A single-atom spin catalyst and method of synthesizing thereof
The scalable synthesis of ferromagnetic single-atom spin catalysts in MoS2 hosts addresses the sluggish OER kinetics in water electrolysis, achieving significant magnetic field enhancement and stability for efficient hydrogen production in both water and seawater.
Patent Information
- Application Number
- PCT/SG2024/050249
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-04
- Filing Date
- 2024-04-16
- Publication Date
- 2024-11-07
AI Technical Summary
The bottleneck for efficient hydrogen production via water electrolysis lies in the sluggish kinetics of the oxygen evolution reaction (OER) with scarce precious metal-based electrocatalysts, and there is a challenge in designing non-precious metal OER spin catalysts with abundant active sites and structure-performance relationships, especially under external magnetic fields.
A scalable hydrothermal synthesis method is developed to create a new class of robust ferromagnetic single-atom spin catalysts (SASCs) with substitutional magnetic atoms in a MoS2 host, such as Ni/MoS2, which exhibit ferromagnetic properties at room temperature and significant magnetic field enhancement, enabling efficient water and saline water electrolysis.
The SASCs demonstrate a dramatic enhancement of oxygen evolution reaction (OER) magnetocurrent by ~2880% under a mild magnetic field, outperforming commercial IrO2 catalysts in both water and seawater splitting, with superior stability and potential for industrial-scale hydrogen production.
Smart Images

Figure SG2024050249_07112024_PF_FP_ABST
Abstract
Description
A SINGLE-ATOM SPIN CATALYST AND METHOD OF SYNTHESIZING THEREOF FIELD OF THE INVENTION
[0001] The present invention generally relates to a single-atom spin catalyst (SASC) for water electrolysis. The present invention also relates to a method of synthesizing the single-atom spin catalyst. BACKGROUND
[0002] World-wide interest in hydrogen production from water electrolysis with renewable electricity has surged in recent years, since a hydrogen-based economy represents one of the best energy alternatives to the increasing concerns over carbon emissions and climate change1-4. However, the bottleneck for efficient hydrogen production via water electrolysis lies in the sluggish kinetics of oxygen evolution reaction (OER) with the utilization of scarce precious metal based electrocatalysts4-6. The sluggish OER kinetics can be attributed to a multiple electron transfer process with the formation of triplet-state molecular oxygen (↑O=O↑) that involves the spin change7,8. Despite extensive efforts devoted, the design of efficient and robust non-precious-metal OER spin catalysis with an abundance of desired active sites for the optimization of the adsorption / desorption strength of oxygen intermediates is still recognized as a major challenge9-14. Moreover, OER spin catalysts may also boost reactions by a mild external magnetic field to further increase the overall efficiency for water splitting towards green H2production11-15.
[0003] Nature has evolved excellent spin catalysis from abundant 3d-metals for photosynthesis and biochemical processes (e.g. bird’s migration)16-18, whose reaction kinetics over spin catalysis can be influenced by external magnetic field through changing the spin multiplicity of pre-reactional state and allowing the switch from spin forbidden into spin-allowed reaction pathways13,19. Inspired by this, heterogeneous OER electrocatalysts including ferromagnetic mix-metal oxide / metal have been developed to boost OER performance under external magnetic field11-15,19-24. These ferromagnetic OER catalysts often yield a mild enhancement of OER currents under the external magnetic field (typically lower than 200%), attributed to the fact that magnetic field favors the parallel alignment of oxygen radicals towards the formation of triplet-state molecularoxygen (↑O=O↑)13,19. In addition, the surface reconstruction of active sites in these materials during OER reaction makes it challenging to establish the structure- performance relationship12-15,20. To date, a fundamental understanding of magnetic field enhancement (MFE) to further improve the efficiency of water electrolysis has remained elusive due to the challenge in identification of well-defined active sites in these systems. Therefore, rational design of heterogeneous spin catalyst with atomically precise active sites, enabling giant MFE with maximized atom and energy efficiency, is highly desired to create industrially-relevant water splitting technologies. To realize this goal, one must tackle multiple challenges including the ability to engineer a high density of well-defined active sites with both short-range QSEI and long-range room-temperature ferromagnetic ordering, as well as weakly-interacting spin centers that can be altered under commonly accessible magnetic fields (e.g., permeant magnets).
[0004] The present invention not only provides a new platform to explore the mechanistic insights into giant MFE over atomically-precise spin active centers but also offers unprecedented opportunities to design non-precious metal based ferromagnetic single-atom spin catalysts (SASCs) for both water and saline water electrolyser technologies, as well as a new synthetic protocol to prepare the single metal atom catalysts. SUMMARY
[0005] This disclosure develops a new class of robust ferromagnetic single-atom spin catalysts (SASCs) with giant magnetic field enhancement (MFE), which can be applied to dramatically accelerate both water and saline water (such as seawater) electrolysis under commonly accessible magnetic fields (permeant magnet). Specifically, this disclosure reports a general and scalable approach for the synthesis of a new class of single-atom spin catalysts (SASCs) consisting of various substitutional magnetic atoms (M1) in the MoS2 host. Hydrothermal synthesis under acidic conditions allows to achieve isolated magnetic dopants with a widely tunable atomic doping ratio (M1 / Mo) up to ~20:100. Ni1 / MoS2presents the ferromagnetic property at room temperature, much different from the other reported Ni1 / MoS2materials. M1 / MoS2SASCs (Mn1, Fe1, Co1) adopt trigonal prismatic geometries, while Ni1 / MoS2 exhibits distorted tetragonal structure with local ferromagnetic coupling between Ni and nearest S atoms, and global room-temperature ferromagnetism. A mild magnetic field of ~0.5 T over Ni1 / MoS2yieldsa dramatic enhancement of OER magnetocurrent by ~2880%, revealing an excellent activity and stability in both seawater and pure water splitting cells, superior to commercial IrO2. In addition, the stability of Ni1 / MoS2 as OER catalyst is also superior to that of IrO2in pure water and seawater splitting cell, demonstrating its great potential in practical seawater splitting technology. This disclosure reveals that ferromagnetic SASCs provide a powerful magnetoelectric effect to accelerate both water and saline water electrolysis.
[0006] In one aspect, the present disclosure refers to a single-atom spin catalyst (SASC) consisting of a substitutional magnetic atom M embedded in a Molybdenum Disulfide (MoS2) host, with the formula of M1 / MoS2, wherein M1 / MoS2 has ferromagnetic property at room temperature.
[0007] In another aspect, the present disclosure refers to a water or seawater splitting cell comprising an electrode loaded with the SASC as disclosed herein.
[0008] In another aspect, the present disclosure refers to a method of synthesizing the SASC as disclosed herein, comprising the following steps: (a) dissolving molecular precursors comprising a metal salt, (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) and CH3CSNH2(thioacetamide) in distilled water to form a solution; (b) autoclaving the solution and cooling the solution to room temperature to result in a product; (c) washing the product with distilled water and ethanol and drying the product under vacuum; (d) heating the product in a furnace, and cooling the product to room temperature, to thereby form the SASC.
[0009] Advantageously, the method as disclosed herein is a scalable, low-cost method of synthesis of catalysts, costing less than S$ 350 per kilogram. The method as disclosed herein has broad applicability, which works for most scenarios of preparation of acid resistant SASC materials. In addition, the SASC as disclosed herein has high performance, with overpotential of < 320 mV at 50 mA cm-2, and high stability (stability > 50 h). The SASC achieves giant magnetic field enhancement. A dramatic enhancement of OER magnetocurrent by ~2880% was achieved with a mild magnetic field of ~0.5 T.BRIEF DESCRIPTION OF THE DRAWINGS
[0010] The invention will be better understood with reference to the detailed description when considered in conjunction with the non-limiting examples and the accompanying drawings, in which:
[0011] Figure 1 illustrates the synthesis and characterization of a series of M1 / MoS2SASCs. a, Illustration of the hydrothermal synthesis of M1 / MoS2 SASCs under acidic conditions and the giant magnetic field enhancement of ferromagnetic SASCs for water splitting. b, Metal dopant K-edge FT-EXAFS spectra of M1 / MoS2(Mn1, Fe1, Co1). c, Trigonal prismatic geometry of M1 / MoS2 (Mn1, Fe1, Co1). d, Ni K-edge FT-EXAFS spectra of Ni1 / MoS2 SASCs with different Ni contents and the reference samples. e, Non- centrosymmetric distorted tetragonal structure of Ni1 / MoS2. Yellow, blue and green spheres denote S, Mo and Ni atoms, respectively. f, TEM image of Ni1 / MoS2. g, STEM image of Ni1 / MoS2 resolves a characteristic triangular lattice consisting of brighter and darker sites (red circle), which can be assigned to Mo and Ni atomic sites, respectively. h, A zoom-in HAADF-STEM image of a single NiMosite (marked by red circle) with a darker contrast. i, The simulated HAADF-STEM image of DFT-optimized NiMo structure.
[0012] Figure 2 illustrates ferromagnetism of Ni1 / MoS2. a, Magnetization curves (M-H) of ferromagnetic Ni1 / MoS2with different Ni contents at 300 K. (Ni:Mo = 0.8:100, 1.6:100, 4:100, 6:100, 10:100, 14:100, 19:100). b, M-H curve of Ni1 / MoS2 with extremly low loadig of 0.05 wt% Ni (Ni:Mo = 0.2:100). c, The staurated magnetization and coercivity of Ni1 / MoS2with different Ni contents at 300 K. The average value in (c), including its error bar, is obtained from the analysis of three data points: the maximum value and its adjacent points to the right and left, with an interval of 100 mT. d, Temperature-dependent electron spin resonance (ESR) spectra of Ni1 / MoS2(14:100). e, Temperature-dependent M-H curves of Ni1 / MoS2 (14:100). f, d-orbital spliting of a NiMo site with the distorted tetragonal gemetry.
[0013] Figure 3 illustrates giant MFE of ferromagentic Ni1 / MoS2 for OER and wafer splitting. a, LSV curves of Ni1 / MoS2under different magnetic fields. Inset: Photo images of Ni1 / MoS2 as OER catalysts in water splitting cells at 1.65 V without (left) and with (right) magnetic fields. The oxygen bubbles formed on catalyst surface are highlighted with blue false color for visual guidance. Scale bar: 100 µm. b, Giant MFE of Ni1 / MoS2with dramatically increased magnetocurrent density for OER. c, Current density plot of IrO2 and Ni1 / MoS2 at 1.5-1.8 V before and after applying a magnetic field of 502 mT inwater splitting cells. d, I-T curves of Ni1 / MoS2under the magentic field to comapre with that of IrO2 catalyst in water splitting cells. e, Current density plot of IrO2 and Ni1 / MoS2 at 1.5-1.8 V before and after applying a magnetic field of 502 mT in seawater splitting cells. f, I-T curves of Ni1 / MoS2under the magentic field to comapre with that of IrO2catalyst in seawater splitting cells.
[0014] Figure 4 illustrates the origin of ferromagnetic Ni1 / MoS2. a-c, Spin density plots of (a) a single NiMosite, two adjacent NiMosites with (b) ferromagnetic and (c) antiferromagnetic coupling. d, Total and projectecd DOS of individal NiMosite with neighboring six S and Mo atoms in ferromagnetic Ni1 / MoS2 as shown in Fig.4b. Yellow, blue and green spheres denote S, Mo and Ni atoms, respectively. The light blue and purple isosurfaces represent the spin-up and spin-down of Ni1 / MoS2, respectively.
[0015] Figure 5 illustrates the origin of giant MFE of ferromagentic Ni1 / MoS2. a, Adsorption energy contour map of a single *OH on the NiMo region, three different S sites are labeled as S1, S2, S3respectively. b, The corresponding charge difference density of a single NiMosite upon the adsorption of *OH. c, PDOS of S1and S2atoms of Ni1 / MoS2models (shown in d) consisting two ajdacent NiMo sites with ferromagnetic (dark blue) and antiferromagnetic (pink) coupling. d, Free energy profile of OER with the corresponding adsorption configurations of reaction intermediates over ferromagnetic (dark blue) and antiferromagnetic (pink) Ni1 / MoS2. Insets: The spin density plot of *OOH on S site over ferromagnetic (top) and antiferromagnetic (bottom) Ni1 / MoS2 model towards the transition from *OOH to O2. The light blue and purple isosurfaces represent the spin-up and spin- down, respectively. e, f, Operando S K-edge XANES spectra for Ni1 / MoS2 under 112 mT (e) and 0 mT (f). OCP: open circuit potential. g, The first derivative curves at 1.8 V vs. RHE under 0 and 112 mT.
[0016] Figure 6 illustrates the structural characterization of Ni1 / MoS2with different metal loading. a, HRTEM image of Ni1 / MoS2 (14:100). b, HAADF-STEM image and corresponding EDS maps of Ni1 / MoS2(14:100). c, XRD patterns of Ni1 / MoS2with different Ni contents. d, The experimental (green) linear intensity profile of STEM (Fig. 1h) and the calculated data (Fig. 1i) (yellow) of Ni1 / MoS2. e, The experimental (solid line) and simulation (dotted line) curves of Ni K-edge XANES spectra. f, Comparison of the experimental (solid line) FT-EXAFS curves with the calculated data (dotted line).
[0017] Figure 7 illustrates the characterization and the origin of ferromagnetism in Ni1 / MoS2. a, The peak seperation of ESR spectra for Ni1 / MoS2 (14:100) under different temperatures. b, c, Comparison of the Ni K-edge XANES (b) and FT-EXAFS (c) spectra for Ni1 / MoS2(14:100) with and without magnetic field. d, d-orbtial spliting of a NiMosite for six (left, Es = 0.461 eV, C3h) and four (right, Es = 1.129 eV, C2v) coordination numbers. e, The energy localized function (ELF) of one Ni dopant- substituted Mo site in MoS2. f, Total and projected DOS of individual NiMosite with neighboring six S and Mo atoms in antiferromagnetic Ni1 / MoS2as shown in Fig. 4c. Yellow, blue and green spheres are S, Mo and Ni atoms, respectively.
