Negative electrode active material and negative electrode including the same
The negative electrode active material, featuring silicon particles with oxidized surfaces and a carbon layer, along with zirconium, addresses the limitations of carbon-based materials by suppressing volume expansion and enhancing conductivity, thereby improving the energy capacity and lifespan of lithium-ion batteries.
Patent Information
- Application Number
- PCT/KR2024/004880
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-04-11
- Publication Date
- 2024-11-07
AI Technical Summary
Lithium-ion secondary batteries using carbon-based negative electrode materials suffer from limited capacity and mechanical instability due to volume expansion during lithium insertion, leading to reduced lifespan and performance issues.
A negative electrode active material comprising silicon particles with oxidized surfaces, a carbon layer, and zirconium, which suppresses volume expansion and enhances mechanical and electrical conductivity, improving energy capacity and lifespan.
The solution effectively reduces volume expansion, enhances mechanical strength, and improves electrical conductivity, resulting in increased energy capacity and extended lifespan of lithium-ion secondary batteries.
Smart Images

Figure 000001 
Figure 000002 
Figure 000003
Abstract
Description
NEGATIVE ELECTRODE ACTIVE MATERIAL AND NEGATIVE ELECTRODE INCLUDING THE SAME
[0001] The present invention relates to a negative electrode active material and a negative electrode including the same.
[0002]
[0003] As the electronics, communications, and space industries develop, the demand for secondary batteries as an energy power source is rapidly increasing. In particular, as the importance of global eco-friendly policies is emphasized, the electric vehicle market is growing rapidly, and research and development on secondary batteries are being actively conducted at home and abroad.
[0004] Secondary batteries generally consist of a positive electrode containing a positive active material, a negative electrode containing a negative electrode active material, a separator, and an electrolyte. In particular, lithium secondary batteries have high energy density and high capacity, thereby being applied in various fields.
[0005] A negative electrode active material constituting a negative electrode is made of a carbon-based material or a silicon oxide. However, in the case of a carbon-based material, the theoretical capacity is only about 400 mAh / g, thereby having the disadvantage of a small capacity.
[0006] Accordingly, research has been conducted to replace a carbon-based material using silicon having a high theoretical capacity, as a negative electrode active material. However, the volume of a silicon material expands by about 300% due to lithium insertion, which causes a negative electrode to be destroyed and cycle characteristics to deteriorate. In addition, as the cycle continues, volume expansion continues to occur due to the lithium insertion, causing problems such as loss of contact with a conductive material and a current collector or formation of an unstable Solid Electrolyte Interphase (SEI).
[0007]
[0008] Therefore, the present invention has been made in view of the above problems, and it is one object of the present invention to provide a negative electrode active material having excellent mechanical properties and electrical conductivity, high energy capacity, and improved lifespan characteristics by suppressing the volume expansion of a negative electrode active material; and a negative electrode including the negative electrode active material.
[0009]
[0010] In accordance with an aspect of the present invention, the above and other objects can be accomplished by the provision of a negative electrode active material, including: a silicon particle; a silicon oxide in which a surface of the silicon particle is oxidized; and a carbon layer formed on at least a portion of a surface of the silicon oxide, wherein 1,000 ppm to 6,000 ppm of zirconium is included in the negative electrode active material.
[0011] In an embodiment of the present invention, 40,000 ppm to 50,000 ppm of nitrogen may be included in the negative electrode active material.
[0012] In an embodiment of the present invention, a content of carbon contained in the negative electrode active material may be 3 times to 6 times, compared to a content of the nitrogen.
[0013] In an embodiment of the present invention, the silicon oxide may be represented by Formula 1 below:
[0014] [Formula 1]
[0015] SiOx(0<x≤9)
[0016] In an embodiment of the present invention, the silicon oxide may have a thickness of 0.01 nm to 30 nm.
[0017] In an embodiment of the present invention, the silicon oxide may have a concentration gradient region.
[0018] In an embodiment of the present invention, in the concentration gradient region, a content of oxygen atoms, compared to a content of the silicon atoms, in a center direction of the silicon particle from the surface of the silicon oxide may be continuously reduced.
[0019] In an embodiment of the present invention, the silicon particle may have a diameter of 10 nm to 150 nm.
[0020] In an embodiment of the present invention, the carbon layer may have a thickness of 10 nm to 50 nm.
[0021] In an embodiment of the present invention, the carbon layer may be included in a content of 15 % by weight to 30 % by weight in the negative electrode active material.
[0022] In an embodiment of the present invention, the negative electrode active material may have a BET specific surface area of 1 m2 / g to 5 m2 / g.
[0023] In accordance with another aspect of the present invention, there is provided a negative electrode, including: a negative electrode current collector; and a negative electrode active material layer formed at least one surface of the negative electrode current collector, wherein the negative electrode active material layer includes a negative electrode active material, wherein the negative electrode active material includes a silicon particle, a silicon oxide in which a surface of the silicon particle is oxidized, and a carbon layer formed on at least a portion of a surface of the silicon oxide, and 1,000 ppm to 6,000 ppm of zirconium is included in the negative electrode active material.
[0024]
[0025] The present invention includes a silicon-based active material as a negative electrode active material, so that the energy capacity of a secondary battery can be improved compared to using a carbon-based material as a negative electrode active material.
[0026] In addition, the present invention includes a silicon particle as a negative electrode active material; and a silicon oxide in which the surface of the silicon particle is oxidized, so that the volume expansion of silicon particles due to insertion of lithium ions can be suppressed, thereby improving lifespan characteristics.
[0027] In addition, since the negative electrode active material of the present invention includes zirconium in a predetermined range, the mechanical properties of the negative electrode active material can be improved, so that breakage of the negative electrode active material due to a manufacturing process of a secondary battery and external impact can be minimized.
[0028] Further, the negative electrode active material of the present invention includes zirconium in a predetermined range; and a carbon layer formed on at least a portion of the surface of the silicon oxide, so that electrical conductivity can be improved.
