Electrolyte, lithium metal battery and preparation method therefor, and electrical device

By using the electrolyte additive R-M-X in lithium metal batteries to form a lithium-philic layer, the lithium dendrites problem during the circulation of lithium metal batteries is solved, the circulation performance and safety of the battery are improved, and the lithium uniform nuclear formation and battery performance are improved. .

WO2024230001A1PCT designated stage expired Publication Date: 2024-11-14CONTEMPORARY AMPEREX TECHNOLOGY CO LTD

Patent Information

Application Number
PCT/CN2023/112953
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-05
Filing Date
2023-08-14
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

There is a lithium dendrite problem during the circulation of lithium metal batteries, which leads to unstable battery performance and security threats. The existing technology is difficult to effectively solve the problems of lithiation of the negative electrode surface and the uniform nucleation of lithium.

Method used

The electrolyte additive R-M-X is used, where R is a hydrocarbon group, M is a metal whose standard electrode potential is higher than Li, X is an anion or hydrocarbon group, M and Li form an intermetallic compound or alloy solid solution, which is used to form a lithium-philic layer on the surface of the negative electrode current collector. , slowly release M ions to reduce the lithium nucleus overpotential and inhibit dendrites.

Benefits of technology

By forming a lithium-philic layer, it promotes the uniform nucleation of lithium, improves the cyclic performance and Coulomb efficiency of lithium metal batteries, extends the battery life, reduces the nucleation overpotential of lithium on the anode, and reduces dendrites.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2023112953_14112024_PF_FP_ABST
    Figure CN2023112953_14112024_PF_FP_ABST
Patent Text Reader

Abstract

An electrolyte, a lithium metal battery and a preparation method therefor, and an electrical device, relating to the field of batteries. The electrolyte comprises a lithium salt, an organic solvent, and an electrolyte additive, and the electrolyte additive has a structure of R-M-X, wherein R comprises a hydrocarbyl group, M comprises a metal having a standard electrode potential higher than that of Li, X comprises anions or a hydrocarbyl group, and M can form an intermetallic compound or an alloy solid solution with Li. The lithium metal battery comprises a negative electrode, the negative electrode comprises a negative current collector and a lithiophilic layer covering the surface of the negative current collector, the lithiophilic layer comprises M, and M comprises a metal having a standard electrode potential higher than that of Li and capable of forming an intermetallic compound or an alloy solid solution with Li. The electrolyte can improve the lithiophilicity of the surface of the negative electrode, promote uniform nucleation of the lithium, and improve the cycle performance of the lithium metal battery.
Need to check novelty before this filing date? Find Prior Art

Description

Electrolyte, lithium metal battery, preparation method thereof, and power-using device

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Chinese patent application 202310493792.X filed on May 5, 2023, entitled “An electrolyte, a lithium metal battery, a preparation method thereof, and an electrical device”, the entire contents of which are incorporated herein by reference. Technical Field

[0003] The present application relates to the field of batteries, and specifically to an electrolyte, a lithium metal battery, a preparation method thereof, and an electrical device. Background Art

[0004] Energy conservation and emission reduction are key to the sustainable development of the automotive industry. Electric vehicles, due to their energy-saving and environmentally friendly advantages, have become a crucial component of this industry's sustainable development. Battery technology is a crucial factor in the development of electric vehicles. Lithium secondary batteries, a widely used type of battery, use lithium metal or lithium alloys as the negative electrode material and a non-aqueous electrolyte solution. Lithium secondary batteries are further categorized as lithium-ion batteries and lithium metal batteries. Current lithium metal batteries suffer from the problem of lithium dendrites in the negative electrode during cycling.

[0005] Summary of the Invention

[0006] In view of the above problems, the present application provides an electrolyte, a lithium metal battery and its preparation method, and an electrical device, which can improve the lithium affinity of the negative electrode surface, promote uniform nucleation of lithium, and enhance the cycle performance of the lithium metal battery.

[0007] In a first aspect, the present application provides an electrolyte comprising an electrolyte additive, wherein the structure of the electrolyte additive comprises RMX, wherein R comprises a hydrocarbon group, M comprises a metal having a standard electrode potential higher than Li, X comprises an anion or a hydrocarbon group, M can form an intermetallic compound or alloy solid solution with Li, and M is used to form a lithium-philic layer on the surface of the negative electrode current collector of the battery.

[0008] In the technical solution of the embodiment of the present application, RMX is used as an electrolyte additive, wherein a semi-covalent bond is formed between C and M in the R hydrocarbon group, and the semi-covalent bond energy is close to the covalent bond energy. When the potential reaches the reaction potential, the semi-covalent bond slowly breaks and the ions of M are slowly released. When this electrolyte is applied to a lithium metal battery, on the one hand, the standard electrode potential of M is higher than that of Li, and it can preferentially obtain electrons than Li and thus deposit preferentially than Li, forming a lithium-philic layer on the surface of the anode current collector, effectively increasing the active sites for lithium deposition; on the other hand, since M in the lithium-philic layer can form an intermetallic compound or alloy solid solution with Li, the binding force between M and lithium ions is stronger than the binding force between the current collector and lithium ions, even if the negative electrode surface is lithiated, specifically, the overpotential for lithium ions to obtain electrons from M is less than the overpotential for obtaining electrons from the current collector. Therefore, the lithium-philic ability of M deposited to form a lithium-philic layer is stronger than that of the current collector, which can reduce the nucleation overpotential of lithium on the anode, reduce localized nucleation of lithium, inhibit dendrite formation, thereby uniformly nucleating lithium, and ultimately improve battery performance.

[0009] In some embodiments, the weight percentage of the electrolyte additive is no greater than 10%. Alternatively, the weight percentage of the electrolyte additive is 1% to 10%, optionally 2% to 9%, or optionally 3% to 6%. Adding a small amount of the electrolyte additive can form a lithium-philic layer on the anode surface after battery formation, thereby reducing the nucleation overpotential of lithium and reducing the impact of residual electrolyte additive on the electrolyte itself.

[0010] In some embodiments, M includes at least one of Mg, Al, Mn, and Zn. Each metal has a higher standard electrode potential (reaction potential) than lithium and can be deposited preferentially over lithium, thereby forming a lithiophilic layer on the current collector surface. Furthermore, these metals can form intermetallic compounds or alloy solid solutions with lithium, i.e., the formed lithiophilic layer can render the negative electrode surface lithiophilic.

[0011] In some embodiments, R is a hydrocarbon group having 1 to 10 carbon atoms. Optionally, R includes C n H 2n+1 , n is 1 to 10. The bond energy between C and M in the hydrocarbon group with 1 to 10 carbon atoms is close to that of a covalent bond, allowing M to be slowly released, forming a uniformly deposited lithium-philic layer on the current collector surface, reducing the problem of uneven lithium ion deposition caused by metal agglomeration to form islands due to the rapid release of M metal ions; the C in the alkane group is surrounded by saturated single bonds, which can reduce the increase in battery impedance and capacity loss caused by the polymerization of organic groups on the negative electrode surface.

