Polycarbonate oligomer having unsaturated double bonds, preparation method therefor, curable composition, and preparation method for low-dielectric cured product

The unsaturated double bond polycarbonate oligomers were prepared through alcoholylation and esterification reactions and copolymerized with polyphenylene ether resin, which solved the problem of recycling and reuse of waste polycarbonate, and realized the heat resistance of high-frequency circuit board materials and Improved electrical performance to meet environmental protection and high-frequency application needs.

WO2024229685A1PCT designated stage expired Publication Date: 2024-11-14SWANCOR INNOVATION & INCUBATION CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2023/092929
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The prior art is difficult to effectively recycle and reuse waste polycarbonate, resulting in a decrease in molecular weight during the crushing process, deterioration of mechanical properties, and chemical recycling methods require a large number of solvents and catalysts, which is difficult to industrialize and cannot meet the needs of high-frequency circuit boards. The heat resistance and electrical properties of the material.

Method used

Through alcoholylation and esterification reactions, the waste polycarbonate is prepared as a polycarbonate oligomer with unsaturated double bonds, and copolymerized with polyphenylene ether resin to form a low dielectric with good heat resistance and electrical properties. The cured substance is cured by free radical polymerization.

Benefits of technology

The high-value utilization of waste polycarbonate is realized, and cured substances compatible with high-frequency circuit board materials are prepared, with excellent heat resistance and electrical properties, meeting environmental protection and high-frequency application needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023092929_14112024_PF_FP_ABST
    Figure CN2023092929_14112024_PF_FP_ABST
Patent Text Reader

Abstract

A polycarbonate oligomer having unsaturated double bonds. The polycarbonate oligomer has a structure as represented by formula (I). The structure does not contain a high-polarity alcohol group, can be cured by means of a free radical polymerization reaction, and has application potential in products such as a high-frequency circuit board. In addition, the polycarbonate oligomer can be copolymerized with a currently widely used polyphenylene ether resin, and the cured product can have good electrical characteristics and heat resistance, which can provide a balanced solution for developing a high-order material and environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Polycarbonate oligomer with unsaturated double bonds, preparation method thereof, curable composition and preparation method of low dielectric curable material Technical Field

[0001] The present disclosure relates to a polycarbonate oligomer having unsaturated double bonds, a preparation method thereof, a curable composition, and a preparation method for a low-dielectric cured product. In particular, the present disclosure relates to a polycarbonate oligomer having unsaturated double bonds that can be copolymerized with a polyphenylene ether resin, a preparation method thereof, a curable composition, and a preparation method for a low-dielectric cured product. Background Art

[0002] Polycarbonate (PC) is a thermoplastic polymer formed by the transesterification of bisphenol A and diphenyl carbonate at high temperatures. Polycarbonate possesses excellent heat resistance and mechanical strength, and is widely used in consumer products such as eyeglass lenses, optical discs, data storage devices, and automotive headlights.

[0003] With the increasing use of polycarbonate, the issue of polycarbonate recycling is gaining increasing attention. Currently, the recycling of discarded polycarbonate products in the market primarily involves physical processing, separating the polycarbonate from the metal components, followed by pulverization, mixing, and high-temperature processing before being transformed into other products. However, the pulverization process reduces the molecular weight of the polycarbonate, resulting in a decrease in the mechanical and other physical properties of the recycled product, significantly limiting its application.

[0004] Many studies are currently exploring chemical recycling methods for polycarbonate waste, most of which involve degradation to recover bisphenol A (BPA) monomer for reuse in polycarbonate synthesis. However, this method requires large amounts of solvents or catalysts and cumbersome purification steps to obtain high-purity BPA. Environmental and cost considerations make this method difficult to commercialize.

[0005] In recent years, demand for consumer electronics has surged, and with it, the demand for circuit boards. For example, Japan already has a precedent for using polycarbonate in electronic materials (e.g., Publication No. TW 202024175A). This patent utilizes polycarbonate oligomers as epoxy hardeners. Copolymerization of the two forms an epoxy resin with excellent heat resistance and electrical properties. This material has a measured dielectric constant (Dk) of 2.68 and a dielectric loss tangent (Df) of 0.0132, making it a promising material for printed circuit boards.