[0029]
[0030] Structural or functional descriptions of embodiments disclosed in the present specification or application are merely illustrated for the purpose of explaining embodiments according to the technical idea of the present invention, embodiments according to the technical idea of the present invention may be implemented in various forms other than the embodiments disclosed in the present specification or application, and it is not to be construed that the technical idea of the present invention is limited to the embodiments described in the present specification or application.
[0031] In the present specification or application, when a certain component is "included", this indicates that only the component is included or the component may further include another component unless there is no different disclosure. In addition, it should be understood that all numerical ranges representing physical property values, dimensions, etc. of components described in the present specification or application are modified by the term 'about' in all cases unless otherwise specified.
[0032] In this specification or application, 'negative electrode active material' refers to a negative electrode active material particle or a secondary particle to which a negative electrode active material particle is coupled.
[0033]
[0034] Hereinafter, a negative electrode active material according to the present invention and a negative electrode including the same are described.
[0035]
[0036] <Negative electrode active material>
[0037] A negative electrode active material according to the present invention includes a silicon particle, a silicon oxide in which the surface of the silicon particle is oxidized, and a carbon layer formed on at least a portion of the surface of the silicon oxide, wherein 1,000 ppm to 6,000 ppm of zirconium is included in the negative electrode active material.
[0038] The silicon particle may be a spherical silicon nanoparticle. The silicon particle may have a diameter of 1 nm to 500 nm, 1 nm to 400 nm, 10 nm to 400 nm, 10 nm to 350 nm, 10 nm to 300 nm, 10 nm to 250 nm, 10 nm to 200 nm, or 10 nm to 150 nm. The diameter may be measured in the same method as the diameter measurement method of the first silicone-based particle. When the range is satisfied, manufacturing costs may not be significantly increased, and battery capacity and lifespan characteristics may be improved.
[0039] The negative electrode active material includes a silicon oxide in which the surface of the silicon particle is oxidized. Conventionally, a negative electrode active material was manufactured by physically or chemically mixing nano-sized silicon particles and silicon oxide. Accordingly, when charging and discharging a secondary battery, cracks occurred at the boundary between the silicon particles and the silicon oxide. Since the negative electrode active material according to the present invention includes the silicon oxide in which the surface of the silicon particle is oxidized, a boundary between the silicon particle and the silicon oxide is not formed. Accordingly, cracks occurring at the boundary between the silicon particle and the silicon oxide when charging and discharging a secondary battery may be suppressed.
[0040] The silicon oxide may be represented by Formula 1 below:
[0041] [Formula 1]
[0042] SiOx(0<x≤9)
[0043] In Formula 1, when x satisfies the range, the generation of irreversible products such as Li2O and Li-silicate (LixSiyOz) due to reaction between lithium ions and oxygen may be minimized and, accordingly, the problem that lithium ions, which have reacted with a negative electrode active material, are trapped inside a negative electrode rather than returning to an electrolyte or a positive electrode to cause capacity reduction may be minimized.
[0044] The silicon oxide may have a concentration gradient region. In the concentration gradient region, the content of oxygen atoms relative to the content of silicon atoms in the center direction of the silicon particle may be continuously reduced on the surface of the silicon oxide. The concentration gradient region may mean that at least one element has a concentration distribution that continuously changes according to a certain tendency or trend. The certain tendency may mean that the concentration of the elements is continuously decreasing or increasing.
[0045] For example, x in Formula 1 has a value close to 0.9 in the surface region of the silicon oxide among the concentration gradient region of the silicon oxide, and x in Formula 1 has a value close to 0 as approaching the center of the silicon particle from the surface of the silicon oxide, so the concentration gradient region may have a relatively reduced content of oxygen atoms compared to the content of silicon atoms as approaching from the surface of the silicon oxide to the center of the silicon particle. Accordingly, the volume expansion of the silicon particles due to insertion of lithium ions may be suppressed because the surface of the silicon oxide has a relatively high content of oxygen atoms compared to the content of the silicon atoms, and energy capacity may be increased while suppressing cracks occurring at the boundary between silicon particles and silicon oxide when charging and discharging a secondary battery because the content of silicon atoms is relatively high as approaching the center of the silicon particle.
[0046] The silicon oxide may have a thickness of 0.01 nm to 30 nm, 0.05 nm to 30 nm, 0.1 nm to 30 nm, 0.15 nm to 30 nm, 0.20 nm to 30 nm, 0.30 nm to 30 nm, or 1 nm to 30 nm. When the range is satisfied, the movement of lithium ions is not hindered and, at the same time, the volume expansion of silicon particles due to the insertion of lithium ions may be suppressed.
[0047]
[0048] The negative electrode active material includes a carbon layer formed on at least a portion of the surface of the silicon oxide. The carbon layer may improve the electrical conductivity of the negative electrode active material.
[0049] The carbon layer may be formed on at least a portion of the surface of the silicon oxide or on the entire surface of the silicon oxide. When the carbon layer is formed only on at least a portion of the surface of the silicon oxide and, accordingly, a carbon layer with a rough morphology is formed on the surface of the silicon oxide, diffusion of lithium ions may be improved, and destruction of the carbon layer due to the volume expansion of the silicon particles during charging and discharging of a secondary battery may be minimized, so that the capacity and lifespan of the secondary battery may be improved.
[0050] To form the carbon layer, a carbonaceous conductive material may be used. The carbonaceous conductive material may be one or more selected from among natural graphite, artificial graphite, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, graphene, carbon nanotubes, and a conductive polymer.
[0051] The carbonaceous conductive material may be amorphous carbon. The amorphous carbon may refer to an amorphous structure in which carbon corresponding to a diamond structure and carbon corresponding to a graphite structure are irregularly mixed. A ratio of carbon atoms corresponding to a diamond structure among the amorphous carbon may be 5 % to 70 %, 10 % to 70 %, 15 % to 70 %, 18 % to 70 %, 20 % to 70 %, or 30 % to 70 %. When the range is satisfied, electrical conductivity may be improved while partially suppressing the volume expansion of the silicone particle, thereby improving the capacity and lifespan characteristics of a secondary battery. The ratio of carbon atoms corresponding to the diamond structure and carbon atoms corresponding to the graphite structure may be calculated by electron energy-loss spectroscopy using a transmission electron microscope (TEM).
