Ester-containing epoxy cured product and degradation method for composite material thereof

By using low-carbon fatty amine compounds and ester-containing epoxy cured substances to undergo amine decomposition reaction at low temperatures, the problem of difficulty in recycling and high-temperature degradation of epoxy resin materials is solved, and the low energy consumption degradation effect is achieved.

WO2024229652A1PCT designated stage expired Publication Date: 2024-11-14SWANCOR INNOVATION & INCUBATION CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/092740
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-08
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Epoxy resin materials are difficult to recycle and reuse after curing. The existing degradation methods require high temperature conditions, consume a lot of energy, and are difficult to degrade without heating.

Method used

A low-carbon fatty amine compound was used as a degradation solution, and the amine-containing epoxy cured product was mixed with an ester-containing epoxy cured product and placed at a low temperature of 10°C to 50°C to decompose the ester-containing epoxy cured product.

Benefits of technology

Degradation of ester-containing epoxy cured substances without high temperature conditions reduces energy consumption and provides a low energy consumption recovery and treatment method.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092740_14112024_PF_FP_ABST
    Figure CN2023092740_14112024_PF_FP_ABST
Patent Text Reader

Abstract

An ester-containing epoxy cured product and a degradation method for a composite material thereof. The degradation method for the ester-containing epoxy cured product comprises a mixing step and a degradation step; the mixing step is to mix an ester-containing epoxy cured product with aliphatic amines to form a degradation system; and the degradation step is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured product. In this way, a low carbon aliphatic amine compound is used as a degradation liquid to decompose an ester-containing epoxy cured product at a low temperature, thereby achieving the objective of degradation without energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Degradation method of ester-containing epoxy cured product and composite material thereof Technical Field

[0001] The present invention relates to a method for degrading an ester-containing epoxy cured product and a composite material thereof, in particular to a method for degrading an ester-containing epoxy cured product and a composite material thereof which can be implemented at low temperature. Background Art

[0002] Epoxy resins offer advantages such as low viscosity and easy workability before curing, and excellent thermal stability, mechanical strength, and chemical resistance after curing. These properties have led to their widespread application in various fields, and are often used in fiber composites requiring both high strength and lightweighting. However, due to the chemical cross-linking nature of thermosets, they are non-reprocessable, making them difficult to recycle and reuse after disposal. With the rise of environmental awareness in recent years, the disposal of these wastes has become a priority, becoming a primary issue in the development of composite materials.

[0003] In addition, after curing, epoxy resin will form a stable covalent network bond, which is difficult to decompose and recycle through chemical degradation. Therefore, in order to achieve the purpose of easy recycling after the product is retired, introducing easily destructible bonds into the epoxy structure is the main research direction of academia and industry.

[0004] Currently, one research team has introduced a carbonate structure into the backbone of epoxy resin and found that the resulting cured epoxy resin can be completely degraded by hexylamine at high temperatures (125°C). Another research team has synthesized an active ester hardener derived from waste polycarbonate. After curing with epoxy resin, this active ester hardener still exhibits the property of being degraded by hexylamine at high temperatures. Therefore, introducing ester groups into epoxy cured products will allow for degradation and recovery via aminolysis, but degradation at high temperatures has the disadvantage of being energy-intensive.

[0005] In view of this, how to find a suitable amine degradation liquid to enable the degradation of epoxy curing materials containing ester groups without heating, thereby achieving the advantage of not requiring energy consumption, has become the goal of relevant industries.

[0006] Summary of the Invention

[0007] An object of the present invention is to provide a method for degrading ester-containing epoxy cured products and composite materials thereof, wherein a low-carbon aliphatic amine compound is used as a degradation liquid to decompose the ester-containing epoxy cured products at low temperatures.

[0008] One embodiment of the present invention provides a method for degrading an ester-containing epoxy cured product, comprising a mixing step and a degradation step. The mixing step comprises mixing the ester-containing epoxy cured product with an aliphatic amine to form a degradation system, and the degradation step comprises subjecting the degradation system to a degradation temperature to degrade the ester-containing epoxy cured product.

[0009] According to the method for degrading an ester-containing epoxy cured product described in the preceding paragraph, the aliphatic amine may be a diamine having 2 to 5 carbon atoms or pentylamine.

[0010] According to the method for degrading an ester-containing epoxy cured material described in the preceding paragraph, the ester group in the ester-containing epoxy cured material may refer to an ester group, a carbonate group, or a urethane group.

[0011] According to the degradation method of the epoxy cured material containing ester groups described in the previous paragraph, the epoxy cured material containing ester groups can be obtained by curing an epoxy compound containing an ester structure with a hardener.

