PBET copolyester and preparation method therefor
By controlling the components and preparation steps, the problems of high heavy metal content and poor mechanical properties of PBET copolyester in the prior art were solved, and PBET copolyester suitable for toys and precision instruments were prepared, with low heavy metal content and excellent mechanical properties. Performance and dimensional stability.
Patent Information
- Application Number
- PCT/CN2024/091551
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-05-08
- Publication Date
- 2024-11-14
AI Technical Summary
In the prior art, the recycled PBET copolyester has high heavy metal content, poor mechanical properties, and insufficient dimensional stability, making it difficult to meet the requirements of toys and precision instruments for dimensional stability.
Using PBET copolyester with aromatic dicarboxylic acid, butanediol and ethylene glycol as components, the content of zinc and titanium is controlled at extremely low levels through the initial depolymerization, repolymerization and polycondensation steps, and the content of zinc and titanium is used. The acid used as a chelating agent to remove metal ions residues and prepares PBET copolyester with suitable crystallinity and excellent mechanical properties.
The prepared PBET copolyester has extremely low heavy metal content, excellent impact resistance and good dimensional stability. It is suitable for toys and precision instruments and replaces some PBT and PET applications.
Smart Images

Figure CN2024091551_14112024_PF_FP_ABST
Abstract
Description
A kind of PBET copolyester and preparation method thereof Technical Field
[0001] The present invention relates to the technical field of recycled polyesters, in particular to a PBET copolyester and a preparation method thereof. Background Art
[0002] Currently, biodegradable plastics account for approximately 58% of plastic production worldwide, while non-degradable plastics account for 42%. The disposal of waste plastics is an urgent issue. my country will gradually address the environmental hazards of traditional waste plastic disposal through methods such as source reduction, reuse, the use of bio-based or biodegradable plastics instead of fossil-based materials, and the recycling of plastics through physical or chemical recovery.
[0003] Polyesters such as PBT and PET are the primary raw materials for plastics. Due to the presence of carbonyl groups in PET's backbone, it is thermodynamically and kinetically valuable and easily recyclable on an industrial scale. Its recyclability is high, and compared to other plastics, it is susceptible to physical and chemical depolymerization. Currently, the main methods for recycling PET are physical and chemical recycling. The main chemical recycling methods include alcoholysis, hydrolysis, aminolysis, glycolysis, and chemical combinations.
[0004] There is an existing technology (Zhou Nan, Song Chenxing. Research and Development of PBET Copolyester [J]. Chemical Technology Market, 2001, 24(8):3.) that reports the use of dimethyl terephthalate (DMT), 1,4-butanediol (1,4-BG), and ethylene glycol (EG) as raw materials to produce a terpolymer: PBET copolyester. PBET copolyester has the advantages of PBT and PET. However, in this preparation method, all three fossil-based raw materials are used, rather than waste polyester, and the preparation requires special processes and reactors.
[0005] Chinese patent application CN114031756A discloses a closed-loop method for recycling waste polyester to produce recycled polyester, which is a typical green and low-carbon method. The method comprises depolymerizing the waste polyester under microwave conditions; removing the polyol solvent from the depolymerization product, and then purifying it to remove byproducts to obtain a depolymerized monomer; and mixing the depolymerized monomer with a dibasic acid, a polyol, a polymerization catalyst, and a chain extender to undergo esterification and polycondensation to produce the recycled polyester. Although this prior art provides a method for producing recycled polyester from waste polyester, the method requires separating ethylene glycol after alcoholysis and purifying the monomer, which is not only cumbersome but also removes certain reinforcing additives in the waste polyester during the purification process, resulting in poor mechanical properties of the resulting recycled polyester.
[0006] There is also an existing technology (Zhang Hongming, Zhao Junyu, Gao Fengxiang, et al. Research on the "One-Pot Method" for Synthesizing Biodegradable Polymers by Depolymerization and Co-condensation of PET [J]. Acta Polymerica Sinica, 2022(009):053.) that uses diols of different structures to hydrolyze PET into low molecular weight prepolymers, and then adds dibasic acids for further esterification and polycondensation, so that the depolymerization and copolymerization of PET are completed in a "one-pot method", eliminating the monomer purification process. Although this method uses a one-pot method to eliminate the purification process, since the recycled materials usually contain different levels of heavy metals and heavy metal catalysts are also used in the depolymerization process, the catalyst residue will seriously affect the physical properties and aging resistance of the product.