[0006] In response to the high-frequency and high-speed demands of today's high-end circuit boards, SABIC's NORYL™ SA9000 resin has become increasingly mainstream. This is a polyphenylene ether (PPE) oligomer with a difunctional unsaturated group at one end. After free radical polymerization, it exhibits excellent heat resistance and rigidity. Furthermore, because it does not produce polar functional groups after curing, it has a relatively lower dielectric loss tangent and dielectric constant than traditional epoxy resins.

[0007] With growing environmental awareness worldwide, plastic recycling is becoming increasingly important. The European Union has even implemented a ban on general plastic products, requiring some to contain a certain amount of recycled plastic. This trend has also gradually spread to various chemical products, with brands implementing proactive restrictions on raw materials. However, currently, high-end circuit board products are difficult to manufacture using recycled plastics. Coupled with the inherent electrical performance requirements of these products, free radical polymerization curing systems are becoming increasingly popular. Given this, if waste polycarbonate could be modified into short-chain unsaturated resins, it would have the potential to retain excellent electrical properties and heat resistance, and could potentially be used as a recycled raw material in circuit board materials in response to future trends.

[0008] Summary of the Invention

[0009] The purpose of the present disclosure is to provide a method for recycling and preparing oligomers from waste polycarbonate. The prepared oligomers have good copolymerization operability with polyphenylene ether materials widely used in high-frequency circuit boards on the market today, and have excellent heat resistance and electrical properties after curing. This can provide the industry with a high-end circuit board material obtained by high-value recycling of raw materials.

[0010] One embodiment of the present disclosure provides a polycarbonate oligomer having an unsaturated double bond, which has a structure as shown in formula (I):

[0011] wherein R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), (2), (3), (4), (5), (6), (7), (8), or (9):

[0012] wherein X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; Y is a hydrogen atom or a methyl group; a is an integer from 0 to 4; and n is any number from 0 to 30.

[0013] Another embodiment of the present disclosure provides a method for preparing the aforementioned polycarbonate oligomer having an unsaturated double bond, comprising the following steps: performing an alcoholysis step, wherein a polycarbonate is dissolved in a reaction solvent, and a first compound and a first catalyst are added thereto, followed by an alcoholysis reaction, to obtain a reaction solution of a polycarbonate oligomer having a unilaterally unsaturated double bond, wherein the first compound has a structure as shown in formula (II), and the polycarbonate oligomer having a unilaterally unsaturated double bond has a structure as shown in formula (III):

[0014] An esterification step is performed by adding a second compound and a second catalyst to the reaction solution to carry out an esterification reaction to obtain a product to be purified, wherein the second compound has a structure as shown in formula (IV):

[0015] A washing step is performed in which the product to be purified is precipitated and washed with an alcohol solvent to form a product to be dried. A drying step is performed in which the product to be dried is filtered and dried to obtain a polycarbonate oligomer having an unsaturated double bond. wherein R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8), or formula (9):

[0016] wherein X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; Y is a hydrogen atom or a methyl group; a is an integer from 0 to 4; and n is any number from 0 to 30.

[0017] According to the aforementioned preparation method, the molar ratio of the polycarbonate to the first compound may be 1:10 to 1:50.

[0018] According to the aforementioned preparation method, the reaction solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, and cyclohexanone.

[0019] According to the aforementioned preparation method, the first catalyst and the second catalyst can be respectively selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

[0020] According to the aforementioned preparation method, the molar ratio of the first compound to the first catalyst may be 1:0.002 to 1:0.004.

[0021] According to the aforementioned preparation method, in the alcoholysis step, the polycarbonate and the first compound may undergo an alcoholysis reaction at 70° C. to 180° C.

[0022] According to the aforementioned preparation method, the added amount of the first catalyst and the second catalyst may be 10 weight percent to 30 weight percent of the content of the first compound.

[0023] According to the aforementioned preparation method, the molar ratio of the first compound to the second compound may be 1:1 to 1:5.

[0024] According to the aforementioned preparation method, in the esterification step, the polycarbonate oligomer having a unilaterally unsaturated double bond and the second compound can be subjected to an esterification reaction at 70° C. to 100° C.

[0025] Another embodiment of the present disclosure provides a curable composition comprising the aforementioned polycarbonate oligomer having unsaturated double bonds, a polyphenylene ether resin having unsaturated double bonds, a solvent, and a free radical initiator.

[0026] According to the aforementioned curable composition, the mass ratio of the polycarbonate oligomer having unsaturated double bonds to the polyphenylene ether resin having unsaturated double bonds may be 0.1 to 1.

