Carbon black modified polyester fiber and preparation method therefor
Through the preparation method of carbon black modified polyester fiber, combined with copolyester, modified polyester and crystallization accelerator, the problem of insufficient durability and environmental protection of traditional polyester fibers is solved, and high wear resistance, anti-static and Its ultraviolet resistance and enhances the environmental protection and application value of the material.
Patent Information
- Application Number
- PCT/CN2023/093302
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-14
AI Technical Summary
Traditional polyester fibers have problems such as insufficient durability and service life and poor environmental protection, which limits their application scope.
The preparation method of carbon black modified polyester fiber is adopted, and the material content and mixing ratio are controlled by the combination of copolyester, modified polyester, crystallization accelerator and regenerated polyester, and the carbon black is evenly dispersed by mechanical or ultrasonic waves. Fibers with excellent physical and chemical properties were prepared by extrusion and hot press bonding processes.
It improves the wear resistance, anti-static, ultraviolet radiation and other characteristics of copolyester, and has good softness and breathability, enhancing the sustainability and environmental protection of the material.
Smart Images

Figure CN2023093302_14112024_PF_FP_ABST
Abstract
Description
Carbon black modified polyester fiber and preparation method thereof Technical Field
[0001] The present invention relates to the field of fiber technology, in particular to a carbon black modified polyester fiber and a preparation method thereof. Background Art
[0002] Polyester fiber is a synthetic fiber material widely used in textiles and nonwovens due to its excellent mechanical properties, chemical stability, breathability, and softness. However, conventional polyester fibers suffer from issues such as insufficient durability and service life, as well as poor environmental performance, which limit their application. While existing technologies have achieved some success in modifying polyester fibers using additives and surface treatments, they still face challenges such as insufficient durability and service life, as well as poor environmental performance.
[0003] In view of this, the present invention is proposed. Summary of the Invention
[0004] The technical problem to be solved by the present invention is to overcome the shortcomings of the existing technology and provide a carbon black modified polyester fiber and a preparation method thereof, which improves the wear resistance, antistatic, anti-ultraviolet radiation and other properties of the copolyester and has good softness and breathability.
[0005] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is:
[0006] The invention discloses a carbon black modified polyester fiber, which consists of copolyester, modified polyester, a crystallization accelerator and recycled polyester.
[0007] In a preferred embodiment of any of the above schemes, the mass percentage of the copolyester is 15-16%, the mass percentage of the modified polyester is 20-30%, the mass percentage of the crystallization accelerator is 14-20%, and the mass percentage of the recycled polyester is 15-20%.
[0008] In a preferred embodiment of any of the above schemes, the modified polyester is a polyester containing carbon black.
[0009] In a preferred embodiment of any of the above schemes, the copolyester contains a side-group-containing aliphatic diol structural unit with no more than 8 carbon atoms.
[0010] In a second aspect, a method for preparing a carbon black modified polyester fiber comprises the following steps:
[0011] Select and screen the copolyester raw materials, dissolve the copolyester raw materials in an appropriate amount of solvent at room temperature, and stir evenly;
[0012] Add 14-20% of crystallization accelerator to the copolyester;
[0013] Add 20-30% of modified polyester containing carbon black and mix thoroughly so that the modified polyester is evenly dispersed in the copolyester to form a mixture;
[0014] preparing the mixture into a polyester sheet through an extrusion process;
[0015] The recycled polyester sheet and the polyester sheet are stacked layer by layer in a certain proportion, and heated at a certain temperature and pressure to bond the recycled polyester sheet and the polyester sheet into one;
[0016] After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths.
[0017] In a preferred embodiment of any of the above schemes, the diameter of the polyester sheet is 1 to 3 mm.