[0052] The carbon layer may be formed by the carbonization of a carbon precursor such as a saccharide. The saccharide may be a compound including a CnH2ncycloalkane ring having 3 to 6 carbon atoms. For example, the saccharide may be any one or more selected from the group consisting of glucose, fructose, galactose, sucrose, maltose, and lactose.
[0053] The carbon layer may have a thickness of 1 nm to 1,000 nm, 5 nm to 500 nm, 5 nm to 100 nm, 5 nm to 50 nm, or 10 nm to 50 nm. The carbon layer may be included in an amount of 1 % by weight to 50 % by weight, 1 % by weight to 40 % by weight, 5 % by weight to 40 % by weight, 10 % by weight to 40 % by weight, or 15 % by weight to 30 % by weight in the negative electrode active material. When the range is satisfied, electrical conductivity is increased without interfering with the movement of lithium ions, thereby improving the capacity and lifespan of a secondary battery.
[0054]
[0055] The negative electrode active material includes 1,000 ppm to 6,000 ppm of zirconium (Zr) in the negative electrode active material. The content of zirconium means a content relative to the total weight of the negative electrode active material. The content of zirconium may be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES).
[0056] When observing the cross-section of the negative electrode active material, the zirconium may be included in at least a portion of the surface of the silicon particle, the silicon oxide, and the carbon layer. The zirconium may be incorporated by a milling process with the silicon particles and zirconia beads (YTZ) during the manufacturing process of the negative electrode active material. The content of the zirconium may be controlled by the milling time.
[0057] When the content of the zirconium in the negative electrode active material satisfies the range, the mechanical strength of the negative electrode active material is improved, thereby effectively protecting the structure of the negative electrode active material. Accordingly, breakage of the negative electrode active material due to the manufacturing process of a secondary battery or external shock may be minimized, preventing deterioration of the performance of a secondary battery. In addition, zirconium, which exhibits higher electrical conductivity compared to carbon, is included in the negative electrode active material, thereby increasing the capacity of a secondary battery. Further, as the mechanical properties and electrical conductivity of a secondary battery are improved, the swelling phenomenon may be reduced during long-term use of the secondary battery, and the lifespan characteristics thereof may be improved.
[0058] The negative electrode active material may include 30,000 ppm to 60,000 ppm, 30,000 ppm to 50,000 ppm, or 40,000 ppm to 50,000 ppm of nitrogen. The content of nitrogen means a content relative to the total weight of the negative electrode active material. The content of nitrogen may be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). When the range is satisfied, electrical conductivity may be improved while not causing a decrease in the initial efficiency of a secondary battery.
[0059] The content of carbon contained in the negative electrode active material compared to the content of the nitrogen may be 3 times to 6 times, 3.5 times to 6 times, 3.5 times to 5.5 times, or 4 times to 5 times. The content of carbon and nitrogen means a content relative to the total weight of the negative electrode active material. The content of carbon and nitrogen may be measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). When the range is satisfied, the electrical conductivity of the secondary battery may be improved.
[0060]
[0061] The negative electrode active material may have a BET specific surface area of 0.5 m2 / g to 30 m2 / g, 1 m2 / g to 30 m2 / g, 1 m2 / g to 20 m2 / g, 1 m2 / g to 15 m2 / g, 1 m2 / g to 10 m2 / g, or 1 m2 / g to 5 m2 / g. The BET specific surface area may be measured from the amount of nitrogen gas adsorption at liquid nitrogen temperature (77K) using BELSORP-mini II manufactured by BEL Japan. When the range is satisfied, the performance of the secondary battery may be maintained even using a relatively small content of binder and conductive material, and side reactions in the secondary battery may be reduced, thereby improving the capacity and lifespan of the secondary battery.
[0062]
[0063] The negative electrode active material according to the present invention may further include natural graphite particles. The natural graphite particles may include a carbon layer formed on the natural graphite particles. the carbon layer may reduce micropores of the natural graphite particles, may reduce a side reaction with an electrolyte solution, and may improve structural stability.
[0064] The carbon layer may include the natural graphite particles in an amount of 1 % by weight to 10 % by weight, 1 % by weight to 9 % by weight, 2 % by weight to 9 % by weight, 2 % by weight to 8 % by weight, or 3 % by weight to 8 % by weight. When the range is satisfied, excessive lithium insertion and desorption may be prevented while improving the structural stability of the natural graphite particles.
[0065] The carbon layer may include amorphous carbon. For example, the carbon layer may be formed by providing at least one carbon layer precursor selected from the group consisting of pitch, rayon, and polyacrylonitrile-based resin to the natural graphite particles, followed by heat treatment.
[0066] The natural graphite particles may have a BET specific surface area of 1.0 m2 / g to 5.0 m2 / g, 1.2 m2 / g to 5.0 m2 / g, 1.2 m2 / g to 4.8 m2 / g, 1.5 m2 / g to 4.8 m2 / g, or 1.5 m2 / g to 4.5 m2 / g. When the range is satisfied, the lifespan characteristics of a secondary battery may be improved by preventing a side reaction with an electrolyte solution, and high output characteristics may be realized.
[0067] The natural graphite particles may have a sphericity degree of 0.6 to 1, 0.7 to 1, 0.8 to 1, 0.9 to 1, or 0.95 to 1. The sphericity degree may be measured using a known sphericity measurement method. When the range is satisfied, packing between particles may be smoothened, and stress applied to particles when manufacturing a negative electrode may be alleviated, reducing the swelling phenomenon.
[0068]
[0069] The negative electrode active material according to the present invention may further include artificial graphite particles. The artificial graphite particles may be a primary particle, a secondary particle, or a mixture of a primary particle and a secondary particle. The primary particle may refer to a single particle that is not aggregated. The secondary particle may refer to an aggregate of the primary particles.