[0012] In some embodiments, X comprises a halogen, optionally selected from at least one of Cl, Br, I, and F. A Grignard-like reagent RMX is used as an electrolyte additive, with M and X connected by an ionic bond. When the charging potential reaches the reaction potential, the Grignard-like reagent slowly releases R hydrocarbon groups, M metal ions, and X halogen ions. The X halogen ions facilitate the formation of a stable SEI interface film. The SEI contains lithium halide, which improves the SEI ion conductivity and facilitates the uniform deposition of lithium ions.

[0013] In some embodiments, X includes a hydrocarbon group. Alternatively, X includes a hydrocarbon group with 1 to 10 carbon atoms. Alternatively, X includes C n H 2n+1 , n is 1 to 10. The metal organic compound R1-M-R2 (R1 and R2 are both hydrocarbon groups) is used as an electrolyte additive to slowly release the M metal ions.

[0014] In some embodiments, M is Mg and X is Br. n H 2n+1 MgBr is used as an electrolyte additive in lithium metal batteries, which can simultaneously achieve good in-situ lithium affinity and promote SEI formation.

[0015] In a second aspect, the present application provides a lithium metal battery comprising a negative electrode, the negative electrode comprising a negative electrode current collector and a lithium-philic layer sequentially located on the surface of the negative electrode current collector, the lithium-philic layer comprising M, M comprising a metal having a standard electrode potential higher than Li and capable of forming an intermetallic compound or alloy solid solution with Li.

[0016] In the technical solution of the embodiment of the present application, the lithium-philic layer makes the negative electrode surface lithiophilic. When the battery is charging, lithium can form an intermetallic compound or alloy solid solution with the M metal in the lithium-philic layer, that is, it can promote the uniform nucleation of lithium and improve the cycle performance of the lithium metal battery. When the battery is discharging, the lithium in the lithium-philic layer can dissolve normally, thereby achieving the effect of cyclic charge and discharge.

[0017] In some embodiments, the average thickness of the lithiophilic layer is 50 nm to 100 nm. A lithiophilic layer that is too thin is difficult to form. Specifically, when using M metal to form a lithiophilic layer on the surface of the negative electrode current collector through chemical formation, if there is too little M metal, the corresponding lithiophilic layer is too thin, which can easily lead to uneven aggregation of the M metal in the lithiophilic layer due to the nano-effect, resulting in leakage of the current collector. If the lithiophilic layer is too thick, the M metal will consume active lithium, reducing the battery's coulombic efficiency.

[0018] In some embodiments, the negative electrode further comprises an interface film located on the surface of the lithium-philic layer, wherein the thickness of the interface film does not exceed 1 μm. A micrometer-sized interface film SEI can seriously damage the dynamics of the battery.

[0019] In some embodiments, the interfacial film contains LiX, where X comprises an anion, and optionally, X comprises a halogen. The lithium halide in the SEI interfacial film enables uniform lithium deposition and improves SEI ionic conductivity. LiCl, LiBr, and other materials can act as lithiophiles to enable uniform lithium deposition. LiI, LiF, and other materials can also enhance SEI ionic conductivity and mechanical strength.

[0020] In some embodiments, the interface film contains R, R includes a hydrocarbon group, optionally, R includes a hydrocarbon group with 1 to 10 carbon atoms, optionally, R includes C n H 2n+1 , n is 1 to 10.

[0021] In some embodiments, an electrolyte is further included, the electrolyte including a lithium salt, the lithium salt including at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(oxalatoborate), and lithium difluorooxalatoborate.

[0022] In a third aspect, the present application provides an electrical device comprising the lithium metal battery provided in the second aspect, wherein the battery is used to provide electrical energy.

[0023] In a fourth aspect, the present application provides a method for preparing the lithium metal battery provided in the second aspect, comprising the following steps:

[0024] Assembling a positive electrode, a negative electrode current collector, and an electrolyte into a battery, wherein the electrolyte includes a lithium salt, an organic solvent, and an electrolyte additive, wherein the structure of the electrolyte additive includes RMX, wherein R includes a hydrocarbon group, M includes a metal having a standard electrode potential higher than Li, X includes an anion or a hydrocarbon group, and M can form an intermetallic compound or an alloy solid solution with Li;

[0025] The battery is formed.

[0026] In the technical solution of the embodiment of the present application, the above-mentioned electrolyte additive is added to the electrolyte. After the battery is formed, M can be used to form a lithium-philic layer on the surface of the negative electrode current collector. During the charging process, M in the lithium-philic layer can form an intermetallic compound or alloy solid solution with Li to achieve lithium deposition, and can also use the dissolution of lithium to achieve discharge.

[0027] In some embodiments, the formation conditions are as follows: first, charging in constant current mode at a fixed rate of 0.15C to 0.25C to a voltage of 3V to 4V, then switching to constant voltage mode with a cutoff current of 0.04C to 0.06C to fully charge the battery. During the formation process, the electrolyte additives take effect during the charging process, thereby forming a lithium metal battery for subsequent charging and discharging.

[0028] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Various other advantages and benefits will become apparent to those skilled in the art upon reading the detailed description of the preferred embodiment below. The accompanying drawings are for illustration purposes only and are not to be considered as limiting the present application. The same reference numerals are used throughout the drawings to represent the same components. In the drawings:

[0030] FIG1 is a schematic structural diagram of a vehicle according to some embodiments of the present application;

[0031] FIG2 is a schematic diagram of the exploded structure of a battery according to some embodiments of the present application;

[0032] FIG3 is a schematic structural diagram of a battery cell provided in some embodiments of the present application;

[0033] FIG4 is a schematic diagram of the exploded structure of a battery cell according to some embodiments of the present application.

[0034] Icon: 1000-vehicle; 100-battery; 10-housing; 11-accommodation space; 12-first part; 13-second part; 20-battery cell; 21-housing; 211-opening; 22-end cover assembly; 221-end cover; 222-electrode terminal; 23-electrode assembly; 24-current collecting member; 25-insulating protection member; 200-controller; 300-motor. DETAILED DESCRIPTION

[0035] The following embodiments of the technical solution of the present application will be described in detail with reference to the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application and are therefore only examples and are not intended to limit the scope of protection of the present application.

[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those skilled in the art to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" and any variations thereof in the specification and claims of this application and the above-mentioned figure descriptions are intended to cover non-exclusive inclusions.

[0037] In the description of the embodiments of this application, the technical terms "first" and "second" are used only to distinguish different objects and should not be understood to indicate or imply relative importance or implicitly specify the quantity, specific order, or primary and secondary relationship of the indicated technical features. In the description of the embodiments of this application, the meaning of "plurality" is more than two, unless otherwise clearly and specifically defined.

[0038] References herein to "embodiments" mean that a particular feature, structure, or characteristic described in connection with the embodiments may be included in at least one embodiment of the present application. The appearance of this phrase in various places in the specification does not necessarily refer to the same embodiment, nor does it constitute an independent or alternative embodiment that is mutually exclusive of other embodiments. It is understood, both explicitly and implicitly, by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0039] In the description of the embodiments of the present application, the term "plurality" refers to more than two (including two), and similarly.