[0018] Figure 8 illustrates MFE of Ni1 / MoS2for OER and the comparison with commercial IrO2 catalysts. a, Overpotentials of Ni1 / MoS2(14:100) at current density of 40 mA cm-2and Tafel slopes. The averaged value in (a) togather with the error bar is obtained from the analysis of five sets of experimental results. b, EIS spectra of MoS2 and Co1 / MoS2with and withot magnetic field. c, LSV curves of Ni1 / MoS2(0.8:100). d, I-T curves of Ni1 / MoS2upon switching on and switching off different magnetic fields at 1.6 V vs. RHE. e, I-T curves of Ni1 / MoS2 after switching off magnetic fields at 1.6 V vs. RHE. f, I-T curves of Ni1 / MoS2at different voltages upon switching on and switching off the magnetic field at 502 mT. g, I-T curves of Ni1 / MoS2under 502 mT and IrO2catalyst at 1.6 V vs. RHE.
[0019] Figure 9 illustrates the origin of giant MFE of ferromagentic Ni1 / MoS2. a, The second possible free energy profile of OER with the corresponding adsorption configurations of reaction intermediates over ferromagnetic (cyan) and antiferromagnetic (dark red) Ni1 / MoS2. b, c, The spin density plot of *OOH on S site over ferromagnetic (b) and antiferromagnetic (c) Ni1 / MoS2model towards the transition from *OOH to O2. Yellow, blue, green, red and light blue spheres are S, Mo, Ni, O and H atoms, respectively. The light blue and purple isosurfaces represent the spin-up and spin-down density, respectively.
[0020] Figure 10 illustrates probing the catalytic OER site and the origin of giant MFE for ferromagnetic Ni1 / MoS2. a, b, The first derivative curves of operando S K- edge XANES at different potentials under 0 mT (a) and 112 mT (b). c, d, PDOS of O species over AFM (c) and FM (d) coupled counterparts of Ni1 / MoS2.
[0021] Figure 11 shows giant MFE of 2.4 inch-sized ferromagnetic Ni1 / MoS2(14:100) electrode for a large water splitting cell. a, Photograph of the inch-sizedNi1 / MoS2and Pt / C electrodes. b-c, inch-sized Ni1 / MoS2as anode (b) for magnetic-field enhanced water splitting (c).
[0022] Figure 12 illustrates the crucial role of the operando acidic conditions during the synthesis of M1 / MoS2SASCs.
[0023] Figure 13 shows TEM and HRTEM images of MoS2without doping.
[0024] Figure 14 shows structural characterization of various M1 / MoS2 SASCs. TEM, HRTEM, STEM images and linear intensity profiles of Mn1 / MoS2(a-d), Fe1 / MoS2(e-h) and Co1 / MoS2(i-l). It is noted that M1 / MoS2materials possess the 3D morphological structure, similar to that of pure MoS2.
[0025] Figure 15 are HAADF-STEM images and corresponding EDS maps of various M1 / MoS2SASCs. a, Mn1 / MoS2. b, Fe1 / MoS2. c, Co1 / MoS2.
[0026] Figure 16 shows XRD patterns of M1 / MoS2 and pure MoS2 samples.XRDpatterns of M1 / MoS2 only present the peaks associated with the 2H phase of MoS2 support, consistent with the behavior observed in other reported MoS2-based SACs materilas63-65.
[0027] Figure 17 showsRaman spectra of M1 / MoS2and pure MoS2samples. The red shift of E2g and A1g modes in Raman spectra of M1 / MoS2 (M = Mn, Fe, Co and Ni) compared to these modes of pure MoS2suggests the successful incorporation of dopant atoms into the MoS2 lattice, similar to other reported single-metal-atom doped MoS266,67. This red shift of E2g and A1g modes is attributed to the lattice distortion and charge doping effect after the substitutional metal dopant introduced to the MoS2lattice, consistent with MoS2doped by other metal atoms with different level of strain and charge doping67. The red shift of E2g mode indicates the increased number of strained MoS2 sites due to the presence of single metal atom dopant68. The red shift of A1g mode indicates the increased electron density of MoS2after the substitutional replacement of Mo sites by single metal atoms69. These changes induce the spin polarization of Mo and S atoms near Ni atoms, leading to the formation of ferromagnetism at room temperature (Fig.2 and Fig.4), and resulting in the enhanced OER activity under external magnetic field.
[0028] Figure 18 are TEM, HAADF-TEM images and corresponding EDS maps of Ni1 / MoS2 (19:100).
[0029] Figure 19 areSTEM images acquired at different thinner flake regions ofNi1 / MoS2(14:100).
[0030] Figure 20 showssimulation of XANES spectra of different single NiMosites in MoS2. a, Partial four coordination number of Ni. b, Six coordination number of Ni. c, Four coordination number of Ni. Yellow, blue and green spheres denote S, Mo and Ni atoms, respectively. d, The simulation of Ni K-edge XANES spectra of Ni coordinated with six S atoms. e, The simulation of Ni K-edge XANES spectra of Ni coordinated with four S atoms. The partial tetra-coordination configuration and tetra-coordination configuration can be distinguished from each other through the analysis of the Ni−S length. Note that the Ni−S length in the partial tetra-coordination and tetra-coordination is calculated to be 2.285Å and 2.217Å, respectively. The magnetic properties observed for Ni1 / MoS2sample also suggest a partial tetra-coordination configuration for single Ni dopant in MoS2 host.
[0031] Figure 21 are EDS spectra of M1 / MoS2 SASCs. a, Mn1 / MoS2. b, Fe1 / MoS2. c, Co1 / MoS2. d, Ni1 / MoS2.
[0032] Figure 22 showsXANES characterization of M1 / MoS2(Mn1, Fe1, Co1). a-c, experimental data and simulation of (a) Mn, (b) Fe, (c) Co K-edge XANES. d, Comparison of the experimental (solid line) FT-EXAFS with the calculated data (dotted line).
[0033] Figure 23 shows FT-EXAFS in k space of M1 / MoS2 (Mn1, Fe1, Co1 andNi1). a-d,experimental data and fitting (red balls) of (a) Mn, (b) Fe, (c) Co, (d) Ni K- edge EXAFS.
[0034] Figure 24 shows the comparison of the experimental K-edge XANES spectrafor all thesubstitutional single metal atoms, M (M = Mn, Fe, Co and Ni) and Mo atoms of M1 / MoS2 SASCs. a, Mn1 / MoS2. b, Fe1 / MoS2. c, Co1 / MoS2. d, Ni1 / MoS2. The spectraare plotted as a function of ΔE(denote the energy difference between the photon energy E and the peak in the first derivative of thedata E0).
[0035] Figure 25 shows the comparison of the experimental K-edge FT-EXAFSspectra for all thesubstitutional single metal dopants (M = Mn, Fe, Co and Ni) of M1 / MoS2 SASCs.
[0036] Figure 26 shows thecomparison of XANES spectra for M1 / MoS2(M=Mn, Fe, Co, Ni). The spectra are plotted as a function of ΔE (denote the energy difference between the photon energy E and the peak in the first derivative of the data E0).
[0037] Figure 27 shows the energy profile as a function of the diagonal displacement of transition M atom (M=Mn, Fe, Co, Ni).
[0038] Figure 28 shows the electronic structures of Ni1 / MoS2. a, d, DOS of Ni1 / MoS2 with six (a) and four (d) coordinated number of Ni atom. b, e, PDOS of d orbital in Ni1 / MoS2with six (b) and four (e) coordinated number of Ni atom. c, f, configuration of Ni1 / MoS2 with six (c) and four (f) coordinated number of Ni atom. Yellow, blue and green spheres are S, Mo and Ni atoms, respectively.
[0039] Figure 29 shows thesoft XAS of Ni L-edge spectrum of Ni1 / MoS2(14:100). Ni L-edge spectrum demonstrates the existence of Ni3+in Ni1 / MoS2, similar to the cases of other reported Ni-based materials71,72.
[0040] Figure 30 shows ESR spectra of Ni1 / MoS2(14:100). a, ESR spectra acquired from 2 K to 300 K. b, The model of peak seperation (ΔHpp) obtained from ESR spectrum at 2K for Ni1 / MoS2. The plot of ΔHpp of ESR spectra taken at different tempeatures are shown in Fig. 7a. The ferromagnetic property of Ni1 / MoS2is also supported by the decreasing ΔHpp with increasing temperatures, as shown in Fig. 7a, which is similar to other reported ferromagnetic materials73,74.
[0041] Figure 31 shows the magnetic hysteresis loops of Ni1 / MoS2 (14:100) measured at 50-300 K. a, M-H loops after normalization. b, M-H loops of Ni1 / MoS2(14:100).
[0042] Figure 32 shows the magnetic hysteresis loops measured at 300 K.
[0043] Figure 33 shows thespin density plots of M1 / MoS2with two substituted metal atoms. a, Mn1 / MoS2. b, Fe1 / MoS2. c, Co1 / MoS2. The light blue and purple isosurfacesrepresent the up and downdirections of spin, respectively.
[0044] Figure 34 are photo images of bubbles before and after applying magnetic field in water splitting cell. Ni1 / MoS2 (14:100) as water oxidation electrocatalyst without and with magnetic field of 502 mT at 1.65 V. Scale bar: 100 µm.
[0045] Figure 35shows Tafel slopes of Ni1 / MoS2 (14:100) measured under differentmagneticfields.
[0046] Figure 36 shows the electrochemically active surface area characterization. a, b, CV curves of Ni1 / MoS2 (14:100) under magnetic (a) and zero-magnetic (b) field. c, CV curves of MoS2. d, Charging current density differences (Δj = ja – jc) plotted against scan rates of MoS2, Ni1 / MoS2(under magnetic and zero-magnetic field), jais the positive current density and jc is the negative current density. The linear slope is equivalent to twice of the double-layer capacitance Cdl.
[0047] Figure 37 shows the magneticproperties analysis of Ni1 / MoS2. a, Orbital-resolved spin up and spin down band structures of Ni atom in Ni1 / MoS2. b, Electronic density of states for the Ni d states in Ni1 / MoS2.
[0048] Figure 38 shows current density plot of Ni1 / MoS2 (14:100) after switching offthe magneticfield. a, b, I-T curves (a) and ratio percentage (b) of current density after and before switching off the magnetic fields at 1.6 V vs. RHE. c, d, I-T curves (c) and ratio percentage (d) of the current density after and before switching off the magnetic field (502 mT) at different voltages. The averaged value in (c, d) togather with the error bar is obtained from the analysis of five sets of cycling-experimental results.
[0049] Figure 39 shows LSV curves of M1 / MoS2 under magnetic (502 mT) / zero- magnetic fields.
[0050] Figure 40 shows EIS spectra of Ni1 / MoS2 (14:100) under magnetic field.
[0051] Figure 41 showsMagnetic field dependent LSV and MFE curves of Ni1 / MoS2. a, b, Ni1 / MoS2(6:100). c, d, Ni1 / MoS2(19:100).
[0052] Figure 42 showscurrent density plot of Ni1 / MoS2after switching on / off the magnetic field at 1.6 V vs. RHE. a, Ni1 / MoS2 (6:100). b, Ni1 / MoS2 (19:100).
[0053] Figure 43 shows LSV curves of Ni1 / MoS2 (4:100) under the 502 mT.
[0054] Figure 44 shows LSV curves of Ni1 / MoS2(14:100) under different magnetic fields. It is noted that the magnetocurrent remains nearly constant in a large potential range upon the switch of the orientation of magnetic field.
[0055] Figure 45 shows the labelling of different atoms in Ni1 / MoS2.
[0056] Figure 46 shows possible configurations of Ni1 / MoS2 with two Ni atoms.Yellow, blue andgreen spheres are S, Mo and Ni atoms, respectively.
[0057] Figure 47 shows PDOS of different S atoms in Ni1 / MoS2. Blue and yellowlines refer to thePDOS of S atoms nearby Mo and Ni, respectively.More states occur atFermi energy (EF) for the S atoms near Ni, indicating that S atoms near Ni are moreactivefor catalyzing OER than those of S atoms near Mo.
[0058] Figure 48 shows magnetic evolution of Ni1 / MoS2with different Ni contents. a, PDOS of Ni and MoS2 for Ni1 / MoS2 with different ratios of Ni:Mo from 1:48 to 1:15. b, The electronic densities at fermi energy for Ni1 / MoS2 with different ratios of Ni:Mo. c, The critical concentration of FM-PM transition based on Stoner criterion for Ni1 / MoS2. Note: The yellow line refers to the calculated electronic density at fermi energy D(EF) ofNi1 / MoS2, and the blue line represents the product of Stoner parameter I (as shown in Table 5) and D(EF).
[0059] Figure 49 show magnetic property analysis of M1 / MoS2. a, c, e, Orbital- resolved spin up and spin down band structures of Mn atom in Mn1 / MoS2(a), Fe atom in Fe1 / MoS2(c) and Co atom in Co1 / MoS2(e). b, d, f, Electron density of states for the Mn d states in Mn1 / MoS2 (b), Fe d states in Fe1 / MoS2 (d) and Co d states in Co1 / MoS2 (f).
[0060] Figure 50 shows electron transfer between Ni and S atoms. a, PDOS of singleNi inNi1 / MoS2. b, PDOS of S1and S2in Ni1 / MoS2. c, Schematic illustration of electron transfer from Ni to S1 and S2. d, Diagram of electron transfer from Ni 3d to S1 and S22p orbitals.
