Method for manufacturing layered optical film
The method enhances adhesiveness and productivity in laminated optical film production by using a boron-containing compound and optimizing adhesive composition water content and film thickness ratios, addressing the challenge of increasing production line speed while maintaining excellent adhesion.
Patent Information
- Application Number
- PCT/JP2024/009464
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-03-12
- Publication Date
- 2024-11-14
AI Technical Summary
The existing methods for manufacturing laminated optical films face challenges in increasing production line speed while maintaining excellent adhesiveness between optical films, particularly due to issues with water content and reaction rates in adhesive compositions.
A method involving the application of a boron-containing compound and a curable component with a polymerization initiator, where the adhesive composition has a water content of 40% or less and a film thickness ratio design that allows for rapid curing without a drying step, enhancing adhesion and productivity.
This approach results in improved adhesiveness and water-resistant properties between the optical films, enabling higher production line speeds without compromising bonding quality.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Method for manufacturing laminated optical film
[0001] The present invention relates to a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer. The laminated optical film can be used to form image displays such as liquid crystal displays (LCDs), organic EL displays, CRTs, and PDPs.
[0002] Liquid crystal display devices (LCDs) are rapidly expanding into the market for watches, mobile phones, PDAs, laptops, PC monitors, DVD players, TVs, and more. Liquid crystal display devices visualize the polarization state through the switching of liquid crystals, and polarizers are used for this display principle. In particular, applications such as TVs require increasingly higher brightness, contrast, and a wider viewing angle, which in turn requires increasingly higher transmittance, polarization degree, and color reproducibility in polarizing films.
[0003] The most commonly used polarizers are iodine-based polarizers, which have a structure in which iodine is adsorbed into polyvinyl alcohol (hereinafter also simply referred to as "PVA") and stretched, due to their high transmittance and polarization degree. A typical polarizing film is one in which transparent protective films are bonded to both sides of a polarizer using a so-called aqueous adhesive in which a polyvinyl alcohol-based material is dissolved in water (see Patent Document 1 below). Examples of transparent protective films that can be used include triacetyl cellulose, which has high moisture permeability. When using the aqueous adhesive (so-called wet lamination), a drying process is required after bonding the polarizer and the transparent protective film together.
[0004] Meanwhile, active energy ray-curable adhesives have been proposed as an alternative to the water-based adhesives. When a polarized film is produced using an active energy ray-curable adhesive, a drying step is not required, and therefore productivity of the polarized film can be improved. For example, a radical polymerization type active energy ray-curable adhesive that uses an N-substituted amide monomer as a curable component has been proposed (see Patent Document 2 below).
[0005] Patent Document 3 listed below discloses a method for producing a polarizing film in which a transparent protective film is provided on at least one surface of a polarizer via an adhesive layer, and the method includes a first coating step in which a solvent-containing easy-adhesion composition is applied to the bonding surface of the polarizer while transporting the polarizer to form a wet first coating film, a second coating step in which an adhesive composition is applied to the bonding surface of the transparent protective film while transporting the transparent protective film to form a second coating film, a first thickness measurement step in which the thickness of the wet first coating film is measured inline, a drying step in which, after the first thickness measurement step, the solvent in the wet first coating film is removed using a dryer to form a dry first coating film, and a drying step in which the thickness of the dry first coating film is measured inline after the drying step. The document describes a method for producing a polarized film, including: a second thickness measurement step for measuring the thickness in-line; a dryness adjustment step for adjusting the dryness of the newly formed dry first coating film by adjusting the temperature and / or air volume of a dryer so that the ratio of the thickness of the wet first coating film obtained by in-line measurement to the thickness of the dry first coating film satisfies a specific formula; a lamination step for laminating the dry first coating film formed on the lamination surface of a polarizer with the second coating film formed on the lamination surface of a transparent protective film to form an uncured adhesive layer; and an adhesion step for adhering the polarizer and the transparent protective film via the adhesive layer obtained by curing the uncured adhesive layer.
[0006] JP 2001-296427 A JP 2012-052000 A JP 2020-160391 A
[0007] In Patent Document 3, a dryness degree adjusting step is performed, but in recent years, it has become necessary to increase the line speed of the laminated optical film production line, particularly from the viewpoint of improving productivity. For this reason, it has been found that there is room for further improvement in both the materials and the process, such as the adhesive composition and the easy-adhesion composition that constitute the adhesive layer.
[0008] The present invention was developed to solve the above-mentioned problems, and aims to provide a method for manufacturing a laminated optical film that has excellent adhesion between a first optical film and a second optical film while increasing the line speed of the laminated optical film manufacturing line.
[0009] The above-mentioned problems can be solved by the following configuration: That is, the present invention is a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, the method comprising: conveying the first optical film while applying a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 each independently represent a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and water; a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator onto the bonding surface of the second optical film while transporting the second optical film; a laminating step of laminating the first optical film and the second optical film; and a bonding step of bonding the first optical film and the second optical film via the adhesive layer formed by irradiating the first optical film surface side or the second optical film surface side with active energy rays to cure at least the adhesive composition, wherein the content of the water in the easy-adhesion composition is 40 mass % or less, and where α is the film thickness of the easy-adhesion composition after the first coating step and β is the film thickness of the adhesive composition after the second coating step, β satisfies the relationship β>α.
[0010] In the method (1) for producing a laminated optical film, a method (2) for producing a laminated optical film is preferred in which a drying step is not provided between the first coating step and the laminating step.
[0011] In the method (1) or (2) for producing a laminated optical film, a method (3) for producing a laminated optical film is preferred, in which the time required from the end of the first coating step to the start of the laminating step is 5 seconds or less.
[0012] In any one of the above-mentioned laminated optical film manufacturing methods (1) to (3), a laminated optical film manufacturing method (4) is preferred, in which the first optical film is a polarizer.
[0013] In any one of the above-mentioned laminated optical film manufacturing methods (1) to (4), a laminated optical film manufacturing method (5) is preferred in which the second optical film is a transparent protective film.
[0014] In any one of the methods (1) to (5) for producing a laminated optical film, the adhesive composition contains, as a polymerizable component, a polymerizable compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 may form a cyclic heterocycle).
[0015] In any one of the above-mentioned methods (1) to (6) for producing a laminated optical film, a method (7) for producing a laminated optical film is preferred, in which the easy-adhesion composition contains a compound represented by the general formula (2).
[0016] In the method for producing a laminated optical film according to the present invention, an easy-adhesion composition is applied to the bonding surface of a first optical film (first coating step), an adhesive composition is applied to the bonding surface of a second optical film (second coating step), and the first optical film and the second optical film are bonded together so that their bonding surfaces overlap (bonding step). Here, the method for producing a laminated optical film according to the present invention incorporates the following innovations in terms of materials: (i) At least a specific boron-containing compound (a compound represented by general formula (1)) and water are blended into the easy-adhesion composition, and the water content in the easy-adhesion composition is designed to be 40 mass% or less. (ii) At least a curable component and a polymerization initiator are blended into the adhesive composition. In addition, the method for producing a laminated optical film according to the present invention incorporates the following innovations in terms of processes: (iii) When the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, the relationship β is designed to be greater than α. By providing all of the above configurations (i), (ii), and (iii), the method for producing a laminated optical film according to the present invention can produce a laminated optical film having excellent adhesion between the first optical film and the second optical film while increasing the line speed of the laminated optical film production line. The reason for this effect can be presumed to be as follows.
[0017] The specific boron-containing compound blended in the easy-adhesion composition significantly contributes to improving the adhesion between the first optical film and the adhesive layer, particularly improving the adhesion under humid conditions. However, when the line speed of the production line for the laminated optical film is increased, the water in the easy-adhesion composition is hardly removed, and the amount of water in the easy-adhesion composition increases. This reduces the relative concentration of the polymerization initiator migrating from the adhesive composition, and the boron-containing compound cannot sufficiently react with the curable component blended in the adhesive composition. As a result, it is expected that the adhesion between the first optical film and the adhesive layer will deteriorate. However, in the method for producing a laminated optical film according to the present invention, the water content in the easy-adhesion composition is set to 40% by mass or less, that is, the water content is designed to be lower than that of conventional easy-adhesion compositions ((i) above), and when the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, β is designed to be > α ((iii) above). This makes it easier for the polymerization initiator blended in the adhesive composition to migrate into the easy-adhesion composition, that is, by increasing the relative concentration of the polymerization initiator migrating from the adhesive composition, the reaction rate between the curable component blended in the adhesive composition and the boron-containing compound is increased ((ii) above). As a result, for example, by not providing a drying step between the first coating step and the lamination step, or by designing the time required from the end of the first coating step to the start of the lamination step to be short, it is estimated that a laminated optical film having excellent adhesion, particularly water-resistant adhesion, between the first optical film and the second optical film can be produced, even when the line speed of the laminated optical film production line is increased.