[0040] In the description of the embodiments of the present application, the orientations or positional relationships indicated by technical terms such as "thickness", "up", "down", "front", "back", "top", "bottom", "inside", and "outside" are based on the orientations or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the embodiments of the present application.

[0041] In the description of the embodiments of this application, unless otherwise expressly specified or limited, technical terms such as "connection" and "fixed" should be understood in a broad sense. For example, they can refer to fixed connection, detachable connection, or integration; mechanical connection or electrical connection; direct connection or indirect connection through an intermediate medium; internal communication between two components or interaction between two components. For those skilled in the art, the specific meanings of the above terms in the embodiments of this application can be understood according to specific circumstances.

[0042] Currently, market developments indicate that power batteries are becoming increasingly widely used. They are not only used in energy storage systems such as hydropower, thermal, wind, and solar power plants, but are also widely used in electric vehicles like electric bicycles, electric motorcycles, and electric vehicles, as well as in military equipment and aerospace. As power battery applications continue to expand, market demand is also growing.

[0043] Lithium-ion batteries have been widely used in technological products such as automobiles and mobile phones. Existing lithium-ion batteries mainly use graphite as the negative electrode material, and its theoretical specific capacity is 350mAh / g to 400mAh / g. The capacity of commercial lithium-ion batteries is already close to the theoretical value, and it is difficult to significantly increase the capacity of the battery. Due to the high theoretical specific capacity of metallic lithium, about 3860mAh / g, and the low electrode potential (-3.04V vs standard hydrogen electrode), the development of lithium metal batteries with metallic lithium as the negative electrode has attracted the attention of researchers. When you want to maximize the energy density of the battery, you usually need to use ultra-thin lithium metal (usually less than 25μm thick) in the lithium metal battery, which brings great difficulties to actual processing and battery assembly. At this time, negative electrode-free lithium metal batteries become an ideal choice.

[0044] A negative-electrode-free lithium metal secondary battery refers to a battery in which no negative electrode active material layer is actively placed on the negative electrode side during the battery manufacturing process. For example, during the battery manufacturing process, lithium metal is not placed on the negative electrode through a process such as coating or deposition to form a negative electrode active material layer. Instead, the battery system uses only a current collector such as copper foil as the negative electrode, while the positive electrode is composed of a common lithium-containing material (such as lithium iron phosphate, ternary cathode, lithium cobalt oxide, etc.). Compared with lithium-ion batteries, the direct use of copper foil for the negative electrode rather than highly chemically active lithium metal brings great convenience and protection to battery assembly and safety.

[0045] In some embodiments, to improve battery performance, the negative electrode side of the negative electrode-less lithium metal battery may be provided with some conventional negative electrode active materials, such as metal oxides and alloys. Although these materials have a certain capacity, due to the small amount of these materials, they are not used as the main negative electrode active material in the battery. Therefore, the lithium metal secondary battery constructed in this way can still be considered a negative electrode-less lithium metal secondary battery.

[0046] The structure and basic principle of the negative electrode-free lithium metal secondary battery are as follows: During the first charge, the lithium ions in the positive electrode combine with the electrons on the surface of the negative electrode current collector, and lithium deposition occurs to form a lithium metal phase (Li + +e - →Li); during discharge, the lithium metal deposited on the negative electrode current collector dissolves (Li-e - →Li + ), and then return to the positive electrode, and so on, to achieve cyclic charge and discharge. Since there is no negative electrode active material, the energy density of the negative electrode-free lithium metal secondary battery has been greatly improved.

[0047] However, when constructing anode-free lithium metal batteries, the nucleation overpotential of lithium metal on commonly used anode current collectors is high, leading to a significant tendency for localized nucleation. In severe cases, this can cause dendrites, threatening the battery's safety and long-cycle performance. For example, the copper in the commonly used anode current collector copper foil cannot form an intermetallic compound or alloy solid solution with lithium. Therefore, the copper foil has a high nucleation overpotential for lithium and a significant tendency for localized nucleation.

[0048] Since the smaller the lithium metal nucleation overpotential on the negative electrode, the stronger the negative electrode's lithiophilicity and the easier it is to combine with lithium, the surface of the negative electrode current collector can be first covered with a lithiophilic material layer with a lower overpotential. Compared with directly depositing lithium metal on the surface of the negative electrode current collector, this can make the lithium metal more uniformly deposited.

[0049] At the same time, in order to promote SEI film formation, certain electrolyte additives are often added to the electrolyte to improve the mechanical strength or ionic conductivity of SEI and other properties.

[0050] In order to solve the problem that lithium metal is easily aggregated during deposition at the negative electrode, an electrolyte can be designed to which a specific electrolyte additive is added. When the electrolyte is applied to a negative electrode-free lithium metal battery, through formation charging, the electrolyte additive is first deposited on the negative electrode current collector to form a lithium-philic layer, thereby improving the lithium-philicity of the negative electrode surface, so that the negative electrode-free lithium metal battery can deposit and dissolve lithium metal on the surface of the lithium-philic layer of the negative electrode according to its basic principle. Since the lithium-philic layer can promote the uniform nucleation of lithium, the cycle life and coulombic efficiency of the lithium metal battery can be improved.

[0051] This electrolyte can be used to prepare battery cells, which can be used, but not limited to, in electrical devices such as vehicles, ships, or aircraft. A power supply system comprising the battery cells and batteries disclosed herein can be used to construct such electrical devices. This improves the lithiation affinity of the negative electrode surface, promotes uniform lithium nucleation, and enhances the cycle life and coulombic efficiency of the metallic lithium negative electrode.

[0052] The present invention provides an electric device that uses a battery as a power source. The electric device may be, but is not limited to, a mobile phone, a tablet, a laptop computer, an electric toy, an electric tool, a battery-powered vehicle, an electric car, a ship, a spacecraft, etc. The electric toy may include a fixed or mobile electric toy, such as a game console, an electric car toy, an electric ship toy, and an electric airplane toy, etc. The spacecraft may include an airplane, a rocket, a space shuttle, and a spacecraft, etc.

[0053] For the convenience of description, the following embodiments are described by taking a vehicle 1000 as an example of an electrical device according to an embodiment of the present application.

[0054] Please refer to Figure 1, which is a schematic diagram of the structure of a vehicle 1000 provided in some embodiments of the present application. A battery 100 is disposed within vehicle 1000. Battery 100 can be located at the bottom, front, or rear of vehicle 1000. Battery 100 can be used to power vehicle 1000, for example, as an operating power source for vehicle 1000.

[0055] The vehicle 1000 may further include a controller 200 and a motor 300 . The controller 200 is used to control the battery 100 to supply power to the motor 300 , for example, to meet the power requirements of the vehicle 1000 during startup, navigation, and driving.

[0056] In some embodiments of the present application, the battery 100 can not only serve as the operating power source of the vehicle 1000, but also serve as the driving power source of the vehicle 1000, replacing or partially replacing fuel or natural gas to provide driving power for the vehicle 1000.

[0057] FIG2 is a schematic diagram of the exploded structure of a battery 100 provided in some embodiments of the present application. Referring to FIG2 , the battery 100 includes a housing 10 and a battery cell 20 , wherein the battery cell 20 is housed in the housing 10 .