[0061] Figure 51 show configurations of chemical *OH adsorption over Ni1 / MoS2. a, Ni site. b, Mo site. c, bridge site between two S atoms. d, S1 site. e, S2 site. f, S3 site. The calculated results are shown in Table 9, and the OH* is more likely to adsorb on the S1 or S2sites.
[0062] Figure 52 shows electronic features of atoms in Ni1 / MoS2. a, Localized potential of Mo and Ni atoms in Ni1 / MoS2. b, Comparison of localized potentials of Mo, Ni and different S atoms for Ni1 / MoS2. S1, S2and S3represent adjacent S atom with the Ni−S bonding length of 2.521 Å, 2.285 Å, and S atom bonded with Mo, respectively.
[0063] Figure 53 shows free energy profiles of Ni1 / MoS2 with the step of *O to *OOH. Inset is the configuration of *OOH over the top S site. Yellow, blue, green, red and light blue spheres are S, Mo, Ni, O and H atoms, respectively.
[0064] Figure 54 shows free energy profiles of FM and AFM Ni1 / MoS2 for OER. Inset is the configuration of each step for OER. Yellow, blue, green, red and light blue spheres are S, Mo, Ni, O and H atoms, respectively.
[0065] Figure 55 are photographs of the home-customized electrochemical cell foroperandoXAS characterizations of Ni1 / MoS2 (14:100) during OER under magnetic field.
[0066] Figure 56 are XAS characterizations of Ni1 / MoS2(14:100) under OCP. a, S K-edge XANES spectra. b, The corresponding first derivative curves.
[0067] Figure 57 shows Operando S K-edge XANES measurements of Ni1 / MoS2 (14:100) during OER reactions at different potentials under 0 mT (a) and 112 mT (b).
[0068] Figure 58shows water oxidation with IrO2and Ni1 / MoS2(14:100) in water splitting cells.
[0069] Figure 59 showswater oxidation with IrO2and Ni1 / MoS2(14:100) in seawater.The watersplitting cells use the electrolyte (1 M KOH) of KOH dissolved in seawater.
[0070] Figure 60 shows stability characterization of the Ni1 / MoS2 (14:100) catalyst. a-d, TEM and HRTEM images of Ni1 / MoS2after stability tests (25 h) in water splitting cell in 1 M KOH solution (a, b) and electrolyte (1 M KOH) of KOH dissolved in seawater (c, d). e, XRD patterns of Ni1 / MoS2 before and after OER measurement in 1 M KOH solution.
[0071] Figure 61 shows stability characterization of the Ni1 / MoS2(14:100) catalyst. a, Mo 3d XPS spectra. b, S 2p XPS spectra. c, Ni 2p XPS spectra. d, Raman spectra.
[0072] Figure 62 shows DFT calculations of Cl- adsorption over IrO2 and Ni1 / MoS2 materials. The lowest energy of configuration for Cl- adsorption is set to 0 eV in (a) and (b).
[0073] Figure 63 shows adsorption energy of Cl- over IrO2 and Ni1 / MoS2 materials.
[0074] Figure 64 shows calibration curve of the permanent neodymium magnet. The Gauss meter is used for the determination of magnetic field experienced by the electrode. Error bars represent the standard deviation of the experimental values. The averaged value in this figure together with the error bar is obtained from the analysis of five sets of experimental results. DETAILED DESCRIPTION
[0075] Heterogeneous single-atom spin catalysts (SASCs) combined with magnetic fields provides a powerful means for accelerating chemical reactions with enhanced metal utilization and reaction efficiency. However, designing these catalysts remains challenging due to the need for a high density of atomically dispersed active sites with short-range quantum spin exchange interaction (QSEI) and long-range ferromagnetic ordering. In this disclosure, a scalable hydrothermal approach was devised, involving operando acidic environment for synthesizing various SASCs with widely tunable substitutional magnetic atoms (M1) in a MoS2host. Among all the M1 / MoS2, Ni1 / MoS2adopts a distorted tetragonal structure that prompts both ferromagnetic coupling to nearby S atoms as well as adjacent Ni1 sites, resulting in global room-temperature ferromagnetism. Such coupling benefits spin-selective charge transfer in oxygen evolution reactions (OER) to produce triplet O2. Furthermore, a mild magnetic field of ~0.5 T enhances the OER magnetocurrent by ~2880% over Ni1 / MoS2, leading to anexcellent activity and stability in both seawater and pure water splitting cells. As supported by operando characterizations and theoretical calculations, a giant magnetic- field enhanced OER performance over Ni1 / MoS2 is attributed to field-induced spin alignment and spin density optimization over S active sites arising from field-regulated S(p)-Ni(d) hybridization, which in turn optimizes the adsorption energies for radical intermediates to reduce overall reaction barriers.
[0076] In one aspect, the present disclosure refers to a single-atom spin catalyst (SASC) consisting of a substitutional magnetic atom M embedded in a Molybdenum Disulfide (MoS2) host, with the formula of M1 / MoS2, wherein M1 / MoS2 has ferromagnetic property at room temperature.
[0077] The substitutional magnetic atom M is selected from the group consisting of nickel (Ni), manganese (Mn), iron (Fe), and cobalt (Co), or mixtures thereof. Nickel (Ni), manganese (Mn), iron (Fe), and cobalt (Co) are transition metals. They have atomic numbers 28, 25, 26, and 27, respectively. In one example, the substitutional magnetic atom M is Ni. In another example, the substitutional magnetic atom M is Mn. In another example, the substitutional magnetic atom M is Fe. In another example, the substitutional magnetic atom M is Co. In one particular example, the substitutional magnetic atom M is Ni, and the formula of the SASC is Ni1 / MoS2.
[0078] The bottleneck for efficient hydrogen production via water electrolysis lies in the sluggish kinetics of oxygen evolution reaction (OER) with the utilization of scarce precious metal based electrocatalysts. The rationally designed heterogeneous single-atom spin catalyst (SASC) as disclosed herein has atomically precise active sites, enabling giant magnetic field enhancement (MFE) at room temperature, with maximized atom and energy efficiency, and can be used to create industrially-relevant water splitting technologies towards green H2 production.
[0079] M1 / MoS2 (M = Mn, Fe and Co) are coordinated with six adjacent S atoms to form the trigonal prismatic MS6configuration. In addition, Ni1 / MoS2adopts a distorted tetragonal structure that prompts both ferromagnetic coupling to nearby S atoms as well as adjacent Ni1 sites, resulting in global room-temperature ferromagnetism. Such coupling benefits spin-selective charge transfer in oxygen evolution reactions (OER) to produce triplet O2. Furthermore, a mild magnetic field of ~0.5 T enhances the OER magnetocurrent by ~2880% over Ni1 / MoS2, leading to an excellent activity and stability in both seawater and pure water splitting cells.
[0080] The atomic doping ratio (Mi / Mo) of the SASC as disclosed herein is up to about 20: 100. In one example, the atomic doping ratio (Mi / Mo) of the SASC as disclosed herein is about 0.8:100, about 1:100, about 1.6:100, about 2:100, about 3:100, about 4:100, about 5:100, about 6:100, about 7:100, about 8:100, about 9:100, about 10:100, about 1 1 :100, about 12:100, about 13:100, about 14:100, about 15:100, about 16:100, about 17:100, about 18:100, about 19:100, about 20:100. In one particular example, the formula of the SASC is Ni 1 / M0S2. and the atomic doping ratio (Nii / Mo) of Ni 1 / M0S2 is about 14:100.
[0081] In one example, the content of the substitutional magnetic atom M in M1 / M0S2 is 0.2-4.8 wt%. In another example, The Ni content in Nii / MoSz is selected from the group consisting of 0.20, 0.38, 0.95, 1.42, 2.41, 3.12 and 4.20 wt%. In one particular example, the Ni content in Nii / MoS2 is 3.12 wt%.
[0082] The Ni-Ni distance in Nii / MoS2 is about 5.460-8.263 A. In one example, the Ni-Ni distance in Nii / MoS2 is about 6.390 A. Ni-Ni distance of -6.390 A represents the most stable configuration due to its lowest formation energy.
[0083] In another aspect, the present disclosure refers to a water or seawater splitting cell comprising an electrode loaded with the SASC as disclosed herein.
[0084] In one example, the SASC of the water or seawater splitting cell as disclosed herein is Nii / MoS2. In another example, the SASC of the water or seawater splitting cell as disclosed herein is Mm / MoSz. In another example, the SASC of the water or seawater splitting cell as disclosed herein is Fei / MoS2. In another example, the SASC of the water or seawater splitting cell as disclosed herein is C01 / M0S2.
[0085] In one example, the splitting cell comprising an electrode loaded with the SASC as disclosed herein uses pure water for water electrolysis. In another example, the splitting cell comprising an electrode loaded with the SASC as disclosed herein uses seawater (saline water) for water electrolysis.
[0086] Compared to pure water, seawater splitting is recognized as a more economically-vital water splitting technology. However, the catalyst instability due to the presence of a variety of components in seawater, especially chloride ions, poses a great challenge for the practical utilization of seawater in water splitting technology. Commercial IrCF catalyst shows a rapid decay and drops in current density by 19.2 mA cm-2within 25 h. In contrast, Nii / MoS2 as disclosed herein demonstrates a negligible decrease in current density by 2.3 mA cm'2within the same period, revealing an excellentOER stability in seawater, likely due to a high tolerance of Ni1 / MoS2to the Cl adsorption against the catalyst deactivation. As a result, Ni1 / MoS2 (3.12 wt%) reveals a remarkably improved OER performance at 502 mT for seawater splitting, much better than commercial IrO2in terms of current density in a wide potential range of 1.5-1.8 V.
[0087] In another aspect, the present disclosure refers to a method of synthesizing the SASC as disclosed herein, comprising the following steps: (a) dissolving molecular precursors comprising a metal salt, (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) and CH3CSNH2(thioacetamide) in distilled water to form a solution; (b) autoclaving the solution and cooling the solution to room temperature to result in a product; (c) washing the product with distilled water and ethanol and drying the product under vacuum; (d) heating the product in a furnace, and cooling the product to room temperature, to thereby form the SASC.
[0088] In one example, the metal salt used in the method as disclosed herein is selected from the group consisting of Mn(CH3COO)2·4H2O, Fe(CH3COO)2·4H2O, Co(CH3COO)2·4H2O and Ni(CH3COO)2·4H2O. In another example, the metal salt used in the method as disclosed herein is Mn(CH3COO)2·4H2O. In another example, the metal salt used in the method as disclosed herein is Fe(CH3COO)2·4H2O. In another example, the metal salt used in the method as disclosed herein is Co(CH3COO)2·4H2O. In another example, the metal salt used in the method as disclosed herein is Ni(CH3COO)2·4H2O.
[0089] In one example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method as disclosed herein is 1 to 5 mmol. In another example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method as disclosed herein is 1-3 mmol, 2-4 mmol, 3-5 mmol, 1-4 mmol, or 2-3 mmol. In another example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method as disclosed herein is about 1 mmol. In another example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method as disclosed herein is about 2 mmol. In another example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method as disclosed herein is about 3 mmol. In another example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method asdisclosed herein is about 4 mmol. In another example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) used in the method as disclosed herein is about 5 mmol.
[0090] In one example, the amount of CH3CSNH2(thioacetamide) used in the method as disclosed herein is 5 to 20 mmol. In another example, the amount of CH3CSNH2(thioacetamide) used in the method as disclosed herein is 5-10 mmol, 6-11 mmol, 7-12 mmol, 8-13 mmol, 9-14 mmol, 10-15 mmol, 11-16 mmol, 12-17 mmol, 13-18 mmol, 14- 19 mmol, 15-20 mmol, 6-19 mmol, 7-18 mmol, 8-17 mmol, 9-16 mmol, 10-15 mmol, 11- 14 mmol, or 12-13 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 5 mmol. In another example, the amount of CH3CSNH2(thioacetamide) used in the method as disclosed herein is about 6 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 7 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 8 mmol. In another example, the amount of CH3CSNH2(thioacetamide) used in the method as disclosed herein is about 9 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 10 mmol. In another example, the amount of CH3CSNH2(thioacetamide) used in the method as disclosed herein is about 11 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 12 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 13 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 14 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 15 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 16 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 17 mmol. In another example, the amount of CH3CSNH2(thioacetamide) used in the method as disclosed herein is about 18 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 19 mmol. In another example, the amount of CH3CSNH2 (thioacetamide) used in the method as disclosed herein is about 20 mmol.
[0091] In one example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2 used in the method as disclosed herein is 4 to 10. In another example, the molar ratio of(NH4)6Mo7O24·4H2O to CH3CSNH2used in the method as disclosed herein is 4 to 6, 5 to 7, 6 to 8, 7 to 9, 8 to 10, 5 to 9, or 6 to 8. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2 used in the method as disclosed herein is about 4. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2used in the method as disclosed herein is about 5. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2 used in the method as disclosed herein is about 6. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2used in the method as disclosed herein is about 7. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2 used in the method as disclosed herein is about 8. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2 used in the method as disclosed herein is about 9. In another example, the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2 used in the method as disclosed herein is about 10.
[0092] In one example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is below 20% (nM:nMo max). In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 19%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 18%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 17%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 16%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 15%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 14%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 13%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 12%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 11%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 10%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 9%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 8%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 7%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 6%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 5%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 4%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 3%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 2%. In another example, the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is about 1%.
[0093] In one particular example, the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) is about 1 mmol, and the amount of CH3CSNH2 (thioacetamide) is about 10 mmol.
[0094] In one example, the metal salt is below 0.2 mmol when (NH4)6Mo7O24·4H2O is 0.143 mmol.