[0012] According to the degradation method of the epoxy cured material containing an ester group as described in the preceding paragraph, the ester group in the epoxy compound containing an ester structure may refer to an ester group, a carbonate group or a urethane group.

[0013] According to the degradation method of the ester-containing epoxy curing material described in the previous paragraph, the hardener can be one of an amine hardener, a phenol hardener, an acid anhydride hardener, and an ester hardener, or a mixture of more than one of them.

[0014] According to the degradation method of the epoxy cured material containing ester groups described in the previous paragraph, the epoxy cured material containing ester groups can be obtained by curing an epoxy compound with an acid anhydride hardener or an ester hardener.

[0015] According to the degradation method of the ester-containing epoxy cured material described in the previous paragraph, the ester-containing epoxy cured material can be obtained by catalyzing an epoxy compound containing an ester structure with an acid-base catalyst and then subjecting it to epoxy self-curing.

[0016] According to the degradation method of the ester-containing epoxy cured product described in the previous paragraph, the degradation temperature can be 10°C to 50°C.

[0017] Another embodiment of the present invention provides a method for degrading a composite material containing an epoxy cured product with an ester group, comprising a mixing step and a degradation step. The mixing step comprises mixing the composite material containing an epoxy cured product with an aliphatic amine to form a degradation system. The degradation step comprises subjecting the degradation system to a degradation temperature to degrade the composite material containing an epoxy cured product with an ester group, and filtering to separate the polyol oligomer and the fiber.

[0018] According to the degradation method of the ester-containing epoxy cured material composite material described in the previous paragraph, the aliphatic amine can be a diamine having 2 to 5 carbon atoms or pentylamine.

[0019] According to the degradation method of the epoxy cured material composite material containing ester groups as described in the previous paragraph, the ester group in the epoxy cured material composite material containing ester groups may refer to an ester group, a carbonate group or a urethane group.

[0020] According to the degradation method of the ester-containing epoxy cured material composite material described in the previous paragraph, the degradation temperature can be 10°C to 50°C.

[0021] Therefore, the present invention mainly selects low-carbon amine compounds, and immerses the ester-containing epoxy cured product in the amine compounds, so that the aminolysis reaction can be carried out without a high-temperature environment, thereby achieving the purpose of decomposing the ester-containing epoxy cured product.

[0022] BRIEF DESCRIPTION OF THE DRAWINGS

[0023] To make the above and other objects, features, advantages and embodiments of the present invention more apparent, the following descriptions of the accompanying drawings are given:

[0024] FIG. 1 is a flow chart illustrating the steps of a method for degrading an ester-containing epoxy cured product according to one embodiment of the present invention.

[0025] FIG. 2 is a flow chart illustrating the steps of a method for degrading an ester-containing epoxy cured material composite material according to another embodiment of the present invention.

[0026] [Main Component Symbols] 100: Degradation method of epoxy cured material containing ester group 200: Degradation method of composite material containing epoxy cured material containing ester group 110, 120, 210, 220: Steps

[0027] The best way to implement the invention

[0028] The following will discuss various embodiments of the present invention in more detail. However, this embodiment can be applied to various inventive concepts and can be specifically implemented in various specific scopes. The specific embodiments are for illustrative purposes only and are not intended to limit the scope of the disclosure.

[0029] <Degradation Method of Ester-containing Epoxy Cured Material>

[0030] 1 , which is a flow chart illustrating a method 100 for degrading an epoxy cured material containing an ester group according to one embodiment of the present invention. In FIG1 , the method 100 for degrading an epoxy cured material containing an ester group comprises steps 110 and 120 .

[0031] Step 110 is a mixing step, in which an ester-containing epoxy curing material is mixed with an aliphatic amine to form a degradation system. The aliphatic amine can be a diamine having 2 to 5 carbon atoms or amylamine. Examples of diamines having 2 to 5 carbon atoms include ethylenediamine, propylenediamine, butanediamine (1,4-butanediamine), or pentamethylenediamine (1,5-pentanediamine). Specifically, the ester group in the ester-containing epoxy curing material can be an ester group, a carbonate group, or a urethane group.

