Fluorine-containing amorphous carbon film and method for producing same

A single-layer fluorine-containing amorphous carbon film, produced using plasma CVD with optimized gas ratios and pressure, addresses the complexity of conventional display coatings by integrating hard coating, antireflection, and antifouling properties, offering a cost-effective and efficient solution for mobile displays.

WO2024232153A1PCT designated stage expired Publication Date: 2024-11-14KEIO UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008463
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-05-08
Filing Date
2024-03-06
Publication Date
2024-11-14

AI Technical Summary

Technical Problem

Conventional display devices require multiple thin films with different functions, leading to complex and expensive production processes, particularly for achieving hard coating, antireflection, and antifouling properties, as seen in existing antireflection films that necessitate separate layers or complicated composite film production methods.

Method used

A single-layer fluorine-containing amorphous carbon film is developed, composed of carbon, fluorine, and oxygen, with specific atomic content ratios, and a method using plasma CVD to form the film on a substrate with a raw material gas and inert gas, optimizing the gas flow rate ratio and pressure to achieve hard coating, antireflection, and antifouling properties in a single layer.

Benefits of technology

The fluorine-containing amorphous carbon film provides a cost-effective, single-layer solution with high hardness, low refractive index, and excellent water repellency, simplifying the production process while maintaining high light transmittance and antifouling properties, suitable for mobile displays.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008463_14112024_PF_FP_ABST
    Figure JP2024008463_14112024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a fluorine-containing amorphous carbon film which has characteristics of hard coating, antireflection, and antifouling; and a method for producing the same. This fluorine-containing amorphous carbon film is a monolayer film that is composed of carbon, fluorine, and oxygen. The average fluorine content in the film thickness direction is 30% by atom to 40% by atom inclusive, the average oxygen content in the film thickness direction is 5% by atom to 20% by atom inclusive, and the remainder is made up of carbon atoms. With respect to this fluorine-containing amorphous carbon film, a substrate is located in a chamber, and a starting material gas which is represented by a chemical formula that is composed only of carbon and fluorine, and an inert gas for diluting the starting material gas are introduced into the chamber, so that a fluorine-containing amorphous carbon film is formed on the substrate under plasma generation. The mixing ratio of the inert gas into the starting material gas is set to be larger than 1 / 4 but smaller than 11 / 1 in terms of the flow rate ratio into the chamber.
Need to check novelty before this filing date? Find Prior Art

Description

Fluorine-containing amorphous carbon film and method for producing the same

[0001] The present invention relates to a fluorine-containing amorphous carbon film and a method for producing the same, and more particularly to a fluorine-containing amorphous carbon film that provides a hard coating with a low refractive index and excellent water repellency, and a method for producing the same.

[0002] In portable display devices such as smartphones and tablet terminals, multiple functional layers are laminated on the surface of a glass substrate, which serves as the display base. For example, a hard coat layer to prevent scratches and damage, an anti-reflection layer to reduce light reflection, and an anti-fouling layer to prevent dirt and fingerprints from adhering are provided. A coating liquid using a fluorine-containing alkoxysilane has been proposed to form an anti-reflection film with a low refractive index (see, for example, Patent Document 1). Furthermore, an anti-reflection film with scratch resistance and anti-fouling properties has been proposed, which is formed by laminating a hard coat layer and a low refractive index layer containing hollow inorganic nanoparticles (see, for example, Patent Document 2).

[0003] JP 2015-224302 A JP 2021-76849 A

[0004] Conventional display devices are coated with multiple thin films with different functions, such as anti-reflection layers and anti-fouling layers, making their production process complicated and costly. When using the low-refractive-index anti-reflection film proposed in Patent Document 1, a hard coating layer and an anti-fouling layer are required separately. The anti-reflection film proposed in Patent Document 2 is a composite film of a hard coating layer and a low-refractive-index layer, and its production process is complicated and costly.

[0005] In view of the above problems, an object of the present invention is to provide a fluorine-containing amorphous carbon film having hard coat, anti-reflection, and anti-fouling properties, and a method for producing the same.

[0006] In one aspect of the present invention, the fluorine-containing amorphous carbon film is a single layer film composed of carbon, fluorine, and oxygen, in which the average fluorine content in the film thickness direction is 30 atomic % or more and 40 atomic % or less, the average oxygen content in the film thickness direction is 5 atomic % or more and 20 atomic % or less, and the remainder is carbon atoms.

[0007] In another aspect of the present invention, a method for producing a fluorine-containing amorphous carbon film includes placing a substrate in a chamber; introducing a source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas into the chamber; and forming a fluorine-containing amorphous carbon film on a surface of the substrate under plasma generation; and setting a mixture ratio of the inert gas to the source gas in terms of a flow rate into the chamber to be greater than 1 / 4 and less than 11 / 1.

[0008] A fluorine-containing amorphous carbon film having hard coat, anti-reflection, and anti-fouling properties and a method for producing the same are realized.