[0070] The carbon layer may be included in an amount of 1 % by weight to 10 % by weight, 1 % by weight to 9 % by weight, 2 % by weight to 9 % by weight, 2 % by weight to 8 % by weight, or 3 % by weight to 8 % by weight based on the artificial graphite particles. When the range is satisfied, excessive lithium insertion and desorption may be prevented while improving the structural stability of the artificial graphite particles.
[0071] The carbon layer may include amorphous carbon. For example, the carbon layer may be formed by providing at least one carbon layer precursor selected from the group consisting of pitch, rayon, and polyacrylonitrile-based resin to the natural graphite particles, followed by heat treatment.
[0072] The natural graphite particles may have a BET specific surface area of 0.5 m2 / g to 3.0 m2 / g, 0.5 m2 / g to 2.5 m2 / g, 0.5 m2 / g to 2.0 m2 / g, 0.5 m2 / g to 1.8 m2 / g, or 0.5 m2 / g to 1.5 m2 / g. When the range is satisfied, the lifespan characteristics of a secondary battery may be improved by preventing a side reaction with an electrolyte solution, and high output characteristics may be realized.
[0073] The natural graphite particles may have a sphericity degree of 0.65 to 1, 0.68 to 1, 0.7 to 1, 0.8 to 1, or 0.9 to 1. The sphericity degree may be measured using a known sphericity measurement method. When the range is satisfied, packing between particles may be smoothened, and stress applied to particles when manufacturing a negative electrode may be alleviated, reducing the swelling phenomenon.
[0074]
[0075] <Method of manufacturing negative electrode active material>
[0076] A method of manufacturing a negative electrode active material according to the present invention may include a step (a) of adding silicon particles and beads to a solvent and then milling it for 1 to 40 hours to prepare a first silicon slurry, a step (b) of adding the first silicon slurry to a carbon-based polymer solution and then stirring it to prepare a second silicon slurry, and a step (c) of heat-treating the second silicon slurry in a temperature range of 1,000 ℃ to 1,500 ℃ in an inert atmosphere.
[0077]
[0078] In the step (a), the milled silicon particles may be a spherical silicon nanoparticle. The milled silicon particles may have a diameter of 0.5 nm to 500 nm, 1 nm to 400 nm, 10 nm to 400 nm, 10 nm to 350 nm, 10 nm to 300 nm, 10 nm to 250 nm, 10 nm to 200 nm, or 10 nm to 150 nm.
[0079] The beads may be zirconium oxide balls (YTZ). Each of the zirconium oxide balls may have a diameter of 0.01 mm to 1 mm, 0.05 mm to 1 mm, 0.05 mm to 0.5 mm, or 0.05 mm to 0.3 mm. The solvent is not particularly limited, but may be isopropyl alcohol. The silicon particles and beads are included in an amount of 10 % by weight to 50 % by weight, 10 % by weight to 40 % by weight, 10 % by weight to 35 % by weight, or 15 % by weight to 35 % by weight based on a total weight of the solvent and may be subjected to a milling process.
[0080] In the step (a), a milling process may be performed for 1 to 40 hours under a temperature condition of 45 ℃. As the temperature condition is satisfied, a silicon-based active material with suppressed oxidation reaction may be manufactured. If necessary, the solvent may be additionally added in the milling process. By adjusting the milling time, the content of zirconium in the manufactured negative electrode active material may be adjusted, and by satisfying the milling time, 1,000 ppm to 6,000 ppm of zirconium may be included in the manufactured negative electrode active material.
[0081] In the step (b), carbon may be attached to the surface of the silicon oxide by the carbon-based polymer solution.
[0082] After the step (b), a step (b-1) of homogenizing the second silicon slurry under a pressure condition of 800 bar to 1,200 bar may be included. By the homogenizing step, the mixing property between the second silicon slurry and the carbon-based polymer solution may be improved.
[0083] After the step (b-1), a step (b-2) of spray-drying the second silicon slurry may be included. By the spray-drying step, a silicone-based carbon polymer precursor may be manufactured. As the precursor is manufactured, the density of the negative electrode active material may be improved.
[0084] By the heat-treating of the step (c), a carbon coating layer may be formed on the surface of the silicon oxide.
[0085]
[0086] <Negative electrode>
[0087] A negative electrode according to the present invention includes a negative electrode current collector; and a negative electrode active material layer formed on at least one surface of the negative electrode current collector, the negative electrode active material layer includes a negative electrode active material, the negative electrode active material includes silicon particle, a silicon oxide in which the surface of the silicon particle is oxidized, and a carbon layer formed on at least a portion of the surface of the silicon oxide, and 1,000 ppm to 6,000 ppm of zirconium is included in the negative electrode active material.
[0088] The negative electrode active material may be the same as the above-described negative electrode active material.
[0089] The negative electrode current collector is not particularly limited as long as it is conductive without causing chemical changes in a secondary batter and may be made of, for example, copper; stainless steel; aluminum; nickel; titanium; fired carbon; copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc.; aluminum-cadmium alloy; or the like. In addition, fine irregularities may be formed on the surface to strengthen the bonding power of a negative electrode active material, and various forms such as a film, a sheet, a foil, a net, a porous material, a foam, and a non-woven material may be used.
[0090]
[0091] The negative electrode active material layer may further include a binder. The binder may be used to maintain a molded body by binding particles contained in the negative electrode active material. The binder may be a non-aqueous binder or an aqueous binder. For example, the non-aqueous binder may be, polyvinyl alcohol, carboxymethyl cellulose, hydroxypropylene cellulose, diacetylene cellulose, polyvinyl chloride, polyvinylpyrrolidone, polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), polyethylene, polypropylene, or the like, and the aqueous binder may be one selected from the group consisting of acrylonitrile-butadiene rubber, styrene-butadiene rubber, and acrylic rubber, or a mixture of two or more thereof. The aqueous binder is more economical and environmentally friendly than the non-aqueous binder, is harmless to workers' health, and has a superior binding effect compared to the non-aqueous binder, so the ratio of an active material per same volume may be increased, enabling high capacity. Particularly, a styrene-butadiene rubber may be used as the aqueous binder.
