Silicon dioxide ceramic material, foam ceramic filter, and preparation method and use
By using foam ceramic filters prepared with silica ceramic materials, the existing foam ceramic filters are solved, and the problems of high cost and insufficient heat resistance at high temperatures are achieved, and the filtration effect of low cost and high heat resistance is achieved. Suitable for liquid metal filtration at 1500~1600℃.
Patent Information
- Application Number
- PCT/CN2023/113466
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2023-08-17
- Publication Date
- 2024-11-14
AI Technical Summary
The existing foam ceramic filters are costly and have insufficient heat resistance at high temperatures, especially the zirconia foam ceramic filters are extremely costly and cannot effectively filter metal liquids of 1500-1600℃.
Using silica ceramic materials, including ceramic powders and auxiliary materials, by preparing silica foam ceramic filters, using components such as silica, alumina and silicon carbide, combined with binders and dispersants, to form high resistance. Thermal and low-cost filter has a maximum operating temperature of 1600℃.
A foam ceramic filter with low cost and high temperature resistance is realized, which can effectively filter metal liquids of 1500-1600℃, reduce production costs, and improve filtration efficiency and impact resistance.
Smart Images

Figure CN2023113466_14112024_PF_FP_ABST
Abstract
Description
Silica ceramic material, ceramic foam filter, and preparation method and application thereof
[0001] This application claims priority to the Chinese patent application filed with the Patent Office of China on May 10, 2023, with application number CN202310517405.1 and invention name “Silica Ceramic Materials, Foam Ceramic Filters, Preparation Methods and Applications”, the entire contents of which are incorporated by reference into this application. Technical Field
[0002] The present invention relates to the field of casting technology, in particular to a silicon dioxide ceramic material, a foam ceramic filter, a preparation method and an application thereof. Background Art
[0003] With the rapid development of the foundry industry, the requirements for the performance and appearance of castings are becoming increasingly stringent. Non-metallic inclusions in castings are the main cause of casting defects. They affect the surface finish, mechanical and processing properties of castings, and lead to increased scrap rates. Therefore, before filling the mold, it is necessary to filter out inclusions in the molten metal.
[0004] Currently, in the foundry industry, ceramic foam filters are commonly used to filter molten metal for iron and steel castings. Ceramic foam filters feature a three-dimensional mesh skeleton structure that effectively removes inclusions from the molten metal, reduces turbulence, and allows the molten metal to quickly and stably reach the mold filling velocity, thereby improving casting quality. Currently, silicon carbide (SiC) or zirconia (ZrO2) foam filters are commonly used. Both types of ceramic foam filters utilize silicon carbide (SiC) or zirconium oxide (ZrO2) powder as their primary raw materials, resulting in high costs. Zirconia foam filters are more expensive (approximately five times that of SiC foam filters). Furthermore, ceramic foam filters are disposable and consumable, placing significant financial pressure on users. Furthermore, SiC foam filters have a maximum operating temperature of 1500°C, while zirconium oxide filters have a maximum operating temperature of 1700°C. Therefore, for molten metals at temperatures between 1500 and 1600°C, zirconia foam filters are the only option. Currently, no cost-effective ceramic foam filter with a maximum operating temperature of 1600°C exists in the market.
[0005] Summary of the Invention
[0006] In light of this, the present invention provides a silica ceramic material, a ceramic foam filter, and preparation methods and applications. The silica ceramic material provided herein uses silica as its primary component. The silica foam filter prepared using the material is low-cost and has a maximum operating temperature of 1600°C, making it suitable for filtering molten metals at temperatures below 1600°C.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] A silicon dioxide ceramic material, comprising ceramic powder and auxiliary materials;
[0009] The ceramic powder comprises the following components by mass fraction: 40-80% silicon dioxide, 8-30% aluminum oxide, and 8-30% silicon carbide;
[0010] The auxiliary materials include a binder and a dispersant; the mass of the binder is 1-5% of the mass of the ceramic powder; the mass of the dispersant is 0.5-1% of the mass of the ceramic powder.