[0009] 1 is a schematic diagram of a fluorine-containing amorphous carbon film according to an embodiment formed on a substrate; FIG. 2 is a schematic diagram of a film formation apparatus used to form a fluorine-containing amorphous carbon film; FIG. 3 is a diagram showing the relationship between gas flow rate ratio and light transmittance in Example 1; FIG. 4 is a diagram showing the relationship between gas flow rate ratio and extinction coefficient in Example 1; FIG. 5 is a diagram showing the relationship between gas flow rate ratio and refractive index in Example 1; FIG. 6 is a diagram showing the relationship between gas flow rate ratio and water droplet contact angle in Example 1; FIG. 7 is a diagram showing the relationship between film formation pressure and light transmittance in Example 2; FIG. 8 is a diagram showing the elemental content of films formed at different pressures in Example 2; FIG. 9 is a diagram showing the relationship between film formation pressure and refractive index in Example 2; FIG. 10 is a diagram showing the relationship between film formation pressure and water droplet contact angle in Example 2; FIG. 11 is a diagram showing the elemental content when the gas flow rate ratio is changed in Example 3; FIG. 12 is a diagram showing the relationship between gas flow rate ratio and refractive index in Example 3; FIG. 13 is a diagram showing the relationship between gas flow rate ratio and light transmittance in Example 3; FIG. 14 is a diagram showing the relationship between gas flow rate ratio and water droplet contact angle in Example 3; FIG. 15 is a diagram showing the relationship between gas flow rate ratio and film formation rate.

[0010] The fluorine-containing amorphous carbon film and its manufacturing method of the present invention will be described in detail below with reference to the drawings. The following embodiments are examples for embodying the technical concept of the invention, and the present invention is not limited to the described configurations and numerical values. In the drawings, components having the same function are given the same reference numerals, and redundant description may be omitted. Partial substitution or combination between different embodiments and configuration examples is possible. The size, positional relationship, etc. of each component shown in each drawing may be exaggerated to facilitate understanding of the invention.

[0011] <Configuration of Fluorine-Containing Amorphous Carbon Film> Fig. 1 is a schematic diagram of a fluorine-containing amorphous carbon film 10 according to an embodiment formed on the surface of a substrate 11 serving as a base material. The fluorine-containing amorphous carbon film 10 is a single-layer thin film formed in a single film formation process. The thickness of the fluorine-containing amorphous carbon film 10 can be appropriately designed depending on the member to which the fluorine-containing amorphous carbon film 10 is applied, and is, for example, 25 nm to 500 nm, preferably 50 nm to 250 nm. The fluorine-containing amorphous carbon film 10 has a different fluorine content between the surface region and a region 12 deeper on the substrate 11 side. Near the surface of the fluorine-containing amorphous carbon film 10, specifically a region shallower than 10 nm from the surface, is a high-fluorine-concentration region 13 having a higher fluorine content than the region 12 deeper than 10 nm.

[0012] The fluorine-containing amorphous carbon film 10 is a single layer film made of carbon, fluorine, and oxygen. In the embodiments and claims, when the fluorine-containing amorphous carbon film 10 is expressed as a film "made of carbon, fluorine, and oxygen" or a film "composed of carbon, fluorine, and oxygen," this means that trace amounts of impurities that are inevitably or unintentionally mixed in are not considered as constituent elements.

[0013] The fluorine-containing amorphous carbon film 10 has an average fluorine content in the thickness direction of 30 atomic % to 40 atomic %, an average oxygen content in the thickness direction of 5 atomic % to 20 atomic %, and the remainder being carbon atoms. In the high-concentration fluorine-containing region 13 at the surface, the fluorine content is 50 atomic % to 75 atomic %, an oxygen content is 5 atomic % to 20 atomic %, and the remainder being carbon atoms. In the composition of the region 12 at a depth of 10 nm or more from the surface, the fluorine content is 30 atomic % to 40 atomic %, an oxygen content is 5 atomic % to 20 atomic %, and the remainder is carbon atoms. The average content of each element in the thickness direction is dominated by the composition of the region 12 at a depth of 10 nm or more from the surface.

[0014] The fluorine-containing amorphous carbon film 10 is a highly hard film with a low refractive index and excellent water repellency, and a single layer combines hard coating, anti-reflection, and anti-fouling functions. The fluorine-containing amorphous carbon film 10 is applied to the surface of glass substrates such as displays and transparent panels. Hard coating properties are properties that prevent scratches and cracks from occurring on the glass substrate when subjected to external impact, and include abrasion resistance and scratch resistance. To be called a hard coating, the film itself must not only be able to prevent scratches and cracks, but also have high hardness to protect the substrate. The substrate is formed from a glass material such as quartz glass, soda-lime glass, sapphire glass, or optical glass. To protect the substrate, the fluorine-containing amorphous carbon film 10 preferably has a hardness of 0.65 GPa or more as measured by nanoindentation. When applied to display terminals and transparent panels, high light transmittance is also required. As will be described later, the light transmittance of the fluorine-containing amorphous carbon film 10 of this embodiment is 90%, preferably 95% or more, and more preferably 98% or more.

