Flame-retardant material

Through the compounding technology of adding halogen-free environmentally friendly flame retardant at low amount, the industrial production and environmental safety problems of polyhydroxy fatty acid ester materials are solved, and the V-0 level flame retardant performance and material performance are achieved, and the production is simplified. Craft.

WO2024230453A1PCT designated stage expired Publication Date: 2024-11-14BEIJING PHABUILDER BIOTECHNOLOGY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
PCT/CN2024/088840
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-09
Filing Date
2024-04-19
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

The synthesis process of existing polyhydroxy fatty acid ester materials is difficult to produce in industrialized, and it is expensive, and the amount of added inorganic flame retardant is large, resulting in a decline in material performance and cannot meet the requirements of flame retardant and environmental safety.

Method used

Using a low amount of added halogen-free environmentally friendly flame retardant, a stable carbonization layer and foam structure is formed through the combination of bio-based phosphorus, polyhydroxy and nitrogen flame retardants, which improves the flame retardant performance of the material while maintaining the material's Other performance.

Benefits of technology

The V-0 flame retardant performance of halogen-free environmentally friendly polyhydroxy fatty acid ester material is achieved, the amount of flame retardant is reduced, the production process is simplified, the production process is suitable for industrial production, and the comprehensive performance of the material is ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure PCTCN2024088840-FTAPPB-I100001
    Figure PCTCN2024088840-FTAPPB-I100001
  • Figure PCTCN2024088840-FTAPPB-I100002
    Figure PCTCN2024088840-FTAPPB-I100002
  • Figure PCTCN2024088840-FTAPPB-I100003
    Figure PCTCN2024088840-FTAPPB-I100003
Patent Text Reader

Abstract

The present invention relates to the technical field of flame-retardant polymer materials, and particularly relates to a flame-retardant material and a preparation method therefor. The flame-retardant material comprises a polyhydroxyalkanoate, a halogen-free flame retardant and an auxiliary agent, wherein the halogen-free flame retardant comprises a bio-based phosphorus flame retardant, a bio-based poly-hydroxyl flame retardant and a bio-based nitrogen flame retardant. The flame-retardant material prepared in the present invention has good comprehensive properties, is halogen-free and environment-friendly, involves small flame retardant dosages, mostly involves bio-based materials and achieves a flame-retardant effect of V-0 class, and therefore the flame-retardant material can satisfy the flame retardance requirements in the application fields requiring materials to have flame-retardant properties, such as building and construction materials, home decoration and home textiles, aerospaces, military industry, automobiles and packaging.
Need to check novelty before this filing date? Find Prior Art

Description

A flame retardant material Technical Field

[0001] The present invention relates to the technical field of flame-retardant polymer materials, and in particular to a flame-retardant degradable polyhydroxyalkanoate (PHA) material. Background Art

[0002] With the rapid development of the economy, people's living standards are improving, and people's requirements for environmental quality are getting higher and higher. However, the global use of non-degradable disposable plastics has exacerbated the white pollution of the human living environment. Common biodegradable materials at home and abroad, such as polylactic acid (PLA), polycaprolactone (PCL), polybutylene adipate / terephthalate (PBAT), polybutylene succinate (PBS) and polyhydroxyalkanoates (PHA), have developed well, their performance has been continuously improved, and their applications are becoming more and more extensive, such as daily necessities, medical fields, packaging fields, catering fields, etc. However, because biodegradable materials have a low limiting oxygen index of only about 20, they are usually flammable, so they are greatly limited in application areas that require flame retardancy.

[0003] Flame-retardant biodegradable materials primarily focus on PLA, PBS, and PBAT. For example, Patent Publication No. CN1733828A discloses flame-retardant polyester materials achieved through synthetic methods. Patent Publication No. CN101010381A discloses the preparation of flame-retardant injection molded products using metal hydroxides, PLA, and acrylic resins. Patent Publication No. CN101148498A discloses flame-retardant polyesters achieved by copolymerizing a phosphorus-containing component with polyester to form a degradable, flame-retardant copolyester and blending it with an aliphatic copolyester. Publication No. CN101245174A discloses a method for flame-retarding PBS and PLA blends using aluminum hydroxide. However, research on flame-retardant modification of polyhydroxyalkanoates is limited, with only a few literature reports. Publication No. CN1733828A uses a synthetic method to achieve flame retardancy, but this method has drawbacks: first, it is difficult to commercialize and is costly; second, the toxicity of bromine combustion is detrimental to environmental protection and human safety, and this aspect has been restricted by countries such as the European Union. Publication No. CN102924888A discloses a method for flame-retarding PHA with sodium aluminum hydroxide. This method primarily employs the addition of inorganic salts, but only large amounts are required to achieve the desired flame retardant effect, ultimately degrading the material's other physical properties. Therefore, there is an urgent need to develop polyhydroxyalkanoate materials with excellent flame retardancy while maintaining superior material properties.

[0004] Summary of the Invention

[0005] The purpose of the present invention is to overcome the problems in the prior art that the synthesis process is difficult to industrialize and is costly, and that a large amount of inorganic flame retardant is added, which reduces the performance of the material itself.

[0006] In order to achieve the above object, the present invention adopts a low amount of halogen-free environmentally friendly flame retardant to prepare a biodegradable polyhydroxyalkanoate material with good flame retardancy and good comprehensive material properties and environmental safety.