[0027] According to the aforementioned curable composition, the free radical initiator can be selected from the group consisting of peroxides and azo initiators.

[0028] According to the aforementioned curable composition, the amount of the free radical initiator added may be 0.5 weight percent to 3.0 weight percent of the total content of the polycarbonate oligomer having unsaturated double bonds and the polyphenylene ether resin having unsaturated double bonds.

[0029] According to the aforementioned curable composition, the solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, γ-butyrolactone, butanone, cyclohexanone, toluene and xylene.

[0030] Another embodiment of the present disclosure provides a method for preparing a low-dielectric cured product, wherein the low-dielectric cured product is obtained by subjecting the aforementioned curable composition to a curing reaction at a curing temperature, wherein the curing temperature is 140° C. to 250° C.

[0031] Based on this, the present disclosure proposes a method for recycling and reusing waste polycarbonate, which utilizes the principles of alcoholysis and esterification to prepare a bifunctional polycarbonate oligomer with an unsaturated group at the end. The oligomer can be co-cured with materials commonly used in high-frequency circuit boards. The resulting cured product can have good electrical and physical properties, enabling the waste to achieve the goal of high-value recycling while meeting the needs of environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] To make the above and other objects, features, advantages and embodiments of the present disclosure more apparent and understandable, the accompanying drawings are described as follows:

[0033] FIG1 is a flow chart showing the steps of the method for preparing a polycarbonate oligomer having unsaturated double bonds according to the present invention.

[0034]

Description of symbols

[0035] The following will discuss various embodiments of the present disclosure in more detail. However, this embodiment can be an application of various inventive concepts and can be specifically implemented within a variety of specific scopes. The specific embodiments are for illustrative purposes only and are not intended to limit the scope of the disclosure.

[0036] In this disclosure, compound structures are sometimes represented using skeleton formulas. This representation may omit carbon atoms, hydrogen atoms, and carbon-hydrogen bonds. If a functional group is explicitly depicted in a structural formula, the depicted functional group shall prevail.

[0037] In this disclosure, for the sake of brevity and fluency, “a first compound having a structure as shown in formula (II)” is sometimes expressed as “a first compound as shown in formula (II)” or “first compound (II)”, and the representation of other compounds or groups is similar.

[0038] <Polycarbonate oligomer having unsaturated double bonds>

[0039] One embodiment of the present disclosure provides a polycarbonate oligomer having an unsaturated double bond, which has a structure as shown in formula (I):

[0040] wherein R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), (2), (3), (4), (5), (6), (7), (8), or (9):

[0041] wherein X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30, where n represents the degree of polymerization.

[0042] Based on this, the aforementioned polycarbonate oligomers with unsaturated double bonds lack highly polar alcohol groups in their structure and can be cured via free radical polymerization, showing potential for application in products such as high-frequency circuit boards. Polycarbonate oligomers with unsaturated double bonds can be copolymerized with currently popular polyphenylene ether resins, and the resulting cured products exhibit excellent electrical properties and heat resistance.

[0043] <Method for preparing polycarbonate oligomer having unsaturated double bonds>

[0044] 1 is a flowchart of a method 100 for preparing a polycarbonate oligomer having unsaturated double bonds according to the present disclosure. Another embodiment of the present disclosure provides a method 100 for preparing a polycarbonate oligomer having unsaturated double bonds, comprising steps 110, 120, 130, and 140.

[0045] Step 110 is an alcoholysis step, wherein a polycarbonate is dissolved in a reaction solvent, and a first compound and a first catalyst are added thereto, followed by an alcoholysis reaction to obtain a reaction solution of a polycarbonate oligomer having a unilaterally unsaturated double bond, wherein the first compound has a structure as shown in formula (II), and the polycarbonate oligomer having a unilaterally unsaturated double bond has a structure as shown in formula (III):

[0046] Step 120 is an esterification step, in which a second compound and a second catalyst are added to the reaction solution to perform an esterification reaction to obtain a product to be purified, wherein the second compound has a structure as shown in Formula (IV):

[0047] Step 130 is a cleaning step in which the product to be purified is precipitated and cleaned with an alcohol solvent to form a product to be dried.

[0048] Step 140 is a drying step in which the product to be dried is filtered and dried to obtain a polycarbonate oligomer having unsaturated double bonds. In Formulas (II), (III), and (IV), R1, R2, X, X1, X2, Y, a, and n are as defined in the preceding paragraphs and are not further described here.