[0018] The method for producing a laminated optical film according to the present invention is a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, and the method comprises the steps of: conveying the first optical film; applying a compound represented by the following general formula (1): to a bonding surface of the first optical film; (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2the adhesive composition includes a first coating step of coating an adhesive composition containing water and an adhesive layer formed by irradiating the adhesive layer with active energy rays from the first optical film side or the second optical film side to cure the adhesive composition, and a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator onto the laminating surface of the second optical film while conveying the second optical film. The adhesive layer is formed by irradiating the adhesive layer with active energy rays from the first optical film side or the second optical film side to cure the adhesive composition, and the adhesive layer is formed by irradiating the adhesive layer with active energy rays from the first optical film side or the second optical film side to cure the adhesive composition. The adhesive composition has a water content of 40 mass% or less, and when the film thickness of the adhesive composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, the relationship β > α is satisfied. First, the materials used in the method for producing a laminated optical film according to the present invention will be described.
[0019] (Easy-Adhesion Composition) The easy-adhesion composition contains at least a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent, and R 1 and R 2 each independently represents a hydrogen atom, an aliphatic hydrocarbon group, an aryl group, or a heterocyclic group which may have a substituent) and water.
[0020] In the compound represented by general formula (1), examples of the aliphatic hydrocarbon group include a linear or branched alkyl group having 1 to 20 carbon atoms which may have a substituent, a cyclic alkyl group having 3 to 20 carbon atoms which may have a substituent, and an alkenyl group having 2 to 20 carbon atoms; examples of the aryl group include a phenyl group having 6 to 20 carbon atoms which may have a substituent, and a naphthyl group having 10 to 20 carbon atoms which may have a substituent; and examples of the heterocyclic group include a 5- or 6-membered ring group which contains at least one hetero atom and may have a substituent. These may be linked to each other to form a ring. In general formula (1), R 1 and R 2is preferably a hydrogen atom or a linear or branched alkyl group having 1 to 3 carbon atoms, and most preferably a hydrogen atom.
[0021] X in the compound represented by general formula (1) is a reactive group, which is a functional group that can react with the curable component that constitutes the adhesive layer, and examples thereof include a hydroxyl group, an amino group, an aldehyde group, a carboxyl group, a vinyl group, a (meth)acrylic group, a styryl group, a (meth)acrylamide group, a vinyl ether group, an epoxy group, an oxetane group, an α,β-unsaturated carbonyl group, a mercapto group, and a halogen group. When the curable adhesive composition constituting the adhesive layer is active energy ray-curable, the reactive group X is preferably at least one reactive group selected from the group consisting of vinyl groups, (meth)acrylic groups, styryl groups, (meth)acrylamide groups, vinyl ether groups, epoxy groups, oxetane groups, and mercapto groups. When the curable adhesive composition constituting the adhesive layer is radically polymerizable, the reactive group X is preferably at least one reactive group selected from the group consisting of (meth)acrylic groups, styryl groups, and (meth)acrylamide groups. When the compound represented by general formula (1) has a (meth)acrylamide group, this is more preferred because it has high reactivity and increases the copolymerization rate with the curable component in the adhesive layer. Furthermore, this is also preferred because the (meth)acrylamide group has high polarity and excellent adhesion, allowing the effects of the present invention to be obtained efficiently. When the curable adhesive composition constituting the adhesive layer is cationically polymerizable, the reactive group X preferably has at least one functional group selected from a hydroxyl group, an amino group, an aldehyde, a carboxyl group, a vinyl ether group, an epoxy group, an oxetane group, and a mercapto group. In particular, when the reactive group X has an epoxy group, this is preferred because the resulting adhesive layer has excellent adhesion to the adherend, and when the reactive group X has a vinyl ether group, this is preferred because the curability of the curable adhesive composition is excellent.
[0022] Preferred specific examples of the compound represented by general formula (1) include the following compounds (1a) to (1d). 3 is a hydrogen atom or a methyl group.
[0023] In addition to the compounds exemplified above, examples of the compound represented by general formula (1) include esters of (meth)acrylates and boric acid, such as esters of hydroxyethyl acrylamide and boric acid, esters of methylolacrylamide and boric acid, esters of hydroxyethyl acrylate and boric acid, and esters of hydroxybutyl acrylate and boric acid.
[0024] In order to increase the copolymerization rate with the curable component constituting the adhesive layer and improve the adhesion between the first optical film and the adhesive layer, the amount of the compound represented by general formula (1) in the easy-adhesion composition is preferably 0.5 to 15 mass %, and more preferably 1 to 10 mass %.
[0025] The adhesive composition used in the present invention contains water in addition to the compound represented by general formula (1). However, in the method for producing a laminated optical film according to the present invention, the line speed of the laminated optical film production line must be increased, and therefore, almost no water is removed from the adhesive composition. For this reason, the water content in the adhesive composition is preferably 40% by mass or less, and more preferably 30% by mass or less.
[0026] In the present invention, the easy-adhesion composition may contain a solvent other than water. The solvent that may be contained in the easy-adhesion composition is preferably one that can stabilize and dissolve or disperse the compound represented by general formula (1). Examples of such solvents include esters such as ethyl acetate, butyl acetate, and 2-hydroxyethyl acetate; ketones such as methyl ethyl ketone, acetone, cyclohexanone, methyl isobutyl ketone, diethyl ketone, methyl-n-propyl ketone, and acetylacetone; cyclic ethers such as tetrahydrofuran (THF) and dioxane; aliphatic or alicyclic hydrocarbons such as n-hexane and cyclohexane; aromatic hydrocarbons such as toluene and xylene; aliphatic or alicyclic alcohols such as methanol, ethanol, n-propanol, isopropanol, and cyclohexanol; glycol ethers such as ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, and diethylene glycol monoethyl ether; and glycol ether acetates such as diethylene glycol monomethyl ether acetate and diethylene glycol monoethyl ether acetate.
[0027] Furthermore, in the present invention, other additives, such as tackifiers, ultraviolet absorbers, antioxidants, and stabilizers such as heat stabilizers, may be blended into the easily adhesive composition.
[0028] In the present invention, a curable component may be blended into the adhesive composition, and preferably, a compound represented by general formula (2), which is preferably blended into an adhesive composition, may be blended as the curable component. The compound represented by general formula (2) will be described later. When a curable component, preferably a compound represented by general formula (2), is blended into the adhesive composition, the blending amount is preferably 20 to 80 mass %, and more preferably 40 to 70 mass %.
[0029] In the present invention, it is preferable that no polymerization initiator is blended into the easy-adhesion composition used in the first coating step, and even if a polymerization initiator is blended, it is preferably blended in an amount of 3 mass % or less, more preferably 1 mass % or less, and it is particularly preferable that no polymerization initiator is blended.
[0030] (Adhesive Composition) The adhesive composition contains at least a curable component and a polymerization initiator. The adhesive composition used in the present invention is preferably an active energy ray-curable adhesive composition. Active energy ray-curable adhesive compositions can be divided into radical polymerization-curable adhesive compositions and cationic polymerization-curable adhesive compositions. In the present invention, active energy rays in the wavelength range of 10 nm to less than 380 nm are referred to as ultraviolet rays, and active energy rays in the wavelength range of 380 nm to 800 nm are referred to as visible light.
[0031] The curable component to be incorporated into the radical polymerization curable adhesive composition may be, for example, a compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, and R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 The number of carbon atoms in the alkyl moiety of the alkyl group, hydroxyalkyl group, and / or alkoxyalkyl group is not particularly limited, but examples include those having 1 to 4 carbon atoms. 5 and R 6 Examples of the cyclic heterocycle that may be formed include N-acryloylmorpholine.