[0058] The housing 10 is used to provide a storage space 11 for the battery cells 20. In some embodiments, the housing 10 may include a first portion 12 and a second portion 13, which overlap to define the storage space 11 for accommodating the battery cells 20. Of course, the connection between the first portion 12 and the second portion 13 can be sealed by a seal (not shown), such as a sealing ring, sealant, or the like.

[0059] The first portion 12 and the second portion 13 can have various shapes, such as a rectangular parallelepiped, a cylinder, etc. The first portion 12 can be a hollow structure with an opening on one side to form a receiving cavity for accommodating the battery cell 20. The second portion 13 can also be a hollow structure with an opening on one side to form a receiving cavity for accommodating the battery cell 20. The open side of the second portion 13 covers the open side of the first portion 12, thereby forming the box 10 with the receiving space 11. Of course, as shown in Figure 2, the first portion 12 can also be a hollow structure with an opening on one side, and the second portion 13 can be a plate-like structure. The second portion 13 covers the open side of the first portion 12, thereby forming the box 10 with the receiving space 11.

[0060] In the battery 100, there can be one or more battery cells 20. If there are multiple battery cells 20, the multiple battery cells 20 can be connected in series, in parallel, or in a mixed connection. Mixed connection means that the multiple battery cells 20 are connected in series and in parallel. The multiple battery cells 20 can be directly connected in series, in parallel, or in a mixed connection, and then the whole formed by the multiple battery cells 20 is accommodated in the box 10; of course, it is also possible that the multiple battery cells 20 are first connected in series, in parallel, or in a mixed connection to form a battery module, and the multiple battery modules are then connected in series, in parallel, or in a mixed connection to form a whole, and accommodated in the box 10. The battery cell 20 can be cylindrical, flat, rectangular, or in other shapes. Figure 2 exemplifies the case where the battery cell 20 is square.

[0061] In some embodiments, the battery 100 may further include a busbar component (not shown), and the multiple battery cells 20 may be electrically connected via the busbar component to achieve series connection, parallel connection, or mixed connection of the multiple battery cells 20 .

[0062] Figure 3 is a schematic diagram of the structure of a battery cell 20 provided in some embodiments of the present application, and Figure 4 is a schematic diagram of the exploded structure of a battery cell 20 provided in some embodiments of the present application. Referring to Figures 3 and 4, the battery cell 20 may include a housing 21, an end cap assembly 22, and an electrode assembly 23. The housing 21 has an opening 211, and the electrode assembly 23 is accommodated within the housing 21. The end cap assembly 22 is used to seal the opening 211.

[0063] The shape of the housing 21 can be determined according to the specific shape of the electrode assembly 23. For example, if the electrode assembly 23 is a rectangular parallelepiped structure, the housing 21 can be a rectangular parallelepiped structure. Figures 3 and 4 exemplarily show the case where the housing 21 and the electrode assembly 23 are square.

[0064] The shell 21 may be made of a variety of materials, such as copper, iron, aluminum, stainless steel, aluminum alloy, etc., and the embodiment of the present application does not impose any special restrictions on this.

[0065] The end cap assembly 22 includes an end cap 221 and an electrode terminal 222. The end cap assembly 22 is used to seal the opening 211 of the outer shell 21 to form a sealed installation space (not shown), which is used to accommodate the electrode assembly 23. The installation space is also used to accommodate an electrolyte, such as an electrolyte. The end cap assembly 22 serves as a component for outputting the electrical energy of the electrode assembly 23. The electrode terminal 222 in the end cap assembly 22 is used to electrically connect to the electrode assembly 23, that is, the electrode terminal 222 is electrically connected to the tab of the electrode assembly 23. For example, the electrode terminal 222 is connected to the tab through the current collecting member 24 to achieve electrical connection between the electrode terminal 222 and the tab.

[0066] It should be noted that the opening 211 of the shell 21 can be one or two. If the opening 211 of the shell 21 is one, the end cap assembly 22 can also be one, and two electrode terminals 222 can be provided in the end cap assembly 22, and the two electrode terminals 222 are respectively used to electrically connect to the positive electrode tab and the negative electrode tab of the electrode assembly 23. If the opening 211 of the shell 21 is two, for example, the two openings 211 are provided on opposite sides of the shell 21, the end cap assembly 22 can also be two, and the two end cap assemblies 22 are respectively covered at the two openings 211 of the shell 21. In this case, the electrode terminal 222 in one end cap assembly 22 can be a positive electrode terminal, which is used to electrically connect to the positive electrode tab of the electrode assembly 23; and the electrode terminal 222 in the other end cap assembly 22 can be a negative electrode terminal, which is used to electrically connect to the negative electrode sheet of the electrode assembly 23.

[0067] In some embodiments, as shown in FIG4 , the battery cell 20 may further include an insulating protective member 25 secured to the periphery of the electrode assembly 23. The insulating protective member 25 is used to insulate and isolate the electrode assembly 23 from the housing 21. Exemplarily, the insulating protective member 25 is a tape adhered to the periphery of the electrode assembly 23. In some embodiments, there are multiple electrode assemblies 23, and the insulating protective member 25 is disposed around the periphery of the multiple electrode assemblies 23, forming the multiple electrode assemblies 23 into a single integrated structure to maintain structural stability.

[0068] According to some embodiments of the present application, the electrolyte includes a lithium salt, an organic solvent and an electrolyte additive, and the structure of the electrolyte additive includes RMX, wherein R includes a hydrocarbon group, M includes a metal having a standard electrode potential higher than Li, X includes an anion or a hydrocarbon group, M can form an intermetallic compound or an alloy solid solution with Li, and M is used to form a lithium-philic layer on the surface of the negative electrode current collector of the battery.

[0069] Among them, the lithium salt can be at least one of an organic lithium salt or an inorganic lithium salt, specifically at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB) and lithium difluorooxalatoborate (LiDFOB), and can also be other optional lithium salts or any combination.

[0070] The organic solvent may include at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl formate, ethyl formate, ethyl propionate, propyl propionate, methyl butyrate, ethyl acetate, acid anhydride, N-methylpyrrolidone, N-methylformamide, N-methylacetamide, acetonitrile, sulfolane, dimethyl sulfoxide, ethylene sulfite, propylene sulfite, methyl sulfide, diethyl sulfite, dimethyl sulfite, tetrahydrofuran, fluorine-containing cyclic organic esters, and sulfur-containing cyclic organic esters.

[0071] Wherein, "RMX" refers to the structural form of the electrolyte additive, which contains R, M and X, and M is bonded to R and X at the same time, and the R hydrocarbon group refers to a group containing carbon and hydrogen atoms, which is connected to M through carbon. After the bond is broken, R forms an R hydrocarbon group, M forms an M metal ion, and X forms an anion or hydrocarbon group. In some embodiments of the present application, an electrolyte additive (R1-M1-X1) with the above structural form can be added to the electrolyte, or two electrolyte additives with the above structural forms (R1-M1-X1, R2-M2-X2, R1 and R2 can be the same or different, M1 and M2 can be the same or different, X1 and X2 can be the same or different), or even more electrolyte additives with the above structural forms can be added.

