Cellulose derivative and method for producing same, and composition containing cellulose derivative
The production of amide-modified cellulose ethers with a high degree of substitution is achieved through a low-temperature reaction of cellulose derivatives with α-bromocarboxamide, addressing the limitations of existing methods and providing cellulose ethers with enhanced alkali resistance for industrial use.
Patent Information
- Application Number
- PCT/JP2023/033248
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-08
- Filing Date
- 2023-09-12
- Publication Date
- 2024-11-14
AI Technical Summary
Current methods for producing amide-modified carboxymethyl cellulose face challenges such as high water solubility of carboxymethyl cellulose, difficulty in amidation reactions, high temperature requirements, use of toxic cyanide, and limitations with aromatic amines and high total average degree of substitution, making them unsuitable for industrial-scale production.
A method involving a cellulose derivative soluble in general-purpose organic solvents, reacting with an α-bromocarboxamide in the presence of a base catalyst at low temperatures, using aromatic amides, and achieving a total average degree of substitution of 1.5 or more, which allows for the production of amide-modified cellulose ethers with improved alkali resistance.
This method enables the simple production of amide-modified cellulose ethers with high yield and excellent alkali resistance, suitable for industrial applications, particularly in water treatment membranes requiring chemical resistance.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Cellulose derivative, method for producing the same, and composition containing the cellulose derivative
[0001] The present disclosure relates to cellulose derivatives and methods for producing the same, as well as compositions containing the cellulose derivatives.
[0002] Cellulose derivatives are semi-synthetic materials obtained by chemically treating cellulose, a natural polymer, and by chemically treating cellulose, which is insoluble in water or common organic solvents, various cellulose derivatives with different solubility, thermal properties, chemical properties, etc. Specific examples include cellulose esters including cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cellulose acetate phthalate, and nitrocellulose, and cellulose ethers including methyl cellulose, ethyl cellulose, benzyl cellulose, cyanoethyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropylmethyl cellulose, and carboxymethyl cellulose.
[0003] Among these, for example, carboxymethyl cellulose (hereinafter, sometimes referred to as CMC) has excellent thickening properties, water absorption properties, and water retention properties, and is used in a wide range of applications including food, pharmaceuticals, cosmetics, and construction. Furthermore, by amide-modifying carboxymethyl cellulose, its solubility in water and common organic solvents can be changed.
[0004] Patent Document 1 describes a method for producing alkylamide-modified carboxymethyl cellulose by dissolving carboxymethyl cellulose in an ionic liquid, adding an alkylamine having 1 to 6 carbon atoms or ammonia as an amidating agent, and heating the mixture at 120°C to 160°C.
[0005] Patent Document 2 describes a method for producing an aliphatic amide-modified carboxyl-containing polysaccharide, particularly an aliphatic amide-modified carboxymethyl cellulose, by converting carboxymethyl cellulose (CMC) into an aliphatic amine salt in an ethanol / water solvent and heating the resulting solid in xylene at 140°C.
[0006] Patent Document 3 describes a method for forming a polysaccharide acid amide composition by reacting the hydroxyl groups of a polysaccharide with an alkali metal cyanide compound in the presence of a primary or secondary aliphatic amine.
[0007] JP 2009-114437 A JP 08-508538 A U.S. Pat. No. 5,760,199 A
[0008] To obtain amide-modified carboxymethyl cellulose, it is generally necessary to use carboxymethyl cellulose as a raw material. However, as the degree of substitution of the carboxymethyl group increases, carboxymethyl cellulose becomes more water-soluble, making it difficult to modify in the presence of a solvent suitable for the amidation dehydration reaction. When using the ionic liquid described in Patent Document 1, if a high-boiling amine such as an aromatic amine is used, it becomes difficult to recover the ionic liquid. Furthermore, no examples using CMC with a high total average degree of substitution are described. The methods described in Patent Documents 1 and 2 require reactions at high temperatures of 120°C or higher, making them difficult to carry out in an industrial reaction vessel. The method described in Patent Document 3 requires the use of cyanides, which are highly toxic and require careful handling, making them difficult to implement industrially. Furthermore, neither document describes an example using an aromatic amine with low nucleophilicity. The present disclosure discloses a method for directly obtaining amide-modified CMC by using a cellulose derivative soluble in a common organic solvent as a raw material and reacting it with an intermediate that reacts at low temperatures.
[0009] An object of the present disclosure is to produce an amide-modified cellulose ether by a simple method and to provide an amide-modified cellulose ether with an aromatic amide.
[0010] A first aspect of the present disclosure relates to a cellulose derivative having a repeating unit represented by the following formula (1), in which the total average substitution degree of a hydroxyl-protecting group, a group represented by the following formula (1-a), and a group represented by the following formula (1-b) is 1.5 or more. [In the above formula (1), R may be the same or different and represent a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the following formula (1-a), or a group represented by the following formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (1) is a group represented by the following formula (1-a)] (In the above formula (1-a), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-a), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.) (In the above formula (1-b), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-b), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.)
[0011] A second aspect of the present disclosure relates to a method for producing the above-mentioned cellulose derivative, comprising a step (i) of reacting, in the presence of a base catalyst, a hydroxyl group at the 2-, 3-, or 6-position of a cellulose derivative having a repeating unit represented by the following formula (2), with an α-bromocarboxamide represented by the following formula (3): [In the above formula (2), R may be the same or different and is a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the above formula (1-a), or a group represented by the above formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (2) is a hydrogen atom.] [In the above formula (3), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (3), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.]
[0012] According to the present disclosure, it is possible to produce an amide-modified cellulose ether by a simple method, and to provide an amide-modified cellulose ether with an aromatic amide.
[0013] The cellulose derivative obtained in Example 2 1 H-NMR measurement data of the cellulose derivative obtained in Example 8 1 H-NMR measurement data of the cellulose derivative obtained in Example 9 1H-NMR measurement data of the cellulose derivative obtained in Example 11 1 H-NMR measurement data of the cellulose derivative obtained in Example 23 1 H-NMR measurement data of the cellulose derivative obtained in Example 24 1 H-NMR measurement data
[0014] [Cellulose Derivative] The cellulose derivative of the present disclosure (hereinafter may be referred to as "cellulose derivative (1)") has a repeating unit represented by the following formula (1) (hereinafter may be referred to as "glucose unit"), and has a total average degree of substitution of a hydroxyl-protecting group, a group represented by the following formula (1-a), and a group represented by the following formula (1-b) of 1.5 or more. [In the above formula (1), R may be the same or different and represent a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the following formula (1-a), or a group represented by the following formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (1) is a group represented by the following formula (1-a)] (In the above formula (1-a), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-a), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.) (In the above formula (1-b), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-b), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.)
[0015] (Substitution Degree) In the cellulose derivative (1), the total average degree of substitution of the hydroxyl-protecting group, the group represented by the following formula (1-a), and the group represented by the following formula (1-b) is 1.5 or more, preferably 1.7 or more, more preferably 1.8 or more, even more preferably 2.0 or more, and particularly preferably 2.5 or more. The total average degree of substitution may be 3 or less.
[0016] In the present disclosure, the average degree of substitution refers to the average value of the degree of substitution of hydrogen atoms of hydroxyl groups at positions 2, 3, and 6 of glucose units constituting a cellulose derivative with groups other than hydrogen atoms, and in particular, the total average degree of substitution refers to the sum of the average degrees of substitution of the protecting group for the hydroxyl group, the group represented by the following formula (1-a), and the group represented by the following formula (1-b):
[0017] Of all R contained in the cellulose derivative (1), at least one is a group represented by the above formula (1-a), and the average degree of substitution of the group represented by the above formula (1-a) may be greater than 0. The average degree of substitution of the group represented by the above formula (1-a) is preferably 0.1 or more, more preferably 0.5 or more, even more preferably 1.7 or more, even more preferably 1.8 or more, and particularly preferably 2.0 or more. The average degree of substitution of the group represented by the above formula (1-a) may be 3 or less. The higher the ratio of the average degree of substitution of the group represented by the above formula (1-a) to the total value of the average degrees of substitution of the group represented by the above formula (1-a) and the group represented by the above formula (1-b), the better the alkali resistance.
[0018] The average degree of substitution of the hydroxyl-protecting groups in the cellulose derivative (1) may be 0 or more and less than 3. The average degree of substitution of the hydroxyl-protecting groups is preferably 2.5 or less, more preferably 2.2 or less, and even more preferably 1.1 or less.
[0019] When the protecting group for the hydroxyl group in the cellulose derivative (1) contains the following acetyl group, the average substitution degree of the acetyl group is preferably 1.5 or more and less than 3.0, more preferably 1.5 or more and 2.5 or less, even more preferably 1.7 or more and 2.5 or less, and particularly preferably 1.7 or more and 2.2 or less.
[0020] When the protecting group for the hydroxyl group in the cellulose derivative (1) contains the following trityl group, the average substitution degree of the trityl group is preferably more than 0 and not more than 2.5, more preferably not more than 2.2, and even more preferably not more than 1.1.
[0021] (Group represented by (1-a)) In the above formula (1-a), X may be the same or different and represent a hydrogen atom or a methyl group, and it is preferable that at least one of X is a methyl group, and it is particularly preferable that all X are methyl groups. This is because the cellulose derivative (1) can be obtained in a particularly excellent yield in the following step (i) or (iii) in the method for producing the cellulose derivative (1) of the present disclosure.
[0022] In the above formula (1-a), Ar is a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group. In the present disclosure, the monocyclic aromatic hydrocarbon group includes a monocyclic aromatic hydrocarbon group in which hydrogen atoms in an aromatic hydrocarbon are substituted with other groups, and an unsubstituted monocyclic aromatic hydrocarbon group, and the polycyclic aromatic hydrocarbon group includes a polycyclic aromatic hydrocarbon group in which hydrogen atoms in a polycyclic aromatic hydrocarbon are substituted with other groups, and an unsubstituted polycyclic aromatic hydrocarbon group. In addition, the polycyclic aromatic hydrocarbon group is a group having a hydrocarbon in which two or more aromatic rings are fused.