[0007] The invention provides a flame retardant material, which comprises polyhydroxyalkanoate and a halogen-free flame retardant.

[0008] Preferably, the mass ratio of polyhydroxyalkanoate to halogen-free flame retardant is (2-9): 1, preferably (3-6): 1 or (4-6.5): 1. For example, the mass ratio can be (2, 2.5, 3, 3.5, 4, 4.3, 4.5, 4.8, 5, 5.5, 5.6, 5.7, 6, 6.3, 6.4, 6.5, 7, 8, 9): 1.

[0009] Preferably, the amount of the halogen-free flame retardant added is 5%-20% of the flame retardant material in terms of mass ratio, preferably 9%-20%, for example 5%, 8%, 9%, 10%, 13%, 14%, 15%, 16%, 17%, 18%, 20%.

[0010] In a specific embodiment of the present invention, the flame retardant material comprises 95-140 (e.g., 95, 100, 105, 110, 115, 120, 130, 135, 140) parts of polyhydroxyalkanoate and 15-25 (e.g., 15, 20, 18.5, 25) parts of halogen-free flame retardant in parts by mass.

[0011] The polyhydroxyalkanoate comprises a homopolymer or copolymer (such as a random copolymer and a block copolymer) of the monomers constituting the polyhydroxyalkanoate. Further preferably, the PHA comprises a monomer, dimer or polymer of the monomers constituting the PHA, and a material in which the monomers constituting the PHA are polymerized with other substances.

[0012] Preferably, the monomers constituting the polyhydroxyalkanoate include one, two or more of 2-hydroxypropionic acid, 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxypentanoic acid, 5-hydroxypentanoic acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid and 3-hydroxydodecanoic acid. Further preferably, the polyhydroxyalkanoate includes one, two or more of P(HA-LA), P3HP, PHB, P4HB, PHV, PHO, PHN, PHD, PHBV, P34HB, PHBHHp, PHBHHx, P3HB4HB3HV or P3HB4HB5HV. Among them, HA in P(HA-LA) is selected from one, two or more of 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid and 3-hydroxydodecanoic acid; LA is 2-hydroxypropionic acid.

[0013] Preferably, the polyhydroxyalkanoate can be prepared by chemical synthesis, biological fermentation or purchased.

[0014] The molar content of 4HB in the P34HB is any value between 1% and 30%, for example, 1%, 5%, 10%, 15%, 20%, 25%, or 30%. Preferably, the molar content of 4HB in the P34HB is between 10% and 20%.

[0015] The molar content of 3HV in the PHBV is any value between 1% and 30%, such as 1%, 5%, 10%, 15%, 20%, 25%, and 30%. Preferably, the molar content of 3HV in the PHBV is between 5% and 15%.

[0016] The molar content of HHx in the PHBHHx is any value between 1% and 30%, for example, 1%, 5%, 10%, 15%, 20%, 25%, and 30%. Preferably, the molar content of HHx in the PHBHHx is between 1% and 10%.

[0017] Depending on the needs of the specific embodiment, the polyhydroxyalkanoate can be a single species or a combination of two or more. For example, in one embodiment of the present invention, the polyhydroxyalkanoate is 15 parts of PHB and 120 parts of P34HB (preferably a 4HB molar content of 15%), calculated by weight. In another embodiment of the present invention, the polyhydroxyalkanoate is 60 parts of PHBV (preferably a 3HV molar content of 10%) and 60 parts of PHBHHx (preferably a HHx molar content of 5%), calculated by weight. In another embodiment of the present invention, the polyhydroxyalkanoate is 60 parts of PHBV (preferably a 3HV molar content of 5%) and 60 parts of P34HB (preferably a HHx molar content of 25%).

[0018] The halogen-free flame retardant includes but is not limited to one or a combination of two or more of silicon-based flame retardants, bio-based phosphorus-based flame retardants, bio-based polyhydroxy flame retardants or bio-based nitrogen-based flame retardants.

[0019] Preferably, the halogen-free flame retardant includes a bio-based phosphorus flame retardant, a bio-based polyhydroxy flame retardant and / or a bio-based nitrogen flame retardant. Further preferably, the halogen-free flame retardant also includes a silicon flame retardant.

[0020] In one embodiment of the present invention, the halogen-free flame retardant comprises a bio-based phosphorus flame retardant, a bio-based polyhydroxy flame retardant, and a bio-based nitrogen flame retardant. Preferably, the halogen-free flame retardant comprises 4.5-11 (e.g., 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11) parts of the bio-based phosphorus flame retardant, 3-6 (3, 3.5, 4, 4.5, 5, 5.5, 6) parts of the bio-based polyhydroxy flame retardant, and 3-6 (3, 3.5, 4, 4.5, 5, 5.5, 6) parts of the bio-based nitrogen flame retardant, in parts by mass.

[0021] Preferably, the halogen-free flame retardant comprises a bio-based phosphorus flame retardant as a main flame retardant, and a bio-based polyhydroxy flame retardant and a bio-based nitrogen flame retardant as auxiliary flame retardants.