[0018] In a preferred embodiment of any of the above schemes, 20-30% of a modified polyester containing carbon black is added and fully mixed so that the modified polyester is uniformly dispersed in the copolyester to form a mixture, comprising the following steps:
[0019] Select modified polyester material and confirm that the carbon black content is 20-30%;
[0020] Adding the modified polyester to the copolyester raw material, and adding a corresponding amount of solvent to fully mix the modified polyester and the copolyester raw material;
[0021] Gradually add carbon black into the modified polyester, and use a mechanical stirrer or ultrasonic wave to fully disperse the carbon black in the modified polyester;
[0022] The modified polyester and copolyester raw materials that are fully mixed are mixed, and an appropriate amount of solvent is added again. After mixing evenly, the modified polyester and copolyester raw materials are fully mixed using a machine or ultrasonic wave to form a mixture.
[0023] In a preferred embodiment of any of the above schemes, when the modified polyester and the copolyester raw material are fully mixed, the stirring speed is 100 to 500 rpm and the stirring time is 1 to 2 hours.
[0024] In a preferred embodiment of any of the above schemes, the mixture is prepared into a polyester sheet by an extrusion process, comprising the following steps:
[0025] Pour the mixture into the hopper of the extruder and adjust the temperature, speed and extrusion pressure of the extruder to gradually heat up and melt the mixture;
[0026] The mixture injected into the extruder is heated and melted and then extruded into the extruder head to form a plastic strip of a certain shape and size;
[0027] The strip is heated and extruded, and then formed and shaped by a die head mold to form a polyester sheet.
[0028] In a preferred embodiment of any of the above schemes, the recycled polyester sheet and the polyester sheet are stacked layer by layer in a certain ratio, and are heated at a certain temperature and pressure to bond the recycled polyester sheet and the polyester sheet into one, comprising the following steps:
[0029] Prepare recycled polyester sheets and polyester sheets, and cut and stack them according to the required ratio;
[0030] Place the stacked adhesive materials into the hot press and adjust the temperature and pressure;
[0031] Under certain temperature and time, pressure is applied to the interface between the recycled polyester sheet and the polyester sheet, so that the recycled polyester sheet and the polyester sheet are fully in contact and bonded;
[0032] After the heating process, the hot press was turned off and cooled to room temperature.
[0033] After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art.
[0034] The recycled polyester sheet and the polyester sheet are stacked layer by layer in a certain proportion and heated at a certain temperature and pressure to bond the recycled polyester sheet and the polyester sheet into one. After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths, which improves the wear resistance, antistatic, anti-ultraviolet radiation and other properties of the copolyester, and has good softness and breathability.
[0035] The specific embodiments of the present invention will be described in further detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation of the present application. Some specific embodiments of the present application will be described in detail in an illustrative and non-restrictive manner with reference to the drawings. The same reference numerals in the drawings indicate the same or similar components or parts. It should be understood by those skilled in the art that these drawings are not necessarily drawn to scale. In the drawings:
[0037] FIG1 is a schematic diagram of the preparation method of the carbon black modified polyester fiber of the present invention.
[0038] It should be noted that these drawings and text descriptions are not intended to limit the scope of the present invention in any way, but rather to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. The elements in the drawings are schematic and not drawn to scale. DETAILED DESCRIPTION
[0039] In order to enable those skilled in the art to better understand the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the accompanying drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of this application.
[0040] The following examples of the present application take carbon black modified polyester fiber and its preparation method as an example to illustrate the scheme of the present application in detail, but this example does not limit the scope of protection of the present application.