[0049] The reaction solvent may be selected from the group consisting of N,N-dimethylacetamide (DMAc), N-methylpyrrolidone (NMP), dimethylformamide (DMF), anisole, dimethyl sulfoxide (DMSO), propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, and cyclohexanone.

[0050] The first catalyst and the second catalyst can be respectively selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), and 1,5,7-triazabicyclo[4.4.0]dec-5-ene (TBD).

[0051] The molar ratio of polycarbonate to the first compound can be 1:10 to 1:50, preferably 1:20 to 1:40. The molar ratio of the first compound to the first catalyst can be 1:0.002 to 1:0.004, preferably 1:0.002 to 1:0.003. The amount of the first catalyst and the second catalyst added can be 10 to 30 weight percent of the first compound, preferably 20 to 25 weight percent. The molar ratio of the first compound to the second compound can be 1:1 to 1:5, preferably 1:2.2 to 1:4.4.

[0052] Both the alcoholysis and esterification reactions can be carried out using heat. In the alcoholysis step, the polycarbonate and the first compound can be subjected to an alcoholysis reaction at 70°C to 180°C, preferably 130°C to 150°C. In the esterification step, the polycarbonate oligomer having unilaterally unsaturated double bonds and the second compound can be subjected to an esterification reaction at 70°C to 100°C, preferably 70°C to 90°C.

[0053] For example, if in the polycarbonate oligomer having a unilaterally unsaturated double bond represented by formula (III), X has a structure as represented by formula (1), X1, X2, and Y are methyl groups, R1 is a hydrogen atom, and R2 is an ethylidene group, the prepared polycarbonate oligomer having an unsaturated double bond has a structure as represented by formula (Ia), and the polycarbonate oligomer having a unilaterally unsaturated double bond has a structure as represented by formula (III-a):

[0054] <Curable Composition>

[0055] Another embodiment of the present disclosure provides a curable composition comprising the aforementioned polycarbonate oligomer having unsaturated double bonds, a polyphenylene ether resin having unsaturated double bonds, a solvent, and a free radical initiator. The curable composition can undergo a curing reaction at high temperature to produce a low-dielectric cured product. The curable composition can be prepared at a mixing temperature of 50°C to 100°C, preferably 70°C to 90°C.

[0056] The free radical initiator can be selected from the group consisting of peroxides and azo initiators, and the solvent can be selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, γ-butyrolactone, butanone, cyclohexanone, toluene and xylene.

[0057] The mass ratio of the polycarbonate oligomer having unsaturated double bonds to the polyphenylene ether resin having unsaturated double bonds can be 0.1 to 1. The amount of the free radical initiator added can be 0.5 to 3.0 weight percent, preferably 1 to 2.5 weight percent, of the total content of the polycarbonate oligomer having unsaturated double bonds and the polyphenylene ether resin having unsaturated double bonds. Too little free radical initiator can result in incomplete curing, resulting in a decrease in the physical properties of the curable composition. Too much free radical initiator can result in a decrease in the electrical properties of the curable composition.

[0058] <Method for Preparing Low Dielectric Cured Material>

[0059] Another embodiment of the present disclosure provides a method for preparing a low-dielectric cured product, wherein the low-dielectric cured product is obtained by subjecting the aforementioned curable composition to a curing reaction at a curing temperature, wherein the curing temperature is 140°C to 250°C, preferably 180°C to 220°C, but is not limited thereto. Those skilled in the art of the present disclosure can select an appropriate curing temperature, such as 140°C to 180°C, 140°C to 220°C, 150°C to 250°C, etc.

[0060] The present disclosure is further illustrated by the following specific embodiments, which are intended to facilitate those skilled in the art to which the present disclosure relates, so that they can fully utilize and practice the present disclosure without excessive interpretation. These embodiments should not be regarded as limiting the scope of the present disclosure, but are intended to illustrate how to implement the materials and methods of the present disclosure.