[0032] Specific examples of the compound represented by general formula (2) include N-alkyl group-containing (meth)acrylamide derivatives such as N-methyl(meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, N-butyl(meth)acrylamide, and N-hexyl(meth)acrylamide; N-hydroxyalkyl group-containing (meth)acrylamide derivatives such as N-methylol(meth)acrylamide, N-hydroxyethyl(meth)acrylamide, and N-methylol-N-propane(meth)acrylamide; and N-alkoxy group-containing (meth)acrylamide derivatives such as N-methoxymethylacrylamide and N-ethoxymethylacrylamide. Examples of the cyclic ether group-containing (meth)acrylamide derivative include heterocycle-containing (meth)acrylamide derivatives in which the nitrogen atom of the (meth)acrylamide group forms a heterocycle, such as N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, N-acryloylpyrrolidine, etc. Among these, N-hydroxyethylacrylamide and N-acryloylmorpholine are preferred because of their excellent reactivity, ability to produce a cured product with a high elastic modulus, and excellent adhesion to polarizers.
[0033] From the viewpoint of improving the adhesion between the first optical film and the adhesive layer, and further the adhesion between the first optical film and the second optical film, the content of the compound represented by general formula (2) in the curable adhesive composition is preferably 20 to 80 mass %, and more preferably 30 to 60 mass %.
[0034] The curable adhesive composition used in the present invention may contain, as a curable component, other monofunctional radically polymerizable compounds in addition to the compound represented by general formula (2). Examples of the monofunctional radically polymerizable compounds include various (meth)acrylic acid derivatives having a (meth)acryloyloxy group. Specific examples include (meth)acrylic acid (C1-20) alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and n-octadecyl (meth)acrylate.
[0035] Examples of the (meth)acrylic acid derivatives include cycloalkyl (meth)acrylates such as cyclohexyl (meth)acrylate and cyclopentyl (meth)acrylate; aralkyl (meth)acrylates such as benzyl (meth)acrylate; 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, and dicyclopentenyloxy Examples of suitable (meth)acrylates include polycyclic (meth)acrylates such as ethyl (meth)acrylate and dicyclopentanyl (meth)acrylate; and alkoxy or phenoxy group-containing (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, and alkylphenoxy polyethylene glycol (meth)acrylate. Among these, dicyclopentenyloxyethyl acrylate and phenoxyethyl acrylate are preferred because of their excellent adhesion to various protective films.
[0036] In addition, examples of the (meth)acrylic acid derivatives include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate. hydroxyl group-containing (meth)acrylates such as [4-(hydroxymethyl)cyclohexyl]methyl acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-phenoxypropyl (meth)acrylate; epoxy group-containing (meth)acrylates such as glycidyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate glycidyl ether; 2,2,2-trifluoroethyl (meth)acrylate, 2,2,2-trifluoroethylethyl (meth)acrylate; Halogen-containing (meth)acrylates such as acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, and 3-chloro-2-hydroxypropyl (meth)acrylate; alkylaminoalkyl (meth)acrylates such as dimethylaminoethyl (meth)acrylate; 3-oxetanylmethyl (meth)acrylate, 3-methyl-oxetanylmethyl (meth)acrylate; oxetane group-containing (meth)acrylates such as acrylate, 3-ethyl-oxetanylmethyl (meth)acrylate, 3-butyl-oxetanylmethyl (meth)acrylate, and 3-hexyl-oxetanylmethyl (meth)acrylate; (meth)acrylates having a heterocycle such as tetrahydrofurfuryl (meth)acrylate and butyrolactone (meth)acrylate; hydroxypivalic acid neopentyl glycol (meth)acrylic acid adduct; and p-phenylphenol (meth)acrylate. Among these, 2-hydroxy-3-phenoxypropyl acrylate is preferred because of its excellent adhesion to various protective films.
[0037] Furthermore, examples of the monofunctional radically polymerizable compound include carboxyl group-containing monomers such as (meth)acrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, and isocrotonic acid.
[0038] Examples of the monofunctional radically polymerizable compound include lactam vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; and vinyl monomers having a nitrogen-containing heterocycle such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, and vinylmorpholine.
[0039] Furthermore, as the monofunctional radical polymerizable compound, a radical polymerizable compound having an active methylene group can be used. The radical polymerizable compound having an active methylene group is a compound having an active double bond group such as a (meth)acrylic group at the end or in the molecule, and also having an active methylene group. Examples of the active methylene group include an acetoacetyl group, an alkoxymalonyl group, and a cyanoacetyl group. It is preferable that the active methylene group is an acetoacetyl group. Specific examples of radically polymerizable compounds having an active methylene group include acetoacetoxyalkyl (meth)acrylates such as 2-acetoacetoxyethyl (meth)acrylate, 2-acetoacetoxypropyl (meth)acrylate, and 2-acetoacetoxy-1-methylethyl (meth)acrylate; 2-ethoxymalonyloxyethyl (meth)acrylate, 2-cyanoacetoxyethyl (meth)acrylate, N-(2-cyanoacetoxyethyl)acrylamide, N-(2-propionylacetoxybutyl)acrylamide, N-(4-acetoacetoxymethylbenzyl)acrylamide, and N-(2-acetoacetylaminoethyl)acrylamide. The radically polymerizable compound having an active methylene group is preferably an acetoacetoxyalkyl (meth)acrylate.
[0040] A bifunctional or higher polyfunctional radically polymerizable compound can be blended as a curable component constituting the radical polymerization curable adhesive composition. Examples of the polyfunctional radically polymerizable compound include polyfunctional (meth)acrylamide derivatives such as N,N'-methylenebis(meth)acrylamide, tripropylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, 1,10-decanediol diacrylate, 2-ethyl-2-butylpropanediol di(meth)acrylate, bisphenol A di(meth)acrylate, bisphenol A ethylene oxide adduct di(meth)acrylate, bisphenol A propylene oxide adduct di(meth)acrylate, and bisphenol A diglycidyl ether di(meth)acrylate. esters of (meth)acrylic acid with polyhydric alcohols such as acrylate, neopentyl glycol di(meth)acrylate, tricyclodecane dimethanol di(meth)acrylate, cyclic trimethylolpropane formal(meth)acrylate, dioxane glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and EO-modified diglycerin tetra(meth)acrylate; and 9,9-bis[4-(2-(meth)acryloyloxyethoxy)phenyl]fluorene. Specific examples include Aronix M-220 (manufactured by Toagosei Co., Ltd.), Light Acrylate 1,9ND-A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DGE-4A (manufactured by Kyoeisha Chemical Co., Ltd.), Light Acrylate DCP-A (manufactured by Kyoeisha Chemical Co., Ltd.), SR-531 (manufactured by Sartomer Co., Ltd.), and CD-536 (manufactured by Sartomer Co., Ltd.), etc. Furthermore, various epoxy (meth)acrylates, urethane (meth)acrylates, polyester (meth)acrylates, and various (meth)acrylate monomers may be used as needed.It is preferable to include a polyfunctional (meth)acrylamide derivative in the adhesive composition because it has a high polymerization rate, is excellent in productivity, and has excellent crosslinking properties when the adhesive composition is cured.
[0041] From the viewpoint of achieving both adhesiveness to the first optical film and the second optical film and optical durability under harsh environments, it is preferable to use a combination of a monofunctional radically polymerizable compound and a polyfunctional radically polymerizable compound as the radically polymerizable compound. The amount of the monofunctional radically polymerizable compound in the adhesive composition is preferably 30 to 90 mass%, more preferably 50 to 80 mass%. The amount of the polyfunctional radically polymerizable compound in the adhesive composition is preferably 10 to 70 mass%, more preferably 20 to 50 mass%.
[0042] From the viewpoint of improving the adhesion between the first optical film and the adhesive layer, and further between the first optical film and the second optical film, the adhesive composition used in the present invention may contain a compound represented by the general formula (1) as a curable component. The content of the compound represented by the general formula (1) in the curable adhesive composition is preferably 0.1 to 7 mass %, more preferably 1 to 5 mass %.
[0043] <Embodiments of Radical Polymerization-Curable Adhesive Composition> The adhesive composition used in the present invention can be used as an active energy ray-curable adhesive composition when the curable component is an active energy ray-curable component. When ultraviolet light or visible light is used as the active energy ray, it is preferable that the adhesive composition contains a photopolymerization initiator as the polymerization initiator.