[0032] Specifically, an ester-containing epoxy cured product can be obtained by curing an ester-containing epoxy compound with a hardener, wherein the ester group in the ester-containing epoxy compound may be an ester group, a carbonate group, or a urethane group, and the hardener may be one or a mixture of more than one of an amine hardener, a phenol hardener, an acid anhydride hardener, and an ester hardener. Alternatively, an ester-containing epoxy cured product can be obtained by curing an epoxy compound with an acid anhydride hardener or an ester hardener, wherein the epoxy compound is a general epoxy resin, such as bisphenol A epoxy resin (DGEBA), bisphenol F epoxy resin (DGEBF), phenol novolac epoxy resin (PNE), cresol novolac epoxy resin (CNE), dicyclopentadiene-phenol epoxy resin (DNE), naphthalene-containing epoxy resin (Naphthalene-containing epoxy resin), and the like. epoxy), phosphorus epoxy resin or a mixture thereof; alternatively, the ester-containing epoxy cured product can also be obtained by catalyzing an ester-containing epoxy compound with an acid-base catalyst and then subjecting the epoxy compound to epoxy self-curing.

[0033] Step 120 is a degradation step, which is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy curing material, wherein the degradation temperature can be 10°C to 50°C, preferably 20°C to 40°C, so as to maintain the degradation of the ester-containing epoxy curing material at a low temperature.

[0034] <Degradation Method of Ester-containing Epoxy Cured Composite Materials>

[0035] 2 is a flowchart illustrating a method 200 for degrading a composite material containing an ester group and an epoxy cured material according to another embodiment of the present invention. In FIG2 , the method 200 for degrading a composite material containing an ester group and an epoxy cured material comprises steps 210 and 220 .

[0036] Step 210 is a mixing step, in which the ester-containing epoxy cured material composite material is mixed with an aliphatic amine to form a degradation system. The aliphatic amine may be a diamine having 2 to 5 carbon atoms or a pentylamine. Specifically, the ester group in the ester-containing epoxy cured material composite material may be an ester group, a carbonate group, or a urethane group.

[0037] Specifically, the ester-containing epoxy cured material composite material can be obtained by forming an ester-containing epoxy resin composition and fibers through a composite process at room temperature or high temperature, wherein the composite process includes, but is not limited to, pultrusion, vacuum infusion, compression molding, or prepreg molding; and the fibers can be, but are not limited to, glass fibers, carbon fibers, flax fibers, polyamide fibers, or a mixture thereof.

[0038] Step 220 is a degradation step, which is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured material composite material and filter out the polyol oligomers and fibers. The degradation temperature can be 10°C to 50°C, preferably 20°C to 40°C, so as to maintain the ester-containing epoxy cured material composite material at a low temperature and realize a recycling mechanism for separating fibers and organic matter.

[0039] The present invention utilizes a low-carbon aliphatic amine monomer as a degradation solution, allowing the ester-containing epoxy curing material to be immersed in the degradation solution and degraded at room temperature. This allows the decomposition of the ester-containing epoxy curing material to be achieved in a non-high-temperature environment, even without the need for energy-consuming heating, thereby addressing the issues of epoxy waste recycling and energy conservation and carbon reduction.

[0040] The present invention is further illustrated by the following specific examples, which are intended to facilitate those skilled in the art to which the present invention relates, so that they can fully utilize and practice the present invention without excessive interpretation. These examples should not be construed as limiting the scope of the present invention, but are intended to illustrate how to implement the materials and methods of the present invention.

[0041] <Synthesis example>

[0042] Synthesis Example 1: 2 g of an ester-containing epoxy resin DPCEP2 (epoxy equivalent weight 483 g / eq) and 0.26 g of a hardener Jeffamine D230 (available from Huntsman, active hydrogen equivalent weight 62 g / eq) were placed in an aluminum pan and evenly mixed. The mixture was then placed in a 70°C oven for curing for 6 hours to obtain the ester-containing epoxy cured product of Synthesis Example 1.

[0043] Synthesis Example 2: 2 grams of an epoxy resin containing an ester structure, DPCEP2 (epoxy equivalent of 483 g / eq), 0.69 grams of methyltetrahydrophthalic anhydride (MTHPA, purchased from Zhonghou Chemical, reaction equivalent of 166.2 g / eq), and 0.004 grams (0.2 wt% of the epoxy resin) of 2-methylimidazole were placed in an aluminum pan and evenly mixed. The mixture was then placed in an oven at 120°C for half an hour and then in an oven at 150°C for 1 hour to obtain the ester-containing epoxy cured product of Synthesis Example 2.

[0044] Synthesis Example 3: 2 g of bisphenol A epoxy resin (obtained from Changchun Man-Made Resins, product code BE188, epoxy equivalent of 185 g / eq), 1.80 g of methyltetrahydrophthalic anhydride (MTHPA, purchased from Zhonghou Chemical, reaction equivalent of 166.2 g / eq) and 0.004 g (0.2 wt % of epoxy resin) of 2-methylimidazole were placed in an aluminum pan and evenly mixed. The mixture was then placed in an oven at 120° C. for half an hour and then in an oven at 150° C. for 1 hour to obtain the ester-containing epoxy cured product of Synthesis Example 3.