[0061] <Preparation of Polycarbonate Oligomer Having Unsaturated Double Bonds>

[0062] <Example 1>

[0063] Take 100g (4×10-3 10.07 g (0.082 mole, calculated as Mn) of polycarbonate ester pellets (purchased from Chi Mei Industrial, product code PC-122, Mn = 24400, Mw = 45488) were completely dissolved in 150 g of DMAc at 150°C. Then 10.07 g (0.082 mole) of hydroxyethyl methacrylate was added dropwise to the above solution, mixed evenly, and 0.026 g (1.69×10 -4 mole) of DBU, reacted for 5 hours, cooled, poured into methanol for washing, vacuum filtered, and dried in a vacuum oven at 78°C to obtain a compound represented by formula (III-a). The product code is HEPC, and the yield is about 71%. GPC analysis of the product shows Mn = 2721, Mw = 4061.

[0064] <Example 2>

[0065] The first half of the process was the same as in Example 1, except that the reaction mixture was not rinsed with methanol after completion. The temperature was lowered to 70°C, and 2.33 g (22 weight percent of the content of the first compound (II)) of DBU and 27.81 g (0.180 mole) of methacrylic anhydride were added in sequence. The reaction was carried out at 70°C for 6 hours. After completion, the mixture was rinsed with methanol, filtered, and dried in a vacuum oven at 78°C to obtain a white powder of Formula (Ia). The product was designated HAPC-1 with a yield of approximately 73.6%. GPC analysis of the product revealed Mn = 2366 and Mw = 4137.

[0066] <Example 3>

[0067] Take 100g (4×10 -3 16.51 g (0.127 mole, calculated as Mn) of polycarbonate ester pellets (purchased from Chi Mei Industrial, product code PC-122, Mn = 24400, Mw = 45488) were completely dissolved in 150 g of DMAc at 150°C. Then 16.51 g (0.127 mole) of hydroxyethyl methacrylate was added dropwise to the above solution. After uniform mixing, 0.038 g (2.54×10 -4 The reaction mixture was cooled to 70°C and 3.63 g (22 weight percent of the first compound (II)) of DBU and 43.03 g (0.279 mole) of methacrylic anhydride were added in sequence. The mixture was reacted at 78°C for 6 hours. After the reaction, the mixture was washed with methanol, filtered, and dried in a vacuum oven at 78°C to obtain a white powder of formula (Ia). The product was designated HAPC-1.5 with a yield of approximately 59%. GPC analysis of the product revealed Mn = 2673 and Mw = 4479.

[0068] <Example 4>

[0069] Take 100 g (3.8 × 10 -3 150 g (0.115 mole, calculated as Mn) of recycled polycarbonate ester pellets (purchased from Chi Mei Industrial, product code GC-122B, Mn = 26099, Mw = 47827) were completely dissolved in 150 g (0.115 mole) of hydroxyethyl methacrylate at 150°C. 14.97 g (0.115 mole) of hydroxyethyl methacrylate was added dropwise to the above solution, mixed evenly, and then 0.035 g (2.30 × 10 -4 The reaction mixture was cooled to 70°C and 3.29 g (22 weight percent of the first compound (II)) of DBU and 39.00 g (0.253 mole) of methacrylic anhydride were added in sequence. The mixture was reacted at 80°C for 6 hours. After the reaction, the mixture was washed with methanol, filtered, and dried in a vacuum oven at 78°C to obtain a gray powder of formula (Ia). The product was designated HAGC-1.5 with a yield of approximately 70.7%. GPC analysis of the product revealed Mn = 2658 and Mw = 4885.

[0070] <Example 5>

[0071] Take 100 g (3.8 × 10 -3 150 g of DMAc (Mn=26099, Mw=47827) was completely dissolved in 150 g of DMAc at 150°C. 19.91 g (0.153 mole, calculated as Mn) of recycled polycarbonate ester pellets (purchased from Chi Mei Industrial, product code GC-122B, Mn=26099, Mw=47827) was added dropwise to the above solution at 150°C. After uniform mixing, 0.046 g (3.02×10 -4 The reaction mixture was cooled to 80°C and 4.38 g (22 weight percent of the first compound (II)) of DBU and 51.89 g (0.337 mole) of methacrylic anhydride were added in sequence. The mixture was reacted at 80°C for 6 hours. After the reaction, the mixture was washed with methanol, filtered, and dried in a vacuum oven at 78°C to obtain a gray powder of formula (Ia). The product was designated HAGC-2 with a yield of approximately 61.9%. GPC analysis of the product revealed Mn = 2257 and Mw = 4445.