[0022] In one embodiment of the present invention, the bio-based phosphorus flame retardant is present in an amount greater than the bio-based polyhydroxy flame retardant and the bio-based nitrogen flame retardant in parts by weight. Preferably, the total amount of the bio-based polyhydroxy flame retardant and the bio-based nitrogen flame retardant added is approximately 1.5-2.5 times the amount of the bio-based phosphorus flame retardant added, for example, 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2, 2.1, 2.2, 2.3, 2.4, 2.5 times, etc.

[0023] In a specific embodiment of the present invention, the ratio of the bio-based phosphorus flame retardant, the bio-based polyhydroxy flame retardant and the bio-based nitrogen flame retardant can be (1.5-2.2): (0.8-1.2): (0.8-1.2) by mass.

[0024] In a specific embodiment of the present invention, the halogen-free flame retardant includes a silicon flame retardant, a bio-based phosphorus flame retardant, a bio-based polyhydroxy flame retardant, and a bio-based nitrogen flame retardant. Preferably, based on parts by mass, the halogen-free flame retardant includes 0-6 (e.g., 0, 1, 2, 3, 3.5, 4, 4.5, 5, 5.5, 6) parts of silicon flame retardant, 4.5-11 (e.g., 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11) parts of bio-based phosphorus flame retardant, 3-6 (3, 3.5, 4, 4.5, 5, 5.5, 6) parts of bio-based polyhydroxy flame retardant, and 3-6 (3, 3.5, 4, 4.5, 5, 5.5, 6) parts of bio-based nitrogen flame retardant.

[0025] The bio-based phosphorus flame retardant includes but is not limited to one, two or three of DOPO-modified castor oil, phytic acid or sodium phytate.

[0026] The bio-based polyhydroxy flame retardant includes but is not limited to one or a combination of two or more of starch, lignin, cellulose, chitosan, cyclodextrin, tannic acid or itaconic acid.

[0027] The bio-based nitrogen flame retardant includes but is not limited to urea and / or urea-compounded melamine. Preferably, the urea-compounded melamine is prepared by blending (preferably physically blending) urea and melamine in a molar ratio of (1-3):2.

[0028] The silicon-based flame retardant includes but is not limited to one or a combination of two or more of polysilicon boroxane, organic silicon-based fire retardant 3820 or silicon-based flame retardant FCA-107.

[0029] The flame retardant material further includes an additive. The additive is added in an amount of 0% to 7% by mass of the flame retardant material, preferably 0.5% to 4% or 0.05-0.1% or 0.5% to 3.8%, for example, 0.01%, 0.0125%, 0.015%, 0.017%, 0.02%, 0.05%, 0.1%, 0.5%, 1%, 2%, 3%, 3.8%, 4%, 5%, 6%, or 7%.

[0030] In the flame retardant material, the mass ratio of polyhydroxyalkanoate: halogen-free flame retardant: auxiliary agent is (95-140): (15-25): (0%-7%).

[0031] The auxiliary agents include but are not limited to coupling agents, dispersants, lubricants, anti-dripping agents and antioxidants, one or a combination of two or more thereof.

[0032] Preferably, the coupling agent includes but is not limited to one or a combination of two or more of the following: silane coupling agent KH-792, silane coupling agent DL-602, silane coupling agent Y-5475, silane coupling agent Y-5669, titanate coupling agent TMC-201, titanate coupling agent TMC-102, and titanate coupling agent TMC-311.

[0033] Preferably, the dispersant includes but is not limited to one, two or three of ethylene bisstearamide, stearic acid monoglyceride and tristearin.

[0034] Preferably, the lubricant includes but is not limited to low molecular weight fully degradable polyester (eg, 2000-10000 g / mol) and / or low molecular weight PHA (eg, 2500-10000 g / mol).

[0035] Preferably, the anti-dripping agent includes but is not limited to PTFE powder TRG-460 and / or PTFE powder FS-200;

[0036] Preferably, the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] and / or tris(2,4-di-tert-butylphenyl) phosphite; more preferably, the mass ratio of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] to tris(2,4-di-tert-butylphenyl) phosphite is (2-4):1.

[0037] In a specific embodiment of the present invention, the flame retardant material consists of polyhydroxyalkanoate and halogen-free flame retardant.

[0038] In another specific embodiment of the present invention, the flame retardant material consists of polyhydroxyalkanoate, halogen-free flame retardant and additives.

[0039] In a specific embodiment of the present invention, the flame retardant material comprises, by mass:

[0040] Polyhydroxyalkanoate: 95-140 parts, for example, 95, 100, 105, 110, 115, 120, 130, 135, 140 parts;

[0041] Halogen-free flame retardant: 15-25 parts, for example, 15, 20, 18.5, 25 parts;

[0042] Coupling agent: 0.01-1 part, preferably 0.1-0.5 part, for example 0.01, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1;

[0043] Dispersant: 0.01-2 parts, preferably 0.1-1.5 parts, for example 0.01, 0.1, 0.3, 0.5, 0.7, 0.8, 0.9, 1, 1.2, 1.5, 2;

[0044] Lubricant: 0.01-1.5 parts, preferably 0.1-1 parts, such as 0.01, 0.1, 0.3, 0.5, 0.7, 0.9, 1, 1.5;

[0045] Anti-dripping agent: 0.01-1 part, preferably 0.1-0.3 part, such as 0.01, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1;

[0046] Antioxidant: 0.01-1 part, preferably 0.1-0.5 part, for example 0.01, 0.1, 0.2, 0.3, 0.35, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.