[0041] Example 1
[0042] The present invention provides a method for preparing carbon black modified polyester fiber, the preparation method comprising the following steps:
[0043] Step 11, selecting 15% of copolyester and screening, dissolving the copolyester raw material in an appropriate amount of solvent at room temperature, and stirring evenly;
[0044] Step 12, adding 14% of a crystallization accelerator to the copolyester;
[0045] Step 13: Select a modified polyester material and confirm that the carbon black content thereof is 20%; add the modified polyester to the copolyester raw material, and add a corresponding amount of solvent to fully mix the modified polyester and the copolyester raw material, stirring at a speed of 100 to 500 rpm for 1 to 2 hours; gradually add carbon black to the modified polyester, and use a mechanical stirrer or ultrasonic wave to fully disperse the carbon black in the modified polyester; mix the fully mixed modified polyester and copolyester raw materials, and add an appropriate amount of solvent again. After mixing evenly, use a mechanical stirrer or ultrasonic wave to fully mix the modified polyester and copolyester raw materials to form a mixture;
[0046] Step 14: injecting the mixture into the hopper of an extruder, and adjusting the temperature, speed, and extrusion pressure of the extruder to gradually heat and melt the mixture; the mixture injected into the extruder is heated and melted, and then extruded into the die of the extruder to form a plastic strip of a certain shape and size; the strip is heated and extruded, and then formed and shaped by the die of the die to form a polyester sheet;
[0047] Step 15: Prepare recycled polyester sheets and polyester sheets, cut and stack them according to the required ratio; place the stacked adhesive material into a hot press, adjust the temperature and pressure; apply pressure to the interface between the recycled polyester sheet and the polyester sheet at a certain temperature and time to ensure full contact and adhesion between the recycled polyester sheet and the polyester sheet; after the heating treatment, close the hot press and cool to room temperature. The diameter of the polyester sheet is 1 mm.
[0048] Step 16: After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths.
[0049] In an embodiment of the present invention, a copolyester raw material is selected and screened; the copolyester raw material is dissolved in an appropriate amount of solvent at room temperature, and a crystallization accelerator is added; a modified polyester material with a carbon black content of 20% is selected and added to the copolyester raw material, and the carbon black is fully dispersed in the modified polyester using a mechanical stirrer or ultrasound; the modified polyester and the copolyester raw material are mixed to form a mixture; the mixture is injected into an extruder, and the temperature, speed and extrusion pressure of the extruder are controlled to heat and melt the mixture; a polyester sheet is formed by extrusion and molding; recycled polyester sheets and polyester sheets are prepared, cut and stacked according to the required ratio, and placed in a hot press to bond the recycled polyester sheet and the polyester sheet together; the bonded carbon black modified polyester fiber is cooled and cut into appropriate lengths.
[0050] The present invention combines carbon black-modified polyester with copolyester, and then extrudes and bonds them together to create a polyester fiber with a desired shape and size. The addition of an appropriate amount of solvent facilitates the mixing of the modified polyester and copolyester, improving the uniformity of the mixture. A crystallization accelerator promotes crystallization of the copolyester, enhancing the strength and stability of the polyester sheet. The stacking and bonding of recycled polyester and polyester enhances the material's sustainability and environmental friendliness.
[0051] Example 2
[0052] The present invention provides a method for preparing carbon black modified polyester fiber, the preparation method comprising the following steps:
[0053] Step 11, selecting 15.2% of copolyester and screening it, dissolving the copolyester raw material in an appropriate amount of solvent at room temperature, and stirring evenly;
[0054] Step 12, adding 15% of a crystallization accelerator to the copolyester;
[0055] Step 13: Select a modified polyester material and confirm that the carbon black content thereof is 21%; add the modified polyester to the copolyester raw material, and add a corresponding amount of solvent to fully mix the modified polyester and the copolyester raw material, stirring at a speed of 100 to 500 rpm for 1 to 2 hours; gradually add carbon black to the modified polyester, and use a mechanical stirrer or ultrasonic wave to fully disperse the carbon black in the modified polyester; mix the fully mixed modified polyester and copolyester raw materials, and add an appropriate amount of solvent again. After mixing evenly, use a mechanical stirrer or ultrasonic wave to fully mix the modified polyester and copolyester raw materials to form a mixture;
[0056] Step 14: injecting the mixture into the hopper of an extruder, and adjusting the temperature, speed, and extrusion pressure of the extruder to gradually heat and melt the mixture; the mixture injected into the extruder is heated and melted, and then extruded into the die of the extruder to form a plastic strip of a certain shape and size; the strip is heated and extruded, and then formed and shaped by the die of the die to form a polyester sheet;
[0057] Step 15: Prepare recycled polyester sheets and polyester sheets, cut and stack them according to the required ratio; place the stacked adhesive material into a hot press, adjust the temperature and pressure; apply pressure to the interface between the recycled polyester sheet and the polyester sheet at a certain temperature and time to ensure full contact and adhesion between the recycled polyester sheet and the polyester sheet; after the heating treatment, close the hot press and cool to room temperature. The diameter of the polyester sheet is 1.2 mm.