[0023] In the above formula (1-a), Ar is not an aliphatic hydrocarbon group but a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group. This facilitates the production of an α-ketoaziridine derivative represented by the following formula (3-a), which is an intermediate in the reaction of the following step (i) or (iii), in the production method of cellulose derivative (1) of the present disclosure, and makes it possible to obtain cellulose derivative (1) in an excellent yield.
[0024] Examples of monocyclic aromatic hydrocarbon groups include unsubstituted phenyl groups, as well as substituted monocyclic aromatic hydrocarbon groups, such as monocyclic aromatic hydrocarbon groups in which the hydrogen atoms in the phenyl group have been substituted with halogen atoms, alkyl groups having 1 to 24 carbon atoms, alkenyl groups having 1 to 24 carbon atoms, alkynyl groups having 1 to 24 carbon atoms, alkoxy groups having 1 to 24 carbon atoms, acyl groups having 1 to 24 carbon atoms, alkoxycarbonyl groups (ester groups) having 1 to 24 carbon atoms, trifluoromethyl groups, and nitro groups. The number of substituents in the monocyclic aromatic hydrocarbon group may be 1, 2, 3, 4, or 5, and the positions of the substituents are not limited. From the viewpoint of chemical stability, phenyl groups are preferred as monocyclic aromatic hydrocarbon groups. Furthermore, from the viewpoint of improving plasticity as a resin, alkyl group-substituted monocyclic aromatic hydrocarbon groups are preferred.
[0025] In the above formula (1-a), when Ar is a monocyclic aromatic hydrocarbon group and the monocyclic aromatic hydrocarbon group is a phenyl group, it is preferable that at least one of the Xs in the above formula (1-a) is a methyl group. That is, it is preferable that both of the two Xs in the above formula (1-a) are methyl groups, or that one is hydrogen and the other is a methyl group. Furthermore, it is more preferable that both of the two Xs in the above formula (1-a) are methyl groups.
[0026] Examples of polycyclic aromatic hydrocarbon groups include monovalent substituents formed by substituting one hydrogen atom from unsubstituted polycyclic aromatic hydrocarbons such as naphthalene, anthracene, phenanthrene, pyrene, triphenylene, and tetracene, as well as substituted polycyclic aromatic hydrocarbon groups, such as polycyclic aromatic hydrocarbon groups in which a hydrogen atom in the polycyclic aromatic hydrocarbon has been substituted with a halogen atom, an alkyl group having 1 to 24 carbon atoms, an alkenyl group having 1 to 24 carbon atoms, an alkynyl group having 1 to 24 carbon atoms, an alkoxy group having 1 to 24 carbon atoms, an acyl group having 1 to 24 carbon atoms, an alkoxycarbonyl group (ester group) having 1 to 24 carbon atoms, etc., a trifluoromethyl group, or a nitro group. The number of substituents in the polycyclic aromatic hydrocarbon group is not limited and may be, for example, 1 to 12, and the position of the substituent is also not limited.
[0027] (Hydroxyl Group-Protecting Group) Examples of the hydroxyl group-protecting group include well-known and commonly used protecting groups, such as silyl-based protecting groups such as trimethylsilyl, triethylsilyl, triisopropylsilyl, triphenylsilyl, t-butyldimethylsilyl, dimethylthexylsilyl, and t-butyldiphenylsilyl; acetal-based protecting groups such as tetrahydropyranyl and methoxymethyl; aralkyl groups having 6 to 15 carbon atoms such as benzyl and p-methoxybenzyl; alkenyl groups such as allyl; ether-based protecting groups such as trityl and methoxytrityl; aliphatic acyl groups having 1 to 5 carbon atoms or aromatic acyl groups having 6 to 15 carbon atoms such as acetyl, pivaloyl, benzoyl, and trimethylbenzoyl; and ester-based protecting groups such as p-toluenesulfonyl. Among these, an acetyl group or a trityl group is preferred from the viewpoints that it can be subjected to weakly basic reaction conditions, the cellulose derivative as the raw material is soluble in a general-purpose organic solvent, and can be deprotected with an inexpensive acid or base.
[0028] (Group represented by (1-b)) Of all R contained in the cellulose derivative (1) of the present disclosure, at least one may be a group represented by the following formula (1-b), and the average substitution degree of the group represented by the following formula (1-b) may be greater than 0, but is preferably 1 or less, more preferably 0.6 or less.
[0029] Furthermore, in R at the 6-position of the cellulose derivative (1), the group represented by the following formula (1-b) is preferably 50 mol % or less, more preferably 30 mol % or less, and even more preferably 20 mol % or less, based on the total number of moles of the group represented by the following formula (1-a) and the group represented by the following formula (1-b). (In the above formula (1-b), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-b), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.)
[0030] In the above formula (1-b), it is preferable that each X is a methyl group, because this allows the cellulose derivative (1) to be obtained in a particularly excellent yield in the following step (i) or (iii) in the method for producing the cellulose derivative (1) of the present disclosure.
[0031] In the above formula (1-b), Ar is not an aliphatic hydrocarbon group but a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group, which facilitates the production of the α-ketoaziridine derivative represented by the above formula (3-a), which is a reaction intermediate in the production method of the cellulose derivative (1) of the present disclosure, and allows the cellulose derivative (1) to be obtained in an excellent yield.
[0032] Examples of the monocyclic aromatic hydrocarbon group and polycyclic aromatic hydrocarbon group include the same groups as those exemplified as Ar in the above formula (1-a).
[0033] In the above formula (1-b), when Ar is a monocyclic aromatic hydrocarbon group and the monocyclic aromatic hydrocarbon group is a phenyl group, it is preferable that at least one of the Xs in the above formula (1-b) is a methyl group. That is, it is preferable that both of the two Xs in the above formula (1-b) are methyl groups, or that one is hydrogen and the other is a methyl group. Furthermore, it is more preferable that both of the two Xs in the above formula (1-b) are methyl groups.
[0034] The form of the cellulose derivative (1) of the present disclosure is not particularly limited, and it can be used as a resin molding material, and examples thereof include powder, fiber, granule, and sheet forms.
[0035] Cellulose-based materials generally have the properties of being aqueous, having excellent water permeability, and being stain-resistant. Among all R groups contained in the cellulose derivative (1) of the present disclosure, at least one is a group represented by the above formula (1-a) and has an amide group. Therefore, in addition to these properties, the cellulose derivative (1) of the present disclosure has excellent alkali resistance. In particular, it has better alkali resistance than cellulose esters. Therefore, the cellulose derivative (1) of the present disclosure is suitable as a material for water treatment membranes, which require alkali resistance and chemical resistance.
[0036] [Composition] The composition of the present disclosure is a composition containing the cellulose derivative (1).
[0037] The composition may contain optional components other than the cellulose derivative depending on the intended use, such as plasticizers, stabilizers (e.g., antioxidants, ultraviolet absorbers, heat stabilizers, light stabilizers, etc.), colorants (e.g., dyes, pigments, etc.), flame retardants, antistatic agents, lubricants, antiblocking agents, dispersants, fluidizing agents, anti-dripping agents, and antibacterial agents.
[0038] Examples of the plasticizer include di-C phthalates such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dihexyl phthalate, dioctyl phthalate, and di-2-ethylhexyl phthalate. 1-12 Alkyl esters, phthalic acid C such as dimethoxyethyl phthalate 1-6 Alkoxy C 1-12 Alkyl esters, phthalic acid C such as butyl benzyl phthalate 1-12 Alkyl / Aryl-C 1-3 C alkyl esters, ethyl phthalyl ethylene glycolate, butyl phthalyl butylene glycolate, etc. 1-6 Alkylphthalyl C 2-4 Alkylene glycolate, trimellitic acid tri-C such as trimethyl trimellitate, triethyl trimellitate, trioctyl trimellitate, and tri-2-ethylhexyl trimellitate 1-12 Alkyl esters, pyromellitic acid tetra C such as tetraoctyl pyromellitic acid 1-12The plasticizer may contain aromatic carboxylic acid esters such as alkyl esters; azelaic acid esters such as diethyl azelate, dibutyl azelate, and dioctyl azelate; sebacate esters such as dibutyl sebacate and dioctyl sebacate; fatty acid esters such as butyl oleate and methylacetyl ricinoleate; triacetin, diglycerin tetraacetate, and the like; lower fatty acid esters of polyhydric alcohols such as glycerin, trimethylolpropane, pentaerythritol, and sorbitol; benzoic acid esters of polyhydric alcohols such as glycol ester dipropylene glycol dibenzoate; citric acid esters such as acetyl tributyl citrate; amides such as N-butylbenzenesulfonamide; and ester oligomers such as caprolactone oligomer. These plasticizers may be used alone or in combination of two or more.
[0039] [Method for Producing Cellulose Derivative] The cellulose derivative (1) of the present disclosure can be produced, for example, by the following production method: A method for producing a cellulose derivative, comprising step (i) of reacting, in the presence of a base catalyst, a hydroxyl group at the 2-, 3-, or 6-position of a cellulose derivative having a repeating unit represented by the following formula (2) (hereinafter, sometimes referred to as "cellulose derivative (2)") with an α-bromocarboxamide represented by the following formula (3):
[0040] (Cellulose Derivative (2)) The cellulose derivative (2) of the present disclosure has a repeating unit represented by the following formula (2). [In the above formula (2), R may be the same or different and is a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the above formula (1-a), or a group represented by the above formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (2) is a hydrogen atom.]