[0092] The binder may be included in an amount of 0.1 % by weight to 10 % by weight, 0.1 % by weight to 8 % by weight, 0.1 % by weight to 7 % by weight, 0.1 % by weight to 6 % by weight, or 0.1 % by weight to 5 % by weight based on a total weight of a slurry for producing a negative electrode active material layer. When the range is satisfied, the effect as a binder may be excellent without a decrease in capacity per volume due to a decrease in a relative content of a negative electrode active material.
[0093] The negative electrode active material layer may further include a conductive material. The conductive material is not particularly limited as long as it is conductive without causing chemical changes in a secondary batter. The conductive material may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, or summer black; conductive fiber such as carbon fiber or metal fiber; metal powder such as carbon fluoride, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; a conductive metal oxide such as titanium oxide; a conductive material such as a polyphenylene derivative; or the like. The conductive material may be included in an amount of 0.1 % by weight to 10 % by weight, 0.1 % by weight to 8 % by weight, 0.1 % by weight to 7 % by weight, 0.1 % by weight to 6 % by weight, or 0.1 % by weight to 5 % by weight based on a total weight of a slurry for producing a negative electrode active material layer. When the range is satisfied, electrical conductivity may be improved without a decrease in capacity per volume due to a decrease in a relative content of an active material.
[0094]
[0095] <Secondary battery>
[0096] A secondary battery according to the present invention may include a negative electrode, a positive electrode, and a separator interposed between the negative electrode and the positive electrode.
[0097] The negative electrode may be the same as the above-described negative electrode.
[0098] The positive electrode may be manufactured by a general method known in the art. For example, a positive electrode may be manufactured by mixing and stirring a positive active material with a solvent, a binder, a conductive material, and a dispersant to produce a slurry, and then applying the slurry to a positive electrode current collector, followed by compressing and drying it.
[0099]
[0100] The positive electrode current collector is a highly conductive metal to which a slurry of the positive active material can easily adhere, and is not particularly limited as long as it has high conductivity without causing chemical changes in a secondary battery. The positive electrode current collector may be, for example, stainless steel; aluminum; nickel; titanium; calcined carbon; the surface of aluminum or stainless steel treated with carbon, nickel, titanium, silver, etc.; or the like. In addition, the adhesive force of a positive active material may be increased by forming fine irregularities on the surface of the positive electrode current collector. The positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous material, a foam, and a non-woven material, and may have a thickness of 3 ㎛ to 500 ㎛.
[0101]
[0102] The positive active material is a compound capable of reversible intercalation and deintercalation of lithium, and may include, specifically, a lithium composite metal oxide containing lithium and one or more metals such as cobalt, manganese, nickel, or aluminum.
[0103] Particularly, the lithium composite metal oxide may be a lithium-manganese-based oxide (e.g., LiMnO2, LiMn2O4, etc.), a lithium-cobalt-based oxide (e.g., LiCoO2, etc.), a lithium-nickel-based oxide (e.g., LiNiO2, etc.), a lithium-nickel-manganese oxide (e.g., LiNi1-YMnYO2(where 0<Y<1), LiMn2-zNizO4(where 0<Z<2), etc.), a lithium-nickel-cobalt-based oxide (e.g., LiNi1-Y1CoY1O2(where 0<Y1<1), etc.), a lithium-manganese-cobalt-based oxide (e.g., LiCo1-Y2MnY2O2(where 0<Y2<1), LiMn2-z1Coz1O4(where 0<Z1<2), etc.), a lithium-nickel-manganese-cobalt-based oxide (e.g., Li (NipCoqMnr1)O2(where 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) or Li (Nip1Coq1Mnr2)O4(where 0<p1<2, 0<q1<2, 0<r2<2, p1+q1+r2=2), etc.), or a lithium-nickel-cobalt-transition metal (M) oxide (e.g., Li (Nip2Coq2Mnr3MS2)O2(where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg and Mo, p2, q2, r3 and s2 are each independent atomic fraction of elements, 0 < p2 < 1, 0 < q2 <1, 0<r3<1, 0<s2<1, and p2+q2+r3+s2=1), etc.), or the like, and may include a compound of one or more thereof. In terms of improving the capacity characteristics and stability of the battery, the lithium composite metal oxide may be LiCoO2, LiMnO2, LiNiO2, a lithium nickel manganese cobalt oxide (e.g., Li (Ni0.6Mn0.2Co0.2)O2, Li (Ni0.5Mn0.3Co0.2)O2, or Li (Ni0.8Mn0.1Co0.1)O2, etc.), a lithium nickel cobalt aluminum oxide (e.g., Li (Ni0.8Co0.15Al0.05)O2, etc.), or the like among the oxides, and when considering the remarkable improvement effect due to control of the type and content ratio of the constituent elements forming the lithium composite metal oxide, the lithium composite metal oxide may be Li (Ni0.6Mn0.2Co0.2)O2, Li (Ni0.5Mn0.3Co0.2)O2, Li (Ni0.7Mn0.15Co0.15)O2, Li (Ni0.8Mn0.1Co0.1)O2or the like or a mixture of one or more thereof.
[0104]
[0105] The solvent may be an organic solvent such as N-methyl pyrrolidone (NMP), dimethyl formamide (DMF), acetone or dimethyl acetamide, or water, and these solvents may be used alone or in a mixture of two or more thereof. The use amount of the solvent is sufficient so long as it is an amount capable of dissolving and dispersing the positive active material, the binder, and the conductive material, considering the application thickness of a slurry and a manufacturing yield.
[0106]
[0107] The binder may be a variety of binders such as a polyvinylidenefluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidenefluoride, polyacrylonitrile, polymethylmethacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, an ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluorine rubber, poly acrylic acid and its polymers whose hydrogen is substituted with Li, Na, or Ca, and various copolymers.