[0047] In a specific embodiment of the present invention, the flame retardant material comprises, by mass:

[0048] Polyhydroxyalkanoate: 95-140 parts; halogen-free flame retardant: 15-25 parts; auxiliary agent: 0.5-2.15 parts.

[0049] In a specific embodiment of the present invention, the flame retardant material comprises, by mass:

[0050] Polyhydroxyalkanoate: 95-140 parts; halogen-free flame retardant: 15-25 parts; coupling agent: 0.3 parts; dispersant: 0.8 parts; lubricant 0.5 parts; anti-dripping agent: 0.2 parts; antioxidant: 0.3 or 0.35.

[0051] The flame retardant material of the present invention can be prepared by conventional methods in the prior art.

[0052] The present invention also provides a method for preparing the flame-retardant material, comprising mixing raw materials, then melt-blending and extruding the mixture in a twin-screw extruder, and air-cooling and pelletizing the resulting mixture into strands. The raw materials include polyhydroxyalkanoate and a halogen-free flame retardant. An auxiliary agent is preferably also included.

[0053] Preferably, the twin-screw processing temperature is 140-160°C.

[0054] In a specific embodiment of the present invention, the preparation method comprises weighing polyhydroxyalkanoate and halogen-free flame retardant (preferably including auxiliary agent) according to the mass ratio or mass fraction listed above for the flame retardant material, adding them into a high-speed mixer and mixing for 5-10 minutes, then discharging the materials into a twin-screw extruder for melt blending and extrusion, and air-cooling the strands for granulation, wherein the twin-screw processing temperature is 140-160°C.

[0055] The present invention also provides a use of the flame retardant material in products requiring flame retardant properties. Preferably, the products include construction materials, home furnishings and textiles, aerospace, military, automotive or packaging materials.

[0056] Through the above technical solution, the present invention has the following advantages:

[0057] (1) The flame retardant material used in the present invention is halogen-free and environmentally friendly, and is mainly composed of bio-based flame retardants, does not generate pollution, and can achieve V-0 flame retardancy.

[0058] (2) The present invention uses multiple types of flame retardants to produce a synergistic effect, especially the compounding of bio-based phosphorus flame retardants, bio-based polyhydroxy flame retardants and bio-based nitrogen flame retardants, which respectively act as acid sources, carbon sources and gas sources to exert flame retardant effects. Among them, the bio-based phosphorus flame retardant contains more flame retardant elements (as the main flame retardant), which can produce a cross-linked solid substance or carbonized layer with a more stable structure when heated. The formation of the carbonized layer can prevent the polymer from further pyrolysis on the one hand, and prevent the thermal decomposition products inside it from entering the gas phase to participate in the combustion process on the other hand; the bio-based polyhydroxy flame retardant (as the auxiliary flame retardant) is the basis for forming the foamed carbonized layer and strengthens the thickness of the carbonized layer obtained by heating the acid source; coupled with the gas source foaming effect of the bio-based nitrogen flame retardant (as the auxiliary flame retardant), the surface carbonized layer is more porous, and it is difficult for external heat to penetrate the condensed phase, and oxygen is prevented from entering the combustion area, and the gaseous or liquid products generated by degradation are prevented from overflowing the material surface, thereby achieving an ideal flame retardant effect.

[0059] (3) The flame retardant used in the preparation of the flame retardant material of the present invention is low in dosage, and an appropriate amount can achieve the desired effect without affecting the performance and other physical properties of the material.

[0060] (4) The preparation method of the present invention has low cost, simple production process, and is easy to industrialize.

[0061] The term "and / or" as used herein includes all combinations of the items connected by the term, and each combination should be deemed to have been listed separately herein. For example, "A and / or B" includes "A," "A and B," and "B." For another example, "A, B, and / or C" includes "A," "B," "C," "A and B," "A and C," "B and C," and "A and B and C."

[0062] The terms “include” or “comprising” described in the present invention are open-ended descriptions, which include the specified components or steps described and other specified components or steps that will not be substantially affected.

[0063] The English abbreviations and Chinese full names of the present invention are compared in Table 1.

[0064] Table 1: English abbreviations and Chinese full names DETAILED DESCRIPTION

[0065] The following is a clear and complete description of the technical solutions in the embodiments of the present invention. Obviously, the embodiments described are only some embodiments of the present invention, not all. All other embodiments obtained by ordinary technicians in this field based on the embodiments of the present invention without making any creative efforts are within the scope of protection of the present invention.

[0066] Unless otherwise specified, the materials used in the embodiments of the present invention can be obtained commercially.

[0067] Unless otherwise specified, the parts, percentages or ratios described in the embodiments of the present invention are all based on mass.

[0068] The detection standards of the parameters in the embodiment are as follows:

[0069] 1. Tensile strength (MPa), refer to GB / T 1040.2-2006.

[0070] 2. Tensile elongation at break (%), refer to GB / T 1040.2-2006.

[0071] 3. Flexural strength (MPa), refer to GB / T9341-2008.

[0072] 4. Flexural modulus (MPa), refer to GB / T 9341-2008.

[0073] 5. Flame retardancy (-), refer to GB / T 2408-2008. Note: The order of flame retardancy is: V-0>V-1>V-2>HB>HB40>HB75.