[0041] (Degree of substitution) Of all R contained in the cellulose derivative (2), at least one is a hydrogen atom. Furthermore, when at least one is a hydroxyl-protecting group, a group represented by the above formula (1-a), or a group represented by the above formula (1-b), the total average degree of substitution of the hydroxyl-protecting group, the group represented by the above formula (1-a), and the group represented by the above formula (1-b) may be 0.1 or more, 0.5 or more, 1.0 or more, 1.5 or more, 1.7 or more, 1.8 or more, 2.0 or more, or 2.5 or more, and may be less than 3.
[0042] The average degree of substitution of the hydroxyl-protecting groups in the cellulose derivative (2) may be from 0 to less than 3. The average degree of substitution of the hydroxyl-protecting groups is preferably 2.5 or less, more preferably 2.2 or less, and even more preferably 1.1 or less.
[0043] When the protecting group for the hydroxyl group in the cellulose derivative (2) contains the following acetyl group, the average substitution degree of the acetyl group is preferably 1.5 or more and less than 3.0, more preferably 1.5 or more and 2.5 or less, even more preferably 1.7 or more and 2.5 or less, and particularly preferably 1.7 or more and 2.2 or less.
[0044] When the protecting group for the hydroxyl group in the cellulose derivative (2) contains the following trityl group, the average substitution degree of the trityl group is preferably more than 0 and not more than 2.5, more preferably not more than 2.2, and even more preferably not more than 1.1.
[0045] The average degree of substitution of the group represented by the above formula (1-a) in the cellulose derivative (2) may be zero.
[0046] The cellulose derivative (2) is not limited as long as it has a repeating unit represented by the above formula (2), but specific examples thereof include those soluble in general-purpose organic solvents such as acetonitrile (hereinafter sometimes referred to as AN) and tetrahydrofuran (hereinafter sometimes referred to as THF), such as cellulose acetate, trityl cellulose, cellulose acetate propionate, cellulose acetate butyrate, etc. Furthermore, the cellulose derivative (1) can also be the cellulose derivative (2).
[0047] (Group represented by (1-a)) When the cellulose derivative (2) has a group represented by the above formula (1-a), the explanation regarding the group represented by the above formula (1-a) in the cellulose derivative (2) is the same as the explanation regarding the group represented by (1-a) itself in the section "(Group represented by (1-a))" of the cellulose derivative (1) above.
[0048] (Hydroxyl-protecting group) When the cellulose derivative (2) has a hydroxyl-protecting group, specific examples of the hydroxyl-protecting group in the cellulose derivative (2) are the same as the specific examples listed in the section "(Hydroxyl-protecting group)" for the cellulose derivative (1) above. Furthermore, the hydroxyl-protecting group in the production method for the cellulose derivative (1) of the present disclosure is preferably an acetyl group or a trityl group, from the viewpoints that the cellulose derivative as the raw material is soluble in a commonly used organic solvent and can be deprotected with an inexpensive acid or base.
[0049] (Group represented by (1-b)) When the cellulose derivative (2) has a group represented by the above formula (1-b), the explanation regarding the group represented by the above formula (1-b) in the cellulose derivative (2) is the same as the explanation regarding the group represented by (1-b) itself in the section "(Group represented by (1-b))" of the cellulose derivative (1) above.
[0050] (α-Bromocarboxamide) The α-bromocarboxamide of the present disclosure is represented by the following formula (3). [In the above formula (3), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (3), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.]
[0051] In the above formula (3), X may be the same or different and represent a hydrogen atom or a methyl group, and it is preferable that at least one of X is a methyl group, and it is particularly preferable that all X are methyl groups, because this can further increase the yield of the cellulose derivative (1) obtained by the production method of the present disclosure.
[0052] In the above formula (3), when one of X's is hydrogen and the other is a methyl group, it is called α-methylcarboxamide, and when both X's are methyl groups, it can be called α-dimethylcarboxamide. In this embodiment, it is preferable to use α-methylcarboxamide or α-dimethylcarboxamide among the compounds represented by the above formula (3).
[0053] In the above formula (3), Ar is a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group. In the above formula (3), Ar is not an aliphatic hydrocarbon group but a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group, which facilitates the production of the α-ketoaziridine derivative represented by the above formula (3-a), which is an intermediate in the reaction of the above step (i) or (iii), and allows the cellulose derivative (1) to be obtained in high yield. Therefore, by changing the substituent of the monocyclic aromatic hydrocarbon group or polycyclic aromatic hydrocarbon group, it is possible to produce cellulose derivatives (1) having various substituents.
[0054] The explanation regarding specific examples of the monocyclic aromatic hydrocarbon group and polycyclic aromatic hydrocarbon group in the above formula (3) and suitable substituents thereamong is the same as the explanation regarding specific examples of the monocyclic aromatic hydrocarbon group and polycyclic aromatic hydrocarbon group in the above formula (1-a) and suitable substituents thereamong.
[0055] In the above formula (3), when Ar is a monocyclic aromatic hydrocarbon group and the monocyclic aromatic hydrocarbon group is a phenyl group, it is preferable that at least one of the Xs in the above formula (3) is a methyl group. That is, it is preferable that both of the two Xs in the above formula (3) are methyl groups, or that one is hydrogen and the other is a methyl group. Furthermore, it is more preferable that both of the two Xs in the above formula (3) are methyl groups.
[0056] The amount of α-bromocarboxamide represented by the formula (3) used in the step (i) is preferably 1 to 3 molar equivalents, more preferably 1 to 2 molar equivalents, and even more preferably 1 to 1.5 molar equivalents, per mole of the total hydroxyl groups at the 2-, 3-, or 6-positions of the entire cellulose derivative (2).
[0057] (Base Catalyst) The base catalyst used in the step (i) is not particularly limited as long as it can catalyze the reaction in the step (i). Examples of the base catalyst include sodium carbonate, potassium carbonate, and cesium carbonate (Cs 2 CO 3 Examples of suitable inorganic bases include non-nucleophilic inorganic bases such as carbonates containing α-bromocarboxamide, and phosphates such as sodium phosphate, potassium phosphate, and cesium phosphate. Among these, carbonates and phosphates are preferred from the viewpoint of suppressing the decomposition reaction of α-bromocarboxamide, and potassium salts are more preferred as the metal ion from the viewpoint of increasing the activation effect in the reaction, with cesium salts being more preferred. Cesium carbonate is particularly preferred. In the coexistence of the copper compound described below and the copper ligand in the copper compound, carbonates and phosphates are preferred from the viewpoint of suppressing the decomposition reaction of α-bromocarboxamide, and potassium and cesium are more preferred as the metal ion from the viewpoint of suppressing the decomposition reaction of α-bromocarboxamide.
[0058] The amount of the base catalyst used in the above step (i) is preferably 1 to 5 molar equivalents, more preferably 1 to 3 molar equivalents, and even more preferably 1 to 2 molar equivalents, per mole of the α-bromocarboxamide used.
[0059] The reaction in step (i) may be a reaction in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst. By allowing the copper compound and the copper ligand in the copper compound to coexist with the base catalyst, the substitution reaction with the group represented by formula (1-a) proceeds preferentially over the group represented by formula (1-b), and therefore the degree of substitution with the group represented by formula (1-a) for the hydroxyl groups at the 2-, 3-, or 6-position of the cellulose derivative (2) can be increased relative to the degree of substitution with the group represented by formula (1-b). The copper compound also acts as a catalyst for the reaction in step (i).
[0060] The ratio of the average substitution degree of the group represented by formula (1-a) to the total value of the average substitution degrees of the group represented by formula (1-a) and the group represented by formula (1-b) substituted in the reaction of step (i) may be, for example, 50% or more, 70% or more, or 90% or more.
[0061] The copper compound is not particularly limited, and examples thereof include monovalent, divalent, or trivalent copper compounds; inorganic copper compounds; and organic copper compounds. Examples of monovalent copper compounds include copper chloride (I), copper bromide (I), copper bromide (I) dimethyl sulfide complex, and copper halides including copper iodide (I), oxygen-coordinated copper such as copper oxide (I), copper acetate (I), and copper 2-thiophenecarboxylate (I), as well as copper cyanide (I). Examples of divalent copper compounds include copper chloride (II), copper halides including copper bromide (II), copper oxide (I), and copper acetate (I). Among these, monovalent copper compounds are preferred from the viewpoint of enhancing the activation effect in the reaction, and copper chloride (I), copper bromide (I), copper bromide (I) dimethyl sulfide complex, and copper iodide (I) are more preferred.
[0062] The amount of the copper compound used in the reaction of step (i) is preferably 0.005 to 0.3 molar equivalents, more preferably 0.01 to 0.2 molar equivalents, and even more preferably 0.01 to 0.1 molar equivalents, per mole of the total hydroxyl groups at the 2-, 3-, or 6-positions of the entire cellulose derivative (2).
[0063] The copper compound is preferably used in combination with a copper ligand in the copper compound, from the viewpoint of increasing the activation effect in the reaction.
[0064] The copper ligand in the copper compound is not particularly limited, and examples thereof include monodentate phosphine ligands and bidentate phosphine ligands. Examples of monodentate phosphine ligands include triphenylphosphine, tri(o-tolyl)phosphine, tri(2-furyl)phosphine, cyclohexyldiphenylphosphine, dicyclohexylphenylphosphine, dicyclohexylphosphino-2',6'-dimethoxybiphenyl, tricyclohexylphosphine, dicyclohexylphosphino-2',4',6'-triisopropylbiphenyl, tricyclohexylphosphine, tri-n-butylphosphine, tri-t-butylphosphine, and tri-t-butylphosphinium tetrafluoroborate. Examples of bidentate phosphine ligands include bisdiphenylphosphinoferrocene, bisdiphenylphosphinopropane, bisdiphenylphosphinoethane, and bisdiphenylphosphinomethane. Among these, monodentate phosphine ligands are preferred from the viewpoint of increasing the activation effect in the reaction, and among these, triphenylphosphine and tricyclohexylphosphine are more preferred.