[0108]
[0109] The conductive material is not particularly limited as long as it is conductive without causing chemical changes in a secondary batter. The conductive material may be, for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, or summer black; conductive fiber such as carbon fiber or metal fiber; conductive tubes such as carbon nanotubes; metal powder such as fluorocarbon, aluminum, or nickel powder; conductive whiskers such as zinc oxide or potassium titanate; a conductive metal oxide such as titanium oxide; a conductive material such as a polyphenylene derivative; or the like. The conductive material may be used in an amount of 1 % by weight to 20 % by weight based on a total weight of the positive electrode slurry.
[0110] The dispersant may be an aqueous dispersant or an organic dispersant such as N-methyl-2-pyrrolidone.
[0111]
[0112] The separator may be interposed between the negative electrode and the positive electrode. The separator is configured to prevent an electrical short circuit between a negative electrode and a positive electrode and to generate a flow of ions. The separator may include a porous polymer film or a porous non-woven fabric. Here, the porous polymer film may be composed of a single layer or multiple layers containing a polyolefin-based polymer such as an ethylene polymer, a propylene polymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer. The porous non-woven fabric may include glass fiber with a high melting point or polyethylene terephthalate fiber. However, it is not limited thereto, and the separator may be a highly heat-resistant separator (Ceramic Coated Separator; CCS) containing ceramic depending on an embodiment.
[0113] The positive electrode, the negative electrode and the separator may be manufactured into an electrode assembly by a winding, lamination, folding, or zigzag stacking process. In addition, the electrode assembly may be provided with an electrolyte solution so that it may be manufactured into the secondary battery according to the present invention. The secondary battery may be one of cylindrical, square, pouch, and coin types using a can, without being limited thereto.
[0114]
[0115] The electrolyte solution may be a non-aqueous electrolyte. The electrolyte solution may include lithium salt and an organic solvent. The organic solvent may include at least one of propylene carbonate (PC), ethylene carbonate (EC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethylmethyl carbonate (EMC), methylpropyl carbonate (MPC), dipropyl carbonate (DPC), vinylene carbonate (VC), dimethyl sulfoxide, acetonitrile, dimethoxyethane, diethoxyethane, sulfolane, gamma-butyrolactone, propylene sulfide, and tetrahydrofuran.
[0116]
[0117] The present invention may provide a battery module including the secondary battery as a unit battery. The battery module may be used as a power source for medium and large devices that require high-temperature stability, long cycle characteristics, high rate characteristics, and the like.
[0118] Examples of the medium and large devices include, but are not limited to, electric motor-driven power tools; electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs); electric two-wheeled vehicles such as e-bikes and e-scooters; electric golf carts; and systems for storing power.
[0119]
[0120] Hereinafter, the present invention will be described in more detail based on examples and comparative examples. However, the following examples and comparative examples are only examples to explain the present invention in more detail, and the present invention is not limited by the following examples and comparative examples.
[0121]
[0122] Manufacturing examples - Manufacturing of negative electrode active material
[0123] Manufacturing Example 1
[0124] Silicon with a particle size of about 800 nm and zirconia beads (YTZ) with a particle size of about 0.1 mm were added to an isopropyl alcohol solvent. Next, milling was performed for 9 hours while maintaining a temperature of 45°C or lower to produce a first silicon slurry with a particle size of about 100 nm and 25% by weight of metallic silicon solid content.
[0125] The first silicon slurry was stirred in a homogenization reactor (2,500 rpm) for 10 minutes, and then polyvinyl pyrrolidone (PVP) was added thereto, followed by re-stirring in the homogenization reactor for 10 minutes to manufacture a second silicon slurry.
[0126] The second silicon slurry was subjected to a homogenization process twice under a pressure of 1,000 bar in a high-pressure homogenizer. Next, the second silicon slurry was spray-dried. Next, heat treatment was performed at 1,200 ℃ under a nitrogen atmosphere to manufacture a negative electrode active material.
[0127] Manufacturing Example 2
[0128] A negative electrode active material was manufactured by the same process as in Manufacturing Example 1 except that milling was performed for 20 hours instead of the milling for 10 hours in Manufacturing Example 1.
[0129] Manufacturing Example 3
[0130] A negative electrode active material was manufactured by the same process as in Manufacturing Example 1 except that milling was performed for 40 hours instead of the milling for 10 hours in Manufacturing Example 1.
[0131] Manufacturing Example 4
[0132] A negative electrode active material was manufactured by the same process as in Manufacturing Example 1 except that milling was performed for 5 hours instead of the milling for 10 hours in Manufacturing Example 1.
[0133] Manufacturing Example 5
[0134] A negative electrode active material was manufactured by the same process as in Manufacturing Example 1 except that milling was performed for 2 hours instead of the milling for 10 hours in Manufacturing Example 1.
[0135] Manufacturing Example 6
[0136] A negative electrode active material was manufactured by the same process as in Manufacturing Example 1 except that milling was performed for 1 hour instead of the milling for 10 hours in Manufacturing Example 1.
[0137] Manufacturing Example 7
[0138] A negative electrode active material was manufactured by the same process as in Manufacturing Example 1 except that milling was performed for 10 minutes instead of the milling for 10 hours in Manufacturing Example 1.
[0139] Manufacturing Example 8
[0140] Metal silicon having a particle size of about 90 nm was added to an isopropyl alcohol solvent, thereby manufacturing a first silicon slurry having a solid content of 20 % by weight.
[0141] The first silicon slurry was stirred in a homogenization reactor (2,500 rpm) for 10 minutes, and then polyvinyl pyrrolidone (PVP) was added thereto. This was re-stirred in the homogenization reactor for 10 minutes to produce a second silicon slurry.
[0142] The second silicon slurry was subjected to a homogenization process twice under a pressure of 1,000 bar in a high-pressure homogenizer. Next, the second silicon slurry was spray-dried. Next, heat treatment was performed at 1,100 ℃ under a nitrogen atmosphere to manufacture a negative electrode active material.
[0143] Manufacturing Example 9
[0144] Metal silicon with a particle size of about 100 nm and graphite particles with an average diameter (D50) of 7.5 ㎛ were added to an isopropyl alcohol solvent, thereby manufacturing a first silicon slurry having a solid content of 25 % by weight.