[0095] In one example, in step (b) of the method as disclosed herein, the solution is autoclaved at 160 to 200 °C for 12 to 24 h. In another example, the solution in step (b) of the method as disclosed herein, the solution is autoclaved at a temperature selected from the group consisting of about 160 °C, about 165 °C , about 170 °C , about 175 °C , about 180 °C, about 185 °C, about 190 °C, about 195 °C, and about 200 °C, and for a duration selected from the group consisting of about 12 h, about 13 h, about 14 h, about 15 h, about 16 h, about 17 h, about 18 h, about 19 h, about 20 h, about 21 h, about 22 h, about 23 h, and about 24 h.
[0096] In one particular example, in step (b) of the method as disclosed herein, the solution is autoclaved at about 180 °C for about 20 h.
[0097] In one example, in step (c) of the method as disclosed herein, the product is dried under vacuum at 50-80 °C for 8 to 20 h. In another example, in step (c) of the method as disclosed herein, the product is dried under vacuum at a temperature selected from the group consisting of about 50 °C, about 55 °C, about 60 °C, about 65 °C, about 70 °C, about 75 °C, and about 80 °C, and for a duration selected from the group consisting of about 8 h, about 9 h, about 10 h, about 11 h, about 12 h, about 13 h, about 14 h, about 15 h, about 16 h, about 17 h, about 18 h, about 19 h, and about 20 h.
[0098] In one particular example, in step (c) of the method as disclosed herein, the product is dried under vacuum at about 60 °C for about 12 h.
[0099] In one example, in step (d) of the method as disclosed herein, the product is heated to 350 to 500 °C at a rate of 5 to 10 °C min-1. In another example, in step (d) of the method as disclosed herein, the product is heated to a temperature selected from the group consisting of about 350 °C, about 400 °C, about 450 °C, and about 500 °C, and at a rate of about 5 °C min-1, about 6 °C min-1, about 7 °C min-1, about 8 °C min-1, about 9 °C min-1, and about 10 °C min-1.
[0100] In one particular example, in step (d) of the method as disclosed herein, the product is heated to about 400 °C at a rate of about10 °C min-1.
[0101] As disclosed herein, the M1 / M0S2 SASCs with tunable metal content are synthesized via a well-designed hydrothermal approach by introducing different molecular precursors including metal salts (M2+), ammonium molybdate tetrahydrate and thioacetamide in one step, distinct from the chemical vapor deposition growth of single- atom doped M0S2 monolayer and the two-step hydrothermal methods25. Particularly, the decomposition of thioacetamide during hydrothermal reaction not only provides S sources for the formation of 2H-phase M0S2 host but also creates the desired “operando acidic environment” to facilitate the synthesis of atomically dispersed single atoms embedded into the carrier lattice by suppressing the formation of metallic nanoparticlcs. As a result, such a general synthetic protocol allows for the scalable synthesis of various M1 / M0S2 SASCs (Mi=Mn, Fc, Ni, Co) with widely tunable atomic doping ratio (M1 / M0) up to -20:100. Generally, high doping density shortens the averaged spacing between adjacent magnetic dopant sites to promote their magnetic exchange interaction into long- range magnetic order.
[0102] As used in this application, the singular form “a,” “an,” and “the” include plural references unless the context clearly dictates otherwise. For example, the term “a primer” includes a plurality of primers, including mixtures and combinations thereof.
[0103] As used herein, the term “comprising” means “including.” Variations of the word "comprising", such as “comprise” and “comprises,” have correspondingly varied meanings. Thus, for example, a composition “comprising” X may consist exclusively of X or may include one or more additional unrecited components.
[0104] As used herein, the term “about” in the context of concentration of a substance, size of a substance, length of time, or other stated values means + / - 5% of the stated value, or + / - 4% of the stated value, or + / - 3% of the stated value, or + / - 2% of the stated value, or + / - 1% of the stated value, or + / - 0.5% of the stated value.
[0105] Throughout this disclosure, certain embodiments may be disclosed in a range format. It should be understood that the description in range format is merely for convenience and brevity and should not be construed as an inflexible limitation on the scope of the disclosed ranges. Accordingly, the description of a range should be considered to have specifically disclosed all the possible sub-ranges as well as individual numerical values within that range. For example, description of a range such as from 1 to 6 should be considered to have specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6 etc., as well as individual numberswithin that range, for example, 1, 2, 3, 4, 5, and 6. This applies regardless of the breadth of the range.
[0106] The invention illustratively described herein may suitably be practiced in the absence of any element or elements, limitation or limitations, not specifically disclosed herein. Thus, for example, the terms "comprising", "including", "containing", etc. shall be read expansively and without limitation. Additionally, the terms and expressions employed herein have been used as terms of description and not of limitation, and there is no intention in the use of such terms and expressions of excluding any equivalents of the features shown and described or portions thereof, but it is recognized that various modifications are possible within the scope of the invention claimed. Thus, it should be understood that although the present invention has been specifically disclosed by preferred embodiments and optional features, modification and variation of the inventions embodied herein disclosed may be resorted to by those skilled in the art, and that such modifications and variations are considered to be within the scope of this invention.
[0107] The invention has been described broadly and generically herein. Each of the narrower species and subgeneric groupings falling within the generic disclosure also form part of the invention. This includes the generic description of the invention with a proviso or negative limitation removing any subject matter from the genus, regardless of whether or not the excised material is specifically recited herein.
[0108] Unless otherwise indicated, all technical and scientific terms used herein have the same meaning as commonly understood to one of ordinary skill in the art to which the invention belongs.
[0109] Other embodiments arc within the following claims and non-limiting examples.EXAMPLES
[0110] Non-limiting examples of the disclosure will be further described in greater detail by reference to specific Examples, which should not be construed as in any way limiting the scope of the disclosure.
[0111] Example 1 - Methods
[0112] Chemicals
[0113] All chemicals are analytical reagents without any further purification, including ammonium molybdate tetrahydrate ((NFLjeMovChi-dEhO), thioacetamide(CH3CSNH2), manganous (II) acetate tetrahydrate (Mn(CH3COO)2-4H2O), iron (II) acetate tetrahydrate (Fe(CH3COO)2-4H2O), cobalt (II) acetate tetrahydrate (Co(CH3COO)2-4H2O), nickel (II) acetate tetrahydrate (Ni(CH3COO)2-4H2O) and potassium hydroxide (KOH).[001 14] Synthesis of M1 / M0S2 catalysts
[0115] A series of MI / MOS2SASCS were prepared according to the designed synthetic protocol as follows. 176 mg (N[L)<,Mo.-O24-4I I2O («MO=1 mmol), a certain amount of metal salts (Mn(CH3COO)2-4H2O, Fe(CH3COO)2-4H2O, Co(CH3COO)2-4H2O and Ni(CH3COO)2-4H2O) and 750 mg CH3CSNH2(10.0 mmol) were dissolved in 70 ml distilled water. The solution containing precursors was then transferred into a Teflon-lined autoclave (100 ml). Subsequently, it was scaled and maintained at 180 °C for 20 h and then naturally cooled to room temperature. The resulting product was washed with distilled water and absolute ethanol for several times, and dried under vacuum at 60 °C for 12 h. Under the Ar flow of 100 seem, the dried product was heated to 400 °C at a rate of 10 °C min-1and kept there for 2 hours in a furance, then cooled down to room temperature. A series of M1 / M0S2 SASCs can be obtained using this approach by tuning the contents and types of metal salt precursors (nM:nMo max=20 at%).
[0116] Characterization[001 17] The catalysts were characterized by the X-ray diffraction (XRD, Ultima IV, X- ray diffractometer with Cu Ka), transmission electron microscopy (TEM, FEI Tecnai G2 F30, operating at 300 kV) with energy dispersive X-ray spectroscopy (EDS) equipment, inductively coupled plasma-mass spectroscopy (ICP-MS, Optima 5300DV), Raman spectroscopy (LabRAM HR Evolution Raman microscope, laser excitation at 532 nm) and scanning transmission electron microscopy (STEM) with EDS mapping being carried out at 80 kV using a JEOL ARM200F equipped with ASCOR aberration corrector (cold field emission gun, Gatan Quantum ER spectrometer and Oxford X-max TOOTLE SDD EDS). The STEM image simulation was done using the multislice algorithm.
[0118] The X-ray absorption fine structure (XAFS) including X-ray absorption near- edge structure (XANES) and extended X-ray absorption fine structure (EXAFS) spectra measurements of metal (Mn, Fe, Co, Ni) K-edge were carried out at the XAFCA beamline of the Singapore Synchrotron Light Source (SSLS)58. A Si (111) double-crystal monochromator w as applied to monochromatize the X-ray beam. Metal (Mn, Fe, Co, Ni) foils were used for the energy calibration, and all samples were measured undertransmission mode at room temperature. The EXAFS oscillations χ(k) were extracted and analyzed using the Demeter software package. XANES simulations, based on the DFT optimized structures, are performed using the finite difference method as implemented within the FDMNES package. The cluster diameter for all the simulations is 8 Å. Due to the finite mean-free path of the photoelectron and to the core-hole lifetime, broadening contributions were accounted for using an arctangent convolution.
[0119] The S K-edge absorption was obtained by recording fluorescence yield and selected by silicon draft detector (FAST SDD@ Ultra High Performance Silicon Drift Detector, Ametek), using in an ionization chamber at tender x-ray beamline BL16A1 at National Synchrotron Radiation Research Center (NSRRC), which is equipped with double crystal (Si (1110)) monochromater (DCM).
[0120] Electrochemical measurements
[0121] The OER measurments including cyclic voltammetry (CV) and linear sweep voltammetry (LSV) polarization curves were performed using a CHI 760D workstation (CH Instruments) with the counter electrode of graphite rod (diameter 5 mm, 99.999%) and the reference electrode of Hg / Hg2Cl2 (saturated KCl). The electrochemical impedance spectroscopy (EIS) was carried out in the frequency range of 0.01 Hz to 100000 Hz. All the potentials were calibrated to the reversible hydrogen electrode (RHE), ERHE= Eref+ 0.059pH + 0.241. Eref is the experimental potential measured against the Hg / Hg2Cl2 reference electrode, and 0.241 is the standard potential of Hg / Hg2Cl2 at 25 °C48,49.
[0122] Electrode fabrication
[0123] A piece of copper (Cu) foam was sonicated in acetone, ethanol and distilled water for several minutes, prior to the preparation of the electrode. 15 mg MoS2-based catalyst was added into a mixture of 0.90 mL of ethanol and 100 μL of Nafion (Dupont®, 5 wt%) with 1 h ultrasonic treatment. 100 μL of fresh catalyst ink was dropped onto a Cu foam (0.5×2 cm, catalysts are covered with 0.5 cm2, i.e., 0.5×1 cm), and dried at room temperature for 12 h. All tests were performed in 1.0 M KOH solution saturated with oxygen gas (O2). For comparison, 10 mg IrO2catalyst was added into a mixture of 0.90 mL of ethanol and 100 μL of Nafion with 1 h ultrasonic treatment.100 μL of fresh catalyst ink was dropped onto a Cu foam, and the loading of IrO2 on Cu foam is 1 mg cm-2. The samples were run 10 cycles to reach a steady state. The LSV measurements for MoS2and IrO2catalysts were recorded in O2-saturated electrolyte at a scan rate of 5 mV s-1. CV curves were recorded from 0.37 to 0.57 V vs. RHE with a scan rate of 10 mV s-1to 120 mV s-1tomeasure the electrochemical double-layer (Cdl) capacitance. The long-term stability was measured by chronoamperometric (CP) response under magnetic stirring. OER performances under different magnetic field were performed by tuning the distances between the electrode and magnets. Seawater was collected from Sentosa beach (Singapore), and filtrated by filter paper.
[0124] The Cu foil loaded with the catalyst (0.2 mg cm-2) acts as the work electrode (anode), and the Pt wire is the cathode.10 neodymium magnets (one magnet: 3 cm × 2 cm × 0.5 cm) were stacked and palced near the anode of water splitting cell. The magnetic field experienced by electrode was carefully calibrated using Gauss meter (TD8620, Shenzhen, China) (Fig.64). A large water splitting cell was constructed using the two 6 cm × 10 cm carbon papers loaded with Ni1 / MoS2(3 mg cm-2, 6 cm × 7 cm) and Pt / C (20 wt% Pt, 3 mg cm-2, 6 cm × 7 cm) as anode and cathode respectively. 100 neodymium magnets (3 cm × 2 cm × 0.5 cm) were compiled into a large magnet and placed near anode.
[0125] DFT calculations
[0126] The first-principle calculations were performed by using density functional theory (DFT) implement in the Vienna ab initio simulation package (VASP)50-52. The electron exchange and correction were calculated with the generalized gradient approximation (GGA) in the parametrization of Perdew-Burke-Ernzerhof (PBE)53pseudopotentials including Hubbard-U corrections (DFT+U formalism) based on Dudarev’s approach54. The projector augmented wave method with a plane-wave cutoff of 500 eV was used. The electronic states of 4d55s1, 3s23p4, 3p63d84s2, 2p22p4, 1s1were treated as valence states for Mo, S, Ni, O and H atoms, respectively. According to the experimental Ni loading concentration, the 4 × 4 × 1 supercell of MoS2 with one Mo atom replaced by Ni atom was used to simulate the doping effect. A vacuum slab of 16 Å is added to avoid the interlayer interaction. The structures were relaxed with 2 × 2 × 1 Gamma-centered k-points mesh for the supercell, and the electronic self-consistent calculations were performed using the 5 × 5 × 1 k-points mesh. The relaxation is considered to be converged if the Hellmann-Feynman forced is less than 0.01 eV / Å, and the energy convergence is set as 10-7eV for all calculations with a Gaussian smearing of 0.05 eV. The gas-phase O2and H2O were performed in a cubic box with the lattice constant of 15 Å using a single gamma k-point. To consider the strong electron correlation effect, a Ueff = 2.5 eV was assigned to 3d electrons for Ni atoms55,56.