[0011] Preferably, the alumina is α-alumina; the mesh size of the alumina is greater than or equal to 200 meshes, and the purity is ≥98%;
[0012] The mesh size of the silicon dioxide is greater than or equal to 1000 mesh and the purity is greater than or equal to 95%;
[0013] The mesh number of the silicon carbide is greater than or equal to 200 meshes, and the purity is greater than or equal to 95%.
[0014] Preferably, the binder includes one or more of silica sol, methyl cellulose, white latex, sodium carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, phenolic resin and ethyl silicate; the dispersant includes sodium hexametaphosphate and / or sodium tripolyphosphate.
[0015] Preferably, the concentration of the silica sol is 30-50 wt%.
[0016] The present invention also provides a silica foam ceramic filter, which is prepared from the silica ceramic material described in the above solution.
[0017] Preferably, the crystal phase of silicon dioxide in the silicon dioxide foam ceramic filter is one or more of β-quartz, α-quartz, γ-tridymite, β-tridymite, α-tridymite, β-cristobalite, α-cristobalite and quartz glass.
[0018] Preferably, the silica foam ceramic filter has an open porosity of 80-83%.
[0019] The present invention also provides a method for preparing the silica foam ceramic filter described in the above scheme, comprising the following steps:
[0020] Mixing ceramic powder, auxiliary materials and water to obtain ceramic slurry;
[0021] impregnating a foam matrix in the ceramic slurry, and then removing excess slurry absorbed in the foam matrix to obtain a foam-impregnated green body;
[0022] The foam impregnated green body is dried and sintered in sequence to obtain the silica foam ceramic filter.
[0023] Preferably, the amount of water used is 15-25% of the mass of the ceramic powder.
[0024] Preferably, the viscosity of the ceramic slurry is 20,000 to 50,000 mPa·s.
[0025] Preferably, the foam matrix is porous polyurethane foam.
[0026] Preferably, the number of pores of the porous polyurethane foam is 10 to 20 PPI; the size of the porous polyurethane foam is (75 to 100) mm×(75 to 100) mm×22 mm.
[0027] Preferably, the drying is oven drying or natural drying, the oven drying temperature is 100-120° C., and the time is 60-90 min; the time of natural drying is 6-12 h.
[0028] Preferably, the sintering temperature is 1150-1300°C and the holding time is 2-4h;
[0029] The procedure for heating to the sintering temperature is: heating to the first temperature at a first heating rate, then heating to the second temperature at a second heating rate, and then heating to the sintering temperature at a third heating rate; the first heating rate is 70-90°C / h, and the first temperature is 500-550°C; the second heating rate is 200-250°C / h, and the second temperature is 1000-1100°C; the third heating rate is 70-90°C / h.
[0030] The present invention also provides the use of the silica foam ceramic filter described in the above solution or the silica foam ceramic filter prepared by the preparation method described in the above solution in casting.
[0031] Preferably, the operating temperature of the silica foam ceramic filter is ≤1600°C.
[0032] The present invention provides a silica ceramic material comprising ceramic powder and auxiliary materials. The ceramic powder comprises the following components by mass: 40-80% silica, 8-30% alumina, and 8-30% silicon carbide. The auxiliary materials include a binder and a dispersant. The binder comprises 1-5% of the ceramic powder, and the dispersant comprises 0.5-1% of the ceramic powder. The silica ceramic material provided by the present invention has silica as its primary component, is readily available from a wide range of raw materials, is low in cost, and exhibits excellent high-temperature resistance.