[0072] By slowly breaking the semi-covalent bond between the carbon of the hydrocarbon group R and the metal M, the metal M ions are slowly released, and the standard electrode potential of M is higher than that of Li, so that M is in situ deposited on the surface of the anode current collector to form a lithium-philic layer, effectively increasing the active sites for lithium deposition; lithium can form an intermetallic compound or alloy solid solution with the metal M in the lithium-philic layer, reducing the local nucleation of lithium and inhibiting the formation of dendrites, thereby making lithium nucleate uniformly.

[0073] According to some embodiments of the present application, the mass percentage of the electrolyte additive is no more than 10%, and may be 1% to 10%, 2% to 9%, or 3% to 6%.

[0074] The mass percentage of the electrolyte additive refers to the mass concentration of the electrolyte additive in the electrolyte. As an example, the mass percentage of the electrolyte additive is 0.1%, 0.5%, 0.8%, 1%, 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, or 10%, and can also be any value within the above two numerical ranges.

[0075] In some embodiments of the present application, the electrolyte additive is consumed after battery formation, and a lithium-philic layer of a certain thickness is formed on the surface of the anode. Only a very small amount of the electrolyte additive exists in the electrolyte, and the electrolyte additive may even be completely consumed and no longer exist.

[0076] The standard electrode potential of the M metal is higher than that of Li, and it can form an intermetallic compound or alloy solid solution with Li. The standard electrode potential refers to the equilibrium potential measured at a temperature of 25°C and an effective concentration of 1 mol / L (i.e., an activity of 1) for the metal ions. An "intermetallic compound" refers to a new phase formed by Li metal and the M metal with a fixed composition and a specific crystal structure that is different from that of the starting metals. An "alloy solid solution" refers to the ability of the M metal and Li metal to mix and remain mutually soluble (the solute metal can dissolve in the lattice of the solvent metal).

[0077] According to some embodiments of the present application, M includes at least one of Mg, Al, Mn, and Zn. Exemplarily, M can be Mg, Al, Mn, or Zn, or two of these metals, such as Mg and Al, Mg and Mn, Mg and Zn, Al and Mn, Al and Zn, Mn or Zn, and M selects Mg and Mn at the same time (the corresponding electrolyte additives are R-Mg-X and R-Mn-X, or R-Mg-Mn-X). The standard electrode potential of these two metals is higher than that of lithium, and both can be preferentially deposited to form a lithium-philic layer together, and both can form an intermetallic compound or alloy solid solution with lithium metal; M can also be three or four metals, and their combinations are not listed here one by one.

[0078] The hydrocarbon group may be at least one of an alkane group (monovalent saturated group), an olefin group (monovalent unsaturated group), a sub-group (divalent group), and a tri-group with 1 to 10 carbon atoms, and each hydrocarbon group may be a chain hydrocarbon group or a cyclic hydrocarbon group. n H 2n+1 , n is 1 to 10. For example, R can be -CH3, -C2H5, -C3H7, -C4H9, -C5H 11 、-C6H 13 、-C7H 15 、-C8H 17 、-C9H 19 or -C 10 H 21 , R can also be two or more alkane groups. The structure of the corresponding electrolyte additive can be that multiple alkane groups are simultaneously connected to M, or multiple alkane groups are separately connected to electrolyte additives with different structures.

[0079] According to some embodiments of the present application, X includes a halogen, and optionally, X is selected from at least one of Cl, Br, I, and F. Exemplarily, X can be Cl, Br, I, or F, or two or three of these halogens. The corresponding electrolyte additive may have a structure in which two halogens are simultaneously connected to M, or multiple halogens are separately connected to electrolyte additives of different structures. Each halogen is conducive to forming a stable SEI.

[0080] According to some embodiments of the present application, X includes a hydrocarbon group. Alternatively, X includes a hydrocarbon group with 1 to 10 carbon atoms. Alternatively, X includes C n H 2n+1, n is 1 to 10. X can be at least one of an alkane group (monovalent saturated group), an olefin group (monovalent unsaturated group), a sub-group (divalent group), and a secondary group (trivalent group). For example, X can be -CH3, -C2H5, -C3H7, -C4H9, -C5H 11 、-C6H 13 、-C7H 15 、-C8H 17 、-C9H 19 or -C 10 H 21 , or two of the alkane groups.

[0081] According to some embodiments of the present application, the electrolyte additive is a Grignard reagent R-Mg-X, where R is a hydrocarbon group and X is a halogen. For example, the electrolyte additive is R-Mg-Br, R-Mg-Cl, R-Mg-I, or R-Mg-F. In some other embodiments, the electrolyte additive may also be a Grignard-like reagent RMX, where R is a hydrocarbon group, M is a metal other than Mg, and X is a halogen. For example, the electrolyte additive is R-Al-Br2, R-Mn-Br, or R-Zn-Br.

[0082] The above describes an electrolyte that improves the lithiation affinity of the negative electrode surface and promotes uniform lithium nucleation, which is mainly used to construct a lithium metal battery. The following describes a lithium metal battery that can be a negative electrode-free lithium metal secondary battery.

[0083] According to some embodiments of the present application, a lithium metal battery includes a positive electrode and a negative electrode, a separator, and an electrolyte. The positive electrode can provide lithium ions. The negative electrode includes a negative electrode current collector and a lithium-philic layer located on the surface of the negative electrode current collector. The lithium-philic layer includes M, and M includes a metal having a standard electrode potential higher than Li and capable of forming an intermetallic compound or alloy solid solution with Li.

[0084] During the charging process of the lithium metal battery, the lithium ions in the positive electrode combine with electrons on the surface of the lithium-philic layer of the negative electrode, resulting in lithium deposition; during the discharging process of the lithium metal battery, the lithium metal deposited on the negative electrode dissolves and returns to the positive electrode, repeatedly realizing the cyclic charging and discharging of the lithium metal battery.

[0085] During lithium deposition, lithium forms an intermetallic compound or alloy solid solution with the M metal in the lithiophilic layer, thereby forming a lithiophilic layer containing the intermetallic compound or alloy solid solution of lithium metal.

[0086] According to some embodiments of the present application, M may be a metal such as Mg, Al, Mn, Zn, etc., which has a higher standard electrode potential than Li and can form an intermetallic compound or alloy solid solution with Li.

[0087] [negative electrode]

[0088] According to some embodiments of the present application, the average thickness of the lithiophilic layer is 50 nm to 100 nm.

[0089] The average thickness of the lithiophilic layer refers to the average thickness before lithium is deposited. For example, the average thickness of the lithiophilic layer can be 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, or 100 nm, or any value within the range between the two aforementioned values.

[0090] After the battery is formed, an interface film is formed on the negative electrode. According to some embodiments of the present application, the negative electrode further includes an interface film SEI located on the surface of the lithium-philic layer, and the thickness of the interface film does not exceed 1 μm.

[0091] According to some embodiments of the present application, the interface film contains LiX, where X includes an anion, and optionally, X includes a halogen. Exemplarily, the interface film contains at least one of LiCl, LiBr, LiI, and LiF.