[0127] The charge transfer was analyzed by the Bader charge with grid of 384 × 384 × 48057. The differential electron density (DED) was also implemented to analyze the charge transfers during adsorption process. The DED was attained by formula: ∆ρ = ^^ − ^^ − ^^ where ^^^^ ^^represents chargedensity of the whole system after absorption, ^^^^and ^^^^represent charge densities of adsorded species and catalyst, respectively.
[0128] Data availability
[0129] Source data are provided with this paper. Any additional material is available from the corresponding authors upon reasonable request.
[0130] DFT calculations: To obtain the energy profile for the whole catalytic process, the Gibbs energy was calculated for each catalytic step by formula: ∆G = ∆E + ∆ZPE − T∆S^^Where ΔE is the DFT calculated energy difference between isolated reactants, catalyst and the final products, ΔZPE means the zero-point energy correction contributed by the quantum vibration, and ΔS is the vibrational contribution to the entropy at finite temperature. For entropy ΔS, the expwhere R is the ideal gas constant, R=8.314 J / (mol*K), is the speed of light, ℎ is the Planck constant, ^^ is the vibration frequencies calculated by DFT.
[0131] For the OER r en in the following ways59.where * refers to the active site in the surface of Ni1 / MoS2.
[0132] The Gibbs energy changes for the water oxidation were calculated using the following equations:where U is the potential measured against normal electrode (NHE) at T = 298.15 K, P = 1 bar, and a value of U = 1.23 eV is used in our calculation. The free energy change of protons at non-zero pH is represented by Nernst equation as ∆ ^^^^ ^^= − ^^^^^^ × ^^ ^^ × ^^ ^^(10)60, the reaction occurs in alkaline solution, KOH, where pH = 14. And the ZPE and entropy correction are listed in Table 10.
[0133] In order to compare the catalysis performance of IrO2 and Ni1 / MoS2 in the seawater, an implicit solvation was used for correction of chloride ions on the surface of catalyst61,62. The adsorption energy is calculated by:∆E = ^^^^ ^^− ^^^^− ^^^^where ^^ ^^ ^^, ^^ ^^, ^^ ^^ refer to total energy of the systems, catalyst and adsorptions, respectively.
[0134] Example 2 – Results
[0135] Rational Design and Synthesis
[0136] To tackle these challenges, a general and scalable method was devised for the synthesis of a series of single-atom spin catalysts (SASCs) consisting of substitutional magnetic atoms embedded in the MoS2host. M1 / MoS2SASCs with tunable metal content were synthesized via a well-designed hydrothermal approach by introducing different molecular precursors including metal salts (M2+), ammonium molybdate tetrahydrate and thioacetamide in one step (see the experimental section), distinct from the chemical vapor deposition growth of single-atom doped MoS2 monolayer and the two-step hydrothermal methods25-29. Particularly, the decomposition of thioacetamide during hydrothermal reaction not only provides S sources for the formation of 2H-phase MoS2host but also creates the desired “operando acidic environment” to facilitate the synthesis of atomically dispersed single atoms embedded into the carrier lattice (Fig. 1a) by suppressing the formation of metallic nanoparticles. The generation of operando acidic environment during synthesis and its related chemical reactions are further illustrated in the Fig.1227-29. As a result, such a general synthetic protocol allows for the scalable synthesis of various M1 / M0S2 SASCs (Mi=Mn, Fe, Ni, Co) with widely tunable atomic doping ratio (M1 / M0) up to -20:100 (Table 1). Generally, high doping density shortens the averaged spacing between adjacent magnetic dopant sites to promote their magnetic exchange interaction into long-range magnetic order (Fig. la). Atomic dispersion of single magnetic dopants in M0S2 with different loadings can be confirmed using different characterization techniques including X-ray absorption fine- structure spectroscopy (XAFS), X-ray diffraction (XRD) analysis, Raman spectra and electron microscopy imaging (Fig. Ib-f, Fig. 6a-c and Fig. 13-18).
[0137] As shown in Fig. 12, molecular precursors including metal salts (M2+), ammonium molybdate tctrahydratc and thioacctamidc were introduced in this one -pot synthesis. The thioacetamide precursor used here plays a remarkable role, namely “killing two birds with one stone”. Firstly, the decomposition of thioacetamide during hydrothermal reaction not only provides S sources for the formation of 2H-phase M0S2 host but also creates the desired acidic environment (Equation 1-4) to facilitate the synthesis of atomically dispersed single atoms embedded into the carrier lattice by suppressing the formation of metallic nanoparticle. Such a process can be described by the chemical equations 1-4 bellow. The key innovation in creating operando acidic conditions enables us to incorporate a high density of substitutional magnetic single-atom doping beyond the regime that has not been accessed by other hydrothermal synthesis methods. A high density of magnetic dopant favours the long-range magnetic coupling, crucial for realizing the ferromagnetic ordering observed in Ni 1 / M0S2.
[0138] Table 1. Metal contents in M0S2 host determined by EDS and ICP-MS analysis.( The scatte g c oss sect o ( ) o t e age ca be desc bed us g t e ollowing equation, according to STEM imaging theory78:15 ^^ ^^ ^17 4^ ^^ where ^^ is a constant, ^^ is the atomic number and ^^ is the electron wavelength. Considering the thickness ( ^^) and the atomic number per unit volume ( ^^), the obtained electron beam intensity (IS) of atomic element can be described as: IS=^^∙^^ ^^ ^^ where I refers to th i t it f i id t l t bTherefore, I1S(Ni):IS(Mo) =^^ .7(Ni):^^1.7(Mo). The values of^^1.7(M):^^1.7(Mo) and the ratios of electron beam intensity for M:Mo from STEM images have been compared as shand the values of IM / IMoare in good agreement with predicted ratioof^^1.7 17M:^^ .Mo.
[0139] The detailed structural characterization of Ni1 / MoS2 SASCs with ferromagnetism was first presented, in contrast to other paramagnetic M1 / MoS2SASCs. XAFS and high-angle annular dark-field scanning transmission electron microscopy (HAADF-STEM) imaging were used to further elucidate the coordination environment of M atoms in M1 / MoS2(Fig. 14. Table 2)30. HAADF-STEM image resolves a characteristic triangular lattice of Ni1 / MoS2consisting of brighter and darker sites (red circled in Fig.1g, Fig.19), which can be assigned to Mo and Ni atomic sites, respectively. A zoom-in HAADF-STEM image (Fig. 1h and Fig. 6d) further unveils that single Ni atom (marked by red circle) substitutes Mo atom (denoted as NiMo), consistent with the contrast observed in the simulated HAADF-STEM image of DFT-optimized NiMo structure (Fig.1i). In addition, Ni K-edge Fourier transformed extended X-ray absorption fine structure (EXAFS) spectrum of Ni1 / MoS2reveals an absence of any feature associated with Ni−Ni and Ni−O bond but a prominent feature peaked at 1.779 Å31,32, similar to that of commercial NiS2, which can be associated with the Ni−S bonding (Fig.Id). Ni-S bond length and local coordination number of NIMO were determined to be 2.27 + 0.02A and 4.3 ± 0.2 via a detailed EXAFS fitting (Table 3). Among all the proposed structures, DFT-relaxed Ni\i„ consisting of Ni in the replacement of Mo coordinated with adjacent four S atoms (denoted as NiS4) in a non-ccntrosymmctric octahedral configuration shows the best agreement between experimental X-ray absorption near- edge structure (XANES) and simulated spectrum (Fig. le, Fig. 6e, 61f and Fig. 20). Unlike Nii / MoS2, other substitutional dopants in M1 / M0S2 (M = Mn, Fe and Co) are coordinated with six adjacent S atoms to form the trigonal prismatic MSe configuration (Fig. lb, 1c, Fig. 21-25, Table 3, 4). The distinct coordination environment of Ni atom in Nii / MoS2 is also evidenced by the presence of a new feature at 6 eV above the absorption edge energy (Eo) in Ni K-edge XANES as compared to M1 / M0S2 (M = Mn, Fe and Co) (Fig. 26). Individual NiS4 site in M0S2 contains four Ni-S bonds, wherein the shortest Ni-S bond length is 2.285 A, which is further supported by a comparison of the calculated formation energies of various single-metal doped M0S2 (Fig. 27). The in-plane displacement of Ni dopant breaks the rotation symmetry in the trigonal prismatic configuration (D311) to form single Nixio site with non-centrosymmetric distorted tetragonal structure (C2v), leading to the increasing strength of crystal field and reduced level degeneracy (Fig. 2f, Fig. 7d, Fig. 28). Such a local bonding configuration of Nixio site yields a valence state of NiyioQH), as evidenced by characteristic adsorption edge in soft XAS (Fig. 29).
[0140] Analysis showed that the oscillation patterns of the K-edge XANES for substitutional single metal atoms (M), including Mn, Fe, or Co, were almost identical to those of Mo for the corresponding M1 / M0S2SASCS. Notably, the Ni K-edge XANES of the Nii / MoS2 sample exhibited an additional feature approximately 10 eV above the absorption threshold Eo, as compared to its Mo counterpart, while the remaining feature peaks correlated closely (Fig. 24). This finding suggests that although Ni is doped into the M0S2 crystal, it does not replace Mo exactly at the center of the trigonal prism of S atoms, unlike Mn, Fe, and Co. In combination with our previous XANES calculations, it is possible to conclude that the substitutional Ni dopants in place of Mo in M0S2 arc positioned closer to the four S atoms forming one face of the S6 trigonal prism, ultimately resulting in a geometric configuration akin to the NiS4 square planar or, more specifically, the N1S4 triangular pyramid. This result is in good agreement with the simulation of M K-edge XANES and fitting FT-EXAFS spectra (Fig.6, Fig. 22).[00141 J As shown in Fig. 25, in the M K-edge FT-EXAFS spectra of all the M1 / M0S2 (M=Mn, Fe, Co, Ni) S ASCs, a single prominent peak corresponding to the M-S bond can be clearly observed (Fig. 25). The Ni-S bond is found to be shorter (by approximately 0.02 A) than the M-S bond observed for other substitutional single metal dopants (M = Mn, Fe, Co), which is consistent with the results of the EXAFS fitting analysis (Table 3).
[0142] As shown in Fig. 26, there are two peaks located at about 0 and 17 eV for all XANES spectra, while there is one more additional peak located at around 6 eV only in XANES of Nii / MoS2, indicating the local structure of Ni in Nii / MoS2 is different from those of other M1 / M0S2 (M=Mn, Fe, Co) samples. It is also worth mentioning that the EXAFS fitting results reveal that the bond length for Ni-S (2.27 A) is shorter than those of M-S (Mn-S: 2.30 A, Fe-S: 2.29A, Co-S: 2.29A), and coordinate number for Ni-S (4.3) is much smaller than those of M-S (Mn-S: 6.0, Fe-S: 6.1, Co-S: 5.9). All these observations support that Ni atom bonds with four S atoms to form Ni-S4 non- centro symmetric octahedral configuration, as evidenced in Fig. 22. Unlike Ni 1 / M0S2, the coordination environments of metal dopant in these M1 / M0S2 (M=Mn, Fe, Co) samples are rather similar'. These dopant atoms also replace the Mo position but they adopt a trigonometry configuration of the M-Sr> structure. In addition, the simulated XANES spectra with simulated factors (Table 3) are in well accordance with the experimental data, which further prove the validity of proposed models of M1 / M0S2 (M = Mn, Fe, Co and Ni).
[0143] As shown in Fig. 27, the total energies of M1 / M0S2 (M = Mn, Fe and Co) increase with the increasing displacement along the diagonal direction, suggesting that the Mn, Fe and Co atoms energetically prefer to coordinate with six S atoms. In contrast, the energy of Nii / MoS2 exhibits a maximum value around the Ni displacement of 0.28 A and then decreases, which reveals that the partial tetra-coordinated Ni i / MoS? is a metastable state, consistent with experimental observation.
[0144] As shown in Fig. 28, due to the D311 symmetry of six coordinated Nii / MoS2, the d orbital of Ni atoms is split into A(dz2), Ei(dxy,dx2-y2), E2(dxz,dyz) states, where the electrons are mainly located at the spin-up states of Ei and E2 states, resulting in the robust magnetism. However, the symmetry of four coordinated Nii / MoS2 reduces to Ci due to the Jahn-Teller distortion, and the d states will be divided into five states (dxz, dyz, dxy, dx2-y2and dz2) without spin splitting, leading to non-magnetism13. The symmetry of partial four coordinated Nii / MoS2 in our experimental data lies in between the four andsix coordinated Ni1 / MoS2, and thus the magnetism of partial four coordinated Ni1 / MoS2is stronger than four coordinated Ni1 / MoS2 and weaker than six coordinated Ni1 / MoS2.