[0065] In addition, the amount of the copper ligand in the copper compound used in combination with the copper compound in the reaction of the above step (i) is preferably 1 to 3 molar equivalents, more preferably 1 to 2 molar equivalents, and even more preferably 1 to 1.5 molar equivalents, per mole of the copper compound used.
[0066] (Solvent) The reaction in step (i) is preferably carried out in the presence of a solvent. Examples of the solvent include aprotic solvents, such as aromatic hydrocarbons (e.g., benzene, toluene, xylene, ethylbenzene, etc.); halogenated hydrocarbons (e.g., chloroform, dichloromethane, 1,2-dichloroethane, etc.); ethers (e.g., diethyl ether, dimethoxyethane, tetrahydrofuran, dioxane, etc.); ketones (e.g., acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.); esters (e.g., methyl acetate, ethyl acetate, isopropyl acetate, butyl acetate, etc.); amides (e.g., N,N-dimethylformamide, N,N-dimethylacetamide, etc.); nitriles (e.g., acetonitrile, propionitrile, benzonitrile, etc.); and dimethyl sulfoxide. These solvents may be used alone or in combination of two or more. Among these, aromatic hydrocarbons, ethers, esters, and nitriles are preferred from the viewpoint of being less likely to cause side reactions. Furthermore, acetonitrile or tetrahydrofuran is preferred because of their low boiling points, ease of recovery, and excellent versatility.
[0067] When the reaction in step (i) is carried out in the presence of a solvent, the amount of the solvent used may be, for example, 1 to 20 mL, preferably 1 to 10 mL, and more preferably 1 to 5 mL per 1 mmol of the starting cellulose derivative, from the viewpoint of increasing the reaction rate.
[0068] The atmosphere for the reaction in the above step (i) is not particularly limited as long as it does not inhibit the reaction, and may be, for example, any of an air atmosphere, a nitrogen atmosphere, an argon atmosphere, and the like.
[0069] The reaction temperature in step (i) can be adjusted appropriately depending on the solvent used, and may be, for example, 20° C. (room temperature) to 150° C., or 20° C. (room temperature) to 100° C., and preferably about 20° C. (room temperature) to 60° C. The reaction time is, for example, 3 to 24 hours, preferably 5 to 24 hours or 5 to 15 hours, but may be 24 hours or longer.
[0070] The reaction mechanism of the above step (i) is as follows: in the presence of a base catalyst, an α-ketoaziridine derivative represented by the above formula (3-a), which is a reaction intermediate, is generated from the α-bromocarboxamide represented by the above formula (3), and the α-ketoaziridine derivative reacts with the hydroxyl group at the 2-, 3-, or 6-position of the cellulose derivative (2), thereby producing the cellulose derivative (1).
[0071] As shown in the following reaction formula, in the reaction of an α-ketoaziridine derivative with a hydroxyl group at the 2-, 3-, or 6-position of a cellulose derivative (2), substitution with a group represented by the above formula (1-b) is also included, and the resulting cellulose derivative (1) may have a group represented by the above formula (1-b) in addition to the group represented by the above formula (1-a).
[0072] When the reaction of step (i) is carried out in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst, the reaction with the hydroxyl group at the 2-, 3-, or 6-position of cellulose derivative (2) involves oxidative addition to a carbon-bromine bond, followed by ligand exchange with the hydroxyl group, and reductive elimination, to preferentially produce a group represented by formula (1-a), as shown in the following reaction formula:
[0073] According to the above step (i), the cellulose derivative (1) can be produced in an excellent yield. The yield in the above step (i) may be 30% or more, preferably 50% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. The yield in the above step (i) refers to the ratio of the number of moles of the cellulose derivative (1) that is the product of the above step (i) to the number of moles of the cellulose derivative having the repeating unit represented by the above formula (2) charged in the above step (i).
[0074] Furthermore, when at least one of all R contained in the cellulose derivative (2) is a protecting group for a hydroxyl group, the method for producing the cellulose derivative (1) of the present disclosure may include, after the step (i), a step (ii) of removing the protecting group for the hydroxyl group and substituting it with a hydroxyl group.
[0075] As a method for removing the protecting group of the hydroxyl group and substituting it with a hydroxyl group, a known method can be used for each of the well-known and commonly used protecting groups. For example, if the protecting group is a silyl group, a method of treating with a fluoride is used; if the protecting group is an acetal protecting group, a method of treating with an acid such as hydrochloric acid, acetic acid, or hydrogen bromide is used; if the protecting group is a C 1-5 aliphatic acyl group or C 6-15 For aromatic acyl groups, a method of treating under basic conditions such as treating with potassium carbonate in an alcohol / water mixture such as methanol; 7-15 In the case of an aralkyl group, an allyl group, etc., a method of treating by hydrogenation in the presence of a catalyst such as palladium / carbon can be mentioned; in the case of a trityl group, a method of treating with an acid such as acetic acid or hydrochloric acid can be mentioned.
[0076] The case where the hydroxyl-protecting group in step (ii) contains a trityl group and the trityl group is eliminated will be described below. The acid used in step (ii) is not particularly limited as long as it can eliminate the trityl group and replace it with a hydroxyl group, and examples thereof include hydrochloric acid, hydrobromic acid, a hydrobromic acid / acetic acid solution, and hydroiodic acid. Among these, a hydrobromic acid / acetic acid solution is preferred from the viewpoints of high compatibility with organic solvents and easy reaction progress.
[0077] The reaction in step (ii) is preferably carried out in the presence of a solvent, such as a halogenated hydrocarbon such as chloroform or dichloromethane.
[0078] Furthermore, when the reaction in the above step (ii) is carried out in the presence of a solvent, the amount of the solvent used may be, for example, 1 to 20 mL, preferably 1 to 10 mL, and more preferably 1 to 5 mL per 1 mmol of the starting cellulose derivative, from the viewpoint of increasing the reaction rate.
[0079] The atmosphere for the reaction in the above step (ii) is not particularly limited as long as it does not inhibit the reaction, and may be, for example, any of an air atmosphere, a nitrogen atmosphere, an argon atmosphere, and the like.
[0080] The reaction temperature in step (ii) can be adjusted appropriately depending on the solvent used, and may be, for example, room temperature to 60° C. or room temperature to 40° C., preferably room temperature of about 25° C. The reaction time may be, for example, 5 to 180 minutes, 5 to 60 minutes, or 5 to 30 minutes.
[0081] The above is an explanation of the case where the hydroxyl-protecting group in the above step (ii) contains a trityl group and the trityl group is eliminated.
[0082] Even when the step (ii) is included, the cellulose derivative (1) can be produced in an excellent yield. The yield in the step (ii) may be 30% or more, preferably 50% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. The yield in the step (ii) refers to the ratio of the number of moles of the cellulose derivative (1) that is the product of the step (ii) to the number of moles of the cellulose derivative having the repeating unit represented by the formula (2) charged in the step (i).
[0083] Furthermore, the method for producing the cellulose derivative (1) of the present disclosure may include a step (iii) of reacting, in the presence of a base catalyst, an α-bromocarboxamide represented by the above formula (3) with a hydroxyl group at the 2-, 3-, or 6-position of the cellulose derivative obtained in the above step (ii), including a hydroxyl group substituted with a hydrogen atom from a protecting group in the above step (ii).
[0084] The base catalyst used in step (iii) is not particularly limited as long as it can catalyze the reaction in step (iii), and the same catalyst as in step (i) can be used. Cesium carbonate is also preferred as the base catalyst used in step (iii) from the viewpoint of suppressing the decomposition reaction of α-bromocarboxamide. Similarly to step (i), phosphates are preferred, and potassium phosphate is more preferred, from the viewpoint of suppressing the decomposition reaction of α-bromocarboxamide in the coexistence of the copper compound and the copper ligand in the copper compound.
[0085] The amount of the base catalyst used in the above step (iii) is preferably 1 to 5 molar equivalents, more preferably 1 to 3 molar equivalents, and even more preferably 1 to 2 molar equivalents, per mole of the α-bromocarboxamide used.
[0086] Furthermore, the reaction of step (iii) may be a reaction in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst. By allowing the copper compound and the copper ligand in the copper compound to coexist with the base catalyst, the substitution reaction with the group represented by formula (1-a) proceeds preferentially over the group represented by formula (1-b). Therefore, in the cellulose derivative obtained by step (ii), the degree of substitution with the group represented by formula (1-a) for the hydroxyl group at the 2-, 3-, or 6-position, including the hydroxyl group substituted by step (ii), can be increased compared to the degree of substitution with the group represented by formula (1-b). The copper compound also acts as a catalyst for the reaction of step (iii).
[0087] The ratio of the average substitution degree of the group represented by formula (1-a) to the total value of the average substitution degrees of the group represented by formula (1-a) and the group represented by formula (1-b) substituted in the reaction of step (iii) may be, for example, 50% or more, 70% or more, or 90% or more.
[0088] As the copper compound used in the step (iii) above, those exemplified in the step (i) above can be used in the amounts exemplified above.
[0089] The copper compound used in the step (iii) is preferably used in combination with a copper ligand in the copper compound, as in the step (i), and can be used in the amount exemplified in the step (i).
[0090] The reaction in step (iii) is preferably carried out in the presence of a solvent, and the same solvent as in step (i) can be used. As the solvent used in step (iii), acetonitrile or tetrahydrofuran is preferred because of its low boiling point, ease of recovery, and versatility.
[0091] When the reaction in the step (iii) is carried out in the presence of a solvent, the amount of the solvent used may be, for example, 1 to 20 mL, preferably 1 to 10 mL, and more preferably 1 to 5 mL per 1 mmol of the starting cellulose derivative, from the viewpoint of increasing the reaction rate.