[0145] The first silicon slurry was stirred in a homogenization reactor (2,600 rpm) for 10 minutes, and then polyvinyl pyrrolidone (PVP) was added thereto, followed by re-stirring in the homogenization reactor for 10 minutes, thereby manufacturing a second silicon slurry.
[0146] The second silicon slurry was subjected to a homogenization process twice in a high-pressure homogenizer under a pressure of 1,000 bar. Next, the second silicon slurry was spray-dried. Next, heat treatment was performed at 1,100 ℃ under a nitrogen atmosphere, thereby manufacturing a negative electrode active material.
[0147] Manufacturing Example 10
[0148] Silicon with a particle size of about 800 nm and zirconia beads (YTZ) with a particle size of about 0.1 mm were added to an isopropyl alcohol solvent. Next, milling was performed for 70 hours while maintaining a temperature of 45 ℃ or less, thereby manufacturing a first silicon slurry in which the solid content of the metal silicon with a particle size of about 100 nm was 25 % by weight.
[0149] The first silicon slurry was stirred in a homogenization reactor (2,200 rpm) for 15 minutes, and then polyvinyl pyrrolidone (PVP) was added thereto, followed by re-stirring in the homogenization reactor for 15 minutes, thereby manufacturing a second silicon slurry.
[0150] The second silicon slurry was subjected to a homogenization process twice in a high-pressure homogenizer under a pressure of 1,100 bar. Next, the second silicon slurry was spray-dried. Next, heat treatment was performed at 1,300 ℃ under a nitrogen atmosphere to manufacture a negative electrode active material.
[0151]
[0152] Examples
[0153] Example 1
[0154] <Manufacturing of negative electrode>
[0155] A slurry was prepared by mixing the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) of Manufacturing Example 1 in a weight ratio of 8:1:1 in an N-methyl pyrrolidone solvent. Next, the slurry was applied to a copper thin film and then dried in a vacuum oven at 80°C for 8 hours to manufacture a negative electrode.
[0156] <Manufacturing of coin-type half-cell>
[0157] A metal lithium foil with a thickness of 0.3 mm was used as an opposite electrode (positive electrode) of the manufactured negative electrode, and a polypropylene sheet with a thickness of 0.1 mm was used as a separator. A coin-type half-cell was manufactured using an electrolyte solution prepared by dissolving 1M LiPF6 in ethylene carbonate and ethyl methyl carbonate mixed in a volume ratio of 3:7 in a solvent.
[0158] Example 2
[0159] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 2 was used instead of the negative electrode active material of Manufacturing Example 1.
[0160] Example 3
[0161] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 3 was used instead of the negative electrode active material of Manufacturing Example 1.
[0162] Example 4
[0163] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 4 was used instead of the negative electrode active material of Manufacturing Example 1.
[0164] Example 5
[0165] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 5 was used instead of the negative electrode active material of Manufacturing Example 1.
[0166] Example 6
[0167] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 6 was used instead of the negative electrode active material of Manufacturing Example 1.
[0168] Example 7
[0169] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) mixed in a weight ratio of 8.2:0.8:1 of Manufacturing Example 1 was used instead of the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) mixed in a weight ratio of 8:1:1 of Manufacturing Example 1.
[0170] Example 8
[0171] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) mixed in a weight ratio of 8:1.5:0.5 of Manufacturing Example 1 was used instead of the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) mixed in a weight ratio of 8:1:1 of Manufacturing Example 1.
[0172] Example 9
[0173] A coin-type half-cell was manufactured in the same manner as in Example 8 except that the negative electrode active material of Manufacturing Example 4 was used instead of the negative electrode active material of Manufacturing Example 2.
[0174] Example 10
[0175] A coin-type half-cell was manufactured in the same manner as in Example 8 except that the negative electrode active material of Manufacturing Example 5 was used instead of the negative electrode active material of Manufacturing Example 2.
[0176] Comparative Example 1
[0177] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 7 was used instead of the negative electrode active material of Manufacturing Example 1.
[0178] Comparative Example 2
[0179] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 8 was used instead of the negative electrode active material of Manufacturing Example 1.
[0180] Comparative Example 3
[0181] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 9 was used instead of the negative electrode active material of Manufacturing Example 1.
[0182] Comparative Example 4
[0183] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material of Manufacturing Example 10 was used instead of the negative electrode active material of Manufacturing Example 1.
[0184] Comparative Example 5
[0185] A coin-type half-cell was manufactured in the same manner as in Example 1 except that the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) mixed in a weight ratio of 8.5:1:0.5 of Manufacturing Example 7 was used instead of the negative electrode active material:conductive material (Super-P):binder (SBR-CMC) mixed in a weight ratio of 8:1:1 of Manufacturing Example 7 in Comparative Example 1.
[0186]
[0187] Experimental examples
[0188] Experimental Example 1 - Zirconium (Zr) content measurement
[0189] The content of zirconium contained in the negative electrode active material manufactured in each of Manufacturing Examples 1 to 10 was measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES). Results are shown in Table 1 below.
[0190] Experimental Example 2 - Electrical conductivity evaluation
[0191] The negative electrode active material manufactured in each of Manufacturing Examples 1 to 10 was pelletized, and then electrical conductivity was measured by the four-needle method while applying a load of 1,600 kgf to the pelletized negative electrode active material. Results are shown in Table 1 below.
[0192] Experimental Example 3 - Hardness evaluation
[0193] The hardness of the negative electrode manufactured in each of Examples 1 to 10 and Comparative Examples 1 to 5 was measured while applying a force of 30 kgf using a nanoindentation test (VH3300, manufactured by Rockwell Automation). Results are shown in Table 2 below.
[0194] Experimental Example 4 - Life characteristic evaluation
[0195] To perform a battery stabilization process, a process of charging the coin-type half-cell manufactured in each of Examples 1 to 10 and Comparative Examples 1 to 5 with a constant current of 0.1C until the voltage reached 0.01V and discharging it with a constant current of 0.1C until the voltage reached 1.5V was performed three times.