[0044] The photopolymerization initiator is appropriately selected depending on the active energy ray. When curing is performed with ultraviolet light or visible light, a photopolymerization initiator that is cleaved by ultraviolet light or visible light is used. Examples of the photopolymerization initiator include benzophenone-based compounds such as benzil, benzophenone, benzoylbenzoic acid, and 3,3'-dimethyl-4-methoxybenzophenone; aromatic ketone compounds such as 4-(2-hydroxyethoxy)phenyl(2-hydroxy-2-propyl)ketone, α-hydroxy-α,α'-dimethylacetophenone, 2-methyl-2-hydroxypropiophenone, and α-hydroxycyclohexylphenyl ketone; acetophenone-based compounds such as methoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxyacetophenone, and 2-methyl-1-[4-(methylthio)-phenyl]-2-morpholinopropane-1; benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin methyl ether. aromatic sulfonyl chloride compounds such as 2-naphthalenesulfonyl chloride; photoactive oxime compounds such as 1-phenone-1,1-propanedione-2-(o-ethoxycarbonyl)oxime; thioxanthone compounds such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone; camphorquinone; halogenated ketones; acylphosphinoxides; and acylphosphonates.
[0045] From the viewpoint of improving the adhesion between the first optical film and the adhesive layer, and further the adhesion between the first optical film and the second optical film, when a photopolymerization initiator is blended into the adhesive composition in the present invention, the amount is preferably 0.5 to 10 mass %, and more preferably 1 to 5 mass %.
[0046] When the active energy ray-curable adhesive composition is used as a visible light-curable type, it is preferable to use a photopolymerization initiator that is particularly sensitive to light of 380 nm or more. Photopolymerization initiators that are highly sensitive to light of 380 nm or more will be described later.
[0047] The photopolymerization initiator may be a compound represented by the following general formula (3): (In the formula, R 7 and R 8 -H, -CH 2 CH 3 , -iPr or Cl, R 7 and R 8 It is preferable to use a compound represented by general formula (3) alone, or to use a compound represented by general formula (3) in combination with a photopolymerization initiator highly sensitive to light of 380 nm or longer, which will be described later. When a compound represented by general formula (3) is used, the adhesiveness is superior to when a photopolymerization initiator highly sensitive to light of 380 nm or longer is used alone. Among the compounds represented by general formula (3), R 7 and R 8 Ga-CH 2 CH 3 The amount of the compound represented by general formula (3) in the active energy ray-curable adhesive composition is preferably 0.1 to 10 mass %, and more preferably 1 to 5 mass %.
[0048] It is also preferable to add a polymerization initiation aid as needed. Examples of the polymerization initiation aid include triethylamine, diethylamine, N-methyldiethanolamine, ethanolamine, 4-dimethylaminobenzoic acid, methyl 4-dimethylaminobenzoate, ethyl 4-dimethylaminobenzoate, and isoamyl 4-dimethylaminobenzoate, with ethyl 4-dimethylaminobenzoate being particularly preferred. When a polymerization initiation aid is used, the amount added is preferably 0.1 to 10% by mass, and more preferably 1 to 5% by mass.
[0049] In addition, a known photopolymerization initiator can be used in combination as needed. Since the optical functional layer and the base film having UV absorption ability do not transmit light of 380 nm or less, it is preferable to use a photopolymerization initiator that is highly sensitive to light of 380 nm or more. Specific examples include 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, and the like.
[0050] The adhesive composition used in the present invention may contain an acrylic oligomer obtained by polymerizing a (meth)acrylic monomer. By containing the acrylic oligomer in the adhesive composition, cure shrinkage when the composition is irradiated with active energy rays and cured can be reduced, and interfacial stress between the adhesive layer and the first optical film and the second optical film can be reduced, thereby suppressing a decrease in adhesion.
[0051] Considering workability and uniformity during application, it is preferable that the active energy ray-curable adhesive composition has a low viscosity, and therefore it is preferable that the acrylic oligomer obtained by polymerizing a (meth)acrylic monomer also has a low viscosity. As an acrylic oligomer that has a low viscosity and can prevent cure shrinkage of the adhesive layer, one having a weight average molecular weight (Mw) of preferably 15,000 or less, more preferably 10,000 or less, and particularly preferably 5,000 or less. On the other hand, in order to sufficiently suppress cure shrinkage of the cured product layer (adhesive layer), the weight average molecular weight (Mw) of the acrylic oligomer is preferably 500 or more, more preferably 1,000 or more, and particularly preferably 1,500 or more. Specific examples of the (meth)acrylic monomer constituting the acrylic oligomer include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, 2-methyl-2-nitropropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, n-pentyl (meth)acrylate, t-pentyl (meth)acrylate, 3-pentyl (meth)acrylate, 2,(Meth)acrylic acid (C1-20) alkyl esters such as 2-dimethylbutyl (meth)acrylate, n-hexyl (meth)acrylate, cetyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and N-octadecyl (meth)acrylate; further, for example, cycloalkyl (meth)acrylates (for example, cyclohexyl (meth)acrylate, cyclopentyl (meth)acrylate, etc.), aralkyl (meth)acrylates (for example, benzyl (meth)acrylate, etc.), polycyclic (meth)acrylates (for example, 2-isobornyl (meth)acrylate, 2-norbornylmethyl (meth)acrylate, 5-norbornen-2-yl-methyl (meth)acrylate, 3-methyl-2-norbornylmethyl (meth)acrylate, 4-methyl-2-propylpentyl (meth)acrylate, and 4-methyl-2-propylpentyl (meth)acrylate; (meth)acrylate, etc.), hydroxyl group-containing (meth)acrylic acid esters (for example, hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2,3-dihydroxypropylmethyl-butyl (meth)methacrylate, etc.), alkoxy group- or phenoxy group-containing (meth)acrylic acid esters (2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 2-methoxymethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, ethyl carbitol (meth)acrylate, phenoxyethyl (meth)acrylate, etc.), epoxy group-containing (meth)acrylic acid esters (for example, glycidyl (meth)acrylate, etc.), halogen-containing (meth)acrylic acid esters (for example, 2,2,2-trifluoroethyl (meth)acrylate, 2,2,Examples of the acrylic oligomer (E) include 2-trifluoroethylethyl (meth)acrylate, tetrafluoropropyl (meth)acrylate, hexafluoropropyl (meth)acrylate, octafluoropentyl (meth)acrylate, heptadecafluorodecyl (meth)acrylate, etc., and alkylaminoalkyl (meth)acrylates (for example, dimethylaminoethyl (meth)acrylate, etc.). These (meth)acrylates can be used alone or in combination of two or more. Specific examples of the acrylic oligomer (E) include "ARUFON" manufactured by Toagosei Co., Ltd., "Actflow" manufactured by Soken Chemical & Engineering Co., Ltd., and "JONCRYL" manufactured by BASF Japan Ltd.
[0052] The amount of the acrylic oligomer in the adhesive composition is preferably 3 to 40% by mass, and more preferably 5 to 20% by mass.
[0053] The adhesive composition used in the present invention may contain a silane coupling agent. Specific examples of the silane coupling agent include active energy ray-curable compounds such as vinyltrichlorosilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane.
[0054] Preferred are 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0055] Specific examples of non-active energy ray-curable silane coupling agents other than those mentioned above include 3-ureidopropyltriethoxysilane, 3-chloropropyltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, bis(triethoxysilylpropyl)tetrasulfide, 3-isocyanatepropyltriethoxysilane, and imidazole silane.