[0092] According to some embodiments of the present application, the interface film contains R, R includes a hydrocarbon group, optionally, R includes a hydrocarbon group with 1 to 10 carbon atoms, optionally, R includes C n H 2n+1 , n is 1 to 10. The description of R can refer to the above description of R in the electrolyte additive, which will not be repeated here.

[0093] According to some embodiments of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0094] [positive electrode]

[0095] According to some embodiments of the present application, the positive electrode includes a positive electrode current collector and a positive electrode active material layer located on a surface of the positive electrode current collector, and the positive electrode active material layer provides lithium ions.

[0096] The positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (for example, a material substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0097] According to some embodiments of the present application, the positive electrode active material layer comprises a positive electrode active material, a conductive agent, a binder, and any other components. The positive electrode active material provides lithium ions and can be any known positive electrode active material for lithium batteries. For example, the positive electrode active material can include lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron manganese phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium iron phosphate, and lithium-rich manganese-based materials.

[0098] [Isolation film]

[0099] The present application has no particular limitation on the type of isolation membrane, and any known isolation membrane with a porous structure having good chemical stability and mechanical stability can be selected.

[0100] In some embodiments of the present application, the material of the separator can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator can be a single-layer film or a multi-layer composite film, without particular limitation. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.

[0101] [Electrolyte]

[0102] According to some embodiments of the present application, the electrolyte includes a lithium salt and an organic solvent.

[0103] The lithium salt may be at least one of an organic lithium salt or an inorganic lithium salt, specifically at least one of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB) and lithium difluorooxalatoborate (LiDFOB), or other optional lithium salts or any combination thereof.

[0104] The organic solvent may include at least one of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, dipropyl carbonate, ethyl methyl carbonate, methyl formate, ethyl formate, ethyl propionate, propyl propionate, methyl butyrate, ethyl acetate, acid anhydride, N-methylpyrrolidone, N-methylformamide, N-methylacetamide, acetonitrile, sulfolane, dimethyl sulfoxide, ethylene sulfite, propylene sulfite, methyl sulfide, diethyl sulfite, dimethyl sulfite, tetrahydrofuran, fluorine-containing cyclic organic esters, and sulfur-containing cyclic organic esters.

[0105] In some embodiments, the positive electrode, the negative electrode, and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0106] In some embodiments, the lithium metal battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0107] A lithium metal battery is described above. The following describes different preparation methods of the lithium metal battery.

[0108] According to some embodiments of the present application, the present application provides a method for preparing a lithium metal battery, which comprises making an electrode assembly of the positive electrode of the above structure, a negative electrode with a lithium-philic layer, and an isolation membrane, and then encapsulating the electrode assembly and the electrolyte to form a lithium metal battery.

[0109] The negative electrode can be formed by first depositing a lithium-philic layer containing M metal on the surface of the negative electrode current collector, and then assembling the negative electrode to form a lithium metal battery.

[0110] According to some other embodiments of the present application, the present application also provides a method for preparing a lithium metal battery, which includes the following steps:

[0111] Assembling a positive electrode, a negative electrode current collector, and an electrolyte into a battery, wherein the electrolyte includes a lithium salt, an organic solvent, and an electrolyte additive, wherein the structure of the electrolyte additive includes RMX, wherein R includes a hydrocarbon group, M includes a metal having a standard electrode potential higher than Li, and X includes an anion, and M can form an intermetallic compound or an alloy solid solution with Li;

[0112] Then the battery is charged after formation.

[0113] Among them, the electrolyte is the electrolyte added with electrolyte additives introduced above, the positive electrode can adopt the positive electrode in the lithium metal battery structure introduced above, and the battery after formation and charging is a lithium metal battery. The lithium metal battery has the structural characteristics of the lithium metal battery introduced above, which will not be repeated here.

[0114] This preparation method first assembles a battery using a negative electrode current collector and an electrolyte containing an electrolyte additive. The battery is then subjected to formation charging. During charging, the electrolyte additive (RMX) takes effect, with M deposited on the surface of the negative electrode current collector to form a lithium-philic layer. R and X also remain on the negative electrode surface to promote the formation of the SEI, thereby forming a lithium metal battery with the aforementioned structure. After formation, the electrolyte additive in the electrolyte is essentially consumed. The negative electrode structure is: negative electrode current collector + lithium-philic layer (containing M metal) + SEI (containing R and X). After the battery is charged, the lithium-philic layer still contains lithium metal, and the M metal and lithium metal exist in the form of an intermetallic compound or alloy solid solution.

[0115] It should be noted that, for the lithium metal battery in this application, as long as it is assembled to form a battery structure, regardless of whether it is formed or not, the battery falls within the scope of protection requested by this application.

[0116] According to some embodiments of the present application, the formation charging conditions are: first charge at a fixed rate of 0.15C to 0.25C in constant current mode until the voltage rises to 3V to 4V, and then switch to constant voltage mode with a cutoff current of 0.04C to 0.06C to fully charge the battery.

[0117] The formation charge rate of the present application is relatively small, which enables the electrolyte additive to fully play its role and form a lithium-philic layer on the surface of the negative electrode current collector.

[0118] According to some embodiments of the present application, the present application also provides an electrical device, comprising a lithium metal battery according to any of the above schemes, and the lithium metal battery is used to provide electrical energy to the electrical device.

[0119] The power-consuming device may be any of the aforementioned devices or systems using batteries.

[0120] Next, one or more embodiments will be described in more detail with reference to the following examples. Of course, these examples do not limit the scope of one or more embodiments.

[0121] Example 1

[0122] 1) Preparation of electrolyte

[0123] In a glove box, lithium bis(fluorosulfonyl)imide (LiFSI, 99.9%, Zhongyao Biotechnology Co., Ltd.) was dissolved in ethylene glycol dimethyl ether (DME, 99%, Shanghai Jizhi Biochemical Technology Co., Ltd.) to prepare a 1 M solution.

[0124] Commercially available ethylmagnesium bromide (C2H5MgBr, Macklin Reagent Co.) was dissolved as an electrolyte additive in a 1M solution to prepare a solution with a mass percentage of 5% electrolyte additive. The solution was stirred at 700 rpm on a magnetic stirrer in a glove box for 3 h to obtain an electrolyte.

[0125] 2) Preparation of positive electrode sheet

[0126] Lithium iron phosphate (LFP), conductive carbon black, and binder polyvinylidene fluoride (PVDF) were added to N-methylpyrrolidone (NMP) in a weight ratio of 8:1:1 and stirred in a drying room to form a slurry. The slurry was coated on aluminum foil, dried, and cold pressed. The coating amount was 0.2 g / cm 2 , compacted density is 2.0g / cm 3 , made into a positive electrode sheet.

[0127] 3) Preparation of full battery

[0128] Using a polyethylene (PE) porous polymer film as the separator and 8μm copper foil as the negative electrode current collector, the prepared positive electrode sheet, separator, and negative electrode current collector are stacked in order, with the separator positioned between the positive and negative electrodes to provide separation. The cells are then wound to form a bare cell. The bare cell is then placed in an outer packaging, injected with the prepared electrolyte, and packaged to create a full battery.