[0074] 6. Load thermal deformation temperature 0.45MPa (℃), GB / T1634-2019.

[0075] Example 1: Preparation of flame-retardant PHA (PHB+P34HB) material

[0076] 120 parts by mass of P3HB4HB (4HB molar content 15%), 15 parts of PHB, 3 parts of DOPO modified castor oil, 4.5 parts of phytic acid, 1.5 parts of lignin, 2 parts of chitosan, 4 parts of urea composite melamine, 0.15 parts of silane coupling agent KH-792, 0.05 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-201, 0.5 parts of ethylene bis stearamide, 0.3 parts of monoglycerol stearate, 0.5 parts of a low-molecular-weight, fully biodegradable polyester lubricant, 0.2 parts of modified PTFE powder TRG-460, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then melt-blended and extruded in a twin-screw extruder, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The resulting flame-retardant material exhibited excellent flame retardancy and overall properties, with a flame retardancy rating of V-0 and an elongation at break of 42%.

[0077] Example 2: Preparation of flame-retardant PHA (P34HB) material

[0078] 140 parts by mass of P3HB4HB (4HB molar content 12%), 3 parts of polysilicon boroxane, 3 parts of DOPO modified castor oil, 8 parts of sodium phytate, 2 parts of starch, 2.5 parts of lignin, 1.5 parts of cellulose, 2 parts of urea, 3 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearin, 0.2 parts of a low-molecular-weight, fully degradable polyester lubricant, 0.3 parts of a low-molecular-weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The resulting flame-retardant material exhibited good flame retardancy and overall properties. The results are shown in Table 3.

[0079] Example 3: Preparation of flame-retardant PHA (PHB) material

[0080] 95 parts by mass of PHB, 2 parts of silicone fire retardant 3820, 2.5 parts of silicone flame retardant FCA-107, 4.5 parts of DOPO modified castor oil, 1.5 parts of lignin, 1.5 parts of cyclodextrin, 3 parts of urea composite melamine, 0.075 parts of silane coupling agent KH-792, 0.125 parts of silane coupling agent Y-5669, 0.1 parts of titanate coupling agent TMC-311, 0.4 parts of Ethylene bisstearamide, 0.4 parts of tristearin, 0.5 parts of low-molecular-weight PHB, 0.1 parts of modified PTFE powder TRG-460, 0.1 parts of PTFE powder FS-200, and 0.3 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The resulting flame-retardant material exhibited excellent flame retardancy and overall performance.

[0081] The obtained materials were tested and the results are shown in Table 2.

[0082] Table 2: Test data of flame retardant PHA (PHB) materials

[0083] Example 4: Preparation of flame-retardant PHA (PHBHHx) material

[0084] 130 parts by mass of PHBHHx (HHx molar content 10%), 3 parts of polysilicon boroxane, 2 parts of silicone fire retardant 3820, 3.5 parts of DOPO modified castor oil, 4.5 parts of phytic acid, 1.5 parts of cellulose, 1.5 parts of tannic acid, 1 part of itaconic acid, 3 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.125 parts of silane coupling agent Y-5669, 0.075 parts of titanate coupling agent TMC-102, 0.35 parts of stearic acid monoglyceride, 0.45 parts of tristearic acid glyceride, 0.5 parts of low molecular weight fully degradable polyester lubricant, 0.2 parts of modified PTFE powder TRG-460, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 0.1 1 part tris(2,4-di-tert-butylphenyl) phosphite is added to a high-speed mixer and mixed for 5-10 minutes. The mixture is then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature is 140-160°C. The resulting flame-retardant material exhibits excellent flame retardancy and overall performance, achieving a flame retardancy rating of V-0.

[0085] Example 5: Preparation of flame-retardant PHA (PHBHHx+PHBV) material

[0086] 60 parts by mass of PHBHHx (HHx molar content 5%), 60 parts by mass of PHBV (3HV molar content 10%), 2.5 parts by mass of DOPO modified castor oil, 4 parts by mass of phytic acid, 2.5 parts by mass of sodium phytate, 1 part by mass of cellulose, 1 part by mass of cyclodextrin, 1.5 parts by mass of tannic acid, 2 parts by mass of urea, 4 parts by mass of urea composite melamine, 0.15 parts by mass of silane coupling agent Y-5669, 0.075 parts by mass of titanate coupling agent TMC-102, 0.075 parts by mass of titanate coupling agent TMC-311, 0.5 parts of ethylene bisstearamide, 0.3 parts of stearic acid monoglyceride, 0.2 parts of a low-molecular-weight, fully degradable polyester lubricant, 0.3 parts of a low-molecular-weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite are added to a high-speed mixer and mixed for 5-10 minutes. The mixture is then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature is 140-160°C. The resulting flame-retardant material exhibits excellent flame retardancy and overall properties, with a flame retardancy rating of V-0.