[0092] The atmosphere for the reaction in the step (iii) is not particularly limited as long as it does not inhibit the reaction, and may be, for example, an air atmosphere, a nitrogen atmosphere, an argon atmosphere, or the like.
[0093] The reaction temperature in step (iii) can be adjusted appropriately depending on the solvent used, and may be, for example, 20° C. (room temperature) to 150° C., or 20° C. (room temperature) to 100° C., preferably room temperature of about 20° C. (room temperature) to 60° C. The reaction time is, for example, 3 to 24 hours, preferably 5 to 24 hours or 5 to 15 hours, but may be 24 hours.
[0094] The step (iii) also allows the production of cellulose derivative (1) in an excellent yield. The yield in the step (iii) may be 30% or more, preferably 50% or more, more preferably 70% or more, even more preferably 80% or more, and particularly preferably 90% or more. The yield in the step (iii) refers to the ratio of the number of moles of the cellulose derivative (1) produced in the step (iii) to the number of moles of the cellulose derivative having the repeating unit represented by the formula (2) charged in the step (i).
[0095] The reaction products obtained by the steps (i), (ii), and (iii) can be separated and purified by a separation means such as reprecipitation, filtration, drying, concentration, distillation, extraction, crystallization, adsorption, recrystallization, column chromatography, or a combination thereof.
[0096] The above-described configurations and combinations thereof of the present disclosure are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible as appropriate within the scope of the gist of the present disclosure. The present disclosure is not limited by the embodiments, but is limited only by the scope of the claims.
[0097] Additionally, each feature disclosed herein can be combined with any other feature disclosed herein.
[0098] The following items are preferred embodiments of the present disclosure, but the present invention is not limited to them. [Item 1] A cellulose derivative having a repeating unit represented by the following formula (1), in which the total average substitution degree of a hydroxyl-protecting group, a group represented by the following formula (1-a), and a group represented by the following formula (1-b) is 1.5 or more. [In the above formula (1), R may be the same or different and represent a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the following formula (1-a), or a group represented by the following formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (1) is a group represented by the following formula (1-a)] (In the above formula (1-a), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-a), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.) (In the above formula (1-b), X may be the same or different and represent hydrogen or a methyl group. Also, in the above formula (1-b), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.) [Item 2] The cellulose derivative according to item 1, wherein in the above formula (1-a) or (1-b), Ar represents a monocyclic aromatic hydrocarbon group. [Item 3] The cellulose derivative according to item 1, wherein in the above formula (1-a) or (1-b), Ar represents a polycyclic aromatic hydrocarbon group. [Item 4] The cellulose derivative according to any one of items 1 to 3, wherein the total average degree of substitution is 1.7 or more. [Item 5] The cellulose derivative according to any one of items 1 to 4, wherein the hydroxyl-protecting group is an acetyl group or a trityl group. [Item 6] The cellulose derivative according to any one of items 1 to 5, wherein at least one of all R contained in the cellulose derivative having a repeating unit represented by formula (1) is a group represented by formula (1-b). [Item 7] A composition comprising the cellulose derivative according to any one of items 1 to 6. [Item 8] A method for producing the cellulose derivative according to item 1, comprising step (i) of reacting, in the presence of a base catalyst, a hydroxyl group at the 2-, 3-, or 6-position of a cellulose derivative having a repeating unit represented by formula (2): [In the above formula (2), R may be the same or different and is a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the above formula (1-a), or a group represented by the above formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (2) is a hydrogen atom.] [In the formula (3), X may be the same or different and represent hydrogen or a methyl group. Furthermore, in the formula (3), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.] [Item 9] A method for producing a cellulose derivative according to Item 8, wherein at least one of all R contained in the cellulose derivative having a repeating unit represented by the formula (2) is a hydroxyl-protecting group, a group represented by the formula (1-a), or a group represented by the formula (1-b), and the cellulose derivative having a repeating unit represented by the formula (2) has a total average degree of substitution of the hydroxyl-protecting group, the group represented by the formula (1-a), and the group represented by the formula (1-b) of 1.5 or more. [Item 10] A method for producing a cellulose derivative according to Item 8 or 9, wherein Ar in the formula (3) is a monocyclic aromatic hydrocarbon group. [Item 11] A method for producing a cellulose derivative according to Item 8 or 9, wherein Ar in the formula (3) is a polycyclic aromatic hydrocarbon group. [Item 12] A method for producing the cellulose derivative according to any one of Items 8 to 11, wherein at least one of all R contained in the cellulose derivative having a repeating unit represented by Formula (2) is a hydroxyl-protecting group, and the method comprises, after Step (i), Step (ii) of removing the hydroxyl-protecting group and substituting it with a hydroxyl group. [Item 13] A method for producing the cellulose derivative according to any one of Items 8 to 12, wherein the hydroxyl-protecting group is an acetyl group or a trityl group. [Item 14] A method for producing the cellulose derivative according to Item 12 or 13, the method comprising Step (iii) of reacting, in the presence of a base catalyst, the hydroxyl group at the 2-, 3- or 6-position of the cellulose derivative obtained in Step (ii), including the hydroxyl group substituted in Step (ii). [Item 15] The method for producing a cellulose derivative according to any one of Items 8 to 14, wherein the reaction in step (i) is a reaction in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst. [Item 16] The method for producing a cellulose derivative according to Item 14, wherein the reaction in step (iii) is a reaction in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst.
[0099] The present disclosure will be explained in more detail below using examples, but the present invention is not limited to these examples.
[0100] Example 1: Cellulose acetate (1 in the following reaction formula (R1), product name "LL-10" (manufactured by Daicel Corporation), average degree of acetyl substitution of approximately 1.7, 0.10 g, 0.41 mmol) was placed in a two-necked flask as a starting cellulose derivative, and acetonitrile (0.86 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (2 in the following reaction formula (R1), 0.24 g, 0.80 mmol, 1.5 equivalents) and cesium carbonate (0.52 g, 1.60 mmol, 3.0 equivalents) were added as an α-bromocarboxamide, followed by stirring at room temperature (hereinafter also referred to as "rt"; 25°C) for 5 hours. The reaction solution was poured into a methanol aqueous solution (1 / 1, v / v) to reprecipitate the resulting solid, which was then collected by suction filtration. The resulting solid was washed with diethyl ether and dried in vacuo to obtain a cellulose derivative (0.146 g, yield: 92%) having a repeating unit represented by 3 in the following reaction formula (R1) as a pale orange solid. Note that the term "equivalent" used here refers to the relative amount to 1 mole of the total hydroxyl groups at the 2-, 3-, or 6-positions of the entire starting cellulose derivative (the same applies hereinafter to the Examples and Comparative Examples).
[0101] 1 From the results of H-NMR measurement, the average degree of substitution of the acetyl group of the obtained cellulose derivative was calculated to be about 1.7, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 1.3, and the total average degree of substitution to be about 3.0.
[0102] The cellulose derivative obtained in Example 1 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 8.4-8.7(br), 7.6(br), 7.2-7.4(br, overlapped with CHCl 3 ), 6.3-6.9(br), 2.8-5.9(br, CH, CH 2 : cellulose), 1.8-2.2 (br, CH 3 : acetyl) 1.2-1.8 (br, CH3 : (1-a) or (1-b))
[0103] Example 2 Cellulose acetate (1 in the following reaction formula (R1), trade name "FL-70" (manufactured by Daicel Corporation), average degree of acetyl substitution of approximately 2.1, 0.10 g, 0.40 mmol) was placed as a starting cellulose derivative in a two-necked recovery flask, and tetrahydrofuran (0.86 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (2 in the following reaction formula (R1), 0.13 g, 0.54 mmol, 1.5 equivalents) and cesium carbonate (0.35 g, 0.11 mmol, 3.0 equivalents) were added as an α-bromocarboxamide, and the mixture was stirred at room temperature for 24 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) to reprecipitate the resulting solid, which was collected by suction filtration. The resulting solid was washed with diethyl ether and dried in vacuo to obtain a cellulose derivative (0.151 g, yield: 86%) having a repeating unit represented by 3 in the following reaction formula (R1) as a pale orange solid.
[0104] 1 From the results of H-NMR measurement, the average degree of substitution of the acetyl group of the obtained cellulose derivative was calculated to be about 2.1, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) was about 0.9, and the total average degree of substitution was calculated to be about 3.0.
[0105] The cellulose derivative obtained in Example 2 1 The H-NMR spectrum data is shown in FIG. 1, and the chemical shift values are shown below. 1 H-NMR (500MHz, CDCl 3 ,r. t. ): δ 8.4-8.7(br), 7.6(br), 7.2-7.4(br, overlapped with CHCl 3 ), 6.3-6.9(br), 2.8-5.9(br, CH, CH 2 : cellulose), 1.8-2.2 (br, CH 3 : acetyl) 1.2-1.8 (br, CH 3 : (1-a) or (1-b)
[0106] Example 3: Trityl cellulose (4 in the following reaction formula (R2) [below], average trityl group substitution degree: approximately 1.0, 0.16 g, 0.40 mmol) was placed in a two-necked recovery flask as the starting cellulose derivative, and tetrahydrofuran (0.86 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (2 in the following reaction formula (R2) [below], 0.29 g, 1.20 mmol, 1.5 equivalents) and cesium carbonate (0.78 g, 2.40 mmol, 3.0 equivalents) were added as the α-bromocarboxamide, followed by stirring at room temperature for 24 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) for reprecipitation, and the resulting solid was collected by suction filtration. The resulting solid was washed with diethyl ether and dried in vacuo to obtain a cellulose derivative (0.250 g, yield: 86%) having a repeating unit represented by 5 in the following reaction formula (R2) as a pale orange solid.
[0107] 1 From the results of H-NMR measurement, the average degree of substitution of the trityl group in the obtained cellulose derivative was calculated to be about 1.0, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 2.0, and the total average degree of substitution to be about 3.0.