[0045] Synthesis Example 4: 2 g of bisphenol A epoxy resin (obtained from Changchun Man-Made Resins, product code BE188, epoxy equivalent weight 185 g / eq), 1.37 g of polycarbonate (purchased from Chi Mei Industrial, product code PC-122, reaction equivalent weight 127 g / eq), and 0.004 g (0.2 wt % of the epoxy resin) of 2-methylimidazole were melt-mixed in an aluminum pan and then cured in a 175° C. oven for half an hour to obtain the ester-containing epoxy cured product of Synthesis Example 4.

[0046] Synthesis Example 5: 2 g of bisphenol A epoxy resin (obtained from Changchun Synthetic Resins, product code BE188, epoxy equivalent weight 185 g / eq) and 0.67 g of hardener Jeffamine D230 (purchased from Huntsman, active hydrogen equivalent weight 62 g / eq) were placed in an aluminum pan and evenly mixed. The mixture was then placed in a 70°C oven for curing for 6 hours to obtain the epoxy cured product of Synthesis Example 5.

[0047] Synthesis Example 6: 2 grams of an ester-containing epoxy resin DPCEP2 (epoxy equivalent of 483 g / eq) and 0.004 grams (0.2 wt% of the epoxy resin) of 2-methylimidazole were placed in an aluminum pan and evenly mixed. The mixture was then cured in an oven at 120°C for half an hour and then at 150°C for 1 hour to obtain the ester-containing epoxy cured product of Synthesis Example 6.

[0048] In addition, according to different process operation requirements, the epoxy resin compositions in the above-mentioned Synthesis Examples 1 to 6 can be adjusted to an appropriate gelation time for fiber impregnation molding at room temperature, and then a baking process is applied according to the curing conditions described in each synthesis example to obtain an ester-containing epoxy cured material composite material containing fibers.

[0049] <Examples / Comparative Examples>

[0050] Examples 1 to 5: 1 gram of the ester-containing epoxy cured products of Synthesis Examples 1 to 4 and Synthesis Example 6 were soaked in 10 mL of pentamethylenediamine, respectively, and the degradation conditions were observed at room temperature.

[0051] Comparative Example 1: 1 gram of the epoxy cured product of Synthesis Example 5 was soaked in 10 mL of pentamethylenediamine, and the degradation condition was observed at room temperature.

[0052] Comparative Example 2: 1 gram of the ester-containing epoxy curing material of Synthesis Example 1 was mixed with 10 grams of hexamethylenediamine. However, since the hexamethylenediamine solidified at room temperature and could not be mixed smoothly, the mixture was placed in an oven at 60°C to melt the hexamethylenediamine, and then immersed in the oven at 60°C to observe the degradation.

[0053] Comparative Example 3: 1 gram of the ester-containing epoxy cured product of Synthesis Example 1 was soaked in 10 mL of hexylamine, and the degradation status was observed at room temperature.

[0054] Comparative Example 4: 1 gram of the ester-containing epoxy cured product of Synthesis Example 1 was soaked in 10 mL of tris-ethylenetetramine, and the degradation status was observed at room temperature.

[0055] Comparative Example 5: 1 gram of the ester-containing epoxy cured product of Synthesis Example 1 was soaked in 10 mL of tris-ethylenetetramine and the degradation was observed at 135°C.

[0056] <Degradation Status Assessment>

[0057] The degradation temperatures, degradation times and residual weights of Examples 1 to 5 and Comparative Examples 1 to 5 are listed in Table 1 below.

[0058] As shown in Table 1 above, Examples 1 to 5 were all completely degraded by pentamethylenediamine at room temperature (25°C). Furthermore, Examples 2 and 5, which contained a higher proportion of ester groups in the epoxy cured product, exhibited the best degradation efficiency. Comparative Example 1, which contained no ester groups in the epoxy cured product, showed no significant degradation after being immersed in pentamethylenediamine for 7 days at room temperature.

[0059] Comparative Example 2 replaces pentamethylenediamine with hexamethylenediamine. However, hexamethylenediamine transforms from a liquid to a solid at room temperature, making room-temperature degradation difficult. Therefore, after heating Comparative Example 2 to 60°C to melt it into a liquid state, it was found that despite the immersion in Comparative Example 2 above room temperature, the effect achieved after three days of immersion was still significantly inferior to that achieved by Example 1 at room temperature. Furthermore, Comparative Example 3, in which hexamethylenediamine was replaced with hexamethylenediamine, which is liquid at room temperature, showed no significant degradation effect after seven days of immersion at room temperature. This demonstrates that increasing the carbon number of the amine compound negatively impacts the overall low-temperature degradation performance.