[0033] The present invention also provides a silica ceramic foam filter, prepared from the silica ceramic material described in the above scheme. The silica ceramic foam filter provided by the present invention uses silica as its primary raw material. Silica is widely available and low-cost, costing only about 50% of silicon carbide powder. The resulting ceramic foam filter significantly reduces the cost of silicon carbide and zirconia ceramic foam filters commonly used in the field. Furthermore, the silica ceramic foam filter provided by the present invention exhibits excellent heat resistance, with a maximum operating temperature of 1600°C, filling the gap in ceramic foam filters operating within the 1500-1600°C temperature range. Furthermore, the silica ceramic foam filter provided by the present invention exhibits excellent filtration performance, effectively filtering inclusions from molten metal. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] FIG1 is a process flow chart for preparing a silica ceramic foam filter according to an embodiment of the present invention. DETAILED DESCRIPTION
[0035] The present invention provides a silicon dioxide ceramic material, including ceramic powder and auxiliary materials;
[0036] The ceramic powder comprises the following components by mass fraction: 40-80% silicon dioxide, 8-30% aluminum oxide, and 8-30% silicon carbide;
[0037] The auxiliary materials include a binder and a dispersant; the mass of the binder is 1-5% of the mass of the ceramic powder; the mass of the dispersant is 0.5-1% of the mass of the ceramic powder.
[0038] Unless otherwise specified, all raw materials used in the present invention are commercially available products.
[0039] The silica ceramic material provided by the present invention includes ceramic powder and auxiliary materials, which are described in detail below.
[0040] In terms of mass fraction, the ceramic powder includes 40 to 80% silicon dioxide, preferably 40 to 75%. In the present invention, the mesh size of the silicon dioxide is preferably greater than or equal to 200 mesh (i.e., the particle size of the silicon dioxide is less than or equal to 74 μm), and the purity is preferably ≥95%. The present invention has no special requirements for the silicon dioxide, and the silicon dioxide powder commonly used in the art can be used. In the present invention, the silicon dioxide mainly plays a skeleton role, which is beneficial to improving the impact resistance of the foam ceramic filter at high temperatures. In the art, silicon dioxide is often added to silicon carbide foam ceramic filters as a sintering aid in order to reduce the sintering temperature and improve the sintering effect, but the amount added is very small. The present invention uses silicon dioxide as the main raw material to provide a silicon dioxide ceramic material. The foam ceramic filter prepared using the ceramic material of the present invention not only has good filtration performance and good heat resistance, but also has greatly reduced costs.
[0041] The ceramic powder comprises 8-30% by mass, preferably 10-25% alumina. In the present invention, the alumina is preferably α-alumina; the mesh size of the alumina is preferably greater than or equal to 1000 mesh (i.e., the particle size of the alumina is ≤13 μm), and the purity is preferably ≥98%. The alumina acts as a matrix, which helps to improve the sintering strength of the foam ceramic filter and reduce the firing temperature of the product.
[0042] The ceramic powder comprises 8-30% silicon carbide by mass, preferably 10-20%, and more preferably 10-15%. In the present invention, the silicon carbide preferably has a mesh size of 1000 or greater (i.e., a particle size of 13 μm or less) and a purity of 95% or greater. The silicon carbide can increase the thermal conductivity and reduce the coefficient of expansion of the ceramic foam filter, thereby improving the thermal stability of the product.
[0043] In the present invention, the auxiliary materials preferably include a binder and a dispersant; the mass of the binder is 1-5% of the mass of the ceramic powder, preferably 2-4%; the mass of the dispersant is 0.5-1% of the mass of the ceramic powder, preferably 0.6-0.8%.
[0044] In the present invention, the binder preferably includes one or more of silica sol, methyl cellulose, white latex, sodium carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, phenolic resin and ethyl silicate; the concentration of the silica sol is preferably 30-50wt%, more preferably 40wt%; the dispersant preferably includes sodium hexametaphosphate and / or sodium tripolyphosphate.
[0045] The present invention also provides a silica ceramic foam filter prepared from the silica ceramic material described in the above scheme; the crystal phase of the silica in the silica ceramic foam filter is preferably one or more of β-quartz, α-quartz, γ-tridymite, β-tridymite, α-tridymite, β-cristobalite, α-cristobalite, and quartz glass; the present invention strictly controls the ratio of ceramic powder and auxiliary materials in the silica ceramic material, and can produce a foam ceramic filter with excellent filtration performance and heat resistance using silica as the main raw material, meeting the requirements of molten metal filtration. In the present invention, the total porosity of the silica ceramic foam filter is preferably 78-85%, and the open porosity is preferably 80-83%.