[0015] Anti-reflection properties refer to the ability to reduce light reflection by utilizing optical interference. When the fluorine-containing amorphous carbon film 10 is applied to a display, it reduces light reflection on the display surface, improving visibility. To achieve this, it is required that the film have a low refractive index relative to the underlying substrate. Even at its highest refractive index, the fluorine-containing amorphous carbon film 10 has a refractive index of 1.40±0.02, which is lower than the refractive index of quartz glass (1.50). When formed under favorable conditions, the refractive index can be reduced to 1.32, providing a high anti-reflection function.

[0016] Antifouling properties refer to the property of being resistant to dirt. When applied to a display, the outermost surface of the display is required to have a low surface free energy or a large contact angle with water (high water repellency) to prevent dirt and fingerprints from adhering thereto. The fluorine-containing amorphous carbon film 10 has a large water droplet contact angle of 95° or more, and is therefore highly water repellent. The basis for this will be described later.

[0017] 2 is a schematic diagram of a film formation apparatus 100 used to produce a fluorine-containing amorphous carbon film 10. The fluorine-containing amorphous carbon film 10 is formed using a source gas whose chemical formula is represented only by carbon (C) and fluorine (F) and an inert gas. That is, a mixed gas of a fluorocarbon gas that does not contain hydrogen atoms and an inert gas is used.

[0018] The film formation apparatus 100 is a CVD (Chemical Vapor Deposition) film formation apparatus. CVD has a high film formation rate, a large processing area, and can form a high-density film compared to vacuum deposition. In this example, the film formation apparatus 100 is a capacitively coupled high-frequency plasma CVD apparatus, and has a pair of parallel plate electrodes 101 and 102 in a chamber 104. The chamber 104 is configured so that a substrate 11 can be placed between the electrodes 101 and 102; for example, the substrate 11 can be placed on the lower electrode 101.

[0019] During film formation, the chamber 104 is maintained at a medium or high vacuum of 24 Pa or less. One electrode 101 is connected to a high-frequency power supply 103, and the other electrode 102 is grounded. High-frequency power is applied between the electrodes 101 and 102 to generate plasma. Frequencies used to excite low-temperature plasma include the HF band (3-30 MHz), VHF band (30-300 MHz), and UHF band (300-3000 MHz). In this embodiment, a power supply frequency of 13.56 MHz, which is common in plasma excitation processes, is used. A source gas and an inert gas that dilutes the source gas are introduced into the chamber 104 through the gas inlet Pin, generating a gas plasma within the chamber 104. The plasma within the chamber 104 decomposes the source gas molecules, and the chemical species generated by the decomposition are deposited on the substrate 11. Unnecessary gases are exhausted through the exhaust port Pout.

[0020] As the raw material gas, tetrafluoromethane (CF 4 ), hexafluoroethane (C 2 F 6 ), octafluoropropane (C 3 F 8 ), octafluorocyclobutane (C 4 F 8) can be used. The inert gas for dilution is argon (Ar), nitrogen (N), krypton (Kr), xenon (Xe), etc. By using a fluorocarbon gas that does not contain hydrogen atoms as the source gas, it is possible to eliminate C-H bonds that tend to increase the refractive index due to polarization.

[0021] The method for producing a fluorine-containing amorphous carbon film includes the steps of: a) placing a substrate 11 in a chamber 104 of a film formation apparatus 100; b) introducing a source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas into the chamber 104, and forming a fluorine-containing amorphous carbon film on the surface of the substrate 11 under plasma generation; and c) setting the mixture ratio of the inert gas to the source gas, in terms of the flow rate ratio into the chamber 104, to be greater than 1 / 4 and less than 11 / 1. More preferably, the flow rate ratio of the inert gas to the source gas into the chamber 104 is greater than 1 / 2 and less than 7 / 2. The basis for the preferred range of the mixture ratio of the inert gas to the source gas will be described later.

[0022] <Characteristics Evaluation> In the following, a plurality of types of samples are produced by changing the film formation conditions of the fluorine-containing amorphous carbon film 10, and the characteristics are evaluated.

[0023] Example 1: SiO as the substrate 11 2 The substrate is SiO 2 A substrate is placed on the electrode 101, and a high frequency power of 13.56 MHz and 200 W is applied to the film forming apparatus 100 to excite low-temperature plasma. The pressure inside the chamber 104 before plasma ignition is set to 24 Pa, and Ar gas and C 4 F 8 Gas is introduced. 4 F 8 The ratio of the flow rate of Ar gas to the flow rate of Ar gas (Ar / C 4 F 8) is changed to 1 / 4, 1 / 2, and 1 / 1. High-frequency power is applied to generate plasma, and three types of samples are fabricated by depositing films at each flow rate ratio to final film thicknesses of 50 nm, 100 nm, and 150 nm. Using the fabricated samples, the film thickness, element content, light transmittance, extinction coefficient, refractive index, water droplet contact angle, and hardness are measured. The film thickness is determined by fitting the measurement data after creating a structural model of the thin film using spectroscopic ellipsometry, which is used to measure the extinction coefficient and refractive index, as described below.