[0072] <Comparative Example 1>

[0073] Take 100g (4×10 -3Polycarbonate ester pellets (purchased from Chi Mei Industrial, product code PC-122, Mn = 24400, Mw = 45488) (calculated as Mn) were dissolved in 150 g of DMAc and heated to 120°C for dissolution. After dissolution, 7.28 g (0.0846 mole) of methacrylic acid and 0.129 g (2.47 mole) of DBU were added dropwise. The reaction was allowed to proceed for 3 hours. After completion, the mixture was cooled, washed with methanol, filtered, and dried in a vacuum oven at 78°C to obtain a white powder. The product code is MAPC. The resulting product has poor solubility in organic solvents, presumably due to free radical crosslinking during the reaction, making further handling and analysis impossible.

[0074] <Curing Reaction of Curable Composition>

[0075] The aforementioned polycarbonate oligomer having unsaturated double bonds can be further prepared into a curable composition and subjected to a curing reaction. Specifically, the aforementioned polycarbonate oligomer having unsaturated double bonds, a polyphenylene ether resin having unsaturated double bonds, a solvent, and a free radical initiator can be mixed to form a curable composition. The polycarbonate oligomer, polyphenylene ether resin, solvent, and free radical initiator can then form a prepolymer containing the curable composition. The details are as described in the previous paragraph and will not be further elaborated here.

[0076] Next, the polycarbonate oligomer having unsaturated double bonds and the polyphenylene ether resin can be cross-linked and cured under the catalysis of a free radical initiator. The curing reaction can be completed by heating the curable composition. Specific examples are provided below to illustrate this.

[0077] <Example 6>

[0078] Take 0.24 g of polycarbonate oligomer HAPC-1 with unsaturated double bonds and 0.96 g of polyphenylene ether resin NORYL TM SA9000 (available from SABIC) was dissolved in 2.856 g of cyclohexanone and heated at 80°C. After mixing, 0.024 g (2.0 weight percent of the total content of the polycarbonate oligomer and polyphenylene ether resin) of dicumyl peroxide was added as a free radical initiator. After stirring evenly, a mixed prepolymer was obtained. This prepolymer was then baked out of an 80°C oven for 12 hours to partially remove the solvent. The subsequent curing reaction was then gradually heated from 140°C to 220°C to obtain a low-dielectric cured product.

[0079] <Example 7>

[0080] The preparation steps of Example 7 are the same as those of Example 6, except that the amount of the polycarbonate oligomer HAPC-1 with unsaturated double bonds is changed to 0.36 g, and the polyphenylene ether resin NORYL TM The dosage of SA9000 was changed to 0.84 g.

[0081] <Example 8>

[0082] The preparation steps of Example 8 are the same as those of Example 6, except that the amount of the polycarbonate oligomer HAPC-1 with unsaturated double bonds is changed to 0.48 g, and the polyphenylene ether resin NORYL TM The dosage of SA9000 was changed to 0.72 g.

[0083] <Example 9>

[0084] The preparation steps of Example 9 are the same as those of Example 6, except that the amount of the polycarbonate oligomer HAPC-1 with unsaturated double bonds is changed to 0.60 g, and the polyphenylene ether resin NORYL TM The dosage of SA9000 was changed to 0.60 g.

[0085] <Comparative Example 2>

[0086] Take 0.24g of polycarbonate oligomer HEPC with unsaturated double bonds and 0.96g of polyphenylene ether resin NORYL TM SA9000 (available from SABIC) was dissolved in 2.856 g of cyclohexanone and heated at 80°C. After mixing, 0.024 g (2.0 weight percent of the total content of the polycarbonate oligomer and polyphenylene ether resin) of dicumyl peroxide was added as a free radical initiator. After stirring, a mixed prepolymer was obtained. The mixture was placed in an 80°C oven for 12 hours to partially remove the solvent. The subsequent curing reaction was followed by gradually increasing the temperature from 140°C to 220°C. After curing, the product of Comparative Example 2 exhibited severe shrinkage and phase separation.

[0087] <Comparative Example 3>

[0088] The preparation steps of Comparative Example 3 are the same as those of Comparative Example 2, except that the amount of the polycarbonate oligomer HEPC with unsaturated double bonds is changed to 0.36 g, and the polyphenylene ether resin NORYL TM The amount of SA9000 was changed to 0.84 g. After the curing reaction, the product of Comparative Example 3 had severe shrinkage and phase separation.