[0145] Table 2. The experimental and theoretical value of electron beam intensity ratio of M1 / Mo for all M1 / MoS2 SASCs.Note: IM is the electron beam intensity of metals in M1 / MoS2 from HR-STEM images, and^^Mis the atomic number of metals. The values of IM / IMoare well in accordance with values of^^1.7M:^^1.7Mo.[ S M F CNi1 / MoS2 . . . . . . 0.83 . 0.013 Ni–Mo 2.2 ± 0.3 3.11 ± 0.02 8.4 ± 1.4 -5.31 Note: N is coordination number, R is interatomic distance (the bond length between the central atom and surrounding coordination atoms), σ2is the Debye-Waller factor, ∆E0is edge-energy shift, R-factor is used to value the goodness of the fitting. S02is the amplitude reduction factor. The S02used in the Fe, Co and Ni K-edge EXAFS fittings are obtained from the fitting of their metal foil EXAFSs The S02used in the Mn K-ed e EXAFS fitting is obtained from th
[0147] Table 4.Co1 / MoS2Co–S 6 2.295
[0148] Magnetic Property and OER Performance
[0149] NIMO(III) with a Civ symmetry is expected to yield unpaired 3d. electron, leading to the formation of local magnetic moment around Nixie site and potentially creating long-range magnetic order in Nii / MoSi at increased doping density. To verify this, both Electron Spin Resonance (ESR) spectra and Superconducting Quantum Interference Device (SQUID) measurements were performed to probe the magnetism of Nii / MoSi sample with different metal loadings (Fig. 2). First, Nii / MoSi with the lowest Ni content of 0.05 wt% only reveals the paramagnetism without long-range magnetic ordering (Fig. 2b). In contrast, ferromagnetism emerges in Ni i / MoS; samples with increased Ni loading of 0.20, 0.38, 0.95, 1.42, 2.41, 3.12 and 4.20 wt%, whose saturated magnetization and coercivity increase monotonically as a function of Ni contents (Fig. 2a-c), similar to TMD materials doped by other metals33-36. Detailed characterizations of ferromagnetic properties of one representative Ni i / MoS? with a metal loading of 3.12 wt% was then conducted. Temperature-dependent ESR spectra of this Nii / MoS2 acquired from 2 K to 300 K (Fig. 2d, Fig. 30) reveal a characteristic line- shape feature at the magnetic field of -335 mT, consistent with the expected absorption behavior of Ni(III) (Fig. 30)37,38. In addition, the linewidth of the ESR signal of Nii / MoSz (Fig. 7a), defined as the peak-to-peak distance decreases as a function of temperature, indicating the emergence of ferromagnetic order39,40. The ferromagnetism of Nii / MoS2 is also reflected in the field-dependent magnetization measurements (M-H) acquired from 50 to 300 K (Fig. 2e, Fig. 31), revealing a clear hysteresis loop and a saturation magnetic field of -5000 Oc. Unlike Nii / MoS2, pure M0S2 and other M1 / M0S2 (M = Mn, Fc and Co) show the paramagnetism at room temperature (Fig. 32, 33). All these observations confirm that a high doping density of Ni atoms leads to ferromagnetism in Nit / MoSi, which may boost its OER performance under external magnetic field (B -field).
[0150] B-field dependent OER performance of ferromagnetic Nii / MoS2 samples was then evaluated by performing linear scan voltammogram (LSV) and chronoamperometric response (CP) measurements in 1 M KOH. It is noted that the current density (overpotential at 20 mA cm-2) increases (decreases) from 3.52 to 64.19 mA cm-2at 1.6 V vs. RHE (from 465 to 174 mV) as B-field increases from zero to 502 mT (Fig. 3a). The enhanced OER performance can be directly visualized from more rigorous oxygen gasbubbling over the N11 / M0S2 electrode under B-field (Inset of Fig. 3a, Fig. 34). At 502 mT, OER current densities can be improved by 5 to 28 times at 1.7 and 1.55 V vs. RHE, respectively (Fig. 3b). The B-field enhanced current density and Tafel slope reaches a plateau above 502 mT, consistent with the saturation magnetic field determined from the M-H curve. In addition, overpotentials at 40 mA cm-2decreases from 547 to 283 mV, and Tafel slopes also gradually decrease from 75 to 44 mV dec-1upon the increase of B-field from 0 to 502 mT (Fig. 8a, Fig. 35). A small reduction of overpotential can generate a rapid increase of the OER current density41 ,42. It is noted that the electrochemically active surface area (ECSA) shows a negligible change under B-ficld. All these results indicate that the giant MFE of the OER activity of Ni 1 / M0S2 results from the ferromagnetic spin alignment under mild B-ficld (Fig. 2e, Fig. 36, 37).
[0151] As shown in Fig. 35, OER process over N11 / M0S2 catalyst:M and * represent the Nii / MoSz catalyst and catalytic OER site over Nii / MoSa, respectively.
[0152] As shown in Fig. 36, the electrochemical specific surface area of Nii / MoS2 (14:100) is larger than that of pure M0S2, indicating that Ni dopant increases the exposed surface area of M0S2 in electrolyte. Simultaneously, the ECSA of Nii / MoSz under 502 mT shows negligible difference compared to that measured without magnetic field, indicating the number of active sites for OER remains unchanged.
[0153] Next, systematic experimental studies were carried out to probe the origin of the B-field enhanced OER activity. First, it was found that OER current density after removing B-field does not immediately return its initial value with respect to Ni 1 / M0S2 under zero field (Fig. 8d, 8f). The retention ratio of current density between B-field off and on gradually decreases from 92% to 54% at 1.6 V vs. RHE, when the applied B-field increases from 118 to 502 mT (Fig. 38). In addition, OER activity also undergoes a slow decay and returns the initial status 4 hours after switching off the B-field (Fig. 8e). Such a behavior in the evolution of OER activity between B-ficld on and off is presumably associated with the rotation of ferromagnetic domains, in accordance with the characteristics of the ferromagnetic alignment and relaxation between B-field on and off.The ferromagnetic domains tend to align with magnetic field but it usually doesn’t immediately return to the original randomized magnetization state, and retain some of the net magnetization due to the intrinsic spin exchange interactions after switching off B- field43-45. In addition, it was also found that N11 / M0S2 with a Ni content lower than 0.20 wt% exhibits a negligible MFE of OER (Fig. 8c), presumably due to its low density of ferromagnetic domains. In addition, as-synthesized Mn, Co and Fe doped M0S2 with paramagnetic behavior also show the independence of OER performance on B -field (Fig. 39). Furthermore, the conductivity of both C01 / M0S2 and undoped M0S2 can be improved upon the application of B -field but their OER current densities remain nearly unchanged, ruling out the role of improved conductivity in MFE of OER activity (Fig. 8b, Fig. 40). Although the ion transfer rate can be improved under magnetic field, the intrinsic OER activity of catalyst is largely determined by its electronic structure of active sites11,19. Therefore, all these results point out that the ferromagnetic spin alignment can be attributed to the B-field enhanced OER activity over Nii / MoS2 regardless of the orientation of magnetic field (Fig. 3a, Fig. 40-44).
[0154] The metallic character and non-integer magnetic moments suggest that the Stoner itinerant model should be used to understand the ferromagnetism of Ni doped M0S2, rather than the localized Heisenberg model. According to Stoner theory75,76, the ferromagnetic order will be adopted if the criterion (I X D(EF) > 1) is satisfied. I is Stoner parameter, and D(EF) is the density of states at Fermi level (EF). I can be obtained by relationship (efc) = 1 X Mavg77, where (cfc) refers to average exchange splitting energy between bands of spin up and spin down around Fermi level (EF), and refers to average magnetic moment of Ni atoms. It is evaluated {ek) = 0.218 eV, and Mavg= 0.156 / A.Bfor each Ni atom, then 1 = 1.397 cV / gBis obtained. Fig. 37b shows that the D(EF) = 2.208 states / (eV x Ni x spin). Therefore, 1 x D(EF) = 3.086 > 1. Stoner’s criterion is satisfied, indicating that Ni doped M0S2 can be classified as a Stoner-type itinerant ferromagnetic material.
[0155] For Fig. 38, all OER curves with / without external magnetic fields are obtained at the stable state (after running CV tests). It is noted that the current is nearly zero at potential lower than < 1.2 V vs. RHE. The current in the low potential range (non-OER region) is subtracted.
[0156] Mechanistic insights into giant MFE for Nii / MoS2
[0157] DFT calculations were then performed to gain atomic-level understanding of the origin of ferromagnetism in Ni1 / MoS2 and its B-field enhancement of OER performance. First, spin-polarized DFT calculations reveal the presence of unpaired Ni 3d electron over NiMoand induced ferromagnetic spin polarization over nearby Mo and S atoms, yielding a net spin of ~ 1.610 µB for NiMoand its surrounding S and Mo atoms (defined as NiMo-S-Mo region, Fig.4a, Fig. 45, 46). The ferromagnetic ground state of NiMo-S-Mo arises from the spin exchange interactions of the itinerant electron in the region, which can be described from the Stoner criteria (Fig. 47-49, Table 5, 6). According to the ratio of Ni:Mo for ferromagentic Ni1 / MoS2, a supercell of Ni2Mo14S32 was further constructed to calculate the magnetic ground states of two adjacent NiMo sites. Among all the possible configurations with different Ni-Ni seperation distances (Fig.46, Table 7), the one with Ni-Ni distance of ~6.390 Å represents the most stable configuration due to its lowest formation energy. Importantly, the DFT calculations reveal that the ferromagnetic (FM) coupling between these two NiMosites is favorable by 30.67 meV per Ni atom over the anti-ferromagnetic (AFM) coupling (Fig. 4b, 4c), consistent with the RT ferromangetism observed in experiment. The ferromagnetic ground state of Ni1 / MoS2is further reflected in the density of states (DOS) plot of NiMo-S-Mo region that shows an asymmetric distribution of spin-up and spin-down electron densities near the Fermi level (EF) (Fig.4d). Specifically, spin-polarized states near EF are mainly from the 3dxz / dyz orbitals of Ni dopant, 3px / py orbitals of six nearest-neighboring S atoms, and 4dz2 orbitals of six nearest-neighboring Mo atoms as revealed in the projected density of states (PDOS) in Fig.4d. The electron localized function (ELF) plot of Ni1 / MoS2 demonstrates that the Ni dopants increase electron delocalization involving a large charge transfer with the surrounding S atoms, as further reflected from the Bader charge analysis (Fig. 7e, Table 8). In order to accommodate the transfer electron of Ni with a specific direction of spin polarization, the highest half-filled px / py orbitals of S atoms will be occupied by two parallel spin polarized electrons due to the Hund rules, where the direction of spin polarization is opposite to that of the tranferred electrons. As a result, the direction of m i i h i i l i M i li ih i Fi . 50
[00158] Table 5. Detailed values of Ni1 / MoS2materials according to the Stoner theory. Ni:Mo (eV / atom)Note: Detailed values of Ni 1 / M0S2 with different Ni:Mo ratios are obtained from Fig. 48.
[0159] As shown in Fig. 48. the electronic states near fermi energy contributed by Ni atoms of Nii / MoSj still exhibit the metallic feature when the content of Ni dopant decreases, which suggests that the Stoner criterion can be also applied to the Nii / MoSz materials with different ratios of Ni:Mo. The calculated Stoner parameter I presents a slight increase with increasing Ni contents shown in Table 5. By contrast, the electronic density at fermi energy D(EF) increases with increasing Ni content at a lower doping level. It is noted that the magnetic property of Nii / MoS2 is closely related to the ratios of Ni:Mo. The magnetism of Nii / MoS2 changes from paramagnetism to ferromagnetism when the ratio of Ni:Mo is 1:19. Based on DFT results, a single Ni dopant plays a critic role in tuning the magnetic property of M0S2.
[0160] As shown in Fig. 50, the higher degree of overlapping in PDOS at certain energy window between Ni and S2 atoms indicates the stronger bonding interaction between Ni and S2 compared to the Ni and Si, resulting in more electron transfer between Ni and S2 atoms. To receive the transferred electrons with the specific spin component, the spin direction of the electrons occupying at px / py orbitals of S atoms will align to the antiparallel direction. As a result, the S atoms are magnetized. The more electrons transfer to S atoms, the smaller net magnetic moments over S atoms, which is consistent with the calculated results shown in Fig. 4b. The more electrons at Fermi level of Si suggests that Si atoms possess higher OER activity than that of S2 atoms.
[0161] Table 6. Detailed values of M1 / M0S2 according to the Stoner theory.The similar bands of different spin states near fermi energy (E 1 ) are used to calculate < >. M1 / M0S2 (M = Mn, Fe and Co) are the paramagnetic materials according to the Stoner theory.
[0162] Table 7. DFT calculated energies of five configurations.Note: The configurations of Ni i / MoS? materials are shown in Fig. 46.
[0163] Table 8. Average Bader charge of atoms in single Ni atom doped M0S2.Note: Moi: Mo atoms nearby Ni atoms, M02: Mo atoms far away from Ni atoms, Si: the second nearest S atoms to Ni atoms, S2: the nearest S atoms to Ni atoms, S3: S atoms far away from Ni atoms (Fig. 45).
[0164] The key question that remains to be addressed lies in mechanistic insights into remarkable MFE of OER performance of Nii / MoS2. DFT calculations were first used to identify the active site of individual NiMo site for OER. To facilitate the discussion, three types of nearest S atoms to individual Nivio site were labelled as Si, S2, S3, which represents adjacent S atom with a Ni-S bond length of 2.521 A, adjacent S atom with a Ni-S bond length of 2.285 A, and nearby S atom located at the center of Mo prism, respectively (Fig. 5a). The adsorption of *OH over Si is energetically favorable by 0.475 eV, 0.715 eV, 1.703 eV, 1.809 eV compared to that over S2, S3, Ni and nearest Mo site, respectively. This suggests that Si site is the most favorable active site for OER, mainly due to the strong electronic interaction between Si and the *OH (Fig. 5a, Fig. 51, Table 9), as evidenced by the large electron difference density, the dominant electron states atEF and the largest localized potential of Si among all three types of S atoms (Fig. 5b, Fig. 52). As a result, more charge transfer to the *OH facilitates the occurrence of the first step of OER process (Fig. 5b), which can greatly improve the intrinsic activity of OER over S atoms.