[0024] (1) Element content Ar / C 4 F 8 The elemental content is measured using a sample with a film thickness of 150 nm, which was fabricated with a flow rate ratio set to 1 / 4 and 1 / 1, respectively. The elemental proportions on the sample surface and inside the film, which was etched with Ar at an acceleration energy of 700 kV, are measured using X-ray photoelectron spectroscopy (XPS). The depths measured inside the film are 10 nm and 30 nm from the surface. The XPS device used is a JPS-9010TR manufactured by JEOL Ltd. The depth resolution for measurements on the film surface and inside the film is approximately 5 nm. Since the elemental proportions inside the film were the same at depths of 10 nm and 30 nm, these are collectively referred to as the elemental proportions inside the film.

[0025] Specifically, Ar / C 4 F 8 For the sample with a flow rate ratio of 1 / 4, the elemental ratios on the film surface were F content 50 atomic %, C content 38 atomic %, and O content 12 atomic %, and the elemental ratios inside the film were F content 32 atomic %, C content 58 atomic %, and O content 10 atomic %.

[0026] On the other hand, Ar / C 4 F 8 In the sample with a flow rate ratio of 1 / 1, the elemental ratios on the film surface were: F content 73 atomic %, C content 23 atomic %, O content 4 atomic %, and the elemental ratios inside the film were: F content 38 atomic %, C content 54 atomic %, O content 8 atomic %. Ar / C 4 F 8By changing the flow rate ratio to 1 / 1, the F content on the film surface increased to 73 atomic %. The F content also increased inside the film, although not as much as on the film surface. 4 F 8 It is understood that the flow rate ratio affects the element profile in the film thickness direction of the fluorine-containing amorphous carbon film 10 .

[0027] (2) Light Transmittance Figure 3 shows the light transmittance characteristics of samples fabricated with different film thicknesses and gas flow ratios. The light transmittance of samples fabricated with film thicknesses set to 50 nm, 100 nm, and 150 nm for each of the three gas flow ratios described above was measured using an ultraviolet-visible spectrometer (Shimadzu UV-Vis 3600 Plus). The gray circles indicate Ar / C 4 F 8 Light transmittance of the sample with a flow rate ratio of 1 / 1. The gray squares indicate Ar / C. 4 F 8 Light transmittance of the sample with a flow rate ratio of 1 / 2, and the open triangles indicate Ar / C 4 F 8 The light transmittance of the sample with a flow rate ratio of 1 / 4 is shown. The slight variation in film thickness among samples is due to process variations. Regardless of the gas flow rate ratio, high light transmittance was achieved in all samples. Even at a film thickness of 150 nm, a light transmittance of over 90% was obtained, making it highly practical as a protective film for displays. When the film thickness is 100 nm or less, the light transmittance is 94% or more, and at a film thickness of 50 nm, the light transmittance is 97% or more. Ar / C 4 F 8 Even when the flow rate ratio is 1 / 4, the optical transmittance is high enough to be applicable to displays.

[0028] (3) Extinction Coefficient Figure 4 shows the light absorption characteristics of samples fabricated with different gas flow ratios. Sample A corresponds to the sample shown with gray squares in Figure 3, where the film thickness dependency of the transmission characteristics is indicated. Sample B corresponds to the sample shown with gray circles in Figure 3, where the film thickness dependency of the transmission characteristics is indicated. Sample C corresponds to the sample shown with white triangles in Figure 3, where the film thickness dependency of the transmission characteristics is indicated. The horizontal axis represents wavelength, and the vertical axis represents extinction coefficient. The extinction coefficient, along with the refractive index (described later), is measured by spectroscopic ellipsometry using an Accurion Imaging Ellipsometer EP4. The extinction coefficient represents the degree of light absorption. All samples have a small extinction coefficient of 0.025 or less at a wavelength of 350 nm, and there is almost no light absorption for visible light. In particular, the Ar / C 4 F 8 When the flow rate ratio is 1 / 2, the extinction coefficient becomes 0.010 or less. 4 F 8 Even when the flow rate ratio is 1 / 4, the extinction characteristics are sufficient for use in displays.

[0029] (4) Refractive Index Figure 5 shows the refractive index at a wavelength of 550 nm of samples fabricated with different gas flow ratios. 4 F 8 The refractive index of the sample with a flow rate ratio of 1 / 2 is 1.40, Ar / C 4 F 8 The refractive index of the sample with a flow rate ratio of 1 / 1 is 1.39. 4 F 8 The refractive index of the sample with a flow ratio of 1 / 4 is 1.46. 4 F 8 The sample with a flow rate ratio of 1 / 4 has good light transmittance and extinction coefficient, but the refractive index cannot be sufficiently reduced, making it difficult to apply in situations where anti-reflection function is a priority.