[0087] Example 6: Preparation of flame-retardant PHA (P34HB+PHBV) material

[0088] 60 parts by mass of P3HB4HB (4HB molar content 25%), 60 parts by mass of PHBV (3HV molar content 5%), 2 parts by mass of polysiloxane, 3.5 parts by mass of silicon-based flame retardant FCA-107, 4 parts by mass of DOPO-modified castor oil, 6 parts by mass of sodium phytate, 2 parts by mass of lignin, 2 parts by mass of chitosan, 1.5 parts by mass of itaconic acid, 4 parts by mass of urea-compounded melamine, 0.15 parts by mass of silane coupling agent KH-792, 0.05 parts by mass of silane coupling agent Y-5475, 0.01 parts by mass of silane coupling agent Y-5475, 0.01 parts by mass of silane coupling agent KH-792, 0.01 ... Y-5475, 0.01 parts by mass of silane coupling agent Y-5475, 0.01 parts by mass of silane coupling agent Y-547 1 part titanate coupling agent TMC-201, 0.35 part monoglycerol stearate, 0.45 part triglycerol stearate, 0.5 part low molecular weight PHB, 0.1 part modified PTFE powder TRG-460, 0.1 part PTFE powder FS-200, and 0.35 part tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The resulting flame-retardant material exhibited excellent flame retardancy and overall properties, with a flame retardancy rating of V-0.

[0089] Example 7: Preparation of flame retardant PHA (P34HB) material

[0090] 140 parts by weight of P3HB4HB (12% 4HB molar content), 3 parts of polysilicon boroxane, 3 parts of DOPO-modified castor oil, 8 parts of sodium phytate, 2 parts of starch, 2.5 parts of lignin, 1.5 parts of cellulose, 2 parts of urea, and 3 parts of urea-compounded melamine were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then melt-blended and extruded in a twin-screw extruder, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The resulting flame-retardant material exhibited excellent flame retardancy and overall properties, with a flame retardancy rating of V-0 and a heat deflection temperature under load of 104°C at 0.45 MPa.

[0091] Comparative Example 1: Preparation of flame-retardant PHA (P34HB) material with excessive flame retardant addition

[0092] 140 parts by mass of P3HB4HB (4HB molar content 12%), 5 parts of polysiloxane, 5 parts of DOPO modified castor oil, 12 parts of sodium phytate, 4 parts of starch, 3.5 parts of lignin, 2.5 parts of cellulose, 3 parts of urea, 5 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide 0.4 parts of tristearin, 0.2 parts of a low-molecular-weight, fully degradable polyester lubricant, 0.3 parts of low-molecular-weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The flame retardant and comprehensive properties of the prepared flame-retardant material are shown in Table 3.

[0093] Comparative Example 2: Preparation of flame-retardant PHA (P34HB) material with different flame retardant types

[0094] 140 parts by weight of P3HB4HB (12% 4HB molar content), 7 parts of boron oxide, 18 parts of magnesium hydroxide flame retardant, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearate, 0.2 parts of low molecular weight fully degradable polyester lubricant, 0.3 parts of low molecular weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The flame retardant properties and comprehensive properties of the prepared flame retardant materials are shown in Table 3.

[0095] Comparative Example 3: Preparation of PHA (P34HB) material without bio-based phosphorus flame retardant, the balance is supplemented with other types of flame retardants

[0096] 140 parts by mass of P3HB4HB (4HB molar content 12%), 5 parts of polysiloxane, 3.5 parts of starch, 4 parts of lignin, 2.5 parts of cellulose, 4 parts of urea, 6 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearate, 0.2 parts of low molecular weight fully degradable polyester lubricant, 0.3 parts of low molecular weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were prepared. After mixing in a high-speed mixer for 5-10 minutes, the material was fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The flame retardant and overall properties of the prepared flame-retardant material are shown in Table 3.

[0097] Comparative Example 4: Preparation of PHA (P34HB) material without bio-based polyhydroxy flame retardant, the balance is supplemented with other types of flame retardants

[0098] 140 parts by mass of P3HB4HB (4HB molar content 12%), 4 parts of polysilicon boroxane, 4 parts of DOPO modified castor oil, 10.5 parts of sodium phytate, 2.5 parts of urea, 4 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bis stearamide, 0.4 parts of tristearic acid Glycerol ester, 0.2 parts of a low-molecular-weight, fully biodegradable polyester lubricant, 0.3 parts of a low-molecular-weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The flame retardant and overall properties of the prepared flame-retardant material are shown in Table 3.

[0099] Comparative Example 5: Preparation of PHA (P34HB) material without bio-based nitrogen flame retardant, the balance is supplemented with other types of flame retardants

[0100] 140 parts by mass of P3HB4HB (4HB molar content 12%), 4 parts of polysilicon boroxane, 4 parts of DOPO modified castor oil, 10 parts of sodium phytate, 2.5 parts of starch, 3 parts of lignin, 1.5 parts of cellulose, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bis stearamide, 0.4 parts of tristearate A mixture of glycerol ester, 0.2 parts of a low-molecular-weight, fully degradable polyester lubricant, 0.3 parts of a low-molecular-weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite was added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then fed into a twin-screw extruder for melt blending and extrusion, followed by air-cooling and strand pelletization. The twin-screw processing temperature was 140-160°C. The flame retardant and comprehensive properties of the prepared flame retardant material are shown in Table 3.