[0007] Currently, PBT materials used in engineering plastics are also widely used in toys and precision instruments, which require good dimensional stability. Therefore, as PCR is used more and more widely, ABS and recycled PBT or recycled PET are generally used in toys to increase the content of PCR. However, the dimensional stability of PBT and PET is slightly poor.
[0008] Therefore, it is necessary to provide a recycled PBET copolyester that meets the requirements of low residual heavy metal content, good mechanical properties, good dimensional stability and low mold shrinkage, meets the dimensional stability requirements of toys and precision instruments, and can replace some of the application areas of PBT and PET.
[0009] Summary of the Invention
[0010] The purpose of the present invention is to overcome the defects of the prior art such as high heavy metal content and poor mechanical properties, and to provide a PBET copolyester.
[0011] Another object of the present invention is to provide a method for preparing the above-mentioned PBET copolyester.
[0012] To achieve the above object, the present invention adopts the following technical solutions:
[0013] A PBET copolyester derived from repeating units of:
[0014] Component A: aromatic dicarboxylic acid;
[0015] Component B: based on the total molar amount of component B, comprising 60 to 96 mol% of 1,4-butanediol or 1,3-butanediol and 4 to 40% mol% of ethylene glycol;
[0016] The crystallinity of the PBET copolyester is 5-20%, including but not limited to 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, and 20%;
[0017] The zinc content in the PBET copolyester is ≤100 ppm, and the titanium content is ≤120 ppm.
[0018] The PBET copolyester of the present invention is a recycled PBET copolyester comprising a dicarboxylic acid component containing an aromatic dicarboxylic acid as repeating units and a diol component containing butanediol and ethylene glycol as repeating units. The PBET copolyester has an extremely low heavy metal content, with a zinc content of ≤100 ppm and a titanium content of ≤120 ppm. Residual zinc and titanium in the PBET copolyester are introduced by the catalysts used in the depolymerization and polycondensation processes, as well as by impurities in waste polyester raw materials.
[0019] The crystallinity of recycled polyester is a key parameter in standard polymer properties and an important indicator of its quality. The PBET copolyester of the present invention has a low crystallinity of 5-20%. The PBET copolyester exhibits excellent mechanical properties, particularly impact resistance. Furthermore, within this suitable crystallinity range, the PBET copolyester also exhibits excellent dimensional stability and low mold shrinkage, making it suitable for use in toys and precision instrument modification materials.
[0020] Preferably, the zinc content in the PBET copolyester is 25 to 70 ppm, and the titanium content is 40 to 85 ppm.
[0021] Preferably, the calcium content in the PBET copolyester is ≤50 ppm.
[0022] More preferably, the calcium content in the PBET copolyester is 15 to 35 ppm.
[0023] In the present invention, the crystallinity of the PBET copolyester is analyzed using an X-ray diffractometer (XRD) according to the standard JY / T0587-2020. Specifically, a D8 ADVANCE X-ray diffractometer from BRUKER, Germany, is used at room temperature, with Cu Ka radiation (λ = 0.154 nm) collected every 0.05°, and a scanning angle range of 6° to 60°.
[0024] In the present invention, the zinc content and titanium content are tested according to the following method:
[0025] Inductively coupled plasma optical emission spectrometer ICP-OES was used according to the standard inductively coupled plasma atomic emission spectrometer method US EPA6010C:2014.
[0026] Preferably, the melting point of the PBET copolyester is 200-220°C, including but not limited to 200°C, 201°C, 202°C, 203°C, 204°C, 205°C, 206°C, 207°C, 208°C, 209°C, 210°C, 211°C, 212°C, 213°C, 214°C, 215°C, 216°C, 217°C, 218°C, 219°C, and 220°C.
[0027] The melting point was measured using a differential scanning calorimeter according to ISO 11357-3:2018.
[0028] Preferably, the relative viscosity of the PBET copolyester is 1.4 to 1.8.
[0029] The relative viscosity is tested as follows:
[0030] According to the standard method of GB / T 17931-1999, the sample concentration was 5 mg / ml in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05°C.