[0030] (5) Water Droplet Contact Angle Figure 6 shows the water drop contact angle of samples prepared at different gas flow ratios. The water drop contact angle of each sample was measured by the sessile drop method using a DM-500 manufactured by Kyowa Interface Science Co., Ltd. 4 F 8 The water droplet contact angle of the sample with a flow rate ratio of 1 / 2 is 95°, and Ar / C 4 F8 The water droplet contact angle of the sample with a flow rate ratio of 1 / 4 is 92.5°. Both samples have a sufficient water droplet contact angle and have a high antifouling effect. For reference, the Ar ratio was further increased to Ar / C 4 F 8 The sample prepared with a flow rate ratio of 2 / 1 had a water droplet contact angle of 101.7°, which indicates high water repellency. 4 F 8 The flow rate ratio is 1 / 4 or more, preferably 1 / 2 or more.

[0031] (6) Hardness The hardness of each sample is measured by nanoindentation. When measuring by nanoindentation, the film thickness is preferably 250 nm or more, so the hardness is measured using a sample with a film thickness of 250 nm. The measurement is performed using a Nano Indenter G200 manufactured by Toyo Corporation. Ar / C 4 F 8 The hardness of the sample with a flow rate ratio of 1 / 2 is 0.76 GPa, Ar / C 4 F 8 The hardness of the sample with a flow ratio of 1 / 1 is 0.65 GPa. 4 F 8 The hardness of the sample with a flow rate ratio of 1 / 4 is 0.48 GPa, which is slightly insufficient compared to the other samples.

[0032] In Example 1, according to the above characteristic evaluation, in order to satisfy all the requirements for hard coating, anti-reflection, and anti-fouling, the flow rate ratio of the raw material gas (fluorocarbon gas) to the inert gas is preferably greater than 1 / 4, and more preferably greater than 1 / 2.

[0033] Example 2 In Example 2, Ar / C 4 F 8 A plurality of types of samples are fabricated by changing the film formation pressure while fixing the flow rate ratio. The same high-frequency plasma CVD film formation apparatus 100 as in Example 1 is used. The inert gas is Ar, the source gas is C 4 F 8Under reduced pressure, a high frequency power of 13.56 MHz and 200 W is applied to the electrode 101 to excite plasma between the electrode 102 and the opposing electrode 102, and a fluorine-containing amorphous carbon film 10 is formed on a quartz glass substrate 11 placed on the electrode 101. 4 F 8 The flow rate ratio was set to 1 / 2, and the film formation pressure was changed to 12 Pa, 24 Pa, and 48 Pa. For the samples fabricated at each film formation pressure, the film thickness, light transmittance, element content inside the film, refractive index, and water droplet contact angle were measured.

[0034] 7 shows the relationship between film formation pressure and light transmittance. The film formation pressure is shown as the combined pressure of the gas pressures in the chamber 104 during film formation. When the film formation pressure is 12 Pa and 24 Pa, a light transmittance of 90% or more is obtained, but when the film formation pressure is 36 Pa, the light transmittance drops to less than 85%. Therefore, it is preferable to set the film formation pressure to less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less.

[0035] Figure 8 shows the elemental content of films deposited at different pressures. The elemental content was measured at a depth of 20 nm from the film surface by etching and XPS. While no significant difference in carbon (C) content was observed, the fluorine (F) content was 45 atomic % at deposition pressures of 12 Pa and 24 Pa, but was 40 atomic % at a deposition pressure of 36 Pa, resulting in a corresponding increase in oxygen (O) content. To increase the fluorine content and lower the refractive index while ensuring hardness and transparency, it is desirable for the deposition pressure to be less than 36 Pa, e.g., 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less.

[0036] 9 shows the relationship between the film formation pressure and the refractive index. When the film formation pressure is 24 Pa, a refractive index of 1.38 is obtained, and when the film formation pressure is 12 Pa, a refractive index lower than 1.36 is realized. When the film formation pressure is 36 Pa, the refractive index becomes 1.40. Although a film with a refractive index of 1.40 can be used as an anti-reflective film, taking into consideration hardness and transparency, it is clear that the film formation pressure is preferably less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less.

[0037] Figure 10 shows the relationship between the film formation pressure and the water droplet contact angle. A contact angle of nearly 95° was obtained at film formation pressures of 24 Pa and 36 Pa, and a contact angle of over 100° was obtained at 12 Pa. Even at a pressure of 36 Pa, a fluorine-containing amorphous carbon film with antifouling properties was obtained.

[0038] From the results of Example 2, it was confirmed that in order to provide all the functions of hard coating, anti-reflection, and anti-fouling, the film formation pressure should be less than 36 Pa, for example, 35 Pa or less, preferably 30 Pa or less, and more preferably 24 Pa or less. On the other hand, since the film formation rate also decreases as the film formation pressure decreases (1 nm / s at a film formation pressure of 24 Pa, 0.5 nm / s at 12 Pa), in order to achieve a film formation rate suitable for practical use at an industrial level, the film formation pressure is preferably 6 Pa or more.