[0129] Example 2

[0130] Except that ethyl zinc bromide (C2H5ZnBr, Alfa Aesar) is used as the electrolyte additive in step 1), the rest is the same as that in Example 1.

[0131] Example 3

[0132] Except that ethyl manganese bromide (C2H5MnBr, Alfa Aesar) is used as the electrolyte additive in step 1), the rest is the same as that in Example 1.

[0133] Example 4

[0134] Except that ethylaluminum bromide (C2H5AlBr2, Macklin) is used as the electrolyte additive in step 1), the rest is the same as that in Example 1.

[0135] Example 5

[0136] Except that ethyl magnesium chloride (C2H5MgCl, Macklin) is used as the electrolyte additive in step 1), the rest is the same as that in Example 1.

[0137] Example 6

[0138] Except that ethyl magnesium iodide (C2H5MgI, Macklin) is used as the electrolyte additive in step 1), the rest is the same as that in Example 1.

[0139] Example 7

[0140] Except that ethyl magnesium fluoride (C2H5MgF, Macklin) is used as the electrolyte additive in step 1), the rest is the same as that in Example 1.

[0141] Example 8

[0142] Except that the mass percentage of the electrolyte additive (C2H5MgBr) in the electrolyte formed in step 1) is 9%, other aspects are the same as those in Example 1.

[0143] Example 9

[0144] Except that the mass percentage of the electrolyte additive (C2H5MgBr) in the electrolyte formed in step 1) is 6%, other aspects are the same as those in Example 1.

[0145] Example 10

[0146] Except that the mass percentage of the electrolyte additive (C2H5MgBr) in the electrolyte formed in step 1) is 3%, other aspects are the same as those in Example 1.

[0147] Example 11

[0148] Except that the mass percentage of the electrolyte additive (C2H5MgBr) in the electrolyte formed in step 1) is 1%, the rest is the same as in Example 1.

[0149] Example 12

[0150] Except that the mass percentage of the electrolyte additive (C2H5MgBr) in the electrolyte formed in step 1) is 10%, other aspects are the same as those in Example 1.

[0151] Example 13

[0152] Except that the mass percentage of the electrolyte additive (C2H5MgBr) in the electrolyte formed in step 1) is 0.5%, other aspects are the same as those in Example 1.

[0153] Example 14

[0154] Except that n-butylmagnesium bromide (C4H9MgBr, Macklin) is used as the electrolyte additive in step 1), and the mass percentage of the electrolyte additive (C4H9MgBr) in the formed electrolyte is 3%, the rest is the same as Example 1.

[0155] Example 15

[0156] Except for step 1) using n-hexylmagnesium bromide (C6H 13 MgBr, Macklin) as an electrolyte additive, and the electrolyte additive (C6H 13Except that the mass percentage of MgBr) is 3%, other aspects are the same as those in Example 1.

[0157] Example 16

[0158] In addition to step 1) using n-dodecylmagnesium bromide (C 12 H 25 MgBr, Macklin) as an electrolyte additive, and the electrolyte additive (C 12 H 25 Except that the mass percentage of MgBr) is 3%, other aspects are the same as those in Example 1.

[0159] Example 17

[0160] Except that vinyl magnesium bromide (C2H3MgBr, Macklin) is used as the electrolyte additive in step 1), and the mass percentage of the electrolyte additive (C2H3MgBr) in the formed electrolyte is 3%, the rest is the same as Example 1.

[0161] Example 18

[0162] Except that diethyl magnesium ((C2H5)2Mg, Macklin) is used as the electrolyte additive in step 1) and the mass percentage of the electrolyte additive ((C2H5)2Mg) in the formed electrolyte is 3%, the rest is the same as Example 1.

[0163] Example 19

[0164] Except that n-propyl manganese chloride (C 3 H 7 MnCl, Macklin) is used as the electrolyte additive in step 1), and the mass percentage of the electrolyte additive (C 3 H 7 MnCl) in the formed electrolyte is 6%, the rest is the same as Example 1.

[0165] Example 20

[0166] Except for step 1) using n-pentylzinc iodide (C5H 11 ZnI, Macklin) as electrolyte additives, and the electrolyte additives in the formed electrolyte (C5H 11 The same as in Example 1 except that the mass percentage of ZnI) is 9%.

[0167] Example 21

[0168] Except that ethyl magnesium chloride (C2H5MgCl, Macklin) is used as the electrolyte additive in step 1), and the mass percentage of the electrolyte additive (C2H5MgCl) in the formed electrolyte is 3%, the rest is the same as Example 1.

[0169] Comparative Example 1

[0170] Except that no electrolyte additive was added, other aspects were the same as those in Example 1.

[0171] Comparative Example 2

[0172] Except that hexamethyldisilazane magnesium chloride (HMDSMgCl, Macklin) is used as the electrolyte additive in step 1), and the mass percentage of the electrolyte additive (HMDSMgCl) in the formed electrolyte is 3%, other aspects are the same as those in Example 1.

[0173] Comparative Example 3

[0174] Except that ethyl nickel bromide (C2H5NiBr, Macklin) is used as the electrolyte additive in step 1), and the mass percentage of the electrolyte additive (C2H5NiBr) in the formed electrolyte is 3%, the rest is the same as Example 1.

[0175] The performance of the batteries prepared in the above embodiments and comparative examples was tested:

[0176] (1) Full battery cycle performance test

[0177] Charging conditions: The battery was charged at room temperature (25°C) using constant current-constant voltage (CC-CV) mode. First, the battery was charged at a fixed rate of 0.2C in constant current mode until the voltage reached 3.65V. The battery was then switched to constant voltage mode with a cutoff current of 0.05C to fully charge.

[0178] Discharge conditions: Discharge in constant current mode at a discharge rate of 0.5C to 2V and cycle 200 times.

[0179] Each charge followed by discharge is a charge-discharge cycle process, and the first discharge capacity is the discharge capacity of the first cycle; repeat the above charge-discharge cycle process, and record the number of cycles when the discharge capacity retention rate is 50%.

[0180] (2) Half-cell overpotential test

[0181] A half-cell was made with 8μm copper foil as the positive electrode, 400μm lithium sheet as the negative electrode, and a polyethylene (PE) porous polymer film as the separator. The electrolyte used was the electrolyte of the above examples and comparative examples. The test method was: the battery was tested at 1mA / cm 2 The current density is discharged, and the lowest potential during the discharge process is recorded as the overpotential (indicates the battery's Li / Li + The potential of the copper foil is shown in FIG. 1 , which indicates that the lithium deposition potential of the copper foil is reduced after using the electrolyte of the embodiment of the present application).