[0046] The present invention also provides a method for preparing the silica foam ceramic filter described in the above scheme, comprising the following steps:
[0047] Mixing ceramic powder, auxiliary materials and water to obtain ceramic slurry;
[0048] impregnating a foam matrix in the ceramic slurry, and then removing excess slurry absorbed in the foam matrix to obtain a foam-impregnated green body;
[0049] The foam impregnated green body is dried and sintered in sequence to obtain the silica foam ceramic filter.
[0050] The present invention mixes ceramic powder, auxiliary materials, and water to obtain a ceramic slurry. In the present invention, the amount of water used is preferably 15-25% by mass of the ceramic powder, more preferably 18-22%. The mixing is preferably performed using a high-speed mixer. The viscosity of the ceramic slurry is preferably 20,000-50,000 mPa·s, more preferably 20,000-30,000 mPa·s or 40,000-50,000 mPa·s.
[0051] After obtaining the ceramic slurry, the present invention immerses the foam matrix in the ceramic slurry, and then removes the excess slurry absorbed in the foam matrix to obtain a foam-impregnated green body. In the present invention, the foam matrix is preferably porous polyurethane foam, and the number of pores of the porous polyurethane foam is preferably 10 to 20 PPI; the size of the porous polyurethane foam is preferably (75 to 100) mm × (75 to 100) mm × 22 mm; in a specific embodiment of the present invention, the porous polyurethane foam also includes the steps of cutting and slicing and die-cutting before impregnation to obtain a porous polyurethane foam that meets the size requirements; in the present invention, the impregnation temperature is preferably room temperature, and the impregnation time is preferably 1 to 3 minutes; the present invention has no special requirements for the specific operating conditions of the impregnation, and the porous polyurethane foam is placed in the ceramic slurry and fully impregnated; in the present invention, the method for removing excess slurry adsorbed in the foam matrix is preferably extrusion, and the extrusion is preferably carried out by a roller press, and the gap of the roller press is preferably 2 to 10 mm. The present invention squeezes out about 60% of the slurry impregnated in the foam matrix by controlling the gap of the roller press to obtain a foam impregnated blank.
[0052] After obtaining the foam-impregnated body, the present invention sequentially dries and sinters the foam-impregnated body to obtain the silica foam ceramic filter. In the present invention, the drying is preferably oven drying or natural drying. The oven drying temperature is preferably 100-120°C, preferably 105-110°C, and the oven drying time is preferably 60-90 minutes, more preferably 60-70 minutes. The natural drying time is preferably 6-12 hours, more preferably 8-10 hours.
[0053] In the present invention, the sintering temperature is preferably 1150-1300°C, more preferably 1200-1250°C, the sintering holding time is preferably 2-4h, more preferably 2.5-3.5h; the procedure for heating to the sintering temperature is preferably: heating to the first temperature at a first heating rate, then heating to the second temperature at a second heating rate, and then heating to the sintering temperature at a third heating rate; the first heating rate is preferably 70-90°C / h, more preferably 75-85°C / h; the first temperature is preferably 500-550°C, more preferably 500-520°C; the second ... The heating rate is preferably 200-250°C / h, more preferably 230-250°C / h, the second temperature is preferably 1000-1100°C, more preferably 1000-1050°C; the third heating rate is preferably 70-90°C / h, more preferably 75-85°C / h; the present invention preferably heats according to the above method, which is useful for uniformly heating the foam impregnated body and improving the sintering effect; during the sintering process, the foam matrix is decomposed by heat, leaving a foam-like ceramic product, which is the silica foam ceramic filter of the present invention; after the insulation is completed, the obtained product is cooled to 100°C in the furnace and then taken out.
[0054] The present invention also provides the use of the silica ceramic foam filter described in the above embodiment, or the silica ceramic foam filter prepared by the preparation method described in the above embodiment, in casting. In the present invention, the silica ceramic foam filter is used to filter molten metal during the casting process. The operating temperature of the silica ceramic foam filter is preferably ≤ 1600°C, more preferably 1500-1600°C.
[0055] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative efforts are within the scope of protection of the present invention.