[0165] As shown in Fig. 52, Ni atoms possess a lower localized potential than that of Mo atoms, which indicates a stronger electron affinity of Ni. Si possesses the lowest electron affinity among three types of S, indicating that Si in Nii / MoS: represents the most active site for OER.
[0166] Table 9. DFT calculated energy of *OH adsorption at different site.— : no data.
[0167] An increase of B field increases total magnetic polarization and the density of aligned magnetic moments from neighboring NiMo sites. To mimic this picture, the OER energy profiles over two neighboring NiMo sites were calculated under two representative magnetic configurations including ferromagnetic (FM) and antiferromagnetic (AFM) ordering (Fig. 5d, Fig. 9a). FM-coupled active site exhibits a lower energy barrier of 0.315 eV in the rate-limiting step of OER (from *OOH to O2 process), compared to AFM- coupled active sites with a higher energy barrier of 0.387 eV (Fig. 5d). As shown in Fig. 5c, the near-Er occupied spin density of Si of two FM-coupled Nixio sites is significantly reduced but the empty state above EF increases, as compared to that of AFM-coupled counterparts. Therefore, the reduction of energy barrier in FM configuration can be attributed to the optimization of spin density over S active sites upon spin alignment under mild magnetic field, which give rises to the optimal adsorption energy for radical intermediate with reduced reaction barrier. Meanwhile, it is also found that the spin density of *OH and:'O species exhibits the parallel alignment over Si and S2 sites in the FM configuration, but shows the antiparallcl spin ahgnmcnt in the AFM configuration(Fig. 5d, inset). Therefore, the desorption of *OH and *0 to form spin-triplet state O2 over FM coupled N1S4 sites is energetically more favorable by 0.072 eV than that on the AFM coupled sites, leading to a lower energy barrier of O2 formation. It is noted that current OER reaction profile is the one with the lowest barrier as compared with other reaction paths (Fig. 53, 54, Table 10). Tn addition, another OER pathway involving the formation of a bridge-type O-H-O intermediate was also considered and the corresponding OER energy profile was evaluated (Fig. 9a). The FM-coupled configuration showed a superior OER activity with an energy barrier of 0.418 eV in the rate-limiting step of *OOH to O2, lower than that of AFM-couplcd configuration (0.668 eV). Similarly, two O atoms in *OOH species show the parallel spin alignment over FM- couplcd active sites, whereas anti-parallel spin alignment of *OOH over AFM coupled active sites doesn’t favor the *OOH desorption (Fig. 9b, 9c). The theoretical insights discussed above are further supported by the operando XANES spectroscopic measurements during OER reactions with and without B -field (Fig. 5e-g, Fig. 10 and Fig. 55). The rising edge of S K-edge for N11 / M0S2 shows a higher red shift at 1.8 V vs. RHE under 112 mT than zero-magnetic field (Fig. 5e, 5f, Fig. 56, 57), which indicates that S atom at the basal plane serves as catalytic site with the accumulation of more electron density under magnetic field that facilitates the electron transfer from O* -related species to the active site during OER. Tn addition, a pre-edge feature around 2469.2 eV emerges in the first derivative curve of S K-edge XAS spectra acquired at 1 T2 mT (Fig. 5g). This indicates that electronic hybridization between S 3p and Ni 3d electron orbitals becomes stronger under B-field, consistent with a larger overlap between the calculated PDOS for Ni and S under the FM-coupled configuration as compared to the AFM-couplcd one (Fig. 10). A strong Ni-S hybridization will modulate the spin density over S site, whereby the adsorption strength of O*-related intermediate species can be further optimized to facilitate the O2 formation, consistent with DFT calculations as discussed above (Fig. 5d, Table 11).[00168J As shown in Fig. 53, the energy barriers of *O to *OOH over Si site are determined to be 1.535 eV and 1.624 eV for the FM-and AFM-coupled active sites, respectively. This result suggests that the chemial adsorption of *OOH over Si sites is rather inert for OER in this path.
[0169] As shown in Fig. 56, there is a slight white line intensity increase for S K-edge under magnetic field (1 12 mT). The rising edge of S K-edge under magnetic field (1 12mT) also shows a blue shift comparing to that under zero field. The above result is further revealed by the corresponding first derivative curves. Such an observation indicates that S site possesses more empty states under magnetic field, thus facilitating more electron transfer / accumulation on S atom during OER when external magnetic field is applied. As well known, two H2O molecules lose four electrons in order to form one O2 molecule. Electrons transfer process occurs between the catalytic site and related O species during OER. Therefore, the catalytic S site acquires electrons from the related O species during reaction over N11 / M0S2 material, leading to more electrons accumulated on S site. Therefore, S K-cdgc XAS spectra exhibit a gradual negative shift with increasing applied potential during OER (Fig. 5e), which again reflects the dopant effect from single Ni site.
[0170] Table 10. DFT calculated energy correction for OER reaction.
[0171] Table 11. DFT calculated values of Si and S2 at magnetic order of FM and AFM.n(Ep) refers to the electronic concentration at the Fermi energy level.
[0172] MFE for water splitting using Nii / MoS2
[0173] After gaining new insights into the mechanism of MFE of OER performance of Nii / MoSz, its technological relevance was also tested by evaluating B-field dependent electrocatalytic performance in both water and seawater splitting cells. Nii / MoS2 (3.12 wt%) also presents an outstanding OER performance under B-field for water splitting, much superior to commercial IrO2 (Fig. 3c, Fig. 58). The current density of N11 / M0S2 at 502 mT is determined to be ~ 5.2- 11.7 times higher than that under zero- B field in the potential range of 1.5-1.8 V. Moreover, N11 / M0S2 at 502 mT also presents a high stability with a minor current density drop from 39.8 to 38.4 mA cm'2within 25 h, in contrast to commercial IrO2 catalyst with a large current density decrease from 17.8 to 8.7 mA cm-2within the same period (Fig. 3d). In addition, Nii / MoS2 (3.12 wt%) also reveals a remarkably improved OER performance at 502 mT for seawater splitting, much better than commercial I1O2 in terms of current density in a wide potential range of 1.5- 1.8 V (Fig. 3e, Fig. 59). Seawater splitting is recognized as a more economically - vital water splitting technology. However, the catalyst instability due to the presence of a variety of components in seawater, especially chloride ions46,47, poses a great challenge for the practical utilization of seawater in water splitting technology. Commercial lr()2catalyst shows a rapid decay and drops in current density by 19.2 mA cm2within 25 h. In contrast, Nii / MoS2 demonstrates a negligible decrease in current density by 2.3 mA cm'2within the same period, revealing an excellent OER stability in seawater. This is likely due to a high tolerance of Nii / MoS2 to the Cl adsorption against the catalyst deactivation (Fig. 3f, Fig. 60, 61, Table 12), corroborated by our DFTcalculations (Fig. 62, 63). A large cell with an electrode (6 cm x 7 cm) loading Ni 1 / M0S2 exhibits a promising application in water splitting technology (Fig. 11).
[0174] As shown in Fig. 61, additional characterization of N11 / M0S2 (14:100) catalysts was performed before and after reactions using a series of techniques including XPS, Raman, TEM, XRD and TCP analysis. Specifically, TEM measurement reveals the same lattice structure of 2H M0S2 without the formation of new phase of material or any particle after reactions. This is consistent with XRD measurement that only reveals the diffraction peaks contributed by 2H MoS2- In addition, ICP analysis of catalyst samples before and after reactions also shows negligible variation, indicating a superior stability of Nii / MoS2 catalysts under reaction conditions.
[0175] As shown in Fig. 62, total energies for the three relaxed structures of Cl" adsorption over IrCh, i.e., Ir top site, bright site and O top site, are shown in Fig. 62. The Ir top site possesses the lowest energy of Cl" adsorption, suggesting that the Ir top site is the active site for Cl" adsorption. Similarly, Si atoms have the lowest energy of Cl" adsorption, also suggesting that Si atoms are the active sites for Cl" adsorption.
[0176] As shown in Fig. 63, The Ir top site in IrCh shows a 1.641 eV barrier of Cl" adsorption, much lower than that of 3.642 eV over Si atoms in N11 / M0S2, which indicates that the chemical adsorption of Cl" over IrCh is more likely than that of Nii / MoS2. Therefore, Nii / MoSz possesses an excellent tolerance to chloride ion using seawater as electrolyte, thus exhibiting an excellent OER stability, much better than that of the commercial IrCE
[0177] Table 12. Concentration of elements in the solution.— : not detected in the solution.The solution is obtained from seawater, alkaline seawater, and alkaline seawater after water-splitting test at a potential of 1.6 V for 25 hours (ICP-MS results).
[0178] Example 3 - Conclusions
[0179] In summary, a general and scalable approach for the synthesis of a series of SASCs (M1 / M0S2) with widely tunable loadings have been demonstrated. High-loading Nii / MoSi also exhibits the room-temperature ferromagnetism arising from the ferromagnetic coupling between adjacent NiS4 sites embedded in M0S2 lattice, offering a giant MFE of OER activity. In the water splitting cells, N11 / M0S2 delivers an excellent catalytic performance with a large current density under magnetic field up to 502 mT, approximately one order of magnitude higher than that without applying magnetic field in 1.5-1.8 V, outperforming the commercial IrCh catalyst. A large B-ficld enhancement of OER performance of Nii / MoS2 is attributed to their weakly coupled spin centers and the optimization of spin density over S active sites arising from ficld-rcgulatcd Ni-S electronic hybridization, which yields the optimal adsorption / desorption energy for radical intermediate with reduced reaction barrier, as corroborated by the operando characterizations and DFT calculations. In addition, the stability of Nii / MoS2 as OER catalyst is also superior to that of IrO2 in pure water and seawater splitting cell, demonstrating its great potential in practical seawater splitting technology. The findings reveal that ferromagnetic SASCs provide a powerful magnetoelectric effect to accelerate both water and saline water electrolysis.
[0180] Industrial Applicability
[0181] It will be apparent that various other modifications and adaptations of the invention will be apparent to the person skilled in the art after reading the foregoing disclosure without departing from the spirit and scope of the invention and it is intended that all such modifications and adaptations come within the scope of the appended claims.