[0101] Comparative Example 6: Preparation of PHA (P34HB) material without bio-based phosphorus and nitrogen flame retardants, the balance is supplemented with other types of flame retardants

[0102] 140 parts by mass of P3HB4HB (4HB molar content 12%), 7 parts of polysilicon boroxane, 6 parts of starch, 6.5 parts of lignin, 5.5 parts of cellulose, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearate, 0.2 parts of low molecular weight fully degradable polyester lubricant, 0.3 parts of low molecular weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The mixture was then put into a twin-screw extruder for melt blending and extrusion, and air-cooled to form strands. The twin-screw processing temperature is 140-160°C. The flame retardant properties and comprehensive properties of the prepared flame retardant material are shown in Table 3.

[0103] Comparative Example 7: Preparation of PHA (P34HB) material without bio-based phosphorus and polyhydroxy flame retardant, the balance is supplemented with other types of flame retardants

[0104] 140 parts by mass of P3HB4HB (4HB molar content 12%), 9 parts of polysilicon boroxane, 7 parts of urea, 9 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearate, 0.2 parts of low molecular weight fully degradable polyester lubricant, 0.3 parts of low molecular weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added into a high-speed mixer and mixed for 5-10 minutes, then discharged into a twin-screw extruder for melt blending and extrusion, and air-cooled and stranded into granules. The twin-screw processing temperature is 140-160°C. The flame retardant properties and comprehensive properties of the prepared flame retardant material are shown in Table 3.

[0105] Comparative Example 8: Preparation of PHA (P34HB) material without bio-based polyhydroxyl and nitrogen flame retardants, the balance is supplemented with other types of flame retardants

[0106] 140 parts by mass of P3HB4HB (4HB molar content 12%), 5 parts of polysilicon boroxane, 5 parts of DOPO modified castor oil, 15 parts of sodium phytate, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearate, 0.2 parts of low molecular weight fully degradable polyester lubricant, 0.3 parts of low molecular weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes, then discharged into a twin-screw extruder for melt blending and extrusion, and air-cooled and stranded into granules. The twin-screw processing temperature is 140-160°C. The flame retardant properties and comprehensive properties of the prepared flame retardant material are shown in Table 3.

[0107] Comparative Example 9: Preparation of flame-retardant PHA (P34HB) materials with other ratios

[0108] 140 parts by mass of P3HB4HB (4HB molar content 12%), 3 parts of polysilicon boroxane, 2 parts of DOPO modified castor oil, 3 parts of sodium phytate, 2 parts of starch, 1.5 parts of lignin, 2.5 parts of cellulose, 4 parts of urea, 7 parts of urea composite melamine, 0.1 parts of silane coupling agent DL-602, 0.1 parts of silane coupling agent Y-5475, 0.1 parts of titanate coupling agent TMC-102, 0.4 parts of ethylene bisstearamide, 0.4 parts of tristearin, 0.2 parts of low molecular weight fully degradable polyester lubricant, 0.3 parts of low molecular weight PHB, 0.2 parts of PTFE powder FS-200, 0.2 parts of pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], and 0.1 parts of tris(2,4-di-tert-butylphenyl) phosphite were added to a high-speed mixer and mixed for 5-10 minutes. The materials were then put into a twin-screw extruder for melt blending and extrusion, and air-cooled to form strands for granulation. The twin-screw processing temperature was 140-160°C. The flame retardant properties and comprehensive properties of the prepared flame retardant material are shown in Table 3. In addition, the experimental results of Example 2 and Comparative Examples 1-9 are summarized in Table 3.

[0109] Table 3: Test data of Example 2 and Comparative Examples 1-9

[0110] As can be seen from the results in Tables 1-3, Examples 1-7 in which the flame-retardant polyhydroxyalkanoates were prepared using the method of the present invention have good flame retardant effects and excellent properties, especially in tensile strength, elongation at break, flexural strength, and flexural modulus, due to the use of the specific components and specific combined contents of the present invention. In addition, the present invention has low cost, a simple production process, and is easy to industrialize.

[0111] Compared with Example 2, the amount of flame retardant added in Comparative Example 1 is increased, and the overall performance of the material is affected.

[0112] Compared with Example 2, Comparative Example 2 changed the type of flame retardant, the flame retardant performance decreased, the bio-based component of the material was reduced, the overall performance was affected, and the effect was not good.

[0113] Compared with Example 2, the flame retardant properties of Comparative Examples 3-8 are greatly reduced due to the lack of synergistic effect between the bio-based phosphorus flame retardant, the bio-based polyhydroxy flame retardant and the bio-based nitrogen flame retardant, and the comprehensive performance of the material is affected.

[0114] Compared with Example 2, in Comparative Example 9, the halogen-free flame retardant contains too little bio-based phosphorus flame retardant and too much bio-based nitrogen flame retardant, resulting in an uncoordinated ratio and affected comprehensive performance of the material.

[0115] The preferred embodiments of the present invention have been described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, various simple variations of the technical solution of the present invention may be made, including combining the various technical features in any other appropriate manner. These simple variations and combinations should also be regarded as disclosed in the present invention and fall within the scope of protection of the present invention.

Claims

1. A flame retardant material, characterized in that: The flame retardant material comprises polyhydroxyalkanoate and halogen-free flame retardant, and the halogen-free flame retardant comprises bio-based phosphorus flame retardant, bio-based polyhydroxy flame retardant and / or bio-based nitrogen flame retardant.

2. The flame retardant material according to claim 1, characterized in that: in, The mass ratio of polyhydroxyalkanoate to halogen-free flame retardant is (2-9):

1.