[0031] Preferably, the terminal carboxyl content of the PBET copolyester is 20 to 37 mmol / t, including but not limited to 20 mmol / t, 21 mmol / t, 22 mmol / t, 23 mmol / t, 24 mmol / t, 25 mmol / t, 26 mmol / t, 27 mmol / t, 28 mmol / t, 29 mmol / t, 30 mmol / t, 31 mmol / t, 32 mmol / t, 33 mmol / t, 34 mmol / t, 35 mmol / t, 36 mmol / t, and 37 mmol / t.
[0032] The terminal carboxyl content was tested according to standard FZ / T 50012-2006 using automatic potentiometric titration analysis.
[0033] The present invention also provides a method for preparing the above-mentioned PBET copolyester, comprising the following steps:
[0034] S1. Initial depolymerization:
[0035] The waste polyester is dissolved in an alcohol solvent containing a depolymerization catalyst, and a primary depolymerization reaction is carried out under normal pressure, an inert gas atmosphere and microwave conditions to obtain a primary depolymerization product;
[0036] The waste polyester includes one or more of recycled polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and PET / PBT alloy;
[0037] The temperature of the initial depolymerization reaction is 180-230°C and the time is 20-120 minutes;
[0038] S2. Re-disaggregation:
[0039] Extracting a portion of the diol from the primary depolymerization product obtained in step S1, adding a chelating agent, and performing a re-depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions. After filtering the reactants, the obtained filtrate is the re-depolymerization product;
[0040] The temperature of the re-depolymerization reaction is 160-190° C. and the time is 10-20 minutes;
[0041] S3. Polycondensation:
[0042] After removing excess alcohol from the re-depolymerization product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, and subjected to a polycondensation reaction under vacuum conditions to obtain the PBET copolyester.
[0043] The preparation method of the PBET copolyester of the present invention uses waste polyester as raw material, and through two steps of alcoholysis and polycondensation, and by controlling factors such as the temperature and time of depolymerization and re-depolymerization, a PBET copolyester with low heavy metal content, suitable crystallinity and excellent dimensional stability is prepared.
[0044] In the primary depolymerization step, the waste polyester undergoes a preliminary alcoholysis in the presence of a depolymerization catalyst under normal pressure, an inert gas atmosphere, and microwave conditions. The temperature of the initial depolymerization reaction is relatively high, allowing the majority of the waste polyester to be alcoholyzed into monomers or oligomers. Ethylene glycol is then removed from the product of the initial depolymerization, and after adding a chelating agent, a second alcoholysis, or re-depolymerization, is performed. The re-depolymerization temperature is lower than that of the initial depolymerization, and the duration is shorter. The chelating agent simultaneously removes most of the heavy metal ions from the waste polyester during the re-depolymerization process, and the addition of the chelating agent does not negatively impact the mechanical properties, dimensional stability, or crystallinity of the recycled polyester.
[0045] In the preparation method of the present invention, a portion of the diol is extracted in step S2, which is a byproduct of the initial depolymerization, and excess alcohol is removed in step S3, both to obtain a PBET copolyester with an appropriate monomer content. The resulting PBET copolyester satisfies the following characteristics: the PBET copolyester is derived from repeating units of the following components: Component A: an aromatic dicarboxylic acid; Component B: 60-96 mol% of 1,4-butanediol or 1,3-butanediol and 4-40 mol% of ethylene glycol, based on the total molar weight of Component B;
[0046] In step S2, the method for extracting part of the diol can be vacuum distillation, and the extraction time is 15-60 minutes.
[0047] Optionally, sources of the waste polyester include but are not limited to post-consumer recycled plastics (PCR), post-industry recycled plastics (PIR), ocean-bound plastics (OBP), and in-the-ocean plastics (IOP).
[0048] Preferably, the waste polyester further includes the steps of impurity removal, cleaning and crushing before the initial depolymerization.
[0049] Preferably, in step S2, the chelating agent is a biomass chelating agent.
[0050] Preferably, the chelating agent includes at least one of chitosan, activated carbon, lignin, and phytic acid.
[0051] More preferably, the chelating agent is phytic acid.