[0056] Figure 1 is a process flow chart for preparing a silica foam ceramic filter in an embodiment of the present invention, wherein porous polyurethane foam (i.e., polyurethane sponge) is first cut, sliced, and die-cut into shape, then impregnated with ceramic slurry, and then dried and fired. The resulting product is packaged and stored after passing inspection.
[0057] Example 1
[0058] 40 kg of commercially available 95% purity, 200 mesh silica, 30 kg of 98% purity, 1000 mesh α-alumina, 30 kg of 95% purity, 1000 mesh silicon carbide, 15 kg of pure water, 5 kg of silica sol (concentration of 40wt%) and 1.0 kg of sodium hexametaphosphate were added, and stirred evenly in a high-speed mixer to form a thixotropic mud with a viscosity of 40,000 mPa.s, which is the ceramic slurry. A 10PPI (100×100×22mm) polyurethane foam was immersed in the prepared ceramic slurry, fully impregnated, and then approximately 60% of the slurry was squeezed out through a roller press to obtain a foam-impregnated green body. The resulting foam-impregnated green body was dried at 110°C for 1 hour, then placed in a sintering furnace and heated to 500°C at a heating rate of 90°C / h, then to 1000°C at a heating rate of 250°C / h, and then to 1150°C at a heating rate of 90°C / h, held at this temperature for 2 hours, and then cooled to approximately 100°C in the furnace before removal. This resulted in a silica foam ceramic filter with specifications of 100×100×22mm (10PPI). Testing revealed that the open porosity of the silica foam ceramic filter was 82%.
[0059] The silica foam ceramic filter prepared in Example 1 was used to filter molten steel at a temperature of 1527° C., and inclusions in the molten steel were effectively filtered with a filtration efficiency of 95%. 800 kg of filtered molten steel was not dispersed. After filtering 800 kg of molten steel using the silica foam ceramic filter prepared in Example 1, the filter remained intact, indicating that it has good impact resistance.
[0060] Molten steel at a temperature of 1527°C was filtered using an ordinary silicon carbide foam ceramic filter. The results showed that the silicon carbide foam ceramic filter was broken when filtering 500 kg, indicating that ordinary silicon carbide foam ceramic filters are difficult to filter molten metal above 1500°C. The silica foam ceramic filter provided by the present invention is not only low in cost, but also has good high temperature resistance and impact resistance, and is suitable for filtering molten metal at 1500-1600°C.
[0061] Example 2
[0062] 75 kg of commercially available 98% purity, 325 mesh silica, 10 kg of 99% purity, 2000 mesh α-alumina, 15 kg of 96% purity, 3000 mesh silicon carbide, 18 kg of pure water, 3 kg of polyvinyl alcohol and 0.5 kg of sodium tripolyphosphate are added, and stirred evenly in a high-speed mixer to obtain a thixotropic mud with a viscosity of 30,000 mPa.s, which is the ceramic slurry. A 20PPI (75×75×22mm) polyurethane foam was impregnated into the prepared ceramic slurry. After thorough impregnation, approximately 60% of the slurry was squeezed out by roller pressing to obtain a foam-impregnated body. The foam-impregnated body was then naturally dried for 12 hours. The body was then placed in a sintering furnace and heated to 500°C at a heating rate of 90°C / h, then to 1000°C at a heating rate of 250°C / h, and then to 1250°C at a heating rate of 90°C / h. The temperature was maintained for 2 hours, and the body was cooled to 100°C in the furnace before removal. This resulted in a silica foam ceramic filter with specifications of 75×75×22mm (20PPI). Testing revealed that the open porosity of the silica foam ceramic filter was 81%.
[0063] The silica foam ceramic filter prepared in Example 2 was used to filter molten steel at a temperature of 1600° C., which effectively filtered out inclusions in the molten steel with a filtration efficiency of 96%, and 500 kg of filtered molten steel was not dispersed.
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as within the scope of protection of the present invention.
Claims
1. A silicon dioxide ceramic material, It is characterized in that Including ceramic powder and auxiliary materials; The ceramic powder comprises the following components by mass fraction: 40-80% silicon dioxide, 8-30% aluminum oxide, and 8-30% silicon carbide; The auxiliary materials include a binder and a dispersant; the mass of the binder is 1-5% of the mass of the ceramic powder; the mass of the dispersant is 0.5-1% of the mass of the ceramic powder.