[0056] The adhesive composition used in the present invention may be a cationic polymerization-curable adhesive composition. Cationic polymerizable compounds used in cationic polymerization-curable adhesive compositions are classified into monofunctional cationic polymerizable compounds having one cationic polymerizable functional group in the molecule and polyfunctional cationic polymerizable compounds having two or more cationic polymerizable functional groups in the molecule. Monofunctional cationic polymerizable compounds have relatively low liquid viscosity, and their inclusion in a cationic polymerization-curable adhesive composition can reduce the liquid viscosity. Furthermore, monofunctional cationic polymerizable compounds often have functional groups that impart various functions. By including them in a cationic polymerization-curable adhesive composition, various functions can be imparted to the cationic polymerization-curable adhesive composition and / or the cured product of the cationic polymerization-curable adhesive composition. Polyfunctional cationic polymerizable compounds are preferably included in cationic polymerization-curable adhesive compositions because they can three-dimensionally crosslink the cured product of the cationic polymerization-curable adhesive composition. The ratio of the monofunctional cationic polymerizable compound to the polyfunctional cationic polymerizable compound is preferably in the range of 10 to 1,000 parts by mass per 100 parts by mass of the monofunctional cationic polymerizable compound. Examples of the cationically polymerizable functional group include an epoxy group, an oxetanyl group, and a vinyl ether group. Examples of compounds having an epoxy group include an aliphatic epoxy compound, an alicyclic epoxy compound, and an aromatic epoxy compound. The cationically polymerizable adhesive composition of the present invention particularly preferably contains an alicyclic epoxy compound because of its excellent curability and adhesive properties. Examples of the alicyclic epoxy compound include 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, caprolactone-modified products, trimethylcaprolactone-modified products, and valerolactone-modified products of 3,4-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, and specific examples thereof include Celloxide 2021, Celloxide 2021A, Celloxide 2021P, Celloxide 2081, Celloxide 2083, and Celloxide 2085 (all manufactured by Daicel Chemical Industries, Ltd.), and Cyracure UVR-6105, Cyracure UVR-6107, Cyracure 30, and R-6110 (all manufactured by Dow Chemical Japan Ltd.).Compounds having an oxetanyl group are preferably contained because they have the effect of improving the curing properties of the cationically polymerizable adhesive composition and reducing the liquid viscosity of the composition. Examples of compounds having an oxetanyl group include 3-ethyl-3-hydroxymethyloxetane, 1,4-bis[(3-ethyl-3-oxetanyl)methoxymethyl]benzene, 3-ethyl-3-(phenoxymethyl)oxetane, di[(3-ethyl-3-oxetanyl)methyl]ether, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, and phenol novolac oxetane. Commercially available compounds include Aronoxetane OXT-101, Aronoxetane OXT-121, Aronoxetane OXT-211, Aronoxetane OXT-221, and Aronoxetane OXT-212 (all manufactured by Toagosei Co., Ltd.). Compounds having a vinyl ether group are preferably contained because they have the effect of improving the curing properties of the cationically polymerizable adhesive composition and reducing the liquid viscosity of the composition. Examples of compounds having a vinyl ether group include 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, triethylene glycol divinyl ether, cyclohexanedimethanol divinyl ether, cyclohexanedimethanol monovinyl ether, tricyclodecane vinyl ether, cyclohexyl vinyl ether, methoxyethyl vinyl ether, ethoxyethyl vinyl ether, and pentaerythritol tetravinyl ether.
[0057] The cationic polymerization-curable adhesive composition contains at least one compound selected from the group consisting of the epoxy group-containing compound, the oxetanyl group-containing compound, and the vinyl ether group-containing compound described above as a curable component. Since all of these compounds cure by cationic polymerization, a photocationic polymerization initiator is incorporated into the composition. This photocationic polymerization initiator generates cationic species or Lewis acids upon irradiation with active energy rays such as visible light, ultraviolet light, X-rays, and electron beams, thereby initiating the polymerization reaction of the epoxy group or oxetanyl group. The photoacid generator described below is preferably used as the photocationic polymerization initiator. Furthermore, when the cationic polymerization adhesive composition is used as a visible light-curable adhesive, it is preferable to use a photocationic polymerization initiator that is highly sensitive to light of 380 nm or longer. However, since photocationic polymerization initiators generally exhibit a maximum absorption in the wavelength range around 300 nm or shorter, incorporating a photosensitizer that exhibits a maximum absorption in the longer wavelength range, specifically, light of wavelengths longer than 380 nm, can enhance the generation of cationic species or acids from the photocationic polymerization initiator by reacting to light of this wavelength range. Examples of photosensitizers include anthracene compounds, pyrene compounds, carbonyl compounds, organic sulfur compounds, persulfides, redox compounds, azo and diazo compounds, halogen compounds, and photoreducible dyes, and two or more of these may be used in combination. Anthracene compounds are particularly preferred because of their excellent photosensitizing effect, and specific examples include Anthracure UVS-1331 and Anthracure UVS-1221 (manufactured by Kawasaki Chemical Industries, Ltd.). The content of the photosensitizer is preferably 0.1% by mass to 5% by mass, and more preferably 0.5% by mass to 3% by mass.
[0058] In the present invention, the active energy ray-curable adhesive composition may contain a photoacid generator. When the active energy ray-curable adhesive composition contains a photoacid generator, the water resistance and durability of the adhesive layer can be dramatically improved compared to when the active energy ray-curable adhesive composition does not contain a photoacid generator. The photoacid generator can be represented by the following general formula (3):
[0059] General formula (4) (However, L +represents any onium cation. - is PF6 6 - , SbF 6 - , AsF 6 - , SbCl 6 - , BiCl 5 - , SnCl 6 - , ClO 4 - , a dithiocarbamate anion, and a counter anion selected from the group consisting of SCN-.
[0060] Next, the counter anion X in the general formula (4) - This article explains:
[0061] Counter anion X in general formula (4) - Although there is no particular limitation in principle, a non-nucleophilic anion is preferred. - When PF is a non-nucleophilic anion, nucleophilic reactions are unlikely to occur with cations coexisting in the molecule or with various materials used in combination, and as a result, it is possible to improve the stability over time of the photoacid generator represented by general formula (4) itself and compositions using it. The non-nucleophilic anion here refers to an anion with a low ability to cause a nucleophilic reaction. Examples of such anions include PF 6 - , SbF 6 - , AsF 6 - , SbCl 6 - , BiCl 5 - , SnCl 6 - , ClO 4 - , B(C 6 H 5 ) 4 - , dithiocarbamate anion, SCN - Examples include:
[0062] Specifically, "Cyracure UVI-6992" and "Cyracure UVI-6974" (both manufactured by Dow Chemical Japan Co., Ltd.), "ADEKAOPTOMER SP150", "ADEKAOPTOMER SP152", "ADEKAOPTOMER SP170", and "ADEKAOPTOMER SP172" (all manufactured by ADEKA Corporation), and "Omnicat250" (IGM Resins B.V.), "CI-5102", "CI-2855" (all manufactured by Nippon Soda Co., Ltd.), "SAN-AID SI-60L", "SAN-AID SI-80L", "SAN-AID SI-100L", "SAN-AID SI-110L", "SAN-AID SI-180L" (all manufactured by Sanshin Chemical Industry Co., Ltd.), "IK-1", "CPI-100P", "CPI-101A", "CPI-110P", "CPI-200K", "CPI-210S", "CPI Specific preferred examples of the photoacid generator of the present invention include "WPI-310B", "CPI-410B", and "CPI-410S" (all manufactured by San-Apro Ltd.), "WPI-069", "WPI-113", "WPI-116", "WPI-041", "WPI-044", "WPI-054", "WPI-055", "WPAG-281", "WPAG-567", and "WPAG-596" (all manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.).
[0063] (First optical film) Examples of the first optical film used in the present invention include a polarizer, a transparent protective film, and a retardation film. In particular, when a polarizer is used as the first optical film, it is preferred because of excellent adhesion between the polarizer and the adhesive layer.
[0064] In the present invention, the polarizer is not particularly limited, and various polarizers can be used. Examples of polarizers include those obtained by uniaxially stretching a hydrophilic polymer film, such as a polyvinyl alcohol film, a partially formalized polyvinyl alcohol film, or a partially saponified ethylene-vinyl acetate copolymer film, after iodine has been adsorbed thereon. The thickness of the polarizer can be, for example, 3 to 20 μm.
[0065] However, in the present invention, from the viewpoint of improving humidification reliability in a severe environment of high temperature and high humidity, it is preferable to use a thin polarizer having a thickness of 3 μm or more and 15 μm or less as the polarizer. A thickness of 12 μm or less is particularly preferable, and a thickness of 10 μm or less, particularly 8 μm or less, is further preferable. Such a thin polarizer has little thickness unevenness, excellent visibility, and is excellent in durability against thermal shock due to little dimensional change.
[0066] A polarizer obtained by dyeing a polyvinyl alcohol-based film with iodine and uniaxially stretching it can be produced, for example, by immersing the polyvinyl alcohol in an iodine aqueous solution to dye it and then stretching it to 3 to 7 times its original length. If necessary, the polyvinyl alcohol-based film may contain boric acid, zinc sulfate, zinc chloride, or the like, or may be immersed in an aqueous solution of potassium iodide or the like. Furthermore, if necessary, the polyvinyl alcohol-based film may be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water not only removes dirt and antiblocking agents from the polyvinyl alcohol-based film surface, but also swells the polyvinyl alcohol-based film, thereby preventing unevenness such as uneven dyeing. Stretching may be performed after dyeing with iodine, or the film may be stretched while dyeing, or the film may be dyed with iodine after stretching. Stretching may also be performed in an aqueous solution of boric acid, potassium iodide, or the like, or in a water bath.