[0108] The cellulose derivative obtained in Example 3 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 8.9-9.8 (br, NH), 6.8-8.0 (br, overlapped with CHCl 3 ), 6.3-6.8(br), 2.8-6.0(br, CH, CH 2 : cellulose), 0.7-1.8 (br, CH 3 : (1-a) or (1-b))
[0109] Example 4 The same procedure as in Example 3 was carried out except that α-bromodimethylaceto(3,4,5-trimethoxy)anilide (6 in the following reaction formula (R3), 0.40 g, 1.20 mmol, 1.5 equivalents) was used instead of α-bromodimethylacetanilide as the α-bromocarboxamide, to obtain a cellulose derivative (0.214 g, yield: 59%) having a repeating unit represented by 7 in (R3) as a pale orange solid.
[0110] 1 From the results of H-NMR measurement, the average degree of substitution of the trityl group in the obtained cellulose derivative was calculated to be about 1.0, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 2.0, and the total average degree of substitution to be about 3.0.
[0111] The chemical shift values of the cellulose derivative obtained in Example 4 are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 9.1-9.4 (br, NH), 8.4 (s), 6.6-7.8 (br, overlapped with CHCl 3 ), 6.8(s), 6.2-6.6(br), 2.3-5.0(br, CH, CH 2 : cellulose), 3.85 (s), 3.80 (s), 1.3-1.7 (br, CH 3 : (1-a) or (1-b))
[0112] Example 5 A cellulose derivative (0.288 g, yield: 72%) having a repeating unit represented by 9 in (R2) was obtained as a pale orange solid by the same procedure as in Example 3, except that α-bromodimethylaceto(4-trifluoromethyl)anilide (8 in the following reaction formula (R4), 0.37 g, 1.20 mmol, 1.5 equivalents) was used instead of α-bromodimethylacetanilide as the α-bromocarboxamide.
[0113] 1 From the results of H-NMR measurement, the average degree of substitution of the trityl group in the obtained cellulose derivative was calculated to be about 1.0, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 2.0, and the total average degree of substitution to be about 3.0.
[0114] The chemical shift values of the cellulose derivative obtained in Example 5 are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 9.3-9.8 (br, NH), 6.8-8.2 (br, overlapped with CHCl 3 ), 6.2-6.6(br), 2.5-5.7(br, CH, CH 2 : cellulose), 0.7-2.3 (br, CH 3 : (1-a) or (1-b))
[0115] Example 6 The same procedure as in Example 3 was carried out except that 1-(α-bromodimethylacetoxy)aminopyrene (10 in the following reaction formula (R5), 0.44 g, 1.20 mmol, 1.5 equivalents) was used as the α-bromocarboxamide instead of α-bromodimethylacetanilide, to obtain a cellulose derivative (0.260 g, yield: 67%) having a repeating unit represented by 11 in (R5) as a pale orange solid.
[0116] 1 From the results of H-NMR measurement, the average degree of substitution of the trityl group in the obtained cellulose derivative was calculated to be about 1.0, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 2.0, and the total average degree of substitution to be about 3.0.
[0117] The chemical shift values of the cellulose derivative obtained in Example 6 are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 9.5-10.2 (br, NH), 7.6-8.4 (br), 6.6-7.6 (br, overlapped with CHCl 3 ), 2.5-5.0 (br, CH, CH 2 : cellulose), 0.8-2.0 (br, CH 3 : (1-a) or (1-b), overlapped with H 2 O)
[0118] Example 7 The same procedure as in Example 3 was carried out except that α-bromoacetanilide (12 in the following reaction formula (R6), 0.26 g, 1.20 mmol, 1.5 equivalents) was used instead of α-bromodimethylacetanilide as the α-bromocarboxamide, to obtain a cellulose derivative (0.187 g, yield: 70%) having a repeating unit represented by 13 in (R6) as a pale orange solid.
[0119] 1 From the results of H-NMR measurement, the average degree of substitution of the trityl group in the obtained cellulose derivative was calculated to be about 1.0, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 2.0, and the total average degree of substitution to be about 3.0.
[0120] The chemical shift values of the cellulose derivative obtained in Example 7 are shown below. 1 H-NMR (500MHz, CDCl 3 ,r. t. ): δ 6.8-7.7 (br, overlapped with CHCl 3 ), 2.3-4.8 (br, CH, CH 2 : cellulose), 4.6 (s, CH 2 : (1-a) or (1-b))
[0121] Example 8: The cellulose derivative obtained in Example 3 (5, 0.15 g, 0.20 mmol of reaction formula (R7) below) was placed in a two-necked recovery flask as the starting cellulose derivative. Chloroform (1 mL) was added under a nitrogen atmosphere and the mixture was stirred to dissolve. A 30 wt % hydrogen bromide solution in acetic acid (0.4 mL, 2 mmol) was added and stirred at room temperature (25°C) for 5 minutes. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) to reprecipitate the resulting solid, which was collected by suction filtration and washed with ethanol. The resulting solid was vacuum-dried to obtain a cellulose derivative (0.080 g, yield: 82%) having a repeating unit represented by 14 of reaction formula (R7) below as a pale orange solid.
[0122] 1 From the results of H-NMR measurement, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) of the obtained cellulose derivative was calculated to be about 2.0, and the total average degree of substitution was calculated to be about 2.0.
[0123] The cellulose derivative obtained in Example 8 1 The H-NMR measurement data is shown in FIG. 2, and the chemical shift values are shown below. 1 H-NMR (500MHz, DMSO-d6, rt.): δ 9.5-10.0 (br, NH), 7.6 (br), 7.25 (br), 7.0 (br) 6.4-6.8 (br), 2.5-5.5 (br, CH, CH 2 : Cellulose, overlapped with H 2 O), 0.8-1.7 (br, CH 3 : (1-a) or (1-b))
[0124] Example 9: The cellulose derivative obtained in Example 8 (14 in the following reaction formula (R8) (0.096 g, 0.20 mmol)) was placed in a two-necked recovery flask as the starting cellulose derivative. Tetrahydrofuran (0.86 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (2 in the following reaction formula (R8) (0.073 g, 0.30 mmol, 1.5 equivalents)) and cesium carbonate (0.20 g, 0.60 mmol, 3.0 equivalents) were added as the α-bromocarboxamide, and the mixture was stirred at room temperature (25°C) for 18 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) to reprecipitate the resulting solid. The resulting solid was collected by suction filtration and washed with diethyl ether. The resulting solid was dried in vacuo to obtain a cellulose derivative (0.044 g, yield: 34%) having a repeating unit represented by 15 in the following reaction formula (R8) as a pale orange solid.
[0125] 1 From the results of H-NMR measurement, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) of the obtained cellulose derivative was calculated to be about 3.0, and the total average degree of substitution was calculated to be about 3.0.
[0126] The cellulose derivative obtained in Example 9 1 The measured data of the H-NMR spectrum is shown in FIG. 3, and the chemical shift values are shown below. 1 H-NMR (500MHz, DMSO-d6, rt.): δ 9.6-10.4 (br, NH), 7.6 (br), 7.25 (br), 7.0 (br) 6.3-6.6 (br), 3.0-6.1 (br, CH, CH 2 : Cellulose, overlapped with H 2 O), 0.9-1.8 (br, CH 3 : (1-a) or (1-b))
[0127] Comparative Example 1 Trityl cellulose (4 in the following reaction formula (R9) , average degree of trityl group substitution: approximately 1.0, 0.315 g, 0.78 mmol) was placed in a two-necked recovery flask as a starting cellulose derivative, and pyridine (3.1 mL) was added under a nitrogen atmosphere and stirred to dissolve. 3-Phenylpropionic acid chloride (described in the following reaction formula (R9) , 0.58 mL, 3.90 mmol, 5 equivalents) was added and stirred at 80°C for 24 hours. The reaction solution was poured into methanol for reprecipitation, and the resulting solid was collected by suction filtration. The resulting solid was washed with methanol and dried in vacuo to obtain a 3-phenylpropanoyl cellulose derivative (0.493 g, yield: 94%) having a repeating unit represented by 16 in the following reaction formula (R9) as a pale orange solid.
[0128] 1 From the results of H-NMR measurement, it was calculated that the average degree of substitution of the trityl group in the obtained cellulose derivative was about 1.0, the average degree of substitution of the 3-phenylpropanoyl group was about 2.0, and the total average degree of substitution was about 3.0.
[0129] The cellulose derivative obtained in Comparative Example 1 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl 3 ,r. t. ): δ 6.2-7.8 (br, overlapped with CHCl 3 ), 1.7-5.4 (br, CH, CH 2 : Cellulose, CH 2 : 3-phenylpropanoyl)
[0130] The results of Examples 1 to 9 and Comparative Example 1 are shown in Table 1.
[0131]
[0132] From Table 1, it can be seen that aromatic amide-modified cellulose with a high degree of substitution could be obtained in good yield.
[0133] (Evaluation) The cellulose derivatives obtained in Example 3 and Example 24 below, and the 3-phenylpropanoyl cellulose derivative obtained in Comparative Example 1 were subjected to a hydrolysis reaction, and their alkali resistance was evaluated from the change in the average substitution degree of the substituents over time by the method described below.
[0134] The cellulose derivative obtained in Example 3 (0.071 g, 0.1 mmol), the cellulose derivative obtained in Example 24 below (0.070 g, 0.1 mmol), or the 3-phenylpropanoyl cellulose derivative obtained in Comparative Example 1 (0.067 g, 0.1 mmol) was placed in a two-necked recovery flask as the raw cellulose derivative, and tetrahydrofuran (1 mL) was added under a nitrogen atmosphere and stirred to dissolve. A 10 wt % aqueous sodium hydroxide solution (0.1 mL) was added and stirred at room temperature. After 24 hours, a saturated ammonium chloride solution was added to terminate the reaction. The target product was extracted from the aqueous layer with dichloromethane, dried over sodium sulfate, and the solvent was removed using an evaporator. The residue was vacuum dried, and 1 The degree of substitution was evaluated by H-NMR measurement, and the results are shown in Table 2.
