. <x<2)를 10 중량부 이하로 포함하는 것인 음극 활물질.
5. In claim 1, A negative electrode active material having a carbon content of 0.03 parts by weight or more and 0.3 parts by weight or less based on 100 parts by weight of the above negative electrode active material.
6. A negative electrode comprising a negative electrode active material according to claim 1.
7. In claim 6, the silicon-based particles are SiO based on 100 parts by weight of the negative electrode active material. x A cathode containing 90 parts by weight or more of (x=0).
8. In claim 7, the cathode further comprises a cathode conductive material; and a cathode binder.
9. A secondary battery comprising a negative electrode according to claim 6.
10. Silicon particles; and A method for manufacturing a negative electrode active material comprising silicon carbide distributed within the above silicon particles, A method for manufacturing a negative electrode active material, wherein the above silicon carbide is included in an amount of 0.1 part by weight or more and 1 part by weight or less based on 100 parts by weight of the total negative electrode active material.
11. In claim 10, A method for manufacturing a negative electrode active material, wherein the above silicon carbide is included in an amount of 0.2 parts by weight or more and 0.8 parts by weight or less based on 100 parts by weight of the total negative electrode active material.
12. In claim 10, The above silicon particles are SiO based on 100 parts by weight of the negative active material. x A method for producing a negative electrode active material comprising 90 parts by weight or more of (x=0).
13. In claim 10, The above silicon particles are SiO based on 100 parts by weight of the negative active material. x (0 <x<2)를 10 중량부 이하로 포함하는 것인 음극 활물질의 제조 방법.
14. In claim 10, A method for manufacturing a negative electrode active material, wherein the carbon content is 0.03 parts by weight or more and 0.3 parts by weight or less based on 100 parts by weight of the negative electrode active material.
15. A step of reducing silicon dioxide to silicon by reacting it with carbon; and A method for producing a negative active material, comprising a step of forming silicon carbide using residual carbon after the above reducing step.
16. In claim 15, The step of forming the above silicon carbide is: A method for manufacturing a negative electrode active material, which is a step of forming silicon carbide by cooling reduced silicon according to a preset cooling rate.
17. In claim 16, A method for manufacturing a negative electrode active material, wherein the above-mentioned preset cooling rate is 20 to 70°C / min.
Citation Information
Patent Citations
Negative electrode active material, negative electrode, secondary battery, and method for preparing negative electrode active material
KR1020240161572A
Negative electrode material for nonaqueous electrolyte secondary battery, and lithium ion secondary battery
JP2013171627A
Si / c composite, anode materials and lithium battery using the same
KR1020090011888A
Negative active material for rechargable lithium battery, preparation method thereof and rechargable lithium battery
KR1020140087376A
Silicon-silicon oxycarbide glass composite, preparation method of thereof, and anode materials and lithium secondary battery comprising the same