[0052] Phytic acid, as a chelating agent, not only effectively complexes residual metal ions in waste polyester, but also serves as an excellent antioxidant and stabilizer for recycled PET and PBT. The inventors have found that using phytic acid as a chelating agent results in PBET copolyesters with lower metal ion content, improved toughness, and superior dimensional stability.
[0053] Preferably, in step S2, the amount of the chelating agent added is 0.01 to 0.1 wt.% of the waste polyester.
[0054] The chelating agent can be added in a relatively low amount to effectively remove metal ions from waste polyester.
[0055] Preferably, in step S1, the depolymerization catalyst includes at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate.
[0056] Preferably, in step S1, the amount of the depolymerization catalyst added is 0.05 to 0.5 wt.% of the waste polyester.
[0057] Preferably, when the waste polyester contains PET, the alcohol solvent contains 1,4-butanediol; when the waste polyester contains PBT, the alcohol solvent contains ethylene glycol.
[0058] Preferably, the mass ratio of the waste polyester to the alcohol solvent is 1:0.5 to 1:2.
[0059] The alcohol solvent plays the role of alcoholysis. The inventors have found that 1,4-butanediol has a good alcoholysis effect on the recycled PBT and PET. Therefore, the preferred alcohol solvent is 1,4-butanediol.
[0060] Preferably, in step S3, the polycondensation catalyst includes at least one of butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds, titanium-magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide.
[0061] Preferably, in step S3, the amount of the polycondensation catalyst added is 0.03 to 0.1 wt.% of the waste polyester.
[0062] Preferably, in step S3, the temperature of the polycondensation reaction is 240-250° C., the time is 2-5 hours, and the pressure is 20-100 Pa.
[0063] Preferably, in step S3, the stabilizer is one or more of organic phosphites, trimethyl phosphates, and hindered phenols.
[0064] Optionally, the organic phosphite stabilizer may be one or more of trimethyl phosphite, triethyl phosphite or triphenyl phosphite.
[0065] Optionally, the phosphate stabilizer may be one or more of triphenyl phosphate, trimethyl phosphate or triethyl phosphate.
[0066] Optionally, the hindered phenol stabilizer may be 3,5-di-tert-butyl-4-hydroxybenzyl diethylphosphonate (antioxidant 1222) and / or antioxidant 1010.
[0067] Preferably, in step S1, the microwave reaction conditions are as follows: frequency of 2450 Hz, temperature of 180-230° C., and time of 20-120 min.
[0068] Preferably, in step S2, the microwave reaction conditions are as follows: frequency of 2450 Hz, temperature of 160-190° C., and time of 10-20 min.
[0069] In addition, the present invention also provides an application of the PBET copolyester in toys and precision instruments.
[0070] Compared with the prior art, the present invention has the following beneficial effects:
[0071] The present invention develops a PBET copolyester and a preparation method thereof. The PBET copolyester of the present invention is prepared from waste polyester through the steps of primary depolymerization, secondary depolymerization, and polycondensation to obtain a PBET copolyester with low heavy metal content and suitable crystallinity.
[0072] The initial depolymerization and re-depolymerization are carried out under microwave conditions, wherein the re-depolymerization includes the addition of a chelating agent. The addition of the chelating agent and the re-depolymerization reaction synergistically remove most of the metal ion residues in the waste polyester. The prepared PBET copolyester has an extremely low heavy metal content, wherein the zinc content is ≤100ppm and the titanium content is ≤120ppm.
[0073] The PBET copolyester of the present invention utilizes waste polyester, including electronic pallet materials, bottle materials and textiles, effectively reducing the use of petroleum resources and reducing waste generation; the utilization rate of waste polyester is improved; the produced PBET copolyester has the advantages of PBT and PET, and when used as fiber, has the characteristics of nylon and spandex fibers, and is closer to the excellent performance of natural fibers such as cotton, linen, wool, and silk; when used as engineering plastics, it has excellent physical and mechanical properties, high impact resistance, low mold shrinkage, and good dimensional stability, and can be widely used in industrial and civilian fields such as electronics and electrical engineering, machinery manufacturing, automobiles, instruments, aviation, household appliances, sporting goods, children, and toys. BRIEF DESCRIPTION OF THE DRAWINGS
[0074] FIG1 is an infrared spectrum of the PBET copolyester of Example 1;
[0075] FIG2 is a hydrogen NMR spectrum of the PBET copolyester of Example 1;
[0076] FIG3 is an XRD pattern of the PBET copolyester of Example 1. DETAILED DESCRIPTION
[0077] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below with reference to specific embodiments, but the embodiments do not limit the present invention in any form.