[0067] The polarizer preferably contains boric acid from the viewpoints of stretching stability and humidification reliability. Furthermore, the content of boric acid in the polarizer is preferably 22% by mass or less, and more preferably 20% by mass or less, of the total amount of the polarizer, from the viewpoint of suppressing the occurrence of through cracks. From the viewpoints of stretching stability and humidification reliability, the content of boric acid in the polarizer is preferably 10% by mass or more, and more preferably 12% by mass or more, of the total amount of the polarizer.
[0068] Representative examples of the thin polarizer include the thin polarizers described in Japanese Patent No. 4751486, Japanese Patent No. 4751481, Japanese Patent No. 4815544, Japanese Patent No. 5048120, WO 2014 / 077599, and WO 2014 / 077636, and the like, as well as thin polarizers obtained by the manufacturing methods described therein.
[0069] Among the thin polarizers obtained by manufacturing methods including a stretching step and a dyeing step in a laminated state, those obtained by a manufacturing method including a stretching step in a boric acid aqueous solution as described in Japanese Patent Nos. 4751486, 4751481, and 4815544 are preferred because they can be stretched at a high magnification and have improved polarization performance. In particular, those obtained by a manufacturing method including a supplementary in-air stretching step before stretching in a boric acid aqueous solution as described in Japanese Patent Nos. 4751481 and 4815544 are preferred. These thin polarizers can be obtained by a manufacturing method including a stretching step and a dyeing step of a polyvinyl alcohol-based resin (hereinafter also referred to as PVA-based resin) layer and a stretching resin substrate in a laminated state. With this manufacturing method, even if the PVA-based resin layer is thin, it can be stretched without problems such as breakage due to stretching because it is supported by the stretching resin substrate.
[0070] (Second Optical Film) Examples of the second optical film used in the present invention include a polarizer, a transparent protective film, and a retardation film. In particular, when a polarizer is used as the first optical film, it is preferable to use a transparent protective film as the second optical film.
[0071] The transparent protective film is made of a thermoplastic resin that exhibits excellent transparency, mechanical strength, thermal stability, moisture barrier properties, and isotropy. Specific examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose-based resin films, polyester resins, polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins (norbornene-based resins), polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof. The transparent protective film may contain one or more suitable additives. Examples of additives include ultraviolet absorbers, antioxidants, lubricants, plasticizers, release agents, color inhibitors, flame retardants, nucleating agents, antistatic agents, pigments, and colorants. The content of the thermoplastic resin in the transparent protective film is preferably 50 to 100% by weight, more preferably 50 to 99% by weight, even more preferably 60 to 98% by weight, and particularly preferably 70 to 97% by weight. If the content of the thermoplastic resin in the transparent protective film is 50% by weight or less, the inherent high transparency of the thermoplastic resin may not be fully exhibited.
[0072] The material for forming the transparent protective film is preferably one that is excellent in transparency, mechanical strength, thermal stability, moisture blocking property, isotropy, etc., and in particular, a moisture permeability of 150 g / m 2 / 24h or less is more preferable, and 140g / m 2 / 24h or less is particularly preferred, and 120g / m 2 / 24 hours or less is even more preferable.
[0073] The surface of the transparent protective film to which the polarizer is not bonded can be provided with a functional layer such as a hard coat layer, an antireflection layer, an antisticking layer, a diffusion layer, an antiglare layer, etc. The functional layer such as the hard coat layer, the antireflection layer, the antisticking layer, the diffusion layer, or the antiglare layer can be provided on the transparent protective film itself, or can be provided separately from the transparent protective film.
[0074] The thickness of the transparent protective film can be determined as appropriate, but is generally about 1 to 500 μm, preferably 1 to 300 μm, more preferably 5 to 200 μm, further preferably 10 to 200 μm, and more preferably 20 to 80 μm, from the viewpoints of workability such as strength and handleability, thinness, etc.
[0075] As the transparent protective film, a retardation film having a front retardation of 40 nm or more and / or a thickness direction retardation of 80 nm or more can be used. The front retardation is usually controlled in the range of 40 to 200 nm, and the thickness direction retardation is usually controlled in the range of 80 to 300 nm. When a retardation film is used as the transparent protective film, the retardation film also functions as the transparent protective film, thereby enabling a thinner film to be achieved.
[0076] Examples of the retardation film include a birefringent film obtained by uniaxially or biaxially stretching a polymer material, an oriented film of a liquid crystal polymer, an oriented layer of a liquid crystal polymer supported by a film, etc. The thickness of the retardation film is not particularly limited, but is generally about 20 to 150 μm.
[0077] The retardation film may be a film satisfying the following formulas (1) to (3): 0.70<Re
[450] / Re
[550] <0.97 (1) 1.5×10 -3 < Δn < 6 × 10 -3 ... (2) 1.13<NZ<1.50 ... (3) (wherein Re
[450] and Re
[550] are in-plane retardation values of the retardation film measured at 23°C with light of wavelengths of 450 nm and 550 nm, respectively; Δn is in-plane birefringence, which is nx-ny, where nx and ny are the refractive indices in the slow axis direction and the fast axis direction of the retardation film, respectively; and NZ is the ratio of nx-nz, which is the birefringence in the thickness direction, to nx-ny, which is the in-plane birefringence, where nz is the refractive index in the thickness direction of the retardation film).
[0078] The method for producing a laminated optical film according to the present invention is a method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, and includes the following steps: a first coating step of coating an adhesive composition containing at least a compound represented by general formula (1) and water onto the bonding surface of the first optical film while transporting the first optical film; a second coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator onto the bonding surface of the second optical film while transporting the second optical film; a laminating step of laminating the first optical film and the second optical film; and a bonding step of irradiating the first optical film or the second optical film with active energy rays from the first optical film side or the second optical film side to cure at least the adhesive composition, thereby bonding the first optical film and the second optical film via the adhesive layer formed. Each step will be described below.
[0079] (Coating Step) The method for producing a laminated optical film according to the present invention includes a first coating step in which an adhesive composition containing at least a compound represented by general formula (1) and water is applied to the bonding surface of a first optical film while the first optical film is being transported, and a second coating step in which an adhesive composition containing at least a curable component and a polymerization initiator is applied to the bonding surface of a second optical film while the second optical film is being transported. In the present invention, when the film thickness of the adhesive composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, β is designed to be greater than α. In order to produce a laminated optical film having excellent adhesion between the first optical film and the second optical film while increasing the line speed of the laminated optical film production line, β is preferably greater than 1.0 × α, and more preferably greater than 1.1 × α. The film thickness α of the adhesive composition after the first coating step is preferably 200 to 2,000 nm, and more preferably 300 to 1,500 nm. Furthermore, the film thickness β of the adhesive composition after the second coating step is preferably 200 to 2000 nm, and more preferably 300 to 1500 nm.
[0080] The method for applying the adhesion-promoting composition and adhesive composition is appropriately selected depending on the viscosity of the composition and the desired thickness, and examples thereof include a reverse coater, a gravure coater (direct, reverse, or offset), a bar reverse coater, a roll coater, a die coater, a bar coater, and a rod coater. The viscosity of the adhesion-promoting composition and adhesive composition is preferably 0.1 to 200 mPa·s, more preferably 1 to 100 mPa·s, and most preferably 5 to 50 mPa·s. A high viscosity of the composition is undesirable because it results in poor surface smoothness after application and poor appearance. For this reason, each composition can be heated or cooled to adjust the viscosity to a preferred range before application.
[0081] The first optical film and / or the second optical film may be subjected to a surface modification treatment before the coating step. In particular, when a polarizer is used as the first optical film, the surface modification treatment is preferable. Examples of the surface modification treatment include corona treatment, plasma treatment, and Itro treatment, with corona treatment being particularly preferable. By performing corona treatment, reactive functional groups such as carbonyl groups and amino groups are generated on the polarizer surface, improving adhesion to the adhesive layer. Furthermore, the ashing effect removes foreign matter from the surface and reduces surface irregularities, allowing the production of a laminated optical film with excellent appearance characteristics.
[0082] (Laminating Step) The first optical film and the second optical film are laminated together via the adhesive composition and the adhesive composition applied as described above, using a roll laminator or the like.
[0083] In the method for producing a laminated optical film according to the present invention, in order to increase the line speed of the production line, it is preferable not to provide a drying step for removing water contained in the easy-adhesion composition between the first coating step and the laminating step. Also, in order to increase the line speed of the production line, the time required from the end of the first coating step to the start of the laminating step is preferably within 10 seconds, more preferably within 5 seconds.