[0089] <Comparative Example 4>

[0090] The preparation steps of Comparative Example 4 are the same as those of Comparative Example 2, except that the amount of the polycarbonate oligomer HEPC with unsaturated double bonds is changed to 0.48 g, and the polyphenylene ether resin NORYL TM The amount of SA9000 was changed to 0.72 g. After the curing reaction, the product of Comparative Example 4 had severe shrinkage and phase separation.

[0091] <Comparative Example 5>

[0092] The preparation steps of Comparative Example 5 are the same as those of Comparative Example 2, except that the amount of the polycarbonate oligomer HEPC with unsaturated double bonds is changed to 0.60 g, and the polyphenylene ether resin NORYL TM The amount of SA9000 was changed to 0.60 g. After the curing reaction, the product of Comparative Example 5 had severe shrinkage and phase separation.

[0093] <Property Test of Low Dielectric Cured Material>

[0094] The low dielectric cured products obtained in Examples 6 to 9 were measured by differential scanning calorimeter (DSC) to determine their glass transition temperatures (T g ) were measured at a heating rate of 10°C / min, and the measurement results are listed in Table 1 below.

[0095] Based on the above results, the polycarbonate oligomers with unsaturated double bonds synthesized in the present disclosure do exhibit good reactivity with polyphenylene ether resins, reacting and curing readily under the aforementioned oven conditions. The two exhibit excellent compatibility and film-forming properties, facilitating easy processing. Furthermore, the polycarbonate oligomers with unsaturated double bonds synthesized in the present disclosure can be used in combination with polyphenylene ether resins in the aforementioned ratios.

[0096] Furthermore, in terms of heat resistance, the glass transition temperature decreases as the amount of polycarbonate oligomer with unsaturated double bonds added increases, but it can still maintain good heat resistance, sufficient to meet various application requirements.

[0097] The following will further conduct electrical tests on the low dielectric curing materials of Examples 6 to 9 to obtain their dielectric properties. The frequency used in the test is 10 GHz, and the dielectric constant (D k ) and dielectric loss tangent (D f ) are listed in Table 2 below.

[0098] According to the above experimental results, compared with the SA9000 cured product cured by pure polyphenylene ether resin, the low dielectric cured product cured by adding the polycarbonate oligomer with unsaturated double bonds synthesized in the present disclosure has better D k Performance, but in D f In addition, the above results show that as the amount of polycarbonate oligomer with unsaturated double bonds increases, the dielectric properties of the low dielectric curing material can be further improved, making D f Return to the best performance and obtain better D than SA9000 cured product k The performance shows the potential of the low dielectric cured product disclosed in the present invention in high frequency applications.

[0099] In summary, the present disclosure provides a method for recycling and reusing waste polycarbonate, which is to use a monoalcohol compound containing a double bond structure to perform alcoholysis on the polycarbonate, and after the polycarbonate is prepared into an oligomer, the residual terminal phenol group is modified to obtain a polycarbonate oligomer with unsaturated double bonds, and all of its ends have unsaturated double bonds. The polycarbonate oligomer with unsaturated double bonds is compatible with the polyphenylene ether resin in an organic solvent, and the two can be cured by free radical polymerization to prepare a sample. During the sample preparation process, the ratio of the polycarbonate oligomer with unsaturated double bonds and the polyphenylene ether resin can be adjusted to achieve the desired physical and electrical properties, and the resulting low-dielectric cured product can have good dielectric loss tangent and dielectric constant performance, and is expected to be implemented on high-frequency circuit board materials.

[0100] The above examples are merely illustrative of the principles of this disclosure and are not intended to limit its scope. For example, other alcohols or polycarbonate resins can be used and similar reactions can be used to produce polycarbonate oligomers with unsaturated double bonds of varying chemical structures. Therefore, any modifications or extensions of the above examples are intended to fall within the scope of this disclosure.

Claims

1. A polycarbonate oligomer having unsaturated double bonds, characterized in that: The polycarbonate oligomer having unsaturated double bonds has a structure as shown in formula (I): Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9): Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; wherein Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30.