[0182] The commercial R11O2 catalyst (~US$ 44000 / kg, Macklin) for water splitting as oxygen evolution electrocatalyst exhibits poor durability. Moreover, this kind of electrocatalyst is easily poisoned by other impurities in water splitting cell using seawater as recourse. These critical factors dramatically increase the cost of the industrial application of water splitting technology to generate hydrogen energy. This invention provides a new class of ferromagnetic single-atom spin catalyst not only at low cost (US$ 260 / kg) but also be equipped with high activity and stability. Thus, the ferromagnetic SASCs provides a promising industrial application of both water and saline water electrolyser technologies.Reference1. Seh, Z. W. el al. Combining theory and experiment in electrocatalysis: insights into materials design. Science 355, eaad4998 (2017).2. Glenk, G. et al. Economics of converting renewable power to hydrogen. Nat. Energy 4, 216-222 (2019).3. Davis, S. J. et al. Net-zero emissions energy systems. Science 360, eaas9793 (2018).4. Tong, W. M. etal. Electrolysis of low-grade and saline surface water. Nat. Energy 5, 367-377 (2020).5. Song, F. et al. Transition metal oxides as electrocatalysts for the oxygen evolution reaction in alkaline solutions: an application-inspired renaissance. J. Am. Chem. Sac. 140, 7748-7759 (2018).6. Sun, T. et al. Design of local atomic environments in single-atom electrocatalysts for renewable energy conversions. Adv. Mater. 33, 2003073 (2021).7. Gracia, J. Spin dependent interactions catalyse the oxygen electrochemistry. Phys. Chem. Chem. Phys. 19, 20451-20456 (2017).8. Gracia, J. et al. Principles determining the activity of magnetic oxides for electron transfer reactions. J. Catal. 361, 331-338 (2018).9. Zhang, Y. Y. et al. Recent advances in magnetic field-enhanced electrocatalysis. ACS Appl. Energy Mater. 3, 10303-10316 (2020).10. Li, X. N. et al. Optimized electronic configuration to improve the surface absorption and bulk conductivity for enhanced oxygen evolution reaction. J. Am. Chem. Soc. 141, 3121-3128 (2019).11. Ren, X. el al. Spin-polarized oxygen evolution reaction under magnetic field. Nat. Commun. 12, 2608 (2021).12. Yan, J. H. et al. Direct magnetic reinforcement of electrocatalytic ORR / OER with electromagnetic induction of magnetic catalysts. Adv. Mater. 33, 2007525 (2021).13. Wu, T. Z. et al. Spin pinning effect to reconstructed oxyhydroxide layer on ferromagnetic oxides for enhanced water oxidation. Nat. Commun. 12, 3634 (2021).14. Zhou, G. et al. Spin-sate reconfiguration induced by alternating magnetic field for efficient oxygen evolution reaction. Nat. Commun. 12, 4827 (2021).15. Sun, Z. M. et al. Regulating the spin state of Fenienhances the magnetic effect of the molecular catalysis mechanism. J. Am. Chem. Soc. 144, 8204-8213 (2022).16. Buchachenko, A. L. et al. Electron spin catalysis. Chem. Rev. 102, 603-612 (2002).17. Naaman, R. et al. Chiral molecules and the electron spin. Nat. Rev. Chem. 3, 250- 260 (2019).18. McCusker, J. M. Elclcctronic structure in the transition metal block and its implications for light harvesting. Science 363, 484-488 (2019)19. Garces-Pineda, F. A. et al. Direct magnetic enhancement of electrocatalytic water oxidation in alkaline media, Nat. Energy 4, 519-525 (2019).20. Chen, R. R. et al. SmCos with a reconstructed oxyhydroxide surface for spin- selective w'ater oxidation at elevated temperature. Angew. Chem. Int. Ed. 60, 25884- 25890 (2021).21. Hunt, C. et al. Quantification of the effect of an external magnetic field on water oxidation with cobalt oxide anodes. J. Am. Chem. Soc. 144, 733-739 (2022).22. Zhang, Z. M. el al. Significant change of metal cations in geometric sites by magnetic-field annealing FeCo2O4 for enhanced oxygen catalytic activity. Small 18, 210418 (2022).23. Zhang, Y. Y. et al. Magnetic field assisted electrocatalytic oxygen evolution reaction of nickel-based materials. J. Mater. Chem. A 10, 1760-1767 (2020).Niether, C. el al. Improved water electrolysis using magnetic heating of FeC-Ni core- shell nanoparticles. Nat. Energy 3, 476-483 (2018). Duan, H. L. et al. Single-atom-layer catalysis in a M0S2 monolayer activated by long- range ferromagnetism for the hydrogen evolution reaction: beyond single-atom catalysis. Angew. Chem. Int. Ed. 60, 7251 (2021). Fu, S. C. et al. Enabling room temperature ferromagnetism in monolayer M0S2 via in situ iron-doping. Nat. Commun. 11, 2034 (2020). Zhang, ,1. et al. Engineering water dissociation sites in M0S2 nanosheets for accelerated electrocatalytic hydrogen production. Energy Environ. Sci. 9, 2789-2793 (2016). Deng, J. et al. Multiscale structural and electronic control of molybdenum disulfide foam for highly efficient hydrogen production. Nat. Commun. 8, 14430 (2017). Zheng, Z. et al. Boosting hydrogen evolution on M0S2 via co-confming selenium in surface and cobalt in inner layer. Nat. Commun. 11, 3315 (2020). Liu, J. L. et al. In situ tracing of atom migration in Pt / NiPt hollow spheres during catalysis of CO oxidation. Chem. Commun. 50, 1804-1807 (2014). Hai, X. et al. Scalable two-step annealing method for preparing ultra-high-density single-atom catalyst libraries. Nat. Nanotechnol. 17, 174-181 (2022). Zhang, H. B. el al. Surface modulation of hierarchical M0S2 nanosheets by Ni single atoms for enhanced electrocatalytic hydrogen evolution. Adv. Fund. Maier. 28, 1807086 (2018). Li, J. F. el al. Robust ferromagnetism in Cr-doped ReS2 nanosheets demonstrated by experiments and density functional theory calculations. Nanotechnology 31, 175702 (2020). Zhang, F. et al. Monolayer vanadium-doped tungsten disulfide: a room- temperature dilute magnetic semiconductor. Adv. Sci. 7, 2001174 (2020). Ahmed, S. et al. High coercivity and magnetization in WSe2 by codoping Co and Nb. Small 16, 1903173 (2020). Ahmed, S. et al. Colossal magnetization and giant coercivity in ion-implanted (Nb and Co) M0S2 crystals. ACS Appl. Mater. Interfaces 12, 58140-58148 (2020). Zhecheva, E. et al. EPR analysis of the local structure of Ni3+ions in Ni-based electrode materials obtained under high-pressure. J. Mater. Sci. 42, 3343-3348 (2007). Wongnatc, T. et al. The radical mechanism of biological methane synthesis by methyl-coenzyme M reductase. Science 352, 953-958 (2016). Krellner, C. et al. Relevance of ferromagnetic correlations for the electron spin resonance in Kondo Lattice systems. Phys. Rev. Lett. 100, 066401 (2008). Yahya, M. et al. ESR studies of transition from ferromagnetism to superparamagnetism in nano-ferromagnet Lao.sSro.zMnCh. J- Magn. Magn. Maier. 466, 341-350 (2018). Wu, Z. P. et al. Non-noble-metal-based electrocatalysts toward the oxygen evolution reaction. Adv. Fund. Maier. 30, 1910274 (2020). Wang, Y. Y. et al. Recent progress on layered double hydroxides and their derivatives for electrocatalytic water splitting. Adv. Sci. 5, 1800064 (2018). Meng, L. J. et al. Anomalous thickness dependence of Curie temperature in air-stable two-dimensional ferromagnetic lT-CrTe2 grown by chemical vapor deposition. Nat. Commun. 12, 809 (2021). Shi, S. Y. et al. All-electric magnetization switching and Dzyaloshinskii-Moriya interaction in WTe2 / ferromagnet heterostructures. Nat. Nanotechnol. 14, 945-949(2019). Gambardella, P. et al. Ferromagnetism in one -dimensional monatomicmetal chains. Nature 416, 301-304 (2002). Tong, W. M. et al. Electrolysis of low-grade and saline surface water. Nat. Energy 5, 367-377 (2020). Yu, J. et al. Seawater electrolyte -based metal-air batteries: from strategies to applications. Energy Environ. Sci. 13, 3253-3268 (2020). Wang, Q. C. et al. Pyridinic-N-dominated doped defective graphene as a superior oxygen electrocatalyst for ultrahigh-energy-density Zn-air batteries. ACS Energy Lett. 3, 1183-1191 (2018). Chen, R. et al. Layered structure causes bulk NiFe layered double hydroxide unstable in alkaline oxygen evolution reaction. Adv. Mater. 31, 1903909 (2019). Krcssc, G. et al. Ab initio molecular dynamic for liquid metals. Phys. Rev. B 47, 558 (1993). Krcssc, G. et al. From ultrasoft pscudopotcntials to the projector augmented-wave method. Phys. Rev. B 59, 1758 (1999). Blochl, P. E. Projector augmented-wave method. Phys. Rev. B 50, 17953 (1994). Perdew, J. P. et al. Gneralized gradient approximaion made simple. Phys. Rev. Lett. 77, 3865 (1996). Dudarev, S. L. et al. Electron-energy-loss spectra and the structural stability of nickel oxide: an LSDA+U study. Phys. Rev. B 57, 1505 (1998). Andriotis, A. N. et al. Tunable magnetic properties of transition metal doped MoS2- Phys. Rev. B 90, 125304 (2014). Mishra, R. et al. Long-range ferromagnetic ordering in manganese-doped two- dimensiaonal dichalcogenides. Phys. Rev. B 88, 144409 (2013). Tang, W. et al. A grid-based Bader analysis algorithm without lattice bias. J. Phys.: Condens. Matter. 21, 084204 (2009). Du, Y. H. etal. XAFCA: anew XAFS beamline for catalysis research. J. Synchrotron Radial. 22, 839-843 (2015). Nprskov, J. K. et al. Origin of the overpotential for oxygen reduction at a fuel-cell cathode. J. Phys. Chem. B 108, 17886-17892 (2004). Huang, Z. F. et al. Chemical and structural origin of lattice oxygen oxidation in Co- Zn ixyhydroxidc oxygen evolution electrocatalysts. Nat. Energy 4, 329-338 (2019). Mathew, K. et al. Implicit solvation model for density-functional study of nanocrystal surfaces and reaction pathways. J. Chem. Phys. 140, 084106 (2014). Mathew, K. et al. Implicit self-consistent electrolyte model in plane-wave density- functional theory. J. Chem. Phys. 151, 234101 (2019). Meng, X. et al. Distance synergy of MoSj-con fined rhodium atoms for highly efficient hydrogen evolution. Ange w. Chem. Int. Ed. 59, 10502-10507 (2020). Zheng, Z. el al. Boosting hydrogen evolution on M0S2 via co-confining selenium in surface and cobalt in inner layer. Nat. Commun. 11, 3315 (2020). Meng, X. et al. Three-dimensionally hierarchical MoS2 / graphene architecture for high-performance hydrogen evolution reaction. Nano Energy 61, 611-616 (2019). Deng, J. et al. Multiscale structural and electronic control of molybdenum disulfide foam for highly efficient hydrogen production. Nat. Commun. 8, 14430 (2017). Zou, J. Y. et al. Doping concentration modulation in vanadium-doped monolayer molybdenum disulfide for synaptic transistors. ACS Nano 15, 7340 (2021). Li, L. et al. Role of sulfur vacancies and undercoordinated Mo regions in M0S2 nanosheets toward the evolution of hydrogen, ACS Nano 13, 6824 (2019).Qi, K. el al. Single-atom cobalt array bound to distorted IT M0S2 with ensemble effect for hydrogen evolution catalysis, Nat. Commun. 10, 5231 (2019). Cheng, Y. C. et al. Prediction of two-dimensional diluted magnetic semiconductors: Doped monolayer M0S2 systems. Phys. Rev. B 87, 100401 (2013). Kang, J. S. et al. Valence and spin states in delafossite AgNiCh and the frustrated Jahn-Teller system AN1O2 (A=Li, Na). Phys. Rev. B 76, 195122 (2007). Montoro, L. A. et al. Electronic structure of the transition metal ions in LiCoO2, LiNiO2and LiCoo.5Nio.5O2. Chem. Phys. Lett. 309, 14-18 (1999). Krellner, C. et al. Relevance of ferromagnetic correlations for the electron spin resonance in Kondo Lattice systems. Phys. Rev. Lett. 100, 066401 (2008). Yahya, M. et al. ESR studies of transition from ferromagnetism to superparamagnetism in nano-ferromagnet Lao.sSro^MnOa. J. Magn. Magn. Mater. 466, 341-350 (2018). Stoner, E. C. Collective electron specific heat and spin paramagnetism in metal. Proc. R. Soc. A 154, 656 (1936). Zhuang, H. L. et al. Strong anisotropy and magnetostriction in the two-dimensional stoner ferromagnet FeiGcTe?. Phys. Rev. B 93, 1-7 (2016). Gunnarsson, O. Band model for magnetism of transition metals in the spin-density- functional formalism. J. Phys. F 6, 587 (1976). Liu, J. L. el al. In situ tracing of atom migration in Pt / NiPt hollow spheres during catalysis of CO oxidation. Chem. Commun. 50, 1804-1807 (2014).
Claims
Claims1. A single-atom spin catalyst (SASC) consisting of a substitutional magnetic atom M embedded in a Molybdenum Disulfide (M0S2) host, with the formula of M1 / M0S2, wherein M1 / M0S2 has ferromagnetic property at room temperature.
2. The SASC of claim 1, wherein the substitutional magnetic atom M is selected from the group consisting of Ni, Mn, Fe, and Co.
3. The SASC of claim 2, wherein the substitutional magnetic atom M is Ni, and the formula of the SASC is Nii / MoS2.
4. The SASC of any one of claims 1-3, wherein an atomic doping ratio (M1 / M0) of the SASC is up to about 20:100.
5. The SASC of claim 4, wherein the atomic doping ratio (Nii / Mo) of Ni 1 / M0S2 is 14:100.
6. The SASC of claim 3, wherein the Ni content in Nii / MoS2 is selected from the group consisting of 0.20, 0.38, 0.95, 1.42, 2.41, 3.12 and 4.20 wt%.
7. The SASC of claim 6, wherein the Ni content in Nii / MoS2 is 3.12 wt%.
8. The SASC of any one of claims 3-7, wherein Ni-Ni distance is about 6.390 A.
9. A water or seawater splitting cell comprising an electrode loaded with the SASC of any one of claims 1 -8.
10. The water or seawater splitting cell of claim 9, wherein the SASC is Nii / MoS2.
11. A method of synthesising the SASC of any one of claims 1-8, comprising the following steps:(a) dissolving molecular precursors comprising a metal salt, (NHOeMovCh^ 4H2O (ammonium molybdate tetrahydrate) and CH3CSNH2 (thioacetamide) in distilled water to form a solution;(b) autoclaving the solution and cooling the solution to room temperature to result in a product;(c) washing the product with distilled water and ethanol and drying the product under vacuum;(d) heating the product in a furnace, and cooling the product to room temperature, to thereby form the SASC.
12. The method of claim 11, wherein the metal salt is selected from the group consisting of Mn(CH3COO)2·4H2O, Fe(CH3COO)2·4H2O, Co(CH3COO)2·4H2O and Ni(CH3COO)2·4H2O.
13. The method of claim 12, wherein the metal salt is Ni(CH3COO)2·4H2O.
14. The method of claim 11, wherein the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) is 1 to 5 mmol, the amount of CH3CSNH2 (thioacetamide) is 5 to 20 mmol, and the molar ratio of (NH4)6Mo7O24·4H2O to CH3CSNH2is 4 to 10.
15. The method of claim 11, wherein the molar ratio of the metal salt to (NH4)6Mo7O24·4H2O is below 20% (nM:nMo max).
16. The method of claim 14, wherein the amount of (NH4)6Mo7O24·4H2O (ammonium molybdate tetrahydrate) (nMo) is 1 mmol, and the amount of CH3CSNH2 (thioacetamide) is 10 mmol.
17. The method of claim 15, wherein the metal salt is below 0.2 mmol when (NH4)6Mo7O24·4H2O is 0.143 mmol.
18. The method of claim 11, wherein in step (b) the solution is autoclaved at 160 to 200 °C for 12 to 24 h.
19. The method of claim 18, wherein in step (b) the solution is autoclaved at 180 °C for 20 h.
20. The method of claim 11, wherein in step (c) the product is dried under vacuum at 50-80 °C for 8 to 20 h.
21. The method of claim 20, wherein in step (c) the product is dried under vacuum at 60 °C for 12 h.
22. The method of claim 11, wherein in step (d) the product is heated to 350 to 500 °C at a rate of 5 to 10 °C min-1.
23. The method of claim 22, wherein in step (d) the product is heated to 400 °C at a rate of 10 °C min-1.
Citation Information
Cited By
Composite SERS (Surface Enhanced Raman Scattering) substrate based on needle tip silicon wafer and preparation method and application thereof