[0135]
[0136] As shown in Table 2, the cellulose derivatives obtained in Examples 3 and 24 did not show a decrease in the average degree of substitution even when subjected to alkaline hydrolysis conditions, and it is clear that conversion into amide-modified cellulose improves alkali resistance.
[0137] Example 10: Cellulose acetate (1 in the following reaction formula (R10), product name "LL-10" (manufactured by Daicel Corporation), average degree of acetyl substitution of approximately 1.7, 0.100 g, 0.41 mmol) was placed in a two-necked flask as a starting cellulose derivative, and acetonitrile (1.6 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (2 in the following reaction formula (R10), 0.15 g, 0.61 mmol, 1.5 equivalents), tripotassium phosphate (0.26 g, 1.2 mmol, 3.0 equivalents), copper(I) iodide (1.6 mg, 8.6 μmol, 0.02 equivalents), and triphenylphosphine (3.3 mg, 13 μmol, 0.03 equivalents) were added as an α-bromocarboxamide, and the mixture was stirred at room temperature for 24 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) to reprecipitate the resulting solid, which was then collected by suction filtration. The obtained solid was washed with diethyl ether and dried in vacuum to obtain a cellulose derivative (0.111 g, yield: 70%) having a repeating unit represented by 17 in the following reaction formula (R10) as a pale orange solid.
[0138] 1 From the results of H-NMR measurement, the average degree of substitution of the acetyl group of the obtained cellulose derivative was calculated to be about 1.7, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) to be about 1.3, and the total average degree of substitution to be about 3.0.
[0139] The cellulose derivative obtained in Example 10 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl 3 ,r. t. ): δ 8.4-8.7(br), 7.6(br), 7.2-7.4(br, overlapped with CHCl 3 ), 6.3-6.9(br), 2.8-5.9(br, CH, CH 2 : cellulose), 1.8-2.2 (br, CH 3 : acetyl) 1.2-1.8 (br, CH 3 : (1-a) or (1-b))
[0140] Example 11 Cellulose acetate (1 in the following reaction formula (R10), trade name "FL-70" (manufactured by Daicel Corporation), average degree of acetyl substitution of approximately 2.1, 0.10 g, 0.40 mmol) was placed in a two-necked flask as a starting cellulose derivative, and tetrahydrofuran (1.6 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (2 in the following reaction formula (R10), 0.15 g, 0.60 mmol, 1.5 equivalents), tripotassium phosphate (0.25 g, 1.2 mmol, 3.0 equivalents), copper(I) iodide (1.6 mg, 8.4 μmol, 0.02 equivalents), and triphenylphosphine (3.2 mg, 12 μmol, 0.03 equivalents) were added as an α-bromocarboxamide, and the mixture was stirred at room temperature for 24 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) to reprecipitate the resulting solid, which was then collected by suction filtration. The obtained solid was washed with diethyl ether and dried in vacuo to obtain a cellulose derivative (0.148 g, yield: 84%) having a repeating unit represented by 17 in the following reaction formula (R10) as a pale orange solid.
[0141] 1 From the results of H-NMR measurement, the average degree of substitution of the acetyl group of the obtained cellulose derivative was calculated to be about 2.1, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) was about 0.9, and the total average degree of substitution was calculated to be about 3.0.
[0142] The cellulose derivative obtained in Example 11 1 The H-NMR spectrum data is shown in FIG. 4, and the chemical shift values are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 8.4-8.7(br), 7.6(br), 7.2-7.4(br, overlapped with CHCl 3 ), 6.3-6.9(br), 2.8-5.9(br, CH, CH 2 : cellulose), 1.8-2.2 (br, CH 3 : acetyl) 1.2-1.8 (br, CH 3 : (1-a) or (1-b))
[0143] Example 12: Trityl cellulose (4 in the following reaction formula (R11), average degree of trityl group substitution approximately 1.0, 0.100 g, 0.25 mmol) was placed in a two-necked flask as the starting cellulose derivative, and tetrahydrofuran (1.0 mL) was added under a nitrogen atmosphere and stirred to dissolve. α-Bromodimethylacetanilide (4 in the following reaction formula (R11), 0.18 g, 0.75 mmol, 1.5 equivalents), tripotassium phosphate (0.32 g, 1.5 mmol, 3.0 equivalents), copper(I) iodide (1.0 mg, 5.2 μmol, 0.01 equivalents), and triphenylphosphine (2.0 mg, 7.6 μmol, 0.015 equivalents) were added as the α-bromocarboxamide, and the mixture was stirred at room temperature for 24 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) and reprecipitated, resulting in a solid that was collected by suction filtration. The obtained solid was washed with diethyl ether and dried in vacuo to obtain a cellulose derivative (0.131 g, yield: 73%) having a repeating unit represented by 18 in the following reaction formula (R11) as a pale orange solid.
[0144] The cellulose derivative obtained in Example 12 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl3, rt.): δ 8.9-9.8 (br, NH), 6.8-8.0 (br, overlapped with CHCl 3 ), 6.3-6.8(br), 2.8-6.0(br, CH, CH 2 : cellulose), 0.7-1.8 (br, CH 3 : (1-a) or (1-b))
[0145] (Examples 13-14) The cellulose derivative of Example 13 (0.135 g, yield: 75%) and the cellulose derivative of Example 14 (0.140 g, yield: 77%) were obtained as pale orange solids in the same manner as in Example 12, except that the amount of copper iodide (I) was changed to (0.5 mg, 2.6 μmol, 0.005 equivalents) and the amount of triphenylphosphine was changed to (1.0 mg, 3.8 μmol, 0.0075 equivalents) (Example 13), and the amount of copper iodide (I) was changed to (2.4 mg, 12 μmol, 0.025 equivalents), and the amount of triphenylphosphine was changed to (4.9 mg, 19 μmol, 0.0375 equivalents) (Example 14).
[0146] The cellulose derivatives obtained in Examples 13 and 14 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl3, rt.): δ 8.9-9.8 (br, NH), 6.8-8.0 (br, overlapped with CHCl 3 ), 6.3-6.8(br), 2.8-6.0(br, CH, CH 2 : cellulose), 0.7-1.8 (br, CH 3 : (1-a) or (1-b))
[0147] Examples 15 and 16 Cellulose derivatives were obtained as pale orange solids in the same manner as in Example 12, except that the stirring time after addition of α-bromocarboxamide, the base catalyst, the copper compound, and the ligand was changed to 15 hours (Example 15) or 5 hours (Example 16). These were the cellulose derivative (1) of Example 15 (0.142 g, yield: 78%) and the cellulose derivative of Example 16 (0.134 g, yield: 74%).
[0148] The cellulose derivatives obtained in Examples 15 and 16 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl3, rt.): δ 8.9-9.8 (br, NH), 6.8-8.0 (br, overlapped with CHCl 3 ), 6.3-6.8(br), 2.8-6.0(br, CH, CH 2: cellulose), 0.7-1.8 (br, CH 3 : (1-a) or (1-b))
[0149] (Examples 17-19) Except for changing copper(I) iodide to copper(I) bromide (0.7 mg, 5 μmol, 0.01 equivalent) (Example 17), copper(I) chloride (0.5 mg, 5 μmol, 0.01 equivalent) (Example 18), or copper(II) chloride (0.7 mg, 5 μmol, 0.01 equivalent) (Example 19), the same procedure as in Example 12 was repeated to obtain cellulose derivatives having a repeating unit represented by 18 in the following reaction formula (R12) as pale orange solids. The cellulose derivatives were those of Example 17 (0.142 g, yield: 78%), Example 18 (0.136 g, yield: 75%), and Example 19 (0.107 g, yield: 89%). The reaction formula is as shown in the following reaction formula (R12).
[0150] The cellulose derivatives obtained in Examples 17 and 18 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl3, rt.): δ 8.9-9.8 (br, NH), 6.8-8.0 (br, overlapped with CHCl 3 ), 6.3-6.8(br), 2.8-6.0(br, CH, CH 2 : cellulose), 0.7-1.8 (br, CH 3 : (1-a) or (1-b))
[0151] The cellulose derivative obtained in Example 19 1 The chemical shift values of the H-NMR spectrum are shown below. 1 H-NMR (500MHz, CDCl3, rt.): δ 8.9-9.8 (br, NH), 6.8-8.0 (br, overlapped with CHCl 3 ), 6.3-6.8(br), 2.8-6.0(br, CH, CH 2 : cellulose), 0.7-1.8 (br, CH 3 : (1-a) or (1-b))
[0152] Example 20 A cellulose derivative (0.220 mg, yield: 100%) having a repeating unit represented by 20 of (R13) was obtained as a pale orange solid by the same procedure as in Example 12, except that α-bromodimethylaceto(3,4,5-trimethoxy)anilide (6 in the following reaction formula (R13), 0.25 g, 0.74 mmol, 1.5 equivalents) was used instead of α-bromodimethylacetanilide as the α-bromocarboxamide.
[0153] The chemical shift values of the cellulose derivative obtained in Example 20 are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 9.1-9.4 (br, NH), 8.4 (s), 6.6-7.8 (br, overlapped with CHCl 3 ), 6.8(s), 6.2-6.6(br), 2.3-5.0(br, CH, CH 2 : cellulose), 3.85 (s), 3.80 (s), 1.3-1.7 (br, CH 3 : (1-a) or (1-b))
[0154] Example 21 A cellulose derivative (0.156 g, yield: 73%) having a repeating unit represented by 21 of (R14) was obtained as a pale orange solid by the same procedure as in Example 12, except that α-bromodimethylaceto(4-trifluoromethyl)anilide (8 in the following reaction formula (R14) (0.23 g, 0.74 mmol, 1.5 equivalents) was used instead of α-bromodimethylacetanilide as the α-bromocarboxamide.