2. A method for preparing a polycarbonate oligomer having unsaturated double bonds as claimed in claim 1, characterized in that: Include: The alcoholysis step is to dissolve a polycarbonate in a reaction solvent, add a first compound and a first catalyst, and then perform alcoholysis reaction to obtain a reaction solution of a polycarbonate oligomer having a unilateral unsaturated double bond, wherein the first compound has a structure as shown in formula (II), and the polycarbonate oligomer having a unilateral unsaturated double bond has a structure as shown in formula (III): An esterification step is performed by adding a second compound and a second catalyst into the reaction solution to perform an esterification reaction to obtain a substance to be purified, wherein the second compound has a structure as shown in formula (IV): Performing a washing step, which is to wash the object to be purified by precipitation with an alcohol solvent to form an object to be dried; and Performing a drying step, filtering and drying the substance to be dried to obtain the polycarbonate oligomer having unsaturated double bonds; Wherein, R1 is a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an allyl group, an alkoxy group having 1 to 6 carbon atoms, an aromatic group having 6 to 12 carbon atoms, or a halogen atom; R2 is an alkyl group having 1 to 12 carbon atoms; and X is a single bond, a cycloalkyl group having 3 to 12 carbon atoms, or a structure represented by formula (1), formula (2), formula (3), formula (4), formula (5), formula (6), formula (7), formula (8) or formula (9): Wherein, X1 and X2 are each independently a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, or an aromatic group having 6 to 12 carbon atoms; wherein Y is a hydrogen atom or a methyl group, a is an integer from 0 to 4, and n is any number from 0 to 30.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the polycarbonate to the first compound is 1:10 to 1:

50.

4. The preparation method according to claim 2, characterized in that: The reaction solvent is selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate and cyclohexanone.

5. The preparation method according to claim 2, characterized in that: The first catalyst and the second catalyst are respectively selected from the group consisting of 4-dimethylaminopyridine, imidazole, 2-methylimidazole, 2-phenylimidazole, 2-ethyl-4-methylimidazole, 1,8-diazabicyclo[5.4.0]undec-7-ene and 1,5,7-triazabicyclo[4.4.0]dec-5-ene.

6. The preparation method according to claim 2, characterized in that: The molar ratio of the first compound to the first catalyst is 1:0.002 to 1:0.

004.

7. The preparation method according to claim 2, characterized in that: In the alcoholysis step, the polycarbonate and the first compound undergo an alcoholysis reaction at 70° C. to 180° C.

8. The preparation method according to claim 2, characterized in that: The added amount of the first catalyst and the second catalyst is 10 weight percent to 30 weight percent of the content of the first compound.

9. The preparation method according to claim 2, characterized in that: The molar ratio of the first compound to the second compound is 1:1 to 1:

5.

10. The preparation method according to claim 2, characterized in that: In the esterification step, the polycarbonate oligomer having a unilateral unsaturated double bond and the second compound are subjected to an esterification reaction at 70° C. to 100° C.

11. A curable composition, characterized in that The curable composition comprises the polycarbonate oligomer having unsaturated double bonds as claimed in claim 1 , a polyphenylene ether resin having unsaturated double bonds, a solvent and a free radical initiator.

12. The curable composition according to claim 11, wherein The mass ratio of the polycarbonate oligomer having unsaturated double bonds to the polyphenylene ether resin having unsaturated double bonds is 0.1 to 1.

13. The curable composition according to claim 11, wherein The free radical initiator is selected from the group consisting of peroxides and azo initiators.

14. The curable composition according to claim 11, wherein The added amount of the free radical initiator is 0.5 weight percent to 3.0 weight percent of the total content of the polycarbonate oligomer having unsaturated double bonds and the polyphenylene ether resin having unsaturated double bonds.

15. The curable composition according to claim 11, wherein The solvent is selected from the group consisting of N,N-dimethylacetamide, N-methylpyrrolidone, dimethylformamide, anisole, dimethyl sulfoxide, propylene glycol methyl ether acetate, propylene glycol methyl ether propionate, γ-butyrolactone, butanone, cyclohexanone, toluene and xylene.

16. A method for preparing a low dielectric cured product, characterized in that: A low dielectric cured product is obtained by subjecting the curable composition as claimed in claim 11 to a curing reaction at a curing temperature, wherein the curing temperature is 140° C. to 250° C.

Citation Information

Patent Citations

  • Epoxy resin composition

    TW202024175A

  • Liquid crystal display device and liquid crystal composition included therein

    CN108219803A

  • Coating composition

    CN110437668A

  • Production of liquid crystal optical device and method of driving the same

    JP2001056482A

  • Polymerizable liquid crystal composition and optically anisotropic film

    JP2013071945A