[0058] Step 16: After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths.
[0059] In this embodiment of the present invention, a raw material containing 15.2% copolyester and a modified polyester with a confirmed carbon black content of 21% is selected. The copolyester raw material is dissolved in an appropriate amount of solvent at room temperature, and a crystallization accelerator is added to ensure uniform mixing. The modified polyester is added to the copolyester raw material, and a corresponding amount of solvent is added to ensure thorough mixing. Carbon black is gradually added to the modified polyester using a mechanical stirrer or ultrasonic stirring to ensure thorough dispersion. The thoroughly mixed modified polyester and copolyester raw materials are then mixed again and mechanically or ultrasonically to form a mixture. The mixture is injected into the hopper of an extruder, and the temperature, speed, and extrusion pressure of the extruder are adjusted to gradually heat and melt the mixture. After extrusion and molding, a polyester sheet is formed. Recycled polyester sheet and polyester sheet are prepared, cut and stacked according to the desired ratio, and placed in a hot press to bond the recycled polyester sheet and polyester sheet together. The bonded carbon black-modified polyester fiber is cooled and cut into appropriate lengths. The significance and effect of this preparation method is that, through the first, second, and third steps, the copolyester and modified polyester are thoroughly mixed and the carbon black is evenly dispersed. In the fourth step, the mixture is injected into an extruder, where it is heated and melted before being extruded into the extruder's die, forming a plastic strip of a specific shape and size. This strip is then formed and shaped in the die's die to form a polyester sheet. In the fifth step, recycled polyester sheets and polyester sheets are prepared, cut and stacked according to the required proportions, and bonded together. The sheets are then placed in a hot press, where pressure is applied to the interface of the recycled polyester sheet and polyester sheet at a specific temperature and time to ensure full contact and bonding. Finally, the fibers are cooled and cut to obtain bonded carbon black-modified polyester fibers of appropriate length. The fibers produced using this method possess excellent physical and chemical properties and application value, such as strength, stability, and corrosion resistance. Furthermore, the use of recycled polyester can improve the material's sustainability and environmental friendliness.
[0060] Example 3
[0061] The present invention provides a method for preparing carbon black modified polyester fiber, the preparation method comprising the following steps:
[0062] Step 11, selecting 15.8% of copolyester and screening, dissolving the copolyester raw material in an appropriate amount of solvent at room temperature, and stirring evenly;
[0063] Step 12, adding 16% of a crystallization accelerator to the copolyester;
[0064] Step 13: Select a modified polyester material and confirm that the carbon black content thereof is 22%; add the modified polyester to the copolyester raw material, and add a corresponding amount of solvent to fully mix the modified polyester and the copolyester raw material, stirring at a speed of 100 to 500 rpm for 1 to 2 hours; gradually add carbon black to the modified polyester, and use a mechanical stirrer or ultrasonic wave to fully disperse the carbon black in the modified polyester; mix the fully mixed modified polyester and copolyester raw materials, and add an appropriate amount of solvent again. After mixing evenly, use a mechanical stirrer or ultrasonic wave to fully mix the modified polyester and copolyester raw materials to form a mixture;
[0065] Step 14: injecting the mixture into the hopper of an extruder, and adjusting the temperature, speed, and extrusion pressure of the extruder to gradually heat and melt the mixture; the mixture injected into the extruder is heated and melted, and then extruded into the die of the extruder to form a plastic strip of a certain shape and size; the strip is heated and extruded, and then formed and shaped by the die of the die to form a polyester sheet;
[0066] Step 15: Prepare recycled polyester sheets and polyester sheets, cut and stack them according to the required ratio; place the stacked adhesive material into a hot press, adjust the temperature and pressure; apply pressure to the interface between the recycled polyester sheet and the polyester sheet at a certain temperature and time to ensure full contact and adhesion between the recycled polyester sheet and the polyester sheet; after the heating treatment, close the hot press and cool to room temperature. The diameter of the polyester sheet is 1.5 mm.