2. The silica ceramic material according to claim 1, It is characterized in that The alumina is α-alumina; the mesh number of the alumina is greater than or equal to 200 meshes, and the purity is greater than or equal to 98%; The mesh number of the silicon dioxide is greater than or equal to 1000 mesh, and the purity is ≥95%; The mesh number of the silicon carbide is greater than or equal to 200 meshes, and the purity is greater than or equal to 95%.
3. The silica ceramic material according to claim 1, It is characterized in that The binder includes one or more of silica sol, methyl cellulose, white latex, sodium carboxymethyl cellulose, polyvinyl alcohol, polyvinyl butyral, phenolic resin and ethyl silicate; the dispersant includes sodium hexametaphosphate and / or sodium tripolyphosphate.
4. The silicon dioxide ceramic material according to claim 3, It is characterized in that The concentration of the silica sol is 30-50 wt %.
5. A silica foam ceramic filter, It is characterized in that The silica ceramic material is prepared from the silica ceramic material according to any one of claims 1 to 4.
6. The silica ceramic foam filter according to claim 5, It is characterized in that The crystal phase of silicon dioxide in the silicon dioxide foam ceramic filter is one or more of β-quartz, α-quartz, γ-tridymite, β-tridymite, α-tridymite, β-cristobalite, α-cristobalite and quartz glass.
7. The silica ceramic foam filter according to claim 5, It is characterized in that The open porosity of the silica ceramic foam filter is 80-83%.
8. A method for preparing the silica ceramic foam filter according to any one of claims 5 to 7, It is characterized in that The following steps are involved: Mixing ceramic powder, auxiliary materials and water to obtain ceramic slurry; Impregnating a foam matrix in the ceramic slurry, and then removing excess slurry absorbed in the foam matrix to obtain a foam impregnated body; The foam impregnated green body is dried and sintered in sequence to obtain the silicon dioxide foam ceramic. Porcelain filter.
9. The preparation method according to claim 8, It is characterized in that The amount of water used is 15-25% of the mass of the ceramic powder.
10. The preparation method according to claim 8, It is characterized in that The viscosity of the ceramic slurry is 20000-50000 mpa·s.
11. The preparation method according to claim 8, It is characterized in that The foam matrix is porous polyurethane foam.
12. The preparation method according to claim 8, It is characterized in that The number of pores of the porous polyurethane foam is 10-20 PPI; the size of the porous polyurethane foam is (75-100) mm×(75-100) mm×22 mm.
13. The preparation method according to claim 8, It is characterized in that The drying is oven drying or natural drying. The oven drying temperature is 100-120° C. and the time is 60-90 minutes. The time of natural drying is 6-12 hours.
14. The preparation method according to claim 8, It is characterized in that The sintering temperature is 1150-1300°C and the holding time is 2-4h; The procedure for heating to the sintering temperature is: heating to the first temperature at a first heating rate, then heating to the second temperature at a second heating rate, and then heating to the sintering temperature at a third heating rate; the first heating rate is 70-90°C / h, and the first temperature is 500-550°C; the second heating rate is 200-250°C / h, and the second temperature is 1000-1100°C; the third heating rate is 70-90°C / h.
15. Use of the silica foam ceramic filter according to any one of claims 5 to 7 or the silica foam ceramic filter prepared by the preparation method according to any one of claims 8 to 14 in casting.
16. The use according to claim 15, It is characterized in that The operating temperature of the silica ceramic foam filter is ≤1600°C.
Citation Information
Patent Citations
Method for preparing foam ceramic filter and filter produced by the method
CN101117295A
Mullite ceramic foam filter for casting and preparation method thereof
CN102173856A
Ceramic foam filter, composition for preparing ceramic foam filter and preparation method for ceramic foam filter
CN102557713A
Foamed ceramic filter and making method thereof
CN106220218A
Preparation method for porous ceramic with adjustable pore diameter
CN108689722A