[0084] In the present invention, the film thickness α of the easy-adhesion composition after the first coating step, the film thickness α' of the easy-adhesion composition when the first optical film and the second optical film are bonded together, and the film thickness β of the adhesive composition after the second coating step can be measured by in-line measurement while the first optical film and the second optical film are being conveyed. It is preferable to use an optical (non-contact) film thickness meter as the film thickness meter used for in-line measurement. The optical (non-contact) film thickness meter is not particularly limited, and examples thereof include a spectral interference film thickness meter, a reflection spectral film thickness meter, and a confocal film thickness meter. In particular, a spectral interference film thickness meter capable of measuring the thickness of the coating film across its entire width is preferred.
[0085] (Bonding Step) The first optical film and the second optical film are bonded together via an adhesive layer formed by curing at least the adhesive composition by irradiating the first optical film surface side or the second optical film surface side with active energy rays. The irradiation direction of the active energy rays (electron beams, ultraviolet rays, visible light, etc.) can be any appropriate direction.
[0086] When irradiating with electron beams, any suitable irradiation conditions can be adopted as long as they are sufficient to at least cure the adhesive composition. For example, the acceleration voltage for electron beam irradiation is preferably 5 kV to 300 kV, more preferably 10 kV to 250 kV. If the acceleration voltage is less than 5 kV, the electron beam may not reach the adhesive, resulting in insufficient curing. If the acceleration voltage is greater than 300 kV, the penetration force through the sample may be too strong, potentially damaging the first optical film and the second optical film. The irradiation dose is 5 to 100 kGy, more preferably 10 to 75 kGy. If the irradiation dose is less than 5 kGy, the adhesive may not be cured sufficiently. If the irradiation dose is greater than 100 kGy, the first optical film and the second optical film may be damaged, resulting in a decrease in mechanical strength and yellowing, making it impossible to obtain the desired optical properties.
[0087] Electron beam irradiation is usually performed in an inert gas atmosphere, but may be performed in the atmosphere or with a small amount of oxygen introduced, if necessary. Depending on the materials of the first and second optical films, by appropriately introducing oxygen, oxygen inhibition is intentionally caused on the first and second optical film surfaces that are first hit by the electron beam, thereby preventing damage to the first and second optical films and allowing the electron beam to be efficiently irradiated only on the adhesive.
[0088] When producing the laminated optical film according to the present invention, it is preferable to use active energy rays that include visible light in the wavelength range of 380 nm to 450 nm, and particularly active energy rays that have the highest exposure dose of visible light in the wavelength range of 380 nm to 450 nm. When using ultraviolet light and visible light, if a second optical film with ultraviolet absorption ability, such as an ultraviolet-opaque transparent protective film, is used, light with a wavelength shorter than approximately 380 nm is absorbed, and light with a wavelength shorter than 380 nm does not reach the adhesive composition and does not contribute to the polymerization reaction. Furthermore, light with a wavelength shorter than 380 nm absorbed by the first optical film and the second optical film is converted into heat, which generates heat in the first optical film and the second optical film, causing defects such as curling and wrinkling in the laminated optical film. Therefore, when ultraviolet rays and visible light are used in the present invention, it is preferable to use an active energy ray generator that does not emit light with a wavelength shorter than 380 nm. More specifically, the ratio of the integrated illuminance in the wavelength range of 380 to 440 nm to the integrated illuminance in the wavelength range of 250 to 370 nm is preferably 100:0 to 100:50, more preferably 100:0 to 100:40. When producing the laminated optical film according to the present invention, the active energy ray is preferably a gallium-encapsulated metal halide lamp or an LED light source that emits light in the wavelength range of 380 to 440 nm. Alternatively, light sources containing ultraviolet and visible light, such as low-pressure mercury lamps, medium-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, incandescent lamps, xenon lamps, halogen lamps, carbon arc lamps, metal halide lamps, fluorescent lamps, tungsten lamps, gallium lamps, excimer lasers, or sunlight, can be used. A bandpass filter can also be used to block ultraviolet rays with a wavelength shorter than 380 nm. In order to prevent curling of the laminated optical film while improving the adhesive performance of the adhesive layer between the first optical film and the second optical film, it is preferable to use active energy rays obtained by using a gallium-encapsulated metal halide lamp and passing through a bandpass filter capable of blocking light with wavelengths shorter than 380 nm, or active energy rays with a wavelength of 405 nm obtained by using an LED light source.
[0089] When the laminated optical film according to the present invention is produced on a continuous line, the line speed depends on the curing time of the adhesive composition, but is preferably 1 to 500 m / min, more preferably 5 to 300 m / min, and even more preferably 10 to 100 m / min. If the line speed is too slow, productivity will be poor, or the damage to the first optical film or the second optical film will be too great, making it impossible to produce a laminated optical film that can withstand durability tests and the like. If the line speed is too high, the adhesive composition will not cure sufficiently, and the desired adhesiveness may not be obtained.
[0090] (Laminated Optical Film) The laminated optical film has at least a first optical film and a second optical film laminated via an adhesive layer, and may also have a pressure-sensitive adhesive layer for bonding to other components such as a liquid crystal cell. The pressure-sensitive adhesive forming the pressure-sensitive adhesive layer is not particularly limited, and may be appropriately selected and used, for example, from a base polymer such as an acrylic polymer, a silicone polymer, a polyester, a polyurethane, a polyamide, a polyether, a fluorine-based polymer, or a rubber-based polymer. In particular, a pressure-sensitive adhesive that has excellent optical transparency, exhibits appropriate adhesive properties such as wettability, cohesion, and adhesiveness, and is excellent in weather resistance, heat resistance, etc., such as an acrylic pressure-sensitive adhesive, may be preferably used.
[0091] The adhesive layer can be provided on one or both sides of the polarizing film or optical film as a superimposed layer of layers with different compositions or types. When provided on both sides, the adhesive layers on the front and back of the polarizing film or optical film can have different compositions, types, thicknesses, etc. The thickness of the adhesive layer can be determined appropriately depending on the intended use, adhesive strength, etc., and is generally 1 to 500 μm, preferably 1 to 200 μm, and particularly preferably 1 to 100 μm.
[0092] The exposed surface of the adhesive layer is covered with a temporary separator to prevent contamination until the adhesive layer is put into practical use. This prevents contact with the adhesive layer during normal handling. As the separator, apart from the thickness requirements described above, any suitable conventional separator can be used, such as a suitable thin sheet such as a plastic film, rubber sheet, paper, cloth, nonwoven fabric, net, foam sheet, metal foil, or a laminate thereof, optionally coated with a suitable release agent such as a silicone-based, long-chain alkyl-based, fluorine-based, or molybdenum sulfide-based release agent.
[0093] The laminated optical film can be preferably used to form various devices such as liquid crystal displays. The formation of a liquid crystal display can be carried out in a conventional manner. That is, a liquid crystal display is generally formed by appropriately assembling a liquid crystal cell, a polarizing film or an optical film, and, if necessary, components such as an illumination system, and incorporating a drive circuit, but in the present invention, there are no particular limitations except that the polarizing film or optical film according to the present invention is used, and the formation can be carried out in a conventional manner. Regarding the liquid crystal cell, any type, such as a TN type, an STN type, or a π type, can be used.
[0094] Appropriate liquid crystal display devices can be formed, such as those in which an optical laminate is disposed on one or both sides of a liquid crystal cell, or those in which a backlight or reflector is used in the illumination system. In such cases, the optical laminate according to the present invention can be disposed on one or both sides of the liquid crystal cell. When optical laminates are disposed on both sides, they may be the same or different. Furthermore, when forming a liquid crystal display device, appropriate components such as a diffuser, anti-glare layer, anti-reflection film, protective plate, prism array, lens array sheet, light diffuser, backlight, etc. can be disposed in one or more layers at appropriate positions.
[0095] Examples of the present invention will be described below, but the embodiments of the present invention are not limited to these.
[0096] <First Optical Film (Polarizer)> A laminate having a 9 μm-thick PVA layer formed on an amorphous PET substrate was subjected to in-air auxiliary stretching at a stretching temperature of 130°C to produce a stretched laminate. The stretched laminate was then dyed to produce a dyed laminate. The dyed laminate was then stretched in boric acid water at a stretching temperature of 65°C to produce an optical film laminate including a 5 μm-thick PVA layer, stretched together with the amorphous PET substrate to a total stretch ratio of 5.94 times. This two-stage stretching resulted in highly oriented PVA molecules in the PVA layer formed on the amorphous PET substrate, and an optical film laminate including a 5.5 μm-thick PVA layer was obtained, constituting a thin polarizer in which iodine adsorbed by dyeing was highly oriented in one direction as a polyiodine ion complex. The thin polarizer obtained here was used as the first optical film.