[0039] In Example 3, the film formation pressure is fixed, and the ratio of the inert gas to the source gas is changed in the direction of increasing, and the composition and characteristics are evaluated. A quartz glass substrate 11 is placed in the same film formation apparatus 100 as in Examples 1 and 2, and the film formation pressure is fixed at 24 Pa. The inert gas is Ar gas, and the source gas is C 4 F 8 Gas: Ar / C 4 F 8 The flow rate ratio was changed to 1 / 2, 3 / 2, 5 / 2, and 7 / 2 to prepare samples with a film thickness of 250 nm, and the element content, refractive index, light transmittance, and water droplet contact angle were measured using the same measurement methods as in Examples 1 and 2.

[0040] (1) Element Content Figure 11 shows the element content in the film when the gas flow ratio is changed in Example 3. Etching is performed by accelerating Ar ions at 700 kV, and the element content in the thin film is measured by XPS using a JPS-9010TR manufactured by JEOL Ltd. The XPS measurement is performed at each depth, with the surface layer being defined as the area from the surface to a depth of 5 nm, the intermediate layer being defined as the area from 80 to 160 nm, and the area near the substrate being defined as the area to a depth of 240 nm. In the surface layer up to a depth of 5 nm, the Ar / C 4 F 8 The higher the flow rate ratio, the higher the fluorine (F) content, which is 61 atomic % or more in all cases. 4 F 8When the flow rate ratio is 1 / 2, 3 / 2, or 5 / 2, the F content is stable at 40 atomic %, but when the flow rate ratio is increased to 7 / , the F content increases to 43 atomic %. Even near the substrate, the F content is stable at nearly 40 atomic %, except for the flow rate ratio of 3 / 2, and even at the flow rate ratio of 3 / 2, the F content is 30 atomic % or more. This result is consistent with the result of Example 1. On the other hand, the C element content is higher in the intermediate layer and near the substrate than in the surface layer. There is no significant change in the O element content in the film thickness direction, and the Ar / C 4 F 8 It is not significantly affected by changes in the flow rate.

[0041] (2) Refractive index Figure 12 shows the Ar / C 4 F 8 The relationship between the flow rate ratio and the refractive index is shown. The refractive index at a wavelength of 500 nm is measured for each sample prepared in Example 3 by spectroscopic ellipsometry. 4 F 8 The higher the flow rate ratio, the lower the refractive index. At a flow rate ratio of 7 / 2, the refractive index values ​​are distributed in the range of 1.32 to 1.36, with a median value of 1.34. A stable refractive index of 1.32 is expected to be obtained by reducing the deposition pressure and increasing the gas flow rate ratio. Fluorine-containing amorphous carbon films are effectively used as anti-reflective coatings.

[0042] (3) Light transmittance Figure 13 shows the Ar / C 4 F 8 The relationship between the flow rate ratio and light transmittance is shown. Each sample prepared in Example 3 is measured using ultraviolet-visible spectroscopy. For reference, light with a wavelength of 400 nm to 800 nm is transmitted through a sample of a quartz glass substrate 11 with no film formed on its surface, and the transmittance is measured. D "No film" is the transmission spectrum of a quartz glass substrate 11 with no film formed on its surface. E, F, G, and H are Ar / C 4 F 8 The flow rate ratios are 1 / 2, 3 / 2, 5 / 2, and 7 / 2, respectively. All samples have a transmittance of 90% or more in the visible light region, showing high light transmittance.

[0043] (4) Water droplet contact angle Figure 14 shows the Ar / C 4 F 8The relationship between the flow rate ratio and the water droplet contact angle is shown. The water droplet contact angle is measured by the sessile drop method for each sample produced in Example 3. For reference, the water droplet contact angle is measured for a quartz glass substrate with no film formed on its surface. For all samples, the water droplet contact angle is 90° or more. Increasing the Ar gas ratio increases the water droplet contact angle. The water droplet contact angle is 94.6° when the flow rate ratio is 1 / 2, and 100.3° when the flow rate ratio is 7 / 2. For quartz glass with no film formed on its surface, the water droplet contact angle does not even reach 60°, demonstrating that the fluorine-containing amorphous carbon film of Example 3 has a high antifouling effect.

[0044] Based on the measurements and evaluations of Examples 1 to 3, the fluorine-containing amorphous carbon film 10 of the embodiment is characterized in that the fluorine content in a region shallower than 10 nm from the surface is higher than that in a region 12 at a depth of 10 nm or more. The abundance of CF bonds in the surface layer suppresses polarization, reducing interactions such as reverse polarization induced by light or electromagnetic waves, facilitating light transmission and resulting in low refractive index. The fluorine content inside the film is also 40 atomic % on average, suppressing polarization inside the film and resulting in an extremely low refractive index. Thus, the fluorine-containing amorphous carbon film 10 of the embodiment has an amorphous carbon fluoride film with a high fluorine content formed near the surface, and also has a high fluorine content inside and does not contain hydrogen, resulting in extremely excellent optical properties.