[0078] The raw materials in the examples and comparative examples of the present invention can be obtained commercially;
[0079] in:
[0080] Waste polyester-1, PET, recycled from electronic pallet materials;
[0081] Waste polyester-2, PBT, recycled from Changchun, Taiwan, single glass fiber reinforced PBT product waste;
[0082] Waste polyester-3, OBP-PET, YH002, recycled from Yonghong Recycling Resources Co., Ltd.;
[0083] Depolymerization catalyst and polycondensation catalyst: butyl titanate, purchased from Aladdin;
[0084] Depolymerization catalyst: zinc acetate, purchased from Aladdin;
[0085] Chelating agents: chitosan, activated carbon, lignin, and phytic acid were purchased from Maclean;
[0086] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.
[0087] Examples 1 to 3
[0088] Examples 1 to 3 provide a method for preparing PBET copolyester, respectively, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 1:
[0089] S1. Initial depolymerization:
[0090] Waste polyester with an average particle size of ≤2 mm was dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction in a nitrogen atmosphere under microwave conditions (microwave frequency 2450 Hz) to obtain a primary depolymerization product;
[0091] S2. Re-disaggregation:
[0092] Extracting a portion of the diol from the primary depolymerization product obtained in step S1 by vacuum distillation, adding a chelating agent, and placing the product in a microwave reactor for re-depolymerization under normal pressure, an inert gas atmosphere, and microwave conditions (microwave frequency 2450 Hz). The reactants are filtered to obtain a filtrate as the re-depolymerization product;
[0093] S3. Polycondensation:
[0094] After removing excess alcohol from the depolymerized product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, triphenyl phosphate, and subjected to a polycondensation reaction under vacuum conditions to obtain the PBET copolyester.
[0095] Table 1 Raw materials and reaction conditions of Examples 1 to 3
[0096] Examples 4 to 10
[0097] Examples 4 to 10 provide a method for preparing PBET copolyester. Except for step S2, the other steps are the same as those in Example 1. Specifically, the preparation methods of Examples 4 to 10 differ from those of Example 1 in that:
[0098] In Example 4, the chelating agent is activated carbon and the alcoholysis agent is 1,3-butanediol;
[0099] In Example 5, the type of chelating agent is lignin;
[0100] In Example 6, the type of chelating agent is phytic acid;
[0101] In Example 7, the proportion of the chelating agent to the waste polyester is 0.01 wt.%;
[0102] In Example 8, the proportion of the chelating agent to the waste polyester is 0.1 wt.%;
[0103] The conditions for the re-depolymerization reaction in Example 9 were 190° C., 10 min;
[0104] The conditions for the re-depolymerization reaction in Example 10 were 160° C. for 20 min.
[0105] The monomer contents prepared in Examples 4-10 are shown in Table 2
[0106] Table 2 Monomer content of PBET copolyesters prepared in Examples 4-10
[0107] Comparative Examples 1 to 5
[0108] Comparative Examples 1 to 5 provide a method for preparing PBET copolyester, comprising the following steps. Specific raw materials and reaction conditions are shown in Table 3:
[0109] S1. Initial depolymerization:
[0110] Waste polyester with an average particle size of ≤2 mm was dissolved in an alcohol solvent containing a depolymerization catalyst, placed in a microwave reactor (Yantai Haoming Microwave Company), and subjected to a primary depolymerization reaction in a nitrogen atmosphere under microwave conditions (microwave frequency 2450 Hz) to obtain a primary depolymerization product;
[0111] S2. Re-disaggregation:
[0112] Extracting a portion of the diol from the primary depolymerization product obtained in step S1 by vacuum distillation, adding a chelating agent (or not adding a chelating agent), placing the product in a microwave reactor, and performing a re-depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions (microwave frequency 2450 Hz). The reactants are filtered to obtain a filtrate as the re-depolymerization product;
[0113] S3. Polycondensation:
[0114] After removing excess alcohol from the depolymerized product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, triphenyl phosphate, and subjected to a polycondensation reaction under vacuum conditions to obtain the PBET copolyester.