[0155] The chemical shift values of the cellulose derivative obtained in Example 21 are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 9.3-9.8 (br, NH), 6.8-8.2 (br, overlapped with CHCl 3 ), 6.2-6.6(br), 2.5-5.7(br, CH, CH 2 : cellulose), 0.7-2.3 (br, CH 3: (1-a) or (1-b))
[0156] Example 22 The same procedure as in Example 12 was carried out, except that 1-(α-bromodimethylacetoxy)aminopyrene (10 (0.27 g, 0.74 mmol, 1.5 equivalents) in reaction formula (R15) above) was used instead of α-bromodimethylacetanilide as the α-bromocarboxamide, to obtain a cellulose derivative (0.130 g, yield: 54%) having a repeating unit represented by 22 in (R15) as a pale orange solid.
[0157] The chemical shift values of the cellulose derivative obtained in Example 22 are shown below. 1 H-NMR (500MHz, CDCl 3 , r. t. ): δ 9.5-10.2 (br, NH), 7.6-8.4 (br), 6.6-7.6 (br, overlapped with CHCl 3 ), 2.5-5.0 (br, CH, CH 2 : cellulose), 0.8-2.0 (br, CH 3 : (1-a) or (1-b), overlapped with H 2 O)
[0158] 1 The average degrees of substitution of the trityl group and the group represented by formula (1-a) or (1-b) and the total average degree of substitution of the cellulose derivatives obtained in Examples 12 to 22, calculated from the results of H-NMR measurement, are shown in Table 3. Note that, by changing various reaction conditions, including the amount of copper compound, in Examples 21 and 22, various cellulose derivatives can be obtained in which the average degree of substitution of the trityl group is about 1.0 and the average degree of substitution of the group represented by formula (1-a) or (1-b) is about 1.0 to less than 2.0.
[0159] Example 23 The cellulose derivative obtained in Example 12 (18 in the following reaction formula (R16), 0.15 g, 0.20 mmol) was placed in a two-necked recovery flask as the starting cellulose derivative. Dichloromethane (1 mL) was added under a nitrogen atmosphere and the mixture was stirred to dissolve. A 30 wt % hydrogen bromide solution in acetic acid (0.4 mL, 2 mmol) was added and stirred at room temperature (25°C) for 5 minutes. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) to reprecipitate the resulting solid, which was collected by suction filtration and washed with ethanol. The resulting solid was dried in vacuo to obtain a cellulose derivative (0.083 g, yield: 83%) having a repeating unit represented by 23 in the following reaction formula (R16) as a pale orange solid.
[0160] 1 From the results of H-NMR measurement, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) of the obtained cellulose derivative was calculated to be about 2.0, and the total average degree of substitution was calculated to be about 2.0.
[0161] The cellulose derivative obtained in Example 23 1 The H-NMR measurement data is shown in FIG. 5, and the chemical shift values are shown below. 1 H-NMR (500MHz, DMSO-d6, rt.): δ 9.5-10.0 (br, NH), 7.6 (br), 7.25 (br), 7.0 (br) 6.4-6.8 (br), 2.5-5.5 (br, CH, CH 2 : Cellulose, overlapped with H 2 O), 0.8-1.7 (br, CH 3 : (1-a) or (1-b))
[0162] Example 24: The cellulose derivative obtained in Example 23 (23 in the following reaction formula (R17) (0.083 g, 0.17 mmol)) was placed in a two-necked eggplant flask as the raw cellulose derivative. Tetrahydrofuran (0.68 mL) was added under a nitrogen atmosphere and stirred to dissolve. As the α-bromocarboxamide, α-bromodimethylacetanilide (2 in the following reaction formula (R17) (0.062 g, 0.26 mmol, 1.5 equivalents), tripotassium phosphate (0.11 g, 0.51 mmol, 3.0 equivalents), copper(I) iodide (0.7 mg, 3.7 μmol, 0.02 equivalents), and triphenylphosphine (1.4 mg, 5.3 μmol, 0.03 equivalents) were added and stirred at room temperature (25°C) for 24 hours. The reaction solution was poured into an aqueous methanol solution (1 / 1, v / v) and reprecipitated. The resulting solid was collected by suction filtration and washed with diethyl ether. The obtained solid was dried in a vacuum to obtain a cellulose derivative (0.092 g, yield: 80%) having a repeating unit represented by 24 in the following reaction formula (R17) as a pale orange solid.
[0163] 1 From the results of H-NMR measurement, the average degree of substitution of the group represented by the above formula (1-a) or (1-b) of the obtained cellulose derivative was calculated to be about 3.0, and the total average degree of substitution was calculated to be about 3.0.
[0164] The cellulose derivative obtained in Example 24 1 The measured data of the H-NMR spectrum is shown in FIG. 6, and the chemical shift values are shown below. 1 H-NMR (500MHz, DMSO-d6, rt.): δ 9.6-10.4 (br, NH), 7.6 (br), 7.25 (br), 7.0 (br) 6.3-6.6 (br), 3.0-6.1 (br, CH, CH 2 : Cellulose, overlapped with H 2 O), 0.9-1.8 (br, CH 3 : (1-a) or (1-b))
[0165] The results of Examples 10 to 24 are shown in Table 3.
[0166]
[0167] From Table 3, it is clear that aromatic amide-modified cellulose having a high average substitution degree of the group represented by formula (1-a) or (1-b) could be obtained in good yield.
Claims
1. A cellulose derivative having a repeating unit represented by the following formula (1), in which the total average substitution degree of a hydroxyl-protecting group, a group represented by the following formula (1-a), and a group represented by the following formula (1-b) is 1.5 or more. [In the above formula (1), R may be the same or different and is a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the following formula (1-a), or a group represented by the following formula (1-b). Of all R contained in the cellulose derivative having a repeating unit represented by the above formula (1), at least one is a group represented by the following formula (1-a)] (In the above formula (1-a), X may be the same or different and represents a hydrogen atom or a methyl group. Also, in the above formula (1-a), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.) (In the above formula (1-b), X may be the same or different and represents a hydrogen atom or a methyl group. Also, in the above formula (1-b), Ar represents a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.) 2. The cellulose derivative according to claim 1, wherein in the above formula (1-a) or (1-b), Ar is a monocyclic aromatic hydrocarbon group.
3. The cellulose derivative according to claim 1, wherein in the above formula (1-a) or (1-b), Ar is a polycyclic aromatic hydrocarbon group.
4. The cellulose derivative according to claim 1, wherein the total average degree of substitution is 1.7 or more.
5. The cellulose derivative according to claim 1, wherein the protecting group for the hydroxyl group is an acetyl group or a trityl group.
6. The cellulose derivative according to claim 1, wherein at least one of all R contained in the cellulose derivative having a repeating unit represented by formula (1) is a group represented by formula (1-b).
7. A composition comprising the cellulose derivative according to any one of claims 1 to 6.
8. A method for producing the cellulose derivative according to claim 1, comprising step (i) of reacting, in the presence of a base catalyst, a hydroxyl group at the 2-, 3- or 6-position of a cellulose derivative having a repeating unit represented by the following formula (2): with an α-bromocarboxamide represented by the following formula (3): [In the above formula (2), R is the same or different and is a hydrogen atom, a protecting group for a hydroxyl group, a group represented by the above formula (1-a), or a group represented by the above formula (1-b). At least one of all R contained in the cellulose derivative having a repeating unit represented by the above formula (2) is a hydrogen atom.] [In the above formula (3), X is the same or different and represents a hydrogen atom or a methyl group. In addition, in the above formula (3), Ar is a monocyclic aromatic hydrocarbon group or a polycyclic aromatic hydrocarbon group.] 9. A method for producing a cellulose derivative according to claim 8, wherein at least one of all R contained in the cellulose derivative having a repeating unit represented by formula (2) is a hydroxyl-protecting group, a group represented by formula (1-a) or a group represented by formula (1-b), and the cellulose derivative having a repeating unit represented by formula (2) has a total average substitution degree of 1.5 or more for the hydroxyl-protecting group, the group represented by formula (1-a) and the group represented by formula (1-b).
10. The method for producing a cellulose derivative according to claim 8, wherein in the above formula (3), Ar is a monocyclic aromatic hydrocarbon group.
11. The method for producing a cellulose derivative according to claim 8, wherein in the above formula (3), Ar is a polycyclic aromatic hydrocarbon group.
12. A method for producing a cellulose derivative according to claim 8, wherein at least one of all R contained in the cellulose derivative having a repeating unit represented by formula (2) above is a protecting group for a hydroxyl group, and the method comprises, after step (i), step (ii) of removing the protecting group for the hydroxyl group and replacing it with a hydroxyl group.
13. The method for producing a cellulose derivative according to any one of claims 8 to 12, wherein the protecting group for the hydroxyl group is an acetyl group or a trityl group.
14. A method for producing a cellulose derivative according to claim 12, comprising a step (iii) of reacting the hydroxyl group at the 2-, 3- or 6-position, including the hydroxyl group substituted in step (ii), of the cellulose derivative obtained in step (ii) with the α-bromocarboxamide represented by formula (3) in the presence of a base catalyst.
15. The method for producing a cellulose derivative according to claim 8, wherein the reaction in step (i) is carried out in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst.
16. The method for producing a cellulose derivative according to claim 14, wherein the reaction in step (iii) is carried out in the presence of a copper compound, a copper ligand in the copper compound, and the base catalyst.
Citation Information
Patent Citations
Cellulose acylate
JP2002179701A
Mixed mode ligands
JP2013033040A
Modified wound dressings
JP2019509853A