[0045] In the above example, C was used as the source gas. 4 F 8 I used CF 4 , C 2 F 6 , C 3 F 8 Alternatively, a fluorocarbon gas such as CF 4 , C 2 F 6 , C 3 F 8 , C 4 F 8A mixed gas of two or more gases selected from the group consisting of Ar, Ar-, Ar-, and CF- may be used. Plasma excitation of Ar gas promotes decomposition of fluorocarbon molecules, promoting radicalization and ionization of C, F, and CF groups. In particular, when the flow rate of Ar gas is 50% or more of the flow rate of the fluorocarbon-based raw material gas, decomposition and activation of the fluorocarbon-based gas are promoted, resulting in a high fluorine content in the film.

[0046] Fluorocarbon gases are dissociated by Ar plasma to produce amorphous CF films. However, Ar ions also have an etching effect. When the Ar gas flow rate is four times or more that of the fluorocarbon source gas, the etching effect becomes greater, resulting in a decrease in the deposition rate. Figure 15 shows the relationship between each flow rate ratio and deposition rate at a deposition pressure of 24 Pa. The deposition rate decreases as the Ar ratio increases. However, extrapolating the bar graph in Figure 15, it is possible to increase the Ar gas flow rate until the deposition rate drops to 0.1 nm / s, which is considered unsuitable for industrial use, and further improvement in optical properties can be expected. In this case, the Ar gas flow rate ratio to the source gas can be increased to 11 / 1. From the above, it is preferable that the Ar gas flow rate ratio to the source gas be greater than 1 / 4 and less than or equal to 11 / 1.

[0047] On the other hand, the moment plasma excitation is stopped, the etching effect of Ar ions decreases, and activated CF radicals and CF ions accumulate near the surface to a thickness of several nanometers, forming an amorphous CF film with a high fluorine content. The higher the surface fluorine content, the lower the surface reflectance due to weak polarization of F atoms, and the better the optical properties, such as increased light transmittance and a lower refractive index. In addition, the surface free energy decreases, increasing water repellency and improving antifouling properties.

[0048] In conclusion, the fluorine-containing amorphous carbon film 10 of the embodiment is a single layer film made of carbon, fluorine, and oxygen, and has an average fluorine content of 30 atomic % to 40 atomic % in the thickness direction, an average oxygen content of 5 atomic % to 20 atomic % in the thickness direction, and the remainder being carbon atoms. On the other hand, a region shallower than 10 nm deep from the surface becomes a high-concentration fluorine-containing region 13, and has a fluorine content of 50 atomic % to 75 atomic % in the thickness direction, an oxygen content of 5 atomic % to 20 atomic % in the thickness direction, and the remainder being carbon atoms.

[0049] The fluorine-containing amorphous carbon film 10 of the embodiment is a thin film with excellent optical properties (low reflectance, high light transmittance, low refractive index) and excellent antifouling properties, and is highly hard, making it suitable as a protective coating for portable displays such as smartphones. Furthermore, it can be formed at low cost in a short time using low-pressure plasma CVD. The fluorine-containing amorphous carbon film 10 can be formed at low cost through a single film formation process, which is cost-effective. Using a source gas whose chemical formula is represented only by carbon and fluorine, a thin film with excellent optical properties and antifouling properties can be produced at low cost, making it suitable for mass production of protective films for displays and transparent panels.

[0050] The above disclosure includes the following aspects: (Item 1) A fluorine-containing amorphous carbon film configured as a single layer film composed of carbon, fluorine, and oxygen, having an average fluorine content in the film thickness direction of 30 atomic % to 40 atomic %, an average oxygen content in the film thickness direction of 5 atomic % to 20 atomic %, and the remainder being carbon atoms. (Item 2) The fluorine-containing amorphous carbon film according to Item 1, having a high-concentration fluorine-containing region in a region shallower than 10 nm deep from the surface, the fluorine content being higher than that in a region 10 nm deep or more, and the fluorine content in the high-concentration fluorine-containing region being 50 atomic % to 75 atomic %, an oxygen content being 5 atomic % to 20 atomic %, and the remainder being carbon atoms. (Item 3) The fluorine-containing amorphous carbon film according to Item 1 or 2, wherein the refractive index of the single layer film is 1.32 or more but less than 1.40. (Item 4) The fluorine-containing amorphous carbon film according to any one of Items 1 to 3, wherein the monolayer film has a light transmittance of 90% or more. (Item 5) The fluorine-containing amorphous carbon film according to any one of Items 1 to 4, wherein the monolayer film has a water droplet contact angle of 90° or more. (Item 6) The fluorine-containing amorphous carbon film according to any one of Items 1 to 5, wherein the monolayer film has a hardness of 0.65 GPa or more as measured by a nanoindentation method. (Item 7) The fluorine-containing amorphous carbon film according to any one of Items 1 to 6, wherein the monolayer film has a thickness of 25 nm or more and 500 nm or less. (Item 8) The fluorine-containing amorphous carbon film according to Item 7, wherein the monolayer film has a thickness of 50 nm or more and 250 nm or less. (Item 9) A method for producing a fluorine-containing amorphous carbon film, comprising: placing a substrate in a chamber; introducing a source gas whose chemical formula is represented only by carbon and fluorine and an inert gas that dilutes the source gas into the chamber; and forming a fluorine-containing amorphous carbon film on the surface of the substrate under plasma generation; and setting a mixture ratio of the inert gas to the source gas in terms of a flow rate into the chamber greater than 1 / 4 and less than 11 / 1. (Item 10) A method for producing a fluorine-containing amorphous carbon film according to Item 9, wherein a mixture ratio of the inert gas to the source gas in terms of a flow rate into the chamber is set to 1 / 2 or more and 7 / 2 or less. (Item 11) A method for producing a fluorine-containing amorphous carbon film according to Item 9 or 10, wherein a pressure inside the chamber is set to 24 Pa or less.(Item 12) The source gas is CF. 4 , C 2 F 6 , C 3 F 8 , C 4 F 8 11. The method for producing a fluorine-containing amorphous carbon film according to any one of Items 9 to 10, wherein the inert gas is Ar gas, or a mixed gas of two or more gases selected from these.