[0115] Table 3 Raw materials and reaction conditions of Comparative Examples 1 to 5
[0116] Performance Testing
[0117] The performance tests of the PBET copolyesters prepared in the above examples and comparative examples were carried out as follows:
[0118] Melting point: ISO 11357-3:2018;
[0119] Relative viscosity: measured according to GB / T 17931-1999 standard method in a phenol / chloroform solution with a weight ratio of 1:1 in a constant temperature water bath at 25±0.05°C, with a sample concentration of 5 mg / ml;
[0120] Terminal carboxyl content: FZ / T 50012-2006;
[0121] Metal ion residue: US EPA 6010C:2014;
[0122] Crystallinity: JY / T 0587-2020;
[0123] Izod notched impact strength: GB / T1843-2008, impact energy 2.75kJ.
[0124] Mold shrinkage: tested in accordance with GB / T 17037.4-2003.
[0125] The PBET copolyester prepared in Example 1 was subjected to infrared spectroscopy, nuclear magnetic hydrogen spectrum, and XRD detection. The specific method is as follows:
[0126] Infrared spectrum: The sample preparation method adopts hot pressing film forming, and the wave number range is 4000~400cm -1 , scan times: 16 times, resolution: 4, sampling method: transmission;
[0127] H NMR spectrum: Deuterated trifluoroacetic acid was used as solvent and tetramethylsilane (TMS) was used as internal standard.
[0128] XRD: X-ray diffractometer (XRD) was used according to the standard JY / T 0587-2020.
[0129] Using XRD testing, the crystallization peak (sharp peak) and the non-crystallization peak area (diffuse peak) are obtained, and the crystallinity is calculated according to the following formula:
[0130] Where:
[0131] Wc-crystallinity
[0132] I C -Integrated area of diffraction peak in crystalline state
[0133] I a -Integrated area of diffraction peak of amorphous state
[0134] The infrared spectrum of the PBET copolyester of Example 1 is shown in FIG1 , the H-NMR spectrum is shown in FIG2 , and the XRD pattern is shown in FIG3 .
[0135] The test results for the examples are shown in Table 4, and the test results for the comparative examples are shown in Table 5. The mold shrinkage was evaluated for an ABS / PBET alloy containing 35% PBET. 65 parts of ABS (grade PA757) resin, 35 parts of PBET resin, 0.2 parts of an antioxidant (antioxidant 1076 and antioxidant 168 in a 1:1 mass ratio), and 0.2 parts of a weathering agent (UV770) were uniformly mixed. The mixture was then melt-mixed and extruded into pellets at 230-245°C using a twin-screw extruder.
[0136] Table 4
[0137] Table 5
[0138] The test results in Table 4 show that the PBET copolyesters produced using recycled PBT and PET as raw materials have extremely low metal ion content, with some examples showing zinc ion content ≤70 ppm, titanium ion content ≤85 ppm, and calcium ion content ≤35 ppm. Furthermore, the PBET copolyesters produced in these examples also exhibit good dimensional stability and excellent toughness, with an Izod notched impact strength of ≥4.0 kJ / m. 2 .
[0139] Examples 1, 4, and 6 show that when phytic acid is used as a chelating agent, the metal ion content of the PBET copolyester is relatively lower, the notched Izod impact strength is relatively higher, and the PBET copolyester exhibits excellent mechanical properties. Comparative Example 1 and Comparative Example 2 show that, without the addition of a chelating agent, the metal ion content of the PBET copolyester obtained is very high. Excessive residual metal ions also degrade the toughness of the PBET copolyester. Furthermore, Comparative Examples 1 and 2 exhibit high mold shrinkage, indicating decreased dimensional stability.
[0140] According to the test results of Comparative Examples 3 and 4, it can be seen that during the re-depolymerization process in step S2, when the re-depolymerization temperature is greater than 190°C and when the re-depolymerization temperature is less than 160°C, the removal effect of metal ions is poor, and the residual amount of metal ions is high. In addition, the mold shrinkage rate of the products obtained in Comparative Examples 3-4 shows an increasing trend, that is, the dimensional stability decreases. Comparative Example 5 has a high crystallinity and a high mold shrinkage rate.