[0196] Next, the coin-type half-cell was charged with a constant current of 0.5C until the voltage reached 0.01V, and discharged with a constant current of 0.5C until the voltage reached 1.0V. This process was performed 50 times. After the 50th charge and discharge, a discharge capacity maintenance rate compared to the 1st charge and discharge was measured. Results are shown in Table 1 below.
[0197] Experimental Example 5 - Swelling evaluation
[0198] A swelling ratio during the charge / discharge process according to Experimental Example 4 was measured and calculated according to Equation 1 below. Results are shown in Table 2 below.
[0199] [Equation 1]
[0200] Swelling ratio (%) = [ (t2-t1) / t1] Х 100
[0201] where t1 represents the thickness of a negative electrode before the 1st charge and discharge, and t2 is the thickness of the negative electrode after the 50th charge and discharge.
[0202]
[0203] Zr content1)Electrical conductivityUnitppmS / cmManufacturing Example 13,22039.8Manufacturing Example 24,58040.1Manufacturing Example 35,80042.5Manufacturing Example 42,51038.5Manufacturing Example 51,83032.3Manufacturing Example 61,05032.1Manufacturing Example 712020.5Manufacturing Example 8-2)11.5Manufacturing Example 9-3)35.6Manufacturing Example 107,10045.61) Zr content: content in negative electrode active material (based on total weight of negative electrode active material)2),3) -: Zr non-detected
[0204]
[0205] Negative electrode active materialHardnessDischarge capacity maintenance rateSwelling ratioUnit-MPa%Example 1Manufacturing Example 120094.820Example 2Manufacturing Example 221094.321Example 3Manufacturing Example 322094.120Example 4Manufacturing Example 419896.520Example 5Manufacturing Example 519096.720Example 6Manufacturing Example 618596.820Example 7Manufacturing Example 120294.921Example 8Manufacturing Example 220894.320Example 9Manufacturing Example 419796.620Example 10Manufacturing Example 519096.620Comparative Example 1Manufacturing Example 78596.520Comparative Example 2Manufacturing Example 85683.742Comparative Example 3Manufacturing Example 96597.220Comparative Example 4Manufacturing Example 1023582.532Comparative Example 5Manufacturing Example 78896.621
[0206]
[0207] As shown in Tables 1 and 2, it was confirmed that Example 1 to 10, in which the content of zirconium in the negative electrode active material satisfied a range of 1,000 ppm to 6,000 ppm, exhibited excellent electrical conductivity and mechanical properties, high discharge capacity maintenance rate and a significantly reduced change in the thickness of the negative electrode after the cycle, compared to Comparative Example 1 to 5. This indicates that, since the negative electrode active material according to the present invention includes a nano-sized silicon particle, silicon in which the silicon particle is oxidized, and a carbon layer, the volume expansion of the silicon-based particle due to insertion of lithium ions is suppressed to improve lifespan characteristics. In addition, it was confirmed that as zirconium is included in a predetermined content range, electrical conductivity and mechanical properties were improved without deteriorating lifespan characteristics.
[0208]
[0209] An embodiment of the present invention can be applied to a negative electrode active material and a negative electrode including the same.
Claims
1.A negative electrode active material, comprising:a silicon particle;a silicon oxide in which a surface of the silicon particle is oxidized; anda carbon layer formed on at least a portion of a surface of the silicon oxide,wherein 1,000 ppm to 6,000 ppm of zirconium is comprised in the negative electrode active material.2.The negative electrode active material according to claim 1, wherein 40,000 ppm to 50,000 ppm of nitrogen is comprised in the negative electrode active material.3.The negative electrode active material according to claim 2, wherein a content of carbon contained in the negative electrode active material is 3 times to 6 times, compared to a content of the nitrogen.4.The negative electrode active material according to claim 1, wherein the silicon oxide is represented by Formula 1 below:[Formula 1]SiOx(0<x≤9).5.The negative electrode active material according to claim 1, wherein the silicon oxide has a thickness of 0.01 nm to 30 nm.6.The negative electrode active material according to claim 1, wherein the silicon oxide has a concentration gradient region.7.The negative electrode active material according to claim 6, wherein, in the concentration gradient region, a content of oxygen atoms, compared to a content of the silicon atoms, in a center direction of the silicon particle from the surface of the silicon oxide is continuously reduced.8.The negative electrode active material according to claim 1, wherein the silicon particle has a diameter of 10 nm to 150 nm.9.The negative electrode active material according to claim 1, wherein the carbon layer has a thickness of 10 nm to 50 nm.10.The negative electrode active material according to claim 1, wherein the carbon layer is comprised in a content of 15 % by weight to 30 % by weight in the negative electrode active material.11.The negative electrode active material according to claim 1, wherein the negative electrode active material has a BET specific surface area of 1 m2 / g to 5 m2 / g.12.A negative electrode, comprising:a negative electrode current collector; anda negative electrode active material layer formed at least one surface of the negative electrode current collector,wherein the negative electrode active material layer comprises a negative electrode active material,wherein the negative electrode active material comprises a silicon particle, a silicon oxide in which a surface of the silicon particle is oxidized, and a carbon layer formed on at least a portion of a surface of the silicon oxide, and1,000 ppm to 6,000 ppm of zirconium is comprised in the negative electrode active material.
Citation Information
Patent Citations
Negative Active Material for Rechargeable Lithium Battery and Rechargeable Lithium Battery Including Same
US20110097629A1
Lithium-ion secondary battery, anode for lithium-ion secondary battery, power tool, electric vehicle and energy storage system
US20110159368A1
Si / C COMPOSITE MATERIAL, METHOD FOR MANUFACTURING THE SAME, AND ELECTRODE
US20140234722A1
Negative electrode material for lithium-ion secondary battery, negative electrode for lithium-ion secondary battery, lithium-ion secondary battery, and method of producing negative electrode material for lithium-ion secondary battery
US20180114980A1
Composite, electrochemical active material composite using the composite, electrode including the composite or electrochemical active material composite, lithium battery including the electrode , field emission device including the composite, biosensor including the composite , semiconductor device including the composite , and thermoelectric device including the composite
US20190190014A1