[0097] <Second Optical Film (Transparent Protective Film)> Transparent protective film: triacetyl cellulose-based resin film (trade name "TJ25", manufactured by Fujifilm Corporation) The above transparent protective film was used as the second optical film.
[0098] <Active energy rays> Visible light (gallium-filled metal halide lamp) was used as the active energy rays. Irradiation device: Light HAMMER10 manufactured by Fusion UV Systems, Inc. Bulb: V bulb Peak irradiance: 1600 mW / cm 2 , cumulative irradiation dose 1000 / mJ / cm 2 The illuminance of visible light was measured using a Sola-Check system manufactured by Solatell.
[0099] Example 1 (Preparation of Easy-Adhesion Composition) An easy-adhesion composition was prepared in the following proportions: 65 mass % N-acryloylmorpholine (compound represented by general formula (2) (trade name "ACMO", manufactured by Kojin Co., Ltd.)), 7 mass % 3-methacrylamidophenylboronic acid (compound represented by general formula (1) (trade name "MAPBA", manufactured by Junsei Chemical Co., Ltd.)), 27.8 mass % pure water, and 0.2 mass % surface conditioner (trade name "EXP.4200", manufactured by Nissin Chemical Industry Co., Ltd.).
[0100] (Preparation of Adhesive Composition) 40.2% by mass of N-acryloylmorpholine (compound represented by general formula (2) (trade name "ACMO", manufactured by Kojin Co., Ltd.)), 2.9% by mass of 3-methacrylamidophenylboronic acid (compound represented by general formula (1) (trade name "MAPBA", manufactured by Junsei Chemical Co., Ltd.)), 52.6% by mass of tripropylene glycol diacrylate (TPGDA) (trade name "Aronix M-220", manufactured by Toagosei Co., Ltd.), 1.9% by mass of 2-methyl-4'-methylthio-2-morpholinopropiophenone (photopolymerization initiator (trade name "Omnirad 907", manufactured by IGM Resins B.V.)), and 1.9% by mass of diethylthioxanthone (photopolymerization initiator (trade name "KAYACURE"). An adhesive composition was prepared using 1.9% by mass of a surfactant (product name "DETX-S" manufactured by Nippon Kayaku Co., Ltd.) and 0.5% by mass of a surface conditioner (product name "EXP.4200" manufactured by Nissin Chemical Industry Co., Ltd.).
[0101] (Production of Laminated Optical Film (Polarizing Film)) Using an MCD Coater (manufactured by Fuji Machine Co., Ltd.) (cell shape: honeycomb, gravure roll line count: 1000 lines / inch, rotation speed 200% / relative to line speed), the adhesive composition was applied to the bonding surface of a first optical film (thin polarizer) (first coating step). The film thickness α of the adhesive composition after the first coating step was 550 nm. Furthermore, using an MCD Coater (manufactured by Fuji Machine Co., Ltd.) (cell shape: honeycomb, gravure roll line count: 1000 lines / inch, rotation speed 160% / relative to line speed), the adhesive composition was applied to the bonding surface of a second optical film (transparent protective film) (second coating step). The film thickness β of the adhesive composition after the second coating step was 600 nm. The film thicknesses α and β were measured by in-line measurement using a spectral interference film thickness meter (manufactured by Ocean Optics: spectrometer "USB2000+", light source "HL-2000", fiber "OCF-103995").
[0102] Next, the transparent protective film and the optical film laminate including the thin polarizer were bonded to each other from the coated side using a roller (bonding step). No drying step was performed between the first coating step and the bonding step, and the time required from the first coating step to the bonding step was designed to be 3 seconds.
[0103] The thin polarizer and the transparent protective film were then bonded together via an adhesive layer obtained by irradiating the laminated transparent protective film with visible light using an active energy ray irradiation device to cure the adhesive composition and the adhesive composition. Next, the amorphous PET substrate of the optical film laminate was peeled off to produce a laminated optical film (polarizing film).
[0104] Examples 2 to 3 and Comparative Examples 1 to 2 Laminated optical films (polarizing films) were produced in the same manner as in Example 1, except that the film thickness α (nm) of the easy-adhesion composition after the first coating step and the film thickness β (nm) of the adhesive composition after the second coating step were changed to those shown in Table 1.
[0105] Example 4 (Preparation of Easy-Adhesion Composition) An easy-adhesion composition was prepared in the following proportions: 77.8 mass % N-acryloylmorpholine (compound represented by general formula (2) (trade name "ACMO", manufactured by Kojin Co., Ltd.)), 7 mass % 3-methacrylamidophenylboronic acid (compound represented by general formula (1) (trade name "MAPBA", manufactured by Junsei Chemical Co., Ltd.)), 15 mass % pure water, and 0.2 mass % surface conditioner (trade name "EXP.4200", manufactured by Nissin Chemical Industry Co., Ltd.).
[0106] A laminated optical film (polarizing film) was produced in the same manner as in Example 1, except that the film thickness α (nm) of the easy-adhesion composition after the first coating step and the film thickness β (nm) of the adhesive composition after the second coating step were changed to those shown in Table 1.
[0107] <Evaluation of Water-Resistant Peel Strength (Water-Resistant Adhesion)> Double-sided tape (No. 500, manufactured by Nitto Denko Corporation) was attached to the PET release surface of the polarizing film. Furthermore, a piece measuring 200 mm parallel to the stretching direction of the thin polarizer and 15 mm perpendicular thereto was cut out, and a slit was made between the thin polarizer and the transparent protective film with a utility knife. The release film of the double-sided tape was then peeled off, and the adhesive surface was attached to a glass plate. The resulting polarizing film attached to the glass plate was then exposed to an environment of 20°C and 98% RH for 240 hours, removed, and then excess moisture was removed. The thin polarizer and the transparent protective film were peeled off in a 90° direction at a peel speed of 1000 mm / min using an angle-flexible adhesive / film peeling analyzer (VPA-2, manufactured by Kyowa Interface Science Co., Ltd.), and the peel strength (N / 15 mm) was measured. ◯: >1.5 N, △: 1.0 N or more but less than 1.5 N, ×: less than 1.0 N
[0108]
Claims
1. A method for producing a laminated optical film in which at least a first optical film and a second optical film are laminated via an adhesive layer, comprising: conveying the first optical film while applying a compound represented by the following general formula (1): (wherein X is a reactive group, Y is an alkylene group having 1 to 12 carbon atoms which may have a branched chain, or a phenylene group which may have a substituent; R 1 and R 2 a first coating step of coating an adhesive composition containing at least a curable component and a polymerization initiator onto a bonding surface of the second optical film while transporting the second optical film; a laminating step of laminating the first optical film and the second optical film; and a bonding step of bonding the first optical film and the second optical film via the adhesive layer formed by irradiating the first optical film surface side or the second optical film surface side with active energy rays to cure at least the adhesive composition, wherein the content of the water in the easy-adhesion composition is 40 mass% or less, and wherein when the film thickness of the easy-adhesion composition after the first coating step is α and the film thickness of the adhesive composition after the second coating step is β, β>α.
2. The method for producing a laminated optical film according to claim 1, wherein no drying step is provided between the first coating step and the laminating step.
3. The method for producing a laminated optical film according to claim 1, wherein the time required from the end of the first coating step to the start of the laminating step is within 5 seconds.
4. The method for producing a laminated optical film according to claim 1, wherein the first optical film is a polarizer.
5. The method for producing a laminated optical film according to claim 1, wherein the second optical film is a transparent protective film.
6. The adhesive composition contains, as a polymerizable component, a compound represented by the following general formula (2): A compound represented by the formula (wherein R 4 is a hydrogen atom or a methyl group, R 5 and R 6 are each independently a hydrogen atom, an alkyl group, a hydroxyalkyl group, an alkoxyalkyl group, or a cyclic ether group, and R 5 and R 6 The method for producing a laminated optical film according to claim 1 , further comprising the step of:
7. The method for producing a laminated optical film according to claim 1, wherein the adhesive composition contains a compound represented by the general formula (2).
Citation Information
Patent Citations
Process for Preparing Polarizer
KR1020150052777A
Polarizing film manufacturing method
WO2020196618A1
Method for manufacturing polarizing film
WO2020196625A1
Method for producing multilayer polarizing film
WO2021095304A1
Method for producing polarizing film
WO2021141037A1