[0141] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the essence and scope of the technical solutions of the present invention.
Claims
1. A PBET copolyester, characterized in that: The PBET copolyester is derived from repeating units of the following components: Component A: aromatic dicarboxylic acid; Component B: based on the total molar amount of component B, comprising 60 to 96 mol% of 1,4-butanediol or 1,3-butanediol and 4 to 40 mol% of ethylene glycol; The crystallinity of the PBET copolyester is 5-20%, the zinc content in the PBET copolyester is ≤100ppm, and the titanium content is ≤120ppm.
2. The PBET copolyester according to claim 1, characterized in that The melting point of the PBET copolyester is 200-220°C.
3. The PBET copolyester according to claim 1, characterized in that The relative viscosity of the PBET copolyester is 1.4 to 1.
8.
4. The PBET copolyester according to claim 1, characterized in that The terminal carboxyl content of the PBET copolyester is 20 to 37 mmol / t.
5. The PBET copolyester according to claim 1, characterized in that: The zinc content in the PBET copolyester is 35-70 ppm, and the titanium content is 40-85 ppm.
6. The method for preparing the PBET copolyester according to any one of claims 1 to 5, characterized in that: The steps include: S1. Initial depolymerization: Dissolving the waste polyester in an alcohol solvent containing a depolymerization catalyst, and carrying out a primary depolymerization reaction under normal pressure, an inert gas atmosphere, and microwave conditions to obtain a primary depolymerization product; The waste polyester includes one or more of recycled polyethylene terephthalate, polybutylene terephthalate, and PET / PBT alloy; The temperature of the initial depolymerization reaction is 180-230°C and the time is 20-120 minutes; S2. Re-depolymerization: Extract part of the diol from the primary depolymerization product obtained in step S1, add a chelating agent, and perform a re-depolymerization reaction under normal pressure, inert gas atmosphere, and microwave conditions. After filtering the reactant, the filtrate obtained is is the re-depolymerization product; The temperature of the re-depolymerization reaction is 160-190°C and the time is 10-20 minutes; S3. Polycondensation: After removing excess alcohol from the re-depolymerization product of step S2, the product is mixed with a polycondensation catalyst and a stabilizer, and a polycondensation reaction is carried out under vacuum conditions until the relative viscosity is 1.4 to 1.8 to obtain the PBET copolyester.
7. The preparation method according to claim 6, characterized in that: In step S2, the chelating agent includes at least one of chitosan, activated carbon, lignin, and phytic acid, preferably phytic acid.
8. The preparation method according to claim 6, characterized in that: In step S2, the amount of the chelating agent added is 0.01-0.1 wt.% of the waste polyester.
9. The preparation method according to claim 6, characterized in that: Includes at least one of the following features (a) to (c): (a) The depolymerization catalyst comprises at least one of zinc acetate, antimony acetate, sodium carbonate, titanate nanotubes, titanium phosphate, and butyl titanate; (b) When the waste polyester contains PET, the alcohol solvent contains 1,4-butanediol or 1,3-butanediol; when the waste polyester contains PBT, the alcohol solvent contains ethylene glycol; (c) The polycondensation catalyst includes at least one of butyl titanate, tetraisopropyl titanate, titanium-phosphorus compounds, titanium-silicon compounds, titanium-magnesium composite catalysts, ethylene glycol titanate, butanediol titanate, titanium dioxide, antimony dioxide, and monobutyl tin oxide.
10. Use of the PBET copolyester according to any one of claims 1 to 5 in the preparation of toys and precision instruments.
Citation Information
Patent Citations
Preparation method of 1,3-butanediol modified PBTPET (Polybutylece Terephthalate Polyethylene Terephthalate) copolymer fiber
CN101824140A
Improved process for the preparation of modified poly(alkylene terephthalate) employing an in-situ titanium-containing catalyst
CN105452330A
Amorphous copolyester and preparation method thereof
CN106866948A
Continuous preparation method of biodegradable block co-polyester and biodegradable block co-polyester
CN112745489A
Method for preparing regenerated polyester by closed-loop recovery of waste polyester with typical green and low-carbon characteristics
CN114031756A
Cited By
Solvent type amorphous polymer copolyester as well as preparation method and application thereof