[0060] Comparative Example 4, in which pentamethylenediamine was replaced with the multifunctional triethylenetetramine, showed no significant improvement in degradation at room temperature, and the results obtained after immersion for 7 days were also unsatisfactory. However, Comparative Example 5, in which the temperature was raised to 135°C, showed excellent degradation, achieving complete degradation in approximately 12 hours. This is consistent with prior art observations that amine compounds exhibit the property of aminolysis of ester groups at high temperatures, but their reactivity at low temperatures is extremely low. Even with highly alkaline multifunctional amines, achieving low-temperature degradation is difficult. This suggests that the alkalinity of the amine used is not an indicator of room-temperature degradation.

[0061] In summary, the present invention utilizes a low-carbon fatty amine compound as a degradation solution, which, to a certain extent, facilitates the penetration of the degradation solution into ester-containing epoxy cured products, enabling the degradation of ester-containing epoxy cured products at low temperatures. This overcomes the prior art's technical bias of requiring high-temperature processes (>100°C) for degradation, solves long-standing problems of the prior art, and provides a low-energy recycling and reuse approach for ester-containing epoxy cured products.

[0062] Although the present invention has been disclosed above in terms of embodiments, this is not intended to limit the present invention. Anyone skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the claims.

Claims

1. A method for degrading an ester-containing epoxy cured product, characterized in that: Include: performing a mixing step of mixing the ester group-containing epoxy curing material with aliphatic amines to form a degradation system; and The degradation step is carried out by placing the degradation system at a degradation temperature to degrade the ester-containing epoxy cured product.

2. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The aliphatic amine is a diamine having 2 to 5 carbon atoms or pentylamine.

3. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester group in the ester group-containing epoxy cured product refers to an ester group, a carbonate group or a urethane group.

4. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester-containing epoxy cured product is obtained by curing an epoxy compound containing an ester structure with a hardener.

5. The method for degrading an ester group-containing epoxy cured product according to claim 4, wherein: The ester group in the epoxy compound containing an ester structure refers to an ester group, a carbonate group or a urethane group.

6. The method for degrading an ester group-containing epoxy cured product according to claim 4 or 5, characterized in that: The hardener is one of an amine hardener, a phenol hardener, an acid anhydride hardener, and an ester hardener, or a mixture of more than one of the above.

7. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester-containing epoxy cured product is obtained by curing an epoxy compound with an acid anhydride curing agent or an ester curing agent.

8. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The ester-containing epoxy cured product is obtained by epoxy self-curing after the epoxy compound containing the ester structure is catalyzed by an acid-base catalyst.

9. The method for degrading an ester group-containing epoxy cured product according to claim 1, wherein: The degradation temperature is between 10°C and 50°C.

10. A method for degrading a composite material containing an ester group epoxy cured product, characterized in that: Include: A mixing step is performed, which is to mix the ester group-containing epoxy cured material composite material with aliphatic amines to form a degradation system; as well as The degradation step is carried out, which is to place the degradation system at a degradation temperature to degrade the ester-containing epoxy cured material composite material, and filter and separate the polyol oligomer and the fiber.

11. The method for degrading the composite material containing ester group epoxy cured material according to claim 10, characterized in that: The aliphatic amine is a diamine having 2 to 5 carbon atoms or pentylamine.

12. The method for degrading the composite material containing ester group epoxy cured material according to claim 10, characterized in that: The ester group in the ester group-containing epoxy cured material composite material refers to an ester group, a carbonate group or an urethane group.

13. The method for degrading the composite material containing ester group epoxy cured material according to claim 10, characterized in that: The degradation temperature is between 10°C and 50°C.

Citation Information

Patent Citations

  • Method for recycling waste thermosetting resin and composite material thereof

    CN109897216A

  • Method for recovering carbon fibers in composite material in lossless closed-loop manner

    CN113683815A

  • Method for preparing aromatic polyol by degrading anhydride and curing epoxy resin material

    CN113845493A

  • Degradable and recoverable epoxy cured product, preparation method, recovery method and application

    CN115651167A

  • Carbonate-containing epoxy resin, preparation method thereof, epoxy cured product prepared from carbonate-containing epoxy resin and method for degrading epoxy cured product

    CN115873215A