[0067] Step 16: After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths.
[0068] The present invention utilizes a combination of copolyester and modified polyester. By controlling the material content and mixing ratio, and adding a crystallization accelerator, the copolyester and modified polyester are thoroughly mixed to form a uniform mixture. Simultaneously, carbon black is evenly dispersed in the modified polyester through mechanical or ultrasonic addition. The mixture is extruded and formed using an extruder to produce a polyester sheet. Finally, a hot press is used for bonding, tightly bonding the recycled polyester and polyester together, forming a carbon black-modified polyester fiber with excellent physical properties and corrosion resistance.
[0069] Example 4
[0070] The present invention provides a method for preparing carbon black modified polyester fiber, the preparation method comprising the following steps:
[0071] Step 11, selecting and screening 16% of copolyester, dissolving the copolyester raw material in an appropriate amount of solvent at room temperature, and stirring evenly;
[0072] Step 12, adding 20% of a crystallization accelerator to the copolyester;
[0073] Step 13: Select a modified polyester material and confirm that the carbon black content thereof is 30%; add the modified polyester to the copolyester raw material, and add a corresponding amount of solvent to fully mix the modified polyester and the copolyester raw material, stirring at a speed of 100 to 500 rpm for 1 to 2 hours; gradually add carbon black to the modified polyester, and use a mechanical stirrer or ultrasonic wave to fully disperse the carbon black in the modified polyester; mix the fully mixed modified polyester and copolyester raw materials, and add an appropriate amount of solvent again. After mixing evenly, use a mechanical stirrer or ultrasonic wave to fully mix the modified polyester and copolyester raw materials to form a mixture;
[0074] Step 14: injecting the mixture into the hopper of an extruder, and adjusting the temperature, speed, and extrusion pressure of the extruder to gradually heat and melt the mixture; the mixture injected into the extruder is heated and melted, and then extruded into the die of the extruder to form a plastic strip of a certain shape and size; the strip is heated and extruded, and then formed and shaped by the die of the die to form a polyester sheet;
[0075] Step 15: Prepare recycled polyester sheets and polyester sheets, cut and stack them according to the required ratio; place the stacked adhesive material into a hot press, adjust the temperature and pressure; apply pressure to the interface between the recycled polyester sheet and the polyester sheet at a certain temperature and time to ensure full contact and adhesion between the recycled polyester sheet and the polyester sheet; after the heating treatment, close the hot press and cool to room temperature. The diameter of the polyester sheet is 3 mm.
[0076] Step 16: After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths.
[0077] The present invention utilizes a combination of copolyester and modified polyester, controls the material content and mixing ratio, and adds a crystallization accelerator to ensure thorough mixing of the copolyester and modified polyester to form a uniform mixture. Mechanical or ultrasonic addition is used to evenly disperse carbon black in the modified polyester. An extruder is then used to extrude and shape the mixture into a strip-shaped polyester material. Finally, a hot press is used to bond the recycled polyester and polyester together, forming a carbon black-modified polyester fiber with excellent physical properties and corrosion resistance.
[0078] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit them. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein. These modifications or replacements do not deviate the essence of the corresponding technical solutions from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A carbon black modified polyester fiber, characterized in that: It consists of copolyester, modified polyester, crystallization accelerator and recycled polyester.
2. The carbon black modified polyester fiber according to claim 1, characterized in that: The mass percentage of the copolyester is 15-16%, the mass percentage of the modified polyester is 20-30%, the mass percentage of the crystallization accelerator is 14-20%, and the mass percentage of the recycled polyester is 15-20%.