[0182] The performance of the battery tested is shown in Table 1:

[0183] Table 1 Battery performance

[0184] Combined with the results in Table 1, we can see that:

[0185] The overpotential for lithium nucleation deposition on copper foil is -0.12V. The test results for Comparative Example 1 and Examples 1-21 show that the overpotential for lithium nucleation deposition on copper foil decreases after using the electrolytes of the present invention. Compared with Comparative Example 1, Examples 1-21 add an electrolyte additive (RMX, where R is a hydrocarbon group, M is a metal with a standard electrode potential higher than that of Li and capable of forming an intermetallic compound or alloy solid solution with Li, and X is a halogen or hydrocarbon group) to the electrolyte, which can reduce the lithium nucleation overpotential and improve battery cycling performance.

[0186] Compared with Comparative Example 1, the number of full battery cycles was significantly higher when the electrolyte additive dosage in Examples 1 and Examples 8 to 13 was within the range of 0.5% to 10%. Furthermore, the cycling performance was even better when the electrolyte additive dosage was between 1% and 10%. Furthermore, the cycling performance was even better when the electrolyte additive dosage was between 2% and 9%. Furthermore, the cycling performance was significantly better when the electrolyte additive dosage was between 3% and 6% than in other dosage ranges.

[0187] Compared with Comparative Examples 1 to 3, when the M metal in the electrolyte additive (RMX) of Examples 1 to 4 is Mg, Zn, Mn or Al, the battery cycle performance can be improved.

[0188] Compared with Comparative Example 1, R in the electrolyte additives (RMX) of Examples 1, 10, and 14 to 17 is a different hydrocarbon group, which can significantly improve the cycle performance of the battery. Among them, the hydrocarbon group with a carbon number of 1 to 10 has a more significant effect on improving the cycle performance of the battery than the hydrocarbon group with a larger carbon number.

[0189] Compared with Comparative Example 2, the R in the electrolyte additive (RMX) of Example 5 and Example 21 is a hydrocarbon group, which can reduce the nucleation overpotential of lithium and improve the battery cycle performance compared to when R is a non-hydrocarbon group.

[0190] According to the performance comparison between Example 10 and Example 18, when X in the electrolyte additive (RMX) is a halogen, the nucleation overpotential of lithium can be reduced compared to when X is a hydrocarbon group, and the cycle performance of the battery can be significantly improved.

[0191] Compared with Comparative Example 3, the M metal in the electrolyte additive (RMX) of Examples 1 to 4 can form an intermetallic compound or alloy solid solution with Li, which can reduce the nucleation overpotential of lithium and improve the battery cycle performance.

[0192] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of this application.

Claims

1. An electrolyte, characterized in that: The invention comprises an electrolyte additive, wherein the structure of the electrolyte additive comprises RMX, wherein R comprises a hydrocarbon group, M comprises a metal having a standard electrode potential higher than that of Li, X comprises an anion or a hydrocarbon group, the M can form an intermetallic compound or an alloy solid solution with Li, and the M is used to form a lithium-philic layer on the surface of the negative electrode current collector of the battery.

2. The electrolyte according to claim 1, characterized in that The mass percentage of the electrolyte additive is not greater than 10%.

3. The electrolyte according to claim 1, characterized in that The mass percentage of the electrolyte additive is 2% to 9%.

4. The electrolyte according to claim 1, characterized in that The mass percentage of the electrolyte additive is 3% to 6%.

5. The electrolyte according to claim 1 or 2, characterized in that: The M includes at least one of Mg, Al, Mn and Zn.

6. The electrolyte according to claim 1 or 2, characterized in that The R includes a hydrocarbon group having 1 to 10 carbon atoms.

7. The electrolyte according to claim 6, characterized in that The R includes C n H 2n+1 , n is 1 to 10.

8. The electrolyte according to claim 1 or 2, characterized in that: The X includes halogen.

9. The electrolyte according to claim 8, characterized in that The X is selected from at least one of Cl, Br, I and F.

10. The electrolyte according to claim 1 or 2, characterized in that: The X includes a hydrocarbon group.

11. The electrolyte according to claim 10, characterized in that The X includes a hydrocarbon group having 1 to 10 carbon atoms.

12. The electrolyte according to claim 6, characterized in that The M is Mg and X is Br.

13. A lithium metal battery, characterized in that: Using the electrolyte as described in any one of claims 1 to 12, the lithium metal battery includes a negative electrode, the negative electrode includes a negative electrode collector and a lithium-philic layer located on the surface of the negative electrode collector, the lithium-philic layer includes M, and M includes a metal having a standard electrode potential higher than Li and capable of forming an intermetallic compound or alloy solid solution with Li.

14. The lithium metal battery according to claim 13, characterized in that The average thickness of the lithium-philic layer is 50 nm to 100 nm.

15. The lithium metal battery according to claim 13 or 14, characterized in that: The negative electrode further includes an interface film located on the surface of the lithium-philic layer, and the thickness of the interface film does not exceed 1 μm.

16. The lithium metal battery according to claim 15, characterized in that The interface film contains LiX, wherein X includes an anion.

17. The lithium metal battery according to claim 16, characterized in that X includes halogen.

18. The lithium metal battery according to claim 15, characterized in that The interface film contains R, and the R includes a hydrocarbon group.

19. The lithium metal battery according to claim 18, characterized in that R includes a hydrocarbon group having 1 to 10 carbon atoms.

20. The lithium metal battery according to claim 13, characterized in that The invention also includes an electrolyte, wherein the electrolyte includes a lithium salt, and the lithium salt includes at least one of lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethyl)sulfonylimide, lithium bis(oxalatoborate), and lithium difluorooxalatoborate.

21. An electrical device, characterized in that: A lithium metal battery comprising the lithium metal battery according to any one of claims 13 to 20.

22. A method for preparing a lithium metal battery according to any one of claims 13 to 20, characterized in that: It includes the following steps: Assembling a positive electrode, a negative electrode current collector and an electrolyte into a battery, wherein the electrolyte comprises a lithium salt, an organic solvent and an electrolyte additive, and the structure of the electrolyte additive comprises RMX, wherein R comprises a hydrocarbon group, M comprises a metal having a standard electrode potential higher than that of Li, X comprises an anion or a hydrocarbon group, and the M can form an intermetallic compound or an alloy solid solution with Li; The battery is formed.

23. The method for preparing a lithium metal battery according to claim 22, characterized in that: The formation conditions are: firstly charge at a fixed rate of 0.15C to 0.25C in a constant current mode to a voltage of 3V to 4V, and then switch to a constant voltage mode with a cut-off current of 0.04C to 0.06C to fully charge the battery.

Citation Information

Patent Citations

  • Metal lithium support and preparation method and application thereof

    CN109585855A

  • Electrolyte and lithium ion battery containing the same and / or negative electrode

    CN109698314A

  • Preparation method of lithiophilicity negative electrode, lithium-lithium negative electrode and lithium battery

    CN110299513A

  • Electrolyte containing composite additive and application thereof

    CN113659203A

  • Electrolyte, lithium metal battery, preparation method of lithium metal battery and electric device

    CN116231085A

Cited By

  • High-voltage wide-temperature-range composite electrolyte of lithium metal battery as well as preparation and application of high-voltage wide-temperature-range composite electrolyte

    CN119650840A

  • High-voltage wide-temperature-range composite electrolyte for lithium metal battery and preparation and application thereof

    CN119650840B