[0051] This application claims priority based on Japanese Patent Application No. 2023-076611, filed on May 8, 2023, and includes the entire contents of this Japanese patent application.

[0052] REFERENCE SIGNS LIST 10 Fluorine-containing amorphous carbon film 11 Substrate 12 Region 13 High-concentration fluorine-containing region 100 Film-forming apparatus 104 Chamber

Claims

1. A fluorine-containing amorphous carbon film, which is configured as a single layer film consisting of carbon, fluorine, and oxygen, and has an average fluorine content in the film thickness direction of 30 atomic % to 40 atomic %, an average oxygen content in the film thickness direction of 5 atomic % to 20 atomic %, and the remainder being carbon atoms.

2. The fluorine-containing amorphous carbon film according to claim 1, comprising a high-concentration fluorine-containing region in a region shallower than 10 nm in depth from the surface, the high-concentration fluorine-containing region having a higher fluorine content than a region having a depth of 10 nm or more, the fluorine content being 50 atomic % or more and 75 atomic % or less, the oxygen content being 5 atomic % or more and 20 atomic % or less, and the remainder being carbon atoms.

3. The fluorine-containing amorphous carbon film according to claim 1, wherein the refractive index of the single layer film is 1.32 or more and less than 1.

40.

4. The fluorine-containing amorphous carbon film according to claim 1, wherein the light transmittance of the single layer film is 90% or more.

5. The fluorine-containing amorphous carbon film according to claim 1, wherein the monolayer film has a water droplet contact angle of 90° or more.

6. The fluorine-containing amorphous carbon film according to claim 1, wherein the hardness of the single layer film is 0.65 GPa or more as measured by a nanoindentation method.

7. The fluorine-containing amorphous carbon film according to any one of claims 1 to 6, wherein the thickness of the monolayer film is 25 nm or more and 500 nm or less.

8. The fluorine-containing amorphous carbon film according to claim 7, wherein the thickness of the single layer film is 50 nm or more and 250 nm or less.

9. A method for producing a fluorine-containing amorphous carbon film, comprising: placing a substrate in a chamber; introducing into the chamber a source gas whose chemical formula is represented only by carbon and fluorine and an inert gas for diluting the source gas; and forming a fluorine-containing amorphous carbon film on a surface of the substrate under plasma generation; and setting a mixture ratio of the inert gas to the source gas in terms of a flow rate into the chamber to be greater than 1 / 4 and less than 11 / 1.

10. The method for producing a fluorine-containing amorphous carbon film according to claim 9, wherein a mixture ratio of said inert gas to said source gas is set to 1 / 2 or more and 7 / 2 or less in terms of a flow rate ratio into said chamber.

11. The method for producing a fluorine-containing amorphous carbon film according to claim 9, wherein the pressure inside the chamber is set to 24 Pa or less.

12. The source gas is CF 4 , C 2 F 6 , C 3 F 8 , C 4 F 8 10. The method for producing a fluorine-containing amorphous carbon film according to claim 9, wherein the gas is a mixture of two or more gases selected from the group consisting of fluorine-containing gases, fluorine-containing amorphous carbon film, and fluorine-containing amorphous carbon film.

13. The method for producing a fluorine-containing amorphous carbon film according to any one of claims 9 to 12, wherein the inert gas is Ar gas.

Citation Information

Patent Citations

  • Fluorine-containing amorphous hard carbon film and method of manufacturing the same

    JP2020143348A

  • Method for producing fluorinated diamond-like carbon films

    US20020098285A1

  • Fluorinated and Hydrogenated Diamond-Like Carbon Materials for Anti-Reflective Coatings