3. The flame retardant material according to claim 1 or 2, characterized in that: The polyhydroxyalkanoate comprises a homopolymer or a copolymer of monomers constituting the polyhydroxyalkanoate. Wherein, the monomers constituting the polyhydroxyalkanoic acid ester include one, two or more of 2-hydroxypropionic acid, 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid and 3-hydroxydodecanoic acid.

4. The flame retardant material according to claim 3, characterized in that: The polyhydroxyalkanoate comprises one, two or more of P(HA-LA), P3HP, PHB, P4HB, PHV, PHO, PHN, PHD, PHBV, P34HB, PHBHHp, PHBHHx, P3HB4HB3HV or P3HB4HB5HV; Among them, HA in P(HA-LA) is selected from one, two or more of 3-hydroxypropionic acid, 3-hydroxybutyric acid, 4-hydroxybutyric acid, 3-hydroxyvaleric acid, 5-hydroxyvaleric acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid and 3-hydroxydodecanoic acid; LA is 2-hydroxypropionic acid.

5. The flame retardant material according to claim 1, characterized in that: The bio-based phosphorus flame retardant is selected from one, two or three of DOPO-modified castor oil, phytic acid or sodium phytate.

6. The flame retardant material according to claim 1, characterized in that: The bio-based polyhydroxy flame retardant is selected from one or a combination of two or more of starch, lignin, cellulose, chitosan, cyclodextrin, tannic acid or itaconic acid.

7. The flame retardant material according to claim 1, characterized in that: The bio-based nitrogen flame retardant is selected from urea and / or urea-compounded melamine.

8. The flame retardant material according to claim 1, characterized in that: The halogen-free flame retardant comprises, by weight, 4.5-11 parts of a bio-based phosphorus flame retardant, 3-6 parts of a bio-based polyhydroxy flame retardant and 3-6 parts of a bio-based nitrogen flame retardant.

9. The flame retardant material according to claim 1, characterized in that: The halogen-free flame retardant also includes a silicon-based flame retardant. Preferably, the halogen-free flame retardant includes, by weight, 0-6 parts of silicon-based flame retardant, 4.5-11 parts of bio-based phosphorus-based flame retardant, 3-6 parts of bio-based polyhydroxy flame retardant and 3-6 parts of bio-based nitrogen-based flame retardant.

10. The flame retardant material according to claim 9, characterized in that: The silicon-based flame retardant is selected from one or a combination of two or more of polysilicon boroxane, organic silicon-based fire retardant 3820 or silicon-based flame retardant FCA-107.

11. The flame retardant material according to any one of claims 1 to 10, characterized in that: The flame retardant material further comprises an auxiliary agent. Preferably, in the flame retardant material, the mass ratio of polyhydroxyalkanoate: halogen-free flame retardant: auxiliary agent is (95-140): (15-25): (0%-7%).

12. The flame retardant material according to claim 11, characterized in that: The auxiliary agent comprises one or a combination of two or more of a coupling agent, a dispersant, a lubricant, an anti-dripping agent and an antioxidant.

13. The flame retardant material according to claim 12, characterized in that: in, The coupling agent is selected from one or a combination of two or more of silane coupling agent KH-792, silane coupling agent DL-602, silane coupling agent Y-5475, silane coupling agent Y-5669, titanate coupling agent TMC-201, titanate coupling agent TMC-102, and titanate coupling agent TMC-311; The dispersant is selected from one, two or three of ethylene bisstearamide, stearic acid monoglyceride and tristearic acid glyceride; The lubricant is selected from low molecular weight fully degradable polyester and / or low molecular weight PHA; The anti-dripping agent is selected from PTFE powder TRG-460 and / or PTFE powder FS-200; The antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate and / or tris(2,4-di-tert-butylphenyl) phosphite.

14. The flame retardant material according to any one of claims 1 to 13, characterized in that: The flame retardant material includes, by mass: Polyhydroxyalkanoate: 95-140 parts; Halogen-free flame retardant: 15-25 parts; Coupling agent: 0.01-1 part; Dispersant: 0.01-2 parts; Lubricant: 0.01-1.5 parts; Anti-dripping agent: 0.01-1 part; Antioxidant: 0.01-1 part.

15. A method for preparing the flame retardant material according to any one of claims 1 to 14, characterized in that: The preparation method comprises mixing raw materials, then melting and blending and extruding in a twin-screw extruder, and air-cooling and drawing into granules, wherein the raw materials comprise polyhydroxyalkanoate and halogen-free flame retardant; Preferably, the raw material also includes an auxiliary agent.

16. Use of the flame retardant material according to any one of claims 1 to 14 in a product requiring the material to have flame retardant properties, characterized in that: The products mentioned include construction materials, home furnishings and textiles, aerospace, military industry, automobiles or packaging materials.

Citation Information

Patent Citations

  • Halogen-free flame-retardant photo-curing epoxy resin composition

    CN101407597A

  • Flame Retardant Resin Composition And Molded Product

    CN104031362A

  • Degradable PLA for data line protection sleeve and preparation method of degradable PLA

    CN112980166A

  • Flame-retardant material

    CN116218180A

  • Spring element, fire-retardant coating for a spring element and material mixture for such a coating

    DE102022100398A1