3. The carbon black modified polyester fiber according to claim 2, characterized in that: The modified polyester is a polyester containing carbon black.
4. The carbon black modified polyester fiber according to claim 3, characterized in that: The copolyester contains a side-group-containing aliphatic diol structural units with no more than 8 carbon atoms.
5. A method for preparing a carbon black modified polyester fiber as claimed in any one of claims 1 to 4, characterized in that: The preparation method comprises the following steps: Select and screen the copolyester raw materials, dissolve the copolyester raw materials in a suitable amount of solvent at room temperature, and stir evenly; Add 14-20% of crystallization accelerator to the copolyester; Add 20-30% of modified polyester containing carbon black, and mix thoroughly so that the modified polyester is evenly dispersed in the copolyester to form a mixture; preparing the mixture into a polyester sheet through an extrusion process; The recycled polyester sheet and the polyester sheet are stacked layer by layer in a certain proportion, and heated at a certain temperature and pressure to make the recycled polyester sheet and the polyester sheet bonded together; After cooling, the bonded carbon black modified polyester fiber is cut into appropriate lengths.
6. The method for preparing carbon black modified polyester fiber according to claim 5, characterized in that: The diameter of the polyester sheet is 1 to 3 mm.
7. The method for preparing carbon black modified polyester fiber according to claim 6, characterized in that: Adding 20-30% of modified polyester containing carbon black and fully mixing so that the modified polyester is evenly dispersed in the copolyester to form a mixture, comprising the following steps: Select modified polyester material and confirm that the carbon black content is 20-30%; Adding the modified polyester to the copolyester raw material, and adding a corresponding amount of solvent to fully mix the modified polyester and the copolyester raw material; gradually adding carbon black into the modified polyester, and using a mechanical stirrer or ultrasonic waves to fully disperse the carbon black in the modified polyester; The modified polyester and copolyester raw materials that are fully mixed are mixed, and an appropriate amount of solvent is added again. After the mixture is evenly mixed, the modified polyester and copolyester raw materials are fully mixed mechanically or ultrasonically to form a mixture.
8. The method for preparing carbon black modified polyester fiber according to claim 7, characterized in that: When the modified polyester and the copolyester raw materials are fully mixed, the stirring speed is 100 to 500 rpm and the stirring time is 1 to 2 hours.
9. The method for preparing carbon black modified polyester fiber according to claim 8, characterized in that: The mixture is prepared into a polyester sheet through an extrusion process, comprising the following steps: The mixture is injected into the hopper of the extruder, and the temperature, speed and extrusion pressure of the extruder are adjusted to gradually heat up and melt the mixture; The mixture injected into the extruder is heated and melted and then extruded to the head of the extruder to form a plastic strip of a certain shape and size; The strip is heated and extruded, and then formed and shaped by a die head mold to form a polyester sheet.
10. The method for preparing carbon black modified polyester fiber according to claim 9, characterized in that: The recycled polyester sheet and the polyester sheet are stacked layer by layer in a certain ratio, and heated at a certain temperature and pressure to bond the recycled polyester sheet and the polyester sheet into one, including the following steps: Prepare recycled polyester sheets and polyester sheets, and cut and stack them according to the required ratio; Place the stacked adhesive materials into the heat press and adjust the temperature and pressure; At a certain temperature and time, pressure is applied to the interface between the recycled polyester sheet and the polyester sheet, so that the recycled polyester sheet and the polyester sheet are fully in contact and bonded; After the heating process, the heat press was turned off and allowed to cool to room temperature.
Citation Information
Patent Citations
Durable carbon black conductive fiber and preparation method thereof
CN102031588A
Normal temperature and pressure disperse dyeable modified polyester fiber
CN103132174A
Polyester-fiber conductive masterbatch pre-dispersion and preparation method thereof
CN103214802A
Modified polyester fibre and regenerated cellulose fibre fabrics, and preparation method of the same
CN106592039A
Modified polyester fiber and preparation method thereof
CN106637481A